Nickel-based single crystal alloy fatigue life forecasting method considering second orientation and recrystallization defect

By establishing a crystal plasticity model that considers recrystallization defects and second orientations, and introducing a fatigue indicator factor, the accuracy and reliability issues of fatigue life prediction for single-crystal alloys were solved, and accurate prediction of high-temperature fatigue performance was achieved.

CN122050642APending Publication Date: 2026-05-15SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610145741.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-02
Publication Date
2026-05-15

AI Technical Summary

Technical Problem

Existing methods for predicting fatigue life of single-crystal alloys fail to effectively consider the effects of recrystallization defects and secondary orientations, resulting in large dispersion of prediction results, insufficient accuracy and reliability, and inability to accurately predict high-temperature fatigue performance.

Method used

By establishing a crystal plasticity model, considering recrystallization defects and different secondary orientations, a fatigue indicator factor is introduced to construct a fatigue life prediction model. Combining the crystal plasticity model and fatigue stress parameters, the cumulative plastic shear strain and plastic slip deformation energy are calculated, and the relationship between the fatigue indicator factor and fatigue life is established.

Benefits of technology

The model significantly improves the accuracy and reliability of fatigue life prediction for single-crystal alloys, reduces the influence of uncontrollable factors, and is applicable to single-crystal alloys with different orientations and recrystallization defects, especially nickel-based single-crystal alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122050642A_ABST
    Figure CN122050642A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of single crystal alloy fatigue life prediction, in particular to a nickel-based single crystal alloy fatigue life prediction method considering second orientation and recrystallization defects. The specific method comprises the following steps: obtaining a plurality of nickel-based single crystal alloys as single crystal alloy samples which have different second orientations and have recrystallization defects partially; establishing a crystal plastic model; acquiring fatigue life and fatigue stress parameters; inputting the fatigue stress parameter into a crystal plastic model to calculate the accumulated plastic shear strain of the dangerous point; 1 / 2 of the product of the cumulative plastic cutting strain and the fatigue load in the crystal plasticity or the cumulative plastic cutting strain is used as a fatigue indication factor; and fitting by taking the fatigue indication factor as a vertical coordinate and the fatigue life as a horizontal coordinate to obtain a fatigue life prediction model. According to the method, the recrystallization defect and the influence of different second orientations are considered, the related fatigue indication factors are introduced to construct the fatigue life prediction model between the fatigue indication factors and the fatigue life, and the accuracy and reliability of the prediction result are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fatigue life prediction technology for single-crystal alloys, and more specifically to a method for predicting the fatigue life of nickel-based single-crystal alloys that takes into account second orientation and recrystallization defects. Background Technology

[0002] In high-end engineering fields such as modern aerospace and energy, single-crystal alloys, with their outstanding high-temperature mechanical properties, such as excellent high-temperature strength, good creep resistance, and excellent oxidation resistance, have become core materials for manufacturing critical hot-end components such as turbine blades and guide vanes for aero-engines. These components operate under extremely complex and harsh conditions, enduring various severe conditions such as high temperature, high stress, and alternating loads. Their fatigue life directly affects the reliability, safety, and service life of the entire equipment. Therefore, accurately predicting the fatigue life of single-crystal alloys is of vital importance for ensuring the stable operation of engineering equipment, reducing maintenance costs, and improving overall economic efficiency.

[0003] Currently, in the fabrication of high-temperature nickel-based alloy turbine blades, the secondary orientation is often not specifically controlled. However, previous studies have shown that the secondary orientation has a significant impact on the fatigue life of nickel-based superalloys. Nevertheless, recrystallization defects are inevitable during turbine blade service. Recrystallization defects are phenomena such as abnormal grain growth and grain boundary migration that occur during high-temperature service. The presence of these defects significantly affects the mechanical properties of single-crystal alloys, especially under fatigue loading conditions. Defect locations easily become stress concentration points, initiating and propagating cracks, thereby accelerating the accumulation of fatigue damage.

