Method for producing single crystal spherical carbon nanoparticles
Single-crystal spherical carbon nanoparticles are prepared by lithium, sodium or potassium and fused aromatic compounds at low temperatures and reacting with halogenated carbon raw material liquid. The fluorescence efficiency and biological phase in the prior art are solved. The problem of insufficient capacitance has achieved efficient application of fluorescent labeling and battery electrode materials.
Patent Information
- Application Number
- CN202280095253.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-14
- Filing Date
- 2022-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to manufacture single crystal spherical carbon nanoparticles that can be used as fluorescent markers and battery electrode materials in the human body, and their fluorescence efficiency and biocompatibility are insufficient.
By mixing lithium, sodium or potassium with the fused aromatic compound at low temperature, an anion of the fused aromatic compound is generated and mixed with the halogenated carbon raw material liquid, reacted using a relatively rotating fluid treatment device to prepare a non-existent one without Single-crystal spherical carbon nanoparticles that reduce fluorescence efficiency.
Single-crystal spherical carbon nanoparticles with high fluorescence quantum efficiency can be used as non-toxic drug delivery fluorescent markers and high-density filled battery electrode materials, improving the fluorescence efficiency and biocompatibility of carbon nanoparticles.
Smart Images

Figure CN119095794A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing single-crystal spherical carbon nanoparticles. Background Art
[0002] Carbon nanoparticles are nanoparticles composed of carbon atoms, and carbon nanoparticles with a particle size of less than 10 nm are also called carbon quantum dots. Among quantum dots, those formed from metal elements such as CdSe and CdTe and showing fluorescence are known. However, since these quantum dots are not suitable for use in the human body, alternative substances have been explored.
[0003] Known carbon nanoparticles can be manufactured by top-down or bottom-up methods. As a method for manufacturing carbon nanoparticles from top to bottom, for example, known methods for manufacturing carbon nanoparticles from carbon materials of at least micrometer size such as graphite, carbon nanotubes, diamonds, etc. are used by laser ablation, arc discharge, and electrochemical methods. And as a method for manufacturing carbon nanoparticles from bottom to top, for example, known methods for heat-treating pure water and organic solvents under high temperature and high pressure conditions and methods for utilizing chemical vapor phase growth methods (CVD) are used as hydrothermal methods.
[0004] When carbon nanoparticles are used as drugs for delivery in the human body, hydrophobic carbon nanoparticles must be hydrophilized. Therefore, an oxidation reaction in the atmosphere is performed; a surfactant is mixed in an aqueous solution to disperse in the aqueous solution and then the surface of the carbon nanoparticles is hydrophilized using an oxidant or the like. As for the hydrophilization of carbon nanoparticles in an aqueous solution when a surfactant is used in combination, a cleaning process is required to remove the surfactant after treatment, and such a complicated treatment has become a problem.
[0005] Claim 1 of Patent Document 1 describes a carbon nanoparticle phosphor containing carbon atoms, oxygen atoms, nitrogen atoms, and hydrogen atoms as required. Since the carbon nanoparticle phosphor has CN bonds and CO bonds, it can be dispersed in an aqueous solution. Claim 9 of Patent Document 1 discloses a method for manufacturing a carbon nanoparticle phosphor comprising the following steps: a solution in which an organic substance selected from citric acid, benzoic acid, glucose, fructose, and sucrose, an amine, and one or more selected from an inorganic acid and acetic acid are dissolved in a water-soluble solvent is subjected to hydrothermal synthesis. The spatial lattice as structural information of the carbon nanoparticle phosphor is not disclosed.
[0006] Patent Document 2 describes a carbon composite for an oxygen reduction catalyst comprising nanosheet-shaped graphene oxide or its reduced product and carbon quantum dots (claim 1). It is described that the carbon quantum dots may be carbon obtained by a conventional hydrothermal reaction, for example, carbon obtained by heating an aqueous solution comprising a carbon source compound such as citric acid and a nitrogen source compound such as ethylenediamine at a temperature above the boiling point of water (claim 6,
[0031] , etc.). The carbon quantum dots are different from the single-crystal spherical carbon nanoparticles of the present invention, and it is not disclosed that the carbon nanoparticle phosphor is single-crystal and spherical.
[0007] Patent document 3 describes a method for producing luminescent nanocarbon, which includes a reaction step of reacting a raw material solution containing a carbon source compound and a nitrogen source compound by a solvent thermal synthesis method or the like (claim 1,
[0013] ). The luminescent nanocarbon is produced by the same hydrothermal synthesis as the production method of patent document 1, and does not disclose that the carbon nanoparticle phosphor is single crystal or spherical.
[0008] Patent document 4 describes a method for forming carbon dots, comprising: (a) mixing carbon powder with sulfuric acid and nitric acid to form a carbon powder mixture; (b) heating the carbon powder mixture under reflux to form a reflux carbon powder mixture; then, (c) cooling the reflux carbon powder mixture; (d) neutralizing the reflux carbon powder mixture to form a neutralized carbon powder mixture containing soluble carbon dots, etc. (Claim 1,
[0036] ). By using an acid in step (a), the carbon powder is oxidized to a quantum size of 1.5 to 6 nm (
[0037] ,
[0038] ). The carbon dots modulated by the formation method have abundant carboxyl groups on the surface, and the carboxyl groups may have negative charges (
[0048] ). Since the carbon dots have abundant carboxyl groups on the surface, they are different from the single-crystal spherical carbon nanoparticles of the present invention. In addition, Patent document 4 does not disclose that the carbon nanoparticle phosphor is single-crystal and spherical.
[0009] In patent document 5, the applicant of the present application discloses a method for producing semiconductor particles, which uses a fluid processing device with a relatively rotating processing surface that can be approached and / or separated (claim 1). As a specific example of a semiconductor element, an element selected from silicon, germanium, carbon and tin is described (
[0037] ). However, there is no specific embodiment in which the semiconductor element is carbon. Based on patent document 5, single crystal spherical carbon nanoparticles cannot be obtained.
[0010] Patent document 6, to which the applicant of the present application is related, describes a method for producing crystals composed of fullerenes, which uses a fluid processing device having a relatively rotating processing surface that can be approached and / or separated (claim 1). This production method is a method of using fullerenes in the raw material in advance and re-crystallizing, and is not a method for producing fullerenes themselves. As mentioned above, Patent document 6 does not disclose that the carbon nanoparticle phosphor is single crystal and spherical.
[0011] In non-patent document 1, it is described that carbon quantum dots are synthesized by reducing carbon tetrachloride with a hydride reducing agent such as lithium aluminum hydride to form carbon quantum dots, and then reacting with an arylamine in the presence of a platinum catalyst. The carbon quantum dots of non-patent document 1 have NH2 groups on the surface, and are therefore different from the single-crystal spherical carbon nanoparticles of the present invention. In addition, it is not disclosed that the carbon quantum dots are single crystal and spherical.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: WO2018 / 163955
[0015] Patent Document 2: Japanese Patent Application Laid-Open No. 2019-155349
[0016] Patent Document 3: Japanese Patent Application Laid-Open No. 2021-183548
[0017] Patent Document 4: Japanese Patent Application Laid-Open No. 2019-511442
[0018] Patent Document 5: Japanese Patent 4458202
[0019] Patent Document 6: Japanese Patent 4363495
[0020] Non-patent literature
[0021] Non-patent document 1: Journal of Material Chemistry, Volume 2, pp. 6025-6031 (2014) Summary of the invention
[0022] Problems to be solved by the invention
[0023] The present invention aims to provide a method for producing carbon nanoparticles that can generate blue to red fluorescence using excitation wavelengths from ultraviolet light to visible light, can be used as a fluorescent marker that can be injected into the body as an almost non-toxic drug delivery, and can be densely filled with electrode materials for secondary batteries.
[0024] Means for solving problems
[0025] The present inventors conducted in-depth research to solve the above-mentioned problems, and found that: by mixing lithium, sodium or potassium with a condensed aromatic compound at a temperature below 0°C, an anion of a condensed aromatic compound is prepared; by mixing a raw material liquid containing a carbon halide with a prepared reducing liquid containing the anion of the condensed aromatic compound and reacting them, single-crystal, spherical single-crystal spherical carbon nanoparticles can be produced; the produced single-crystal spherical carbon nanoparticles are single crystals without grain boundaries that reduce luminescence efficiency, and therefore can produce high fluorescence quantum efficiency by utilizing excitation of light with a wide wavelength from ultraviolet light to visible light, can be used as a fluorescent marker for drug delivery, and can be densely filled with electrode materials for secondary batteries, thereby completing the present invention.
[0026] That is, the present invention is as follows.
[0027] [1] A method for producing single-crystal, spherical single-crystal spherical carbon nanoparticles, comprising the steps of mixing and reacting a raw material liquid containing a halogenated carbon with a reducing liquid containing an anion of the condensed aromatic compound generated from lithium, sodium or potassium and a condensed aromatic compound, wherein the anion of the condensed aromatic compound is obtained by mixing lithium, sodium or potassium with the condensed aromatic compound at a temperature below 0°C.
