Water-based polyurethane adhesive composition

By adjusting the ratio of soft to hard segments and molecular weight of polyurethane polymers, a water-based PU adhesive with low-temperature activation was prepared, solving the problems of high-temperature activation and insufficient strength, and achieving excellent initial and final adhesive strength at low temperatures.

CN121420045APending Publication Date: 2026-01-27HENKEL KGAA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380099953.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-07-05
Publication Date
2026-01-27

AI Technical Summary

Technical Problem

Existing water-based PU adhesives have the problem of high activation temperature and inability to achieve excellent initial and final bond strength when bonding temperature-sensitive substrates.

Method used

A water-based polyurethane adhesive composition was prepared by selecting a specific weight ratio and weight-average molecular weight (Mw) between the soft and hard segments of the polyurethane polymer, which was then activated at low temperatures to achieve excellent initial and final adhesive strength.

Benefits of technology

When activated at temperatures below 40°C, the water-based polyurethane adhesive composition achieves both excellent initial bond strength and excellent final bond strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to a water-based polyurethane adhesive composition comprising: (a) a polyurethane polymer comprising a soft segment derived from a polyester polyol and a hard segment derived from a polyisocyanate; wherein the weight ratio between the soft segment and the hard segment is greater than 5.6, and the weight average molecular weight of the polyurethane polymer does not exceed 20000 g / mol; (b) water; (c) optionally a thickener; (d) optionally, a defoaming agent; and (e) optionally a matting agent. The invention also relates to an activation product obtained from the composition, and an article comprising the activation product or assembled using the composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to water-based polyurethane adhesive compositions, cured products obtained from said compositions, and articles comprising said cured products or assembled using said compositions. Background Technology

[0002] Today, water-based adhesives are replacing solvent-based adhesives due to environmental concerns. Water-based polyurethane (PU) adhesives use water as a solvent or dispersant, with PU particles dispersed in the water. Compared to solvent-based PU adhesives, water-based PU adhesives have advantages such as being non-toxic, non-flammable, having low volatile organic compounds (VOCs), and being low-cost.

[0003] Commercially available water-based PU dispersion (PUD) adhesives typically have activation temperatures of 50-60°C and 80-100°C. Such high activation temperatures limit their use in bonding temperature-sensitive substrates such as foams, films, synthetic leather in suitcases, footwear, and textiles. Some water-based PUD adhesives exist with lower activation temperatures, but they do not achieve both excellent initial and final bond strength.

[0004] Therefore, there is a need in the art to develop water-based PU adhesive compositions that have a low activation temperature but can achieve both excellent initial bond strength and excellent final bond strength. Summary of the Invention

[0005] The inventors of this application have discovered through in-depth research that by specifically selecting the weight ratio between the soft and hard segments of the polyurethane polymer and the weight-average molecular weight (Mw), water-based polyurethane adhesive compositions can be activated at low temperatures and simultaneously achieve both excellent initial adhesive strength and excellent final adhesive strength.

[0006] In a first aspect, this application provides a water-based polyurethane adhesive composition comprising: (a) A polyurethane polymer comprising soft segments derived from polyester polyols and hard segments derived from polyisocyanates; wherein the weight ratio between the soft segments and the hard segments is greater than 5.6, and the weight-average molecular weight (Mw) of the polyurethane polymer does not exceed 20,000 g / mol. (b) Water; (c) Any available thickener, (d) Any available defoamer; and (e) An optional matting agent.

[0007] In a second aspect, this application provides an activated product obtained from the composition of the first aspect.

[0008] In a third aspect, this application provides articles comprising a cured product of the second aspect or articles assembled using the composition of the first aspect.

[0009] In a fourth aspect, this application provides a method for bonding a substrate with a composition according to the first aspect, the method comprising: (i) Apply the composition to one or two substrates, (ii) Activate the composition at a temperature not exceeding 40°C, such as 35°C, for 3-4 minutes. (iii) Fit the two substrates together and press them together.

