Microlens array and solid-state imaging element
By forming a low refractive index layer on the microlens array of solid-state imaging elements and forming a diffraction grating thereon, the problem of cracks and spots forming on the anti-reflection layer is solved, and effective interface reflection suppression and stability of the functional layer are achieved. Ensures improvements in optical characteristics and sensor performance.
Patent Information
- Application Number
- CN202380034454.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-10
- Filing Date
- 2023-04-12
- Publication Date
- 2024-12-06
AI Technical Summary
In solid-state imaging elements, especially in 3D sensors, when a diffraction grating pattern is formed on an anti-reflection layer containing hollow silica filler, it is prone to adverse conditions such as cracks or spots, which affects optical characteristics and sensor performance.
Using a low refractive index layer with a smaller refractive index layer than a microlens, by forming a low refractive index layer with hollow fillers and medium on the microlens array and appropriately forming a diffraction grating thereon, the refractive index of the low refractive index layer is controlled to be close to air, reducing the refractive index of the low refractive index layer. Interface reflection, and adjust the filler content and configuration during the manufacturing process to avoid the formation of face-centered cubic lattice structure.
Effectively suppress interface reflection, prevent cracks and spots, ensure the stability of optical characteristics and sensor performance, and provide a microlens array suitable for low refractive index layers on which other functional layers can be formed.
Smart Images

Figure CN119096170A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a microlens array and a solid-state imaging element using the microlens array.
[0002] This application claims priority based on patent application No. 2022-077426 filed in Japan on May 10, 2022, and the contents are incorporated herein by reference. Background Art
[0003] There is known a distance image sensor using a solid-state imaging element that can be carried and incorporated into a thin mobile phone.
[0004] For example, Patent Document 1 describes a photoelectric conversion substrate including a plurality of photoelectric conversion sections and a microlens array provided on the photoelectric conversion sections. The microlens array has a function of focusing incident light onto each photoelectric conversion section.
[0005] In order to increase the light-gathering efficiency, a material with a relatively large refractive index is used for the microlenses constituting the microlens array. However, if the refractive index is high, reflection occurs at the interface with air, causing loss of incident light.
[0006] In order to alleviate this loss, it is known to provide an antireflection layer formed of a material having a lower refractive index than that of the material of the microlens on the microlens.
[0007] Patent Document 2 describes a material in which silica particles having a cavity inside are added to a fluorine-containing silicone resin as a low refractive index material. Hollow silica has a refractive index substantially the same as that of air, and thus has the advantage that the refractive index of the formed antireflection layer can be adjusted relatively easily by changing the content.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2019-195051
[0011] Patent Document 2: Japanese Patent No. 5668276 Summary of the invention
[0012] Problems to be solved by the invention
[0013] In recent years, as the use of solid-state imaging devices has expanded and their structures have become more complex, other layers have been formed on the anti-reflection layer described above. For example, in a 3D sensor using a solid-state imaging device, a diffraction grating pattern is sometimes formed on the anti-reflection layer.
[0014] The general diffraction grating pattern is formed by exposing, developing, and patterning a photosensitive resin layer. The details will be described later, but the inventors have found that when such a pattern is formed on an anti-reflection layer containing hollow silica fillers, cracks or spots may sometimes occur.
[0015] The inventors have clarified the cause and completed the present invention.
[0016] An object of the present invention is to provide a microlens array including a low refractive index layer to suppress interface reflection and capable of appropriately forming other layers on the low refractive index layer.
[0017] Means for solving problems
[0018] A first aspect of the present invention is a microlens array in which a plurality of microlenses are arranged in an array.
[0019] The microlens array includes a low refractive index layer which contains a hollow filler and a medium, is formed on a plurality of microlenses, and has a refractive index smaller than that of the plurality of microlenses.
[0020] In the low refractive index layer, the ratio of white pixels in the binary planar image is 76% or less.
[0021] A second aspect of the present invention is a solid-state imaging device including the microlens array according to the first aspect.