[0028] [2] The method according to [1], wherein the perimeter (Z) and area (S) of the projected image of the single-crystal spherical carbon nanoparticle observed using a transmission electron microscope are used to calculate the area of the single-crystal spherical carbon nanoparticle using the mathematical formula: 4πS / Z 2 The calculated average value of the circularity was 0.9 or more.
[0029] [3] The production method according to [1] or [2], wherein the average particle size is 1 nm to 30 nm.
[0030] [4] A manufacturing method according to any one of [1] to [3], wherein the raw material liquid and the reducing liquid are mixed and reacted using the following device, the device comprising: a fluid pressure imparting mechanism for imparting pressure to a processed fluid; at least two processing parts, a first processing part and a second processing part that can be relatively approached and / or separated from the first processing part; and a rotational drive mechanism for causing the first processing part and the second processing part to rotate relative to each other, at least two processing surfaces, a first processing surface and a second processing surface, are provided at positions opposing each other in each of the processing parts, each of the processing surfaces constituting a part of a sealed flow path through which the pressurized processed fluid flows, two or more processed fluids, at least one of which contains a reactant, are mixed and reacted between the two processing surfaces, and among the first processing part and the second processing part, at least the second processing part has a pressure-receiving surface, and the pressure-receiving surface At least a part of the pressure-bearing surface is composed of the second processing surface, and the pressure-bearing surface is subjected to the pressure applied to the processed fluid by the fluid pressure imparting mechanism, thereby generating a force to move the second processing surface in the direction of separation from the first processing surface. By allowing the processed fluid under pressure to pass between the first processing surface and the second processing surface that are accessible and / or separable and relatively rotatable, the processed fluid forms a thin film fluid, and further has another inlet path independent of the flow path between the processing surfaces through which the processed fluid under pressure flows. At least one of the first processing surface and the second processing surface is provided with at least one opening portion connected to the another inlet path, and at least one processed fluid transported from the another inlet path is introduced into the space between the two processing surfaces, and the reactant contained in at least any one of the processed fluids and the processed fluid different from the processed fluid are mixed in the thin film fluid.
[0031] [5] The manufacturing method according to [4], wherein the opening is provided on the downstream side of a point where the flow of the fluid to be processed passing between the two processing surfaces becomes a laminar flow.
[0032] [6] The production method according to any one of [1] to [5], wherein the molar ratio of the lithium, sodium or potassium to the carbon halide is 7:1 to 4:1.
[0033] [7] The production method according to any one of [1] to [6], wherein the condensed aromatic compound is at least one selected from biphenyl, naphthalene, 1,2-dihydronaphthalene, anthracene, phenanthrene and pyrene.
[0034] [8] The production method according to [7], wherein, when the condensed aromatic compound is biphenyl, naphthalene or anthracene, in the IR absorption spectrum of the reducing solution, at 1200 cm -1 ~1100cm -1The absorption peak is shown in the wavenumber range of .
[0035] [9] The production method according to any one of [1] to [8], wherein the solvent contained in the reducing solution is tetrahydrofuran and / or dimethoxyethane having a residual water content of 10 ppm or less.
[0036]
[10] The production method according to any one of [1] to [9], wherein the solvent contained in the reducing solution is tetrahydrofuran containing a phenol-based polymerization inhibitor, having a residual water content of 10 ppm or less, and a residual oxygen concentration of less than 0.1 ppm.
[0037]
[11] The production method according to any one of [1] to
[10] , wherein the solvent contained in the raw material liquid is tetrahydrofuran having a residual water content of 10 ppm or less and a residual oxygen concentration of less than 0.1 ppm.
[0038]
[12] The production method according to any one of [1] to
[11] , wherein the carbon halide is carbon tetrachloride, carbon tetrabromide or carbon tetraiodide.
[0039]
[13] The production method according to any one of [1] to
[12] , wherein the single-crystal spherical carbon nanoparticles are hexagonal crystals, and the spatial lattice is composed of a simple lattice, a rhombohedral lattice, or a simple lattice and a rhombohedral lattice.
[0040]
[14] The production method according to any one of [1] to
[13] , wherein the single-crystal spherical carbon nanoparticles have an IR absorption spectrum at 2800 cm -1 ~2950cm -1 The absorption peak is shown in the wave number range of 900cm -1 ~1900cm -1 The 1000cm -1 ~1100cm -1 The absorption peak area relative to 900 cm -1 ~1900cm -1 The total area of the wavenumber range is less than 15%.
[0041]
[15] The production method according to any one of [1] to
[14] , wherein the single-crystal spherical carbon nanoparticles have a wavelength of 900 cm-1 in the IR absorption spectrum. -1 ~1900cm -1 The 1300 cm -1 ~1400cm -1 The absorption peak area relative to 900 cm -1 ~1900cm -1 The total area of the wavenumber range is less than 10%.
[0042]
[16] The method according to any one of [1] to
[15] , wherein the single-crystal spherical carbon nanoparticles have a Raman scattering spectrum of 1550 cm -1 ~1650cm -1 The intensity of the peak is set as I G , 1250cm -1 ~1350cm -1 The intensity of the peak is set as I D When D / I G The ratio is less than 1.0.
[0043]
[17] The production method according to any one of [1] to
[16] , wherein the single-crystal spherical carbon nanoparticles produce a fluorescence maximum in a wavelength range of 400 nm to 600 nm in a fluorescence spectrum.
[0044] Effects of the Invention
[0045] According to the manufacturing method of the present invention, single crystal, spherical single crystal spherical carbon nanoparticles can be manufactured. The single crystal spherical carbon nanoparticles manufactured by the manufacturing method of the present invention are single crystals without grain boundaries that reduce fluorescence efficiency, so they can produce fluorescence with high fluorescence quantum efficiency by using excitation of light with a wide wavelength from ultraviolet light to visible light, which can increase the fluorescence quantum efficiency of carbon nanoparticles known so far by more than 10%. In addition, the single crystal spherical carbon nanoparticles manufactured by the manufacturing method of the present invention do not have the toxicity to organisms that compound semiconductors formed by cadmium, selenium, tellurium, etc. have, so they can be used in drug delivery. Furthermore, the single crystal spherical carbon nanoparticles manufactured by the manufacturing method of the present invention are spherical, so they can be filled with high-density electrode materials of solar cells and secondary ion batteries, and can be used as negative electrodes of lithium ion batteries and electrode materials of solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is the IR absorption spectrum of naphthalene anions in the reducing solution of single-crystal spherical carbon nanoparticles.
[0047] Figure 2 This figure shows a TEM observation image of the single-crystal spherical carbon nanoparticles produced in Example 1-1.
[0048] Figure 3 The wave number of the single-crystal spherical carbon nanoparticles prepared in Example 1-2 is 2700 cm -1 ~3050cm -1 IR spectrum at .
[0049] Figure 4The wave number 900 cm represents the single crystal spherical carbon nanoparticles prepared in Example 1-2. -1 ~1900cm -1 Waveform separation of the IR spectrum at .
[0050] Figure 5 The normalized fluorescence spectrum of the single-crystalline spherical carbon nanoparticles prepared in Example 1-3 is shown, that is, the normalized fluorescence spectrum in which the maximum intensity is set to 1.0 and the excitation wavelength is changed every 40 nm from 300 nm to 750 nm.
[0051] Figure 6 To express based on Figure 5 The graph of the relationship between the excitation wavelength and the fluorescence peak wavelength prepared based on the results of . The graph shows the excitation wavelength dependency of the fluorescence peak wavelength of the single-crystalline spherical carbon nanoparticles of Example 1-3.
[0052] Figure 7 The wave number 1250 cm-1 represents the single crystal spherical carbon nanoparticles prepared in Example 1-3. -1 Up to 1700cm -1 Raman scattering spectrum at .
[0053] Figure 8 The X-ray diffraction patterns of the single-crystal spherical carbon nanoparticles produced in Examples 1-1 to 1-3 at diffraction angles (2θ) of 42° to 46° are shown.
[0054] Fig. 9 The X-ray diffraction patterns of the single-crystal spherical carbon nanoparticles produced in Examples 3-1 to 3-3 at diffraction angles (2θ) of 42° to 46° are shown.
[0055] Fig.10 The normalized fluorescence spectrum of the single-crystalline spherical carbon nanoparticles prepared in Example 3-3 is shown, that is, the normalized fluorescence spectrum when the maximum intensity is set to 1.0 and the excitation wavelength is changed from 240 nm to 360 nm. DETAILED DESCRIPTION
[0056] The following describes the embodiments of the present invention. However, the present invention is not limited to the embodiments described below. In addition, the application examples of the luminescent material that generates fluorescence are described by way of example, and the use of the single-crystal spherical carbon nanoparticles produced by the production method of the present invention is not limited to these.
