Rust removal lubricant for metal and preparation method of rust removal lubricant

Through the synergistic effect of components such as linoleic acid modified resin acid derivatives, quaternary ammonium salt modified montmorillonite-vegetable oil complex and quaternized lignin derivatives, the problems of strong corrosiveness, slow speed, poor penetration and environmental pollution of existing rust removers are solved, and the effects of high efficiency rust removal, long-term lubrication and rust prevention are achieved. It is suitable for rust removal, lubrication and protection of mechanical equipment and automotive parts.

CN122038023APending Publication Date: 2026-05-15GUANGZHOU HEXIN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610301605.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-12
Publication Date
2026-05-15

AI Technical Summary

Technical Problem

Existing rust removers have problems such as strong corrosiveness to metal substrates, slow rust removal speed, poor penetration, easy secondary rusting after treatment, serious environmental pollution, and lack of lubrication function, making it difficult to meet the high efficiency, environmental protection and safety requirements of industrial production.

Method used

The product utilizes components such as linoleic acid-modified resin acid derivatives, quaternary ammonium salt-modified montmorillonite-vegetable oil complexes, quaternized lignin derivatives, and d-limonene. Through synergistic effects, it achieves rapid penetration, rust removal, film formation, and lubrication, forming a nanoscale dispersion that provides long-lasting rust prevention.

Benefits of technology

It achieves rapid rust removal, long-lasting lubrication and rust prevention, reduces VOC content, meets environmental protection requirements, and is suitable for rust removal, lubrication and protection of mechanical equipment and automotive parts, extending the service life of metal parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a rust removal lubricant for metal and a preparation method of the rust removal lubricant, and belongs to the technical field of metal rust removal and corrosion prevention. The rust removal lubricant for the metal comprises a linoleic acid modified resin acid derivative, a quaternary ammonium salt modified montmorillonite-vegetable oil compound, a quaternized lignin derivative, d-limonene, epoxidized soybean oil, maleic anhydride modified tung oil, benzotriazole, a nonionic surfactant, a pH buffer system and deionized water. Through the molecular design and synergistic effect of core components such as the linoleic acid modified resin acid derivative, the quaternary ammonium salt modified montmorillonite-vegetable oil compound, the quaternized lignin derivative and the d-limonene, excellent permeability, rapid rust removal capacity and long-acting lubricating and anti-rust performance are achieved; the metal rust remover can be widely applied to rust removal, lubrication and protection of metal products such as mechanical equipment, automobile parts and hardware tools, the service life of the metal parts is prolonged, meanwhile, bio-based raw materials are adopted, the VOC content is low, and the environment-friendly requirement is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of metal rust removal and corrosion prevention, and more specifically, relates to a rust-removing lubricant for metals and its preparation method. Background Technology

[0002] Metal corrosion is a common problem in industrial production and daily life, affecting not only the appearance of equipment but also severely reducing its mechanical strength and service life. Various rust removal products have emerged to address this issue, but current technologies still face many challenges.

[0003] Traditional rust removers mostly use inorganic strong acid systems such as hydrochloric acid and sulfuric acid. These products remove rust quickly and are inexpensive. Their pH value is usually between 1.0 and 2.0, and they can remove the surface rust layer in 10-15 minutes at room temperature. However, these products have the following obvious defects: (1) They are highly corrosive to the metal substrate. During the rust removal process, a large amount of hydrogen gas is released, which leads to hydrogen embrittlement and over-corrosion of the metal, and the material loss rate is as high as 5-8%; (2) They cannot distinguish between the rust layer and the base metal. Over-treatment will form a pitted surface; (3) The acid mist volatilizes seriously, the working environment is harsh, and it is very harmful to the health of operators; (4) Waste liquid is difficult to treat, and the cost of treating each ton of waste liquid is about 300-500 yuan; (5) The surface activity of the metal after treatment is high, and it is very easy to rust again. It is necessary to carry out rust prevention treatment immediately.

[0004] To reduce corrosion, organic acid rust removers based on citric acid, oxalic acid, and sulfamic acid have appeared on the market. These products typically have a pH value of 2.5-4.0, which reduces damage to the metal substrate to some extent and slows down the corrosion rate of the metal, showing a significant improvement compared to strong acid systems. However, they have the following problems: (1) slow rust removal speed, usually requiring 30-60 minutes to treat moderate rust; (2) poor penetration, making it difficult to treat crevices and deep rust; (3) the surface remains active after treatment and must be used in conjunction with rust inhibitors; (4) most products still contain 10-20% inorganic acid, with high VOC content, which does not comply with increasingly stringent environmental regulations; (5) they do not have lubrication function and cannot solve the problem of loosening of rusted mechanical parts.

