Grinding fluid, grinding fluid set and grinding method

A cerium oxide-based polishing liquid with ether compounds and a controlled pH stabilizes the polishing speed of silicon oxide, addressing excessive polishing issues and ensuring precise surface finishing.

CN119095930APending Publication Date: 2024-12-06RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035940.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-09
Filing Date
2023-08-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing CMP polishing liquids for silicon oxide often result in excessive polishing speeds, leading to over-polishing and surface irregularities, necessitating a solution to control and reduce the polishing rate.

Method used

A polishing liquid comprising cerium oxide abrasive grains and an ether compound with carboxyl or carboxylate groups, along with a specific pH range, is formulated to stabilize and reduce the polishing speed of silicon oxide.

Benefits of technology

The polishing liquid effectively reduces the polishing speed of silicon oxide to 400 nm/min or less, while maintaining selective polishing of silicon nitride, achieving a controlled polishing rate ratio.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005098520590000182
    Figure BDA0005098520590000182
Patent Text Reader

Abstract

This polishing liquid contains abrasive grains, an ether compound having at least one type selected from the group consisting of a carboxyl group and a carboxylate group, and water. A polishing liquid set in which the constituent components of the polishing liquid are stored in a manner divided into a first liquid and a second liquid, the first liquid containing abrasive grains and water, and the second liquid containing water and an ether compound having at least one type selected from the group consisting of a carboxyl group and a carboxylate group. Also provided is a polishing method including a step for polishing a surface to be polished, which contains silicon oxide, using the polishing liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a grinding liquid, a grinding liquid set, a grinding method and the like. Background Art

[0002] In recent years, the importance of processing technology for high density and miniaturization has been increasing in the manufacturing process of semiconductor elements. CMP (Chemical mechanical polishing) technology, which is one of the processing technologies, has become a technology required for the formation of shallow trench isolation (STI), planarization of pre-metal insulating materials or interlayer insulating materials, and formation of plugs or buried metal wiring in the manufacturing process of semiconductor elements. As a CMP polishing liquid, a CMP polishing liquid containing abrasive particles containing cerium oxide is known (for example, refer to the following patent documents 1 and 2).

[0003] Previous technical literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 10-106994

[0006] Patent Document 2: Japanese Patent Application Laid-Open No. 08-022970 Summary of the invention

[0007] Technical issues to be solved by the invention

[0008] Sometimes, it is required to polish a component (insulating component) containing silicon oxide using a CMP polishing liquid containing abrasive grains to make the polished surface smooth. Sometimes, it is required to reduce the polishing speed of silicon oxide in order to prevent over-polishing of the component containing silicon oxide during the polishing process.

[0009] One object of the present invention is to provide a polishing liquid and a polishing liquid set capable of reducing the polishing speed of silicon oxide. Another object of the present invention is to provide a polishing method using such a polishing liquid or a polishing liquid set.

[0010] Means for solving technical problems

[0011] The present invention, in several aspects, relates to the following [1] to

[10] and the like.

[0012] [1] A polishing liquid comprising abrasive grains, an ether compound having at least one selected from the group consisting of a carboxyl group and a carboxylate group, and water.

[0013] [2] The polishing liquid according to [1], wherein

[0014] The abrasive grains contain cerium oxide.

[0015] [3] The polishing liquid according to [1] or [2], wherein

[0016] The ether compound includes a compound represented by the following general formula (1).

[0017] R 1 -OR 2 -COOR 3 -----(1)

[0018] [In formula (1), R 1 represents an alkyl group having 1 to 10 carbon atoms, R 2 represents an alkylene group having 1 to 10 carbon atoms, R 3 represents a hydrogen atom or a monovalent metal atom.]

[0019] [4] The polishing liquid according to any one of [1] to [3], wherein

[0020] The ether compound includes at least one selected from the group consisting of ethoxyacetic acid, methoxyacetic acid, and salts thereof.

[0021] [5] The polishing liquid according to any one of [1] to [4], wherein

[0022] The content of the ether compound is less than 0.10 mass % based on the total mass of the polishing liquid.

[0023] [6] The polishing liquid according to any one of [1] to [5], wherein the pH thereof is 2.0 to 5.0.

[0024] [7] The polishing liquid according to any one of [1] to [6], which is used for polishing a polished surface containing silicon oxide.

[0025] [8] A polishing liquid set, wherein:

[0026] The polishing liquid according to any one of [1] to [7] is stored as a first liquid containing the abrasive and water and a second liquid containing the ether compound and water.

[0027] [9] A polishing method comprising the step of polishing a polishing surface comprising silicon oxide using the polishing liquid according to any one of [1] to [7].

[0028]

[10] A polishing method comprising the step of polishing a surface to be polished including silicon oxide using a polishing liquid obtained by mixing the first liquid and the second liquid of the polishing liquid set described in [8].

[0029] Effects of the Invention

[0030] According to one aspect of the present invention, a polishing liquid and a polishing liquid set capable of reducing the polishing speed of silicon oxide can be provided. Furthermore, according to another aspect of the present invention, a polishing method using such a polishing liquid can be provided. DETAILED DESCRIPTION

[0031] Hereinafter, embodiments of the present invention will be described.

[0032] In this specification, the numerical range represented by "~" is used to represent the range including the numerical values ​​recorded before and after "~" as the minimum and maximum values, respectively. "Above A" in the numerical range represents A and the range exceeding A. "Below A" in the numerical range represents A and the range less than A. In the numerical range described in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range of other stages. In the numerical range described in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment. "A or B" can include either A and B, or both. The materials exemplified in this specification can be used alone or in combination of two or more, unless otherwise specified. In the case where there are multiple substances equivalent to each component in the composition, the content of each component in the composition represents the total amount of the multiple substances present in the composition unless otherwise specified. The term "process" does not only include independent processes, but also includes processes that cannot be clearly distinguished from other processes as long as the intended effect of the process can be achieved.

[0033] The polishing liquid according to the present embodiment contains abrasive grains, an ether compound having at least one selected from the group consisting of a carboxyl group and a carboxylate group, and water. The polishing liquid according to the present embodiment can be used as a CMP polishing liquid, for example.

[0034] According to the polishing liquid involved in this embodiment, the polishing speed of silicon oxide can be reduced, for example, the polishing speed of silicon oxide can be set to 400nm / min or less. The polishing speed of silicon oxide can be 300nm / min or less, 200nm / min or less, 100nm / min or less, 80nm / min or less, 50nm / min or less, or 40nm / min or less.

