Polishing liquid for CMP, polishing liquid set for CMP, and polishing method
By using a polishing liquid containing cerium hydroxide and specific additives in the CMP process, the problem of uneven polishing of insulating materials is solved, and efficient polishing control is achieved, especially the polishing speed suppression on the polycrystalline silicon and amorphous silicon barrier layers is suppressed. .
Patent Information
- Application Number
- CN202480002328.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-01
- Filing Date
- 2024-01-26
- Publication Date
- 2024-12-06
AI Technical Summary
In the CMP process, it is difficult to control the amount of the insulating material, especially when polycrystalline silicon and amorphous silicon are used as the stop layers, it is difficult to suppress the grinding speed of the stop layer, resulting in uneven grinding.
A CMP abrasive solution containing abrasive particles, an additive A having an ethylenediamine structure bonded with a hydroxyalkyl group or an alkoxy group, and a cationic polymer is used, and cerium hydroxide is added as abrasive particles to the abrasive solution. Combined with additives such as 2,2',2",2"'-ethylenedinitrotetraethanol or 1,1',1",1"'-ethylenediaminetetra-2-propanol, forming excellent grinding Performance abrasive set.
A high grinding speed of insulating material is achieved, while suppressing the grinding speed of polycrystalline silicon and amorphous silicon, improving the controllability and efficiency of the grinding process.
Smart Images

Figure BDA0005103021850000081 
Figure BDA0005103021850000261 
Figure BDA0005103021850000262
Abstract
Description
Technical Field
[0001] The present invention relates to a CMP polishing liquid, a CMP polishing liquid kit, a polishing method and the like. Background Art
[0002] In recent years, the importance of processing technologies for high density and miniaturization has been increasing in the manufacturing process of electronic devices. CMP (Chemical Mechanical Polishing) technology, which is one of the processing technologies, has become a technology required for the formation of shallow trench isolation (STI), planarization of pre-metal insulating materials or interlayer insulating materials, and formation of plugs or buried metal wiring in the manufacturing process of electronic devices. As a CMP polishing liquid used for CMP, a CMP polishing liquid containing abrasive grains containing cerium oxide is known (for example, refer to the following patent documents 1 and 2).
[0003] Previous technical literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 10-106994
[0006] Patent Document 2: Japanese Patent Application Laid-Open No. 08-022970 Summary of the invention
[0007] Technical issues to be solved by the invention
[0008] As one of the methods for stopping grinding at a predetermined position in a CMP process, a stopper layer (grinding stop member. Member including a stopper layer) is sometimes used. In one example of a CMP process using a stopper layer, a substrate having a concave-convex pattern, a stopper layer disposed on the convex portion of the substrate, and a base of an insulating material (e.g., silicon oxide, silicon nitride) disposed on the substrate and the stopper layer in a manner to fill the concave portion are ground to remove unnecessary portions of the insulating material. This is because it is difficult to control the grinding amount of the insulating material (the amount of insulating material removed), and the degree of grinding is controlled by grinding the insulating material until the stopper layer is exposed. In this type of grinding, it is necessary to grind the insulating material at a high grinding speed while suppressing the grinding speed of the stopper layer. In recent years, as polycrystalline silicon and amorphous silicon are increasingly used as stopper layers, it is necessary to suppress the grinding speed of polycrystalline silicon and amorphous silicon, for example.
[0009] The present invention is made in view of such a situation, and its object is to provide a polishing liquid that can polish insulating materials at a high polishing rate while suppressing the polishing rates of polycrystalline silicon and amorphous silicon. The present invention is to provide a polishing liquid set for obtaining the polishing liquid. The present invention is to provide a polishing method using the polishing liquid or the polishing liquid set.
[0010] Means for solving technical problems
[0011] The present invention, in several aspects, relates to the following [1] to
[17] and the like.
[0012] [1] A CMP polishing liquid comprising abrasive grains, an additive A, a cationic polymer and water,
[0013] The additive A includes a compound having an ethylenediamine structure to which a hydroxyalkyl group or an alkoxy group is bonded.
[0014] [2] The CMP polishing liquid according to [1], wherein
[0015] The abrasive grains include at least one selected from the group consisting of cerium hydroxide, cerium oxide, silicon dioxide, and aluminum oxide.
[0016] [3] The CMP polishing liquid according to [1] or [2], wherein
[0017] The abrasive grains contain cerium hydroxide.
[0018] [4] The CMP polishing liquid according to any one of [1] to [3], wherein
[0019] The additive A comprises 2,2',2",2"'-ethylenediyldinitrotetraethanol.
[0020] [5] The CMP polishing liquid according to any one of [1] to [4], wherein
[0021] The additive A comprises 1,1',1",1"'-ethylenediaminetetra-2-propanol.
[0022] [6] The CMP polishing liquid according to any one of [1] to [5], wherein
[0023] The content of the additive A is 0.001 to 5% by mass.
[0024] [7] The CMP polishing liquid according to any one of [1] to [6], wherein
[0025] The cationic polymer includes a polymer having a quaternary ammonium salt structure or a polymer having an amino group.
[0026] [8] The CMP polishing liquid according to any one of [1] to [7], wherein
[0027] The content of the cationic polymer is 2 to 20 parts by mass based on 100 parts by mass of the additive A.
[0028] [9] The CMP polishing liquid according to any one of [1] to [8], further comprising a polyether.
[0029]
[10] The CMP polishing liquid according to any one of [1] to [9], wherein the pH thereof is 4.0 to 10.0.
[0030]
[11] The CMP polishing liquid according to any one of [1] to
[10] , wherein the pH thereof is greater than 6.0 and less than 9.0.
[0031]
[12] The CMP polishing liquid according to any one of [1] to
[11] , which is used for polishing a surface to be polished including silicon oxide, silicon nitride, polycrystalline silicon and amorphous silicon.
[0032]
[13] A CMP polishing liquid kit, wherein:
[0033] The CMP polishing liquid according to any one of [1] to
[12] is stored as a first liquid and a second liquid, wherein the first liquid contains the abrasive and water, and the second liquid contains the additive A, a cationic polymer, and water.
[0034]
[14] A polishing method comprising the step of polishing a surface to be polished using the CMP polishing liquid according to any one of [1] to
[12] .
[0035]
[15] The grinding method according to
[14] , wherein:
[0036] The polished surface includes silicon oxide, silicon nitride, polycrystalline silicon and amorphous silicon.
[0037]
[16] A polishing method comprising the step of polishing a surface to be polished using a CMP polishing liquid obtained by mixing the first liquid and the second liquid in the CMP polishing liquid set according to
[13] .
[0038]
[17] The grinding method according to
[16] , wherein:
[0039] The polished surface includes silicon oxide, silicon nitride, polycrystalline silicon and amorphous silicon.
[0040] Effects of the Invention
[0041] According to one aspect of the present invention, a polishing liquid capable of polishing an insulating material at a high polishing speed while suppressing the polishing speed of a stopper layer can be provided. According to another aspect of the present invention, a polishing liquid set for obtaining the polishing liquid can be provided. According to another aspect of the present invention, a polishing method using the polishing liquid or the polishing liquid set can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic cross-sectional view showing a polishing step when forming an STI structure of a semiconductor. DETAILED DESCRIPTION
[0043] Hereinafter, embodiments of the present invention will be described in detail.
[0044] In this specification, the numerical range represented by "~" is used to represent the range in which the numerical values recorded before and after "~" are included as the minimum and maximum values, respectively. "Above A" in the numerical range represents A and the range exceeding A. "Below A" in the numerical range represents A and the range less than A. In the numerical range described in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range of other stages. In the numerical range described in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment. "A or B" can include either A or B, or both. The materials exemplified in this specification can be used alone or in combination of two or more, unless otherwise specified. In the case where there are multiple substances equivalent to each component in the composition, the content of each component in the composition represents the total amount of the multiple substances present in the composition, unless otherwise specified. The term "layer" or "film" includes a structure formed in a shape of a part in addition to a structure formed in a shape formed on the entire surface when observed as a top view. The term "process" does not only include independent processes, but also includes processes that cannot be clearly distinguished from other processes as long as the intended effect of the process can be achieved.
[0045] <Polishing fluid for CMP>
[0046] The CMP polishing liquid according to the present embodiment is a CMP polishing liquid (hereinafter, sometimes simply referred to as “polishing liquid”) containing abrasive grains, additive A, a cationic polymer, and water. Additive A includes a compound having an ethylenediamine structure to which a hydroxyalkyl group or an alkoxy group is bonded.
[0047] According to the CMP polishing liquid according to the present embodiment, it is possible to polish the insulating material at a high polishing rate while suppressing the polishing rates of polycrystalline silicon and amorphous silicon.
[0048] According to the CMP polishing liquid involved in this embodiment, for example, silicon oxide can be polished at a high polishing speed. In the evaluation method described in the examples described later, the polishing speed of silicon oxide can be, for example, 120nm / min or more, 140nm / min or more, 160nm / min or more, 180nm / min or more, 200nm / min or more, 220nm / min or more, 230nm / min or more, 240nm / min or more, 250nm / min or more, 260nm / min or more, 270nm / min or more, or 280nm / min or more.