[0005] In recent years, new technologies such as nanomaterials and bio-enzymes have been introduced into the field of rust removers. However, these technologies generally suffer from problems such as high cost, complex processes, and unstable effects, and have not yet been industrialized. With the transformation and upgrading of the manufacturing industry and increasingly stringent environmental regulations, the market demand for high-performance rust remover lubricants is becoming increasingly urgent. Therefore, developing a rust remover lubricant that combines excellent rust removal, lubrication, and rust prevention functions while being environmentally friendly and safe has significant technological value and market significance. Summary of the Invention

[0006] The purpose of this invention is to provide a rust-removing lubricant for metals and its preparation method, which has the characteristics of efficient rust removal and long-lasting lubrication.

[0007] The objective of this invention can be achieved through the following technical solutions: A rust-removing lubricant for metals comprises the following components in parts by weight: 10-20 parts of linoleic acid modified resin acid derivative, wherein the resin acid is selected from at least one of rosin, disproportionated rosin, hydrogenated rosin, and polymerized rosin; 8-15 parts of a quaternary ammonium salt modified montmorillonite-vegetable oil complex, wherein the vegetable oil is an epoxidized vegetable oil; 5-12 parts of quaternized lignin derivative, wherein the quaternized lignin derivative is prepared by reacting lignin sulfonate with epichlorohydrin and then quaternizing it with a tertiary amine. 25-35 parts of d-limonene; 8-15 parts of epoxidized soybean oil; 8-12 parts of maleic anhydride-modified tung oil; 2-5 parts of benzotriazole; 1-3 parts of nonionic surfactant; 1-3 parts of pH buffer system; and 5-15 parts deionized water.

[0008] In this technical solution, linoleic acid modified resin acid derivatives are mainly used as fast rust removers, which can quickly release rusted metal parts. d-limonene is mainly used as a biosolvent to reduce surface tension. Quaternary ammonium salt modified montmorillonite-vegetable oil complex and quaternized lignin derivatives enhance permeability and adhesion. The components work together to achieve the functions of penetration, rust removal, film formation and corrosion inhibition.

[0009] Furthermore, the linoleic acid modified resin acid derivative is prepared by pretreating the resin acid and linoleic acid with heat, and then copolyesterifying them with polyethylene glycol and an acidic catalyst, wherein the weight ratio of the resin acid, linoleic acid and polyethylene glycol is 100:(35-45):(55-65).

[0010] Furthermore, the acidic catalyst is p-toluenesulfonic acid, and the amount used is 0.3-0.5% of the resin acid mass.

[0011] Among these methods, thermal pretreatment promotes the acid thermal isomerization of the resin and achieves uniform dispersion; if the proportion of linoleic acid is too low, it is easy to lead to insufficient esterification, while if it is too high, it is easy to lead to a decrease in oxidative stability.

[0012] Furthermore, the resin acid is rosin or disproportionated rosin.

[0013] Furthermore, the molecular weight of the polyethylene glycol is between 400 and 1000 Da. Preferably, the molecular weight of the polyethylene glycol is 600 Da or 800 Da.

[0014] If the molecular weight of polyethylene glycol is too low, it will easily lead to poor film-forming properties; if the molecular weight of polyethylene glycol is too high, it will easily lead to poor flowability.

[0015] Furthermore, the preparation method of the linoleic acid modified resin acid derivative is as follows: The resin acid and linoleic acid were pretreated at 150-170℃ under nitrogen protection for 2-3 hours; then cooled to 110-130℃, polyethylene glycol and an acidic catalyst were added, and the reaction was continued with stirring for 4-5 hours to obtain the linoleic acid modified resin acid derivative.

[0016] Furthermore, the quaternary ammonium salt modified montmorillonite-vegetable oil complex is prepared by modifying sodium montmorillonite with quaternary ammonium salt and then reacting it with epoxidized vegetable oil; wherein the epoxidized vegetable oil is epoxidized castor oil or epoxidized linseed oil; the weight ratio of sodium montmorillonite, quaternary ammonium salt and epoxidized vegetable oil is 100:(12-18):(75-85).

[0017] In particular, if the amount of quaternary ammonium salt is too low, it can easily lead to insufficient interlayer spacing of sodium-based montmorillonite; if it is too high, it may cause quaternary ammonium salt precipitation and increased VOC content. After sodium-based montmorillonite is modified with quaternary ammonium salt, the quaternary ammonium cations exchange with sodium ions in the interlayer of montmorillonite, the interlayer spacing of sodium-based montmorillonite is expanded, providing a slow-release channel and improving dispersibility. Not only can it form nanoscale dispersions under high-speed shear, but it also creates space for the insertion of epoxidized vegetable oil molecules. Epoxidized vegetable oil provides lubrication and film-forming functions. After modification, montmorillonite and epoxidized vegetable oil enhance compatibility through physical intercalation and hydrogen bonding, creating a lubrication-penetration synergy.

[0018] Furthermore, the quaternary ammonium salt is selected from at least one of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, di(hydrogenated tallow alkyl)dimethylammonium chloride, ester-based quaternary ammonium salt, and ethoxylated tallow amine quaternary ammonium salt.