[0035] According to the polishing liquid involved in this embodiment, the polishing speed of silicon nitride can be reduced, for example, the polishing speed of silicon nitride can be set to 70nm / min or less. The polishing speed of silicon nitride can be 50nm / min or less, 30nm / min or less, 20nm / min or less, 10nm / min or less, or 5nm / min or less.

[0036] According to the polishing liquid involved in this embodiment, silicon oxide can be selectively polished relative to silicon nitride. The polishing rate ratio of silicon oxide to silicon nitride can be 8 or more, 10 or more, 12 or more, 15 or more, 30 or more, 50 or more, or 100 or more. The polishing rate ratio of silicon oxide to silicon nitride can be 200 or less, 150 or less, 100 or less, 75 or less, 50 or less, or 30 or less.

[0037] (Abrasive particles)

[0038] The polishing liquid involved in this embodiment contains abrasive grains. In this specification, "abrasive grains" means a collection of multiple particles, but for convenience, one particle constituting the abrasive grains is sometimes referred to as an abrasive grain. The abrasive grains may contain one or more particles. As constituent materials of the abrasive grains, inorganic substances such as cerium oxide (cerium oxide), cerium hydroxide, silicon dioxide, aluminum oxide, zirconium oxide, titanium dioxide, germanium oxide, silicon carbide, etc.; organic substances such as polystyrene, polyacrylic acid, polyvinyl chloride, etc. can be cited. The abrasive grains may contain cerium compounds, may contain at least one selected from the group consisting of cerium oxide and cerium hydroxide, and may contain cerium oxide.

[0039] From the viewpoint of stabilizing the polishing rate of silicon oxide, the content of the cerium compound in the abrasive (the total content of the cerium oxide and the cerium hydroxide when the abrasive contains at least one of cerium oxide and cerium hydroxide) can be more than 95 mass%, 98 mass%, 99 mass%, 99.5 mass%, or 99.9 mass% or more based on the entire abrasive (the entire abrasive contained in the polishing liquid, or the entire one particle constituting the abrasive). The abrasive can be in a form substantially composed of the cerium compound (a form in which substantially 100 mass% of the abrasive is the cerium compound). From the same viewpoint, the content of the cerium oxide in the abrasive can be in the same numerical range as the numerical range of the content of the cerium compound per abrasive weight described above.

[0040] The abrasive grains may be colloidal, for example, they may contain colloidal cerium oxide. The polishing liquid containing colloidal abrasive grains is a suspension of abrasive grains, and has a state in which cerium oxide forming the abrasive grains is dispersed in water. The colloidal abrasive grains can be obtained, for example, by a liquid phase method, and are abrasive grains derived from the liquid phase method. As liquid phase methods, colloidal method, hydrothermal synthesis method, sol-gel method, neutralization decomposition method, hydrolysis method, chemical precipitation method, coprecipitation method, atomization method, reverse micelle method, emulsion method, etc. can be cited. The abrasive grains may have grain boundaries or may not have grain boundaries.

[0041] As the colloidal abrasive, abrasive having a positron lifetime of τ1 to τ4 and a positron lifetime of τ2 of 0.3650 ns or less can be used. 22The time it takes for the positron emitted by Na to annihilate the electron pair can be used as a probe for subnanometer to nanometer-level lattice defects, free volume, and ultrafine voids. In other words, the shorter the positron lifetime, the higher the density of the particle.

[0042] The PAS Type L-II manufactured by TOYO SEIKO CO., LTD. can be used to measure the positron lifetime. After the powder obtained by vacuum drying the abrasive grains at room temperature (25°C) for 24 hours is placed in a powder measurement box, it is set in the positron beam source part and measured until the cumulative number reaches 1 million times. Using the software IPALM attached to the device, the lifetime histogram is divided into two components for analysis. 22 Among the positrons emitted by Na, some are annihilated by the positron beam source itself, such as Kapton and adhesive, and their components are mixed into the measurement results, so the analysis is performed assuming that the proportion of Kapton is 30%. Among the obtained positron lifetimes τ1 to τ4, τ1 and τ2 correspond to the positron lifetimes from the sample, τ3 corresponds to the positron lifetime from Kapton, and τ4 corresponds to the positron lifetime from the adhesive. In addition, τ1 corresponds to a small void such as a single hole, and τ2 corresponds to a void such as a collection of multiple voids.

[0043] As colloidal abrasive grains, abrasive grains in which regular diffraction spots are observed in electron beam diffraction of a transmission electron microscope (TEM) can be used. For example, when colloidal cerium oxide is used as the abrasive grain, in the diffraction spots obtained when the electron beam is irradiated perpendicularly to the cerium oxide (111) surface, when two adjacent diffraction spots A1 and A2 and a diffraction spot B adjacent to the diffraction spots A1 and A2 are observed, the distance R between the diffraction spots (the distance between the diffraction spot A1 and the diffraction spot B, and the distance between the diffraction spot A2 and the diffraction spot B) is Furthermore, the minimum value of the angle α of the diffraction spots A1 and A2 formed with the diffraction spot B as the center is 58 to 62°, that is, the abrasive particles having the diffraction spot B may account for more than 50%.

[0044] In the observation of the abrasive grains and the measurement of the distance R and angle α between the diffraction spots, JEM-2100F manufactured by JEOL Ltd. can be used. TEM sand grains with abrasive grains attached thereto can be subjected to electron beam diffraction for one abrasive grain under the conditions of an accelerating voltage of 200 kV, an electron beam wavelength of 2.508 pm, and a camera length of 30 cm, and the distance R and the angle α can be measured. The distance R and the angle α can be measured at least at three points for one abrasive grain, and the average value thereof can be adopted. All abrasive grains confirmed to be more than 100 in one field of view can be measured at any magnification by TEM observation, and the proportion of abrasive grains satisfying the above conditions can be calculated.

[0045] The average particle size of the abrasive grains may be in the following ranges: The average particle size of the abrasive grains can be adjusted by natural sedimentation, pulverization, dispersion, filtration, etc. For example, the particle size adjustment can be performed before or after mixing the constituent components of the polishing liquid.