[0004] Currently, the main methods for predicting the fatigue life of single-crystal alloys involve using finite element method (FEM) analysis of crystal plasticity and establishing corresponding fatigue indicator factors. These methods consider factors such as slip-shear mechanisms and plastic deformation laws, combined with other macroscopic phenomena, to establish the relationship between microstructure and fatigue life. However, existing methods for predicting the fatigue life of single-crystal alloys at high temperatures do not consider the effects of recrystallization defects and different secondary orientations, leading to a series of problems. For example, the presence of secondary orientations and recrystallization defects makes the microstructure of single-crystal alloys complex and non-uniform, resulting in significant differences in fatigue performance at different locations. When predicting fatigue life, these differences introduce numerous uncontrollable factors, causing significant dispersion in the prediction results, which severely limits the accuracy and reliability of the predictions. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention provides a method for predicting the fatigue life of nickel-based single-crystal alloys that takes into account second orientation and recrystallization defects.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] This invention provides a method for predicting the fatigue life of nickel-based single-crystal alloys considering secondary orientations and recrystallization defects, comprising the following steps: obtaining multiple nickel-based single-crystal alloy samples, wherein the multiple single-crystal alloy samples have different secondary orientations and some have recrystallization defects; establishing a crystal plasticity model based on the crystal plasticity parameters of each single-crystal alloy sample; obtaining the fatigue life and fatigue stress parameters of each single-crystal alloy sample; inputting the fatigue stress parameters corresponding to each single-crystal alloy sample into the corresponding crystal plasticity model to calculate the cumulative plastic shear strain at the critical point; using half of the product of the cumulative plastic shear strain and the fatigue load in the crystal plasticity, or the cumulative plastic shear strain, as a fatigue indicator factor; fitting the fatigue indicator factor as the ordinate and the fatigue life of the single-crystal alloy sample as the abscissa to obtain a fatigue life prediction model for predicting the fatigue life of nickel-based single-crystal alloys.

[0008] This invention, considering the effects of recrystallization defects and different secondary orientations, establishes a crystal plasticity model and takes into account the interaction between cyclic plastic deformation and slip systems. It introduces relevant fatigue indicator factors to construct a fatigue life prediction model between fatigue indicator factors and fatigue life. This model is used for fatigue life prediction of single-crystal alloys, significantly improving the accuracy and reliability of the prediction results. It solves the problems of existing fatigue life prediction models that ignore recrystallization defects and secondary orientations, resulting in many uncontrollable factors, data dispersion, and insufficient accuracy and reliability of prediction results.

[0009] Preferably, the method for obtaining the fatigue life and fatigue stress parameters of each single-crystal alloy sample is as follows: High-temperature fatigue tests were conducted on each single-crystal alloy sample at a constant temperature under different stress levels to obtain the fatigue life and fatigue stress parameters of each single-crystal alloy sample.

[0010] In this invention, fatigue stress parameters are experimental input parameters that determine the magnitude of the fatigue load. Fatigue life is an experimental output parameter, representing the number of cycles required for the single-crystal alloy specimen to fail at a given stress level. In subsequent crystal plasticity calculations, the fatigue stress parameters are input into the crystal plasticity model to calculate the cumulative plastic shear strain and strain energy of plastic slip deformation at critical points. The fatigue life is used to compare with the calculation results and establish a life prediction relationship.

[0011] Preferably, the conditions for high-temperature fatigue testing are as follows: Low-cycle fatigue testing with stress control was conducted at a temperature of 550℃ and a stress ratio of R=0.1 using a sinusoidal loading waveform with a frequency of 10Hz.

[0012] Preferably, the method for calculating the cumulative plastic shear strain at the critical point is: The fatigue stress parameters corresponding to each single-crystal alloy sample are input into the corresponding crystal plasticity model, and the solution is obtained step by step under cyclic loading. i The plastic shear strain of a slip system will i The cumulative plastic shear strain at the critical point is obtained by summing the plastic shear strain of each slip system.

[0013] In this invention, at each incremental step of the solution process, the crystal plasticity model outputs the plastic shear strain increment of each slip system. By summing the plastic shear strain increments from all incremental steps, the result can be obtained. i The cumulative plastic shear strain at the critical point is obtained by summing the plastic shear strains of each active slip system and then calculating the plastic shear strains of all active slip systems. The formula for calculating the cumulative plastic shear strain at the critical point is as follows:

[0014] ; c accum Indicates cumulative plastic shear strain; c acc(i) Indicates the first i Plastic shear strain of a slip system.

