Conductive, flame-retardant polymer solid-state electrolyte and preparation method and application thereof

CN122315055APending Publication Date: 2026-06-30SHANDONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610668513.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-15
Publication Date
2026-06-30

AI Technical Summary

Technical Problem

Existing PEO-based solid polymer electrolytes suffer from problems such as low room temperature ionic conductivity, decreased mechanical properties with increasing temperature, and flammability, making it difficult to balance good ionic conductivity and thermal safety performance.

Method used

A composite solid polymer electrolyte is prepared by combining conductive expanded graphite (EG) and aramid nanofibers (ANF) with polyethylene oxide (PEO). EG provides a uniform current density distribution, ANF enhances mechanical properties, and EG expands at high temperatures to form a heat insulation layer.

Benefits of technology

It improves the ion conductivity and thermal safety performance of the electrolyte, inhibits lithium dendrite growth, reduces the risk of battery thermal runaway, simplifies the preparation process, and facilitates industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122315055A_ABST
    Figure CN122315055A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of solid polymer electrolyte technology, specifically relating to a conductive and flame-retardant polymer solid electrolyte, its preparation method, and its application. The preparation method involves first dissolving chopped aramid fibers in an organic solvent and then leaching them to obtain an ANF membrane; then coating the surface of the ANF membrane with an EG / PEO / LiTFSI electrolyte solution and vacuum drying to obtain an EG / PEO@ANF composite solid electrolyte. ANF can reduce the crystallinity of PEO and improve the crystallinity of Li... + Migration behavior in solid electrolytes; as a reinforcing framework, it effectively improves the mechanical strength and thermal stability of solid electrolytes and inhibits the growth of lithium dendrites; the introduction of EG as a flame-retardant filler significantly improves the thermal safety performance of solid electrolytes under high temperature or combustion conditions; it can also distribute charges uniformly in the electrolyte through its conductivity, suppress the phenomenon of excessively high local current density, improve the contact of the electrode / electrolyte interface, reduce the interface impedance, and effectively improve the ionic conductivity of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid polymer electrolyte technology for solid lithium batteries, specifically relating to a conductive and flame-retardant polymer solid electrolyte, its preparation method, and its application. Background Technology

[0002] In recent years, accidents involving lithium-ion batteries, such as leaks, flammability, and explosions caused by short circuits, have seriously threatened people's lives and property. Solid-state electrolytes have attracted much attention as they can replace flammable organic liquid electrolytes. Among them, solid polymer electrolytes, as a major branch of solid-state electrolytes, are considered one of the most promising electrolyte systems for solid-state lithium batteries due to their high stability, high flexibility, high processability, and good contact with the positive and negative electrode interfaces. Among various polymer matrices, polyethylene oxide (PEO) has become the most widely studied solid polymer electrolyte due to its excellent lithium salt dissolution ability imparted by its high dielectric constant, as well as its good electrochemical stability, environmental friendliness, and low cost.

[0003] However, existing PEO-based solid polymer electrolytes still have several shortcomings: Firstly, PEO has high crystallinity at room temperature, which restricts the mobility of polymer chain segments, resulting in low room temperature ionic conductivity. Secondly, the mechanical properties of PEO-based electrolytes decrease with increasing temperature, making it difficult to effectively suppress the growth of lithium dendrites. In addition, PEO materials themselves are flammable, posing safety hazards under extreme conditions such as high temperatures or flame burning.

[0004] To address the aforementioned issues, existing research has attempted to modify PEO-based solid polymer electrolytes by introducing inorganic reinforcing materials, functional fillers, or flame-retardant components. However, current technologies generally suffer from limited reinforcing effects, difficulty in simultaneously achieving flame retardant and electrochemical properties, and complex or limited preparation processes, making it challenging to obtain PEO-based solid polymer electrolytes that simultaneously possess both good ion conductivity and thermal safety performance.

