Negative electrode active material for sodium ion secondary battery

By using the amorphous phase containing SiO2 and the negative electrode active material of the Fe-Sn-based alloy in a sodium ion secondary battery, the volume change problem caused by charging and discharging of metal Sn is solved, and the stability of the battery characteristics and cycle characteristics are improved. .

CN119096375APending Publication Date: 2024-12-06NAT UNIV CORP NAGAOKA UNIV TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032265.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-27
Filing Date
2023-07-13
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The charge and discharge process of metal Sn in sodium ion secondary batteries leads to large volume changes, resulting in electrode damage and unstable battery characteristics.

Method used

Using an amorphous phase containing SiO2 and an anode active material of a Fe-Sn-based alloy, FeSn2 has a smaller volume change compared with metal Sn, and uses SiO2 as a buffer material to stabilize the battery characteristics.

Benefits of technology

The stable battery characteristics are shown during repeated charging and discharging, improving the cycle characteristics and battery durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005069085210000111
    Figure BDA0005069085210000111
  • Figure HDA0005069085220000011
    Figure HDA0005069085220000011
  • Figure HDA0005069085220000012
    Figure HDA0005069085220000012
Patent Text Reader

Abstract

Provided is a negative electrode active material for sodium ion secondary batteries, which exhibits stable battery characteristics during repeated charging and discharging. The negative electrode active material for a sodium ion secondary battery is characterized by containing an amorphous phase containing SiO2 and an Fe-Sn alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative electrode active material for a sodium ion secondary battery used in, for example, portable electronic devices and electric vehicles. Background Art

[0002] In recent years, the development of lithium ion secondary batteries has become active with the popularization of portable electronic devices, electric vehicles, etc. However, there are concerns about the depletion of Li resources used in lithium ion secondary batteries, and as a solution to this problem, sodium ion secondary batteries that use Na ions instead of Li ions have been studied.

[0003] Among them, metal Sn has a high theoretical capacity of 847 mAhg by alloying with sodium, and is therefore known as a promising candidate for negative electrode materials in sodium ion secondary batteries. + +15e - ←→Na 15 Sn4 reaction. Here, the volume change of metal Sn during charge and discharge is as large as 4.2 times, so the reduction in capacity caused by the destruction of the electrode becomes a technical problem. As a method for alleviating the volume change during charge and discharge, a method of precipitating metal Sn into a glass matrix has been proposed (for example, see Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-229539 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] In the crystallized glass formed by precipitation of metallic Sn, the amorphous components such as SiO2, P2O5, B2O3 contained in the glass matrix play the role of a buffer material to alleviate the expansion and contraction of the Sn component. However, since the volume change during charge and discharge cannot be completely alleviated, there is a problem that the battery characteristics tend to become unstable when charge and discharge are repeated.

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a negative electrode active material for a sodium ion secondary battery that exhibits stable battery characteristics when charge and discharge are repeated.

[0010] Technical solutions for solving technical problems

[0011] The negative electrode active material for a sodium ion secondary battery of the present invention is characterized by comprising an amorphous phase containing SiO2 and a Fe-Sn-based alloy.

[0012] Thus, the negative electrode active material for the sodium ion secondary battery of the present invention contains an Fe-Sn alloy. FeSn2, which is a kind of Fe-Sn alloy, undergoes repeated charge and discharge. + +15e - ←→2Fe+Na 15 Sn4 reaction. Here, FeSn2 has a smaller volume change accompanying alloying during charge and discharge than metallic Sn. In addition, the negative electrode active material for the sodium ion secondary battery of the present invention comprises an amorphous phase containing SiO2. The amorphous phase acts as a buffer material for mitigating the expansion and contraction of Fe-Sn alloys such as FeSn2. Due to the small volume change accompanying alloying during charge and discharge, and the presence of the amorphous phase as a buffer material for mitigating the volume change, stable battery characteristics can be exhibited, especially when charge and discharge are repeated.

[0013] The negative electrode active material for a sodium ion secondary battery of the present invention preferably contains 30% to 90% of SnO, 2% to 69% of SiO2, and 1% to 20% of Fe2O3 in terms of mol% converted to oxides.