[0046] From the viewpoint of stabilizing the polishing speed of silicon oxide, the average particle size D50 of the abrasive grains may be 1 nm or more, 3 nm or more, 5 nm or more, 10 nm or more, 30 nm or more, 50 nm or more, 80 nm or more, 100 nm or more, more than 100 nm, 120 nm or more, 130 nm or more, or 140 nm or more. From the viewpoint of stabilizing the polishing speed of silicon oxide, the average particle size D50 of the abrasive grains may be 500 nm or less, 300 nm or less, 200 nm or less, 180 nm or less, 160 nm or less, 155 nm or less, 150 nm or less, or 145 nm or less. From these viewpoints, the average particle size D50 of the abrasive grains may be 1 to 500 nm. The average particle size D50 of the abrasive grains represents the 50% particle size of the cumulative distribution based on volume, and can be measured, for example, by a laser diffraction particle size analyzer.

[0047] From the viewpoint of easily stabilizing the polishing speed of silicon oxide, the content of abrasive grains can be the following ranges based on the total mass of the polishing liquid. The content of abrasive grains can be 0.01 mass % or more, 0.03 mass % or more, 0.05 mass % or more, 0.08 mass % or more, 0.10 mass % or more, 0.20 mass % or more, or 0.25 mass % or more. The content of abrasive grains can be 10 mass % or less, 5.0 mass % or less, 3.0 mass % or less, 1.0 mass % or less, less than 1.0 mass %, 0.80 mass % or less, 0.50 mass % or less, less than 0.50 mass %, 0.40 mass % or less, 0.30 mass % or less, or 0.25 mass % or less. From these viewpoints, the content of abrasive grains can be 0.01 to 10 mass %.

[0048] (Ether compound)

[0049] From the viewpoint of reducing the polishing speed of silicon oxide, the polishing liquid involved in this embodiment contains at least one ether compound (hereinafter referred to as ether compound A) selected from the group consisting of a carboxyl group and a carboxylate group. The ether compound A is a compound having one or more ether groups and one or more carboxyl groups or carboxylate groups. As the carboxylate group, a functional group in which the hydrogen atom of the carboxyl group is substituted by a metal atom (sodium atom, potassium atom, etc.) can be cited.

[0050] By containing ether compound A in the polishing liquid, the polishing speed of silicon oxide can be reduced. Although the reason is not clear, it is speculated that this is because the oxygen atom of the ether group of ether compound A and the oxygen atom of the carboxyl group or carboxylate group are attached to the surface of the abrasive in a bidentate form, thereby inhibiting the polishing of silicon oxide. However, it is not limited to the above reasons. In addition, by containing ether compound A in the polishing liquid, the polishing speed of silicon nitride can be reduced. As the reason, it is speculated to be the same reason as the above reason for reducing the polishing speed of silicon oxide, but it is not limited to the above reason.

[0051] From the viewpoint of easily reducing the polishing rate of silicon oxide, the carbon number of the ether compound A may be 3 or more. From the viewpoint of easily reducing the polishing rate of silicon oxide, the carbon number of the ether compound A may be 50 or less, 40 or less, 30 or less, 20 or less, 10 or less, 8 or less, 6 or less, 5 or less, or 4 or less. From these viewpoints, the carbon number of the ether compound A may be 3 to 50, 3 to 30, 3 to 10, or 3 to 6. The carbon number of the ether compound A may be 4 or more. The carbon number of the ether compound A may be 3 or less.

[0052] From the viewpoint of easily reducing the polishing rate of silicon oxide, the molecular weight of ether compound A may be in the following range. The molecular weight of ether compound A may be 50 or more, 55 or more, 60 or more, 65 or more, 70 or more, 75 or more, 80 or more, 85 or more, or 90 or more. The molecular weight of ether compound A may be 500 or less, 400 or less, 300 or less, 250 or less, 200 or less, 150 or less, 130 or less, 120 or less, 115 or less, 110 or less, or 105 or less. From these viewpoints, the molecular weight of ether compound A may be 50 to 500. The molecular weight of ether compound A may be 95 or more, or 100 or more. The molecular weight of ether compound A may be 100 or less, or 95 or less.

[0053] From the viewpoint of easily reducing the polishing rate of silicon oxide, the number of ether groups in the ether compound A may be in the following ranges. The number of ether groups may be 10 or less, 8 or less, 5 or less, 4 or less, 3 or less, 2 or less, or 1. The number of ether groups may be 1 or more. From these viewpoints, the number of ether groups may be 1 to 10.

[0054] From the viewpoint of easily reducing the polishing rate of silicon oxide, the total number of carboxyl groups and carboxylate groups of the ether compound A may be in the following ranges. The total number of carboxyl groups and carboxylate groups may be 10 or less, 8 or less, 5 or less, 4 or less, 3 or less, 2 or less, or 1. The total number of carboxyl groups and carboxylate groups may be 1 or more. From these viewpoints, the total number of carboxyl groups and carboxylate groups may be 1 to 10.

[0055] The ether compound A may have functional groups other than ether, carboxyl and carboxylate groups, but may not have functional groups other than ether, carboxyl and carboxylate groups from the viewpoint of easily reducing the polishing rate of silicon oxide. As functional groups other than ether, carboxyl and carboxylate groups, hydroxyl, epoxy, phosphono, phosphonate, amino, cyano, sulfo, sulfonate, etc. may be cited. From the viewpoint of easily reducing the polishing rate of silicon oxide, the total number of functional groups other than ether, carboxyl and carboxylate groups in the ether compound A may be less than 10, less than 8, less than 6, less than 4, less than 3, less than 2, or less than 1.

[0056] The ether compound A may have at least one selected from the group consisting of an aromatic ring and a heteroaromatic ring, and may not have an aromatic ring or a heteroaromatic ring from the viewpoint of easily reducing the polishing rate of silicon oxide. From the viewpoint of easily reducing the polishing rate of silicon oxide, the total number of aromatic rings and heteroaromatic rings of the ether compound A may be 5 or less, 4 or less, 3 or less, 2 or less, or 1 or less.

[0057] The ether compound A may have an unsaturated carbon-carbon bond, but may not have an unsaturated carbon-carbon bond from the viewpoint of easily reducing the polishing rate of silicon oxide. From the viewpoint of easily reducing the polishing rate of silicon oxide, the number of unsaturated carbon-carbon bonds of the ether compound A may be 5 or less, 4 or less, 3 or less, 2 or less, or 1 or less.