[0057] 1. Single crystal spherical carbon nanoparticles
[0058] The single-crystalline spherical carbon nanoparticles manufactured by the manufacturing method of the present invention are single-crystalline and spherical. The average particle size of the single-crystalline spherical carbon nanoparticles is preferably 1nm to 30nm. If the average particle size is greater than 30nm, it is difficult to perform high-density filling when the single-crystalline spherical carbon nanoparticles are used as negative electrode materials for secondary batteries. The single-crystalline spherical carbon nanoparticles are hexagonal crystals. The spatial lattice of the hexagonal crystal can present a structure of a simple lattice and a rhombohedral lattice. The single-crystalline spherical carbon nanoparticles are spherical and can be roughly spherical. For single-crystalline spherical carbon nanoparticles, preferably, the circumference (Z) and area (S) of the projected image of the single-crystalline spherical carbon nanoparticles observed using a transmission electron microscope are used, and the mathematical formula: 4πS / Z 2 The calculated average value of circularity is 0.9 or more, more preferably 0.92 or more, and even more preferably 0.95 or more. When fluorescence from single-crystal spherical carbon nanoparticles is used, the average particle size of the single-crystal spherical carbon nanoparticles is preferably 1.2 nm to 10 nm, more preferably 1.5 nm to 7 nm, and even more preferably 2 nm to 5 nm.
[0059] Carbon has various structures, also known as sp 2 The C=C bond composed of carbon atoms in the hybrid orbital is the basic graphene layer, the graphite in which the graphene layer is stacked in the c-axis direction, and the structure of the carbon nanotube. However, since these do not have a band gap, the excited electrons generated by the excitation light and the holes as the electron holes from which the excited electrons are separated immediately recombine, and no fluorescence is generated. Therefore, it is necessary to use some method to make the sp 2 The carbon atoms with sp hybrid orbitals form a band gap. One method for this is to place sp 2 The region of the carbon atom bonded to the hybrid orbital is cut off, and an sp 3 The combination of carbon atoms with sp 3 The bonding of carbon atoms in the hybrid orbital can generate CH bonds and CO bonds by bonding hydrogen and oxygen at the ends of the graphene layer. Therefore, it is preferred to prepare carbon particles having the following structure: a graphene layer having CH bonds in the graphene layer constituting the single-crystal spherical carbon nanoparticle and a graphene layer having CO bonds at the ends of the graphene layer are stacked. In terms of the presence of CO bonds in the single-crystal spherical carbon nanoparticle, for example, in the IR absorption spectrum, the 2800cm-1 wavelength attributable to the stretching vibration of the CH bond can be used to identify the carbon atoms in the single-crystal spherical carbon nanoparticle. -1 ~2950cm -1 The wave number region of 1000 cm-1 and the wave number region of 1000 cm-1 attributed to the stretching vibration of CO bond -1 ~1100cm -1The single-crystal spherical carbon nanoparticles of Example 1-2 are as follows. Figure 2 and Figure 3 As recorded in 2925cm -1 and 2852cm -1 There are absorption peaks generated by CH bonds and at 1097 cm -1 The presence of an absorption peak due to the CO bond confirms that the sp 3 The presence of hybrid orbitals of carbon atoms causes structural changes that lead to the generation of a band gap.
[0060] As the single-crystal spherical carbon particles, preferably the following single-crystal spherical carbon particles can be cited: -1 ~2950cm -1 The wave number range shows an absorption peak, 900cm -1 ~1900cm -1 The 1000cm -1 ~1100cm -1 The area of the absorption peak (stretching vibration of CO bond) is relative to 900 cm -1 ~1900cm -1 The total area of the wavenumber range is 15% or less (ratio of CO bonds), more preferably 2% or more and 15% or less, further preferably 2% or more and 10% or less, and further preferably 2% or more and 8.5% or less.
[0061] As for the single-crystal spherical carbon particles, preferably, the following single-crystal spherical carbon particles can be cited: -1 ~1550cm -1 The intensity of the peak is set as I G , 1250cm -1 ~1350cm -1 The intensity of the peak is set as I D When D / I G The ratio is 1.0 or less, preferably 0.95 or less, more preferably 0.85 or less, further preferably 0.65 or less, and further preferably 0.55 or less.
[0062] Preferred examples of the single-crystal spherical carbon particles include single-crystal spherical carbon nanoparticles that have a fluorescence maximum in a wavelength range of 400 nm to 600 nm in a fluorescence spectrum.
[0063] The single-crystal spherical carbon particles preferably include the following single-crystal spherical carbon particles: -1 ~1900cm-1 The 1300cm -1 ~1400cm -1 The absorption peak area relative to 900 cm -1 ~1900cm -1 The total area of the wave number range is 10% or less (ratio of CN bonds), more preferably 8% or less, and further preferably 6.5% or less.
[0064] It is known that the fluorescence of carbon nanoparticles occurs due to the following three different mechanisms.
[0065] (A) According to the import of sp 3 The fluorescence color is controlled by controlling the particle size of carbon nanoparticles of carbon atoms in hybrid orbitals and changing the band gap of electron energy, which is a physical factor (known as quantum effect).
[0066] (B) By treating the surface of carbon nanoparticles with various chemical substances, various substituents such as alkyl and amino groups with different molecular chain lengths are chemically bonded to the surface of silicon nanoparticles, thereby controlling the fluorescence color of the surface substituents.
[0067] (C) Control of fluorescent color based on chemical factors caused by changes in the composition of oxygen and nitrogen contained in carbon nanoparticles
[0068] The single-crystal spherical carbon nanoparticles of the present invention produce fluorescence by synergistic action of the mechanism of (A) quantum effect and the mechanism of (C) via oxygen among the three mechanisms (A) to (C). The amino-terminated carbon nanoparticles of non-patent document 1 that utilize the mechanism of (A) quantum effect and the mechanism of (B) surface modification have different mechanisms. The single-crystal spherical carbon nanoparticles of the present invention preferably produce fluorescence maximum in the wavelength range of 400nm to 600nm.
[0069] 2. Method for producing single-crystal spherical carbon nanoparticles
[0070] The manufacturing method of the present invention is a method for manufacturing single-crystal, spherical single-crystal spherical carbon nanoparticles, comprising the steps of mixing and reacting a raw material liquid containing a halogenated carbon with a reducing liquid containing anions of the condensed aromatic compound generated from lithium, sodium or potassium and a condensed aromatic compound, wherein the anions of the condensed aromatic compound are obtained by mixing lithium, sodium or potassium with the condensed aromatic compound at a temperature below 0° C. For example, the single-crystal spherical carbon nanoparticles can be manufactured by mixing a liquid containing a raw material (liquid B) of the single-crystal spherical carbon nanoparticles and a reducing liquid (liquid A) containing metallic lithium and a condensed aromatic compound in a thin film fluid formed between two processing surfaces that are arranged to be accessible and / or separable, at least one of which rotates relative to the other.
[0071] (Single crystal spherical carbon nanoparticle raw material solution (Solution B))
[0072] As the raw material of the single crystal spherical carbon nanoparticles, there is no particular limitation as long as it is a substance that can precipitate the single crystal spherical carbon nanoparticles by reduction. As the raw material, preferably carbon tetrahalides are listed, and more preferably carbon tetrachloride, carbon tetrabromide, carbon tetraiodide, etc. can be listed. More preferably, carbon tetrachloride, carbon tetrabromide, etc. can be listed.
[0073] As the solvent of the raw material liquid of single crystal spherical carbon nanoparticles, as long as it is a material that can reduce the raw material of single crystal spherical carbon nanoparticles so that the single crystal spherical carbon nanoparticles are precipitated and does not affect the reduction reaction and is inactive, there is no particular limitation. As the solvent, preferably ethers etc. can be listed, more preferably tetrahydrofuran (THF), dioxane, 1,2-dimethoxyethane (DME), diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethyl ether, polyethylene glycol dimethyl ether or their mixtures etc. can be listed, more preferably THF, DME etc. can be listed.
[0074] (Residual moisture / residual oxygen in solvent)
[0075] It is preferred to use a solvent in which the residual water content in the solvent used in the present invention is 10 ppm or less. The reason is that when a reduction reaction is used in a solvent to produce single-crystal spherical carbon nanoparticles, when the residual water content is more than 10 ppm, the oxidation reaction of the graphene layer becomes significant, causing deformation in the graphite structure generated by stacking the graphene layers in the c-axis direction. This is because, when the graphene layers fail to stack one another, a disadvantageous situation occurs in which single-crystal spherical carbon nanoparticles are not formed.
[0076] The residual oxygen concentration in the solvent used in the present invention is preferably less than 0.1 ppm.
[0077] (Single crystal spherical carbon nanoparticle reduction solution (Solution A))
[0078] The reducing agent contained in the single-crystal spherical carbon nanoparticle reducing solution is not particularly limited as long as it can reduce the raw material of the single-crystal spherical carbon nanoparticles contained in the single-crystal spherical carbon nanoparticle raw material solution to precipitate the single-crystal spherical carbon nanoparticles. Examples of the reducing agent include a combination of metallic lithium and a condensed aromatic compound.