[0022] Effects of the Invention
[0023] According to the present invention, it is possible to provide a microlens array which includes a low refractive index layer to suppress interface reflection and on which other layers can be appropriately formed. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] [ Figure 1 ] is a schematic cross-sectional view of a solid-state imaging element according to one embodiment of the present invention.
[0025] [ Figure 2 ] is to show the manufacturing Figure 1 A diagram showing a process of manufacturing a solid-state imaging element.
[0026] [ Figure 3 ] is to show the manufacturing Figure 1 A diagram showing a process of manufacturing a solid-state imaging element.
[0027] [ Figure 4 ] is to show the manufacturing Figure 1 A diagram showing a process of manufacturing a solid-state imaging element.
[0028] [ Figure 5 ] is a diagram showing a face-centered cubic lattice structure.
[0029] [ Figure 6 ] is a scanning electron microscope (SEM) image of the low refractive index layer.
[0030] [ Figure 7 ]yes Figure 6 Binarized image of the SEM image shown.
[0031] [ Figure 8 ] is after removing noise Figure 7 The binarized image shown. DETAILED DESCRIPTION
[0032] Below, refer to Figures 1 to 8 One embodiment of the present invention will be described.
[0033] Figure 1 2 is a schematic cross-sectional view of a solid-state imaging device 10 according to the present embodiment. The solid-state imaging device 10 includes a substrate 20, a CMOS image sensor 24, a color filter 28, and a microlens array 30, and functions as a distance image sensor as a whole.
[0034] The substrate 20 is, for example, a silicon (Si) substrate. The material of the substrate 20 is, for example, Si, but it is not particularly limited as long as it is a material that has pixels or light receiving elements of the CMOS image sensor 24 and can make them perform electrical functions. Hereinafter, the thickness direction of the substrate 20 is set as the Z direction, and the direction from the inside of the substrate 20 in the Z direction toward the surface 20a is set as the "front". In addition, a direction parallel to the surface 20a and orthogonal to the Z direction is set as the X direction, and a direction parallel to the surface 20a and orthogonal to the X direction and the Z direction is set as the Y direction.
[0035] The solid-state imaging element 10 includes a plurality of CMOS image sensors 24. The plurality of CMOS image sensors 24 are arranged in the X direction and the Y direction, respectively. In this way, by providing a plurality of CMOS image sensors 24, a pixel array of the solid-state imaging element 10 is formed in the direction along the surface 20a of the substrate 20. The number of CMOS image sensors 24 provided in the solid-state imaging element 10 is appropriately set according to the purpose of the solid-state imaging element 10, and the ... Figure 1 At least a portion of them are exemplified in the examples above.
[0036] Each CMOS image sensor 24 is embedded in the surface 20a of the substrate 20 in the Z direction.
[0037] The light receiving surface 25 of the CMOS image sensor 24 is exposed from the substrate 20 and is substantially coplanar with the surface 20a. Figure 1 Although illustration of the detailed structure of the CMOS image sensor 24 is omitted in the figures, the CMOS image sensor 24 is the same as a known CMOS image sensor.
[0038] The color filter 28 is provided on the light receiving surface 25 of each CMOS image sensor 24 (i.e., in front of the Z direction). The color filter 28 has a function of transmitting light of a wavelength band of any color of the three primary colors of light, namely, red (R) / green (G) / blue (B). The color transmitted by the color filter 28 is appropriately determined for each of the plurality of CMOS image sensors 24 according to the arrangement of the plurality of CMOS image sensors 24, etc.
[0039] The microlens array 30 is formed on the color filter 28, and includes a plurality of microlenses 31 arranged corresponding to the color filter 28, a low refractive index layer 60 formed on the microlenses 31, and a diffraction grating (functional layer) 70 formed on the low refractive index layer 60. Here, the plurality of microlenses 31 arranged corresponding to the color filter 28 means that each of the plurality of color filters 28 and each of the plurality of microlenses 31 are arranged to overlap in a plan view.
