Apparatus, method and use for forming a uniform coating on the inner wall of a pipe to be plated
By setting a coaxial axial magnetic field and a coaxial auxiliary anode inside the metal pipe, the electric field, magnetic field and airflow field are controlled, which solves the problem of uneven thickness of DLC coating on the inner wall of the metal pipe and achieves efficient and uniform deposition, which is suitable for multiple industrial fields.
Patent Information
- Application Number
- CN202610834212.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-10
- Publication Date
- 2026-07-10
AI Technical Summary
Existing DLC coating deposition technology suffers from uneven thickness and low deposition efficiency on the inner wall of metal pipes, especially in small-diameter components where it is difficult to achieve efficient preparation of uniform coatings.
An apparatus is used, comprising a vacuum chamber, an electric field generating component, and a magnetic field generating component. By setting a coaxial axial magnetic field and a coaxial auxiliary anode inside a metal tube, and combining an integrated structure of "extension tube-metal tube to be coated-extension tube", the electric field, magnetic field, and airflow field are controlled to form a uniform electromagnetic environment, thereby achieving uniform deposition of the coating.
It achieves uniform deposition of DLC coating on the inner wall of metal pipes, improving the uniformity of coating thickness and deposition efficiency, and is applicable to fields such as petrochemicals, aerospace, energy transmission, marine engineering, precision machinery, medical devices and automobile manufacturing.
Smart Images

Figure CN122358150A_ABST
Abstract
Description
Technical Field
[0001] This invention relates in particular to an apparatus, method, and application for forming a uniform coating on the inner wall of a pipe fitting to be plated, belonging to the field of metal surface protection technology. Background Technology
[0002] Metal pipe fittings are widely used in critical fields such as petrochemicals, aerospace, energy transmission, marine engineering, precision machinery, medical devices, and automobile manufacturing. The surface properties of their inner walls directly determine their operating efficiency, service life, and safety. Because metal pipe fittings are subjected to complex conditions such as media erosion, chemical corrosion, and mechanical friction over long periods, they are prone to problems such as inner wall wear, corrosion perforation, and excessive frictional resistance, severely restricting the normal operation of equipment. Therefore, high-performance surface modification treatment of the inner walls of metal pipe fittings has become a key path to improve their core service performance and extend their service life.
[0003] Traditional metal pipe inner wall protection technologies have many insurmountable defects. Electroplating and chemical plating processes suffer from heavy metal pollution, thin coatings, poor adhesion, and easy peeling at high temperatures, while being subject to increasingly stringent environmental protection policies. Thermal spraying technology produces coatings with high porosity and insufficient corrosion resistance, and thick coatings are prone to cracking, making it difficult to meet the protection requirements of slender pipe inner walls. Organic coatings have shortcomings such as poor wear resistance and low temperature resistance, and are easily damaged under high-speed fluid erosion, failing to meet the requirements of extreme working conditions.
[0004] Diamond-like carbon (DLC) coatings possess high hardness, low coefficient of friction, excellent wear resistance, good chemical inertness, and biocompatibility, and have a low deposition temperature, making them suitable for most metal substrates. This has made them an ideal coating material for improving the service performance of metal pipe fittings. However, the narrow inner walls and complex structures of metal pipe fittings have long presented a significant technical challenge for achieving uniform deposition of DLC coatings, a problem that the industry urgently needs to solve.
[0005] Currently, mainstream DLC coating deposition technologies, including PVD (magnetron sputtering, cathode arc), microwave / RF PECVD, hollow cathode discharge (HC-PECVD), and ion beam / pulsed laser deposition, cannot meet the high uniformity and low cost requirements of industrial production of coatings for the inner walls of metal pipes. For example, conventional PVD technology is mature and produces dense coatings, but because the target material cannot penetrate deep into the pipe (especially small-diameter pipes), the energy and density of the plasma are prone to attenuation during transmission, resulting in poor uniformity of distribution on the inner wall of the pipe, uneven coating thickness, and problems such as difficulty in discharge and low deposition efficiency. Although microwave / RF PECVD technology is suitable for deposition on workpieces with complex morphology, this technology requires mechanical drive to move the plasma along the pipe axis, resulting in complex equipment structure, high purchase and maintenance costs, slow deposition speed, and the limited space inside the pipe also makes plasma confinement difficult, making it difficult to uniformly deposit coatings on the entire inner wall of the pipe. HC-PECVD technology offers advantages such as high plasma density and fast deposition rate. However, the plasma tends to concentrate in the pipe nozzle area, leading to overheating. Furthermore, uneven plasma distribution within the pipe makes it difficult to address the issue of thin coating thickness and poor quality in the middle of long-axis metal pipes. Ion beam / pulsed laser deposition technology can achieve high purity and high sp2. 3 While DLC coatings with a bond ratio can be applied, the ion beam penetration depth is limited, and structural limitations of some metal tubes make it difficult for the beam to fully cover the inner wall. In addition, the equipment for this technology is expensive and the deposition efficiency is extremely low, making it difficult to apply in large quantities to industrial applications.
[0006] Overall, existing DLC coating deposition technology is limited by the spatial geometry of the inner wall and the uneven distribution of multi-physical coupling fields. It is difficult to control the plasma discharge distribution and the edge effect of the tube opening is obvious. This directly restricts its uniform preparation and reliable protection of the inner wall of metal pipes, especially small-diameter parts (inner diameter ID≤40 mm). Summary of the Invention
[0007] To address the technical problem of uneven thickness of diamond-like carbon coating on the inner wall of metal pipe fittings in existing technologies, this invention provides an apparatus, method, and application for forming a uniform coating on the inner wall of the pipe fitting to be coated. By optimizing the apparatus structure, uniform coating deposition is achieved.
[0008] To achieve the aforementioned objectives, the technical solution adopted by this invention includes:
[0009] A first aspect of the present invention provides an apparatus for forming a uniform coating on the inner wall of a pipe fitting to be coated, comprising: a vacuum chamber, an electric field generating assembly, and a magnetic field generating assembly;
[0010] The vacuum chamber is at least used to provide the sealed environment required for depositing and forming a coating on the inner wall of the pipe to be coated;
[0011] The electric field generating assembly includes a pulse power supply, an auxiliary anode, and a first extension tube and a second extension tube. The first extension tube, the second extension tube, and the auxiliary anode are coaxially arranged in the vacuum chamber. The first extension tube and the second extension tube are spaced apart along the axial direction and are used to fix and connect to the conductive tube to be plated. The inner diameter of the first extension tube and the second extension tube is equal to that of the tube to be plated and both are conductive tubes. A portion of the auxiliary anode is located inside the first extension tube and the second extension tube. The negative terminal of the pulse power supply is used to electrically connect to the tube to be plated, and the positive terminal is used to electrically connect to the auxiliary anode.