[0010] The advantages of this invention include: (1) The composition of this application can be activated at low temperatures (e.g., below 40°C, such as 35°C, 36°C, 37°C, 38°C, 39°C), and (2) The activated product of the composition has both excellent initial adhesive strength and excellent final adhesive strength. Detailed Implementation

[0011] Those skilled in the art will understand that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the invention. Unless explicitly stated otherwise, each aspect so described may be combined with any one or more other aspects. In particular, any feature indicated as preferred or advantageous may be combined with any one or more other features indicated as preferred or advantageous.

[0012] Unless otherwise specified, the terminology used in the context of this invention shall be interpreted in accordance with the following definitions.

[0013] Unless otherwise specified, all weight % (wt.% or % by weight) values ​​listed in this document are weight percentages.

[0014] Unless otherwise specified, the singular forms “a / an” and “the” used herein include both the singular and plural referents.

[0015] The term “comprising / comprises” as used herein is synonymous with “including / includes” or “containing / contains”, and is inclusive or open-ended, and does not exclude additional unlisted members, elements, or method steps.

[0016] As used herein, the term “consistently of” means that the listed components constitute the bulk of the composition, for example, at least 90% by weight of the composition.

[0017] The term “composed of” as used herein is closed and excludes any additional, unlisted, intentionally added members, elements, or method steps.

[0018] The terms “at least one” or “one or more” used in this article to define components refer to the type of component, not the absolute number of molecules.

[0019] In this document, the terms “about” and “approximately” used in conjunction with numerical values ​​refer to values ​​±10%, preferably ±5%. All numerical values ​​in this document should be interpreted as being modified by the term “about”.

[0020] As used herein, the term "water-based polyurethane adhesive composition" means that the composition contains less than 0.5% by weight, preferably less than 0.1% by weight, more preferably less than 0.01% by weight, and most preferably 0% of one or more organic solvents.

[0021] Unless otherwise specified, the definition of numerical endpoints includes all numbers and fractions falling into their respective ranges, as well as the listed endpoints.

[0022] Unless otherwise defined, all terms used in this invention (including technical and scientific terms) have the meanings commonly understood by one of ordinary skill in the art to which this invention pertains.

[0023] The water-based polyurethane adhesive composition will be described in detail below.

[0024] This water-based polyurethane adhesive composition comprises, is substantially composed of, or is composed of the following substances: (a) A polyurethane polymer comprising soft segments derived from polyester polyols and hard segments derived from polyisocyanates; wherein the weight ratio between the soft segments and the hard segments is greater than 5.6, and the weight-average molecular weight of the polyurethane polymer is not more than 20,000 g / mol. (b) Water; (c) Any available thickener, (d) Any available defoamer; and (e) Any matting agent present.

[0025] Component (a): Polyurethane polymer The polyurethane (PU) polymers used in this article necessarily contain soft segments derived from polyester polyols, preferably polyester diols, and hard segments derived from polyisocyanates, preferably diisocyanates; and must meet the following conditions: (1) the weight ratio between soft segments and hard segments is greater than 5.6, such as greater than 5.65, and (2) the Mw of the polyurethane polymer does not exceed 20000 g / mol.

[0026] As used herein, the terms “soft segments derived from polyester polyols” and “hard segments derived from polyisocyanates” mean that during PU preparation, polyester polyols react with polyisocyanates to form PU polymers, and during the reaction, the polyester polyols lose one or more atoms and the polyisocyanates gain one or more atoms, with the remaining portion of the polyester polyols constituting soft segments and the remaining portion of the polyisocyanates constituting hard segments.

[0027] The PU polymer applicable to this application is a non-reactive PU polymer that does not contain any reactive -NCO groups in its molecular chain. Therefore, the PU polymer is obtained by reacting a slightly molar excess of polyester polyol with a polyisocyanate to ensure that no reactive -NCO groups are left in the chain.

[0028] The PU polymers applicable to this application may optionally contain other structural units, but preferably, based on the total weight of the PU polymer, the content of said other structural units is less than 5% by weight, preferably less than 4% by weight, less than 3% by weight, less than 2% by weight, less than 1% by weight, or less than 0.5% by weight.