[0040] The microlens 31 is provided on the surface 28a of the color filter 28 on each CMOS image sensor 24. The microlens 31 is a so-called plano-convex lens having a bottom surface 31b and a lens surface 31a. The material of the microlens 31 has a refractive index higher than at least the refractive index of the air or the low refractive index layer 60. In particular, in order to obtain a refractive index difference with the low refractive index layer 60 and improve the focusing effect of the microlens 31, the material of the microlens 31 is preferably a high refractive index material having a refractive index of, for example, about 1.6. The curvature and shape of the lens surface 31a are appropriately designed according to the refractive index of the material of the microlens 31 at a visible wavelength, etc. In addition, the microlens 31 is formed and configured in such a way that light incident from the front in the Z direction toward the direction opposite to the front in the Z direction is focused on the CMOS image sensor 24 through the color filter 28 below (i.e., behind in the Z direction). Here, it can be considered that each of the plurality of microlenses 31 has the same refractive index.
[0041] The low refractive index layer 60 forms a surface 60a for providing the diffraction grating 70 closer to the front in the Z direction than the microlens 31. The low refractive index layer 60 physically fills the surface 20a of the substrate 20 exposed between the color filter 28 and the microlens 31 adjacent to each other in a plan view. The maximum thickness of the low refractive index layer 60 (i.e., the size in the Z direction between the surface 60a and the surface 20a) is appropriately determined according to the optical path length required for light incident on the microlens 31 from the front in the Z direction, etc.
[0042] The "low" of the low refractive index layer 60 means that it has a refractive index lower than at least the refractive index of the microlens 31. The closer the refractive index of the low refractive index layer 60 is to the refractive index of air, the greater the refractive index difference between the low refractive index layer 60 and the microlens 31 can be. As a result, the refraction of the light incident on the diffraction grating 70 from the front in the Z direction toward the direction opposite to the front in the Z direction can be suppressed, and the travel path of the light incident on the diffraction grating 70 is directed to a predetermined direction. As a result, the light is well focused on the CMOS image sensor 24 through the microlens 31, and the desired optical characteristics are obtained in the solid-state imaging element 10. The refractive index of the low refractive index layer 60 is appropriately adjusted by considering the type of low refractive index material described below and the content of the low refractive index material in the low refractive index layer 60.
[0043] The low refractive index layer 60 contains a hollow filler and a medium. The hollow filler and the medium have transparency at visible wavelengths, for example, having a total light transmittance of more than 90% with respect to light of visible wavelengths. The hollow filler helps to reduce the refractive index of the low refractive index layer 60. The medium is intercalated between the particles of the hollow filler, so that the hollow fillers are bonded to each other, and the low refractive index layer 60 is stabilized.
[0044] As a suitable material for the hollow filler, silicon dioxide (silica, SiO2) can be exemplified. The hollow filler composed of silicon dioxide is cheap and has high transparency and physical stability relative to visible wavelengths. By locating the hollow filler in the low refractive index layer, the air region is dispersed inside the low refractive index layer 60. As a result, the refractive index of the low refractive index layer 60 decreases, and as the content of the hollow filler increases, its refractive index approaches the value of air.
[0045] The diffraction grating 70 is periodically arranged on the surface 60a of the low refractive index layer 60 at predetermined intervals in the X direction and the Y direction. Light incident on the diffraction grating 70 from the front in the Z direction toward the direction opposite to the front in the Z direction is diffracted by the diffraction grating 70 near the surface 60a (i.e., the diffraction surface). That is, it is diffracted at a diffraction angle determined by the wavelength of the light and the pitch 70d of the diffraction grating 70 with respect to the normal line along the Z direction, and travels in different directions for each wavelength. The size 70g and the pitch 70d of the diffraction grating 70 in the X direction and the Y direction are appropriately designed in the following manner: the red, green, and blue color lights among the light diffracted by the diffraction grating 70 as described above are irradiated to the microlens 31 and the CMOS image sensor 24 which overlap with the color filter 28 that transmits the light of the red, green, and blue color wavelength bands in the Z direction.