[0012] During operation, the two ends of the tube to be plated are coaxially fixedly connected to the first extension tube and the second extension tube to form a tube to be plated-extension tube. The cavities of the first extension tube, the second extension tube, and the tube to be plated are seamlessly connected and communicated to form an integral cavity. The cavity wall of the integral cavity forms a continuous equipotential cathode surface. The electric field generating component generates an electric field in the tube to be plated-extension tube, and the direction of the electric field is consistent with the radial direction of the tube to be plated. The magnetic field generating component generates a magnetic field in the tube to be plated-extension tube, and the direction of the magnetic field is consistent with the axial direction of the tube to be plated.
[0013] This invention utilizes an integrated structure of "extension tube-coating tube-extension tube" to isolate physical interference (electric field edge effect, airflow inlet / outlet disturbance, magnetic field end effect) outside the target coating area (i.e. the tube wall of the coating tube). This creates a highly uniform and controllable electric field, magnetic field, and airflow environment within the coating tube. The synergistic effect of these three elements ultimately achieves a uniform distribution of plasma density, active particle flux, and ion bombardment energy on the inner wall surface of the coating tube, thus solving the technical challenge of uniform deposition of DLC coating on the inner wall of the metal tube.
[0014] A second aspect of the present invention provides a method for forming a uniform coating on the inner wall of a pipe fitting to be coated, comprising:
[0015] The apparatus is provided for forming a uniform coating on the inner wall of the pipe fitting to be plated;
[0016] The two ends of the tube to be plated are fixedly connected to the first extension tube and the second extension tube as a whole. A vacuum environment is formed in the vacuum chamber. A reaction gas is introduced into the vacuum chamber. The reaction gas enters the tube-extension tube formed by the tube to be plated, the first extension tube, and the second extension tube along the axial direction. An electric field is formed in the tube-extension tube by the electric field generating component, and a magnetic field is formed in the tube-extension tube by the magnetic field generating component, so as to form a uniform coating on the inner wall of the tube-extension tube.
[0017] A third aspect of the present invention provides the use of the apparatus or method for forming a uniform coating on the inner wall of a pipe fitting to be plated for the protection of the inner wall of metal pipe fittings in the fields of petrochemicals, aerospace, energy transmission, marine engineering, precision machinery, medical devices, and automobile manufacturing.
[0018] Compared with the prior art, the advantages of the present invention include:
[0019] This invention achieves uniform deposition of diamond-like carbon coating on the inner wall of the metal tube by setting a coaxial axial magnetic field outside the tube and a coaxial auxiliary anode inside the tube, combined with an integrated structure of "extension tube-metal fitting to be plated-extension tube", thereby regulating the electric field, magnetic field and airflow field inside the tube.
[0020] Specifically, regarding the electric field distribution, the "extension tube-to-plate tube-extension tube" structure creates a model of an approximately infinitely long coaxial cylindrical capacitor, which allows the electric field lines in the region of the to-plate tube to be approximately radially and uniformly distributed, thus solving the problem of uneven plasma density caused by the bending and concentration of electric field lines at the tube opening in traditional devices.
[0021] In this invention, the extension tube has the same inner diameter as the tube to be plated, is coaxially connected, and is made of conductive material. This makes the entire "tube to be plated - extension tube" system a continuous equipotential cathode surface, ensuring that the electric field boundary is smooth and symmetrical in the region of the tube to be plated. Specifically, regarding the magnetic field distribution, the "extension tube - tube to be plated - extension tube" structure is equivalent to extending the effective area for generating the magnetic field, which helps to form a more uniform axial magnetic field within the effective area of the tube to be plated. Regarding the airflow distribution, the extension tube serves as both the flow development section and the stabilization section, allowing the airflow to fully develop before entering the tube to be plated, forming a stable laminar flow or a uniform diffuse flow, thus avoiding airflow disturbance.
[0022] The device of this invention has a simple structure and strong adaptability. It does not require complex power supply regulation or additional auxiliary tooling and can significantly improve the uniformity of DLC coating thickness inside metal tubes. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of a device for forming a uniform coating on the inner wall of a pipe fitting to be plated, provided in a typical embodiment of the present invention.
[0024] Figure 2 These are cross-sectional topographic images of the DLC coating at different locations on the inner wall of the tube in Embodiment 1 of the present invention;
[0025] Figure 3 These are cross-sectional topographic images of the DLC coating at different locations on the inner wall of the tube in Embodiment 2 of the present invention;
[0026] Figure 4The images show cross-sectional morphology of the DLC coating at different locations on the inner wall of the tube in Comparative Example 1.
[0027] Figure 5 The images show cross-sectional morphology of the DLC coating at different locations on the inner wall of the tube in Comparative Example 2.
[0028] Figure 6 This is a graph showing the axial thickness distribution of the DLC coating on the inner wall of the pipe fitting in the embodiments and comparative examples of the present invention. Detailed Implementation
[0029] In view of the shortcomings of the prior art, the inventors of this case, through long-term research and extensive practice, have proposed the technical solution of this invention. To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0031] like Figure 1 As shown, in a typical embodiment, an apparatus for forming a uniform coating on the inner wall of a pipe to be plated includes a vacuum chamber 1, an electric field generating component, and a magnetic field generating component. The vacuum chamber 1 is used to provide at least a sealed environment required for depositing and forming a coating on the inner wall of the pipe to be plated. The electric field generating component is used to provide an electric field in the vacuum chamber 1 to ionize the reactive gas and form a plasma. The magnetic field generating component is used to generate a magnetic field in the vacuum chamber 1 to confine the plasma.
[0032] Specifically, vacuum chamber 1 is a sealed cavity structure capable of withstanding a negative pressure environment. It is equipped with necessary evacuation ports, inlet ports, and electrical connection ports to maintain the vacuum level and gas environment required for the deposition process. The shape of vacuum chamber 1 can be designed according to actual production needs, such as cylindrical or box-shaped.
[0033] Specifically, the electric field generating assembly includes a pulse power supply 6, an auxiliary anode 4, and a first extension tube 3-1 and a second extension tube 3-2. The first extension tube 3-1, the second extension tube 3-2, and the auxiliary anode 4 are coaxially fixed in the vacuum chamber 1. The first extension tube 3-1 and the second extension tube 3-2 are spaced apart along the axial direction and are used to fix and connect the conductive tube to be plated 2. The inner diameter of the first extension tube 3-1 and the second extension tube 3-2 is the same as that of the tube to be plated 2, and both are conductive tubes. Part of the auxiliary anode 4 is located inside the first extension tube 3-1 and the second extension tube 3-2, and the main body is located between the first extension tube 3-1 and the second extension tube 3-2. The negative terminal of the pulse power supply 6 is electrically connected to the tube to be plated 2, and the positive terminal is electrically connected to the auxiliary anode 4.
[0034] In a specific assembly configuration, the first extension tube 3-1 and the second extension tube 3-2 serve as carriers, fixed on opposite sides inside the vacuum chamber 1, with a pre-defined installation space between them for placing the tube to be plated 2. Both ends of the tube to be plated 2 are respectively connected and fixed to the first extension tube 3-1 and the second extension tube 3-2. Since the inner diameters of the first extension tube 3-1 and the second extension tube 3-2 are equal to those of the tube to be plated 2 and their materials are conductive, the connection points achieve communication between the cavities and conduction of potential. The auxiliary anode 4 is a slender rod-shaped structure that passes through the center of the first extension tube 3-1 and the second extension tube 3-2, suspended on the central axis of the overall cavity formed by the first extension tube 3-1, the tube to be plated 2, and the second extension tube 3-2 connected in series, and is grounded. The pulse power supply 6 provides the energy required for deposition; its negative terminal is connected to the tube assembly (i.e., the first extension tube 3-1, the second extension tube 3-2, and the tube to be plated 2) serving as the cathode, and its positive terminal is connected to the auxiliary anode 4, thereby establishing a radial electric field inside the cavity.