[0014] In the negative electrode active material for a sodium ion secondary battery of the present invention, the Fe—Sn alloy is preferably FeSn 2 .

[0015] The negative electrode active material for a sodium ion secondary battery of the present invention is preferably composed of crystallized glass obtained by precipitating the Fe—Sn-based alloy in a matrix composed of the amorphous phase.

[0016] The crystallinity of the negative electrode active material for a sodium ion secondary battery of the present invention is preferably 30% by mass or more and 99% by mass or less.

[0017] In the negative electrode active material for a sodium ion secondary battery of the present invention, the amount of crystals of the Fe—Sn-based alloy is preferably 0.5% by mass or more and 70% by mass or less.

[0018] The negative electrode active material for a sodium ion secondary battery of the present invention may further contain β-Sn.

[0019] Effects of the Invention

[0020] According to the present invention, it is possible to provide a negative electrode active material for a sodium ion secondary battery that exhibits stable battery characteristics when charge and discharge are repeated. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a graph showing the battery characteristics of the test battery produced in Example 3 in each cycle.

[0022] Figure 2This is a graph showing the battery characteristics of the test battery prepared in Comparative Example 1 in each cycle. DETAILED DESCRIPTION

[0023] Hereinafter, preferred embodiments will be described. However, the following embodiments are merely illustrative, and the present invention is not limited to the following embodiments. In addition, in each of the drawings, components having substantially the same function are sometimes referred to with the same reference numerals.

[0024] The negative electrode active material for a sodium ion secondary battery of the present invention (hereinafter also referred to as the negative electrode active material) is characterized in that it contains an amorphous phase containing SiO2 and an Fe-Sn alloy. Specifically, the negative electrode active material of the present invention preferably contains 30% to 90% SnO, 2% to 69% SiO2, and 1% to 20% Fe2O3 in terms of molar % converted to oxides. The reason for limiting the composition in this way is explained below. In the following description of the composition, "%" means "molar %" unless otherwise specified.

[0025] SnO is an active material component that becomes a site for absorbing (i.e., retaining) and releasing (i.e., releasing) sodium ions. The content of SnO is measured in mole % converted to oxide, for example, preferably more than 30%, more than 35%, more than 40%, more than 45%, particularly preferably more than 50%, preferably less than 90%, less than 80%, less than 75%, less than 70%, particularly preferably less than 68%. When the content of SnO is too little, the charge and discharge capacity per unit mass of the negative electrode active material is easily reduced. On the other hand, if the content of SnO is too much, the amorphous component in the negative electrode active material becomes relatively less, so it is impossible to alleviate the volume change caused by the absorption and release of sodium ions during charging and discharging, resulting in reduced cycle characteristics, etc., and the battery characteristics are prone to become unstable.

[0026] SiO2 is a component that acts as a network-forming oxide and promotes amorphization. As a result, it has the function of absorbing and releasing sites of sodium ions contained in the Sn component and improving the cycle characteristics. In terms of mole % converted to oxide, the content of SiO2 is, for example, preferably more than 2%, more than 5%, more than 10%, more than 15%, particularly preferably more than 20%, preferably less than 69%, less than 65%, less than 55%, less than 45%, particularly preferably less than 35%. When the content of SiO2 is too little, it is difficult to obtain the above-mentioned effect. On the other hand, when the content of SiO2 is too much, there is a tendency for the ion conductivity to decrease and the discharge capacity to decrease. In addition, because the Sn component is relatively less, the charge and discharge capacity tends to decrease.

[0027] Fe2O3 is a component that forms Fe-Sn alloys such as FeSn2 through subsequent heat treatment, and acts as an active material that absorbs and releases sodium ions and electrons. In addition, Fe2O3 is a component that acts as a mesh-forming oxide and promotes amorphization. As a result, it has the effect of improving the cycle characteristics by acting as a component that alleviates the expansion and contraction of the Sn component. Furthermore, it has the function of improving the conductivity of the oxide matrix component in the negative electrode active material, and also has the effect of improving the rapid charge and discharge characteristics. In terms of molar % converted to oxide, the content of Fe2O3 is preferably, for example, more than 1%, more than 1.5%, more than 2%, more than 2.5%, particularly preferably more than 3%, preferably less than 20%, less than 17%, less than 15%, less than 12%, and particularly preferably less than 10%. When the content of Fe2O3 is too little, it is difficult to obtain the above effect. On the other hand, when the content of Fe2O3 is too much, there is a tendency for the ion conductivity to decrease and the discharge capacity to decrease.