[0019] Furthermore, the preparation method of the quaternary ammonium salt modified montmorillonite-vegetable oil complex is as follows: Sodium-based montmorillonite was dispersed in water, the pH was adjusted to 9-10, quaternary ammonium salt was added, and the mixture was stirred at 60-80℃ for 1-3 hours. Solid-liquid separation and drying were performed, and then epoxidized vegetable oil was added. The mixture was stirred at 70-90℃ for 2-4 hours to obtain quaternary ammonium salt modified montmorillonite-vegetable oil complex.

[0020] Furthermore, the specific operation of adjusting the pH to 9-10 is as follows: the pH is adjusted to 9-10 using an 8-15% sodium hydroxide solution. This promotes the exchange of quaternary ammonium cations with sodium ions.

[0021] Furthermore, the weight ratio of the lignin sulfonate, epichlorohydrin and tertiary amine is 100:(20-30):(15-30).

[0022] Epichlorohydrin plays a crucial role as a bifunctional bridging agent in the preparation of quaternized lignin derivatives. On one hand, the phenolic / alcoholic hydroxyl groups in sodium lignin sulfonate molecules nucleophilically attack the epoxy groups of epichlorohydrin, resulting in a ring-opening reaction. This reaction introduces chloromethyl side chains onto the lignin backbone, improving the reaction conversion rate. On the other hand, after the epoxy groups open, the chloromethyl groups remain intact, providing reaction sites for subsequent quaternization. The reactivity of chlorine is significantly higher than that of hydroxyl groups. Furthermore, the C3 segment introduced by epichlorohydrin increases the flexibility of lignin molecules, making it easier for the quaternary ammonium groups to contact metal surfaces. Lignin, which is inherently hydrophilic, exhibits an increased contact angle after modification with epichlorohydrin, optimizing its amphiphilic structure.

[0023] Furthermore, the lignin sulfonate is sodium lignin sulfonate; the tertiary amine is selected from C1-C12 alkyl-substituted tertiary amines.

[0024] Sodium lignosulfonate has a faster dissociation rate in water, ensuring a uniform quaternization reaction. Furthermore, industrial-grade sodium lignosulfonate has a molecular weight of 10,000-30,000, making it suitable for subsequent functionalization modifications.

[0025] More preferably, the tertiary amine is selected from trimethylamine or dimethylethanolamine, wherein the amount of trimethylamine is 15-25% of the weight of lignin sulfonate, and the amount of dimethylethanolamine is 20-30% of the weight of lignin sulfonate.

[0026] Furthermore, the trimethylamine is added in the form of a 25–35 wt% aqueous solution of trimethylamine.

[0027] Among them, the quaternary ammonium group in trimethylamine gives the molecule a permanent positive charge, forming a strong electrostatic adsorption on the metal surface (which is usually negatively charged); the trimethyl structure makes the quaternary ammonium salt remain stable in water with high hardness.

[0028] Furthermore, the preparation method of the quaternized lignin derivative is as follows: At 50-70℃, lignin sulfonate is dissolved in deionized water, with the amount of deionized water being 3-4 times the weight of lignin sulfonate. The pH is adjusted to 10-11, and then epichlorohydrin is continuously added dropwise under nitrogen protection while maintaining the pH at 10-11. After the addition is complete, the reaction is kept at this temperature for 1-3 hours. The temperature is then lowered to 40-60℃, and a tertiary amine is added to adjust the pH to 8-9. The quaternization reaction is carried out for 2-4 hours, and then the reaction solution is spray-dried to obtain the quaternized lignin derivative.

[0029] Further, the specific procedure for adjusting the pH to 10-11 is as follows: continuously add an 8-15% sodium hydroxide solution at a rate of 3-5 mL / min until the pH is detected to be 10-11. The pH adjuster for adjusting the pH to 8-9 is an 8-15% hydrochloric acid solution. The inlet air temperature of the spray dryer is 170-190℃, and the outlet air temperature is 80-100℃.

[0030] Furthermore, the maleic anhydride-modified tung oil refers to maleic anhydride-modified tung oil with an acid value of 20-30 mg KOH / g and an iodine value of 90-110.

[0031] Unmodified tung oil is incompatible with water, while maleic anhydride adds to the conjugated double bonds of tung oil via the Diels-Alder reaction, introducing carboxyl groups, which significantly improves polarity and water dispersibility, and enhances the adsorption capacity of metal surfaces.

[0032] Furthermore, the preparation method of the maleic anhydride-modified tung oil is as follows: Maleic anhydride-modified tung oil is prepared by reacting tung oil with maleic anhydride at 180-190℃ for 3-4 hours under inert gas protection and catalysis of an acidic catalyst.

[0033] Furthermore, the amount of maleic anhydride used is 8-12% of the weight of tung oil, and the amount of acidic catalyst used is 0.3-0.8% of the weight of tung oil; the acidic catalyst is preferably p-toluenesulfonic acid.