[0029] Preferably, the polyester polyol used herein is a polyester diol, which is preferably selected from polyethylene adipate diol (PEA diol), polybutylene adipate diol (PBA diol), polypentyl adipate diol (PNA diol), polyhexyl adipate diol (PHA diol), polypropylene adipate diol (PPA diol), and combinations thereof. These polyester diols can have molecular weights (Mw) in the range of 800 to 3000 g / mol (e.g., 850, 900, 950, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900 g / mol).

[0030] The weight-average molecular weight (Mw) mentioned in this application was determined by gel permeation chromatography (GPC).

[0031] Preferably, the polyisocyanates used herein are selected from 4,4'-diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), dicyclohexylmethane-4,4'-diisocyanate (HMDI), and combinations thereof.

[0032] The PU polymers applicable to this application can be prepared by any method known in the art, for example, with or without the use of a catalyst and a chain extender during preparation.

[0033] By way of example only, the PU polymers applicable to this application can be obtained by reacting PBA diol with HDI, or by reacting PBA diol with a mixture of HDI and IPDI, or by reacting PBA diol with MDI, or by reacting PBA diol with TDI, or by reacting PBA diol with HMDI, or by reacting PEA diol with HDI, or by reacting PEA diol with a mixture of HDI and IPDI, or by reacting PEA diol with MDI, or by reacting PEA diol with TDI, or by reacting PEA diol with HMDI, or by reacting PNA diol with HDI, or by reacting PNA diol with HDI and IPDI. The reaction can be carried out by reacting a mixture of PNA diols with MDI, or by reacting PNA diols with TDI, or by reacting PNA diols with HMDI, or by reacting PHA diols with HDI, or by reacting PHA diols with a mixture of HDI and IPDI, or by reacting PHA diols with MDI, or by reacting PHA diols with TDI, or by reacting PHA diols with HMDI, or by reacting PPA diols with HDI, or by reacting PPA diols with a mixture of HDI and IPDI, or by reacting PPA diols with MDI, or by reacting PPA diols with TDI, or by reacting PPA diols with HMDI, etc.

[0034] One condition that the PU polymer applicable to this application must meet is that the weight ratio between soft segments and hard segments is greater than 5.6, preferably greater than 5.65, but preferably less than 10, less than 9, less than 8, less than 7, or less than 6.5.

[0035] Another condition that the PU polymer applicable to this application must meet is that the Mw of the PU polymer does not exceed 20,000 g / mol; preferably, the Mw of the PU polymer is greater than 15,000 g / mol, such as greater than 16,000 g / mol, greater than 17,000 g / mol, or greater than 18,000 g / mol, but does not exceed 20,000 g / mol, preferably not more than 19,500 g / mol.

[0036] Based on the total weight of the composition, component (a) PU polymer may be included in the composition in an amount of 40 to 55% by weight, or 45 to 50% by weight, such as 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55% by weight, or any range between the two figures listed above.

[0037] Component (b): Water Water constitutes a major component of the compositions of this application. Water may be mixed with the PU polymer during preparation, and / or water may be pre-mixed with a portion of the PU polymer to form a PU aqueous dispersion (PUD), and then water may be added as needed during composition preparation.

[0038] Whether added during composition preparation or pre-mixed with the PU polymer to form a PUD, water may be included in the composition in an amount of 45 to 60% by weight, or 50 to 55% by weight, such as 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59% by weight, or any range between the two figures listed above, based on the total weight of the composition.

[0039] Component (c): Thickener Depending on the requirements of application, the composition of this application may optionally contain a thickener.

[0040] The purpose of a thickener is to increase the viscosity of the composition to facilitate coating or application. Conventional thickeners in the art can be used herein without particular limitation. Preferably, a polyurethane polymer having a structural unit similar to that of component (a) can be used, but the weight ratio of soft to hard segments and Mw of the polyurethane polymer of the thickener are not limited, as long as they achieve the thickening purpose.