[0079] As the condensed aromatic compound, there can be cited a condensed aromatic compound that can generate a lithium ion and a condensed aromatic compound anion (radical anion) by moving one electron from metallic lithium to the condensed aromatic compound. The condensed aromatic compound anion that moves one electron has one electron in the lowest unoccupied orbital (LUMO) of the condensed aromatic compound. For example, in the case where the raw material of the single-crystal spherical carbon nanoparticle is carbon tetrachloride, since the reduction potential of carbon tetrachloride is -1.9V, in order to reduce carbon tetrachloride to carbon nanoparticles, the potential of the condensed aromatic compound anion must be lower than the potential -1.9V. Here, the so-called potential is a value relative to silver (Ag) / silver chloride (AgCl) as a standard electrode (reference electrode). As the condensed aromatic compound having a potential lower than -1.9 V, for example, naphthalene (-2.53 V), DBB (-2.87 V), biphenyl (-2.68 V), 1,2-dihydronaphthalene (-2.57 V), phenanthrene (-2.49 V), anthracene (-2.04 V), pyrene (-2.13 V), or mixtures thereof, preferably, naphthalene, DBB, biphenyl, etc. On the other hand, tetracene (-1.55 V) and azulene (-1.62 V) are not suitable for reduction by carbon tetrachloride.
[0080] The molar ratio of the metal lithium to the condensed aromatic compound may be, for example, 1:1 to 1:5, preferably 1:1 to 1:1.2, and more preferably 1:1 to 1:15.
[0081] The molar ratio of metallic lithium to the raw material of single-crystalline spherical carbon nanoparticles can be, for example, 10:1 to 1.2:1, preferably 7:1 to 1.5:1, and more preferably 5:1 to 3:1. It is preferred to use metallic lithium in excess compared to the raw material of single-crystalline spherical carbon nanoparticles. By using it in excess, single-crystalline spherical carbon nanoparticles can be prepared. In the case of using metallic lithium in an amount less than 3 / 4 of the raw material of single-crystalline spherical carbon nanoparticles, halogen atoms from the raw material remain in the single-crystalline spherical carbon nanoparticles due to incomplete reduction, and the halogen atoms are polycrystalline and no longer spherical. As the solvent of the single-crystalline spherical carbon nanoparticle reduction solution, the above-mentioned solvent used in the single-crystalline spherical carbon nanoparticle raw material solution can be cited. The concentration of metallic lithium in the single-crystalline spherical carbon nanoparticle reduction solution is not particularly limited and is determined according to the molar ratio of the above-mentioned metallic lithium to the raw material of the single-crystalline spherical carbon nanoparticles.
[0082] (Low temperature preparation of reducing fluid)
[0083] Alkali metals can be dissolved in ether-based organic solvents in the presence of condensed aromatic compounds. However, if the dissolution temperature is above 0°C, the anions of the condensed aromatic compounds become unstable, and a chemical reaction between the condensed aromatic compounds and the alkali metal atoms occurs, which may impair the effect of the reducing solution. For example, naphthalene (molecular formula: C10 H8) When lithium (Li) is used as an alkali metal, C 10 Therefore, in the manufacturing method according to the present invention, in order to maintain the liquid adjustment temperature at the stage of preparing the reducing solution of the single-crystal spherical carbon nanoparticles at less than 0°C, the condensed aromatic compound anions can be stably present, thereby suppressing the decomposition of the condensed aromatic compound anions.
[0084] (Solvent molecules mediate between alkali metal cations and fused aromatic compound anions)
[0085] The condensed aromatic compound anions generated by the electron transfer of metal lithium to the condensed aromatic compound can be combined with the metal lithium cations generated by the electron transfer via Coulomb force, and thus, there is a concern that the reduction power may change due to the reverse electron transfer of electrons from the temporarily generated condensed aromatic compound anions to the lithium cations. The change in the reducing power leads to the particle size distribution of the obtained single-crystal spherical carbon nanoparticles, so in order to suppress the change in the reducing power caused by the reverse electron transfer, it is possible to make the lithium cations and the condensed aromatic compound anions have a binding form generated by the Coulomb force of the solvent molecules. It is known that the state of anions and cations in such a solution can be confirmed by the measurement of ultraviolet-visible absorption spectroscopic spectrum. Based on this, it is known that even if it is metal lithium, if the combination of metal lithium and naphthalene is dissolved in tetrahydrofuran as an ether-based organic solvent, the state of THF intervening at 25°C is 60% to 80%, and if the combination of metal sodium and naphthalene is dissolved in THF, it is a state in which the direct sodium cation and the naphthalene anion are directly combined by Coulomb force with almost no THF intervening.
[0086] (Solvation in Low-Temperature Liquid Preparation)
[0087] In order to make the solvent interposed between them, it is possible to make the temperature of the solvent low. That is, the so-called interposing of the solvent between them means that there are solvated cations and solvated anions in which the lithium cations and the condensed aromatic compound anions are surrounded by solvent molecules, and the solvents are in contact with each other. Since such a state in which the solvent is interposed between them and the cations and anions are in contact can be generated in the solution, the condensed aromatic compound anions can exist stably, and the reverse electron transfer from the condensed aromatic compound anions to the lithium cations can be suppressed. The solution state of the solution structure is made into a prepared solution in advance. The reduced solution prepared in the state in which the solvation is not fully performed at a temperature above 0°C and the solvation state is distributed may not be completely solvated even at a low temperature when the carbon nanoparticles are prepared, so the fluctuation of the reducing power occurs, which becomes the cause of the distribution of the particle size of the carbon nanoparticles in the solution. In the state of low temperature, the ions are directly combined with each other by the Coulomb force to form a state of equilibrium. Even if the carbon nanoparticles are cooled to a low temperature, it is difficult for the solvent molecules to overcome the Coulomb force and invade between the cations and anions. Therefore, the temperature during the liquid preparation is important.
[0088] (Polymerization Inhibition by Solvent)
[0089] The necessity of the liquid adjustment at low temperature of the reducing solution is as described from the viewpoint of the solvent. In addition, the storage temperature after the preferred liquid adjustment is also low temperature. When the storage temperature of the reducing solution is high, as a solvent, if a cyclic ether such as THF is used, a reduction polymerization reaction of THF etc. is performed by utilizing a condensed aromatic compound anion. If the polymer produced by the polymerization of such a cyclic ether such as THF is generated, it is mixed in the single crystal spherical carbon nanoparticles generated by the reduction of a halocarbon, so it is preferred to suppress the polymerization reaction. As a polymerization inhibitor of THF, for example, a phenolic polymerization inhibitor added in order to suppress the generation of peroxides of cyclic ethers such as THF can be cited, and preferably BHT (2,6-di-tert-butyl-4-methylphenol) can be cited.
[0090] (Method for producing single-crystal spherical carbon nanoparticles: device)
[0091] The single-crystalline spherical carbon nanoparticles of the present invention can be manufactured, for example, by mixing a liquid (liquid B) containing a raw material of single-crystalline spherical carbon nanoparticles and a reducing liquid (liquid A) containing metallic lithium and a condensed aromatic compound in a thin film fluid generated between two processing surfaces that are relatively arranged, accessible and / or separable, at least one of which rotates relative to the other.
[0092] As the device used in the manufacturing method of the present invention, for example, the fluid treatment device described in Japanese Patent Publication No. 2009-112892 proposed by the applicant of the present application can be cited. The device comprises: a stirring tank having an inner peripheral surface with a circular cross-sectional shape, and a stirring device attached to the inner peripheral surface of the stirring tank with a small gap, the stirring tank includes at least two fluid inlets and at least one fluid outlet, from one of the fluid inlets, a first treated fluid containing one of the reactants in the treated fluid is introduced into the stirring tank, and from one of the fluid inlets other than the above, a second treated fluid containing one of the reactants different from the above reactants is introduced into the stirring tank from a flow path different from the above first treated fluid. By rotating at high speed at least one of the stirring tank and the stirring device relative to the other, the treated fluid is made into a thin film state, and the reactants contained in at least the first treated fluid and the second treated fluid are reacted with each other in the thin film. In addition, devices with the same principle as the fluid treatment devices described in Patent Documents 6 and 7 can be cited.
[0093] Preferably, the single-crystalline spherical carbon nanoparticles are manufactured by mixing a liquid (liquid B) containing the raw material of the single-crystalline spherical carbon nanoparticles with the reducing liquid (liquid A) in the thin film fluid. The single-crystalline spherical carbon nanoparticles are manufactured by the following two-stage steps: First, after the graphene layers as the cores of the single-crystalline spherical carbon nanoparticles are generated, the single-crystalline spherical carbon nanoparticles stacked on each other grow. Even if the B liquid is brought into contact with the A liquid at a temperature of less than 5°C to start the reaction, since the frequency of generation of the cores of the single-crystalline spherical carbon nanoparticles is reduced, the frequency of contact between the graphene layers as the cores of the single-crystalline spherical carbon nanoparticles is also reduced. Therefore, during the growth of the single-crystalline spherical carbon nanoparticles, it is not easily affected by the change in the concentration of the raw material liquid caused by the growth of the surrounding single-crystalline spherical carbon nanoparticles, and the supply of the raw materials required for the growth of the single-crystalline spherical carbon nanoparticles becomes uniform.
[0094] The temperature of the raw material liquid (liquid A) of the single crystal spherical carbon nanoparticles introduced into the thin film fluid generated between two processing surfaces that are relatively arranged, accessible and / or separable, and at least one of which rotates relative to the other, can be, for example, -30°C to 25°C, preferably -10°C to 25°C, and more preferably 0°C to 25°C. In Examples 1 and 3, the temperature of liquid A was set at 17°C for production, and as a result, single crystal spherical carbon nanoparticles that were single crystal and spherical and generated fluorescence with high fluorescence quantum efficiency could be produced.