[0005] Therefore, it is still necessary to provide a PEO-based solid electrolyte that is structurally stable, has a controllable preparation method, and can significantly improve thermal safety while ensuring good electrochemical performance, in order to meet the actual needs of solid-state lithium batteries for high safety and comprehensive performance. Summary of the Invention

[0006] To address the problems in the prior art, this invention provides an aramid nanofiber / polyoxyethylene flame-retardant solid polymer electrolyte containing conductive expanded graphite (EG) and its preparation method. By combining an aramid nanofiber (ANF) membrane with an EG-containing PEO-based polymer electrolyte, wherein the conductive EG can effectively uniformize the negative electrode interface current density and suppress lithium dendrite growth, a composite solid polymer electrolyte with both good ion conductivity and thermal safety performance is prepared. This electrolyte is then applied to solid-state lithium batteries to improve battery safety and overall performance.

[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0008] A conductive and flame-retardant polymer solid electrolyte includes an aramid nanofiber (ANF) membrane and expanded graphite (EG), polyethylene oxide (PEO), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) uniformly distributed on the surface and inside of the aramid nanofiber membrane.

[0009] Preferably, the mass ratio of PEO to LiTFSI is 1:(0.2 to 0.6).

[0010] Preferably, the particle size of the EG particles is 10-70 µm, and more preferably 60 µm.

[0011] Preferably, the amount of EG added is 5 to 40 wt% of the total mass of PEO, LiTFSI and EG, and more preferably 20 wt%.

[0012] The method for preparing the conductive and flame-retardant polymer solid electrolyte includes the following steps: (1) PEO and LiTFSI are added to an organic solvent and mixed under constant temperature stirring to fully dissolve the lithium salt and form a uniform polymer electrolyte solution with PEO. (2) Add EG to the polymer electrolyte solution and mix well to obtain EG / PEO / LiTFSI electrolyte solution; (3) The EG / PEO / LiTFSI electrolyte solution was coated on the surface of the ANF membrane and left to stand at room temperature to allow the electrolyte solution to penetrate into the aramid membrane structure. The membrane was then dried under vacuum to obtain the EG / PEO@ANF composite solid electrolyte.

[0013] Preferably, in step (1), the mass ratio of PEO to organic solvent volume is 1 g:(10-30 mL); more preferably, in step (1), the mass ratio of PEO to organic solvent volume is 1 g:20 mL.

[0014] Preferably, in step (1), the organic solvent is selected from acetonitrile, tetrahydrofuran, etc.N,N -Dimethylformamide, N,N -One or more of dimethylacetamide and acetone; more preferably acetonitrile.

[0015] More preferably, in step (1), PEO and LiTFSI are added to acetonitrile and magnetically stirred at 20-60 °C for 2-10 h to fully dissolve PEO and LiTFSI; in step (2), EG is added and magnetically stirred at 20-60 °C for 1-6 h until a uniformly dispersed electrolyte solution is obtained.

[0016] Preferably, the method for preparing the ANF membrane in step (3) includes the following steps: S1. Place the chopped aramid fibers in a beaker, add anhydrous ethanol, and place the beaker in an ultrasonic instrument for ultrasonic treatment to remove surface impurities; then repeatedly wash the chopped aramid fibers with deionized water, and place the washed chopped aramid fibers in a vacuum drying oven to dry them, thus obtaining pretreated aramid fibers. S2. Add potassium hydroxide (KOH) to dimethyl sulfoxide (DMSO) and stir to mix evenly to prepare a KOH / DMSO alkaline solution; then add the pretreated aramid fiber to the above alkaline solution and stir continuously under water bath conditions to allow ANF to be deprotonated and gradually dissociated in a strongly alkaline environment until a uniform and stable ANF dispersion is formed, i.e., an ANF / DMSO alkaline solution; S3. Using a coating method, the ANF / DMSO alkaline solution prepared in step S2 is coated onto a smooth and clean substrate to form a wet film; then the coated substrate is immersed in deionized water for phase inversion treatment, so that ANF is precipitated and a continuous ANF film is formed; after the phase inversion is completed, the obtained ANF film is immersed in an organic solvent multiple times to further remove residual solvent and moisture.