[0049] According to the CMP polishing liquid involved in this embodiment, for example, silicon nitride can be polished at a high polishing speed. In the evaluation method described in the embodiments described later, the polishing speed of silicon nitride can be, for example, 30 nm / min or more, 40 nm / min or more, 50 nm / min or more, 60 nm / min or more, 70 nm / min or more, or 80 nm / min or more.
[0050] According to the CMP polishing liquid involved in this embodiment, for example, the polishing rate of polycrystalline silicon can be suppressed. In the evaluation method described in the embodiments described later, the polishing rate of polycrystalline silicon can be, for example, less than 60nm / min, less than 50nm / min, less than 40nm / min, less than 30nm / min, less than 20nm / min, less than 10nm / min, less than 5nm / min, less than 3nm / min, or less than 2nm / min.
[0051] According to the CMP polishing liquid involved in this embodiment, for example, the polishing rate of amorphous silicon can be suppressed. In the evaluation method described in the embodiments described later, the polishing rate of amorphous silicon can be, for example, less than 5 nm / min, less than 4 nm / min, less than 3 nm / min, less than 2 nm / min, less than 1.5 nm / min, less than 1 nm / min, or less than 0.5 nm / min.
[0052] Although the main reasons for exerting these effects are not yet clear, they are speculated to be as follows. However, the main reasons are not limited to the following. That is, the CMP polishing liquid involved in this embodiment includes a cationic polymer, and the cationic polymer is adsorbed on polycrystalline silicon and amorphous silicon. As a result, the grinding of polycrystalline silicon and amorphous silicon based on abrasive particles is suppressed, so that the grinding speed of polycrystalline silicon and amorphous silicon can be suppressed. In addition, additive A has a tendency to have a high affinity with any one of insulating materials (silicon oxide, silicon nitride, etc.), polycrystalline silicon and amorphous silicon, but cationic polymers protect polycrystalline silicon and amorphous silicon. Therefore, the CMP polishing liquid involved in this embodiment includes additive A, and the ethylenediamine structure of additive A is selectively adsorbed on the insulating material. As a result, the hydroxyalkyl or alkoxy group of additive A is exposed on the surface, making the insulating material hydrophilic, improving its affinity with abrasive particles, thereby making it easy to be ground, and achieving a high grinding speed of the insulating material.
[0053] (Abrasive particles)
[0054] The CMP polishing liquid involved in this embodiment contains abrasive grains. From the viewpoint of polishing the insulating material at a higher polishing speed, the abrasive grains may include an inorganic compound, or may include at least one selected from the group consisting of hydroxides of metal elements (e.g., cerium hydroxide), cerium oxides (e.g., Ceria (cerium (IV) oxide)), silicon dioxide, aluminum oxide, zirconium oxide, and yttrium oxide, or may include at least one selected from the group consisting of cerium hydroxide, cerium oxide, silicon dioxide, and aluminum oxide, or may include cerium hydroxide.
[0055] The hydroxide of a metal element may be a hydroxide of a tetravalent metal element. "Tetravalent metal element hydroxide" refers to a hydroxide containing a tetravalent metal (M 4+ ) and at least one hydroxide ion (OH - The hydroxide of a tetravalent metal element may contain anions other than hydroxide ions (e.g., nitrate ions, NO3 - and sulfate ion SO4 2- For example, the hydroxide of a tetravalent metal element may include an anion (e.g., a nitrate ion, NO3 - and sulfate ion SO4 2- The hydroxide of a tetravalent metal element can be produced by reacting a salt of a tetravalent metal element (metal salt) with an alkali source (base).
[0056] From the viewpoint of grinding insulating materials at a higher grinding speed, and from the viewpoint of further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the abrasive grains may contain cerium hydroxide (cerium hydroxide). Cerium hydroxide can be made by reacting a cerium salt with an alkali source (base). Cerium hydroxide can be made by mixing a cerium salt and an alkali solution (e.g., an alkali aqueous solution). Thus, particles with extremely fine particle sizes can be obtained, and an excellent effect of reducing grinding scratches can be easily obtained. Cerium hydroxide can be obtained by mixing a cerium salt solution (e.g., an cerium salt aqueous solution) and an alkali solution. As cerium salts, Ce(NO3)4, Ce(SO4)2, Ce(NH4)2(NO3)6, Ce(NH4)4(SO4)4, etc. can be cited.
[0057] When cerium hydroxide is used as the tetravalent cerium hydroxide, it is considered that the cerium hydroxide containing tetravalent cerium (Ce) is generated depending on the production conditions of cerium hydroxide. 4+ ), 1 to 3 hydroxide ions (OH - ) and 1 to 3 anions (X c- ) composed of Ce(OH) a X b (where a+b×c=4) (in addition, such particles are also cerium hydroxide). a X b In the present invention, it is considered that the electron-attracting anion (X c- ) acts to increase the reactivity of hydroxide ions, and as Ce(OH) a X b As the amount of anion (X c- ), NO3 can be cited - 、SO4 2- It is believed that the particles containing cerium hydroxide contain not only Ce(OH) a X b , and can also contain Ce(OH)4, CeO2, etc.
[0058] The particles comprising cerium hydroxide comprise Ce(OH) a X b The situation can be confirmed by the following method: after the particles are fully washed with pure water, the anion (X) equivalent is detected by FT-IR ATR method (Fourier transform Infra Red Spectrometer Attenuated Total Reflection: Fourier transform infrared spectrometer Attenuated Total Reflection measurement method). c- ) peak. It is also possible to confirm the anion (Xc- )’s existence.
[0059] In the case where the abrasive contains cerium hydroxide, from the viewpoint of grinding insulating materials at a higher grinding speed and from the viewpoint of further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the lower limit of the cerium hydroxide content is based on the abrasive as a whole (the abrasive as a whole contained in the CMP polishing liquid. The same below), and can be 50 mass% or more, more than 50 mass%, 60 mass% or more, 70 mass% or more, 80 mass% or more, 90 mass% or more, 95 mass% or more, or 100 mass% (substantially formed from cerium hydroxide).
[0060] From the viewpoint of grinding insulating materials at a higher grinding speed, the lower limit of the average particle size of the abrasive grains in the slurry in the CMP polishing liquid or the CMP polishing liquid set described later can be 1 nm or more, 2 nm or more, 3 nm or more, 4 nm or more, 5 nm or more, more than 5 nm, 6 nm or more, 7 nm or more, 7.5 nm or more, or 8 nm or more. From the viewpoint of easily suppressing the generation of scratches on the polished surface, the upper limit of the average particle size of the abrasive grains can be 200 nm or less, 150 nm or less, 100 nm or less, 70 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 28 nm or less, 26 nm or less, 25 nm or less, 20 nm or less, 15 nm or less, 12 nm or less, 11 nm or less, 10 nm or less, less than 10 nm, 9 nm or less, 8.5 nm or less, or 8 nm or less. The lower limit of the average particle size of the abrasive grains may be 10 nm or more, 15 nm or more, 18 nm or more, 20 nm or more, 22 nm or more, 24 nm or more, or 25 nm or more. From these viewpoints, the average particle size of the abrasive grains may be 1 to 200 nm, 1 to 150 nm, or 1 to 60 nm.
[0061] The "average particle size" of the abrasive grains refers to the average secondary particle size of the abrasive grains. For example, the average particle size of the abrasive grains is the volume average particle size, and the CMP polishing liquid or the slurry in the CMP polishing liquid kit described later can be measured using a light diffraction scattering particle size distribution meter (for example, manufactured by Beckman Coulter, Inc., product name: DelsaMax PRO, manufactured by Malvern Instruments, product name: Zetasizer 3000HSA).
[0062] The content of abrasive grains can be the following ranges based on the total mass of the CMP polishing liquid. From the viewpoint of polishing the insulating material at a higher polishing speed, the lower limit of the content of abrasive grains can be 0.001 mass %, 0.005 mass %, 0.01 mass %, 0.02 mass %, 0.03 mass %, 0.035 mass %, 0.04 mass %, 0.045 mass %, or 0.05 mass %. From the viewpoint of further suppressing the polishing speed of polycrystalline silicon and amorphous silicon, and the viewpoint of easily obtaining excellent dispersion stability of abrasive grains, the upper limit of the content of abrasive grains can be 20 mass %, 15 mass %, 10 mass %, 5 mass %, 1 mass %, 0.5 mass %, 0.1 mass %, 0.09 mass %, 0.08 mass %, 0.07 mass %, 0.06 mass %, or 0.05 mass %. From these viewpoints, the content of the abrasive grains may be 0.001 to 20% by mass, or 0.01 to 10% by mass.
[0063] (additive)
[0064] [Additive A]
[0065] The CMP polishing liquid according to the present embodiment contains an additive A. The additive A contains a compound having an ethylenediamine structure to which a hydroxyalkyl group or an alkoxy group is bonded.