[0046] The diffraction grating 70 has transparency in visible wavelengths, for example, has a total light transmittance of 90% or more with respect to light of visible wavelengths. The material of the diffraction grating 70 is not particularly limited as long as it is transparent with respect to light of visible wavelengths and can diffract incident light in a desired direction for each wavelength as described above. As described below, when the diffraction grating 70 is formed using patterning and photolithography, a material that can be further patterned is suitable for the material of the diffraction grating 70, and for example, a resin material containing acrylic resin can be cited.
[0047] Next, an example of a method for manufacturing the microlens array 30 will be described.
[0048] First, a plurality of microlenses 31 arranged in a two-dimensional array are formed (step A). As a method for forming the microlenses 31, for example, the following method can be cited: a high refractive index material to be the microlenses 31 is applied in layers at least on the surface 28a of the color filter 28, a photoresist layer is provided thereon, and a lens pattern formed by heat melting after a photolithography process is etched and transferred to the layer of the high refractive index material in the lower layer.
[0049] In step A, a plurality of microlenses 31 may be prepared by purchasing a lens sheet or the like having a plurality of microlenses arranged in an array.
[0050] Then, if Figure 2 As shown in the figure, a coating liquid containing a low refractive index material dispersed with a hollow filler and a medium is applied so as to cover the surface 20a of the substrate 20 exposed between the color filter 28 and the microlens 31 adjacent to each other in a plan view (step B), and the coating liquid is cured by heating to remove the solvent (step C). Thus, a low refractive index layer 60 consisting of only the low refractive index material is formed.
[0051] Then, if Figure 3 As shown, the material 72 of the diffraction grating 70 is coated with a predetermined thickness on the surface 60a of the low refractive index layer 60. The material 72 is a photosensitive patternable material that can realize the optical characteristics required for the diffraction grating 70 as described above, such as a resin material such as acrylic resin.
[0052] Then, if Figure 4 As shown in FIG. 1 , a photomask 80 is disposed on the material 72 coated on the surface 60a of the low refractive index layer 60 (i.e., in front of the Z direction) with a gap between the material 72. The photomask 80 has a pattern similar to the diffraction grating 70, for example, Figure 3As shown, a light shielding material 82 such as chromium (Cr) is provided only in the portion where the diffraction grating 70 is formed in the X direction and the Y direction. In the photomask 80, the portion other than the light shielding material 82 is formed of, for example, quartz (SiO2) etc., so that light (such as ultraviolet light etc.) used for pattern transfer in the photolithography process is transmitted in the Z direction.
[0053] Then, in Figure 4 In the arrangement shown in FIG. 1 , patterning of the material using the photomask 80 is performed. That is, the material 72 is exposed to light from the Z direction front of the photomask 80 toward the direction opposite to the Z direction front, and the pattern of the photomask 80 is transferred to the material 72. Through this process, the material 72 is exposed to light except for the portion overlapping with the light shielding material 82 in the Z direction. By removing the photomask 80 from the material 72 and removing the exposed portion of the material 72 using an appropriate chemical solution, the material 72 is exposed to light. Figure 1 As shown in FIG. 1 , a diffraction grating 70 is formed on the surface 60a of the low refractive index layer 60. By performing the above steps, a Figure 1 The solid-state imaging element 10 is shown with a microlens array 30 .
[0054] As described above, the inventors encountered a problem in which cracks were generated in the layer of material 72 or the completed diffraction grating 70 during the process of forming the low refractive index layer 60 on the microlens 31 and further forming the diffraction grating 70 thereon. Due to the generation of multiple cracks, a phenomenon of peeling of the layer formed on the low refractive index layer 60 was also confirmed. In addition, multiple spots were generated in a plan view of the low refractive index layer 60, which impaired the appearance and affected the performance as a sensor.
[0055] The inventors have conducted various studies and believe that the cause of the cracks is not the material of the material 72, but is likely to be in the low refractive index layer 60. In view of this, the inventors have made various changes to the composition of the low refractive index material and conducted studies, and as a result, it has been found that the arrangement of the filler in the low refractive index layer is the main cause of the above-mentioned problem.