[0028] The negative electrode active material of the present invention may contain the following components in addition to the above components.

[0029] Na2O is a component that improves the ion conductivity of the oxide matrix components other than the Sn component. In terms of mole % converted to oxide, the content of Na2O is preferably, for example, 1% or more, 3% or more, 5% or more, 7% or more, particularly preferably 10% or more, preferably 50% or less, 40% or less, 30% or less, 25% or less, particularly preferably 20% or less. If the content of Na2O is too much, a large amount of heterogeneous crystals (e.g., crystals containing Na2O and SiO2) are formed, and the cycle characteristics are easily reduced.

[0030] P2O5 is a component that acts as a network-forming oxide like SiO2 and promotes amorphization. As a result, it has a site for the absorption and release of sodium ions in the Sn component and improves the cycle characteristics. In terms of molar % converted to oxide, the content of P2O5 is, for example, preferably 1% or more, 3% or more, 5% or more, particularly preferably 7% or more, preferably 30% or less, 25% or less, 20% or less, particularly preferably 15% or less. If the content of P2O5 is too much, the water resistance of the negative electrode active material is easily reduced. In addition, because the Sn component is relatively less, there is a tendency for the charge and discharge capacity to decrease.

[0031] B2O3 is also a component that functions as a network-forming oxide like SiO2 and promotes amorphization. As a result, it has the effect of absorbing and releasing sites of sodium ions in the Sn component and improving cycle characteristics. In terms of molar % converted to oxide, the content of B2O3 is, for example, preferably more than 1%, more than 3%, more than 5%, particularly preferably more than 7%, preferably less than 30%, less than 25%, less than 20%, particularly preferably less than 15%. If the content of B2O3 is too much, the coordination bond to the Sn component becomes stronger, the initial charge capacity becomes larger, and as a result, there is a tendency for the initial irreversible capacity to become larger. In addition, because the Sn component is relatively less, there is a tendency for the charge and discharge capacity to decrease.

[0032] In terms of molar % converted to oxides, the content of P2O5+SiO2+B2O3 is, for example, preferably 2% or more, 3% or more, 4% or more, 5% or more, 10% or more, 15% or more, particularly preferably 20% or more, preferably 69% or less, 65% or less, 55% or less, 45% or less, particularly preferably 35% or less. If the content of P2O5+SiO2+B2O3 is too little, the volume change of the Sn component caused by the absorption and release of sodium ions during charge and discharge cannot be alleviated, causing structural degradation, so the cycle characteristics are easily reduced. On the other hand, if the content of P2O5+SiO2+B2O3 is too much, the Sn component becomes relatively less, so there is a tendency for the charge and discharge capacity to decrease. Among them, in this specification, "x+y+..." refers to the total amount of the content of each component. Here, with respect to each component, it is not necessarily necessary to contain each component as an essential component, and components that are not contained (i.e., the content is 0%) may also be included.

[0033] The negative electrode active material of the present invention can contain TiO2, MnO, CuO, ZnO, MgO, CaO, Al2O3 in the range of 0% to 25%, 0% to 23%, 0% to 21%, and further 0.1% to 20% in terms of the total amount of mole % converted to oxide. By containing these components, amorphous materials can be easily obtained. However, when the content is too much, the network composed of SiO2 is easily cut off, resulting in the inability to ease the volume change of the negative electrode active material accompanying charge and discharge, and the cycle characteristics may be reduced.