[0066] Additive A has at least one hydroxyalkyl or alkoxy group bonded to the ethylenediamine structure. Hydroxyalkyl represents an alkyl group substituted with a hydroxyl group. Alkoxy represents a functional group in which the hydrogen atom of the hydroxyl group in the hydroxyalkyl group is replaced by a metal atom (e.g., a sodium atom). In the case where additive A has multiple hydroxyalkyl groups, in a part of the hydroxyalkyl groups in the multiple hydroxyalkyl groups, the hydrogen atom of the hydroxyl group is replaced by a metal atom (e.g., a sodium atom) to become an alkoxy group. The hydroxyalkyl or alkoxy group may be directly bonded to the nitrogen atom of the ethylenediamine structure. In the case where additive A has multiple hydroxyalkyl or alkoxy groups, additive A may be a compound having an ethylenediamine structure bonded with a hydroxyalkyl or alkoxy group, and having more than two nitrogen atoms bonded with a hydroxyalkyl or alkoxy group. The hydroxyalkyl group may have a substituent other than a hydroxyl group, or may not have a substituent. The alkoxy group may further have a substituent, or may not have a substituent.
[0067] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the number of carbon atoms of the alkyl group in the hydroxyalkyl group or the alkoxy group may be in the following ranges. The number of carbon atoms of the alkyl group in the hydroxyalkyl group or the alkoxy group may be 10 or less, 8 or less, 6 or less, 5 or less, 4 or less, or 3 or less. The number of carbon atoms of the alkyl group in the hydroxyalkyl group or the alkoxy group may be 1 or more, 2 or more, or 3 or more. From these viewpoints, the number of carbon atoms of the alkyl group in the hydroxyalkyl group or the alkoxy group may be 1 to 10, or 1 to 5.
[0068] The number of hydroxyl groups in the hydroxyalkyl group may be greater than 1. From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the number of hydroxyl groups in the hydroxyalkyl group may be less than 10, less than 8, less than 6, less than 4, less than 3, or less than 2.
[0069] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the total number of hydroxyalkyl groups and alkoxy groups possessed by the additive A may be in the following ranges. The total number of hydroxyalkyl groups and alkoxy groups possessed by the additive A may be 1 or more, 2 or more, 3 or more, or 4 or more. The total number of hydroxyalkyl groups and alkoxy groups possessed by the additive A may be 10 or less, 8 or less, 6 or less, 5 or less, or 4 or less.
[0070] From the perspective of polishing insulating materials at a higher polishing speed and further suppressing the polishing speed of polycrystalline silicon and amorphous silicon, additive A can be a compound having a nitrogen atom bonded to two hydroxyalkyl or alkoxy groups, or a compound having two nitrogen atoms bonded to two hydroxyalkyl or alkoxy groups.
[0071] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the number of ethylenediamine structures in one molecule of the additive A may be 1 to 3, 1 to 2, or 1.
[0072] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the additive A may contain a compound represented by the following general formula (1).
[0073]
[0074] [Where R 1 , R 2 , R 3 and R 4 Each independently represents a hydrogen atom or an organic group, R 1 , R 2 , R 3and R 4 At least one of them is a hydroxyalkyl group or an alkoxy group.]
[0075] The organic group may be a substituted or unsubstituted alkyl group, or a hydroxyalkyl group or an alkoxy group. As a substituent of the alkyl group, a carboxyl group, an amino group, a sulfo group, a nitro group, etc. may be mentioned. From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the number of carbon atoms in the alkyl group may be 10 or less, 8 or less, 6 or less, 5 or less, 4 or less, or 3 or less, or 1 or more, 2 or more, or 3 or more.
[0076] Examples of the additive A include 1,1',1",1"'-ethylenediaminetetra-2-propanol, 2,2',2",2"'-ethylenediyldinitrotetraethanol, N-(2-hydroxypropyl)ethylenediamine, and ethylenediaminetetrapolyoxyalkylene (ethylenediaminetetrapolyoxyethylene, ethylenediaminepolyoxypropylene, and the like). From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the additive A may include at least one selected from the group consisting of 1,1',1",1"'-ethylenediaminetetra-2-propanol, 2,2',2",2"'-ethylenediyldinitrotetraethanol, N-(2-hydroxypropyl)ethylenediamine, and polyoxyalkylethylenediamine, or may include at least one selected from the group consisting of 1,1',1",1"'-ethylenediaminetetra-2-propanol and 2,2',2",2"'-ethylenediyldinitrotetraethanolethylenediyldinitrotetraethanol, or may include 1,1',1",1"'-ethylenediaminetetra-2-propanol or 2,2',2",2"'-ethylenediyldinitrotetraethanolethylenediyldinitrotetraethanol. The additive A may not include ethylenediaminetetrapolyoxyalkylene.
[0077] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the molecular weight of the additive A may be in the following ranges. The molecular weight of the additive A may be 100 or more, 120 or more, 140 or more, 160 or more, 180 or more, 200 or more, 220 or more, 230 or more, 240 or more, 250 or more, 260 or more, 270 or more, 280 or more, or 290 or more. The molecular weight of the additive A may be 1000 or less, less than 1000, 900 or less, 800 or less, 700 or less, 600 or less, 500 or less, 400 or less, 380 or less, 360 or less, 350 or less, 340 or less, 330 or less, 320 or less, 310 or less, 300 or less, or less than 300. From these viewpoints, the molecular weight of the additive A may be 100 to 1000, 160 to 500, or 200 to 350.
[0078] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the content of additive A, or the content of additive A, based on the total mass of the CMP polishing liquid, can be in the following ranges. The content of additive A, or the content of additive A can be 0.001 mass % or more, 0.003 mass % or more, 0.005 mass % or more, 0.01 mass % or more, more than 0.01 mass %, 0.015 mass % or more, 0.02 mass % or more, more than 0.02 mass %, 0.025 mass % or more, 0.03 mass % or more, more than 0.03 mass %, 0.035 mass % or more, or 0.04 mass % or more. The content of additive A, or the content of additive A, can be 5% by mass or less, 3% by mass or less, 1% by mass or less, 0.5% by mass or less, 0.3% by mass or less, 0.2% by mass or less, 0.15% by mass or less, 0.12% by mass or less, 0.1% by mass or less, less than 0.1% by mass, 0.09% by mass or less, 0.08% by mass or less, 0.07% by mass or less, 0.06% by mass or less, 0.055% by mass or less, 0.05% by mass or less, less than 0.05% by mass, 0.045% by mass or less, or 0.04% by mass or less. From these viewpoints, the content of additive A, or the content of additive A, can be 0.001 to 5% by mass, 0.005 to 1% by mass, 0.01 to 0.5% by mass, 0.02 to 0.2% by mass, or 0.02 to 0.12% by mass.
[0079] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the content of additive A or the content of additive A may be in the following ranges relative to 100 parts by mass of the abrasive grains. The content of additive A or the content of additive A may be 1 part by mass or more, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, 45 parts by mass or more, 50 parts by mass or more, 55 parts by mass or more, 60 parts by mass or more, 65 parts by mass or more, 70 parts by mass or more, 75 parts by mass or more, or 80 parts by mass or more. The content of additive A or the content of additive A can be 1000 parts by mass or less, 800 parts by mass or less, 600 parts by mass or less, 400 parts by mass or less, 350 parts by mass or less, 300 parts by mass or less, 240 parts by mass or less, 200 parts by mass or less, 190 parts by mass or less, 180 parts by mass or less, 170 parts by mass or less, 160 parts by mass or less, 150 parts by mass or less, 140 parts by mass or less, 130 parts by mass or less, 120 parts by mass or less, 110 parts by mass or less, 100 parts by mass or less, 90 parts by mass or less, or 80 parts by mass or less. From these viewpoints, the content of additive A or the content of additive A can be 1 to 1000 parts by mass, 10 to 600 parts by mass, 20 to 400 parts by mass, 40 to 240 parts by mass, or 20 to 160 parts by mass.
[0080] [Cationic polymer]
[0081] The CMP polishing liquid involved in this embodiment contains a cationic polymer. "Cationic polymer" is defined as a polymer having a cationic group or a group that can be ionized into a cationic group in the main chain or side chain. Examples of the cationic group include amino, imino, cyano, etc.
[0082] Examples of cationic polymers include polymers obtained by polymerizing at least one monomer component selected from the group consisting of allylamine, diallylamine, vinylamine, ethyleneimine, and derivatives thereof (allylamine polymers, diallylamine polymers, vinylamine polymers, ethyleneimine polymers); polysaccharides such as chitosan and chitosan derivatives, etc. Cationic polymers may include polymers having a quaternary ammonium salt structure or polymers having an amino group.
[0083] The allylamine polymer is a polymer obtained by polymerizing allylamine or its derivatives. Examples of the allylamine derivatives include alkoxycarbonylated allylamine, methylcarbonylated allylamine, aminocarbonylated allylamine, and ureidated allylamine.
[0084] Diallylamine polymers are polymers obtained by polymerizing diallylamine or its derivatives. Examples of diallylamine derivatives include methyldiallylamine, diallyldimethylammonium salt, diallylmethylethylammonium salt, acylated diallylamine, aminocarbonylated diallylamine, alkoxycarbonylated diallylamine, aminothiocarbonylated diallylamine, and hydroxyalkylated diallylamine. Examples of ammonium salts include ammonium chloride, alkylammonium sulfate (e.g., ethylammonium sulfate), and the like.