[0034] Furthermore, the inert gas is selected from at least one of nitrogen and argon. Without the protection of an inert gas, tung oil is extremely prone to oxidation and polymerization at high temperatures, leading to a sharp increase in product viscosity, darkening of color, and decreased metal adhesion. In severe cases, it may gel and become unusable.

[0035] Furthermore, the nonionic surfactant is a fatty acid diethanolamide or an alkyl glycoside, which plays a role in emulsification and stabilization.

[0036] Furthermore, the pH buffer system is a citric acid-sodium citrate buffer system, maintaining a pH of 5-6; the mass ratio of citric acid to sodium citrate in the citric acid-sodium citrate buffer system is 1:1. The citric acid-sodium citrate buffer system maintains a weakly acidic environment, promoting rust dissolution while preventing strong acid corrosion of the base metal.

[0037] The preparation method of the above-mentioned rust-removing lubricant for metals includes the following steps: S1. Mix d-limonene, epoxidized soybean oil and maleic anhydride-modified tung oil, and stir at 45-55℃ for 20-60 minutes; S2. Add the quaternary ammonium salt modified montmorillonite-vegetable oil complex, shear and disperse it, adjust the temperature to 50-60℃, then add the linoleic acid modified resin acid derivative and the quaternized lignin derivative, and stir for 10-20 minutes. S3. Continue to add benzotriazole, fatty acid diethanolamide and citrate-sodium citrate buffer system, and stir for 10-20 minutes; S4. Add deionized water, emulsify and disperse to obtain the metal rust remover and lubricant.

[0038] Further, in step S2, the shear dispersion refers to stirring at a speed of 2000-4000 rpm for 20-50 minutes; in step S4, the emulsification dispersion refers to stirring at a speed of 3500-4500 rpm for 20-40 minutes.

[0039] The beneficial effects of this invention are: (1) This invention incorporates linoleic acid-modified resin acid derivatives, quaternary ammonium salt-modified montmorillonite-vegetable oil complexes, quaternized lignin derivatives, and d-limonene. d-limonene provides high permeability to dissolve organic pollutants between rust layers; the carboxyl groups of linoleic acid provide a weakly acidic environment, promoting rust dissolution; nano-montmorillonite flakes wed into the micro-gaps of the rust layer; the phenolic hydroxyl / carboxyl groups of quaternized lignin chelate iron ions; and the rigid framework of rosin enhances the interfacial anchoring effect, thereby achieving rapid rust removal. The molecular design and synergistic effect of these core components achieve excellent permeability, rapid rust removal capability, long-lasting lubrication, and rust prevention performance.

[0040] (2) The preparation method of the present invention is simple, the raw materials are readily available, and it is suitable for industrial production. It can be widely used for rust removal, lubrication and protection of metal products such as machinery, automotive parts and hardware tools, and to extend the service life of metal parts. At the same time, it uses bio-based raw materials, which reduces the use of harmful solvents, has low VOC content, and does not contain heavy metals, strong acids or benzene compounds, thus meeting environmental protection requirements. Detailed Implementation

[0041] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described below with reference to specific embodiments, but the scope of protection of this invention is not limited thereto. Experimental methods not specifically described in the embodiments are generally performed under conventional conditions or according to the manufacturer's recommendations. Unless otherwise specified, all reagents and materials used are commercially available. Example

[0042] A rust-removing lubricant for metals comprises the following components in parts by weight: The mixture consisted of 15 parts of linoleic acid-modified resin acid derivatives, 10 parts of quaternary ammonium salt-modified montmorillonite-vegetable oil complex, 8 parts of quaternized lignin derivatives, 30 parts of d-limonene, 12 parts of epoxidized soybean oil, 10 parts of maleic anhydride-modified tung oil, 3 parts of benzotriazole, 2 parts of fatty acid diethanolamide, 2 parts of citric acid-sodium citrate buffer system (1:1), and 8 parts of deionized water.

[0043] The preparation method of linoleic acid modified resin acid derivative is as follows: 100 parts of rosin and 40 parts of linoleic acid are added to a reaction vessel and pretreated at 160°C under nitrogen protection for 2.5 hours; then the temperature is lowered to 120°C, 60 parts of polyethylene glycol with a molecular weight of 600 Da and 0.4 parts of p-toluenesulfonic acid are added, and the mixture is stirred and reacted for 4.5 hours to obtain an amber viscous liquid.

[0044] The preparation method of quaternary ammonium salt modified montmorillonite-vegetable oil complex is as follows: 100 parts of sodium montmorillonite are dispersed in water, the pH is adjusted to 9-10 with 10% NaOH solution, and then 15 parts of hexadecyltrimethylammonium bromide are added and stirred at 70℃ for 2 hours; after separation and drying, it is reacted with 80 parts of epoxidized castor oil at 80℃ for 3 hours to obtain a brownish-yellow complex.