[0017] More preferably, in step S2, KOH and DMSO are prepared at a mass ratio of 1:(50-150) to form a high-concentration alkaline solution.

[0018] More preferably, in step S2, the mass concentration of ANF in the KOH / DMSO alkaline solution is 0.005–0.04 g / mL.

[0019] More preferably, in step S2, the pretreated aramid fiber is added to the alkaline solution and stirred continuously for 3 to 10 days under a water bath at 40 to 70 °C until a uniform and stable dark red solution is formed.

[0020] More preferably, in step S3, the coating process is carried out at room temperature, and the ANF / DMSO solution is coated into a film using a blade coating method, with a blade gap thickness of 50–300 µm; more preferably 100 µm.

[0021] More preferably, in step S3, the substrate is a glass substrate or a silicon substrate, and even more preferably a glass substrate.

[0022] Preferably, in step S3, the ANF membrane is transferred to release paper, and the EG / PEO / LiTFSI electrolyte solution is poured onto the surface of the aramid membrane and left to stand at room temperature for 4–12 h; then it is transferred to a vacuum drying oven and vacuum dried at 40–80 °C for 6–24 h; more preferably, it is vacuum dried at 60 °C for 12 h.

[0023] Application of the conductive and flame-retardant polymer solid electrolyte in lithium batteries.

[0024] The raw materials and solvents used in the embodiments of this invention can all be obtained through commercially available channels. The reagents used in the experiments are of analytical grade or higher, and their purity does not constitute a limitation on this invention.

[0025] Compared with the prior art, the beneficial effects of the present invention are reflected in: 1. This invention improves the migration behavior of lithium ions in solid electrolytes by introducing ANF into PEO-based solid electrolytes, thereby reducing the crystallinity of PEO and increasing the proportion of amorphous phase; it also acts as a reinforcing framework, effectively improving the mechanical strength and thermal stability of solid electrolytes, thereby inhibiting the growth of lithium dendrites.

[0026] 2. By introducing EG as a flame-retardant filler into the PEO-based electrolyte, this invention significantly improves the thermal safety performance of solid electrolytes under high-temperature or combustion conditions. EG can expand in volume under heating conditions, forming a heat-insulating and oxygen-barrier layer, thereby physically blocking the transfer of heat and flammable gases, effectively reducing the risk of thermal runaway of the battery under extreme conditions.

[0027] 3. The EG introduced in this invention not only has good flame retardant properties, but also can uniformly distribute charge in the electrolyte through its conductivity. Its conductive particles dispersed in the polymer matrix help regulate the electric field distribution inside the electrolyte, suppress the phenomenon of excessively high local current density, thereby improving the contact at the electrode / electrolyte interface, reducing interfacial impedance, and effectively improving the ionic conductivity of the battery.

[0028] 4. The preparation method of the composite solid polyelectrolyte provided by the present invention is simple and the raw materials used are widely available, which is conducive to realizing large-scale industrial production. Attached Figure Description

[0029] Figure 1 These are transmission electron microscope images from ANF.

[0030] Figure 2 These are scanning electron microscope (SEM) images of the surface and cross-section of the EG / PEO@ANF solid polymer electrolyte; where (a) is a surface SEM image and (b) is a cross-sectional SEM image.

[0031] Figure 3 These are the X-ray diffraction patterns of three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF.

[0032] Figure 4 These are differential scanning calorimetry curves of three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF.

[0033] Figure 5 This is a comparison chart of the ionic conductivity of three solid polymer electrolytes, PEO, PEO@ANF, and EG / PEO@ANF, at different temperatures.

[0034] Figure 6 These are the AC impedance spectra of three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF.

[0035] Figure 7 This is a graph showing the cycle performance test results of Li / Li batteries containing different electrolytes.

[0036] Figure 8 The graph shows the long-cycle performance test results of LFP (lithium iron phosphate) / / Li batteries using three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF.