[0015] Preferably, the number of slip systems is 12. That is, i =12. The specific method for calculating the strain energy of plastic slip deformation is: multiply the product of the cumulative plastic shear strain and the fatigue load in the crystal plasticity by 1 / 2. That is, the strain energy of plastic slip deformation = In this invention, the strain energy of plastic slip deformation represents the plastic dissipation energy density per unit volume, which is the portion of the mechanical work irreversibly converted into heat and microscopic damage per unit volume of a single-crystal alloy sample under cyclic loading due to plastic deformation.

[0016] Preferably, the plasticity parameters of the single-crystal alloy sample include: h 0、 t 0、 t s , C 11 , C 12 , C 44 , and n ;in, h 0 represents the initial hardening modulus; t 0 represents the initial critical shear stress; t s Indicates saturated flow stress; C 11 , C 12 and C 44 Represents three elastic constants; This represents the initial critical shear rate of the slip system; n This represents the strain hardening index.

[0017] The preferred method for establishing a crystal plasticity model is as follows: Electron backscattering diffraction data of single-crystal alloy samples are acquired, and a single-crystal model is obtained. The crystal plasticity parameters are calibrated to ensure that the experimentally obtained curves are consistent with the simulation curves, thereby determining the crystal plasticity model parameters of the single-crystal alloy samples to establish the calibrated crystal plasticity model. Preferably, the electron backscattering diffraction data includes grain orientation distribution, grain boundary characteristics, and grain size.

[0018] This invention primarily involves obtaining microstructural data related to grain orientation, grain boundary characteristics, and grain size of single-crystal alloy samples from experimental EBSD data, importing this data into Abaqus for modeling, and obtaining a single-crystal model. The microstructural data, such as grain orientation distribution, grain boundary characteristics, and grain size, in the single-crystal model are completely consistent with those observed in the EBSD patterns. Through mechanical parameter calibration, the simulated stress-strain curve is made consistent with the experimentally obtained stress-strain curve, determining the calibrated crystal plasticity parameters of the single-crystal alloy sample, thereby establishing the calibrated crystal plasticity model. EBSD stands for Electron Backscatter Diffraction.

[0019] Preferably, the different second orientations are

[010] orientation and

[110] orientation; the recrystallization defects are grain boundary defects and grain size inhomogeneity defects. In this invention, the

[010] orientation and

[110] orientation are named 0° and 45°, respectively.

[0020] Preferably, when cumulative plastic shear strain is used as a fatigue indicator, the fatigue life prediction model is as follows: FIP=a ( N f ) n ; FIP=c accum ; in, FIP Indicates fatigue indicator factor; N f Indicates fatigue life; a Indicates coefficient; n Indicates the fitted parameters; c accum This represents the cumulative plastic shear strain. In this invention, a =128.66347; n =-0.13839.

[0021] Preferably, half of the product of cumulative plastic shear strain and fatigue load in crystal plasticity is used as the fatigue indicator factor, and the fatigue life prediction model is as follows: FIP=b ( N f ) m ; ; in, FIP Indicates fatigue indicator factor; N f Indicates fatigue life; b Indicates coefficient; m Indicates the fitted parameters; c accum Indicates cumulative plastic shear strain; s max This represents the fatigue load during crystal plasticity. In this invention, b =555.2148, m =-0.13941.

[0022] The beneficial effects of this invention are: 1. Based on the influence of recrystallization defects and different secondary orientations, this invention establishes a crystal plasticity model and considers the interaction between cyclic plastic deformation and slip system. It introduces relevant fatigue indicator factors to construct a fatigue life prediction model between fatigue indicator factors and fatigue life. This model is used for fatigue life prediction of single crystal alloys, improving the accuracy and reliability of prediction results. It solves the problems of uncontrollable factors and dispersion in existing fatigue life prediction methods that do not consider recrystallization defects and secondary orientations, which affect the accuracy and reliability of prediction results.