[0045] The preparation method of quaternized lignin derivatives is as follows: At 60℃, 100 parts of sodium lignin sulfonate are dissolved in 350 parts of deionized water, and 10% NaOH aqueous solution is slowly added dropwise (at a rate ≤5mL / min) while monitoring the pH and controlling the pH to 10.0–10.5. Then, under nitrogen protection, 25 parts of epichlorohydrin are added dropwise, controlling the addition time to 30–45 minutes, and the pH is maintained at 10.0–10.5 by replenishing 10% NaOH aqueous solution. After the addition is completed, the reaction is kept at 55±2℃ for 2 hours, then cooled to 45℃, and 60 parts of 30% trimethylamine aqueous solution are added. The pH is adjusted to 8.5–9.0 with 10% HCl, and the quaternization reaction is continued for 3 hours. Finally, the reaction solution is spray-dried (inlet air temperature 180℃, outlet air temperature 90℃) to obtain quaternized lignin derivatives.

[0046] The preparation method of maleic anhydride modified tung oil is as follows: take 100 parts of tung oil, 10 parts of maleic anhydride, and 0.5 parts of p-toluenesulfonic acid, and react them at 185℃ for 3.5 hours under nitrogen protection at a flow rate of 1.0 L / min.

[0047] The preparation method of the above-mentioned rust-removing lubricant for metals is as follows: S1. Mix d-limonene, epoxidized soybean oil and maleic anhydride-modified tung oil, and stir at 50°C for 30 minutes; S2. Add the quaternary ammonium salt modified montmorillonite-vegetable oil complex, shear at 3000 rpm for 30 minutes, then heat to 55℃, add linoleic acid modified resin acid derivative and quaternized lignin derivative, and stir for 15±5 minutes until uniform. S3. Add benzotriazole, fatty acid diethanolamide and citrate-sodium citrate buffer system, and stir for 15 minutes; S4. Slowly add deionized water and emulsify at 4000 rpm for 30 minutes to obtain a milky white rust remover and lubricant for metals. Example

[0048] A rust-removing lubricant for metals comprises the following components in parts by weight: The mixture consisted of 12 parts of linoleic acid modified resin acid derivative, 9 parts of quaternary ammonium salt modified montmorillonite-vegetable oil complex, 7 parts of quaternized lignin derivative, 32 parts of d-limonene, 10 parts of epoxidized soybean oil, 9 parts of maleic anhydride modified tung oil, 2.5 parts of benzotriazole, 1.8 parts of fatty acid diethanolamide, 1.8 parts of citric acid-sodium citrate buffer system (1:1), and 10 parts of deionized water.

[0049] The preparation method of linoleic acid modified resin acid derivative is as follows: 100 parts of rosin and 35 parts of linoleic acid are added to a reaction vessel and pretreated at 160°C under nitrogen protection for 2.5 hours; the temperature is then lowered to 120°C, 55 parts of polyethylene glycol with a molecular weight of 600 Da and 0.3 parts of p-toluenesulfonic acid are added, and the mixture is stirred and reacted for 4.5 hours to obtain an amber viscous liquid.

[0050] The preparation method of quaternary ammonium salt modified montmorillonite-vegetable oil complex is as follows: 100 parts of sodium montmorillonite are dispersed in water, the pH is adjusted to 9-10 with 10% NaOH solution, 18 parts of dodecyltrimethylammonium bromide (DTAB) and 3 parts of benzyl alcohol are added, and the mixture is stirred at 70℃ for 2.5 hours; after separation and drying, it is reacted with 80 parts of epoxidized castor oil at 80℃ for 3 hours to obtain a brownish-yellow complex.

[0051] The preparation method of quaternized lignin derivatives is as follows: At 60℃, 100 parts of sodium lignin sulfonate are dissolved in 300 parts of deionized water, and 10% NaOH aqueous solution is slowly added dropwise (at a rate ≤5mL / min) while monitoring the pH and controlling the pH to 10.0–10.5. Then, under nitrogen protection, 22 parts of epichlorohydrin are added dropwise, controlling the addition time to 30–45 minutes, and the pH is maintained at 10.0–10.5 by replenishing 10% NaOH aqueous solution. After the addition is completed, the reaction is kept at 55±2℃ for 2 hours, then cooled to 45℃, and 55 parts of 30% trimethylamine aqueous solution are added. The pH is adjusted to 8.5–9.0 with 10% HCl, and the quaternization reaction is continued for 3 hours. Finally, the reaction solution is spray-dried (inlet air temperature 180℃, outlet air temperature 90℃) to obtain quaternized lignin derivatives.

