Negative electrode for all-solid-state battery and all-solid-state battery including the same
Patent Information
- Application Number
- CN202480079527.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-15
- Filing Date
- 2024-03-29
- Publication Date
- 2026-07-24
AI Technical Summary
Existing all-solid-state battery negative electrodes are prone to solid electrolyte degradation during lithium deposition, and are also costly, affecting battery stability and lifespan.
The current collector employs a multilayer structure composed of metal oxides and carbon-based materials that can be alloyed with lithium. By forming lithium deposits between the first and second layers, direct contact between lithium and the solid electrolyte is reduced, preventing electrolyte degradation. Electrochemical performance is optimized by controlling the layer thickness and material ratio.
Stable lithium deposition and uniform distribution were achieved, reducing the degradation of solid electrolytes, improving the electrochemical properties and economy of the battery, and extending battery life.
Smart Images

Figure CN122459927A_ABST
Abstract
Description
Technical Field
[0001] Disclosed negative electrode for all-solid-state batteries and all-solid-state batteries including the same. Background Technology
[0002] Recently, battery-powered electronic devices such as mobile phones, laptops, and electric vehicles have seen rapid development.
[0003] For such batteries, the development of all-solid-state batteries using lithium metal as the negative electrode is underway. All-solid-state batteries are those in which all materials are composed of solids, and specifically, those using solid electrolytes. Because the electrolyte is solid, all-solid-state batteries are structurally rigid, and therefore have a low risk of fire or explosion due to leakage caused by external impacts, etc. Furthermore, the batteries can be formed into various shapes. Summary of the Invention
[0004] Technical issues
[0005] One implementation provides a negative electrode for all-solid-state batteries that exhibits superior electrochemical properties and is cost-effective.
[0006] Another embodiment provides an all-solid-state battery including the negative electrode.
[0007] Technical solution
[0008] One embodiment provides a negative electrode for an all-solid-state battery, comprising: a current collector; a first layer disposed on the current collector and consisting of an oxide of a metal capable of alloying with lithium and a first binder; and a second layer disposed on the first layer and consisting of a carbon-based material and a second binder.
[0009] Another embodiment provides an all-solid-state battery, which includes the negative electrode, the positive electrode, and a solid electrolyte located between the negative electrode and the positive electrode.
[0010] Beneficial effects
[0011] The negative electrode for all-solid-state batteries according to one embodiment exhibits excellent electrochemical properties and is economical. Attached Figure Description
[0012] Figure 1 This is a schematic diagram illustrating a negative electrode for an all-solid-state battery according to one embodiment.
[0013] Figure 2 This is a schematic cross-sectional view of an all-solid-state battery according to one embodiment.
[0014] Figure 3The image shows a cross-sectional SEM image of the negative electrode and solid electrolyte layer according to Example 1.
[0015] Figure 4 It is based on the cross-sectional SEM images of the negative electrode and solid electrolyte layer of Comparative Example 1.
[0016] Figure 5 It is based on the cross-sectional SEM images of the negative electrode and solid electrolyte layer of Comparative Example 2.
[0017] Figure 6 A graph showing the coulombic efficiency of the half-cell cells according to Example 1 and Comparative Examples 1 and 2. Detailed Implementation
[0018] Embodiments of the invention will be described in detail below. However, these are provided by way of example and are not intended to limit the invention; the scope of this disclosure is limited only by the appended claims.
[0019] The terminology used herein is for illustrative purposes and is not intended to limit the invention. Singular expressions include plural expressions unless the context clearly specifies otherwise.
[0020] The term "combination of" may include mixtures, laminates, complexes, copolymers, alloys, blends, reaction products, etc. of the constituent elements.
[0021] The terms “comprising,” “including,” or “having” are intended to indicate the presence of the stated features, figures, steps, components, or combinations thereof, and should be understood not to preclude the possibility of the presence or addition of one or more other features, figures, steps, components, or combinations thereof.
[0022] Throughout the specification, when a section is described as "including" a certain component, it means that, unless explicitly stated otherwise, it does not exclude other components, but may include other components.
[0023] Furthermore, the terms “about” and “substantially” used throughout this specification are intended to mean values at or near the stated values, taking into account inherent preparation and material tolerances, and these terms are used to facilitate understanding of the invention and to prevent unethical infringers from unfairly exploiting the disclosure of precise or absolute values stated herein.
[0024] Throughout the instruction manual, "A and / or B" means "A or B or both A and B".
[0025] Unless otherwise defined in the specification, it will be understood that when an element such as a layer, film, region, plate, etc. is referred to as being "on" another element, it may be directly on said other element, or one or more intermediate elements may be present.