[0023] 2. The fatigue life prediction method for nickel-based single-crystal alloys that considers the second orientation and recrystallization defects of the present invention can supplement the shortcomings of the fatigue life of nickel-based single-crystal alloys in engineering, realize the prediction of fatigue life considering recrystallization and second orientation, and the prediction results are relatively stable, reducing the influence of uncontrollable factors. For 0°-SX, 45°-SX, 0°-RC, and 45°-RC, the results are all near the prediction curve, showing that the model has good applicability and universality.

[0024] 3. The method of the present invention can be applied to the fatigue life prediction of aero-engine turbine blades, and the prediction results are highly accurate. Attached Figure Description

[0025] Figure 1 The fatigue life-fatigue stress curves of single-crystal alloy samples considering recrystallization defects and different second orientations are shown in the embodiments of the present invention.

[0026] Figure 2This is a correlation analysis diagram between the fatigue indicator and fatigue life when cumulative plastic shear strain is used as the fatigue indicator in an embodiment of the present invention.

[0027] Figure 3 This is a correlation analysis diagram between the fatigue indicator factor and fatigue life when the cumulative plastic shear strain and half of the product of the cumulative plastic shear strain and the fatigue load in the crystal plasticity are used as fatigue indicator factors in an embodiment of the present invention.

[0028] Figure 2 and Figure 3 In the diagram, 0°-SX indicates a sample with no recrystallization in the

[010] orientation; 45°-SX indicates a sample with no recrystallization in the

[110] orientation; 0°-RC indicates a sample with recrystallization in the

[010] orientation; and 45°-RC indicates a sample with recrystallization in the

[110] orientation. Detailed Implementation

[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0030] Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] The fatigue predicted in this invention is tensile fatigue, which is a fatigue test for unstable tensile stress.

[0032] In the following embodiments, the full English name of the crystal plasticity model is Crystal Plasticity Finite Element Method, abbreviated as CPFEM.

[0033] The technical solution of the present invention will be further described below through specific embodiments. Unless otherwise specified, the methods described in the following embodiments are conventional methods; the reagents and materials described are commercially available unless otherwise specified.

[0034] A fatigue life prediction method for nickel-based single-crystal alloys considering secondary orientation and recrystallization defects includes the following steps: Step 1: Obtain multiple nickel-based single-crystal alloy samples. These samples have different second orientations and some exhibit recrystallization defects. Establish a crystal plasticity model based on the crystal plasticity parameters of each single-crystal alloy sample.

[0035] In step 1, the different second orientations are

[010] orientation and

[110] orientation, and the

[010] orientation and

[110] orientation are named 0° and 45° respectively; the recrystallization defects are grain boundary defects and grain size inhomogeneity defects.

[0036] Multiple nickel-based single-crystal alloy samples were obtained. These samples had different second orientations and some had recrystallization defects. For example, 0°-SX indicates a sample with no recrystallization in the

[010] orientation; 45°-SX indicates a sample with no recrystallization in the

[110] orientation; 0°-RC indicates a sample with recrystallization in the

[010] orientation; and 45°-RC indicates a sample with recrystallization in the

[110] orientation.

[0037] In this embodiment of the invention, the nickel-based single crystal alloy is specifically: DD6 nickel-based single crystal alloy.

[0038] The method for establishing a crystal plasticity model is as follows: Electron backscatter diffraction data of single-crystal alloy samples were acquired, and a single-crystal model was obtained. The crystal plasticity parameters were calibrated to ensure that the experimental curves were consistent with the simulation curves, thereby determining the crystal plasticity model parameters of the single-crystal alloy samples and establishing the calibrated crystal plasticity model.

[0039] Specifically, electron backscatter diffraction data includes grain orientation distribution, grain boundary characteristics, and grain size.

[0040] The plasticity parameters of the single-crystal alloy sample include: h 0、 t 0、 t s , C 11 , C 12 , C 44 , and n ;in, h 0 represents the initial hardening modulus; t 0 represents the initial critical shear stress; t s Indicates saturated flow stress; C 11 , C 12 and C 44 Represents three elastic constants; This represents the initial critical shear rate of the slip system; n This represents the strain hardening index.

[0041] For example, the single-crystal alloy material parameters used in the crystal plasticity simulation are shown in Table 1 below.