[0034] The negative electrode active material of the present invention preferably has FeSn2 and other Fe-Sn alloys precipitated inside. FeSn2 can be determined by powder X-ray diffraction measurement (XRD) using CuKα rays. Specifically, in the diffraction line profile obtained by powder X-ray diffraction measurement (XRD), the diffraction lines with peak positions at 2θ values ​​of 35.1°, 43.9°, 61.2°, 33.7°, and 67.3° can be attributed to the crystalline phase of FeSn2 (tetragonal system, space group I4 / mcm (140)).

[0035] FeSn2The amount of crystallization is preferably more than 0.5 mass %, more preferably more than 1 mass %, more preferably more than 4 mass %, preferably less than 70 mass %, more preferably less than 60 mass %, more preferably less than 55 mass %. If FeSn2The amount of crystallization is too much, the amorphous component (i.e., amorphous component) in the negative electrode active material is relatively reduced, so there is a tendency that the volume change caused by the absorption and release of sodium ions accompanying charge and discharge cannot be alleviated, and the battery characteristics become unstable. On the other hand, when the amount of crystallization of FeSn2 is too little, there is a tendency that the battery characteristics become unstable when the discharge capacity is reduced or repeatedly charged and discharged.

[0036] The negative electrode active material of the present invention can precipitate β-Sn inside. β-Sn becomes a site for absorbing and releasing sodium ions, which has the effect of further improving the battery capacity. β-Sn can be determined by powder X-ray diffraction measurement (XRD) using CuKα rays. Specifically, in the diffraction line profile obtained by powder X-ray diffraction measurement (XRD), the diffraction lines with peak positions at 2θ values ​​of 30.63° and 32.02° can be attributed to the crystalline phase of β-Sn (tetragonal system, space group I41 / amd(141)).

[0037] The amount of crystallization of β-Sn is preferably 1% by mass or more, more preferably 5% by mass or more, further preferably 10% by mass or more, preferably 70% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less. If the amount of crystallization of β-Sn is too much, the amorphous component in the negative electrode active material becomes relatively less, so there is a tendency that the volume change caused by the absorption and release of sodium ions during charge and discharge cannot be alleviated, and the battery characteristics become unstable. On the other hand, if the amount of crystallization of β-Sn is too little, there is a tendency for the discharge capacity to decrease.

[0038] The negative electrode active material of the present invention can precipitate FeNaSnO4 inside, which can further improve the stability of battery characteristics.

[0039] The crystallinity (i.e., degree of crystallinity) of the negative electrode active material is preferably 30% by mass or more, more preferably 40% by mass or more, and particularly preferably 50% by mass or more. The greater the crystallinity, the easier it is to reduce the initial irreversible capacity. However, when the crystallinity is too large, there is a tendency for the cycle characteristics to decrease. Therefore, from the viewpoint of improving the cycle characteristics, the crystallinity is preferably 99% by mass or less, more preferably 95% by mass or less, and particularly preferably 90% by mass or less.

[0040] The crystallinity is obtained from the diffraction line profile with a 2θ value of 10° to 60° obtained by powder X-ray diffraction measurement (XRD) using CuKα rays. Specifically, when the integrated intensity obtained by peak separation of a wide diffraction line (amorphous halo) at 10° to 45° from a total scattering curve is set as Ia, and the sum of the integrated intensities obtained by peak separation of each crystalline diffraction line detected at 10° to 60° is set as Ic, the crystallinity Xc can be obtained by the following formula, wherein the total scattering curve is obtained by subtracting the background from the diffraction line profile obtained by powder X-ray diffraction measurement (XRD).

[0041] Xc=[Ic / (Ic+Ia)]×100(%)

[0042] The shape of the negative electrode active material is not particularly limited, and is preferably in powder form. The average particle size of the negative electrode active material is preferably 0.1 μm or more, more preferably 0.2 μm or more, further preferably 0.3 μm or more, particularly preferably 0.5 μm or more, preferably 20 μm or less, more preferably 15 μm or less, further preferably 10 μm or less, and particularly preferably 5 μm or less. In addition, the maximum particle size of the negative electrode active material is preferably 150 μm or less, more preferably 100 μm or less, further preferably 75 μm or less, and particularly preferably 55 μm or less. When the average particle size or maximum particle size of the negative electrode active material is too large, the volume change of the negative electrode active material caused by the absorption and release of sodium ions cannot be alleviated during charge and discharge, and there is a tendency for the cycle characteristics to be significantly reduced. On the other hand, when the average particle size of the negative electrode active material is too small, the dispersion state of the powder is poor during paste (paste), and there is a tendency to be difficult to manufacture a uniform electrode. In addition, Fe-Sn alloys such as FeSn2 that are precipitated are easily oxidized by oxygen in the atmosphere.