[0095] The temperature of the single-crystal spherical carbon nanoparticle raw material solution (liquid B) introduced into the thin film fluid generated between two processing surfaces that are relatively arranged, accessible and / or separable, and at least one of which rotates relative to the other, can be, for example, -10°C to 25°C, preferably 0°C to 25°C, and more preferably 10°C to 25°C. In Examples 1 to 3, the temperature of the liquid B was set at 23°C for production, and as a result, single-crystal, spherical, single-crystal spherical carbon nanoparticles that generate fluorescence with high fluorescence quantum efficiency can be produced.
[0096] In the production of single-crystal spherical carbon nanoparticles, for example, lithium chloride is produced as a by-product. Since lithium chloride has high solubility in the reaction solvent, it is easy to separate it from the single-crystal spherical carbon nanoparticles by centrifugal separation.
[0097] 3. Application of single crystal spherical carbon nanoparticles
[0098] The single-crystal spherical carbon nanoparticles produced by the production method of the present invention can be used as, for example, light-emitting elements, light-emitting materials that generate fluorescence, negative electrodes of lithium-ion batteries, electrode materials of solar cells, and bonding materials with substrates of semiconductor devices.
[0099] Example
[0100] Hereinafter, the present invention will be further described with reference to examples, but the present invention is not limited to these examples.
[0101] (Transmission Electron Microscope (TEM): Preparation of Samples for TEM Observation)
[0102] The single-crystal spherical carbon nanoparticles obtained in the examples and comparative examples were dispersed in THF at a concentration of about 0.001% in a container. The container containing the obtained dispersion was introduced into a glove box with an argon atmosphere, and the dispersion was dripped onto a carbon support film and dried to prepare a sample for TEM observation.
[0103] (TEM observation)
[0104] Transmission electron microscope JEM-2100 (manufactured by JEOL Ltd.) was used in TEM observation of single-crystal spherical carbon nanoparticles. As a sample, the above-mentioned TEM observation sample was used. As for the observation conditions, the acceleration voltage was set to 200 kV, and the observation magnification was set to more than 10,000 times. The particle size was calculated by the distance between the maximum peripheries of the single-crystal spherical carbon nanoparticles observed by TEM, and the average value (average particle size) of the results of measuring the diameter of the single-crystal spherical carbon nanoparticles for 50 particles was calculated.
[0105] (Infrared (IR) absorption spectrum)
[0106] The IR absorption spectrum of the single-crystal spherical carbon nanoparticles was measured using a Fourier transform infrared spectrophotometer FT / IR-6600 (manufactured by JASCO Corporation) using the attenuated total reflection (ATR) method. The measurement conditions were a resolution of 4.0 cm -1 , cumulative times 128 times, using a diamond prism (ATR PRO470-H, an accessory of FT / IR-6600), with an incident angle of 45°. Accumulated times 128 times, a diamond prism (PKS-D1F) (wide area): refractive index 2.4) was assembled in the ATRPRO ONE, an accessory of FT / IR-6600, with an incident angle of 45°. The infrared (IR) absorption spectra measured for the single-crystal spherical carbon nanoparticles manufactured in the examples and the polycrystalline carbon nanoparticles manufactured in the comparative examples are labeled as IR spectra.
[0107] (Confirmation of the formation of anions of condensed aromatic compounds)
[0108] As an example of a condensed aromatic compound, the case of naphthalene is described. By adding metallic lithium to a tetrahydrofuran (THF) solution in which naphthalene is dissolved, a naphthalene anion is generated as a reducing species, and its generation is confirmed by IR absorption spectroscopy. For the measurement sample, a reducing solution is dripped onto a potassium bromide (KBr) plate in an argon atmosphere glove box, and after covering the dripping liquid with another KBr plate, it is held with MagHoldIR (manufactured by Jasco Instruments) and taken out of the argon atmosphere glove box. The sample is measured by transmission method using Fourier transform infrared spectrophotometer FT / IR-6600 (manufactured by JASCO Corporation). The measurement conditions are a resolution of 4.0 cm -1 , the cumulative number of times is 8 times.
[0109] (fluorescence spectrum)
[0110] The fluorescence spectrum of single-crystal spherical carbon nanoparticles was measured using a spectrofluorophotometer FT-6500 (manufactured by JASCO Corporation). As a sample, the above-mentioned TEM observation sample was used. As a sample, a sample solution dispersed in THF was placed in a quartz cell (optical path length: 1 cm) in a glove box with an argon atmosphere, and after the upper part was plugged, it was taken out of the glove box and measured. The measurement conditions were an excitation bandwidth of 3 nm, a fluorescence bandwidth of 3 nm, a response of 0.1 seconds, a scanning speed of 100 nm / min, and a data import interval of 0.5 nm. Similarly, for 9,10-diphenylanthracene, a standard substance for relative fluorescence quantum efficiency, the fluorescence spectrum was also measured under the same conditions.
[0111] (Waveform separation of fluorescence spectrum)
[0112] For the fluorescence spectrum of the measured single-crystal spherical carbon nanoparticles, waveform separation was performed to calculate the relative fluorescence quantum efficiency relative to the fluorescence quantum efficiency of 9,10-diphenylanthracene, and the area % of the fluorescence spectrum showing a peak at 430 nm was calculated. The waveform separation was performed using the waveform separation software built into the FT / IR-6600 used for IR absorption spectrum measurement.
[0113] (Relative fluorescence quantum efficiency)
[0114] The fluorescence quantum efficiency in a fluorescent substance can be evaluated by the efficiency of the fluorescence generated by the excitation light. In the present invention, the fluorescence quantum efficiency of the single-crystal spherical carbon nanoparticles is calculated as a relative value, that is, the fluorescence quantum efficiency, by setting the fluorescence quantum efficiency of 9,10-diphenylanthracene as a standard substance to 1.0. 9,10-diphenylanthracene has a fluorescence quantum efficiency of 1.0 at a fluorescence peak wavelength of 430 nm. The relative fluorescence quantum efficiency is calculated using the following formula (1).
[0115] Φ x =Φ s (F x / F s (A s / A x ) (I s / I x ) (n x 2 / n s 2 ) · · · (1)
[0116] [Wherein, x means single crystal spherical carbon nanoparticles. s means 9,10-diphenylanthracene. Φ x is the relative fluorescence quantum efficiency of single-crystal spherical carbon nanoparticles. s is the quantum efficiency of 9,10-diphenylanthracene. F is the area of the fluorescence spectrum. A is the absorbance at the excitation wavelength. I is the intensity of the excitation light. n is the refractive index of the solvent used.]
[0117] In the present invention, in 9,10-diphenylanthracene and single-crystal spherical carbon nanoparticles as standard substances, the bandpass width of the excitation light, the bandpass width of the fluorescence, the scanning speed, the data introduction interval, and the measurement sensitivity as the measurement conditions of the spectrofluorophotometer for measuring fluorescence are all kept constant, and THF is used as the same solvent, so that (I) in formula (1) s / I x )(n x 2 / n s 2) is 1.0. Therefore, it was calculated from the area of each fluorescence spectrum in the THF dispersion of single-crystal spherical carbon nanoparticles and the THF solution of 9,10-diphenylanthracene and the value of absorbance during measurement.
[0118] (UV-visible absorption spectrometry)
[0119] The UV-vis (ultraviolet-visible) absorption spectrum of single-crystalline spherical carbon nanoparticles was measured using a UV-visible near-infrared spectrophotometer (product name: V-770, manufactured by JASCO Corporation). The measurement range was 200nm to 900nm, the sampling rate was 0.2nm, and the measurement speed was set to a low speed for measurement. In the measurement, a quartz cell with a thickness of 10mm was used for liquid. In order to calculate the relative fluorescence quantum efficiency of single-crystalline spherical carbon nanoparticles, the measurement was diluted with THF in such a way that the absorbance at a wavelength of 300nm to 400nm became less than 0.05. The absorbance of the THF solution of 9,10-diphenylanthracene was measured under the same measurement conditions.
[0120] (Circularity)
[0121] As an index for evaluating the sphericity of single-crystalline spherical carbon nanoparticles, the circularity is calculated as described below. As for the circularity of single-crystalline spherical carbon nanoparticles, the image obtained by TEM observation is approximated as an ellipse using TEM image software iTEM (manufactured by OlympusSoft Imaging Solutions GmbH). Next, the major diameter (D), circumference (Z) and area (S) of the ellipse as the projected image of the single-crystalline spherical carbon nanoparticle are obtained from the analysis results of the TEM image analysis software. Using the values of the circumference (Z) and area (S), 4πS / Z is calculated. 2 , which is defined as the circularity. The closer the circularity value is to 1, the closer the particle is to a sphere. When the particle shape is a perfect sphere, the circularity is 1 at the maximum.
[0122] In addition, the average value of the major diameter (D) of the ellipse was determined and defined as the average particle diameter. The measurement was calculated for 50 independent single-crystal spherical silicon nanoparticles.
[0123] (X-ray diffraction: XRD)
[0124] In the X-ray diffraction (XRD) measurement, a powder X-ray diffraction measuring apparatus EMPYREAN (manufactured by MaruVan Pannatical Division of Spectoris Co., Ltd.) was used. The measurement conditions were: measurement range: 10 to 100 [°2θ], Cu counter cathode, tube voltage 45 kV, tube current 40 mA, scanning speed 0.013° / min.