[0042] Table 1 Crystal plasticity parameters of single-crystal alloys Note: Face-Centered Cubic, abbreviated as FCC.

[0043] h 0 represents the initial hardening modulus, which describes the initial value of the material's hardening behavior during plastic deformation.

[0044] t 0 represents the initial critical shear stress, indicating the stress level at which the material begins to undergo plastic deformation.

[0045] t s Saturated flow stress is the flow stress of a material that reaches a stable value when hardening and softening reach equilibrium during the plastic deformation process of a crystal.

[0046] C 11 C 12 and C 44 These are three elastic constants that describe the elastic properties of single-crystal alloys.

[0047] n The strain hardening index describes the rate of change of the hardening behavior of a material during plastic deformation, and is usually used to describe the degree of strain hardening or softening.

[0048] It is usually expressed as the shear strain rate of a slip system.

[0049] In this invention, the microstructure data related to grain orientation, grain boundary characteristics, and grain size of the single-crystal alloy sample are mainly obtained from experimental EBSD data. This data is then imported into Abaqus for modeling to obtain a single-crystal model. The microstructure data, such as grain orientation distribution, grain boundary characteristics, and grain size, in the single-crystal model are completely consistent with those observed in the EBSD pattern. Through mechanical parameter calibration, the simulated stress-strain curve is made consistent with the experimentally obtained stress-strain curve, thus determining the calibrated crystal plasticity parameters of the single-crystal alloy sample and establishing the calibrated crystal plasticity model. EBSD stands for Electron Backscatter Diffraction.

[0050] Step 2: Obtain the fatigue life and fatigue stress parameters of each single-crystal alloy sample; input the fatigue stress parameters corresponding to each single-crystal alloy sample into the corresponding crystal plasticity model, calculate the cumulative plastic shear strain at the critical point, and calculate the strain energy of plastic slip deformation.

[0051] The specific method is as follows: Step 2.1, Method for obtaining fatigue life and fatigue stress parameters of each single crystal alloy sample: High-temperature fatigue tests are performed on each single crystal alloy sample at different stress levels at a constant temperature to obtain the fatigue life and fatigue stress parameters of each single crystal alloy sample.

[0052] In this embodiment of the invention, fatigue stress parameters are experimental input parameters that determine the magnitude of the fatigue load. Fatigue life is an experimental output parameter, representing the number of cycles required for the single-crystal alloy specimen to fail at a given stress level. In subsequent crystal plasticity calculations, the fatigue stress parameters are input into the crystal plasticity model to calculate the cumulative plastic strain and strain energy of plastic slip deformation at critical points. The fatigue life is used to compare with the calculation results and establish a life prediction relationship.

[0053] Specifically, the conditions for high-temperature fatigue testing are as follows: Low-cycle fatigue testing with stress control was conducted at a temperature of 550℃ and a stress ratio of R=0.1 using a sinusoidal loading waveform with a frequency of 10Hz.

[0054] Step 2.2, calculate the cumulative plastic shear strain at the critical point: for each single-crystal alloy specimen The corresponding fatigue stress parameters are input into the corresponding crystal plasticity model, and the solution is obtained step by step under cyclic loading. i The plastic shear strain of a slip system will i The cumulative plastic shear strain at the critical point is obtained by summing the plastic shear strain of each slip system.

[0055] In this embodiment of the invention, in each incremental step of the solution process, the crystal plasticity model outputs the plastic shear strain increment of each slip system. By summing the plastic shear strain increments of all incremental steps, the result can be obtained. i The cumulative plastic shear strain at the critical point is obtained by summing the plastic shear strains of each active slip system and then calculating the plastic shear strains of all active slip systems. The formula for calculating the cumulative plastic shear strain at the critical point is as follows:

[0056] ; c accum Indicates cumulative plastic shear strain; c acc(i) Indicates the first i Plastic shear strain of a slip system.

[0057] Specifically, the number of slip systems is 12. That is, i =12.

[0058] Step 2.3, the specific method for calculating the strain energy of plastic slip deformation is as follows: Multiply the product of the cumulative plastic shear strain and the fatigue load in the crystal plasticity by 1 / 2.