[0043] Here, the average particle size and the maximum particle size are expressed as the median diameter of the primary particles. 50 (50% volume cumulative diameter) and D 90 (90% volume cumulative diameter) refers to a value measured by a laser diffraction particle size distribution measuring device.

[0044] In order to obtain powders of a predetermined size, a general pulverizer or classifier is used. In order to obtain powders of a predetermined size, for example, a mortar, a ball mill, a vibration ball mill, a satellite ball mill, a planetary ball mill, a jet mill, a sieve, a centrifugal separation, an air classification, etc. are used.

[0045] The negative electrode active material of the present invention can be produced by heating an oxide material as a raw material while supplying a reducing gas, thereby reducing SnO and Fe2O3 contained in the oxide material to form an Fe-Sn alloy such as FeSn2.

[0046] The oxide material is produced by heating and melting the raw material powder prepared to have the above composition at, for example, 600° C. to 1500° C. to form a homogeneous melt, and then cooling and solidifying the melt. The obtained melt-solidified product is subjected to post-processing such as pulverization and classification as necessary.

[0047] The heating and melting can be carried out using a furnace such as an electric heating furnace, a rotary kiln, a microwave heating furnace, a high-frequency heating furnace, laser irradiation, or the like.

[0048] The oxide material is produced by heating and melting a part of the composition to form a homogeneous melt, and then cooling and solidifying it. In addition, the oxide material can also be produced by mixing a molten solid powder that has been subjected to post-processing such as crushing and classification with a powder of the remaining composition and subjecting it to mechanical grinding.

[0049] The oxide material is preferably amorphous, and thus, it is easy to obtain the negative electrode active material of the present invention composed of crystallized glass, wherein the crystallized glass is formed by precipitating Fe-Sn alloys such as FeSn2 in a matrix containing SiO2. In addition, crystals (crystals) such as SnO can also be precipitated inside the oxide material. In addition, the matrix can contain Fe2O3.

[0050] The shape of the oxide material is not particularly limited, and it is preferably in powder form like the negative electrode active material. The average particle size of the oxide material is preferably 0.1μm to 20μm, more preferably 0.2μm to 15μm, further preferably 0.3μm to 10μm, and particularly preferably 0.5μm to 5μm. In addition, the maximum particle size of the oxide material is, for example, preferably 150μm or less, more preferably 100μm or less, further preferably 75μm or less, and particularly preferably 55μm or less. If the average particle size or maximum particle size of the oxide material is too large, the particle size of the obtained negative electrode active material also becomes larger, so there is a tendency to produce the above-mentioned undesirable conditions. In addition, it may not be possible to fully reduce SnO and Fe2O3 to Fe-Sn alloys such as FeSn2 using a reducing gas. On the other hand, if the average particle size of the oxide material is too small, the particle size of the obtained negative electrode active material also becomes small, so there is a tendency to produce the above-mentioned undesirable conditions.

[0051] The heating temperature during the heat treatment is, for example, preferably above 250°C, more preferably above 300°C, and particularly preferably above 400°C. If the heating temperature is too low, the thermal energy imparted is small, so SnO and Fe2O3 in the oxide material are difficult to be reduced to Fe-Sn alloys such as FeSn2. Among them, although the upper limit of the heating temperature is not particularly limited, when it is too high, the reduced Fe-Sn alloy particles such as FeSn2 tend to coarsen, and the cycle characteristics of the negative electrode active material may be significantly reduced. Therefore, the heating temperature is preferably below 700°C, and particularly preferably below 600°C.