[0052] The preparation method of the above-mentioned rust-removing lubricant for metals is the same as that in Example 1. Example

[0053] A rust-removing lubricant for metals comprises the following components in parts by weight: The mixture consisted of 16 parts of linoleic acid-modified resin acid derivatives, 11 parts of quaternary ammonium salt-modified montmorillonite-vegetable oil complex, 10 parts of quaternized lignin derivatives, 28 parts of d-limonene, 14 parts of epoxidized soybean oil, 12 parts of maleic anhydride-modified tung oil, 2.8 parts of benzotriazole, 1.5 parts of alkyl glycosides, 2.2 parts of a citric acid-sodium citrate buffer system (1:1), and 7 parts of deionized water.

[0054] The preparation method of linoleic acid modified resin acid derivative is as follows: 100 parts of disproportionated rosin and 42 parts of linoleic acid are added to a reaction vessel and pretreated at 155°C under nitrogen protection for 3 hours; the temperature is then lowered to 115°C, 65 parts of polyethylene glycol with a molecular weight of 600 Da and 0.5 parts of p-toluenesulfonic acid are added, and the mixture is stirred and reacted for 5 hours to obtain a light amber viscous liquid.

[0055] The preparation method of quaternary ammonium salt modified montmorillonite-vegetable oil complex is as follows: 100 parts of sodium montmorillonite are dispersed in water, the pH is adjusted to 9-10 with 10% NaOH solution, 20 parts of ester-based quaternary ammonium salt are added, and the mixture is stirred at 75°C for 2 hours; after separation and drying, it is reacted with 85 parts of epoxidized linseed oil at 75°C for 3.5 hours to obtain a light yellow complex.

[0056] The preparation method of quaternized lignin derivatives is as follows: At 60℃, 100 parts of sodium lignin sulfonate are dissolved in 400 parts of deionized water, and 10% NaOH aqueous solution is slowly added dropwise (at a rate ≤5mL / min) while monitoring the pH and controlling the pH to 10.0–10.5. Then, under nitrogen protection, 22 parts of epichlorohydrin are added dropwise, controlling the addition time to 30–45 minutes, and the pH is maintained at 10.0–10.5 by replenishing 10% NaOH aqueous solution. After the addition is completed, the reaction is kept at 55±2℃ for 2 hours, then cooled to 45℃, and 70 parts of 30% trimethylamine aqueous solution are added. The pH is adjusted to 8.5–9.0 with 10% HCl, and the quaternization reaction is continued for 3 hours. Finally, the reaction solution is spray-dried (inlet air temperature 180℃, outlet air temperature 90℃) to obtain quaternized lignin derivatives.

[0057] The preparation method of the above-mentioned rust-removing lubricant for metals is as follows: S1. Mix d-limonene, epoxidized soybean oil and maleic anhydride-modified tung oil, and stir at 45°C for 35 minutes; S2. Add the quaternary ammonium salt modified montmorillonite-vegetable oil complex, shear at 3200 rpm for 35 minutes, heat to 55℃, add linoleic acid modified resin acid derivative and quaternized lignin derivative, and stir for 15±5 minutes until uniform. S3. Add benzotriazole, alkyl glycoside and citrate-sodium citrate buffer system, and stir for 20 minutes; S4. Slowly add deionized water and emulsify at 4200 rpm for 35 minutes to obtain a milky white rust remover and lubricant for metals.

[0058] Comparative Example 1 Compared with Example 1, this comparative example differs in that it does not contain linoleic acid modified resin acid derivatives, while the other components, preparation steps and parameters are the same.

[0059] Comparative Example 2 Compared with Example 1, this comparative example differs in that it does not contain the quaternary ammonium salt modified montmorillonite-vegetable oil complex, while the other components, preparation steps and parameters are the same.

[0060] Comparative Example 3 Compared with Example 1, this comparative example differs in that it does not contain quaternized lignin derivatives, while the other components, preparation steps, and parameters are the same.

[0061] Comparative Example 4 Compared to Example 1, this comparative example differs in that the linoleic acid-modified resin acid derivative is replaced with an equal amount of rosin, the quaternary ammonium salt-modified montmorillonite-vegetable oil complex is replaced with an equal amount of sodium montmorillonite, and the quaternized lignin derivative is replaced with an equal amount of sodium lignin sulfonate. Due to the insufficient performance of the unmodified raw material, 15 parts of 200# solvent oil are added as a synergistic solvent in this example, added in step S1; simultaneously, to improve emulsification stability, 3 parts of OP-10 emulsifier are added, added together with the rosin in step S2. All other components, preparation steps, and parameters remain the same. A grayish-white turbid liquid is finally obtained.

[0062] Comparative Example 5 Compared to Example 1, this comparative example differs in that the maleic anhydride-modified tung oil is replaced with an equal amount of ordinary unmodified tung oil. All other components, preparation steps, and parameters remain the same.

[0063] The samples obtained in Examples 1-3 and Comparative Examples 1-5 were subjected to the following performance tests: (1) Permeation performance test: Referring to JB / T4323.2, a high-purity quartz capillary tube with an inner diameter of 1.0±0.02mm was used. Under precise temperature control at 25±0.5℃, the liquid rise height was continuously monitored for 30 minutes by an automatic image analysis system. This method reflects the dynamic permeation ability of the product under deep corrosion conditions through EPR parameters.