[0059] That is, the strain energy of plastic slip deformation = In this embodiment of the invention, the strain energy of plastic slip deformation represents the plastic dissipation energy density per unit volume, which is the portion of mechanical work that is irreversibly converted into heat and microscopic damage per unit volume of a single-crystal alloy sample under cyclic loading due to plastic deformation.

[0060] In this embodiment of the invention, a CPFEM model of a single-crystal alloy considering recrystallization defects and different secondary orientations is established. Furthermore, cyclic plastic deformation and slip system interactions are considered, and a relevant fatigue indicator parameter, namely cumulative plastic shear strain, is introduced. The shear strain of each grain across the 12 slip systems is accumulated to obtain... c accum The evolution of fatigue deformation damage within recrystallization and single crystals was analyzed.

[0061] Step 3: Use half of the product of cumulative plastic shear strain and fatigue load in crystal plasticity, or the cumulative plastic shear strain, as the fatigue indicator factor; use the fatigue indicator factor as the ordinate and the fatigue life of the single crystal alloy sample as the abscissa to fit and obtain the fatigue life prediction model, which is used for fatigue life prediction of nickel-based single crystal alloys.

[0062] To better describe the influence of the second crystal orientation and recrystallization on the fatigue life of single-crystal alloys involved in the embodiments of the present invention, it is further examined whether different fatigue indicator factors (FIPs) can take into account the above-mentioned fatigue performance influencing factors. Figure 1 The SN curve is obtained by conducting stress-controlled fatigue tests; Figure 2 and Figure 3 Two different fatigue indicator factors are presented respectively. Figure 2 Based on Figure 1 The fatigue stress parameters of the data points are substituted into the corresponding crystal plasticity model to calculate the cumulative plastic strain at the critical point, thereby obtaining the relationship between the cumulative plastic strain and fatigue life. Then, by fitting the data points, the fatigue life can be predicted. Figure 3 Based on Figure 2 Further calculations based on this yielded the relationship between strain energy and fatigue life in plastic slip deformation.

[0063] Depend on Figure 2 It is evident that using cumulative plastic shear strain can, to some extent, account for the influence of the second crystal orientation and recrystallization on the fatigue life of single-crystal alloys. Correlation analysis of the data yields the following fitting results: Figure 2 The purple dotted lines in the image are shown below: When cumulative plastic shear strain is used as a fatigue indicator, the fatigue life prediction model is as follows: FIP=a ( N f )n ; FIP=c accum ; in, FIP Indicates fatigue indicator factor; N f Indicates fatigue life; 'a' represents a coefficient. a =128.66347; n Represents the fitted parameters, n =-0.13839; c accum This represents the cumulative plastic shear strain.

[0064] Considering the strain energy of plastic slip deformation as a fatigue indicator, similar to the Smith criterion, we examine the ability of the fatigue indicator to describe the factors affecting fatigue life. The results are as follows. Figure 3 As shown.

[0065] Depend on Figure 3 It is evident that the fatigue indicator factor (FIP) can describe the microstructure correlation of fatigue life, compared to... Figure 2 Better data relevance was achieved. Specific results are as follows:

[0066] Using half the product of cumulative plastic shear strain and fatigue load in crystal plasticity as the fatigue indicator factor, the fatigue life prediction model is as follows: FIP=b ( N f ) m ; ; in, FIP Indicates fatigue indicator factor; N f Indicates fatigue life; b Represents the coefficient. b =555.2148; m Represents the fitted parameters, m =-0.13941; c accum Represents cumulative plastic shear strain ;s max This represents the fatigue load during crystal plasticity.

[0067] In summary, this invention has established a method for predicting the fatigue life of single-crystal alloys based on crystal plasticity simulation, considering the effects of second orientation and recrystallized grains. This method shows a good correlation with the fatigue performance data of this invention, and the fitted R0 is high. 2 It is 0.72381.

[0068] The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects, as described in this invention, can supplement the shortcomings of fatigue life prediction for nickel-based single-crystal alloys in engineering, achieving fatigue life prediction that considers recrystallization and second orientation. Figure 2 and Figure 3 The results show that the prediction results are relatively stable, reducing the impact of uncontrollable factors. The prediction results are all near the prediction curves for 0°-SX, 45°-SX, 0°-RC, and 45°-RC, indicating that the model has good applicability and universality.