[0125] (Raman scattering spectroscopy)
[0126] The Raman scattering spectrum of the single-crystal spherical carbon nanoparticles was measured using a PR-1w pad top Raman spectrophotometer manufactured by JASCO Corporation. The wavelength of the excitation laser was 785 nm, the output power of the laser was 5 mW, and the 3 cm -1 / pixel, measured at a wave number of 200 cm -1 ~3000cm -1 .
[0127] Example 1
[0128] In Example 1, a THF solution of carbon tetrachloride (CCl4) as a raw material (single-crystalline spherical carbon nanoparticle raw material solution) was reduced using a THF solution of metallic lithium dissolved in naphthalene (single-crystalline spherical carbon nanoparticle reduction solution) to produce single-crystalline spherical carbon nanoparticles.
[0129] Table 1 shows the formulations of Examples 1-1 to 1-4.
[0130] [Table 1]
[0131]
[0132] The solvent used in Example 1 is ultra-dehydrated tetrahydrofuran (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) having a residual moisture content of less than 10 ppm. In a glove box with an argon atmosphere, a single-crystalline spherical carbon nanoparticle reduction solution (liquid A) and a single-crystalline spherical carbon nanoparticle raw material solution (liquid B) were prepared. Specifically, for the single-crystalline spherical carbon nanoparticle reduction solution of liquid A, metallic lithium was dissolved in a THF solution in which naphthalene was dissolved in a manner of 0.4 mol / L at a liquid adjustment temperature of -5°C using a glass-coated magnetic stirrer to obtain a prepared solution in a concentration of 0.4 mol / L. Similarly, carbon tetrachloride, which is a raw material for single-crystalline spherical carbon nanoparticles of liquid B, was dissolved in THF and stirred for at least 60 minutes using a glass-coated magnetic stirrer. For the substances represented by the chemical formulas and abbreviations recorded in Table 1, CCl4 is carbon tetrachloride (manufactured by Kanto Chemical Co., Ltd.), Li is metallic lithium (manufactured by Kishida Chemical Co., Ltd.), and C 10 H8 is naphthalene (produced by Kanto Chemical Co., Ltd.).
[0133] The generation of naphthalene anions in liquid A was confirmed by IR absorption spectroscopy.
[0134] Figure 1 c shows the result of subtracting the IR absorption spectrum of THF from the IR absorption spectrum of a THF solution in which only naphthalene was dissolved. Figure 1 b shows the result of subtracting the IR absorption spectrum of THF as a solvent from the IR absorption spectrum of a naphthalene THF solution in which metallic lithium was dissolved. Figure 1 a to make Figure 1 c1508cm -1 The intensity of the IR absorption spectrum is related to Figure 1 b's 1508cm -1 The absorbance is consistent with the Figure 1 The intensity correction of the IR absorption spectrum of c is Figure 1 The IR absorption spectrum of b is subtracted Figure 1 The results were obtained by measuring the IR absorption spectrum of c. Figure 1 1488cm confirmed in a -1 and 1183cm -1 The peak of indicates that the electrons generated by the dissolution of metallic lithium move to the LUMO of naphthalene to generate naphthalene anions.
[0135] The particle size distribution of the produced single-crystal spherical carbon particles changes due to the change in the reducing power of liquid A. Therefore, it is preferable to confirm the reducing power. In particular, 1183 cm -1 The absorption peak is steep and can be measured as a single peak. The reducing power can be clearly judged by the decrease in the intensity of the absorption peak. If the reducing power decreases, it can be confirmed that the intensity of the absorption peak decreases significantly.
[0136] When biphenyl or anthracene is used as a fused aromatic compound, the -1 and 1175cm -1 Anions of biphenyl or anthracene were confirmed in liquid A. The reduction in the reducing power of these condensed aromatic compounds was also determined from the intensity of their respective absorption peaks.
[0137] Next, the prepared single-crystal spherical carbon nanoparticle reduction solution (liquid A) and the single-crystal spherical carbon nanoparticle raw material solution (liquid B) are mixed using the fluid processing device described in patent document 6 of the applicant of the present application. The fluid processing device described in patent document 6 is the fluid processing device of the patent document 6. Figure 1 The device described in (A) uses a concentric ring-shaped device in which the opening d2 of the second introduction part is formed into a ring-shaped disk, that is, a concentric ring-shaped device surrounding the central opening of the processing surface 2. Specifically, while the single-crystal spherical carbon nanoparticle reduction liquid or the single-crystal spherical carbon nanoparticle raw material liquid as the A liquid is introduced from the first introduction part d1 into the processing surface 1 and 2, the processing part 10 is operated at a speed of 500rpm to 5000rpm, while the single-crystal spherical carbon nanoparticle raw material liquid or the single-crystal spherical carbon nanoparticle reduction liquid as the B liquid is introduced from the second introduction part d2 into the processing surface 1 and 2, the single-crystal spherical carbon nanoparticle raw material liquid and the single-crystal spherical carbon nanoparticle reduction liquid are mixed in the thin film fluid, and the single-crystal spherical carbon nanoparticles are precipitated between the processing surfaces 1 and 2. The discharge liquid containing the single-crystal spherical carbon nanoparticles is discharged from the processing surface 1 and 2 of the fluid treatment device. The discharged single-crystal spherical carbon nanoparticle dispersion was recovered in a beaker via a container.
[0138] Table 2 shows the operating conditions of the fluid processing device of Example 1. The introduction temperature (liquid delivery temperature) and introduction pressure (liquid delivery pressure) of liquid A and liquid B shown in Table 2 are measured using a thermometer and a pressure gauge provided in the sealed introduction path (first introduction part d1 and second introduction part d2) passing through the processing surfaces 1 and 2. The introduction temperature of liquid A shown in Table 2 is the actual temperature of liquid A under the introduction pressure in the first introduction part d1, and similarly, the introduction temperature of liquid B is the actual temperature of liquid B under the introduction pressure in the second introduction part d2.
[0139] [Table 2]
[0140]
[0141] A wet cake sample was prepared from a single-crystal spherical carbon nanoparticle dispersion discharged from a fluid handling device and recovered in a beaker. As a preparation method, the discharged single-crystal spherical carbon nanoparticle dispersion was recovered according to a conventional method, and the single-crystal spherical carbon nanoparticles were centrifuged (30190G, 2 hours) and precipitated from the recovered liquid to separate the supernatant. Then, ultrasonic cleaning and sedimentation in THF were repeated, and the single-crystal spherical carbon nanoparticles finally obtained were dried at -0.10MPaG and 25°C for 20 hours to prepare a dry powder.
[0142] Figure 2 The TEM observation image of the single-crystal spherical carbon nanoparticles of Example 1-1 is shown. The same result was confirmed for the single-crystal spherical carbon nanoparticles of Examples 1-2 to 1-4. Since lattice fringes were observed in one direction, it was confirmed that they were single crystals.
[0143] (CH bond)
[0144] Figure 3 The IR spectrum measurement results of the single-crystal spherical carbon nanoparticles of Example 1-2 are shown for the wave number 2700 cm -1 ~3050cm -1 The results of the regional measurement. 2855cm -1 The absorption and 2920cm -1 The absorption peak of is attributed to the stretching vibration of the CH bond, and thus it was confirmed that the single-crystal spherical carbon nanoparticles were hydrogenated. The same was confirmed for Examples 1-1, 1-3, and 1-4.
[0145] Figure 4 The IR spectrum measurement results of the single-crystal spherical carbon nanoparticles of Example 1-2 are shown for the wave number 900 cm -1 ~1900cm -1The results of waveform separation were performed after the area measurement. The peak wave number of each band after waveform separation is shown, and the relative area ratio is shown in parentheses. The waveform separation was performed using the waveform separation software built into the FT / IR-6600.
[0146] (CO key)
[0147] Figure 4 The IR spectrum is separated by waveform and divided into 10 equal parts, 1000cm -1 ~1100cm -1 The absorption in the wave number region is attributed to the CO bond. The ratio of the total area of the band 9 and the band 10 separated by the waveform in this wave number region (the ratio of the CO bond) is 10.7%. The CO bond ratio is preferably 2% or more and 15% or less. This is because if it is less than 2%, it becomes difficult to disperse the single-crystalline spherical carbon nanoparticles in the aqueous solution. In addition, if it exceeds 15%, the circularity of the single-crystalline spherical carbon nanoparticles becomes less than 0.9, and the difference from the sphere increases, which has the disadvantage of causing a decrease in the relative fluorescence quantum efficiency.
[0148] With regard to the CO bond of the single crystal spherical carbon nanoparticle, when the single crystal spherical carbon nanoparticle is manufactured in the super dehydrated THF of the grade specified by the reduction reaction in tetrahydrofuran (THF) with residual moisture of less than 10ppm, it is often possible to adopt the moisture managed to be less than 10ppm and generate. Since the graphene layer is easy to react just after the reduction reaction, the stable oxidation reaction produced by a certain amount of moisture can be utilized to protect the single crystal spherical carbon nanoparticle. By protecting the surface of the single crystal spherical carbon nanoparticle in this way, the fluctuation caused by oxidation during the cleaning and recovery operation can be suppressed. The cleaning and recovery needs to be basically temporarily dissolved with THF solvent by residual organic matter, and then cleaned with pure water, and some oxidation reactions are carried out during the cleaning and recovery operation.