[0035] During operation, both ends of the tube to be plated 2 are coaxially fixedly connected to the first extension tube 3-1 and the second extension tube 3-2 respectively to form a tube-extension tube. The cavities of the first extension tube 3-1, the second extension tube 3-2, and the tube to be plated 2 are seamlessly connected and interconnected to form a single integral cavity. The cavity wall of the integral cavity forms a continuous equipotential cathode surface. An electric field generating component generates an electric field inside the tube-extension tube, with the direction of the electric field consistent with the radial direction of the tube to be plated 2. A magnetic field generating component generates a magnetic field inside the tube-extension tube, with the direction of the magnetic field consistent with the axial direction of the tube to be plated 2.
[0036] Specifically, the so-called "seamless connection" refers not only to the tight physical connection but also to the continuity of electrical performance. Since the first extension tube 3-1, the second extension tube 3-2, and the tube to be plated 2 have the same inner diameter and are electrically connected, the tube wall formed by the three is electrically equivalent to a continuous, integral cathode surface. This structure eliminates the electric field edge effect caused by geometric abrupt changes at the tube port in traditional processes. In traditional solutions, the electric field lines at the tube port bend and concentrate, resulting in abnormal plasma density and uneven coating thickness. However, this invention, by setting extension tubes, "pushes" this electric field distortion region to the port of the extension tubes, making the tube to be plated 2 in the middle section a "straight section" with a uniform electric field distribution.
[0037] The so-called "equipotential cathode surface" refers to the continuous and uniform potential distribution on the inner wall of the entire tube-extension tube to be coated, due to the conductive and tightly connected material. This ensures that the potential difference between the tube wall at any position and the central auxiliary anode 4 is basically the same in the axial direction, so that the radial electric field intensity remains uniform in the axial direction. This uniform electric field is the key basis for obtaining a uniform coating.
[0038] In this invention, the magnetic field direction is aligned with the axial direction of the tube to be plated 2, meaning the magnetic field lines are distributed along the central axis of the tube. This axial magnetic field can constrain the trajectory of electrons, lengthen their path within the tube, and increase the probability of collisions between electrons and gas molecules, thereby increasing plasma density and improving its uniformity. It should be understood that although a specific electromagnetic coil winding configuration is shown in the figures, any device capable of generating the aforementioned axial magnetic field falls within the scope of protection of this invention.
[0039] Through the above structure, this invention constructs an integrated deposition environment of "extension tube-plating tube-extension tube". The first extension tube 3-1 and the second extension tube 3-2 not only play a role in homogenizing the electric field, but also serve as the development and stabilization sections of the airflow field. The inlet airflow flows through the extension tube before entering the plating tube 2, which can eliminate turbulence at the inlet and form a stable laminar flow or uniform diffusion flow. Similarly, the extension tube at the outlet end avoids the air extraction port directly disturbing the outlet airflow of the plating tube 2. Therefore, the device of this invention, by synergistically controlling the electric field, magnetic field and airflow field, isolates various physical disturbances outside the plating area, providing the necessary hardware foundation for forming a uniform coating on the inner wall of the plating tube 2.
[0040] Specifically, the lengths of the first extension tube 3-1 and the second extension tube 3-2 are both 1 / 6 to 1 / 3 of the length of the tube to be plated 2. There is a critical range for the length of the extension tubes. When the ratio of the length of the first extension tube 3-1 or the second extension tube 3-2 to the length of the tube to be plated 2 is less than 1 / 6, the extension tube is too short and cannot effectively isolate the edge effect of the electric field at the tube opening and the airflow disturbance outside the effective area of the tube to be plated 2. This results in a significant decrease in the coating thickness at both ends of the tube to be plated 2, with limited improvement in uniformity. When the ratio of the length of the first extension tube 3-1 or the second extension tube 3-2 to the length of the tube to be plated 2 is greater than 1 / 3, although the edge effect can be further eliminated, it will significantly increase the overall volume of the device and the load on the vacuum system. Furthermore, an excessively long extension tube will lead to an increase in the internal pressure gradient, which may introduce new airflow inhomogeneities and increase material costs. Therefore, controlling the length ratio of the first extension tube 3-1, the second extension tube 3-2, and the tube to be plated 2 to be between 1 / 6 and 1 / 3 is the optimal balance between ensuring coating uniformity and controlling equipment cost and size. For example, the lengths of the first extension tube 3-1 and the second extension tube 3-2 are both L, where L satisfies: 50 mm ≤ L ≤ 100 mm.
[0041] Furthermore, the axial length of the auxiliary anode 4 is greater than the length of the tube to be plated 2; preferably, the axial length of the auxiliary anode 4 is greater than or equal to the sum of the lengths of the tube to be plated 2, the first extension tube 3-1, and the second extension tube 3-2. As the core component of the electric field, the length of the auxiliary anode 4 directly determines the uniformity of the electric field distribution along the axial direction. If the auxiliary anode 4 is shorter than the tube to be plated 2, the electric field lines will bend and diverge at both ends of the tube to be plated 2, failing to form an ideal radially uniform electric field, resulting in a decrease in plasma density at the ends. This invention, by setting the length of the auxiliary anode 4 to cover the entire tube-extension tube system, ensures that the electric field strength at any cross-sectional position is essentially consistent throughout the entire axial range of the tube to be plated 2, thus providing a fundamental guarantee for uniform ion deposition.
[0042] In terms of the specific structure of the magnetic field generating component, the magnetic field generating component includes an electromagnetic coil winding 5 and a DC power supply 7. The electromagnetic coil winding 5 is coaxially arranged with the first extension tube 3-1, the second extension tube 3-2, and the auxiliary anode 4. Preferably, the auxiliary anode 4, the electromagnetic coil winding 5, and the tube to be plated 2 are centrally symmetrically arranged. Specifically, after being energized, the electromagnetic coil winding 5 generates an axial magnetic field, which can constrain the trajectory of electrons and increase the probability of collisions between electrons and gas molecules, thereby increasing the plasma density. The coaxial and centrally symmetrical arrangement ensures the spatial symmetry of the magnetic field inside the tube, avoiding uneven plasma distribution caused by magnetic field bias. It should be understood that the number of turns and the current of the electromagnetic coil winding 5 can be adjusted according to the size of the tube to be plated 2 and the required plasma density, and the present invention does not impose strict limitations on this.
