Nb-Cr-Al ternary intermediate alloy and preparation and application method thereof
Through the preparation and application of Nb-Cr-Al ternary master alloy, the problem of high melting point inclusions in Ti-Al-Nb-Cr alloy was solved, high-quality and efficient preparation of ingots was achieved, costs were reduced and the yield was improved.
Patent Information
- Application Number
- CN202511064114.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-31
- Publication Date
- 2025-10-17
AI Technical Summary
The existing Ti-Al-Nb-Cr alloy has a problem of high melting point inclusions during the preparation process, which leads to the alloy being scrapped.
Ti-Al-Nb-Cr alloy is prepared by using Nb-Cr-Al ternary master alloy through metallothermic reduction smelting and combining vacuum consumable arc furnace and plasma beam welding technology to avoid the generation of high melting point inclusions.
The metallurgical quality and yield of the ingot are improved, the cost is reduced, and the uniformity of the chemical composition and the stability of the structural properties of the alloy are ensured.
Smart Images

Figure CN120796807A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the technical field of alloy materials, and relates to a Nb-Cr-Al ternary intermediate alloy and a preparation and application method thereof. BACKGROUND
[0002] Titanium-aluminum intermetallic compound material is a high-temperature titanium alloy with excellent performance, and has the advantages of high specific strength, high specific stiffness, corrosion resistance, excellent creep resistance and oxidation resistance, and is currently used for manufacturing low-pressure turbine blades of an aero-engine. In order to meet the overall performance requirements of components under complex working conditions, the composition of the titanium-aluminum intermetallic compound material develops from a binary alloy to a multi-element alloy. Therefore, in order to ensure that the alloy ingot has good metallurgical quality and stable performance, the raw material needs to select a suitable intermediate alloy, otherwise high-density inclusions and low-density inclusions may occur in the ingot.
[0003] Ti-Al-Nb-Cr alloy is a titanium-aluminum intermetallic compound material, containing a large amount of low-melting-point element Al and high-melting-point element Nb, and the melting points of alloying elements are greatly different. At present, Nb-Al binary intermediate alloy is commonly used to add Nb element in the production of titanium alloy, but the melting point of Ti-Al-Nb-Cr alloy is lower than that of titanium alloy, and the solubility of Nb in pure aluminum is extremely low, which will produce a variety of intermetallic compounds with melting points higher than that of Ti-Al-Nb-Cr alloy, which leads to the fact that the ingot of Ti-Al-Nb-Cr alloy using Nb-Al binary alloy as raw material through multiple VAR melting contains unalloyed Nb-Al intermetallic compounds, and the ingot is scrapped due to the presence of high-density inclusions. SUMMARY
[0004] The first object of the present application is to provide a Nb-Cr-Al ternary intermediate alloy for preparing Ti-Al-Nb-Cr alloy, which solves the problem of high-melting-point inclusions in the preparation process of the existing Ti-Al-Nb-Cr alloy, resulting in the scrap of the alloy.
[0005] The second object of the present application is to provide a preparation method of the Nb-Cr-Al ternary intermediate alloy.
[0006] The third object of the present application is to provide an application method of the Nb-Cr-Al ternary intermediate alloy.
[0007] The first technical solution of the present application is a Nb-Cr-Al ternary intermediate alloy, which comprises 50-60% of Nb, 25-32% of Cr, and the balance of Al and other inevitable impurities.
[0008] The ratio of the mass percentage of Nb to the mass percentage of Cr is greater than 1.79.
[0009] The second technical solution of the present application is a preparation method of the Nb-Cr-Al ternary intermediate alloy, which is smelted by using aluminum as a reducing agent, niobium pentoxide and chromium trioxide as oxidizing agents, calcium fluoride as a slagging agent, and potassium chlorate as a heating agent.
[0010] In the smelting process by the metal thermal reduction method, the weight ratio of aluminum particles, niobium pentoxide and chromium trioxide is 0.08-0.25:0.71-0.86:0.37-0.48, the calcium fluoride is added in an amount of 5%-20% of the total weight, and the potassium chlorate is added in an amount of 0-10% of the total weight.
[0011] The Nb-Cr-Al ternary intermediate alloy is smelted by the metal thermal reduction method, which comprises drying the oxidizing agent, then uniformly mixing the dried oxidizing agent, reducing agent and slagging agent in an argon atmosphere, placing the mixed raw materials into a crucible with an Al2O3 slag lining, placing a heating agent on the upper part of the mixed materials, inserting a magnesium strip for ignition into the heating agent, igniting the magnesium strip, maintaining the temperature of the crucible at 2200-2400 DEG C for 40-60 s, and then standing for 10-15 min for slagging after the reaction is completed.