[0085] The vinylamine polymer is a polymer obtained by polymerizing vinylamine or its derivatives. Examples of the vinylamine derivatives include alkylated vinylamine, amidated vinylamine, oxiraneated vinylamine, propylene oxide vinylamine, alkoxylated vinylamine, carboxymethylated vinylamine, acylated vinylamine, and urea-dextrinated vinylamine.
[0086] The ethyleneimine polymer is a polymer obtained by polymerizing ethyleneimine or its derivatives. Examples of the ethyleneimine derivatives include aminoethylated acrylic acid polymers, alkylated ethyleneimine, ureidated ethyleneimine, and propylene oxide-added ethyleneimine.
[0087] The cationic polymer may have a structural unit derived from a monomer component other than allylamine, diallylamine, vinylamine, ethyleneimine, and derivatives thereof. For example, the cationic polymer may have a structural unit derived from acrylamide, dimethylacrylamide, diethylacrylamide, hydroxyethylacrylamide, acrylic acid, methyl acrylate, methacrylic acid, methyl methacrylate, 2-(dimethylamino)ethyl methacrylate, maleic acid, epichlorohydrin, or sulfur dioxide.
[0088] The cationic polymer may be a homopolymer of allylamine, diallylamine, vinylamine or ethyleneimine (polyallylamine, polydiallylamine, polyethyleneamine or polyethyleneimine), or a copolymer having a structural unit derived from allylamine, diallylamine, vinylamine, ethyleneimine or a derivative thereof. In the copolymer, the arrangement of the structural units is arbitrary. For example, any form may be taken, such as (a) a block copolymerization form in which various structural units of the same type are continuously present, (b) a random copolymerization form in which structural units A and structural units B are particularly randomly arranged, (c) an alternating copolymerization form in which structural units A and structural units B are alternately arranged.
[0089] From the viewpoint of grinding insulating materials at a higher grinding speed and further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the cationic polymer may be a copolymer obtained by polymerizing a composition containing acrylamide as a monomer component. From the viewpoint of grinding insulating materials at a higher grinding speed and further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the cationic polymer may be a copolymer obtained by polymerizing a composition containing diallyldimethylammonium salt and acrylamide as monomer components, or a copolymer obtained by polymerizing a composition containing diallylamine hydrochloride and acrylamide as monomer components. From the viewpoint of grinding insulating materials at a higher grinding speed and further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the cationic polymer may be a diallyldimethylammonium chloride-acrylamide copolymer, or a diallylamine hydrochloride-acrylamide copolymer.
[0090] From the viewpoint of polishing insulating materials at a higher polishing speed and further suppressing the polishing speed of polycrystalline silicon and amorphous silicon, the cationic polymer may be a copolymer obtained by polymerizing a composition containing epichlorohydrin as a monomer component. From the viewpoint of polishing insulating materials at a higher polishing speed and further suppressing the polishing speed of polycrystalline silicon and amorphous silicon, the cationic polymer may be a polycondensate obtained by polycondensing a composition containing dimethylamine, ammonia and epichlorohydrin as monomer components, or a modified polymer obtained by modifying and polymerizing a composition containing methyldiallylamine hydrochloride and epichlorohydrin as monomer components. From the viewpoint of polishing insulating materials at a higher polishing speed and further suppressing the polishing speed of polycrystalline silicon and amorphous silicon, the cationic polymer may be a polycondensate of dimethylamine / ammonia / epichlorohydrin or a modified polymer of methyldiallylamine hydrochloride / epichlorohydrin.
[0091] From the viewpoint of polishing insulating materials at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the cationic polymer may be a copolymer obtained by polymerizing a composition containing 2-(dimethylamino)ethyl methacrylate as a monomer component, or a copolymer obtained by polymerizing a composition containing vinyl pyrrolidone and 2-(dimethylamino)ethyl methacrylate as monomer components, or a vinyl pyrrolidone-N,N-dimethylaminoethyl methacrylate copolymer diethyl sulfate.
[0092] From the viewpoint of polishing insulating materials at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the cationic polymer may be an amine polymer such as an allylamine polymer, a diallylamine polymer, and a vinylamine polymer, or may be at least one selected from the group consisting of polyallylamine and diallyldimethylammonium chloride. For the purpose of adjusting polishing properties such as polishing selectivity and flatness, the cationic polymer may be used alone or in combination of two or more.
[0093] From the viewpoint of grinding insulating materials at a higher grinding speed and further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the lower limit of the weight average molecular weight of the cationic polymer may be 100 or more, 300 or more, 500 or more, 1000 or more, or 1500 or more. From the viewpoint of grinding insulating materials at a higher grinding speed and further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the upper limit of the weight average molecular weight of the cationic polymer may be 1000000 or less, 800000 or less, 600000 or less, 300000 or less, or 200000 or less. From these viewpoints, the weight average molecular weight of the cationic polymer may be 100 to 1000000, or 500 to 300000. The weight average molecular weight of the cationic polymer can be measured, for example, by gel permeation chromatography (GPC) under the following conditions using a calibration curve of standard polystyrene.
[0094] Equipment used: Hitachi L-6000 [manufactured by Hitachi, Ltd.]
[0095] Column: Gel Pak GL-R420 + Gel Pak GL-R430 + Gel Pak GL-R440 [product name manufactured by Hitachi High-Tech Corporation, 3 in total]
[0096] Eluent: Tetrahydrofuran
[0097] Measurement temperature: 40℃
[0098] Flow rate: 1.75mL / min
[0099] Detector: L-3300RI [manufactured by Hitachi, Ltd.]
[0100] From the viewpoint of grinding insulating materials with a higher grinding speed, and further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the content of the cationic polymer is based on the total mass of the CMP polishing liquid, and can be within the following range. The content of the cationic polymer can be 0.0001 mass %, 0.0005 mass %, 0.001 mass %, 0.0015 mass %, 0.002 mass %, 0.0025 mass %, or 0.003 mass %. The content of the cationic polymer can be 5 mass %, 1 mass %, 0.1 mass %, 0.05 mass %, 0.01 mass %, 0.008 mass %, 0.006 mass %, 0.005 mass %, 0.0045 mass %, 0.004 mass %, or 0.003 mass %. From these viewpoints, the content of the cationic polymer may be 0.0001 to 5% by mass, 0.001 to 0.1% by mass, or 0.002 to 0.01% by mass.
[0101] From the viewpoint of grinding insulating materials at a higher grinding speed and further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the content of the cationic polymer can be in the following ranges relative to 100 parts by mass of abrasive. The content of the cationic polymer can be more than 0 parts by mass, 0.1 parts by mass or more, 0.5 parts by mass or more, 0.8 parts by mass or more, 1 parts by mass or more, 1.5 parts by mass or more, 2 parts by mass or more, 2.5 parts by mass or more, 3 parts by mass or more, 3.5 parts by mass or more, 4 parts by mass or more, 4.5 parts by mass or more, 5 parts by mass or more, 5.5 parts by mass or more, or 6 parts by mass or more. The content of the cationic polymer can be less than 100 parts by mass, less than 50 parts by mass, less than 30 parts by mass, less than 20 parts by mass, less than 15 parts by mass, less than 12 parts by mass, less than 10 parts by mass, less than 9.5 parts by mass, less than 9 parts by mass, less than 8.5 parts by mass, less than 8 parts by mass, less than 7.5 parts by mass, less than 7 parts by mass, less than 6.5 parts by mass, or less than 6 parts by mass. From these viewpoints, the content of the cationic polymer may be more than 0 parts by mass and 100 parts by mass or less, 1 to 20 parts by mass, 2 to 15 parts by mass, or 2 to 10 parts by mass.
[0102] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the content of the cationic polymer may be in the following ranges relative to 100 parts by mass of the additive A. The content of the cationic polymer may be more than 0 parts by mass, 0.1 parts by mass or more, 0.5 parts by mass or more, 0.8 parts by mass or more, 1 parts by mass or more, 1.5 parts by mass or more, 2 parts by mass or more, 2.5 parts by mass or more, 3 parts by mass or more, 3.5 parts by mass or more, 3.75 parts by mass or more, 4 parts by mass or more, 4.5 parts by mass or more, 5 parts by mass or more, 5.5 parts by mass or more, 6 parts by mass or more, 6.5 parts by mass or more, 7 parts by mass or more, or 7.5 parts by mass or more. The content of the cationic polymer may be 100 parts by mass or less, 50 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, 15 parts by mass or less, 12 parts by mass or less, 11.5 parts by mass or less, 11.25 parts by mass or less, 11 parts by mass or less, 10.5 parts by mass or less, 10 parts by mass or less, 9.5 parts by mass or less, 9 parts by mass or less, 8.5 parts by mass or less, 8 parts by mass or less, or 7.5 parts by mass or less. From these viewpoints, the content of the cationic polymer may be more than 0 parts by mass and less than 100 parts by mass, 1 to 50 parts by mass, 2 to 20 parts by mass, or 3.5 to 11.5 parts by mass.
[0103] (water)
[0104] The water is not particularly limited, but may include at least one selected from the group consisting of deionized water, ion-exchanged water, and ultrapure water.