[0058] From the viewpoint of easily reducing the polishing rate of silicon oxide, the ether compound A may include a chain ether compound (an ether compound having no ring structure). From the viewpoint of easily reducing the polishing rate of silicon oxide, the ether compound A may include a compound represented by the following general formula (1).

[0059] R 1 -OR 2 -COOR 3 -----(1)

[0060] [In formula (1), R 1 represents an alkyl group having 1 to 10 carbon atoms, R 2 represents an alkylene group having 1 to 10 carbon atoms, R 3 represents a hydrogen atom or a monovalent metal atom.]

[0061] From the viewpoint of facilitating the reduction of the polishing rate of silicon oxide, R 1 The number of carbon atoms in the alkyl group may be 8 or less, 6 or less, 5 or less, 4 or less, 3 or less, or 2 or less. From the viewpoint of facilitating the reduction of the polishing rate of silicon oxide, R 1 The number of carbon atoms in the alkyl group may be 1 to 5. 1The number of carbon atoms in the alkyl group may be 2 or more. 1 The alkyl group may be an unsubstituted alkyl group.

[0062] From the viewpoint of facilitating the reduction of the polishing rate of silicon oxide, R 2 The carbon number of the alkylene group may be 8 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, or 1. From the viewpoint of facilitating the reduction of the polishing rate of silicon oxide, R 2 The number of carbon atoms of the alkylene group may be 1 to 5. 2 The alkylene group may be unsubstituted.

[0063] Examples of the ether compound A include methoxyacetic acid, ethoxyacetic acid, propoxyacetic acid, butoxyacetic acid, 3-methoxypropionic acid, 2-methoxybutyric acid, and salts thereof. From the viewpoint of easily reducing the polishing rate of silicon oxide, the ether compound A may include -O-CH 2 The ether compound of -COOR (R represents a hydrogen atom or a monovalent metal atom) structure may contain at least one selected from the group consisting of methoxyacetic acid, ethoxyacetic acid, and salts thereof. The ether compound A may not contain 2-furancarboxylic acid, 2,5-furandicarboxylic acid, diglycolic acid, and salts thereof.

[0064] The content of the ether compound A may be in the following ranges based on the total mass of the polishing liquid: from the viewpoint of easily reducing the polishing rate of silicon oxide, the content of the ether compound A may be 0.0010 mass % or more, 0.0030 mass % or more, 0.0050 mass % or more, 0.0070 mass % or more, 0.010 mass % or more, 0.015 mass % or more, 0.020 mass % or more, or 0.025 mass % or more. From the viewpoint of stabilizing the polishing rate of silicon oxide, the content of the ether compound A may be 10% by mass or less, 5.0% by mass or less, 1.0% by mass or less, less than 1.0% by mass, 0.70% by mass or less, 0.50% by mass or less, less than 0.50% by mass, 0.40% by mass or less, less than 0.40% by mass, 0.30% by mass or less, 0.20% by mass or less, 0.10% by mass or less, less than 0.10% by mass, 0.070% by mass or less, 0.050% by mass or less, less than 0.050% by mass, 0.030% by mass or less, or 0.025% by mass or less. From these viewpoints, the content of the ether compound A may be 0.0010 to 10% by mass.

[0065] The content of ether compound A can be in the following ranges relative to 100 parts by mass of abrasive grains. From the viewpoint of easily reducing the polishing speed of silicon oxide, the content of ether compound A can be 0.1 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, more than 1 part by mass, 3 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, or 10 parts by mass or more. From the viewpoint of easily stabilizing the polishing speed of silicon oxide, the content of ether compound A can be 200 parts by mass or less, 150 parts by mass or less, 100 parts by mass or less, 70 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, less than 40 parts by mass, 30 parts by mass or less, 20 parts by mass or less, or 10 parts by mass or less. From these viewpoints, the content of ether compound A can be 0.1 to 200 parts by mass.

[0066] (additive)

[0067] The polishing liquid involved in this embodiment may contain components other than abrasive grains, ether compound A and water. Examples of such components include ether compounds other than ether compound A (hereinafter referred to as ether compound B), nitrogen-containing compounds, acid components, oxidants, quaternary ammonium salts, surfactants, chelating agents, etc. The polishing liquid involved in this embodiment may not contain at least one of these components.

[0068] The polishing liquid involved in this embodiment may contain an ether compound B. Examples of the ether compound B include polyether compounds. Examples of the polyether compound include polyglycerol, polysaccharides (e.g., dextrin), polyalkylene glycol, polyoxypropylene polyglyceryl ether, polyoxyethylene polyglyceryl ether, 1,4-bis(2-hydroxyethoxy)benzene, 2,2-bis(4-polyoxyethyleneoxyphenyl)propane, 2,2-bis(4-polyoxypropyleneoxyphenyl)propane, ethylene glycol monophenyl ether, diethylene glycol monophenyl ether, polyoxyalkylene monophenyl ether, propylene glycol monophenyl ether, polyoxypropylene monomethyl phenyl ether, polyethylene glycol monomethyl ether, pentaerythritol polyoxyethylene ether, ethylene glycol monoallyl ether, polyoxyethylene monoallyl ether, alkyl glycosides, and the like.

[0069] The content of ether compound B is based on the total mass of the polishing liquid of the polishing liquid, and can be the following range. From the viewpoint of easily stabilizing the polishing rate of silicon oxide, the content of ether compound B can be 0.001 mass % or more, 0.005 mass % or more, 0.01 mass % or more, 0.05 mass % or more, 0.08 mass % or more, 0.1 mass % or more, 0.2 mass % or more, 0.3 mass % or more, or 0.35 mass % or more. From the viewpoint of easily stabilizing the polishing rate of silicon oxide, the content of ether compound B can be 5 mass % or less, 4 mass % or less, 3 mass % or less, 2 mass % or less, 1 mass % or less, 0.8 mass % or less, 0.6 mass % or less, 0.5 mass % or less, or 0.4 mass % or less. From these viewpoints, the content of ether compound B can be 0.001 to 5 mass %.

[0070] The polishing liquid involved in this embodiment may contain a nitrogen-containing compound (however, compounds corresponding to ether compound A, ether compound B, oxidizing agent, quaternary ammonium salt, surfactant, and chelating agent are excluded). The nitrogen-containing compound refers to a compound containing one or more nitrogen atoms in the molecule. Examples of the nitrogen-containing compound include amino acids, pyridine compounds, pyrazole compounds, triazole compounds, pyrimidine compounds, and imidazole compounds.