[0012] The third technical solution of the present application is an application method of the Nb-Cr-Al ternary intermediate alloy, which comprises preparing a Ti-Al-Nb-Cr alloy by using the Nb-Cr-Al ternary intermediate alloy.
[0013] The Ti-Al-Nb-Cr alloy comprises 30%-35% of Al, 4%-6% of Nb, 2%-4% of Cr, and the balance of Ti and other inevitable impurities.
[0014] The Nb-Cr-Al ternary intermediate alloy, titanium sponge, aluminum beans and Cr70Al alloy are uniformly mixed in a proportion of 0.7-1:5.5-6.5:2.5-3.5:0-1, pressed into an electrode block, then welded by using a plasma beam welding box to form a primary electrode, and then vacuum self-consumption arc smelting is carried out by using a vacuum self-consumption arc furnace to obtain the Ti-Al-Nb-Cr alloy. The electrode block is welded by using a plasma beam welding box, and the specific process is as follows: pre-vacuum < 10 Pa, leakage rate < 5 Pa / min, argon filling pressure > 20 kPa, argon flow rate > 5 L / min, welding current is 200 A-400 A, and welding voltage is 35 V-70 V.
[0015] 1-3 times of vacuum self-consumption arc smelting are carried out by a vacuum self-consumption arc furnace, pre-vacuum in the furnace before smelting is < 5 Pa, and air leakage rate is < 2 Pa / min; during the arc smelting process, the current of each arc smelting is 2.5-5 kA, the voltage of each arc smelting is 23 V-34 V, and the cooling time after the arc is extinguished is > 6 h.
[0016] The beneficial effects of the present application are as follows: At present, the addition of Nb element in Ti-Al-Nb-Cr alloy is mainly realized by the Nb-Al binary intermediate alloy commonly used in titanium alloy, according to the Nb-Al binary alloy phase diagram, the Nb-Al binary intermediate alloy contains high melting point phases Nb2Al and NbAl3, which leads to that the Ti-Al-Nb-Cr alloy ingot prepared by using the Nb-Al binary intermediate alloy contains high melting point inclusions. According to the Nb-Cr-Al ternary alloy phase diagram, the ternary alloy composed of Nb, Cr and Al in the component range proposed in the present application has a melting point of 1100-1400 DEG C, which is lower than the melting point of Ti-Al-Nb-Cr alloy, and does not contain high melting point phases such as Nb3Al, Nb2Al and NbAl3, greatly reducing the risk of high melting point inclusion defects caused by the large difference in melting point between the intermediate alloy and the base alloy. The use of Nb-Cr-Al ternary intermediate alloy to add Nb in Ti-Al-Nb-Cr alloy can effectively avoid the occurrence of high melting point Nb-Al intermetallic compound in the ingot, and effectively improve the metallurgical quality and yield of the ingot.
[0017] By using the ternary intermediate alloy, the Ti-Al-Nb-Cr alloy can be prepared into an ingot without high melting point inclusions by VAR smelting, which greatly reduces the cost. Through repeated tests, the appropriate slag former, heat generating agent, the appropriate ratio of aluminum particles, niobium pentoxide and chromium sesquioxide are determined, and finally the ternary intermediate alloy with suitable performance is obtained. In the preparation process of Ti-Al-Nb-Cr alloy, the stability of the smelting process is improved, the uniformity of the chemical composition of the ingot is ensured, and the stability of the organization and performance of the alloy is ensured. BRIEF DESCRIPTION OF DRAWINGS
[0018] Figure 1 is the X-ray detection result picture of the head of the rod-shaped Ti-33.45Al-5.07Nb-2.58Cr alloy ingot prepared by the Nb-Cr-Al ternary intermediate alloy in the embodiment 6 of the present application; Figure 2is the X-ray detection result picture of the tail part of the rod-shaped Ti-33.45Al-5.07Nb-2.58Cr alloy ingot prepared by the Nb-Cr-Al ternary intermediate alloy in the embodiment 6 of the present application; Figure 3 is the X-ray detection result picture of the head part of the rod-shaped Ti-31.55Al-4.65Nb-2.37Cr alloy ingot prepared by the Nb-Cr-Al ternary intermediate alloy in the embodiment 7 of the present application; Figure 4 is the X-ray detection result picture of the tail part of the rod-shaped Ti-31.55Al-4.65Nb-2.37Cr alloy ingot prepared by the Nb-Cr-Al ternary intermediate alloy in the embodiment 7 of the present application; DETAILED DESCRIPTION The present application will be described in detail below in combination with the drawings and specific embodiments.