[0043] Furthermore, the electromagnetic coil winding 5 is wound outside the vacuum chamber 1. Preferably, the vacuum chamber 1, electromagnetic coil winding 5, auxiliary anode 4, first extension tube 3-1, and second extension tube 3-2 are coaxially arranged. Preferably, the vacuum chamber 1 has a cylindrical structure. Placing the electromagnetic coil winding 5 outside the vacuum chamber 1 not only facilitates installation and maintenance but also avoids the problem of coil outgassing in a vacuum environment, ensuring the cleanliness of the deposition environment. The cylindrical vacuum chamber 1 and the internal tubing are coaxially arranged, which is beneficial for forming a uniform circumferentially symmetrical magnetic field environment.
[0044] Regarding the airflow distribution, vacuum chamber 1 is equipped with an air inlet and an air outlet. The air inlet is located at one end of the vacuum chamber and is coaxial with vacuum chamber 1. The air outlet is located at the other end of the vacuum chamber 1, and its axial direction is parallel to the radial direction of vacuum chamber 1. This coaxial air inlet and radial air outlet layout design allows the gas to form a stable linear flow path within the device, guiding the airflow to flow in along the axial direction of the pipe and smoothly turn and flow out after passing through the pipe to be coated 2. Through the above-mentioned refined design of the electric field, magnetic field, and airflow field structure, this invention further improves the process stability of the device under complex working conditions and ensures high uniformity of coating deposition.
[0045] In a typical implementation, a method for forming a uniform coating on the inner wall of a pipe fitting is provided. This method is based on the apparatus described above and deposits a diamond-like carbon coating of uniform thickness on the inner wall of the pipe fitting by constructing a specific electromagnetic field environment and airflow field environment.
[0046] Specifically, the method includes the following steps:
[0047] Step S100: Provide an apparatus for forming a uniform coating on the inner wall of the pipe fitting to be coated. The specific structure of this apparatus is as described above (see reference). Figure 1 This includes key components such as a vacuum chamber, an electric field generating assembly, and a magnetic field generating assembly. When performing this step, it is essential to ensure that all components of the device are clean, reliably connected, and that the electrical connections of the electromagnetic coil windings are stable.
[0048] In step S200, the two ends of the tube to be plated 2 are fixedly connected to the first extension tube 3-1 and the second extension tube 3-2 to form a vacuum environment in the vacuum chamber 1.
[0049] This step is crucial for constructing the "equipotential cathode surface." During operation, the cleaned tube to be plated (2) must be coaxially placed between the first extension tube 3-1 and the second extension tube 3-2. For example, a conductive connector (such as a flange, clamp, or welding) can be used to achieve physical connection and electrical conductivity. After docking, the tube to be plated and the extension tubes form a continuous conductive cavity, i.e., the aforementioned "tube to be plated - extension tube." Then, the vacuum system is activated to evacuate the vacuum chamber to a preset value (e.g., 3 × 10⁻⁶). -3 (below Pa) to eliminate interference from environmental impurity gases on the deposition process.
[0050] In step S300, a reaction gas is introduced into the vacuum chamber, and an electric field is generated in the tube-to-extension tube formed by the tube to be plated and the first extension tube and the second extension tube using an electric field generating component. A magnetic field is generated in the tube-to-extension tube using a magnetic field generating component, and a uniform coating is formed on the inner wall of the tube-to-extension tube.
[0051] Specifically, after reaching the required vacuum level, the necessary reaction gases are introduced into the vacuum chamber through the gas inlet system. The type of reaction gas is selected based on the composition of the target coating. For example, to deposit a pure DLC coating, a mixture of acetylene (C2H2) and argon (Ar) can be introduced; to deposit a silicon-containing transition layer, an organosilicon source such as hexamethyldisiloxane (HMDSO) is required. The gas flow rate is precisely controlled by a mass flow meter to maintain the stable working pressure required for the deposition process.
[0052] Specifically, the electric field is established by applying voltage through a pulsed power supply. The negative terminal of the pulsed power supply is connected to a cathode system consisting of an extension tube and the tube to be plated, while the positive terminal is connected to an auxiliary anode inside the tube. Under the action of the high-voltage electric field, the reactant gas is ionized to form plasma. Due to the integrated structure of "extension tube-tube to be plated-extension tube", a continuous equipotential surface is formed on the inner wall of the tube cavity, resulting in an ideal radial distribution of electric field lines in the region of the tube to be plated, with consistent axial intensity, thus avoiding uneven plasma density caused by electric field distortion at the port.
[0053] Simultaneously, a magnetic field generating component (such as an electromagnetic coil winding) generates an axial magnetic field within the cavity. This magnetic field is orthogonal to the radial electric field, forming an electromagnetic confinement. Electrons, under the influence of the axial magnetic field, experience a Lorentz force, confining their trajectories to helical motion within the cavity, significantly extending their path and increasing the probability of collisions with gas molecules. This electromagnetic synergistic effect not only enhances the ionization rate and density of the plasma, but more importantly, the high uniformity of the magnetic and electric fields within the coating region results in excellent axial uniformity of the plasma distribution, providing a material basis for uniform coating deposition.
[0054] Under the aforementioned uniform electromagnetic field environment, active particles in the plasma migrate and deposit towards the tube wall under the influence of the electric field. Because the tube to be coated is located in a "straight section" with a uniform electric field, and the airflow is smoothly rectified by the extension tube, the coating grows on the inner wall of the tube at a uniform rate. During the deposition process, power supply parameters (such as voltage, pulse width, and frequency) and magnetic field parameters (such as coil current) can be adjusted according to the coating design requirements to control the coating growth rate, structure, and internal stress. After deposition, the tube can be removed after cooling to room temperature, resulting in a metal tube product with excellent uniformity of inner wall coating thickness.
[0055] It should be understood that in the specific implementation process, gas can be introduced first and then an electromagnetic field can be established, or a magnetic field can be established first and then gas can be introduced, or both can be carried out simultaneously, as long as a stable plasma environment can be ensured before the deposition begins.
[0056] Specifically, the coating may include a first coating and a second coating stacked sequentially. Typically, the first coating is preferably a Si / O-DLC transition layer, and the second coating is preferably a DLC coating.
[0057] The coating formation process includes:
[0058] A first reaction gas, formed by a mixture of hexamethyldisiloxane (HMDSO) and acetylene (C2H2), is introduced into the vacuum chamber to maintain the pressure in the vacuum chamber at 0.4 Pa to 3.0 Pa. The current of the DC power supply providing the magnetic field is set to 1 A to 4 A to form a magnetic field with a strength of 3 Gs to 12 Gs in the vacuum chamber 1. The voltage of the pulse power supply providing the electric field is set to 400 V to 1000 V, the pulse width is set to 10 μs to 100 μs, the frequency is set to 500 Hz to 2000 Hz, and the deposition time is set to 1 min to 5 min to deposit a Si / O-DLC transition layer on the inner wall of the tube to be coated - extension tube.