[0071] Examples of the amino acid include alanine (α-alanine, β-alanine), arginine, asparagine, aspartic acid, cysteine, glutamine, glutamic acid, glycine, histidine, isoleucine, leucine, lysine, methionine, phenylalanine, proline, serine, threonine, tryptophan, tyrosine, and valine.

[0072] Examples of the pyridine compound include pyridine, picoline, acetylpyridine, pyridineamide (nicotinamide), and aminopyridine.

[0073] Examples of the pyrazole compound include pyrazole, N-methylpyrazole, 3,5-dimethylpyrazole, 1-allyl-3,5-dimethylpyrazole, 3,5-di(2-pyridyl)pyrazole, 3,5-diisopropylpyrazole, 3,5-dimethyl-1-hydroxymethylpyrazole, 3,5-dimethyl-1-phenylpyrazole, and 4-methylpyrazole.

[0074] Examples of the pyrimidine compound include pyrimidine, 1,3-diphenyl-pyrimidine-2,4,6-trione, 1,4,5,6-tetrahydropyrimidine, 2,4,5-trihydroxypyrimidine, 2,4,6-trichloropyrimidine, 2,4,6-trimethoxypyrimidine, and 2,4,6-triphenylpyrimidine.

[0075] Examples of the imidazole compound include imidazole, 1,1′-carbonylbis-1H-imidazole, 1,1′-oxalyldiimidazole, 1,2,4,5-tetramethylimidazole, 1,2-dimethyl-5-nitroimidazole, 1,2-dimethylimidazole, 1-butylimidazole, 1-ethylimidazole, 1-methylimidazole, and benzimidazole.

[0076] From the viewpoint of stabilizing the polishing rate of silicon oxide, the nitrogen-containing compound may include at least one selected from the group consisting of amino acids, pyridine compounds, and pyrazole compounds, or may include at least one selected from the group consisting of β-alanine, pyridineamide, and 3,5-dimethylpyrazole.

[0077] The content of the nitrogen-containing compound can be the following ranges based on the total mass of the polishing liquid. From the viewpoint of easily stabilizing the polishing rate of silicon oxide, the content of the nitrogen-containing compound can be 0.0001 mass %, 0.0005 mass %, 0.001 mass %, 0.003 mass %, or 0.005 mass %. From the viewpoint of easily stabilizing the polishing rate of silicon oxide, the content of the nitrogen-containing compound can be 1 mass %, 0.5 mass %, 0.1 mass %, 0.08 mass %, 0.05 mass %, 0.03 mass %, 0.01 mass %, 0.008 mass %, or 0.006 mass %. From these viewpoints, the content of the nitrogen-containing compound can be 0.0001 to 1 mass %.

[0078] The polishing liquid according to the present embodiment may contain an acid component. The polishing liquid according to the present embodiment may contain an organic acid component or an inorganic acid component as the acid component.

[0079] Examples of the organic acid component include organic acids (excluding amino acids), organic acid esters, organic acid salts, and amino acids. Examples of the organic acid include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylvaleric acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, 3-methylphthalic acid, 4-methylphthalic acid, 3-aminophthalic acid, 4-aminophthalic acid, 3-nitrophthalic acid, 4-nitrophthalic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, isophthalic acid, malic acid, tartaric acid, citric acid, p-toluenesulfonic acid, p-phenolsulfonic acid, methanesulfonic acid, lactic acid, itaconic acid, maleic acid, quinaldine acid, adipic acid, pimelic acid, etc. Examples of the organic acid ester include esters of the above-mentioned organic acids. Examples of the organic acid salts include ammonium salts, alkali metal salts, alkaline earth metal salts, and halides of the above-mentioned organic acids.

[0080] Examples of the inorganic acid component include inorganic acids, ammonium salts of inorganic acids, and chromic acid. Examples of the inorganic acid include hydrochloric acid, sulfuric acid, and nitric acid. Examples of the ammonium salts of inorganic acids include monovalent ammonium salts of inorganic acids such as ammonium nitrate, ammonium chloride, and ammonium bromide; divalent ammonium salts of inorganic acids such as ammonium carbonate, ammonium sulfate, and ammonium persulfate; and trivalent ammonium salts of inorganic acids such as ammonium phosphate and ammonium borate.

[0081] The content of the acid component is based on the total mass of the polishing liquid, and can be the following range. From the viewpoint of easily stabilizing the polishing speed of silicon oxide, the content of the acid component can be 0.001 mass %, 0.005 mass %, 0.01 mass %, 0.03 mass %, 0.05 mass %, 0.06 mass %, 0.07 mass %, 0.08 mass %, 0.09 mass %, 0.1 mass %, or 0.11 mass %. From the viewpoint of easily stabilizing the polishing speed of silicon oxide, the content of the acid component can be 5 mass %, 4 mass %, 3 mass %, 2 mass %, 1 mass %, 0.8 mass %, 0.5 mass %, 0.4 mass %, 0.3 mass %, 0.2 mass %, or 0.15 mass %. From these viewpoints, the content of the acid component can be 0.001 to 5 mass %.

[0082] The polishing liquid involved in this embodiment may contain an oxidant or may not contain an oxidant (the content of the oxidant may be substantially 0% by mass based on the total mass of the polishing liquid). Examples of the oxidant include hydrogen peroxide, peroxide, nitrate, iodate, periodate, hypochlorite, chlorite, chlorate, perchlorate, persulfate, dichromate, permanganate, ozone water, silver (II) salt, iron (III) salt, etc. The content of the oxidant may be less than 0.01 mol based on 1L of the polishing liquid.

[0083] The polishing liquid involved in the present embodiment may contain a quaternary ammonium salt or may not contain a quaternary ammonium salt (the content of the quaternary ammonium salt is based on the total mass of the polishing liquid, and can be substantially 0 mass %). As the quaternary ammonium salt, tetramethylammonium salt, tetraethylammonium salt, tetrapropylammonium salt, tetrabutylammonium salt, tetrapentylammonium salt, etc. can be cited. The content of the quaternary ammonium salt is based on the total mass of the polishing liquid, and can be less than 0.00001 mass %.