[0149] (CN key)
[0150] CN bonds are generated by reacting with the outermost surface of the graphene layer that is not protected by oxygen when the single-crystalline spherical carbon nanoparticles are exposed to the air atmosphere during the cleaning and recovery process. Since no raw materials or solvents containing nitrogen are used in the reduction reaction of the single-crystalline spherical carbon nanoparticles, CN bonds are generated after the reaction of the single-crystalline spherical carbon nanoparticles. Therefore, the fluorescence characteristics of the single-crystalline spherical carbon nanoparticles of nitrogen are not greatly affected, but the termination of defects caused by nitrogen is also possible. Figure 4 In the IR spectrum, the CN bond is at 1300 cm -1 ~1400cm -1 The wave number region has absorption, which is equivalent to the peak wave number 1357cm -1Band 7 has a relative area ratio (ratio of CN bonds) of 6.2%. Both CN bonds and CO bonds have the effect of terminating defects that cut off the bonding of carbon atoms in the graphene layer, so the ratio of CN bonds is preferably less than 10%. As for the CN bonds, when the CO bonds terminate the carbon atom bonding defects, they are not detected.
[0151] Figure 3 The CH bonds of the single-crystal spherical carbon nanoparticles confirmed in the present invention can make the surface of the single-crystal spherical carbon nanoparticles hydrophobic, so the single-crystal spherical carbon nanoparticles can be well dispersed in organic solvents. Figure 4 As a result, it was confirmed that dispersibility in aqueous solvents was possible due to the coexistence of CO bonds.
[0152] Figure 5 The fluorescence spectra of the single crystal spherical carbon nanoparticles of Example 1-3 are shown. The fluorescence spectra are normalized by setting the maximum intensity of the fluorescence spectra obtained at each excitation wavelength to 1.0, and are the results of changing the excitation wavelength by 20 nm in the range of 320 nm to 580 nm. Figure 4 The results confirmed that the fluorescence of the single-crystal spherical carbon nanoparticles of Example 1-3 showed a maximum peak at 400 nm to 600 nm depending on the excitation wavelength.
[0153] Figure 6 Based on Figure 5 The graph showing the relationship between the excitation wavelength and the fluorescence peak wavelength is prepared based on the results. The graph shows the excitation wavelength dependence of the fluorescence peak wavelength of the single-crystalline spherical carbon nanoparticles of Examples 1-3. It is known that if the particle size of the single-crystalline spherical carbon nanoparticles increases, the fluorescence peak wavelength shifts to the long wavelength side, so it is judged that the fluorescence from the nanoparticles with a slightly increased particle size of the single-crystalline spherical carbon nanoparticles is obtained.
[0154] The change in the fluorescence peak wavelength in the single-crystalline spherical carbon particles is explained in the (A) quantum effect among the three mechanisms (A) to (C) above. That is, it is believed that with respect to the fluorescence peak wavelength of the single-crystalline spherical carbon nanoparticles, since the band gap increases as the particle size of the single-crystalline spherical carbon nanoparticles decreases, the fluorescence peak wavelength shifts to the short wavelength side, which is a result of the mechanism based on the (A) quantum effect. In addition, it is believed that the single-crystalline spherical carbon nanoparticles of the present invention have not been surface-modified with alkyl groups, amino groups, etc., and the (B) surface modification mechanism among the three mechanisms mentioned above does not exist, so the fluorescence is generated by the synergistic effect of the (C) mechanism based on oxygen bonding to the single-crystalline spherical carbon particles and the (A) quantum effect mechanism.
[0155] Figure 7 The Raman scattering spectra of the single-crystal spherical carbon nanoparticles of Examples 1-3 are shown.
[0156] For comparison, the Raman scattering spectrum of graphite crucible particles crushed in a mortar is shown. The Raman scattering spectrum of graphite is only at 1650 cm -1 Up to 1550cm -1 The wave number region is shown as I G The peak of the band is at 1300 cm-1 when the bonding of graphene layers is disordered and defects are generated in graphite. -1 Up to 1450cm -1 Appearance is called I D The peak of the band can also be used to calculate the spectral intensity ratio of the two, that is, I D / I G The defects of carbon materials are estimated based on the value of Figure 6 To convert the I of each carbon particle G Set the band strength to 100 and I D The results of the relative comparison of the intensity of the bands confirmed that the single-crystal spherical carbon particles prepared in Examples 1-3 D / I G The ratio is 0.23, and there are fewer bond defects.
[0157] Figure 8 The XRD patterns of single crystal spherical carbon particles of Examples 1-1, 1-2, and 1-4 are shown. The graphite crystals are composed of sp 2 The C=C bonds formed by the carbon atoms of the hybrid orbital form a structure in which the graphene layers of the planar layers are stacked in the c-axis direction. As a crystal system, in the hexagonal graphite, as a space lattice, a simple lattice and a rhombohedral lattice can be formed. The peaks with diffraction angles 2θ of 42.2° and 44.6° appear through the simple lattice of the hexagonal structure, and the peak with 2θ of 43.3° appears through the rhombohedral lattice. This result is in the single-crystal spherical carbon nanoparticles with a hexagonal structure. When the space lattice is a simple lattice, if the two-layer graphene layer is set as the A layer and the B layer, it means that it becomes a stacked structure such as ABABAB... In the rhombohedral lattice, if the three-layer graphene layer is set as the A layer, the B layer, and the C layer, it means that they become a stacked structure such as ABCABCABC... As for the average lattice plane spacing, the arithmetic mean of the sum of the two values of the lattice plane spacing calculated using the Bragg formula divided by 2 was calculated from the diffraction peak angles confirmed near the diffraction angles 2θ=44.6° and 2θ=43.3°. After measuring 10 samples, the value of the sum of these values divided by 10 was calculated as the average lattice plane spacing.
[0158] Table 3 shows the average particle size, average circularity, crystal structure, average lattice plane spacing of graphene layers, CO bond ratio obtained by IR spectrum, I obtained by Raman scattering spectrum, and the average particle size, average circularity, crystal structure, average lattice plane spacing of graphene layers, and the average particle size, average circularity, crystal structure, average lattice plane spacing of graphene layers, average lattice plane spacing ... D / IG ratio and relative fluorescence quantum efficiency.
[0159] [Table 3]
[0160]
[0161] Comparative Example 1
[0162] The formulation of Comparative Example 1 is the same as that of Example 1 shown in Table 1. As shown in Table 4, the disk rotation speed was reduced to 600 rpm and 500 rpm to produce single-crystal spherical carbon nanoparticles. Table 5 shows the results of the obtained single-crystal spherical carbon particles. By reducing the disk rotation speed to less than 700 rpm, no change was found in the crystal structure, but the average circularity became less than 0.9, I D / I G The ratio increases to 1.0, and the defects increase compared to Example 1, so that the relative fluorescence quantum efficiency becomes a low value of 5% or less.
[0163] [Table 4]
[0164]
[0165] [Table 5]
[0166]
[0167] Example 2
[0168] In Example 2, the single-crystalline spherical carbon nanoparticle reducing solution was set to -10°C and 10°C, which are lower than 0°C, and the results of single-crystalline spherical carbon nanoparticles produced when the disk rotation number was 5000rpm and 3500rpm are shown. The single-crystalline spherical carbon nanoparticle reducing solution and the single-crystalline spherical carbon nanoparticle raw material solution have the same composition as in Example 1 and are produced under the conditions shown in Table 1. Table 6 shows the production conditions of Example 2, and the results of the obtained single-crystalline spherical carbon nanoparticles are shown in Table 7. In the single-crystalline spherical carbon nanoparticles produced in Example 2, the lower the temperature of the liquid A single-crystalline spherical carbon nanoparticle reducing solution, the smaller the average particle size becomes, and the relative fluorescence quantum efficiency becomes more than 10%.
[0169] [Table 6]
[0170]
[0171] [Table 7]
[0172]
[0173] Comparative Example 2
[0174] The formula of Comparative Example 2 is the same as that of Example 1 shown in Table 1. As shown in Table 8, the number of rotations of the disk is reduced to 700 rpm, and the temperature of the liquid A single-crystal spherical carbon nanoparticle reducing liquid is set to -10°C and 10°C to produce single-crystal spherical carbon particles. Table 9 shows the results of the produced single-crystal spherical carbon nanoparticles. The average circularity of the single-crystal spherical carbon nanoparticles produced by reducing the number of rotations of the disk to 700 rpm and setting the temperature of the liquid A to below 10°C is less than 0.9, and the I representing the existence ratio of defects calculated by Raman scattering spectrum is 0. D / I G The ratio is as high as 1.0 or more, and the relative fluorescence quantum efficiency becomes a low value of 5% or less.