[0056] When the amount of filler in the low refractive index layer is increased, there is an upper limit to the amount. In the upper limit state, the fillers are in contact with each other and are almost unable to move relative to each other. Since the basic shape of the filler is roughly spherical, it is believed that in the above upper limit state, the filler becomes close to Figure 5 Configuration of the face-centered cubic lattice structure shown.
[0057] When the low refractive index layer material is dispersed in a solvent to prepare a coating solution, the solvent penetrates into the interior of the hollow filler. This is because the silica constituting the shell of the hollow filler is relatively porous.
[0058] When the amount of hollow filler in the low refractive index layer material increases, the number of hollow fillers that are not covered by the medium and partially exposed increases on the surface of the low refractive index layer formed. In the process of the coating liquid drying to form a low refractive index layer, the solvent that penetrates into the interior of the hollow filler vaporizes and escapes from the hollow filler exposed to the surface. It is inferred that the solvent escapes not only from the exposed hollow filler, but also from the hollow filler that contacts with the exposed hollow filler and is located in the layer along the porous shell.
[0059] The above-mentioned vaporization does not cause any particular problem when no other layer is formed on the low refractive index layer. However, when other layers are formed on the low refractive index layer, a coating liquid for forming the layer is applied on the low refractive index layer. At this time, the solvent contained in the coating liquid of the other layer enters the interior of the exposed hollow filler.
[0060] Then, when heating is performed to complete other layers, the solvent that has entered the hollow filler will also be vaporized, but since the low refractive index layer is covered by other layers, there is almost no escape path for the vaporized solvent. As a result, it is believed that when the amount of vaporized solvent that escapes to the outside reaches a certain amount, cracks will be generated, causing the upper layer to break or peel off. In addition, part of the solvent remaining in the filler becomes one of the causes of spots.
[0061] In the above phenomenon, it is important that the fillers are in contact with each other. Therefore, by setting the content of the filler to such an extent that the arrangement of the filler in the low refractive index layer does not form the above face-centered cubic lattice structure, it is expected that cracks and spots can be reduced.
[0062] However, the face-centered cubic lattice structure is composed of all spheres that are true spheres of the same size (for example, Figure 5 The example shown is based on a true sphere with a radius a), but although the actual filler is spherical, the probability of a true sphere is low and the size also varies.
[0063] Therefore, it is actually very difficult to find the optimal filler content that can reduce the refractive index of the low refractive index layer as much as possible while preventing the filler from being arranged in the above-mentioned face-centered cubic lattice structure.
[0064] As a result of further research, the inventors found that by evaluating the planar image of the low refractive index layer, it is possible to easily determine whether the filler in the low refractive index layer is arranged close to a face-centered cubic lattice structure that is prone to cracks or spots. The steps are described below.
[0065] First, a scanning electron microscope (SEM) was used to obtain Figure 6 The plan image of the low refractive index layer 60 is shown. It can be confirmed that in the acquired plan image, the portion where the filler 61 exists tends to be bright, and the portion where the filler 61 does not exist tends to be dark.
[0066] Next, the plane image is binarized to obtain Figure 7 The shown binary planar image is of the low refractive index layer 60. As a binarization algorithm, various known algorithms can be used, and for example, Otsu's binarization (discriminant analysis method) can be preferably used.
[0067] exist Figure 7 In the binary plane image shown, the area where filler exists and the area where filler does not exist are roughly distinguished, but there is minute noise in each area. That is, there is black minute noise Nz1 in the area where filler exists, and there is white minute noise Nz2 in the area where filler does not exist.
[0068] These noises become obstacles when the area of each part is detected with high accuracy, so they are removed using a filter. As the filter, for example, a 3×3 median filter can be preferably used. Figure 8 The binary plane image from which noise has been removed by a 3×3 median filter is shown.
[0069] The inventors' research has shown that the ratio of white pixels in the binary planar image of the low refractive index layer after noise removal is a good indicator of the amount and arrangement of the filler contained in the low refractive index layer.