[0084] The polishing liquid involved in this embodiment may contain a surfactant or may not contain a surfactant (the content of the surfactant may be substantially 0% by mass based on the total mass of the polishing liquid). Examples of the surfactant include decylbenzenesulfonic acid, dodecylbenzenesulfonic acid, tetradecylbenzenesulfonic acid, hexadecylbenzenesulfonic acid, dodecylnaphthalenesulfonic acid, and tetradecylnaphthalenesulfonic acid. The content of the surfactant may be less than 0.001 g based on 1 L of the polishing liquid.

[0085] The polishing liquid involved in this embodiment may contain a chelating agent or may not contain a chelating agent (the content of the chelating agent is based on the total mass of the polishing liquid, and may be substantially 0 mass %). As the chelating agent, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, ethylenediaminetetraacetic acid, N,N,N-trimethylenephosphonic acid, ethylenediamine-N,N,N',N'-tetramethylenesulfonic acid, trans-cyclohexanediaminetetraacetic acid, 1,2-diaminopropanetetraacetic acid, ethylenediamine-o-hydroxyphenylacetic acid, ethylenediamine disuccinic acid (SS body), N-(2-carboxylic acid ethyl ester)-L-aspartic acid, β-alanine diacetic acid, 2-phosphonobutane-1,2,4-tricarboxylic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, N,N'-bis(2-hydroxybenzyl)ethylenediamine-N,N'-diacetic acid, 1,2-dihydroxybenzene-4,6-disulfonic acid, etc. can be cited. The content of the chelating agent can be less than 0.0003 mol based on 1 L of the polishing liquid.

[0086] (water)

[0087] The polishing liquid involved in this embodiment may contain water. Water can be contained as the remainder after removing other components from the polishing liquid. The content of water can be the following range based on the total mass of the polishing liquid. The content of water can be 90.0% by mass or more, 93.0% by mass or more, 95.0% by mass or more, 97.0% by mass or more, 99.0% by mass or more, 99.2% by mass or more, 99.4% by mass or more, 99.5% by mass or more, 99.6% by mass or more, or 99.7% by mass or more. The content of water can be less than 100% by mass, less than 99.9% by mass, less than 99.8% by mass, or less than 99.7% by mass. From these viewpoints, the content of water can be 90.0% by mass or more and less than 100% by mass.

[0088] From the viewpoint of easily reducing the polishing speed of silicon oxide, the pH of the polishing liquid involved in this embodiment can be in the following range. The pH of the polishing liquid can be above 2.0, above 2.5, above 2.5, above 2.6, above 2.7, above 2.8, above 2.9, above 3.0, above 3.0, or above 3.1. The pH of the polishing liquid can be below 5.0, less than 5.0, below 4.5, below 4.0, less than 4.0, below 3.8, below 3.6, below 3.5, less than 3.5, below 3.4, or below 3.3. From these viewpoints, the pH of the polishing liquid can be 2.0 to 5.0. From the perspective of increasing the polishing rate ratio of silicon oxide to silicon nitride, the pH of the polishing liquid can be above 2.0, above 2.5, above 3.0, above 3.1, above 3.2, above 3.3, above 3.4, above 3.5, above 3.6, above 3.7, above 3.8, above 3.9, or above 4.0, and can be below 5.0, below 4.9, below 4.8, below 4.7, below 4.6, below 4.5, below 4.4, below 4.3, below 4.2, below 4.1, or below 4.0.

[0089] The pH of the polishing liquid involved in this embodiment can be measured using a pH meter (e.g., model number: PHL-40 manufactured by DKK-TOA CORPORATION). For example, after two-point calibration of the pH meter using a phthalate pH buffer (pH: 4.01) and a neutral phosphate pH buffer (pH: 6.86) as standard buffers, the electrode of the pH meter is immersed in the polishing liquid, and the value after stabilization for more than 2 minutes is measured. At this time, the liquid temperature of the standard buffer and the polishing liquid is set to 25°C.

[0090] (other)

[0091] The polishing liquid according to the present embodiment can be stored as a one-liquid polishing liquid containing at least abrasive grains, an ether compound A, and water. The one-liquid polishing liquid is stored as a polishing liquid storage liquid with a reduced water content, and can be diluted with water before or during polishing for use.

[0092] In the case of a single-liquid polishing liquid, as a method for supplying the polishing liquid to the polishing plate, there can be used a method of directly conveying the polishing liquid for supply; a method of using different pipes to convey the storage liquid for polishing liquid and water, and causing them to merge and mix for supply; a method of pre-mixing the storage liquid for polishing liquid and water and then supplying, etc.

[0093] <Polishing fluid set>

[0094] The polishing liquid involved in this embodiment can be a multi-liquid (e.g., two-liquid) polishing liquid set (e.g., a CMP polishing liquid set), and the constituent components of the polishing liquid are separated into a first liquid and a second liquid in such a manner that the first liquid (slurry) and the second liquid (additive liquid) are mixed to form the above-mentioned polishing liquid. The first liquid, for example, contains at least abrasive grains and water. The second liquid, for example, contains at least ether compound A and water. The constituent components of the polishing liquid can be stored as a polishing liquid set divided into three or more liquids.

[0095] In the polishing liquid set, the first liquid and the second liquid are mixed to prepare the polishing liquid before or during polishing. The multi-liquid polishing liquid set can be stored as a slurry storage liquid and an additive storage liquid with reduced water content, and can be diluted with water before or during polishing for use.

[0096] In the case of storing as a multi-liquid polishing liquid set including a first liquid and a second liquid, the polishing speed can be adjusted by arbitrarily changing the formulation of each liquid. In the case of using the polishing liquid set for polishing, as a method for supplying the polishing liquid to the polishing plate, there are the following methods. For example, a method can be used in which the first liquid and the second liquid are transported using different pipes, and these pipes are merged and mixed for supply; a method can be used in which different pipes are used to transport a slurry storage liquid, an additive storage liquid, and water, and these are merged and mixed for supply; a method can be used in which the first liquid and the second liquid are pre-mixed and then supplied; a method can be used in which the slurry storage liquid, the additive storage liquid, and water are pre-mixed and then supplied, etc. In addition, a method can be used in which the first liquid and the second liquid of the polishing liquid set are separately supplied to the polishing plate. At this time, the polishing liquid obtained by mixing the first liquid and the second liquid on the polishing plate is used to polish the polished surface.

[0097] <Grinding method>

[0098] The polishing method of this embodiment may include a polishing step of polishing the polished surface using a single-liquid polishing liquid, or may include a polishing step of polishing the polished surface using a polishing liquid obtained by mixing a first liquid and a second liquid in a polishing liquid set. The polishing method of this embodiment is, for example, a polishing method of a substrate having a polished surface.