[0037] Figure 9 The thermogravimetric analysis (TGA) and differential thermogravimetric analysis (DGA) curves of three solid polymer electrolytes, PEO, PEO@ANF and EG / PEO@ANF, are shown; (a) is the TGA curve and (b) is the DGA curve.

[0038] Figure 10 These are open flame combustion test diagrams for PEO, PEO@ANF, and EG / PEO@ANF solid polymer electrolyte membranes. Detailed Implementation

[0039] The present invention will be further described below with reference to specific embodiments, and the advantages and features of the present invention will become clearer with the description. However, the embodiments are merely exemplary and do not constitute any limitation on the scope of the present invention. Those skilled in the art should understand that modifications or substitutions can be made to the details and form of the technical solutions of the present invention without departing from the spirit and scope of the present invention, but all such modifications and substitutions fall within the protection scope of the present invention.

[0040] Example 1 A method for preparing an EG / PEO@ANF solid polymer electrolyte includes the following steps: 1) Preparation of ANF solution: First, chopped aramid fibers were placed in a beaker, anhydrous ethanol was added, and the mixture was sonicated for 2 h to remove impurities from the surface of the aramid fibers. Then, the aramid fibers were repeatedly washed with deionized water and dried in a vacuum drying oven to obtain pretreated aramid fibers. 2 g of KOH was weighed and added to 200 mL of DMSO, and stirred magnetically for 1 h to prepare a KOH / DMSO alkaline solution. Subsequently, 4 g of the pretreated aramid fibers were added to the alkaline solution, and the mixture was continuously stirred magnetically for 7 days in a 50 ℃ water bath to allow the aramid fibers to deprotonate and gradually dissociate in a strongly alkaline environment until a uniform and stable dark red aramid nanofiber dispersion was formed, resulting in an ANF / DMSO solution with a mass concentration of 0.02 g / mL.

[0041] 2) Preparation of EG / PEO / LiTFSI electrolyte solution: Weigh 1.0 g PEO and 0.4 g LiTFSI, add them to 20 mL acetonitrile solvent, and stir in a water bath with magnetic stirring at 25 ℃ for 6 h to fully dissolve PEO and LiTFSI and form a homogeneous polymer electrolyte solution. Then add 0.35 g EG (particle size approximately 60 µm) to the above solution, and continue magnetic stirring for 3 h under the same conditions to uniformly disperse EG in the polymer electrolyte system, obtaining a homogeneous and stable EG / PEO / LiTFSI electrolyte solution, wherein the amount of EG added accounts for approximately 20 wt% of the total mass of PEO, LiTFSI and EG.

[0042] 3) Preparation of EG / PEO@ANF composite solid polymer electrolyte: The ANF / DMSO solution prepared in step 1 was coated onto a smooth and clean glass substrate with a blade gap thickness of 100 µm using a four-sided coater to form a wet film. The coated glass substrate was then immersed in deionized water for 10 min for phase inversion treatment, causing ANF to precipitate and form a continuous ANF film. After phase inversion, the resulting ANF film was washed three times in acetonitrile to further remove residual solvent and moisture, and then transferred to release paper. The EG / PEO / LiTFSI electrolyte solution prepared in step 2 was uniformly poured onto the surface of the ANF film, allowing the electrolyte solution to fully penetrate the ANF film structure. The resulting composite system was allowed to stand at room temperature for 6 h, and then transferred to a vacuum drying oven and dried at 60 ℃ under vacuum for 12 h to remove residual solvent, finally obtaining an aramid nanofiber / polyoxyethylene composite solid polymer electrolyte membrane containing expanded graphite, i.e., the EG / PEO@ANF composite solid electrolyte.

[0043] 4) Li was selected as the negative electrode and LFP as the positive electrode. Button cells of Li / / Li and Li / / LFP were assembled using the negative electrode-solid electrolyte-positive electrode structure and their electrochemical performance was tested.