[0019] Embodiment 1 The Nb-Cr-Al ternary intermediate alloy comprises 50% to 60% of Nb, 25% to 32% of Cr, and the balance of Al and other inevitable impurities, wherein the ratio of the mass percentage of Nb to the mass percentage of Cr is greater than 1.79.
[0020] Embodiment 2 The preparation method of the Nb-Cr-Al ternary intermediate alloy comprises smelting the Nb-Cr-Al ternary intermediate alloy by the metal thermal reduction method with aluminum as the reducing agent, niobium pentoxide and chromium trioxide as the oxidizing agent, calcium fluoride as the slag forming agent, and potassium chlorate as the heating agent, and the prepared ternary intermediate alloy comprises 50% of Nb, 28% of Cr, and the balance of Al and other inevitable impurities, and the melting point of the ternary intermediate alloy is 1100 to 1400℃.
[0021] Embodiment 3 The preparation method of the Nb-Cr-Al ternary intermediate alloy comprises smelting the Nb-Cr-Al ternary intermediate alloy by the metal thermal reduction method with aluminum as the reducing agent, niobium pentoxide and chromium trioxide as the oxidizing agent, calcium fluoride as the slag forming agent, and potassium chlorate as the heating agent, and the prepared ternary intermediate alloy comprises 50% of Nb, 28% of Cr, and the balance of Al and other inevitable impurities, and the melting point of the ternary intermediate alloy is 1100 to 1400℃.
[0022] Embodiment 4 A preparation method of Nb-Cr-Al ternary intermediate alloy, comprising smelting Nb-Cr-Al ternary intermediate alloy by metal thermal reduction method with aluminum as reducing agent, niobium pentoxide and chromium trioxide as oxidizing agent, calcium fluoride as slagging agent, and potassium chlorate as heating agent, wherein the weight ratio of aluminum particles, niobium pentoxide and chromium trioxide is 0.08-0.25:0.71-0.86:0.37-0.48, the calcium fluoride is added in an amount of 5%-20% of the total weight of the reducing agent, oxidizing agent, heating agent and slagging agent raw materials, and the potassium chlorate is added in an amount of 0-10% of the total weight of the raw materials.
[0023] The Nb-Cr-Al ternary intermediate alloy is smelted by metal thermal reduction method, which comprises the following steps: drying the oxidizing agent, then uniformly mixing the dried oxidizing agent, reducing agent and slagging agent in an argon atmosphere, placing the mixed raw materials into a crucible with Al2O3 slag as the lining, placing the heating agent on the upper part of the mixed materials, inserting a magnesium strip for ignition into the heating agent, igniting the magnesium strip, maintaining the temperature of the crucible at 2200-2400℃ for 40-60s, and then standing for 10-15min for slagging after the reaction is completed.
[0024] Example 5 An application method of Nb-Cr-Al ternary intermediate alloy, comprising the following steps: preparing Ti-Al-Nb-Cr alloy by using Nb-Cr-Al ternary intermediate alloy, uniformly mixing Nb-Cr-Al ternary intermediate alloy particles, titanium sponge, aluminum beans and Cr70Al alloy according to a proportion of 0.7-0.85:5.8-6:2.6:0.03-0.05, pressing into an electrode block, then welding the electrode block into a primary electrode by using a plasma beam device, and then performing 1-3 times of vacuum self-consumption arc melting by using a vacuum self-consumption arc furnace, wherein the pre-vacuum in the furnace before melting is less than 5Pa, and the air leakage rate is less than 2Pa / min; during the arc melting process, the current of each arc melting is 2.5-5kA, the voltage of each arc melting is 23V-34V, and the cooling time after the arc is extinguished is more than 6h before discharging, thereby obtaining Ti-Al-Nb-Cr alloy, wherein the mass percentage of Al in the Ti-Al-Nb-Cr alloy is 30%-35%, the mass percentage of Nb is 4%-6%, the mass percentage of Cr is 2%-4%, and the balance is Ti and other inevitable impurities.