[0064] (2) Rust removal efficiency test: Referring to ASTM D665-21 and GB / T10125, standard steel bar samples (45# steel, with a uniform rust layer pre-formed on the surface) were immersed in distilled water at 38±1℃ for 24 hours to evaluate the rust removal effect. Subsequently, they were transferred to a neutral salt spray chamber (5% NaCl solution, 35±2℃, pH 6.5-7.2) for 96 hours of continuous spraying test to evaluate the protective performance. The evaluation was carried out in five levels based on the percentage of rust area and the depth of rust. Among them, level 1 indicates no rust; level 2 indicates slight rust spots <5%; level 3 indicates moderate rust 5-15%; level 4 indicates severe rust 15-30%; and level 5 indicates extremely severe rust >30%.

[0065] (3) Lubrication performance test: Referring to ASTM D1894-22 and GB / T12583, a ring-block friction and wear tester was used to test the static friction coefficient (μs) and dynamic friction coefficient (μd) of a standard 45# steel test ring (inner diameter 40mm, surface roughness Ra=0.8μm) with a GCr15 steel test block (25×12.5×6mm) under the conditions of 50N load, 0.35m / s linear speed and 25±1℃, and the ratio (μs / μd) was calculated. At the same time, extreme pressure performance test (1800rpm, 30min, maximum non-seize load PB value) was carried out on a four-ball machine.

[0066] Ideally, the anti-slip performance requires μs to be between 0.45 and 0.55, and the μs / μd ratio to be >1.35.

[0067] (4) VOC content test: According to GB / T38511, gas chromatography-mass spectrometry (GC-MS) was used. After the sample was conditioned at 23±2℃ and 50±5%RH for 24 hours, 1.0±0.1g of the sample was placed in a headspace vial and equilibrated at 80±2℃ for 30 minutes. The temperature was programmed using a DB-624 capillary column (30m×0.25mm×1.4μm) (starting temperature 40℃, holding for 5 minutes, then increasing to 250℃ at 10℃ / min and holding for 5 minutes). The carrier gas was high-purity helium, and the flow rate was 1.0mL / min. The VOC content at 25℃ was quantitatively calculated by the internal standard method (deuterated toluene).

[0068] The test results are shown in Table 1.

[0069] Table 1 As shown in Table 1, the test results of Examples 1-3 are significantly better than those of Comparative Examples 1-5. Comparative Example 4 performed the worst, while Comparative Example 5, although showing good initial rust removal, suffered severe corrosion after 96 hours of salt spray treatment, demonstrating that maleic anhydride modification has a positive effect on long-term rust prevention. Comparative Examples 1-3 demonstrate that linoleic acid-modified resin acid derivatives are crucial for rust removal performance; quaternary ammonium salt-modified montmorillonite-vegetable oil complexes significantly contribute to lubrication performance; and quaternized lignin derivatives are key to long-term rust prevention. Examples 1-3 demonstrate that linoleic acid-modified resin acid derivatives, quaternary ammonium salt-modified montmorillonite-vegetable oil complexes, and quaternized lignin derivatives have a synergistic effect; the nano-reinforcing network formed by quaternary ammonium salt-modified montmorillonite synergistically with the film-forming properties of linoleic acid-modified resin acid derivatives allows for rapid penetration of the rust-preventive layer, removal of rust, and improvement of the metal's rust prevention and lubrication performance.

[0070] The VOC content of Examples 1-3 of this invention is lower than that of Comparative Examples 1-5, with Example 3 having the lowest VOC content. Comparative Example 4, due to the lack of modification of all raw materials, required the addition of solvent oil to improve performance, resulting in a significant increase in VOC content, confirming the crucial role of functional modification in reducing VOCs. In contrast, this invention, through molecular design and component synergy, achieves ultra-low VOC emissions while maintaining excellent rust removal performance. Therefore, the product of this invention has significant advantages in terms of penetration, rust removal efficiency, lubricity, and rust prevention period, while also significantly reducing VOC content, meeting environmental protection requirements.

[0071] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A rust-removing lubricant for metals, characterized in that, The following components are included by weight: 10-20 parts of linoleic acid modified resin acid derivative, wherein the resin acid is selected from at least one of rosin, disproportionated rosin, hydrogenated rosin, and polymerized rosin; 8-15 parts of a quaternary ammonium salt modified montmorillonite-vegetable oil complex, wherein the vegetable oil is an epoxidized vegetable oil; 5-12 parts of quaternized lignin derivative, wherein the quaternized lignin derivative is prepared by reacting lignin sulfonate with epichlorohydrin and then quaternizing it with a tertiary amine. 25-35 parts of d-limonene; 8-15 parts of epoxidized soybean oil; 8-12 parts of maleic anhydride-modified tung oil; 2-5 parts of benzotriazole; 1-3 parts of nonionic surfactant; 1-3 parts of pH buffer system; and 5-15 parts deionized water.