[0041] If present, the amount of thickener in the composition of this application may be adjusted without particular limitation as needed, provided that the desired effect of the composition or adhesive is not negatively affected. Preferably, based on the total weight of the composition, component (c) thickener may be included in the composition in an amount of 0.5 to 2% by weight, or 0.6 to 1.5% by weight, such as 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9% by weight, or any range between the two figures listed above.

[0042] Component (d): Defoamer The compositions of this application may optionally contain a defoamer to reduce foam formation during composition preparation and / or application. Conventional defoamers in the art may be used herein without particular limitation.

[0043] If present, the amount of defoamer in the composition of this application can be adjusted without particular limitation according to actual needs, as long as the desired effect of the composition or adhesive is not negatively affected. Preferably, based on the total weight of the composition, component (d) defoamer may be included in the composition in an amount of 0.01 to 0.2% by weight, or 0.05 to 0.15% by weight, such as 0.02, 0.03, 0.04, 0.05, 0.06, 0.08, 0.12, 0.14, 0.16, 0.18% by weight, or any range between the two figures listed above.

[0044] Component (e): matting agent The compositions of this application may optionally contain a matting agent to reduce the light reflection effect of the adhesive. Conventional matting agents in the art may be used herein without particular limitation.

[0045] If present, the amount of matting agent in the composition of this application may be adjusted without particular limitation as needed, provided that the desired effect of the composition or adhesive is not negatively affected. Preferably, based on the total weight of the composition, component (e) matting agent may be included in the composition in an amount of 0.01 to 0.2% by weight, or 0.05 to 0.15% by weight, such as 0.02, 0.03, 0.04, 0.05, 0.06, 0.08, 0.12, 0.14, 0.16, 0.18% by weight, or any range between the two figures listed above.

[0046] In a second aspect, this application also provides an activated product obtained from the composition of this application. The activated product of the composition can be obtained by heating the applied composition at a temperature not exceeding 40°C (e.g., 35°C, 36°C, 37°C, 38°C, 39°C). The duration of heating activation can be, for example, 3-4 minutes.

[0047] In a third aspect, this application also provides articles comprising the activated product or assembled using the compositions of this application. For example, the articles may be footwear, shoe soles, textiles, and suitcases.

[0048] In a fourth aspect, this application also provides a method for bonding substrates together using the composition of this application, said method comprising, substantially comprising, or comprising the following steps: (i) Apply the composition to one or two substrates, (ii) Activate the composition at a temperature not exceeding 40°C (e.g., 35°C, 36°C, 37°C, 38°C, 39°C) for 3-4 minutes. (iii) Fit the two substrates together and press them together.

[0049] Example The invention will now be described through the following embodiments. These embodiments are intended to help those skilled in the art better understand and practice the invention. The scope of the invention is not limited by the embodiments, but is defined by the appended claims. Unless otherwise stated, all parts and percentages are based on weight.

[0050] Materials used in the examples: Test methods for initial bond strength and final bond strength: The composition was applied to two rubber sheets measuring 20 mm (width) × 100 mm (length), and the sheets were heated at approximately 35°C for 3 minutes. The two sheets were then attached and pressed together. The pressure was 20 kgf, and the pressing time was 15 seconds. Initial bond strength was tested using an Instron LEGEND 2344 tensile testing machine at a peel speed of 150 mm / min, performing a 180° peel test within 1 minute after pressing. Final bond strength was tested using an Instron LEGEND 2344 tensile testing machine at a peel speed of 150 mm / min, performing a 180° peel test 24 hours after pressing.

[0051] Evaluation criteria: An initial bond strength greater than 2.5 kgf / cm is marked as excellent. A final bond strength greater than 4.0 kgf / cm is also marked as excellent.

[0052] Examples 1-2 and Comparative Examples 1-4 (Ex 1 to 2 and CE 1 to 4) Use a mixer to mix all the ingredients listed in Table 1 to form the respective compositions. Test the properties of each composition using the methods described above.