[0052] The heating time during the heat treatment is preferably 20 minutes to 1000 minutes, and particularly preferably 60 minutes to 500 minutes. If the heating time is too short, the thermal energy imparted is small, so SnO and Fe2O3 in the oxide material are difficult to be reduced to Fe-Sn alloys such as FeSn2. On the other hand, when the heating time is too long, the reduced Fe-Sn alloy particles such as FeSn2 tend to coarsen, and the cycle characteristics of the negative electrode active material may be significantly reduced.

[0053] The heat treatment can be performed using a furnace such as an electric heating furnace, a rotary kiln, a microwave heating furnace, a high-frequency heating furnace, laser irradiation, or the like.

[0054] As the reducing gas for heat treatment, at least one gas selected from H2, NH3, CO, H2S and SiH4 can be cited. As the reducing gas, from the viewpoint of operability (usability), at least one gas selected from H2, NH3 and CO is preferred, and H2 is particularly preferred.

[0055] When H2 is used as a reducing gas, it is preferably mixed with an inert gas such as N2 or Ar to suppress the danger of explosion. The mixing ratio of the inert gas to H2 is preferably 85% to 99.5% of the inert gas and 0.5% to 15% of H2 in terms of volume %, more preferably 87% to 99% of the inert gas and 1% to 13% of H2, and further preferably 89% to 99% of the inert gas and 1% to 11% of H2.

[0056] In addition, during the heat treatment process, the oxide material (oxide material powder) has a tendency to soften and flow to form an agglomerate. When the oxide material forms an agglomerate, it is difficult for the reducing gas to spread throughout the oxide material, so there is a tendency that the reduction of the oxide material requires a long time. Alternatively, the generated negative electrode active material particles are coarsened, and the battery characteristics may be reduced. Therefore, it is preferred to add an anti-agglomeration agent when the oxide material is heat treated. In this way, the agglomeration of the oxide material during the heat treatment can be suppressed, and the SnO and Fe2O3 in the oxide material can be reduced to Fe-Sn alloys such as FeSn2 in a short time.

[0057] As the anti-agglomeration agent, carbon materials such as conductive carbon and acetylene black can be cited. Carbon materials also have electronic conductivity, so they can also impart conductivity to the negative electrode active material. Among them, as a carbon material, acetylene black with excellent electronic conductivity is preferred.

[0058] The oxide material and the anti-aggregation agent are preferably mixed in a ratio of 80% to 99.5% of the oxide material and 0.5% to 20% of the anti-aggregation agent by mass %. This makes it easy to obtain a negative electrode active material having good initial charge characteristics and stable cycle characteristics.

[0059] By adding a binder and a conductive aid to the negative electrode active material of the present invention, it can be used as a negative electrode material for an electricity storage device.

[0060] Examples of binders include cellulose derivatives such as carboxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxypropyl cellulose, hydroxyethyl cellulose, ethyl cellulose, and hydroxymethyl cellulose, or water-soluble polymers such as polyvinyl alcohol; thermosetting resins such as thermosetting polyimide, phenolic resin, epoxy resin, urea resin, melamine resin, unsaturated polyester resin, and polyurethane; and polyvinylidene fluoride.

[0061] Examples of the conductive auxiliary agent include highly conductive carbon black such as acetylene black and Ketjen black, carbon powder such as graphite, and fibrous carbon such as carbon fiber and carbon nanotube.

[0062] By applying the negative electrode material for an electricity storage device to the surface of a metal foil or the like that functions as a current collector, it can be used as a negative electrode for an electricity storage device.

[0063] In the present invention, the negative electrode material for an electricity storage device including an oxide material that has not been subjected to the above-mentioned heat treatment may be applied to the surface of a metal foil or the like and then subjected to the heat treatment.

[0064] For example, the oxide material which has not been subjected to the above heat treatment and the negative electrode material for a power storage device which contains a binder and a conductive auxiliary agent as necessary may be applied to the surface of a metal foil or the like, and then the heat treatment may be performed by irradiation with laser light.

[0065] At this time, the laser irradiation is preferably performed while supplying a reducing gas, similar to the heat treatment without the use of laser light described above. In this case, the oxide material can be crystallized by the laser irradiation to obtain a negative electrode active material.