[0044] Figure 1 This is a TEM image of ANF obtained by the method of dissolving crude aramid fibers in an organic solvent and then precipitating them, as described in this invention. From Figure 1 As can be seen, ANF exhibits a slender one-dimensional nanofiber morphology, which interweaves to form a continuous three-dimensional network structure. The fibers are evenly distributed and there is no obvious agglomeration, indicating that the prepared ANF has good dispersibility and structural integrity. Figure 2 These are SEM images of the surface (a) and cross-section (b) of the EG / PEO@ANF solid polymer electrolyte. From... Figure 2 As can be seen, the prepared EG / PEO@ANF solid electrolyte has a dense surface with no obvious pores or cracks observed; the cross-sectional structure is continuous and complete, and the electrolyte layer thickness is uniform, about 100 μm, indicating that the electrolyte membrane has good film-forming properties and structural integrity.

[0045] Comparative Example 1 A method for preparing a solid polymer electrolyte includes the following steps: 1) Preparation of PEO / LiTFSI electrolyte solution: Weigh 1.0 g PEO and 0.4 g LiTFSI, add them to 20 mL acetonitrile solvent, and stir in a water bath with magnetic stirring at 25 °C for 6 h to fully dissolve PEO and LiTFSI and form a homogeneous polymer electrolyte solution.

[0046] 2) Preparation of PEO solid polymer electrolyte: PEO / LiTFSI electrolyte solution was directly poured onto release paper, and after standing at room temperature for 6 h, it was transferred to a vacuum drying oven and dried at 60 ℃ under vacuum for 12 h to obtain PEO solid polymer electrolyte membrane.

[0047] 3) Li was selected as the negative electrode and LFP as the positive electrode. Button cells of Li / / Li and Li / / LFP were assembled using the negative electrode-solid electrolyte-positive electrode structure and their electrochemical performance was tested.

[0048] Comparative Example 2 A method for preparing a solid polymer electrolyte includes the following steps: 1) Preparation of aramid nanofiber solution: First, chopped aramid fibers were placed in a beaker, anhydrous ethanol was added, and the mixture was sonicated for 2 h to remove impurities from the surface of the aramid fibers. Then, the aramid fibers were repeatedly washed with deionized water and dried in a vacuum drying oven to obtain pretreated aramid fibers. 2 g of KOH was weighed and added to 200 mL of DMSO, and stirred magnetically for 1 h to prepare a KOH / DMSO alkaline solution. Subsequently, 4 g of the pretreated aramid fibers were added to the alkaline solution, and the mixture was continuously magnetically stirred at 50 ℃ for 7 days to allow the aramid fibers to deprotonate and gradually dissociate in a strongly alkaline environment until a uniform and stable dark red aramid nanofiber dispersion was formed, resulting in an ANF / DMSO solution with a mass concentration of 0.02 g / mL.

[0049] 2) Preparation of PEO / LiTFSI electrolyte solution: Weigh 1.0 g PEO and 0.4 g LiTFSI, add them to 20 mL acetonitrile solvent, and stir in a water bath with magnetic stirring at 25 °C for 6 h to fully dissolve PEO and LiTFSI and form a homogeneous polymer electrolyte solution.

[0050] 3) Preparation of PEO@ANF solid polymer electrolyte: The ANF / DMSO solution prepared in step 1 was coated onto a smooth and clean glass substrate with a blade gap thickness of 100 µm using a four-sided coater to form a wet film. The coated glass substrate was then immersed in deionized water for 10 min for phase inversion treatment, causing ANF to precipitate and form a continuous ANF film. After phase inversion, the resulting ANF film was washed three times in acetonitrile to further remove residual solvent and moisture, and then transferred to release paper. The PEO / LiTFSI electrolyte solution prepared in step 2 was uniformly cast onto the surface of the aramid nanofiber membrane, allowing the electrolyte solution to fully penetrate the ANF membrane structure. The resulting composite system was allowed to stand at room temperature for 6 h, and then transferred to a vacuum drying oven and dried under vacuum at 60 ℃ for 12 h to remove residual solvent, yielding the PEO@ANF solid polymer electrolyte membrane.