[0059] Subsequently, the first reactive gas supply was stopped, and the DLC coating was deposited. A second reactive gas, a mixture of argon and acetylene, was introduced into the vacuum chamber to maintain the pressure inside the vacuum chamber at 0.4 Pa to 3.0 Pa. The current of the DC power supply providing the magnetic field was set to 1 A to 4 A to form a magnetic field with a strength of 3 Gs to 12 Gs inside the vacuum chamber 1. The voltage of the pulsed power supply providing the electric field was set to 400 V to 1000 V, the pulse width to 10 μs to 100 μs, the frequency to 500 Hz to 2000 Hz, and the deposition time to 30 min to 120 min, so as to deposit a DLC coating on the surface of the Si / O-DLC transition layer.
[0060] It should be noted that the external magnetic field plays a crucial role in the ignition stage of plasma discharge inside the tube. When the system is not equipped with an external magnetic field, a high voltage of thousands of volts is usually required to break through the gas ionization threshold and trigger plasma discharge. However, after introducing an external magnetic field, the movement path of charged particles is constrained, the probability of ionization collision is significantly increased, and only a few hundred volts are needed to successfully ignite the plasma inside the tube.
[0061] To obtain the high-quality coating structure described above, the present invention may further include a plasma etching step on the tube to be plated before deposition, that is, plasma etching is performed on the tube to be plated first, and then the aforementioned coating is formed on the inner wall of the tube to be plated.
[0062] Plasma etching is a key pretreatment process for improving coating adhesion. The specific procedure involves first adjusting the gas pressure inside the vacuum chamber to 3 × 10⁻⁶. -3 Below Pa, an inert gas (such as argon, Ar) is introduced into the vacuum chamber to maintain the pressure within the chamber at 1.0 Pa to 5.0 Pa. Subsequently, the electric field generating component and the magnetic field generating component are activated to create an electromagnetic field within the tube-extension tube to be coated, performing plasma etching on the inner wall of the tube-extension tube. During this process, high-energy argon ions bombard the inner wall of the tube under the acceleration of the electric field, effectively removing the oxide layer, adsorbed gases, and microscopic contaminants from the substrate surface, resulting in a fresh and active substrate surface. Simultaneously, ion bombardment also produces a micro-nano scale roughening effect on the substrate surface, increasing the mechanical bonding force between the coating and the substrate. Preferably, during plasma etching, the voltage of the pulse power supply providing the electric field is set to 400 V to 1000 V, the pulse width to 10 μs to 100 μs, and the frequency to 500 Hz to 2000 Hz; the current of the DC power supply providing the magnetic field is set to 1 A to 4 A; and the plasma etching cleaning time can be 10 min to 30 min. This parameter range ensures sufficient etching intensity while avoiding overheating or damage to the substrate due to excessive voltage.
[0063] To verify the technical effectiveness of the device and method of this invention in improving the uniformity of coating on the inner wall of pipe fittings, multiple sets of comparative experiments were conducted. The experimental subjects were all 316L stainless steel pipe fittings to be coated, with an inner diameter of 40 mm and a length of 300 mm; only the structural configuration of the device was changed.
[0064] Example 1.
[0065] Using the apparatus described above in this invention (such as...) Figure 1 As shown), the length L of the first extension tube and the second extension tube are both 100 mm. The material is the same as the tube to be plated (316L stainless steel), and the inner diameter is the same as the tube to be plated (inner diameter 40 mm), i.e., conductive extension tubes.
[0066] The steps for preparing a DLC coating on the inner wall of the pipe fitting to be coated include:
[0067] 1) Pretreatment. The tube to be plated 2, the first extension tube 3-1, the second extension tube 3-2, and the auxiliary anode 4 (made of titanium rod, with an outer diameter of 5 mm and a length of 520 mm) are placed in acetone and anhydrous ethanol for ultrasonic cleaning for 20 min in sequence, and then dried and installed in vacuum chamber 1.
[0068] 2) Evacuate the vacuum chamber. Reduce the pressure in vacuum chamber 1 to 3 × 10⁻⁶. -3 Below Pa.
[0069] 3) Plasma etching. High-purity Ar at 50 sccm is introduced into vacuum chamber 1, and the pressure is maintained at 4.0 Pa. At the same time, pulse power supply 6 and DC power supply 7 are turned on to perform plasma etching cleaning on the inner wall of the tube to be coated-extended tube for 30 min. The voltage of pulse power supply 6 is 600 V, the pulse width is 10 μs, and the frequency is 1000 Hz. The current of DC power supply 7 is 1 A.
[0070] 4) Deposition to form a Si / O-DLC transition layer. Turn off the Ar source and introduce HMDSO and C2H2 into vacuum chamber 1 at flow rates of 10 sccm and 20 sccm, respectively, to maintain the gas pressure in vacuum chamber 1 at 4.0 Pa. Keep the current of DC power supply 7 at 1 A and adjust the voltage, pulse width, and frequency of pulse power supply 6 to 550 V, 10 μs, and 1000 Hz, respectively, and maintain for 5 min to form a Si / O-DLC transition layer on the inner wall of the tube to be coated - extension tube.
[0071] 5) Deposition to form a DLC coating. Turn off the HMDSO source and introduce Ar and C2H2 into vacuum chamber 1. The flow rates of Ar and C2H2 are 5 sccm and 20 sccm, respectively, to maintain the pressure of vacuum chamber 1 at 5 Pa. Keep the current of DC power supply 7 at 1 A. Adjust the voltage, pulse width, and frequency of pulse power supply 6 to 600 V, 10 μs, and 1000 Hz, respectively. The deposition time is 100 min to form a DLC coating on the surface of the Si / O-DLC transition layer.
[0072] 6) Cooling down. Cool to room temperature under vacuum.
[0073] After removing the tube 2 to be plated, the cross-sectional morphology of the DLC coating at different locations inside the tube is observed using a scanning electron microscope and the coating thickness is measured; the uniformity of the DLC coating thickness in the same direction inside the tube is calculated using formula 1).
[0074] 1)
[0075] In the formula: dmax d represents the maximum thickness of the DLC coating in the same direction inside the pipe; min This represents the minimum thickness of the DLC coating in the same direction within the pipe; d average This represents the average thickness of the DLC coating in the same direction inside the pipe.
[0076] Figure 2 The figures show the cross-sectional morphology of the DLC coating formed at different locations (axially spaced 50 mm) on the inner wall of the pipe in this embodiment. Calculations show that the axial thickness uniformity of the DLC coating prepared on the inner wall of the pipe to be coated is 88.68%.
[0077] Example 2.
[0078] Using the apparatus described above in this invention (such as...) Figure 1 As shown), the length L of both the first and second extension tubes is 50 mm, the material is the same as the tube to be plated (316L stainless steel), and the inner diameter is the same as the tube to be plated (inner diameter 40 mm), i.e., conductive extension tubes.
[0079] The steps for preparing a DLC coating on the inner wall of the pipe fitting to be coated include:
[0080] 1) Pretreatment. The tube to be plated 2, the first extension tube 3-1, the second extension tube 3-2, and the auxiliary anode 4 (made of titanium rod, with an outer diameter of 5 mm and a length of 420 mm) are placed in acetone and anhydrous ethanol for ultrasonic cleaning for 20 min in sequence, and then dried and installed in vacuum chamber 1.