[0066] Of course, in the present invention, after laser irradiation in a non-reducing atmosphere, heat treatment may be further performed while supplying a reducing gas, thereby crystallizing the oxide material to obtain a negative electrode active material.

[0067] The wavelength of the laser is preferably in the near infrared region to the infrared region. Specifically, the wavelength of the laser is preferably 750 nm to 1600 nm, more preferably 900 nm to 1400 nm, further preferably 950 nm to 1200 nm, and particularly preferably 1000 nm to 1100 nm, in which case it is easily absorbed by the laser absorption component.

[0068] Therefore, a laser that can irradiate light with a wavelength in the above-mentioned range as laser light is preferable, and examples thereof include semiconductor lasers, YAG lasers, Yb fiber lasers, and YVO4 lasers.

[0069] The negative electrode active material for sodium ion secondary batteries of the present invention can also be applied to hybrid capacitors and the like in which a negative electrode active material used for sodium ion secondary batteries is combined with a positive electrode material for non-aqueous electric double layer capacitors.

[0070] Sodium ion capacitors, which are hybrid capacitors, are a type of asymmetric capacitors in which the charging and discharging principles of the positive and negative electrodes are different. Sodium ion capacitors have a structure that combines the negative electrode used for sodium ion secondary batteries with the positive electrode used for double-layer capacitors. Here, the positive electrode forms a double electric layer on the surface and charges and discharges using physical action (electrostatic action), while the negative electrode charges and discharges through the chemical reaction (absorption and release) of sodium ions in the same way as sodium ion secondary batteries.

[0071] The positive electrode of the sodium ion capacitor uses a positive electrode active material composed of a carbonaceous powder having a high specific surface area such as activated carbon, polyacene, or mesophase carbon. On the other hand, the negative electrode active material of the present invention can be used for the negative electrode.

[0072] (Example)

[0073] Hereinafter, the present invention will be described in detail based on Examples, but the present invention is not limited to these Examples.

[0074] Table 1 shows Examples 1 to 4 and Comparative Example 1.

[0075] [Table 1]

[0076]

[0077] (1) Preparation of oxide materials

[0078] The raw material powder was adjusted using various oxide raw materials, carbonate raw materials, etc. so that the three components of Na2O, Fe2O3, and SiO2 in the composition described in Table 1 would be the composition of Table 1. The obtained raw material powder was put into a melting container, melted at 1400°C in the atmosphere in an electric heating furnace, and then flowed between a pair of cooling rollers to be formed into a film. The obtained film-shaped formed product was pulverized by a ball mill to prepare a base material powder with an average particle size of 2 μm.

[0079] The obtained matrix material powder and SnO raw material powder were mixed in a manner to form the composition of Table 1, and the mixture and stainless steel beads were added using a 45 mL planetary ball mill device (device name: PULVERISETTE7 Classic Line manufactured by Fritch Co., Ltd.), and mechanical grinding was performed at a revolution speed of 700 rpm for 1 hour in an atmospheric atmosphere to prepare an oxide material powder. The structure was determined by powder X-ray diffraction measurement (XRD) of the obtained oxide material powder, and the result was amorphous, and no crystal was detected.

[0080] (2) Preparation of negative electrode active material

[0081] The obtained oxide material powder was heat treated in a mixed gas atmosphere of 90 volume % N2 and 10 volume % H2 at an atmosphere temperature of 450°C for 10 hours. The heat-treated oxide material was crushed using a mortar and pestle to obtain a negative electrode active material powder with an average particle size of 2 μm. The structure of the negative electrode active material powder was examined by XRD, and as a result, crystals of the types and amounts of crystals shown in Table 1 were precipitated.

[0082] (3) Preparation of negative electrode

[0083] The negative electrode active material powder, carbon black as a conductive aid, and thermosetting polyimide resin as a binder were weighed to a mass ratio of 80:5:15, and dehydrated N-methylpyrrolidone was added to prepare a slurry. The obtained slurry was applied to copper foil, vacuum dried at 80°C for 1 hour, and then vacuum dried at 200°C for 6 hours, and then pressed between a pair of rotating rollers to obtain an electrode sheet. The electrode sheet was punched into a diameter of 16 mm using an electrode punching machine to prepare a negative electrode.