[0051] 4) Li was selected as the negative electrode and LFP as the positive electrode. Button cells of Li / / Li and Li / / LFP were assembled using the negative electrode-solid electrolyte-positive electrode structure and their electrochemical performance was tested.

[0052] Figure 3 These are the XRD patterns of three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF from Example 1. From... Figure 3 As can be seen, the PEO electrolyte exhibits distinct characteristic diffraction peaks at approximately 19.5° and 23.7° at 2θ, indicating its high crystallinity. After the introduction of ANF, the diffraction peak intensity of the PEO@ANF electrolyte is significantly reduced, indicating that the addition of ANF effectively inhibits the crystallization behavior of PEO. Upon further introduction of EG, the diffraction peaks of the EG / PEO@ANF composite electrolyte are further weakened and tend to broaden, indicating an increase in the content of amorphous phase in the system. Figure 4 These are the DSC curves for three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF. From... Figure 4 As can be seen, the melting temperature of the PEO electrolyte is 49 ℃, corresponding to the endothermic melting peak in its crystalline region. After introducing ANF, the melting temperature drops to 46 ℃, indicating that ANF inhibits the ordered arrangement of PEO chains through hydrogen bonding, leading to a decrease in crystallinity. The melting temperature of the EG / PEO@ANF electrolyte further decreases to 44 ℃. This is because the layered structure of EG further restricts the free movement of PEO chain segments through physical filling, thereby reducing the crystallinity of the system.

[0053] Figure 5 This is a comparison of the ionic conductivity of three solid polymer electrolytes—PEO, PEO@ANF, and EG / PEO@ANF—at different temperatures. Figure 5As can be seen, under the same temperature conditions, the ionic conductivity of PEO@ANF and EG / PEO@ANF electrolytes is higher than that of PEO electrolyte; and the ionic conductivity of all three electrolytes shows a gradual increasing trend with increasing temperature. Among them, EG / PEO@ANF electrolyte exhibits the highest ionic conductivity throughout the entire test temperature range. Figure 6 These are the AC impedance spectra of three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF. From... Figure 6 As can be seen, compared with PEO electrolyte, the impedance of PEO@ANF and EG / PEO@ANF electrolytes is significantly reduced, with EG / PEO@ANF electrolyte exhibiting the lowest impedance value, indicating superior ion transport performance. This result demonstrates that the introduction of EG effectively reduces the charge transport impedance within the electrolyte and at the electrode / electrolyte interface, improving interfacial contact and ion transport conditions.

[0054] Figure 7 These are cycle performance test graphs for Li / / Li batteries containing different electrolytes. From... Figure 7 As can be seen, compared with the PEO electrolyte-assembled battery which short-circuited at 240 h, the EG / PEO@ANF electrolyte-assembled battery has a cycle life of more than 1000 hours. This indicates that EG can effectively alleviate the problem of uneven interfacial current density during cycling, significantly improve interfacial stability, and effectively inhibit the growth of lithium dendrites. Figure 8 This is a long-cycle performance test chart of LFP / / Li batteries using three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF. The first 10 cycles were pre-cycled at 0.2 C rate, followed by long-cycle testing at 1.0 C rate. Figure 8 As can be seen, the battery using EG / PEO@ANF electrolyte exhibits higher and more stable discharge capacity during long-term cycling, and its capacity decay rate is significantly lower than that of the battery using PEO electrolyte, indicating that the electrolyte has excellent charge-discharge stability.