[0081] 2) Evacuate the vacuum chamber. Reduce the pressure in vacuum chamber 1 to 3 × 10⁻⁶. -3 Below Pa.
[0082] 3) Plasma etching. High-purity Ar at 50 sccm is introduced into vacuum chamber 1, and the pressure is maintained at 4.0 Pa. At the same time, pulse power supply 6 and DC power supply 7 are turned on to perform plasma etching cleaning on the inner wall of the tube to be coated-extended tube for 30 min. The voltage of pulse power supply 6 is 600 V, the pulse width is 10 μs, and the frequency is 1000 Hz. The current of DC power supply 7 is 1 A.
[0083] 4) Deposition to form a Si / O-DLC transition layer. Turn off the Ar source and introduce HMDSO and C2H2 into vacuum chamber 1 at flow rates of 10 sccm and 20 sccm, respectively, to maintain the gas pressure in vacuum chamber 1 at 4.0 Pa. Keep the current of DC power supply 7 at 1 A and adjust the voltage, pulse width, and frequency of pulse power supply 6 to 550 V, 10 μs, and 1000 Hz, respectively, and maintain for 5 min to form a Si / O-DLC transition layer on the inner wall of the tube to be coated - extension tube.
[0084] 5) Deposition to form a DLC coating. Turn off the HMDSO source and introduce Ar and C2H2 into vacuum chamber 1. The flow rates of Ar and C2H2 are 5 sccm and 20 sccm, respectively, to maintain the pressure of vacuum chamber 1 at 5 Pa. Keep the current of DC power supply 7 at 1 A. Adjust the voltage, pulse width, and frequency of pulse power supply 6 to 600 V, 10 μs, and 1000 Hz, respectively. The deposition time is 100 min to form a DLC coating on the surface of the Si / O-DLC transition layer.
[0085] 6) Cooling down. Cool to room temperature under vacuum.
[0086] Figure 3 The figures show the cross-sectional morphology of the DLC coating formed at different locations (50 mm axial interval) on the inner wall of the pipe in this embodiment. Calculations show that the axial thickness uniformity of the DLC coating prepared on the inner wall of the pipe to be coated is 69.51%.
[0087] Comparative Example 1.
[0088] The apparatus used in Comparative Example 1 is basically the same as that in Example 1, except that: the apparatus in Comparative Example 1 does not have an extension tube, and the tube to be plated is placed directly in the vacuum chamber for deposition, with the auxiliary anode length covering the tube to be plated.
[0089] The steps for preparing a DLC coating on the inner wall of the pipe fitting to be coated include:
[0090] 1) Pretreatment. The tube to be plated 2 and the auxiliary anode 4 (made of titanium rod, with an outer diameter of 5 mm and a length of 320 mm) are placed in acetone and anhydrous ethanol for ultrasonic cleaning for 20 min in sequence, and then dried and installed in vacuum chamber 1.
[0091] 2) Evacuate the vacuum chamber. Reduce the pressure in vacuum chamber 1 to 3 × 10⁻⁶. -3 Below Pa.
[0092] 3) Plasma etching. High-purity Ar at 50 sccm is introduced into vacuum chamber 1, and the pressure is maintained at 4.0 Pa. At the same time, pulse power supply 6 and DC power supply 7 are turned on to perform plasma etching cleaning on the inner wall of the tube to be plated for 30 min. The voltage of pulse power supply 6 is 600 V, the pulse width is 10 μs, and the frequency is 1000 Hz. The current of DC power supply 7 is 1 A.
[0093] 4) Deposition to form a Si / O-DLC transition layer. Turn off the Ar source and introduce HMDSO and C2H2 into vacuum chamber 1. The flow rates of HMDSO and C2H2 are 10 sccm and 20 sccm, respectively, to maintain the gas pressure in vacuum chamber 1 at 4.0 Pa. Keep the current of DC power supply 7 at 1 A, and adjust the voltage, pulse width, and frequency of pulse power supply 6 to 550 V, 10 μs, and 1000 Hz, respectively, and maintain for 5 min to form a Si / O-DLC transition layer on the inner wall of the tube to be plated 2.
[0094] 5) Deposition to form a DLC coating. Turn off the HMDSO source and introduce Ar and C2H2 into vacuum chamber 1. The flow rates of Ar and C2H2 are 5 sccm and 20 sccm, respectively, to maintain the pressure of vacuum chamber 1 at 5 Pa. Keep the current of DC power supply 7 at 1 A. Adjust the voltage, pulse width, and frequency of pulse power supply 6 to 600 V, 10 μs, and 1000 Hz, respectively. The deposition time is 100 min to form a DLC coating on the surface of the Si / O-DLC transition layer.
[0095] 6) Cooling down. Cool to room temperature under vacuum.
[0096] Figure 4 The cross-sectional morphology of the DLC coating formed at different locations (axially spaced 50 mm) on the inner wall of the pipe in Comparative Example 1 is shown. Calculations show that the axial thickness uniformity of the DLC coating prepared on the inner wall of the pipe to be coated is 38.73%.
[0097] Comparative Example 2.
[0098] The apparatus used in Comparative Example 2 is basically the same as that in Example 1, except that the length L of the first extension tube and the second extension tube in Comparative Example 2 is 50 mm, the material is different from that of the tube to be plated (quartz), and the inner diameter is the same as that of the tube to be plated (inner diameter 40 mm), that is, the insulating extension tube.
[0099] The steps for preparing a DLC coating on the inner wall of the pipe fitting to be coated include:
[0100] 1) Pretreatment. The tube to be plated 2, the first extension tube 3-1, the second extension tube 3-2, and the auxiliary anode 4 (made of titanium rod, with an outer diameter of 5 mm and a length of 420 mm) are placed in acetone and anhydrous ethanol for ultrasonic cleaning for 20 min in sequence, and then dried and installed in vacuum chamber 1.
[0101] 2) Evacuate the vacuum chamber. Reduce the pressure in vacuum chamber 1 to 3 × 10⁻⁶. -3 Below Pa.
[0102] 3) Plasma etching. High-purity Ar at 50 sccm is introduced into vacuum chamber 1, and the pressure is maintained at 4.0 Pa. At the same time, pulse power supply 6 and DC power supply 7 are turned on to perform plasma etching cleaning on the inner wall of the tube to be coated-extended tube for 30 min. The voltage of pulse power supply 6 is 600 V, the pulse width is 10 μs, and the frequency is 1000 Hz. The current of DC power supply 7 is 1 A.
[0103] 4) Deposition to form a Si / O-DLC transition layer. Turn off the Ar source and introduce HMDSO and C2H2 into vacuum chamber 1 at flow rates of 10 sccm and 20 sccm, respectively, to maintain the gas pressure in vacuum chamber 1 at 4.0 Pa. Keep the current of DC power supply 7 at 1 A and adjust the voltage, pulse width, and frequency of pulse power supply 6 to 550 V, 10 μs, and 1000 Hz, respectively, and maintain for 5 min to form a Si / O-DLC transition layer on the inner wall of the tube to be coated - extension tube.