[0025] Example 6 A preparation method of Ti-Al-Nb-Cr alloy, comprising the following steps: Step 1, preparing Nb-Cr-Al ternary intermediate alloy Step 1.1, weighing the following component raw materials according to the mass percentage The weight ratio of aluminum particles, niobium pentoxide, chromium sesquioxide, and calcium fluoride is 0.08-0.25:0.71-0.86:0.37-0.48, the addition amount of calcium fluoride is 5%-20% of the total weight of the reducing agent, oxidizing agent, heat generating agent and slag forming agent raw materials, and the addition amount of potassium chlorate is 0-10% of the total weight of the raw materials.
[0026] Step 1.2, the aluminum particles weighed in step 1.1 are used as a reducing agent, the niobium pentoxide and chromium sesquioxide are used as oxidizing agents, the calcium fluoride is used as a slag forming agent, and the potassium chlorate is used as a heat generating agent to prepare a Nb-Cr-Al ternary intermediate alloy by a metal thermal reduction method, and the specific process is as follows: Step 1.2.1, drying: the oxidizing agent is placed in a high-temperature oven for drying and removing crystallization water, the drying temperature is 300°C, and the drying time is 3h; Step 1.2.2, mixing: the oxidizing agent, reducing agent and slag forming agent are loaded into a mixer according to the proportion, and uniform mixing is performed, the mixing time is 30min, and argon is filled in the mixer during the mixing process for protection to prevent the Al particles from self-ignition; Step 1.2.3, furnace loading: the mixed raw materials are placed in a crucible with an Al2O3 slag lining, the heat generating agent is placed on the top of the mixture, and a magnesium strip for ignition is inserted into the heat generating agent; Step 1.2.4, ignition: the placed magnesium strip is ignited, the aluminum thermal reaction of the oxidizing agent and reducing agent is started with the assistance of the heat generating agent, and the reaction temperature in the crucible is maintained at 2300°C, and the reaction lasts for 48s; Step 1.2.5, slagging: after the reaction is completed, the slagging is performed after 15min of standing; Step 1.2.6, crushing: the cooled intermediate alloy ingot is subjected to multi-stage crushing to obtain an intermediate alloy with a particle size of <5mm, the mass percentage of Nb in the Nb-Cr-Al ternary intermediate alloy is 57.09%, the mass percentage of Cr is 29.98%, and the balance is Al and other unavoidable impurities.
[0027] Step 2, using the Nb-Cr-Al ternary intermediate alloy prepared in step 1 to prepare Ti-Al-Nb-Cr alloy, including uniformly mixing the Nb-Cr-Al ternary intermediate alloy particles with titanium sponge, aluminum beans and Cr70Al alloy in a ratio of 0.7:5.8:2.6:0.05, pressing into an electrode block, and then using a plasma beam welding box to weld the electrode block into a primary electrode, and the specific welding process is as follows: pre-vacuum 7.3 Pa, leakage rate 2.5 Pa / min, argon filling pressure 51 kPa, argon flow rate >8.5 L / min, welding current 270 A, welding voltage 45 V, and then performing three times of VAR melting through a vacuum consumable arc furnace, and the specific melting process requirements are as follows: the first / second / third times of melting are performed by using a φ160 / 220 / 280 mm crucible, the pre-vacuum before melting is 3.5 Pa, the air leakage rate is 1.6 Pa / min, the first / second / third times of melting current are 3 / 3.5 / 4.2 kA, the first / second / third times of melting voltage are 25 / 28 / 33 V, and the cooling time after arc collection is 12 h, and a Ti-Al-Nb-Cr alloy ingot containing multiple alloy elements is obtained, and the composition of the Ti-Al-Nb-Cr alloy ingot is Ti-33.45Al-5.07Nb-2.58Cr, and the alloy ingot is in a rod shape and has a diameter of 280 mm.
[0028] The Ti-33.45Al-5.07Nb-2.58Cr alloy prepared in Example 6 is subjected to X-ray detection, and the detection results are shown in Figure 1 and Figure 2 As can be seen from Figure 1 and Figure 2 , the Ti-33.45Al-5.07Nb-2.58Cr alloy prepared by using the Nb-Cr-Al ternary intermediate alloy of the application has no unmeltable substance and no inclusion defects, and the structure is dense.