[0099] In the grinding method involved in the present embodiment, the grinding liquid involved in the present embodiment is used to grind the grinding surface. The grinding surface can contain silicon oxide, and can also contain silicon oxide derived from TEOS. The grinding material having the grinding surface can be a single material, and can also be a plurality of materials. The grinding material can be a film (grinding film), and can also be a silicon oxide film, and can also be a TEOS film.

[0100] The polishing method according to the present embodiment may be a method for polishing a substrate having a polished surface composed of silicon nitride. The polishing method according to the present embodiment may be a method for polishing a substrate having a polished surface composed of silicon oxide and silicon nitride.

[0101] In the grinding process, for example, a substrate having a grinding surface is pressed against a grinding pad (grinding cloth) of a grinding plate, and a grinding liquid is supplied between the grinding surface and the grinding pad, so that the substrate and the grinding plate are relatively moved to grind the grinding surface. In the grinding process, for example, at least a portion of the grinding material is removed by grinding.

[0102] As a base body to be polished, for example, there can be cited a base body on which a polished material is formed in the manufacture of semiconductor elements (for example, a semiconductor substrate on which an STI pattern, a gate pattern, a wiring pattern, etc. are formed). As the material to be polished, there can be cited insulating materials such as silicon oxide; stopper layer materials such as silicon nitride and polysilicon, etc. The material to be polished can be a single material or a plurality of materials. In the case where a plurality of materials are exposed on the polished surface, these can be regarded as the material to be polished. The material to be polished can be in the form of a film (polished film). The shape of the insulating component is not particularly limited, for example, it is in the form of a film (insulating film). The shape of the stopper layer is not particularly limited, for example, it is in the form of a film (stopper layer film: silicon nitride film, polysilicon film, etc.).

[0103] By using the polishing liquid involved in this embodiment, a polished material (for example, an insulating film such as a silicon oxide film) formed on a substrate is polished to remove excess parts, thereby eliminating the unevenness of the surface of the polished material and obtaining a smooth surface on the entire polished surface.

[0104] In this embodiment, the insulating part in the following substrate (a substrate having an insulating part (for example, a silicon oxide film containing silicon oxide at least on the surface), a stopper layer arranged under the insulating part, and a semiconductor substrate arranged under the stopper layer) can be polished, wherein the substrate has a substrate having a concave-convex pattern, a stopper layer arranged on the convex part of the substrate, and an insulating part arranged on the substrate and the stopper layer in a manner of filling the concave part of the concave-convex pattern. The stopper layer material constituting the stopper layer is, for example, a material having a lower polishing speed than the insulating material, and examples thereof include silicon nitride, polysilicon, and the like.

[0105] In the grinding method involved in this embodiment, as a grinding device, a common grinding device having a holder capable of holding a substrate (semiconductor substrate, etc.) having a grinding surface and a grinding plate capable of attaching a grinding pad can be used. A motor capable of changing the rotation speed is respectively installed on the holder and the grinding plate. As a grinding device, for example, a grinding device manufactured by APPLIED MATERIALS: Mirra3400 can be used.

[0106] As grinding pad, usually can use nonwoven fabrics, foam, non-foam etc. As the material of grinding pad, can use polyurethane, acrylic resin, polyester, acrylic acid-ester copolymer, polytetrafluoroethylene, polypropylene, polyethylene, poly-4-methylpentene, cellulose, cellulose ester, polyamide (for example, nylon (trade name) and aramid (aramid)), polyimide, polyimide amide, polysiloxane copolymer, ethylene oxide compound, phenolic resin, polystyrene, polycarbonate, epoxy resin and other resins. As the material of grinding pad, from the viewpoint that flatness is more excellent, can be foamed polyurethane and non-foamed polyurethane. For grinding pad, can implement the groove processing for accumulating grinding fluid.

[0107] Although there is no restriction on the grinding conditions, in order to prevent the substrate from flying out, the rotation speed of the grinding plate can be below 200rpm (=times / min), and from the viewpoint of fully suppressing the generation of grinding scratches, the grinding pressure (processing load) applied to the substrate can be below 100kPa. During the grinding, the grinding liquid can be continuously supplied to the grinding pad by a pump, etc. Although there is no restriction on the supply amount, the surface of the grinding pad can be covered with the grinding liquid all the time.

[0108] After the grinding, the substrate is preferably fully cleaned in running water to remove particles attached to the substrate. During cleaning, dilute hydrofluoric acid or ammonia water can be used in addition to pure water, and a brush can also be used to improve the cleaning efficiency. In addition, after cleaning, it is preferred to use a rotary dryer to remove water droplets attached to the substrate and then dry the substrate.

[0109] The manufacturing method of the device involved in the present embodiment includes a device manufacturing process of obtaining a device using a substrate (grinded body) ground by the grinding method involved in the present embodiment. The device involved in the present embodiment is a device obtained by the manufacturing method of the device involved in the present embodiment. The device involved in the present embodiment is not particularly limited, but can be an electronic device (for example, a semiconductor device such as a semiconductor package), a wafer (for example, a semiconductor wafer), or a chip (for example, a semiconductor chip). As one mode of the manufacturing method of the device involved in the present embodiment, in the manufacturing method of the electronic device involved in the present embodiment, an electronic device is obtained using a substrate ground by the grinding method involved in the present embodiment. As one mode of the manufacturing method of the device involved in the present embodiment, in the manufacturing method of the semiconductor device involved in the present embodiment, a semiconductor device (for example, a semiconductor package) is obtained using a substrate ground by the grinding method involved in the present embodiment. The manufacturing method of the device involved in the present embodiment may include a grinding process of grinding the substrate by the grinding method involved in the present embodiment before the device manufacturing process.

[0110] As one mode of the device manufacturing process, the manufacturing method of the device involved in the present embodiment may include a singulation process of singulating the substrate (ground body) ground by the grinding method involved in the present embodiment. The singulation process may be, for example, a process of cutting a wafer (for example, a semiconductor wafer) ground by the grinding method involved in the present embodiment to obtain a chip (for example, a semiconductor chip). As one mode of the device manufacturing method involved in the present embodiment, the manufacturing method of the electronic device involved in the present embodiment may include a process of obtaining an electronic device (for example, a semiconductor device) by singulating the substrate ground by the grinding method involved in the present embodiment. As one mode of the device manufacturing method involved in the present embodiment, the manufacturing method of the semiconductor device involved in the present embodiment may include a process of obtaining a semiconductor device (for example, a semiconductor package) by singulating the substrate ground by the grinding method involved in the present embodiment.