[0104] 5) Deposition to form a DLC coating. Turn off the HMDSO source and introduce Ar and C2H2 into vacuum chamber 1. The flow rates of Ar and C2H2 are 5 sccm and 20 sccm, respectively, to maintain the pressure of vacuum chamber 1 at 5 Pa. Keep the current of DC power supply 7 at 1 A. Adjust the voltage, pulse width, and frequency of pulse power supply 6 to 600 V, 10 μs, and 1000 Hz, respectively. The deposition time is 100 min to form a DLC coating on the surface of the Si / O-DLC transition layer.
[0105] 6) Cooling down. Cool to room temperature under vacuum.
[0106] Figure 5 The cross-sectional morphology of the DLC coating formed at different locations (axially spaced 50 mm) on the inner wall of the pipe in Comparative Example 2 is shown. Calculations show that the axial thickness uniformity of the DLC coating prepared on the inner wall of the pipe to be coated is 33.95%.
[0107] Specifically, Figure 2 The cross-sectional morphology of the DLC coating prepared at different locations on the inner wall of the tube in Example 1 is shown, and it can be seen that the coating thickness distribution is relatively uniform. Figure 3 The cross-sectional morphology of Example 2 is shown, and the thickness fluctuation is slightly increased compared to Example 1. Figure 4 and Figure 5 The cross-sectional morphology of Comparative Example 1 and Comparative Example 2 are shown respectively, and obvious thickness unevenness can be seen.
[0108] The specific axial thickness distribution curves of the coatings in Examples 1, 2, 1, and 2 are as follows: Figure 6As shown in the figure. Comparing the data of Examples 1 and 2 with Comparative Example 1, it can be seen that the coating uniformity is significantly improved after adding the extension tube. In Comparative Example 1, due to the lack of an extension tube, the port of the tube to be coated is directly exposed to the vacuum chamber environment, resulting in bending and concentration of electric field lines at the port, producing a severe "edge effect". This electric field distortion directly leads to abnormal plasma density near the port, and the coating thickness fluctuates drastically. However, Examples 1 and 2, by setting the extension tube, "push" this edge effect to the port area of the extension tube, making the tube to be coated in a "straight section" with a uniform electric field, thereby greatly improving the coating uniformity. At the same time, comparing the data of Examples 1 and 2, it can be seen that the extension tube length L has a significant impact on uniformity, and the uniformity when L=100 mm is better than that when L=50 mm, verifying the rationality of the extension tube length parameter design in this invention.
[0109] Comparing the data from Example 2 and Comparative Example 2, it can be seen that although both examples incorporate an extension tube, the uniformity of Example 2 (69.51%) is significantly higher than that of Comparative Example 2 (33.95%). This result strongly demonstrates the necessity of the "conductive extension tube" feature. In Comparative Example 2, although the quartz extension tube physically extends the conduit, its insulating properties prevent it from forming a continuous conductive surface with the tube to be coated. During deposition, the quartz tube segment remains suspended, disrupting the equipotential cathode surface conditions within the tube cavity, leading to a distorted electric field distribution and failing to regulate the electric field. In contrast, in Example 2, the conductive extension tube seamlessly connects to the tube to be coated, forming a continuous equipotential cathode surface, ensuring a uniform axial distribution of the electric field strength, thereby achieving highly uniform coating deposition.
[0110] In summary, this invention, through an integrated conductive structure of "extension tube - tube to be coated - extension tube", successfully constructs a uniform electromagnetic field environment, effectively eliminates edge effects, and significantly improves the thickness uniformity of the coating on the inner wall of the tube.
[0111] In existing DLC coating preparation technologies for the inner walls of metal pipes, limitations caused by pipe edge effects, plasma density, electric field distribution, and turbulent airflow result in significant differences in coating thickness and poor uniformity. This invention utilizes an external coaxial electromagnetic coil winding, an internal auxiliary anode, and an integrated "extension tube-plate-extension tube" structure. The conductive extension tube isolates physical interferences (electric field edge effects, airflow inlet / outlet disturbances, and magnetic field end effects) outside the plated area, creating a highly uniform and controllable electric, magnetic, and airflow environment within the main body of the plated pipe. The synergistic effect of these three elements ultimately achieves a uniform distribution of plasma density, active particle flux, and ion bombardment energy on the inner wall surface of the plated pipe, thus solving the technical challenge of uniform DLC coating deposition on the inner walls of metal pipes.
[0112] Regarding the electric field distribution, the "extended tube-coated tube-extended tube" structure creates a model of an approximately infinitely long coaxial cylindrical capacitor. In this model, the region to be coated is located in the middle section of the "infinitely long" structure formed by the two extended tubes. This allows the electric field lines in the region to be approximately radially and uniformly distributed, with the electric field intensity E mainly along the radial direction and equal in magnitude on the same cross-section. This solves the problem of uneven plasma density caused by the bending and concentration of electric field lines at the tube opening (edge effect) in traditional devices.
[0113] In this invention, the extension tube has the same inner diameter as the tube to be plated, is coaxially connected, and is made of conductive material (such as stainless steel), making the entire "tube to be plated-extension tube" system a continuous equipotential cathode surface. This ensures that the electric field boundary in the region of the tube to be plated is smooth and symmetrical, without electric field distortion caused by geometric abrupt changes or material discontinuities.
[0114] Specifically, regarding the magnetic field distribution, the "extension tube-plate-extension tube" structure effectively extends the effective area for generating the magnetic field. The presence of the extension tube improves the magnetic field boundary conditions in the plate-plate region. More importantly, the extension tube (conductive) acts as a boundary for the magnetic field, helping to form a more uniform axial magnetic field within the effective area of the plate-plate. For the airflow distribution, the extension tube serves as both the flow development and stabilization section. The inlet extension tube allows any turbulent or non-uniform incoming flow that may exist at the vacuum chamber inlet to fully develop before entering the plate-plate, forming a stable laminar or uniform diffused flow. The outlet extension tube avoids the pumping disturbance and backflow caused by the plate-plate outlet directly connecting to the vacuum chamber evacuation port, ensuring a smooth flow of air through the plate-plate region.
[0115] The device of this invention has a simple structure and strong adaptability, requiring no complex power supply regulation or additional auxiliary tooling, and can significantly improve the uniformity of DLC coating thickness inside metal pipes. The core components of the device are all conventional and readily available structural parts, which are easy to assemble and can be directly adapted to metal pipes of different lengths and diameters. Precise adaptation can be achieved by adjusting the specifications of the extension tube.