[0175] [Table 8]
[0176]
[0177] [Table 9]
[0178]
[0179] In Example 3, the formula of liquid A and liquid B is the same as Table 1, and the flow ratio of liquid B single crystal spherical carbon nanoparticle raw material liquid and liquid A single crystal spherical carbon nanoparticle reducing liquid is changed to produce single crystal spherical carbon nanoparticles. Table 10 shows the manufacturing conditions of single crystal spherical carbon nanoparticles. Table 11 shows the results of the obtained single crystal spherical carbon nanoparticles.
[0180] [Table 10]
[0181]
[0182] [Table 11]
[0183]
[0184] Fig. 9 The XRD pattern of the single crystal spherical carbon nanoparticles obtained in Example 3 is shown. In Example 3-1, a diffraction peak with a diffraction angle 2θ of 43.25° based on the space lattice of hexagonal crystal and rhombohedron and a diffraction peak with a diffraction angle of 44.6° based on the hexagonal crystal and simple lattice were found. In Example 3-2 and Example 3-3, a diffraction peak with a diffraction angle 2θ of 43.25° based on the space lattice of rhombohedral lattice was found, and the result was almost judged to be a rhombohedral lattice. In Example 3-3, a peak was also found at 43.5°, which was judged to be based on a rhombohedral lattice.
[0185] Fig.10 The fluorescence spectrum of the single-crystal spherical carbon nanoparticles produced in Example 3-3 is shown. The fluorescence peak wavelength measured with an excitation wavelength of 240 nm to 360 nm was 420 nm, and the result showed no excitation wavelength dependency. Figure 4 The fluorescence peak wavelength of Examples 1-3 shown in the figure shows the dependence on the excitation light, and the result is that as the excitation wavelength becomes longer, the fluorescence peak wavelength also shifts to the longer wavelength side. In this case, the structure of the single crystal spherical carbon nanoparticles is as follows: Figure 7 In Example 3-3, only the result of rhombohedral lattice was obtained, and it is considered that the difference in the excitation light dependence of the fluorescence peak wavelength is based on the difference in the spatial lattice of the single crystal spherical carbon particles.
[0186] In the manufacture of single-crystal spherical carbon nanoparticles, the flow rate of liquid A single-crystal spherical carbon nanoparticle reducing solution is greater than the flow rate of liquid B single-crystal spherical carbon nanoparticle raw material solution. The results show that by increasing the reduction reaction rate, a large number of tiny graphene layers are manufactured, and these fine graphene layers are stacked on each other in the c-axis direction, so that smaller single-crystal spherical carbon nanoparticles can be manufactured. In this way, the flow rate of liquid A single-crystal spherical carbon nanoparticle reducing solution is greater than the flow rate of liquid B single-crystal spherical carbon nanoparticle raw material solution, so that the symmetry of the fluorescence spectrum can be improved, and the fluorescence spectrum can be obtained. The full width at half maximum of the fluorescence spectrum is 70nm, and the color purity is high.
[0187] Industrial Applicability
[0188] By adopting the manufacturing method of the present invention, single-crystal, spherical single-crystal carbon nanoparticles can be manufactured. Since the manufactured single-crystal spherical carbon nanoparticles are single crystals without grain boundaries that reduce the fluorescence efficiency, fluorescence can be generated with high fluorescence quantum efficiency by using excitation of light with a wide wavelength from ultraviolet light to visible light, which can increase the fluorescence quantum efficiency of carbon nanoparticles known so far by more than 10%. In addition, the single-crystal spherical carbon nanoparticles of the present invention do not have the toxicity to organisms that compound semiconductors formed by cadmium, selenium, tellurium, etc. have, so they can be used in drug delivery. Furthermore, the single-crystal spherical carbon nanoparticles manufactured by the manufacturing method of the present invention are spherical, so they can be filled with high-density electrode materials for solar cells and secondary ion batteries, and can be used as negative electrodes of lithium ion batteries and electrode materials for solar cells.
Claims
1. A manufacturing method, which is a manufacturing method for single-crystal, spherical single-crystal spherical carbon nanoparticles, comprising the steps of mixing and reacting a raw material liquid containing a halogenated carbon with a reducing liquid containing anions of the condensed aromatic compound generated from lithium, sodium or potassium and a condensed aromatic compound, wherein the anions of the condensed aromatic compound are obtained by mixing lithium, sodium or potassium with the condensed aromatic compound at a temperature below 0°C.
2. The manufacturing method according to claim 1, in, The perimeter (Z) and area (S) of the projected image of the single-crystal spherical carbon nanoparticle observed by transmission electron microscopy were used, and the mathematical formula: 4πS / Z was used. 2 The calculated average value of the circularity was 0.9 or more.
3. The manufacturing method according to claim 1 or 2, in, The average particle size is 1nm~30nm.
4. The production method according to any one of claims 1 to 3, in, The raw material solution and the reducing solution are mixed and reacted using the following device: The device comprises: a fluid pressure imparting mechanism for imparting pressure to a processed fluid; at least two processing parts, a first processing part and a second processing part that can be relatively approached and / or separated from the first processing part; and a rotation driving mechanism for relatively rotating the first processing part and the second processing part. At least two processing surfaces, a first processing surface and a second processing surface, are provided at positions facing each other in each processing portion, each processing surface constituting a part of a sealed flow path through which the processed fluid under pressure flows, and two or more processed fluids containing at least one of the reactants are mixed between the two processing surfaces and reacted. In the first processing part and the second processing part, at least the second processing part has a pressure-bearing surface, and at least a part of the pressure-bearing surface is composed of the second processing surface. The pressure-bearing surface is subjected to the pressure applied to the processed fluid by the fluid pressure imparting mechanism, generating a force to move the second processing surface in the direction of separation from the first processing surface. By allowing the processed fluid under pressure to pass between the first processing surface and the second processing surface that are accessible and / or separable and relatively rotatable, the processed fluid forms a thin film fluid, and further has another inlet path independent of the flow path between the processing surfaces through which the processed fluid under pressure flows. At least one opening connected to the other inlet path is provided in at least any one of the first processing surface and the second processing surface, and at least one processed fluid transported from the other inlet path is introduced into the space between the two processing surfaces, and the reactant contained in at least any one of the processed fluids and the processed fluid different from the processed fluid are mixed in the thin film fluid.
5. The manufacturing method according to claim 4, in, The opening is provided on the downstream side of a point where the flow of the fluid to be processed passing between the two processing surfaces becomes a laminar flow.
6. The production method according to any one of claims 1 to 5, in, The molar ratio of the lithium, sodium or potassium to the carbon halide is 7:1 to 4:
1.
7. The production method according to any one of claims 1 to 6, in, The condensed aromatic compound is at least one selected from the group consisting of biphenyl, naphthalene, 1,2-dihydronaphthalene, anthracene, phenanthrene and pyrene.
8. The manufacturing method according to claim 7, in, When the condensed aromatic compound is biphenyl, naphthalene or anthracene, in the IR absorption spectrum of the reducing solution, at 1200 cm -1 ~1100cm -1 The absorption peak is shown in the wavenumber range of .
9. The production method according to any one of claims 1 to 8, in, The solvent contained in the reducing liquid is tetrahydrofuran and / or dimethoxyethane having a residual water content of 10 ppm or less.
10. The production method according to any one of claims 1 to 9, in, The solvent contained in the reducing liquid is tetrahydrofuran containing a phenolic polymerization inhibitor, a residual water content of 10 ppm or less, and a residual oxygen concentration of less than 0.1 ppm.
11. The production method according to any one of claims 1 to 10, in, The solvent contained in the raw material liquid is tetrahydrofuran having a residual water content of 10 ppm or less and a residual oxygen concentration of less than 0.1 ppm.
12. The production method according to any one of claims 1 to 11, in, The carbon halide is carbon tetrachloride, carbon tetrabromide or carbon tetraiodide.
13. The production method according to any one of claims 1 to 12, in, The single crystal spherical carbon nanoparticles are hexagonal crystals, and the space lattice is composed of a simple lattice, a rhombohedral lattice, or a simple lattice and a rhombohedral lattice.
14. The production method according to any one of claims 1 to 13, in, The single-crystal spherical carbon nanoparticles have a peak at 2800 cm-1 in the IR absorption spectrum. -1 ~2950cm -1 The absorption peak is shown in the wave number range of 900cm -1 ~1900cm -1 The 1000cm -1 ~1100cm -1 The absorption peak area relative to 900 cm -1 ~1900cm -1 The total area of the wavenumber range is less than 15%.
15. The production method according to any one of claims 1 to 14, in, The single-crystal spherical carbon nanoparticles have a wavelength of 900 cm-1 in the IR absorption spectrum. -1 ~1900cm -1 The 1300 cm -1 ~1400cm -1 The absorption peak area relative to 900 cm -1 ~1900cm -1 The total area of the wavenumber range is less than 10%.
16. The production method according to any one of claims 1 to 15, in, The single-crystal spherical carbon nanoparticles have a Raman scattering spectrum of 1550 cm -1 ~1650cm -1 The intensity of the peak is set as I G , 1250cm -1 ~1350cm -1 The intensity of the peak is set as I D When D / I G The ratio is less than 1.
0.
17. The production method according to any one of claims 1 to 16, in, The single crystal spherical carbon nanoparticles generate a fluorescence maximum in the wavelength range of 400nm to 600nm in the fluorescence spectrum.