[0105] (Other additives)
[0106] The CMP polishing liquid involved in this embodiment may contain ingredients other than abrasive grains, additive A, cationic polymer and water. Such ingredients include polyether, pH adjuster, preservative, peroxide, organic solvent, surfactant, defoamer, etc. The CMP polishing liquid involved in this embodiment may not contain at least one of these ingredients.
[0107] [Polyether]
[0108] From the viewpoint of grinding insulating materials at a higher grinding speed and further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the polishing liquid involved in this embodiment may contain polyether. Polyether is a compound having two or more ether groups. The "ether group" in the polyether does not include the "-O-" structure in hydroxyl (hydroxyl), carboxyl, carboxylate group, ester group, sulfonic group and phosphoric acid group.
[0109] Examples of the polyether include polyglycerol, polysaccharides, polyalkylene glycols, polyoxypropylene polyglycerol ether, polyoxyethylene polyglycerol ether, 1,4-bis(2-hydroxyethoxy)benzene, 2,2-bis(4-polyoxyethyleneoxyphenyl)propane, 2,2-bis(4-polyoxypropyleneoxyphenyl)propane, ethylene glycol monophenyl ether, diethylene glycol monophenyl ether, polyoxyalkylene monophenyl ether, propylene glycol monophenyl ether, polyoxypropylene monomethylphenyl ether, polyethylene glycol monomethyl ether, pentaerythritol polyoxyethylene ether, ethylene glycol monoallyl ether, polyoxyethylene monoallyl ether, alkyl glycoside, etc. The polyether may include polyglycerol from the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon.
[0110] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the polyether may contain polyglycerol having an average degree of polymerization of glycerol in the following range. The average degree of polymerization of glycerol may be 3 or more, 4 or more, 5 or more, 8 or more, or 10 or more. The average degree of polymerization of glycerol may be 100 or less, 80 or less, 60 or less, 50 or less, 40 or less, or 30 or less. From these viewpoints, the average degree of polymerization of glycerol may be 3 to 100, or 5 to 60.
[0111] From the viewpoint of grinding insulating materials at a higher grinding speed, and from the viewpoint of further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the weight average molecular weight of the polyether can be in the following range. The weight average molecular weight can be 250 or more, 300 or more, 350 or more, 400 or more, 450 or more, or 500 or more. The weight average molecular weight of the polyether can be 5000 or less, 4000 or less, 3500 or less, 3000 or less, 2500 or less, or 2000 or less. From these viewpoints, the weight average molecular weight can be 250 to 5000. The weight average molecular weight of the polyether can be measured by the same method as the weight average molecular weight of the cationic polymer.
[0112] From the viewpoint of grinding insulating materials at a higher grinding speed, and from the viewpoint of further suppressing the grinding speed of polycrystalline silicon and amorphous silicon, the content of polyether can be the following ranges based on the total mass of the CMP polishing liquid. The content of polyether can be more than 0 mass%, more than 0.01 mass%, more than 0.05 mass%, more than 0.1 mass%, more than 0.1 mass%, more than 0.2 mass%, more than 0.3 mass%, more than 0.35 mass%, more than 0.4 mass%, more than 0.45 mass%, or more than 0.5 mass%. The content of polyether can be less than 10 mass%, less than 8 mass%, less than 5 mass%, less than 3 mass%, less than 2 mass%, less than 1 mass%, less than 1 mass%, less than 0.8 mass%, less than 0.7 mass%, less than 0.65 mass%, less than 0.6 mass%, less than 0.55 mass%, or less than 0.5 mass%. From these viewpoints, the content of polyether can be more than 0 mass% and less than 10 mass%, or 0.1 to 3 mass%.
[0113] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the content of the polyether may be in the following ranges relative to 100 parts by mass of the abrasive. The content of the polyether may be more than 0 parts by mass, 10 parts by mass or more, 50 parts by mass or more, 100 parts by mass or more, 150 parts by mass or more, 200 parts by mass or more, 250 parts by mass or more, 300 parts by mass or more, 350 parts by mass or more, 400 parts by mass or more, 450 parts by mass or more, 500 parts by mass or more, 550 parts by mass or more, 600 parts by mass or more, 650 parts by mass or more, 700 parts by mass or more, 750 parts by mass or more, 800 parts by mass or more, 850 parts by mass or more, 900 parts by mass or more, 950 parts by mass or more, or 1000 parts by mass or more. The content of the polyether may be 10000 parts by mass or less, 8000 parts by mass or less, 6000 parts by mass or less, 5000 parts by mass or less, 4000 parts by mass or less, 3000 parts by mass or less, 2000 parts by mass or less, 1900 parts by mass or less, 1800 parts by mass or less, 1700 parts by mass or less, 1600 parts by mass or less, 1500 parts by mass or less, 1400 parts by mass or less, 1300 parts by mass or less, 1200 parts by mass or less, 1100 parts by mass or less, or 1000 parts by mass or less. From these viewpoints, the content of the polyether may be more than 0 parts by mass and 10000 parts by mass or less, or 300 to 1500 parts by mass.
[0114] From the viewpoint of polishing the insulating material at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the content of the polyether may be in the following ranges relative to 100 parts by mass of the additive A. The content of the polyether may be more than 0 parts by mass, 10 parts by mass or more, 50 parts by mass or more, 100 parts by mass or more, 200 parts by mass or more, 300 parts by mass or more, 350 parts by mass or more, 400 parts by mass or more, 450 parts by mass or more, 500 parts by mass or more, 550 parts by mass or more, 600 parts by mass or more, 650 parts by mass or more, 700 parts by mass or more, 750 parts by mass or more, 800 parts by mass or more, 850 parts by mass or more, 900 parts by mass or more, 950 parts by mass or more, 1000 parts by mass or more, 1100 parts by mass or more, 1200 parts by mass or more, or 1250 parts by mass or more. The content of the polyether may be 10000 parts by mass or less, 8000 parts by mass or less, 7000 parts by mass or less, 6500 parts by mass or less, 6000 parts by mass or less, 5500 parts by mass or less, 5000 parts by mass or less, 4500 parts by mass or less, 4000 parts by mass or less, 3500 parts by mass or less, 3000 parts by mass or less, 2500 parts by mass or less, 2000 parts by mass or less, 1800 parts by mass or less, 1600 parts by mass or less, 1400 parts by mass or less, 1300 parts by mass or less, or 1250 parts by mass or less. From these viewpoints, the content of the polyether may be more than 0 parts by mass and 10000 parts by mass or less, or 500 to 5000 parts by mass.
[0115] [pH adjuster]
[0116] The pH adjuster is not particularly limited, and examples thereof include acid components such as acetic acid, nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, and boric acid; base components such as sodium hydroxide, ammonia (e.g., aqueous ammonia), potassium hydroxide, and calcium hydroxide. From the viewpoint of improving productivity, the CMP polishing liquid can be prepared without using a pH adjuster.
[0117] The content of the acid component is based on the total mass of the CMP polishing liquid, and can be, for example, more than 0 mass%, more than 0.001 mass%, more than 0.005 mass%, more than 0.008 mass%, more than 0.01 mass%, more than 0.012 mass%, more than 0.014 mass%, or more than 0.016 mass%, or less than 5 mass%, less than 3 mass%, less than 1 mass%, less than 0.5 mass%, less than 0.1 mass%, less than 0.05 mass%, less than 0.03 mass%, less than 0.02 mass%, less than 0.018 mass%, or less than 0.016 mass%. The polishing liquid may contain an acid component or may not contain an acid component.
[0118] The content of the base component is based on the total mass of the CMP polishing liquid, and can be, for example, more than 0 mass%, 0.00001 mass% or more, 0.00005 mass% or more, 0.0001 mass% or more, 0.0005 mass% or more, 0.0008 mass% or more, 0.001 mass% or more, or 0.013 mass% or more, or 5 mass% or less, 3 mass% or less, 1 mass% or less, 0.5 mass% or less, 0.1 mass% or less, 0.05 mass% or less, 0.04 mass% or less, 0.031 mass% or less, 0.02 mass% or less, 0.015 mass% or less, or 0.013 mass% or less. The polishing liquid may contain the base component or may not contain the base component.
[0119] (pH)
[0120] From the viewpoint of polishing insulating materials at a higher polishing rate and further suppressing the polishing rate of polycrystalline silicon and amorphous silicon, the pH of the CMP polishing liquid involved in this embodiment can be in the following ranges. The pH can be 10.0 or less, less than 10.0, 9.5 or less, 9.0 or less, less than 9.0, 8.8 or less, 8.5 or less, 8.2 or less, 8.0 or less, less than 8.0, 7.9 or less, 7.8 or less, 7.7 or less, 7.6 or less, 7.5 or less, 7.4 or less, 7.3 or less, 7.2 or less, 7.1 or less, or 7.0 or less. The pH may be more than 4.0, more than 4.0, more than 4.5, more than 5.0, more than 5.0, more than 5.2, more than 5.5, more than 5.7, more than 6.0, more than 6.0, more than 6.1, more than 6.2, more than 6.3, more than 6.4, more than 6.5, more than 6.6, more than 6.7, more than 6.8, more than 6.9, or more than 7.0. From these viewpoints, the pH may be 4.0 to 10.0, 5.0 to 9.0, more than 5.0 and less than 9.0, 5.5 to 8.5, more than 6.0 and less than 9.0, 6.0 to 8.0, more than 6.0 and less than 9.0, more than 6.0 and less than 8.0, or 6.5 to 7.5. The pH can be measured by the method described in the Examples.