[0116] It should be understood that the above embodiments are merely illustrative of the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
Claims
1. An apparatus for forming a uniform coating on the inner wall of a pipe fitting to be plated, characterized in that, include: Vacuum chamber (1), electric field generating component and magnetic field generating component; The vacuum chamber (1) is used to provide at least the sealed environment required for depositing and forming a coating on the inner wall of the pipe fitting (2) to be coated; The electric field generating component includes a pulse power supply (6), an auxiliary anode (4), a first extension tube (3-1), and a second extension tube (3-2). The first extension tube (3-1), the second extension tube (3-2), and the auxiliary anode (4) are coaxially arranged in the vacuum chamber (1). The first extension tube (3-1) and the second extension tube (3-2) are spaced apart along the axial direction and are used to fix and connect the conductive tube to be plated (2). The inner diameter of the first extension tube (3-1) and the second extension tube (3-2) is equal to that of the tube to be plated (2) and both are conductive tubes. Part of the auxiliary anode (4) is located inside the first extension tube (3-1) and the second extension tube (3-2). The negative terminal of the pulse power supply (6) is used to electrically connect with the tube to be plated (2), and the positive terminal is used to electrically connect with the auxiliary anode (4). During operation, the two ends of the tube to be plated (2) are coaxially fixedly connected with the first extension tube (3-1) and the second extension tube (3-2) to form a tube to be plated-extension tube. The tube cavities of the first extension tube (3-1), the second extension tube (3-2) and the tube to be plated (2) are seamlessly connected and connected to form an integral tube cavity. The cavity wall of the integral tube cavity forms a continuous equipotential cathode surface. The electric field generating component generates an electric field in the tube to be plated-extension tube, and the direction of the electric field is consistent with the radial direction of the tube to be plated (2). The magnetic field generating component generates a magnetic field in the tube to be plated-extension tube, and the direction of the magnetic field is consistent with the axial direction of the tube to be plated (2).
2. The apparatus for forming a uniform coating on the inner wall of a pipe fitting according to claim 1, characterized in that: The lengths of the first extension tube (3-1) and the second extension tube (3-2) are both 1 / 6 to 1 / 3 of the length of the tube to be plated (2).
3. The apparatus for forming a uniform coating on the inner wall of a pipe fitting according to claim 1 or 2, characterized in that: The axial length of the auxiliary anode (4) is greater than the length of the pipe fitting (2) to be plated; Alternatively, the axial length of the auxiliary anode (4) is greater than the sum of the lengths of the tube to be plated (2), the first extension tube (3-1), and the second extension tube (3-2).
4. The apparatus for forming a uniform coating on the inner wall of a pipe fitting according to claim 1, characterized in that: The magnetic field generating component includes an electromagnetic coil winding (5) and a DC power supply (7). The electromagnetic coil winding (5) is coaxially arranged with the first extension tube (3-1), the second extension tube (3-2), and the auxiliary anode (4). And / or, the auxiliary anode (4), the electromagnetic coil winding (5), and the tube to be plated (2) are arranged in a centrally symmetrical configuration.
5. The apparatus for forming a uniform coating on the inner wall of a pipe fitting according to claim 4, characterized in that: The electromagnetic coil winding (5) is wound around the outside of the vacuum chamber (1); And / or, the vacuum chamber (1), the electromagnetic coil winding (5), the auxiliary anode (4), the first extension tube (3-1), and the second extension tube (3-2) are coaxially arranged; And / or, the vacuum chamber (1) is a cylindrical structure; And / or, the vacuum chamber (1) is provided with an air inlet and an air outlet. The air inlet is located at one end of the vacuum chamber and is coaxial with the vacuum chamber (1). The air outlet is located at the other end of the vacuum chamber (1) and the axial direction of the air outlet is parallel to the radial direction of the vacuum chamber (1).
6. A method for forming a uniform coating on the inner wall of a pipe fitting to be plated, characterized in that, include: Provide an apparatus for forming a uniform coating on the inner wall of a pipe fitting as described in any one of claims 1-5; The two ends of the tube to be plated (2) are fixedly connected to the first extension tube (3-1) and the second extension tube (3-2) to form a vacuum environment in the vacuum chamber (1). The reaction gas is introduced into the vacuum chamber (1). The reaction gas enters the tube to be plated-extension tube formed by the tube to be plated (2), the first extension tube (3-1), and the second extension tube (3-2) along the axial direction. The electric field generating component forms an electric field in the tube to be plated-extension tube, and the magnetic field generating component forms a magnetic field in the tube to be plated-extension tube, so as to form a uniform coating on the inner wall of the tube to be plated-extension tube.
7. The method for forming a uniform coating on the inner wall of a pipe fitting according to claim 6, characterized in that, The coating comprises a first coating and a second coating stacked sequentially.
8. The method for forming a uniform coating on the inner wall of a pipe fitting according to claim 7, characterized in that, The first coating is a Si / O-DLC transition layer, the second coating is a DLC coating, and the method includes: A first reaction gas formed by a mixture of hexamethyldisiloxane and acetylene is introduced into the vacuum chamber (1) to maintain the gas pressure in the vacuum chamber (1) at 0.4 Pa to 3.0 Pa. The current of the DC power supply (7) providing the magnetic field is set to 1 A to 4 A to form a magnetic field with a magnetic field strength of 3 Gs to 12 Gs in the vacuum chamber (1). The voltage of the pulse power supply (6) providing the electric field is set to 400 V to 1000 V, the pulse width is set to 10 μs to 100 μs, and the frequency is set to 500 Hz to 2000 Hz to deposit a Si / O-DLC transition layer on the inner wall of the tube to be plated-extended tube. Stop the first reaction gas and introduce a second reaction gas formed by a mixture of argon and acetylene into the vacuum chamber (1) to maintain the gas pressure in the vacuum chamber (1) at 0.4 Pa to 3.0 Pa. Set the current of the DC power supply (7) that provides the magnetic field to 1 A to 4 A to form a magnetic field with a magnetic field strength of 3 Gs to 12 Gs in the vacuum chamber (1). Set the voltage of the pulse power supply (6) that provides the electric field to 400 V to 1000 V, the pulse width to 10 μs to 100 μs, and the frequency to 500 Hz to 2000 Hz to deposit a DLC coating on the surface of the Si / O-DLC transition layer.
9. The method for forming a uniform coating on the inner wall of a pipe fitting according to claim 6 or 7, characterized in that: First, plasma etching is performed on the tube to be plated (2), and then a coating is formed on the inner wall of the tube to be plated (2); Among them, the plasma etching method for the tube to be plated (2) includes: First, adjust the air pressure in the vacuum chamber (1) to 3×10. -3 Below Pa, inert gas is introduced into the vacuum chamber (1) to maintain the gas pressure in the vacuum chamber (1) at 1.0 Pa to 5.0 Pa. The electric field generating component forms an electric field in the tube to be plated-extended tube, and the magnetic field generating component forms a magnetic field in the tube to be plated-extended tube, so as to perform plasma etching on the inner wall of the tube to be plated-extended tube. Furthermore, when performing plasma etching on the tube to be plated-extended tube, the voltage of the pulse power supply (6) providing the electric field is set to 400 V~1000 V, the pulse width is set to 10 μs~100 μs, the frequency is set to 500 Hz~2000 Hz, and the current of the DC power supply (7) providing the magnetic field is set to 1 A~4 A.
10. The apparatus for forming a uniform coating on the inner wall of a pipe fitting as described in any one of claims 1-5, or the method for forming a uniform coating on the inner wall of a pipe fitting as described in any one of claims 6-9, is used for the protection of the inner wall of metal pipe fittings in the fields of petrochemicals, aerospace, energy transmission, marine engineering, precision machinery, medical devices, and automobile manufacturing.