[0069] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for predicting the fatigue life of nickel-based single-crystal alloys considering secondary orientation and recrystallization defects, characterized in that, Includes the following steps: Multiple nickel-based single-crystal alloys were obtained as single-crystal alloy samples. These samples had different secondary orientations and some exhibited recrystallization defects. A crystal plasticity model was established based on the crystal plasticity parameters of each single-crystal alloy sample. Obtain the fatigue life and fatigue stress parameters of each single-crystal alloy specimen; input the fatigue stress parameters corresponding to each single-crystal alloy specimen into the corresponding crystal plasticity model, and calculate the cumulative plastic shear strain at the critical point; Half of the product of cumulative plastic shear strain and fatigue load in crystal plasticity, or the cumulative plastic shear strain, is used as the fatigue indicator factor. By fitting the fatigue indicator factor as the ordinate and the fatigue life of the single-crystal alloy sample as the abscissa, a fatigue life prediction model is obtained and used for fatigue life prediction of nickel-based single-crystal alloys.

2. The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects according to claim 1, characterized in that, The method for obtaining the fatigue life and fatigue stress parameters of each single-crystal alloy specimen is as follows: High-temperature fatigue tests were conducted on each single-crystal alloy sample at a constant temperature under different stress levels to obtain the fatigue life and fatigue stress parameters of each single-crystal alloy sample.

3. The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects according to claim 2, characterized in that, The conditions for high-temperature fatigue testing are as follows: Low-cycle fatigue testing with stress control was conducted at a temperature of 550℃ and a stress ratio of R=0.1 using a sinusoidal loading waveform with a frequency of 10Hz.

4. The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects according to claim 1, characterized in that, The method for calculating the cumulative plastic shear strain at the critical point is as follows: The fatigue stress parameters corresponding to each single-crystal alloy sample are input into the corresponding crystal plasticity model, and the solution is obtained step by step under cyclic loading. i The plastic shear strain of a slip system will i The cumulative plastic shear strain at the critical point is obtained by summing the plastic shear strain of each slip system.

5. The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects according to claim 1, characterized in that, The plasticity parameters of single-crystal alloy samples include: crystal phase, h 0、 τ 0、 τ s , C 11 , C 12 , C 44 , and n ; in, h 0 represents the initial hardening modulus; τ 0 represents the initial critical shear stress; τ s Indicates saturated flow stress; C 11 , C 12 and C 44 Represents three elastic constants; This represents the initial critical shear rate of the slip system; n This represents the strain hardening index.

6. The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects according to claim 5, characterized in that, The method for establishing a crystal plasticity model is as follows: Electron backscatter diffraction data of single-crystal alloy samples were acquired, and a single-crystal model was obtained. The crystal plasticity parameters were calibrated to ensure that the experimental curves were consistent with the simulation curves, thereby determining the crystal plasticity model parameters of the single-crystal alloy samples and establishing the calibrated crystal plasticity model.

7. The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects according to claim 1, characterized in that, The different second orientations are [010] orientation and [110] orientation; the recrystallization defects are grain boundary defects and grain size inhomogeneity defects.

8. The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects according to claim 1, characterized in that, When cumulative plastic shear strain is used as a fatigue indicator, the fatigue life prediction model is as follows: FIP=a ( N f ) n ; FIP=γ accum ; in, FIP Indicates fatigue indicator factor; N f Indicates fatigue life; a Indicates coefficient; n Indicates the fitted parameters; γ accum This represents the cumulative plastic shear strain.

9. The fatigue life prediction method for nickel-based single-crystal alloys considering second orientation and recrystallization defects according to claim 1, characterized in that, Using half the product of cumulative plastic shear strain and fatigue load in crystal plasticity as the fatigue indicator factor, the fatigue life prediction model is as follows: FIP=b ( N f ) m ; ; in, FIP Indicates fatigue indicator factor; N f Indicates fatigue life; b Indicates coefficient; m Indicates the fitted parameters; γ accum σ represents the cumulative plastic shear strain. max This represents the fatigue load during crystal plasticity.