[0070] Using silica filler with an average particle size of 60nm, multiple samples of low refractive index layers with various contents were prepared. For each sample, a plane image based on SEM was obtained, and a binary plane image with noise removed was obtained using Otsu's binarization and a 3×3 median filter. After obtaining the SEM image, a diffraction grating material was applied to the low refractive index layer, and the presence or absence of spots was visually confirmed. The results are shown in Table 1.
[0071] [Table 1]
[0072] White pixel ratio (%) Produce spots Sample 1 67.7 none Sample 2 69.2 none Sample 3 70.4 none Sample 4 72.6 none Sample 5 74.1 none Sample 6 75.3 none Sample 7 76.9 have Sample 8 82.1 have Sample 9 84.2 have Sample 10 86.5 have
[0073] As shown in Table 1, when the ratio of white pixels in the binary planar image of the low refractive index layer from which noise has been removed is 76% or less, no spots are observed, indicating that the white pixel ratio is a suitable indicator for preventing spots or cracks. The refractive index of the low refractive index layer in the sample without spots in Table 1 is 1.27 or more, and by setting the ratio of white pixels to 67% or more, it is shown that both a sufficiently low refractive index and the prevention of spots and cracks can be achieved. From the perspective of obtaining a sufficient refractive index difference with the microlens, the refractive index of the low refractive index layer is preferably 1.35 or less.
[0074] Note that in Table 1, samples 1 to 10 are arranged in numerical order of white pixel ratio, but not in order of filler content, indicating that the white pixel ratio is an index independent of the filler content in the low refractive index layer.
[0075] Above, one embodiment of the present invention has been described in detail, but the present invention is not limited to a specific embodiment, and also includes changes and combinations of the configurations within the scope of the present invention. Some changes are exemplified below, but these are not all, and other changes may also be made. These changes may also be appropriately combined with two or more.
[0076] In the above embodiment, an on-chip solid-state imaging element in which a color filter is directly formed on a substrate is shown, but the scope of application of the technical concept involved in the present invention is not limited thereto, and can be widely applied to a microlens array in which a low refractive index layer containing a hollow filler is formed on a microlens and other layers are further formed thereon. Therefore, for example, it can also be applied to a lens sheet configured on an organic EL (OLED), etc.
[0077] Organic EL is sometimes covered by a cover layer such as glass. In this case, when a microlens is formed on the organic EL, it is possible that the lens peels off from the cover layer due to the unevenness of the lens. Therefore, it is preferred to provide a low refractive index layer between the microlens and the cover layer. In this case, the organic EL, the color filter, the microlens array of the present invention (microlens and low refractive index layer), and the cover layer such as glass are stacked in sequence to form a layer structure. Even in this case, the generation of spots and cracks can be suppressed by adopting the present invention.
[0078] The functional layer formed on the low refractive index layer is not limited to the above-mentioned diffraction grating, and the technical concept of the present invention can be applied to all layers formed using a coating liquid containing a solvent, such as an anti-glare layer and an anti-fouling layer. Although not a layer formed using a coating liquid, the above-mentioned cover layer is also a form of a functional layer.
[0079] The material of the hollow filler is not limited to silica, and resin fillers and the like may also be used. However, the technical concept of the present invention is particularly effective when the shell of the hollow filler is a porous silica filler and the like.
[0080] Industrial Applicability
[0081] According to the present invention, it is possible to provide a microlens array which includes a low refractive index layer to suppress interface reflection and on which other layers can be appropriately formed.
[0082] Explanation of symbols
[0083] 10 Solid-state imaging element
[0084] 30 Microlens Array
[0085] 31 Microlens
[0086] 60 Low refractive index layer
[0087] 70 Diffraction grating (functional layer)
Claims
1. A microlens array, which is a microlens array in which a plurality of microlenses are arranged and configured, A low refractive index layer is provided, which contains a hollow filler and a medium and is formed on the plurality of microlenses and has a refractive index smaller than that of the plurality of microlenses. In the low refractive index layer, a ratio of white pixels in a binary planar image is 76% or less.
2. The microlens array according to claim 1, in, The ratio of white pixels is 67% or more.
3. The microlens array according to claim 1, The invention further comprises a functional layer formed on the low refractive index layer.