[0111] As one mode of the device manufacturing process, the manufacturing method of the device involved in the present embodiment may include a connection process of connecting (for example, electrically connecting) a substrate (a polished body) polished by the polishing method involved in the present embodiment to other connected bodies. The connected body connected to the substrate polished by the polishing method involved in the present embodiment is not particularly limited, and may be a substrate polished by the polishing method involved in the present embodiment, or may be a connected body different from the substrate polished by the polishing method involved in the present embodiment. In the connection process, the substrate and the connected body may be directly connected (the substrate and the connected body are connected in a contacting state), or the substrate and the connected body may be connected via other components (conductive components, etc.). The connection process can be performed before the singulation process, after the singulation process, or before and after the singulation process.

[0112] The connection process may be a process of connecting the polished surface of the substrate polished by the polishing method involved in the present embodiment and the connected body, or may be a process of connecting the connecting surface of the substrate polished by the polishing method involved in the present embodiment and the connecting surface of the connected body. The connecting surface of the substrate may be the polished surface polished by the polishing method involved in the present embodiment. Through the connection process, a connected body having a substrate and a connected body can be obtained. In the connection process, when the connecting surface of the substrate has a metal part, the connected body can be brought into contact with the metal part. In the connection process, when the connecting surface of the substrate has a metal part and the connecting surface of the connected body has a metal part, the metal parts can be brought into contact with each other. The metal part may contain copper.

[0113] The device according to the present embodiment (for example, an electronic device such as a semiconductor device) includes at least one selected from the group consisting of a substrate polished by the polishing method according to the present embodiment and a device according to the present embodiment.

[0114] Example

[0115] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited thereto.

[0116] <Preparation of polishing liquid>

[0117] (Examples 1 to 4 and Comparative Examples 1 to 8)

[0118] Water was added to a liquid containing colloidal cerium oxide particles (manufactured by Solvay, product name: Zenus (registered trademark) HC60, particle content: 30 mass %), and then the particle size was adjusted to obtain a slurry containing 5.0 mass % of colloidal cerium oxide particles (abrasive grains).

[0119] A polishing liquid containing 0.25 mass % of colloidal cerium oxide particles (abrasive grains) and 0.025 mass % of additives was obtained by adding water and the additives shown in Table 1 to the above slurry. In Examples 4 and 5, aqueous ammonia was added to adjust the pH.

[0120] <Measurement of pH>

[0121] The pH of the polishing liquids of Examples 1 and 2 was measured using a pH meter (Model: PHL-40 manufactured by DKK-TOA CORPORATION). After two-point calibration of the pH meter using a phthalate pH buffer (pH: 4.01) and a neutral phosphate pH buffer (pH: 6.86) as standard buffers, the pH meter electrode was immersed in the polishing liquid and the value after stabilization for more than 2 minutes was measured. The pH of the polishing liquid of Example 1 was 3.26, the pH of the polishing liquid of Example 2 was 3.19, the pH of the polishing liquid of Example 3 was 4.00, and the pH of the polishing liquid of Example 4 was 4.54.

[0122] <Measurement of average particle size>

[0123] The average particle size D50 of the colloidal cerium oxide particles in the polishing liquid was determined using "Microtrac MT3300EXII" manufactured by Microtrac BEL Corp. The measurement results are shown in Table 1.

[0124] <Grinding evaluation>

[0125] In a polishing device (manufactured by APPLIED MATERIALS, product name: Mirra3400), a substrate having a film to be polished (silicon oxide film (TEOS film) or silicon nitride film (SiN film)) formed on a φ200 mm silicon wafer is set on a substrate mounting holder to which an adsorption pad is attached. The holder is placed on a flat plate to which a pad made of porous polyurethane resin is attached so that the film to be polished and the pad are opposite to each other. Each of the above-mentioned polishing liquids is supplied to the pad at a supply amount of 200 mL / min, and the substrate is pressed onto the pad at a polishing load of 20 kPa. At this time, the flat plate is subjected to a 93 min -1 Speed ​​and cage at 87min -1 The polishing was performed by rotating for 30 seconds at a speed of 100°. The polished substrate was thoroughly washed with pure water and then dried. The polishing speed (TEOS RR and SiN RR) was calculated by measuring the thickness change of the polished film before and after polishing using an optical interference film thickness measuring device. Unit: / min). In addition, the polishing rate ratio of silicon oxide to silicon nitride (polishing rate of silicon oxide / polishing rate of silicon nitride) was determined. The results are shown in Table 1.

[0126] [Table 1]

[0127]

Claims

1. A polishing liquid comprising abrasive grains, an ether compound having at least one selected from the group consisting of a carboxyl group and a carboxylate group, and water.

2. The polishing liquid according to claim 1, wherein The abrasive grains contain cerium oxide.

3. The polishing liquid according to claim 1, wherein The ether compound includes a compound represented by the following general formula (1): R 1 -OR 2 -COOR 3 -----(1) In formula (1), R 1 represents an alkyl group having 1 to 10 carbon atoms, R 2 represents an alkylene group having 1 to 10 carbon atoms, R 3 It represents a hydrogen atom or a monovalent metal atom.

4. The polishing liquid according to claim 1, wherein The ether compound includes at least one selected from the group consisting of ethoxyacetic acid, methoxyacetic acid, and salts thereof.

5. The polishing liquid according to claim 1, wherein The content of the ether compound is less than 0.10 mass % based on the total mass of the polishing liquid. The polishing liquid according to claim 1 , wherein the pH value thereof is 2.0 to 5.

0. The polishing liquid according to claim 1 , which is used for polishing a polished surface containing silicon oxide.

8. A polishing liquid set, wherein: The constituent components of the polishing liquid according to any one of claims 1 to 7 are separated into a first liquid and a second liquid and stored, the first liquid containing the abrasive and water, and the second liquid containing the ether compound and water. 9 . A polishing method comprising the step of polishing a polishing surface comprising silicon oxide using the polishing liquid according to claim 1 . 10 . A polishing method comprising the step of polishing a surface to be polished including silicon oxide using a polishing liquid obtained by mixing the first liquid and the second liquid of the polishing liquid set according to claim 8 .