[0053] Table 1:

[0054] As shown in Table 1, when the weight ratio of the soft segment to the hard segment of the PU polymer is greater than 5.6 and the Mw of the PU polymer is less than 20,000 g / mol (Ex1 to Ex2), the activated PU adhesive can achieve both excellent initial adhesive strength and excellent final adhesive strength. When the weight ratio of the soft segment to the hard segment of the PU polymer is less than 5.6, neither excellent initial adhesive strength nor excellent final adhesive strength is achieved (CE1 to CE2), or excellent initial adhesive strength is not achieved (CE3). When the weight ratio of the soft segment to the hard segment of the PU polymer is greater than 5.6 but the Mw of the PU polymer is greater than 20,000 g / mol (CE4), excellent initial adhesive strength is not achieved.

[0055] Although some preferred embodiments have been described, many modifications and variations can be made to them based on the above teachings. Therefore, it should be understood that the invention can be practiced in ways different from those specifically described without departing from the scope of the appended claims.

Claims

1. A water-based polyurethane adhesive composition, said water-based polyurethane adhesive composition comprising: (a) A polyurethane polymer comprising soft segments derived from polyester polyols and hard segments derived from polyisocyanates; wherein the weight ratio between the soft segments and the hard segments is greater than 5.6, and the weight-average molecular weight of the polyurethane polymer is not more than 20,000 g / mol. (b) Water; (c) Any available thickener, (d) Any available defoamer; and (e) Any matting agent present.

2. The composition according to claim 1, wherein the polyester polyol is a polyester diol.

3. The composition according to claim 2, wherein the polyester diol is selected from poly(ethylene adipate) diol, poly(butylene adipate) diol, poly(neopentyl adipate) diol, poly(hexyl adipate) diol, poly(propylene adipate) diol, and combinations thereof.

4. The composition according to any one of claims 1-3, wherein the polyisocyanate is selected from 4,4'-diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), dicyclohexylmethane-4,4'-diisocyanate (HMDI), and combinations thereof.

5. The composition according to any one of claims 1-4, wherein, Based on the total weight of the composition, the content of the polyurethane polymer (a) is 40-55% by weight, preferably 45-50% by weight.

6. The composition according to any one of claims 1-5, wherein, Based on the total weight of the composition, the water (b) content is 50-60% by weight, preferably 50-55% by weight.

7. The composition according to any one of claims 1-6, wherein, Based on the total weight of the composition, the content of the thickener (c) is 0.5-2% by weight, preferably 0.6-1.5% by weight.

8. The composition according to any one of claims 1-7, wherein, Based on the total weight of the composition, the content of the defoamer (d) is 0.01-0.2% by weight, preferably 0.05-0.15% by weight.

9. The composition according to any one of claims 1-8, wherein, Based on the total weight of the composition, the content of the matting agent (e) is 0.01-0.2% by weight, preferably 0.05-0.15% by weight.

10. The composition according to any one of claims 1-9, wherein the polyurethane polymer has a weight-average molecular weight greater than 15,000 g / mol, such as greater than 16,000 g / mol, or greater than 18,000 g / mol, but not exceeding 20,000 g / mol, preferably not exceeding 19,500 g / mol.

11. The composition according to any one of claims 1-10, wherein the weight ratio between the soft segment and the hard segment is greater than 5.65, and preferably less than 10 and less than 8.

12. An activated product obtained from the composition according to any one of claims 1-11, wherein the composition is activated at a temperature not exceeding 40°C, such as 35°C.

13. An article comprising the activated product according to claim 12, or assembled using a composition according to any one of claims 1-11.

14. The article of claim 13, wherein the article of claim 13 is selected from footwear, shoe soles, textiles and suitcases.

15. A method for bonding a substrate with the composition according to any one of claims 1-11, the method comprising: (i) Apply the composition to one or two substrates, (ii) Activate the composition at a temperature not exceeding 40°C, such as 35°C, for 3-4 minutes. (iii) The two substrates are fitted together and pressed together.