[0029] The compositions of the Ti-33.45Al-5.07Nb-2.58Cr alloy at different positions prepared in Example 6 are analyzed, and the analysis results are shown in Table 1. Table 1 Composition list of Ti-33.45Al-5.07Nb-2.58Cr alloy at different positions
[0030] The percentages of Al, Nb and Cr in the head, middle and tail of the rod-shaped Ti-33.45Al-5.07Nb-2.58Cr alloy ingot are listed in Table 1, and the balance is Ti and other unavoidable impurities. As can be seen from Table 1, the chemical composition of the Ti-33.45Al-5.07Nb-2.58Cr alloy prepared by using the Nb-Cr-Al ternary intermediate alloy of the application is uniform.
[0031] Example 7 A preparation method of a Ti-Al-Nb-Cr alloy, comprising the following steps: Step 1, preparing a Nb-Cr-Al ternary intermediate alloy Step 1.1, the following component raw materials are weighed according to the mass percentage The weight ratio of aluminum particles, niobium pentoxide, chromium sesquioxide, calcium fluoride and potassium chlorate is 0.08-0.25:0.71-0.86:0.37-0.48, the addition amount of calcium fluoride is 5%-20% of the total weight of the raw materials, and the addition amount of potassium chlorate is 0-10% of the total weight of the raw materials.
[0032] Step 1.2, using the aluminum particles weighed in step 1.1 as a reducing agent, the niobium pentoxide and chromium sesquioxide as oxidizing agents, the calcium fluoride as a slag forming agent, and the potassium chlorate as a heating agent, a Nb-Cr-Al ternary intermediate alloy is prepared by a metal thermal reduction method, comprising the following steps: Step 1.2.1, drying: the oxidizing agent is placed in a high-temperature oven for drying and removing crystallization water, the drying temperature is 300°C, and the drying time is 3h; Step 1.2.2, mixing: the oxidizing agent, reducing agent and slag forming agent are loaded into a mixer according to the proportion, and uniformly mixed, the mixing time is 30min, and argon is filled in the mixer during the mixing process to prevent the Al particles from self-igniting; Step 1.2.3, furnace loading: the mixed raw materials are placed in a crucible with an Al2O3 slag lining, the heating agent is placed on the top of the mixture, and a magnesium strip for ignition is inserted into the heating agent; Step 1.2.4, ignition: the placed magnesium strip is ignited, the aluminum thermal reaction of the oxidizing agent and the reducing agent is started with the assistance of the heating agent, and the reaction temperature in the crucible is maintained at 2350°C, and the reaction lasts for 55s; Step 1.2.5, slagging: after the reaction is completed, the slagging is carried out after 13min; Step 1.2.6, crushing: the cooled intermediate alloy ingot is crushed in multiple stages to obtain an intermediate alloy with a particle size of <5mm, the mass percentage of Nb in the Nb-Cr-Al ternary intermediate alloy is 57.05%, the mass percentage of Cr is 29.88%, and the balance is Al and other unavoidable impurities.
[0033] Step 2, using the Nb-Cr-Al ternary intermediate alloy prepared in step 1 to prepare Ti-Al-Nb-Cr alloy, including uniformly mixing the Nb-Cr-Al ternary intermediate alloy particles with titanium sponge, aluminum beans and Cr70Al alloy in a ratio of 0.85:5.9:2.6:0.03, pressing into an electrode block, and then using a plasma beam welding box to weld the electrode block into a primary electrode, and the specific welding process is as follows: pre-vacuum <2.5 Pa, leakage rate <1.5 Pa / min, argon pressure 55 kPa, argon flow rate 6.5 L / min, welding current 280 A, welding voltage 48 V, and then performing two VAR melting through a vacuum consumable arc furnace, and the specific melting process requirements are as follows: the first melting and the second melting are performed using a φ160 / 220 mm crucible, the pre-vacuum before melting is 1.2 Pa, the air leakage rate is 0.8 Pa / min, the first melting and the second melting currents during melting are 3.5 kA and 4.2 kA respectively, the first melting and the second melting voltages are 24 V and 32 V respectively, and the alloy ingot is taken out after cooling for 8 h after arc collection, and a Ti-Al-Nb-Cr alloy ingot containing multiple alloy elements is obtained, and the composition of the Ti-Al-Nb-Cr alloy ingot is Ti-31.55Al-4.65Nb-2.37Cr, and the alloy ingot is in a rod shape and has a diameter of 220 mm.
[0034] The Ti-31.55Al-4.65Nb-2.37Cr alloy prepared in Example 7 is subjected to X-ray detection, and the detection results are shown in Figure 3 and Figure 4 As can be seen from Figure 3 and Figure 4 , the Ti-31.55Al-4.65Nb-2.37Cr alloy prepared by using the Nb-Cr-Al ternary intermediate alloy of the application has no unmeltable substances in the interior.