[0055] Figure 9 The figures show the TG(a) and DTG(b) curves for three solid polymer electrolytes: PEO, PEO@ANF, and EG / PEO@ANF. From... Figure 9As can be seen, the initial thermal decomposition temperature of the electrolyte increases after the introduction of ANF, indicating that the introduction of ANF improves the thermal stability of the electrolyte to a certain extent. For the EG / PEO@ANF electrolyte, a significant mass change occurs at approximately 290 °C. This behavior is mainly due to the expansion reaction of EG under heating conditions, rather than the premature thermal decomposition of the polymer matrix. At the same time, its DTG peak intensity decreases significantly, and the char residue in the TG curve increases significantly at high temperatures, indicating that EG can form a stable expanded char layer under high-temperature conditions, thereby effectively blocking heat and oxygen transfer and significantly improving the flame retardant performance and thermal safety of the electrolyte. Figure 10 These are open flame combustion test images of PEO, PEO@ANF, and EG / PEO@ANF solid polymer electrolyte membranes. From... Figure 10 As can be seen, the EG / PEO@ANF electrolyte exhibits significant flame retardant effect, and the introduction of EG effectively suppresses the droplet behavior of the PEO matrix at high temperatures.

[0056] Example 2 A method for preparing EG / PEO@ANF solid polymer electrolyte differs from Example 1 in that the coating thickness of the ANF membrane is different during preparation, while the remaining steps and conditions are the same as in Example 1.

[0057] Specifically, in step 3, the ANF / DMSO solution prepared in step 1 is coated onto a smooth and clean glass substrate with a blade gap thickness of 200 µm using a four-sided coater to form a wet film. Subsequently, the film undergoes deionized water phase conversion treatment, multiple acetonitrile immersion, transfer to release paper, casting of EG / PEO / LiTFSI electrolyte solution, standing at room temperature, and vacuum drying to finally obtain the EG / PEO@ANF solid polymer electrolyte membrane.

[0058] Example 3 A method for preparing an EG / PEO@ANF solid polymer electrolyte differs from Example 1 in that the amount of EG added is different, while the remaining steps and conditions are the same as in Example 1.

[0059] Specifically, in step 2, 0.155 g of EG was weighed and added to a polymer electrolyte solution formed by 1.0 g of PEO, 0.4 g of LiTFSI, and 20 mL of acetonitrile, so that the amount of EG added accounted for approximately 10 wt% of the total mass of PEO, LiTFSI, and EG. The mixture was then magnetically stirred for 3 h at 25 °C to ensure uniform dispersion of EG in the electrolyte system, resulting in an EG / PEO / LiTFSI electrolyte solution with a low EG content. Subsequently, a composite solid polymer electrolyte membrane was prepared according to the method in step 3 of Example 1.

[0060] Example 4 A method for preparing an EG / PEO@ANF solid polymer electrolyte differs from Example 1 in that the electrolyte solution is introduced into the ANF membrane in a different way; the remaining steps and conditions are the same as in Example 1.

[0061] Specifically, in step 3, the ANF membrane prepared by phase inversion and washed with acetonitrile is directly immersed in the EG / PEO / LiTFSI electrolyte solution prepared in step 2 and allowed to stand at room temperature for 6 h to allow the electrolyte solution to fully penetrate into the ANF membrane. Then, the ANF membrane is removed and placed in a vacuum drying oven and dried at 60 °C under vacuum for 12 h to remove residual solvent, finally obtaining the EG / PEO@ANF composite solid polymer electrolyte membrane prepared by impregnation.

Claims

1. An electrically conductive, flame-retardant, polymeric solid-state electrolyte, characterized in that, It includes aramid nanofiber membranes, and expanded graphite (EG), polyethylene oxide (PEO), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) uniformly distributed on the surface and inside of the aramid nanofiber membranes.

2. The electrically conductive, flame-retardant, polymer solid-state electrolyte of claim 1, wherein, The mass ratio of PEO to LiTFSI is 1:(0.2-0.6); preferably, the particle size of the EG particles is 10-70 µm, more preferably 60 µm; preferably, the amount of EG added is 5-40 wt% of the total mass of PEO, LiTFSI and EG, more preferably 20 wt%.