[0121] <Preparation and use of CMP polishing liquid>
[0122] The CMP polishing liquid involved in this embodiment can be divided into (a) a normal type, (b) a concentrated type, and (c) a multi-liquid type (for example, a two-liquid type. CMP polishing liquid set), and the preparation method and use method of each are different according to the type. (a) The normal type is a CMP polishing liquid that can be used directly without pretreatment such as dilution during polishing. (b) The concentrated type polishing liquid is a CMP polishing liquid in which the components contained are concentrated compared to the (a) normal type polishing liquid in consideration of the convenience of storage or transportation. (c) The multi-liquid type is a CMP polishing liquid that is prepared in a state where the components contained are divided into a plurality of liquids during storage or transportation (for example, a state where the components are divided into a first liquid containing a certain component and a second liquid containing other components), and these liquids are mixed and used when used.
[0123] (a) The conventional type can be obtained by dissolving or dispersing abrasive grains and additives in water as the main dispersion medium. When preparing the CMP polishing liquid, for example, a stirrer, a homogenizer, an ultrasonic disperser, a wet ball mill, etc. can be used. In addition, during the preparation of the CMP polishing liquid, the abrasive grains can be micronized so that the average particle size of the abrasive grains is within the desired range. The micronization of the abrasive grains can be implemented by a sedimentation classification method or a method using a high-pressure homogenizer. The sedimentation classification method is a method including a process of forcibly sedimenting a slurry containing abrasive grains with a centrifuge and a process of taking out only the supernatant. On the other hand, the method using a high-pressure homogenizer is a method of causing the abrasive grains in the dispersion medium to collide with each other under high pressure.
[0124] The (b) concentrated type is diluted with water immediately before use so that the content of the components is the desired content. After dilution, stirring can be continued for an arbitrary time until the liquid properties (pH, abrasive particle size, etc.) and polishing properties (silicon oxide polishing rate, silicon oxide and silicon nitride polishing selectivity, etc.) of the same degree as those of the (a) normal type are obtained. In this (b) concentrated type, the volume becomes smaller according to the degree of concentration, so the cost related to storage and transportation can be reduced.
[0125] The concentration ratio may be 1.5 times or more, 2 times or more, 3 times or more, or 5 times or more. If the concentration ratio is 1.5 times or more, advantages related to storage and transportation tend to be more easily obtained compared to a case of less than 1.5 times. The concentration ratio may be 40 times or less, 20 times or less, or 15 times or less. If the concentration ratio is 40 times or less, aggregation of abrasive particles tends to be more easily suppressed compared to a case of more than 40 times.
[0126] The (c) multi-liquid type is appropriately divided into each liquid (first liquid, second liquid, etc.), thereby having advantages such as being able to avoid agglomeration of abrasive particles compared to the (b) concentrated type. However, the components contained in each liquid may be arbitrary. The (c) multi-liquid type (polishing liquid set for CMP) is a polishing liquid set for CMP that is used to obtain a polishing liquid for CMP by mixing a first liquid (slurry) and a second liquid (additive liquid). In the (c) multi-liquid type, the constituent components of the polishing liquid for CMP are stored as a first liquid and a second liquid, the first liquid contains abrasive particles and water, and the second liquid contains at least one of the additives and water. In the first embodiment of the (c) multi-liquid type, the first liquid contains abrasive particles and water, and the second liquid contains additive A, a cationic polymer, and water. In the second embodiment of the (c) multi-liquid type, the first liquid contains abrasive particles, one of the additive A and the cationic polymer, and water, and the second liquid contains the other of the additive A and the cationic polymer, and water. The first liquid and the second liquid may contain other components as required. In order to improve the dispersibility of the abrasive in the first liquid, any acid component or base component may be added to the first liquid and the pH may be adjusted.
[0127] (c) A multi-liquid CMP polishing liquid is useful in the following case: a combination of components that tend to reduce polishing properties in a relatively short period of time due to agglomeration of abrasive particles when mixed. In addition, from the viewpoint of reducing costs related to storage and transportation, at least one of the liquids (first liquid, second liquid, etc.) can be set to a concentrated type. In this case, when using the CMP polishing liquid, it is sufficient to mix the liquids with water. The concentration ratio and pH of each liquid are arbitrary, and from the viewpoint of polishing properties, the concentration degree of the final mixture can be the same as that of the (a) conventional CMP polishing liquid.
[0128] <Grinding method>
[0129] The polishing method according to the present embodiment may include a polishing step of polishing the surface to be polished using the polishing liquid, or may include a polishing step of polishing the surface to be polished using a polishing liquid obtained by mixing the slurry in the polishing liquid set with an additive liquid.
[0130] The polished surface may include a stopper layer. The polished surface may include a stopper layer and an insulating material, or may include a stopper layer, silicon oxide, and silicon nitride. The polishing method involved in this embodiment may include, for example, a polishing step of polishing the polished surface using the above-mentioned CMP polishing liquid, or a CMP polishing liquid obtained by mixing the slurry in the above-mentioned CMP polishing liquid kit and an additive liquid. According to the polishing method involved in this embodiment, the polishing speed of the stopper layer can be suppressed while polishing the insulating material at a high polishing speed.
[0131] Examples of the insulating material include silicon oxide, silicon nitride, etc. Examples of the stopper layer include polysilicon, amorphous silicon, etc.
[0132] As a method for producing the insulating material and the stopper layer, for example, there can be cited CVD methods such as low-pressure CVD method, quasi-normal-pressure CVD method, and plasma CVD method; and a spin coating method of coating a liquid raw material on a rotating substrate.
[0133] The insulating material and the stopper layer can be a single material or multiple materials. When multiple materials are exposed on the polished surface, they can be regarded as the insulating material and the stopper layer. The insulating material and the stopper layer can be in the form of a film, or can be a silicon oxide film, a silicon nitride film, a polysilicon film, an amorphous silicon film, etc.
[0134] The polishing method involved in the present embodiment can be a method for polishing a substrate. The substrate, for example, has a stopper layer (a component including a stopper layer). The substrate, for example, can have a stopper layer and a component including an insulating material. In the present embodiment, the stopper layer can be used to stop the polishing of a substrate having a stopper layer (polycrystalline silicon, amorphous silicon, etc.) and a component including an insulating material (silicon oxide, silicon nitride, etc.). According to the present embodiment, a method for polishing a substrate having an insulating material and a stopper layer can be provided, which includes a polishing step of polishing the surface to be polished using the above-mentioned CMP polishing liquid, or the CMP polishing liquid obtained by mixing the slurry and additive liquid in the above-mentioned CMP polishing liquid set. According to the polishing method involved in the present embodiment, the insulating material can be polished at a high polishing speed while suppressing the polishing speed of polycrystalline silicon and amorphous silicon.
[0135] As the base body of the grinding object, there can be a substrate, for example, a substrate including a component containing an insulating material and a stopper layer formed on a substrate involved in the manufacture of semiconductor elements (for example, a semiconductor substrate having an STI pattern, a gate pattern, a wiring pattern, etc.).
[0136] In the grinding process, for example, the grinding surface of the substrate is pressed against the grinding pad of the grinding plate, and the CMP grinding liquid is supplied between the grinding surface and the grinding pad, so that the substrate and the grinding plate are relatively moved to grind the grinding surface. In the grinding process, for example, at least a portion of the insulating material in the grinding surface is removed by grinding.
[0137] Figure 1 It is a schematic cross-sectional view showing a polishing step when forming an STI structure of a semiconductor. Figure 1 (a) is a schematic cross-sectional view showing a substrate before grinding. Figure 1 (b) is a schematic cross-sectional view showing the substrate during polishing. Figure 1 (c) is a schematic cross-sectional view showing the substrate after grinding. Figure 1 As shown in (a), the base body comprises: a substrate (e.g., a semiconductor substrate such as a silicon substrate) 1 having a concave-convex pattern; a stopper layer 2 disposed on the convex portion of the substrate 1; and an insulating material 3 disposed on the substrate 1 and the stopper layer 2 in a manner of filling the concave portion. A step D is formed on the surface of the insulating material 3. Figure 1 As shown in (b), during the grinding process, the unnecessary part protruding locally on the surface of the insulating material 3 is preferentially removed by CMP, thereby eliminating the step D of the insulating material 3. Figure 1 As shown in (c), during this polishing, at the stage where the stopper layer 2 is exposed, the polishing of the insulating material 3 is stopped by the stopper layer 2, thereby forming an STI structure having a buried portion 5.
[0138] As described above, the insulating material formed on the substrate is polished with the CMP polishing liquid to remove the excess part, thereby eliminating the unevenness of the surface of the insulating material, and the insulating material is prevented from being over-polished by stopping the polishing when the stopper layer is exposed, so that a smooth surface can be obtained on the entire surface of the insulating material. The CMP polishing liquid involved in this embodiment can be used to polish the polished surface including the stopper layer (polysilicon, amorphous silicon, etc.). The CMP polishing liquid involved in this embodiment can be used to polish the polished surface including at least one of silicon oxide and silicon nitride.