[0035] The compositions of the Ti-31.55Al-4.65Nb-2.37Cr alloy at different positions prepared in Example 7 are analyzed, and the analysis results are shown in Table 2. Table 2 Composition list of Ti-31.55Al-4.65Nb-2.37Cr alloy at different positions
[0036] The percentages of Al, Nb and Cr in the head, middle and tail of the rod-shaped Ti-31.55Al-4.65Nb-2.37Cr alloy ingot are listed in Table 2, and the balance is Ti and other unavoidable impurities. As can be seen from Table 2, the chemical composition of the Ti-Al-Nb-Cr alloy prepared by using the Nb-Cr-Al ternary intermediate alloy of the application is uniform, which ensures the stability of the organization and performance of the alloy.
Claims
1. Nb-Cr-Al ternary master alloy, characterized in that: It includes 50% to 60% by mass of Nb, 25% to 32% by mass of Cr, and the remainder is Al and other inevitable impurities.
2. The Nb-Cr-Al ternary master alloy according to claim 1, characterized in that: The ratio of the mass percentage of Nb to the mass percentage of Cr is greater than 1.
79.
3. A method for preparing a Nb-Cr-Al ternary master alloy, characterized in that the Nb-Cr-Al ternary master alloy is smelted by a metallothermic reduction method using aluminum as a reducing agent, niobium pentoxide and chromium trioxide as oxidants, calcium fluoride as a slagging agent, and potassium chlorate as a heating agent.
4. The method for preparing the Nb-Cr-Al ternary master alloy according to claim 3, characterized in that: During the metallothermic reduction smelting process, the weight ratio of aluminum particles, niobium pentoxide, and chromium trioxide is 0.08-0.25:0.71-0.86:0.37-0.48, the amount of calcium fluoride added is 5%-20% of the total weight, and the amount of potassium chlorate added is 0-10% of the total weight.
5. The method for preparing the Nb-Cr-Al ternary master alloy according to claim 3, characterized in that: The Nb-Cr-Al ternary master alloy is smelted by a metallothermic reduction method, which includes drying an oxidant, then uniformly mixing the dried oxidant, reducing agent and slagging agent in an argon atmosphere, placing the mixed raw materials into a crucible lined with Al2O3 slag, placing a heating agent on top of the mixture, inserting a magnesium rod for ignition into the heating agent, igniting the magnesium rod, maintaining the crucible temperature at 2200-2400°C for a reaction of 40s-60s, and standing for 10min-15min after the reaction to skim off the slag.
6. Application method of Nb-Cr-Al ternary master alloy, characterized in that: The invention comprises adopting Nb-Cr-Al ternary master alloy to prepare Ti-Al-Nb-Cr alloy.
7. The application method of the Nb-Cr-Al ternary master alloy according to claim 6, characterized in that: The Ti-Al-Nb-Cr alloy comprises 30% to 35% by mass of Al, 4% to 6% by mass of Nb, 2% to 4% by mass of Cr, and the remainder being Ti and other inevitable impurities.
8. The application method of the Nb-Cr-Al ternary master alloy according to claim 7, characterized in that: The Nb-Cr-Al ternary master alloy is uniformly mixed with sponge titanium, aluminum beans and Cr70Al alloy in a ratio of 0.7-1:5.5-6.5:2.5-3.5:0-1, and pressed into an electrode block. The electrode block is then welded using a plasma beam welding box to form a primary electrode, and then vacuum consumable arc melting is performed in a vacuum consumable arc furnace to obtain a Ti-Al-Nb-Cr alloy.
9. The application method of the Nb-Cr-Al ternary master alloy according to claim 8, characterized in that: The electrode block is welded using a plasma beam welding box. The specific process is: pre-vacuum <10Pa, leak rate <5Pa / min, argon filling pressure >20kPa, argon flow >5L / min, welding current 200A~400A, and welding voltage 35V~70V.
10. The application method of the Nb-Cr-Al ternary master alloy according to claim 8, characterized in that: The vacuum consumable arc furnace is used to perform vacuum consumable arc melting 1 to 3 times, with the pre-vacuum in the furnace being less than 5 Pa and the gas leakage rate being less than 2 Pa / min before melting. During the arc melting process, the current of each arc melting is 2.5-5 kA, the voltage of each arc melting is 23 V-34 V, and the cooling time after arc closure is greater than 6 hours before the furnace is removed.