[0084] (4) Preparation of test battery

[0085] The obtained negative electrode, a separator composed of a 16 mm diameter polypropylene porous film dried under reduced pressure at 70°C for 8 hours, and metallic sodium as the opposite electrode were stacked, and the electrolyte was infiltrated to produce a test cell. The electrolyte used was 1M NaPF6 solution / EC:DEC=1:1 (EC=ethylene carbonate, DEC=diethyl carbonate). The test cell was assembled in an argon environment with a dew point temperature below -70°C.

[0086] (5) Charge and discharge test

[0087] For the test battery produced, CC (constant current) charging (absorption of sodium ions into the negative electrode active material) was performed from the open circuit voltage to 0V at 25°C, and the amount of electricity (charge capacity) charged to the unit mass of the negative electrode active material was calculated. Next, CC discharge was performed from 0V to 2V (sodium ions were released from the negative electrode active material), and the amount of electricity (discharge capacity) discharged from the unit mass of the negative electrode active material was calculated. In addition, the C value (C rate, charge and discharge rate) was 0.1C. These charges and discharges were regarded as 1 cycle, and 50 cycles of charge and discharge were performed. Based on these results, the coulomb efficiency (discharge capacity / charge capacity) of each cycle was obtained.

[0088] Figure 1 : is a graph showing the battery characteristics in each cycle of the test battery produced in Example 3. In addition, Figure 2 Graph showing the battery characteristics of the test battery produced in Comparative Example 1 in each cycle. Figure 1 As shown, it can be seen that the battery characteristics such as the charge capacity, discharge capacity, and coulombic efficiency at 2 to 50 cycles are stable in the test battery produced in Example 3. On the other hand, in the test battery produced in Comparative Example 1, the battery characteristics such as the charge capacity, discharge capacity, and coulombic efficiency are not stable, especially at 15 to 30 cycles.

[0089] In addition, in each embodiment and comparative example, the maximum and minimum values ​​of the coulomb efficiency at 2 cycles to 50 cycles are shown in Table 1. As shown in Table 1, embodiments 1 to 4 contain Fe2O3 in the composition, and FeSn2 is precipitated at 2 mass % to 53 mass %, so the deviation of the coulomb efficiency at 2 cycles to 50 cycles is small. On the other hand, comparative example 1 does not contain Fe2O3 in the composition, and there is no precipitation of Fe-Sn alloys such as FeSn2, so the deviation of the coulomb efficiency at 2 cycles to 50 cycles becomes large.

[0090] Industrial Applicability

[0091] The negative electrode active material of the present invention can be suitably used in sodium ion secondary batteries used as main power sources for mobile communication devices, portable electronic devices, electric bicycles, electric motorcycles, electric vehicles, and the like.

Claims

1. A negative electrode active material for a sodium ion secondary battery, characterized in that: Contains an amorphous phase containing SiO2 and a Fe-Sn alloy.

2. The negative electrode active material for sodium ion secondary battery according to claim 1, characterized in that: In terms of molar % converted into oxides, it contains 30% to 90% SnO, 2% to 69% SiO2, and 1% to 20% Fe2O3.

3. The negative electrode active material for sodium ion secondary battery according to claim 1 or 2, characterized in that: The Fe-Sn alloy is FeSn2.

4. The negative electrode active material for sodium ion secondary battery according to claim 1 or 2, characterized in that: The crystallized glass is formed by precipitation of the Fe-Sn alloy in a matrix composed of the amorphous phase.

5. The negative electrode active material for sodium ion secondary battery according to claim 1 or 2, characterized in that: The crystallinity is 30% by mass or more and 99% by mass or less.

6. The negative electrode active material for sodium ion secondary battery according to claim 1 or 2, characterized in that: The Fe—Sn alloy has a crystal content of 0.5 mass % or more and 70 mass % or less.

7. The negative electrode active material for a sodium ion secondary battery according to claim 1 or 2, characterized in that: Also contains β-Sn.