[0139] In the grinding method involved in this embodiment, as a grinding device, a common grinding device having a holder capable of holding a substrate having a grinding surface (e.g., a semiconductor substrate) and a grinding plate capable of attaching a grinding pad can be used. A motor capable of changing the rotation speed is respectively installed on the holder and the grinding plate. As a grinding device, for example, a grinding device manufactured by APPLIED MATERIALS, Inc., product name: Reflexion; a grinding device manufactured by Ebara Corporation, product name: F-REX can be used.
[0140] As grinding pad, usually can use nonwoven fabrics, foam, non-foam etc. As the material of grinding pad, can use polyurethane, acrylic resin, polyester, acrylic acid-ester copolymer, polytetrafluoroethylene, polypropylene, polyethylene, poly-4-methylpentene, cellulose, cellulose ester, polyamide (for example, nylon and aramid), polyimide, polyimide amide, polysiloxane copolymer, ethylene oxide compound, phenolic resin, polystyrene, polycarbonate, epoxy resin and other resins. As the material of grinding pad, especially from the viewpoint of grinding speed and flatness, can be foamed polyurethane and non-foamed polyurethane. For grinding pad, groove processing for accumulating grinding fluid can be implemented.
[0141] There is no restriction on the grinding conditions, but in order to prevent the substrate from flying out, the rotation speed (rotation speed) of the grinding plate can be 200min -1 Below, from the viewpoint of fully suppressing the generation of grinding scratches, the grinding pressure (processing load) applied to the matrix can be below 100kPa. During grinding, the grinding liquid can also be continuously supplied to the grinding pad by a pump etc. There is no restriction on this supply rate, and the surface of the grinding pad can also be covered by the grinding liquid always.
[0142] After grinding, the substrate can be fully cleaned in running water to remove particles attached to the substrate. In addition to pure water, dilute hydrofluoric acid, ammonia water and other cleaning liquids can also be used for cleaning. In order to improve the cleaning efficiency, a brush can also be used. In addition, after cleaning, a rotary dryer can be used to wipe off water droplets attached to the substrate and then dry the substrate.
[0143] The CMP polishing liquid, CMP polishing liquid set, and polishing method according to the present embodiment can be used in the STI formation process, polishing of pre-metal insulating materials, interlayer insulating materials, etc. As the pre-metal insulating material, for example, phosphorus-silicate glass, boron-phosphorus-silicate glass, silicon oxide, fluorinated amorphous carbon, etc. can be used in addition to silicon oxide.
[0144] The CMP polishing liquid, CMP polishing liquid kit and polishing method involved in this embodiment can be applied not only to film-shaped polishing objects, but also to various substrates composed of glass, silicon, SiC, SiGe, Ge, GaN, GaP, GaAs, sapphire, plastic, etc.
[0145] The CMP polishing liquid, CMP polishing liquid kit and polishing method involved in this embodiment can be used not only in the manufacture of semiconductor elements, but also in the manufacture of image display devices such as TFT liquid crystals and organic ELs; optical devices such as photomasks, lenses, prisms, optical fibers, and single crystal scintillators; optical elements such as optical switch elements and optical waveguides; light-emitting elements such as solid lasers and blue laser LEDs; and magnetic storage devices such as disks and magnetic heads.
[0146] <Manufacturing method, etc.>
[0147] The manufacturing method of the device involved in the present embodiment includes a device manufacturing process of obtaining a device using a substrate (polished component) polished by the polishing method involved in the present embodiment. The device involved in the present embodiment is a device obtained by the manufacturing method of the device involved in the present embodiment. The device involved in the present embodiment is not particularly limited, but can be an electronic device (for example, a semiconductor device such as a semiconductor package), a wafer (for example, a semiconductor wafer), or a chip (for example, a semiconductor chip). As one mode of the manufacturing method of the device involved in the present embodiment, in the manufacturing method of the electronic device involved in the present embodiment, an electronic device is obtained using a substrate polished by the polishing method involved in the present embodiment. As one mode of the manufacturing method of the device involved in the present embodiment, in the manufacturing method of the semiconductor device involved in the present embodiment, a semiconductor device (for example, a semiconductor package) is obtained using a substrate polished by the polishing method involved in the present embodiment. The manufacturing method of the device involved in the present embodiment may include a polishing process of polishing the substrate by the polishing method involved in the present embodiment before the device manufacturing process.
[0148] As one mode of the device manufacturing process, the manufacturing method of the device involved in the present embodiment may include a singulation process of singulating the substrate (polished component) polished by the polishing method involved in the present embodiment. The singulation process may be, for example, a process of cutting a wafer (for example, a semiconductor wafer) polished by the polishing method involved in the present embodiment to obtain a chip (for example, a semiconductor chip). As one mode of the device manufacturing method involved in the present embodiment, the manufacturing method of the electronic device involved in the present embodiment may include a process of obtaining an electronic device (for example, a semiconductor device) by singulating the substrate polished by the polishing method involved in the present embodiment. As one mode of the device manufacturing method involved in the present embodiment, the manufacturing method of the semiconductor device involved in the present embodiment may include a process of obtaining a semiconductor device (for example, a semiconductor package) by singulating the substrate polished by the polishing method involved in the present embodiment.
[0149] As one mode of the device manufacturing process, the manufacturing method of the device involved in the present embodiment may include a connection process of connecting (for example, electrically connecting) a substrate (a polished part) polished by the polishing method involved in the present embodiment to other connected bodies. The connected body connected to the substrate polished by the polishing method involved in the present embodiment is not particularly limited, and may be a substrate polished by the polishing method involved in the present embodiment, or may be a connected body different from the substrate polished by the polishing method involved in the present embodiment. In the connection process, the substrate and the connected body may be directly connected (the substrate and the connected body are connected in a contacting state), or the substrate and the connected body may be connected via other components (conductive components, etc.). The connection process can be performed before the singulation process, after the singulation process, or before and after the singulation process.
[0150] The connection process may be a process of connecting the polished surface of the substrate polished by the polishing method involved in the present embodiment and the connected body, or may be a process of connecting the connecting surface of the substrate polished by the polishing method involved in the present embodiment and the connecting surface of the connected body. The connecting surface of the substrate may be the polished surface polished by the polishing method involved in the present embodiment. Through the connection process, a connected body having a substrate and a connected body can be obtained. In the connection process, when the connecting surface of the substrate has a metal part, the connected body can be brought into contact with the metal part. In the connection process, when the connecting surface of the substrate has a metal part and the connecting surface of the connected body has a metal part, the metal parts can be brought into contact with each other. The metal part may contain copper.
[0151] The device according to the present embodiment (for example, an electronic device such as a semiconductor device) includes at least one selected from the group consisting of a substrate polished by the polishing method according to the present embodiment and a device according to the present embodiment.
[0152] Example
[0153] Hereinafter, the present invention will be described in further detail based on examples, but the present invention is not limited to these examples.
[0154] <Synthesis of particles of tetravalent metal hydroxide>
[0155] 350 g of a 650 mass % aqueous solution of Ce(NH4)2(NO3) (manufactured by NIHON KAGAKU SANGYOCO., LTD., product name: CAN50 solution) was dissolved in 7825 g of pure water to obtain a solution. Then, the solution was stirred and 750 g of an imidazole aqueous solution (10 mass % aqueous solution) was added dropwise at a rate of 5 mL / min to obtain a precipitate containing particles of cerium hydroxide.
[0156] The obtained precipitate containing cerium hydroxide was centrifuged (4000 min -1 , 5 minutes), the liquid phase was removed by decantation, thereby implementing solid-liquid separation. In addition, 10 g of the obtained particles and 990 g of water were mixed, and the particles were dispersed in water using an ultrasonic cleaning machine to prepare a storage solution for cerium hydroxide slurry (particle content: 1.0 mass %).
[0157] The average particle size of the abrasive grains (abrasive grains containing cerium hydroxide) in the cerium hydroxide slurry was measured using the product name: DelsaMax Pro manufactured by Beckman Coulter, Inc. The result was 8 nm. The measurement method is as follows. First, a measurement sample (cerium hydroxide slurry, aqueous dispersion) containing 1.0% by mass of abrasive grains was placed in a 1 cm square sample tank for about 1 mL, and a sample tank was set in the DelsaMaxPro. Next, the refractive index of the measurement sample information of the DelsaMax Pro software was set to 1.333, the viscosity was set to 0.887 mPa·s, the measurement was performed at 25°C, and the value displayed as Unimodal SizeMean was read.
[0158] Take an appropriate amount of cerium hydroxide slurry storage solution, dilute it with water in a way that the content of particles becomes 0.0065% by mass, and obtain a measurement sample (aqueous dispersion). The measurement sample is placed in a 1 cm square sample tank for about 4 mL, and a sample tank is set in a spectrometer (device name: U3310) manufactured by Hitachi, Ltd. The absorbance is measured in the range of wavelength 200 to 600 nm, and the absorbance relative to the light of wavelength 290 nm and the absorbance relative to the light of wavelength 450 to 600 nm are measured. The absorbance relative to the light of wavelength 290 nm is 1.192, and the absorbance relative to the light of wavelength 450 to 600 nm is less than 0.010.