2. The rust-removing lubricant for metals according to claim 1, characterized in that, The linoleic acid modified resin acid derivative is prepared by pretreating the resin acid and linoleic acid with heat, and then copolyesterifying them with polyethylene glycol and an acidic catalyst. The weight ratio of the resin acid, linoleic acid, and polyethylene glycol is 100:(35-45):(55-65); the acidic catalyst is p-toluenesulfonic acid, and its dosage is 0.3-0.5% of the mass of the resin acid. The molecular weight of the polyethylene glycol is between 400 and 1000 Da.

3. A rust-removing lubricant for metals according to claim 1 or 2, characterized in that, The preparation method of the linoleic acid modified resin acid derivative is as follows: The resin acid and linoleic acid were pretreated at 150-170℃ under nitrogen protection for 2-3 hours; then cooled to 110-130℃, polyethylene glycol and an acidic catalyst were added, and the reaction was continued with stirring for 4-5 hours to obtain the linoleic acid modified resin acid derivative.

4. The rust-removing lubricant for metals according to claim 1, characterized in that, The quaternary ammonium salt modified montmorillonite-vegetable oil complex is prepared by modifying sodium montmorillonite with quaternary ammonium salt and then reacting it with epoxidized vegetable oil. The epoxidized vegetable oil is epoxidized castor oil or epoxidized linseed oil; The weight ratio of sodium montmorillonite, quaternary ammonium salt and epoxidized vegetable oil is 100:(12-18):(75-85); The quaternary ammonium salt is selected from at least one of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, di(hydrogenated tallow alkyl)dimethylammonium chloride, ester-based quaternary ammonium salt, and ethoxylated tallow amine quaternary ammonium salt.

5. A rust-removing lubricant for metals according to claim 1 or 4, characterized in that, The preparation method of the quaternary ammonium salt modified montmorillonite-vegetable oil complex is as follows: Sodium-based montmorillonite was dispersed in water, the pH was adjusted to 9-10, quaternary ammonium salt was added, and the mixture was stirred at 60-80℃ for 1-3 hours. Solid-liquid separation and drying were performed, and then epoxidized vegetable oil was added. The mixture was stirred at 70-90℃ for 2-4 hours to obtain quaternary ammonium salt modified montmorillonite-vegetable oil complex.

6. The rust-removing lubricant for metals according to claim 1, characterized in that, The preparation method of the quaternized lignin derivative is as follows: At 50-70℃, lignin sulfonate is dissolved in deionized water, with the amount of deionized water being 3-4 times the weight of lignin sulfonate. The pH is adjusted to 10-11, and then epichlorohydrin is continuously added dropwise under nitrogen protection while maintaining the pH at 10-11. After the addition is complete, the reaction is kept at this temperature for 1-3 hours. The temperature is then lowered to 40-60℃, and a tertiary amine is added to adjust the pH to 8-9. The quaternization reaction is carried out for 2-4 hours, and then the reaction solution is spray-dried to obtain the quaternized lignin derivative. The weight ratio of the lignin sulfonate, epichlorohydrin, and tertiary amine is 100:(20-30):(15-30); The lignin sulfonate is sodium lignin sulfonate; the tertiary amine is selected from C1-C12 alkyl-substituted tertiary amines.

7. The rust-removing lubricant for metals according to claim 1, characterized in that, The preparation method of the maleic anhydride-modified tung oil is as follows: Maleic anhydride-modified tung oil is prepared by reacting tung oil with maleic anhydride at 180-190℃ for 3-4 hours under inert gas protection and catalysis of an acidic catalyst.

8. A rust-removing lubricant for metals according to claim 1, characterized in that, The nonionic surfactant is a fatty acid diethanolamide or an alkyl glycoside; the pH buffer system is a citric acid-sodium citrate buffer system.

9. A method for preparing a rust-removing lubricant for metal as described in any one of claims 1-8, characterized in that, The preparation method includes the following steps: S1. Mix d-limonene, epoxidized soybean oil and maleic anhydride-modified tung oil, and stir at 45-55℃ for 20-60 minutes; S2. Add the quaternary ammonium salt modified montmorillonite-vegetable oil complex, shear and disperse it, adjust the temperature to 50-60℃, then add the linoleic acid modified resin acid derivative and the quaternized lignin derivative, and stir for 10-20 minutes. S3. Continue to add benzotriazole, fatty acid diethanolamide and citrate-sodium citrate buffer system, and stir for 10-20 minutes; S4. Add deionized water, emulsify and disperse to obtain the metal rust remover and lubricant.

10. The preparation method according to claim 9, characterized in that, In step S2, the shear dispersion refers to stirring at a speed of 2000-4000 rpm for 20-50 minutes; in step S4, the emulsification dispersion refers to stirring at a speed of 3500-4500 rpm for 20-40 minutes.