3. A method of preparing an electrically conductive, flame-retardant polymer solid-state electrolyte according to claim 1 or 2, characterized in that, Includes the following steps: (1) PEO and LiTFSI are added to an organic solvent and mixed under constant temperature stirring to fully dissolve the lithium salt and form a uniform polymer electrolyte solution with PEO. (2) Add EG to the polymer electrolyte solution and mix well to obtain EG / PEO / LiTFSI electrolyte solution; (3) The EG / PEO / LiTFSI electrolyte solution was coated on the surface of the ANF membrane and left to stand at room temperature to allow the electrolyte solution to penetrate into the ANF membrane structure. The membrane was then dried under vacuum to obtain the EG / PEO@ANF composite solid electrolyte.

4. The method for preparing a conductive and flame-retardant polymer solid electrolyte according to claim 3, characterized in that, In step (1), the mass ratio of PEO to organic solvent is 1 g: (10-30) mL; more preferably, in step (1), the mass ratio of PEO to organic solvent is 1 g: 20 mL. Preferably, in step (1), the organic solvent is selected from acetonitrile, tetrahydrofuran, N,N - dimethylformamide, N,N - dimethylacetamide, acetone, one or more of them; further preferably acetonitrile.

5. The method for preparing a conductive and flame-retardant polymer solid electrolyte according to claim 4, characterized in that, In step (1), PEO and LiTFSI are added to acetonitrile and magnetically stirred at 20-60 °C for 2-10 h to fully dissolve PEO and LiTFSI; in step (2), EG is added and magnetically stirred at 20-60 °C for 1-6 h until a uniformly dispersed electrolyte solution is obtained.

6. The method for preparing a conductive and flame-retardant polymer solid electrolyte according to claim 4, characterized in that, The method for preparing the ANF membrane in step (3) includes the following steps: S1. Add chopped aramid fibers to anhydrous ethanol and sonicate to remove surface impurities; then repeatedly wash the chopped aramid fibers with deionized water and dry them in a vacuum drying oven to obtain pretreated aramid fibers. S2. Add potassium hydroxide (KOH) to dimethyl sulfoxide (DMSO) and stir to mix evenly to prepare a KOH / DMSO alkaline solution; add the pretreated aramid fiber obtained in step S1 to the above alkaline solution and stir continuously under water bath conditions to allow ANF to undergo deprotonation and gradually dissociate in a strongly alkaline environment until a uniform and stable ANF dispersion is formed, i.e., ANF / DMSO solution. S3. Using a coating method, the ANF / DMSO solution prepared in step S2 is coated onto a smooth and clean substrate to form a wet film; then the coated substrate is immersed in deionized water for phase inversion treatment, so that ANF is precipitated and a continuous ANF film is formed; after the phase inversion is completed, the obtained ANF film is immersed in an organic solvent multiple times to further remove residual solvent and moisture.

7. The method for preparing a conductive and flame-retardant polymer solid electrolyte according to claim 6, characterized in that, In step S2, the mass ratio of KOH to DMSO is 1:(50-150); preferably, in step S2, the mass concentration of ANF in the KOH / DMSO alkaline solution is 0.005-0.04 g / mL.

8. The method for preparing a conductive and flame-retardant polymer solid electrolyte according to claim 6, characterized in that, In step S2, the pretreated aramid fibers are added to the alkaline solution and stirred continuously for 3 to 10 days under a water bath at 40 to 70 ℃ until a uniform and stable dark red solution is formed.

9. The method for preparing a conductive and flame-retardant polymer solid electrolyte according to claim 6, characterized in that, In step S3, the coating process is carried out at room temperature, and the ANF / DMSO solution is coated into a film using a doctor blade coating method. The thickness of the doctor blade gap is 50-300 µm; more preferably, it is 100 µm. Preferably, in step S3, the ANF film is transferred to release paper, and the EG / PEO / LiTFSI electrolyte solution is poured onto the surface of the ANF film. After that, it is left to stand at room temperature for 4-12 h; then it is transferred to a vacuum drying oven and vacuum dried at 40-80 °C for 6-24 h; more preferably, it is vacuum dried at 60 °C for 12 h.

10. The application of the conductive, flame-retardant polymer solid electrolyte according to claim 1 or 2 in the preparation of solid-state lithium batteries.