[0159] About 4 mL of the cerium hydroxide slurry storage solution (particle content: 1.0 mass%) was placed in a 1 cm square sample tank, and the sample tank was set in a spectrometer (device name: U3310) manufactured by Hitachi, Ltd. The absorbance was measured in the range of 200 to 600 nm, and the absorbance relative to the light of wavelength 400 nm and the transmittance relative to the light of wavelength 500 nm were measured. The absorbance relative to the light of wavelength 400 nm was 2.25, and the transmittance relative to the light of wavelength 500 nm was 92% / cm.
[0160] For a sample obtained by taking a proper amount of a storage solution for cerium hydroxide slurry, vacuum drying to separate abrasive grains, and fully washing with pure water, a measurement based on the FT-IR ATR method was performed, and the result showed that in addition to the peak based on the OH group, a peak based on the NO3 group was also observed. In addition, for the same sample, an XPS (N-XPS) measurement relative to nitrogen was performed, and the result showed that no peak based on NH4 was observed, but a peak based on NO3 was observed. Through these results, it was confirmed that at least a portion of the abrasive grains contained in the storage solution for cerium hydroxide slurry contained particles having NO3 groups bonded to the cerium element.
[0161] <Preparation of CMP polishing slurry>
[0162] The CMP polishing liquid used in each example and each comparative example was adjusted to contain 0.05 mass % of cerium hydroxide as abrasive, the amounts of the additives described later shown in Tables 1 to 4, the amounts of the cationic polymers described later shown in Tables 1 to 4, the amounts of acetic acid shown in Tables 1 to 4, the amounts of ammonia water (solid content) shown in Tables 1 to 4, 0.5 mass % of polyglycerol, and the remainder was prepared as pure water. The following compounds were used as additives.
[0163] [additive]
[0164] A1: 1,1',1",1"'-ethylenediaminetetra-2-propanol
[0165] A2: 2,2',2",2"'-ethylenediyl dinitrotetraethanol
[0166] A3: N-(2-Hydroxypropyl)ethylenediamine
[0167] A4: Ethylenediamine tetrapolyoxyalkylene (weight average molecular weight 6000, hydroxyl groups at the ends of the polyoxyalkylene chains, ratio of polyoxypropylene chains to polyoxyethylene chains (PO chains / EO chains): 65 / 35)
[0168] A5: Tetramethylethylenediamine
[0169] A6: Monoethanolamine
[0170] A7: 3-Amino-1-propanol
[0171] [Cationic polymer]
[0172] B1: Diallyldimethylammonium chloride-acrylamide copolymer
[0173] B2: Dimethylamine / ammonia / epichlorohydrin condensation product
[0174] B3: Diallylamine hydrochloride / acrylamide copolymer
[0175] B4: Methyldiallylamine hydrochloride / epichlorohydrin modified polymer
[0176] B5: Vinyl pyrrolidone-N,N-dimethylaminoethyl methacrylate copolymer diethyl sulfate
[0177] Specifically, water is added to the above-mentioned cerium hydroxide slurry storage solution to dilute it 5 to 10 times, thereby obtaining a slurry containing particles containing cerium hydroxide as abrasive grains. Then, each component other than the abrasive grains is dissolved in pure water to obtain an additive liquid. Then, the above-mentioned slurry and the above-mentioned additive liquid are mixed and stirred to prepare a CMP polishing liquid. The average particle size of the abrasive grains in the CMP polishing liquid of each embodiment measured by the same method as the average particle size of the abrasive grains in the above-mentioned slurry is the same as the average particle size of the abrasive grains in the above-mentioned slurry.
[0178] <pH measurement>
[0179] The pH of the CMP polishing liquid was measured under the following conditions. The results are shown in the tables.
[0180] Measurement temperature: 25℃
[0181] Measuring device: HORIBA, Ltd. Product name: Model (D-71)
[0182] Measurement method: After three-point calibration of the pH meter using a phthalate pH standard solution (pH: 4.01), a neutral phosphate pH standard solution (pH: 6.86), and a borate pH standard solution (pH: 9.18) as pH standard solutions, the pH meter electrode was immersed in the CMP polishing liquid, and the pH was measured by the above-mentioned measuring device after stabilization for more than 2 minutes. The pH of the CMP polishing liquid is shown in Tables 1 and 2.
[0183] <Evaluation of polishing characteristics>
[0184] Using the CMP polishing liquid of each embodiment and each comparative example, a polished film (silicon oxide film (TEOS film), silicon nitride film (SiN film), polycrystalline silicon film (p-Si film), or amorphous silicon film (a-Si film)) formed on a silicon substrate was polished under the following CMP polishing conditions.
[0185] (CMP polishing conditions)
[0186] Polishing device: F-REX300X (manufactured by Ebara Corporation)
[0187] CMP polishing liquid flow rate: 200mL / min
[0188] Polishing pad: Foamed polyurethane resin with independent cells (manufactured by Rohm and Haas Japan company, model number IC1000)
[0189] Grinding pressure: 14.7kPa (2psi)
[0190] Plate speed: 93rpm
[0191] Head speed: 87rpm
[0192] Grinding time: 30 seconds
[0193] Cleaning: After the CMP treatment, the film was cleaned with water and then dried with a spin dryer.
[0194] (Evaluation items for polishing products)
[0195] The polishing speed of the polished film (silicon oxide film, silicon nitride film, polycrystalline silicon film, or amorphous silicon film) polished and cleaned under the above conditions was calculated by the following formula. In addition, the film thickness difference of the polished film before and after polishing was calculated using an optical interference film thickness measuring device (manufactured by Filmetrics, INC., product name: F80). The polishing speeds of silicon oxide film, silicon nitride film, polycrystalline silicon film, and amorphous silicon film are shown in Tables 1 and 2. In addition, when the polishing speed is greater than 0 nm / min and less than 1 nm / min, it is expressed as "<1" in the table.
[0196] (Polishing speed) = (Thickness difference of silicon oxide film, silicon nitride film, polysilicon film, or amorphous silicon film before and after polishing (nm)) × (60 / (Polishing time) ( / min))
[0197] [Table 1]
[0198]
[0199] [Table 2]
[0200]
[0201] [Table 3]
[0202]
[0203] [Table 4]
[0204]
[0205] Explanation of symbols
[0206] 1-substrate, 2-stop layer, 3-insulating material, 5-buried part, D-step difference.
Claims
1. A CMP polishing liquid comprising abrasive grains, an additive A, a cationic polymer and water, The additive A includes a compound having an ethylenediamine structure to which a hydroxyalkyl group or an alkoxy group is bonded.
2. The CMP polishing liquid according to claim 1, wherein The abrasive grains include at least one selected from the group consisting of cerium hydroxide, cerium oxide, silicon dioxide, and aluminum oxide.
3. The CMP polishing liquid according to claim 1, wherein The abrasive grains contain cerium hydroxide.
4. The CMP polishing liquid according to claim 1, wherein The additive A comprises 2,2',2",2"'-ethylenediyldinitrotetraethanol.
5. The CMP polishing liquid according to claim 1, wherein The additive A comprises 1,1',1",1"'-ethylenediaminetetra-2-propanol.
6. The CMP polishing liquid according to claim 1, wherein The content of the additive A is 0.001 to 5% by mass.
7. The CMP polishing liquid according to claim 1, wherein The cationic polymer includes a polymer having a quaternary ammonium salt structure or a polymer having an amino group.
8. The CMP polishing liquid according to claim 1, wherein The content of the cationic polymer is 2 to 20 parts by mass based on 100 parts by mass of the additive A. 9 . The CMP polishing liquid according to claim 1 , further comprising a polyether.
10. The CMP polishing liquid according to claim 1, wherein the pH thereof is 4.0 to 10.
0. The CMP polishing liquid according to claim 1 , wherein the pH thereof is higher than 6.0 and lower than 9.
0. 12 . The CMP polishing liquid according to claim 1 , which is used for polishing a surface to be polished including silicon oxide, silicon nitride, polycrystalline silicon and amorphous silicon.
13. A CMP polishing liquid kit, wherein: The CMP polishing liquid according to any one of claims 1 to 12 is stored as a first liquid and a second liquid, wherein the first liquid contains the abrasive and water, and the second liquid contains the additive A, the cationic polymer, and water. 14 . A polishing method comprising the step of polishing a surface to be polished using the CMP polishing liquid according to claim 1 .
15. The grinding method according to claim 14, wherein: The polished surface includes silicon oxide, silicon nitride, polycrystalline silicon and amorphous silicon. 16 . A polishing method comprising the step of polishing a surface to be polished using a CMP polishing liquid obtained by mixing the first liquid and the second liquid in the CMP polishing liquid set according to claim 13 .
17. The grinding method according to claim 16, wherein: The polished surface includes silicon oxide, silicon nitride, polycrystalline silicon and amorphous silicon.