[0026] In this invention, "particle size" or "particle diameter" may refer to the average particle diameter. Alternatively, the average particle diameter may be defined as the average particle diameter (D50), which represents the diameter of the particle at the 50% cumulative volume point in the cumulative size distribution curve. The particle diameter can be measured using methods well known to those skilled in the art, such as by a particle size analyzer or by transmission electron microscopy, scanning electron microscopy, or field emission scanning electron microscopy (FE-SEM). In another embodiment, the average particle diameter (D50) can be obtained by measuring using a dynamic light scattering measurement device, followed by data analysis to count the number of particles for each particle size range, and thus calculating the value; or it can be measured using a laser diffraction method. More specifically, if measured via a laser diffraction method, the particles to be measured are dispersed in a dispersion medium and introduced into a commercially available laser diffraction particle size analyzer (e.g., the MT 3000 from Microtrac, Inc.), and then irradiated with ultrasound at approximately 28 kHz with an output power of 60 W to calculate the average particle diameter (D50) at 50% of the particle size distribution in the measurement device.
[0027] The term "thickness" can be measured, for example, by photographs taken with an optical microscope, such as a scanning electron microscope.
[0028] A negative electrode for an all-solid-state battery according to one embodiment includes: a current collector; a first layer located on the current collector and consisting of an oxide of a metal capable of alloying with lithium and a first binder; and a second layer located on the first layer and consisting of a carbon-based material and a second binder.
[0029] Figure 1 The structure of a negative electrode 400 according to one embodiment is schematically shown, and the negative electrode 400 includes a current collector 401, a first layer 403 and a second layer 405.
[0030] According to one embodiment, the negative electrode for an all-solid-state battery can be a deposition-type negative electrode. A deposition-type negative electrode is one in which lithium ions released from the positive electrode active material migrate to the negative electrode during battery charging and discharging, resulting in lithium deposition on the surface of the current collector. For example, due to the deposition of lithium ions, a lithium deposition layer is formed between the current collector and the negative electrode coating, and this lithium deposition layer can serve as the negative electrode active material. Oxides of metals capable of alloying with lithium and carbon-based materials do not act as negative electrode active materials directly involved in the charging and discharging reactions. This refers to a negative electrode in which the negative electrode active material is not included during battery assembly, but the lithium deposition layer serves as the negative electrode active material.
[0031] The first layer consists of an oxide of a metal capable of alloying with lithium and a first binder. The oxide of the metal capable of alloying with lithium may be ZnO, SnO2(IV), SnO(II), Bi2O3, or a combination thereof.
[0032] Metal oxides capable of alloying with lithium irreversibly form a metal and lithium oxide, such as Li₂O, upon reaction with lithium. Subsequently, the metal can react further with lithium, allowing the formation and decomposition of the lithium-metal alloy phase to occur reversibly. If this reaction is represented by a scheme using Zn as an example of metal, it is as follows.
[0033] [Reaction Scheme 1]
[0034] ZnO + 2Li → Zn + 2Li₂O
[0035] [Reaction Scheme 2]
[0036] Zn+Li Li-Zn
[0037] In one embodiment, the oxide of the metal capable of alloying with lithium is located in a layer separate from the carbon-based material. For example, the oxide of the metal capable of alloying with lithium is included in a first layer located on the current collector, and the carbon-based material is included in a second layer located on the first layer.
[0038] Since the first layer, located between the current collector and the second layer, comprises an oxide of a metal capable of alloying with lithium, lithium deposition can occur between the first and second layers according to reaction scheme 1 during the charging and discharging of the all-solid-state battery, thereby forming a lithium deposit therebetween. Additionally, a reaction represented by reaction scheme 2 can occur, thereby forming a lithium alloy phase between the first and second layers.
[0039] Because the reaction occurs between the first and second layers, which are not in direct contact with the solid electrolyte, direct contact between the lithium deposit and the solid electrolyte is minimized, thus preventing the degradation of the solid electrolyte. Furthermore, lithium can be stably deposited due to the alloying phase of Zn with lithium, and because Li₂O does not directly electrochemically react with lithium, the structure of the second layer remains unchanged.
[0040] If lithium metal generated at the interface between the second layer (including amorphous carbon) and the solid electrolyte migrates along the surface of the carbon particles toward the current collector via creep deformation, the lithium alloy phase formed in the first layer allows lithium to be uniformly deposited in a columnar shape on the surface of the current collector. Therefore, a lithium deposition layer can be stably and uniformly formed on the current collector.
[0041] It is unsuitable to have the oxide of the lithium-alloyed metal and the carbon-based material coexist in a single layer, as this would fail to prevent lithium deposits from contacting the solid electrolyte. Furthermore, in this case, during the initial cycling, lithium can migrate via creep deformation due to the influence of the carbon-based material, allowing lithium deposits to form between the first layer and the current collector; however, as cycling continues, the pores of the carbon-based material can become blocked, allowing lithium deposits to form at the interface between the first and second layers. Such variations in deposition location are undesirable because they lead to electrode instability.
[0042] Furthermore, if the negative electrode does not include a second layer containing carbon-based material, the first layer directly contacts the solid electrolyte layer, and lithium deposition can occur at the interface between the first layer and the solid electrolyte layer. Here, due to the high reactivity of lithium and the solid electrolyte, the degradation of the solid electrolyte can be promoted.
[0043] Furthermore, it is unsuitable to include the oxide of the metal that can be alloyed with lithium in the second layer instead of the first layer that contacts the current collector, because the lithium deposit can directly contact the solid electrolyte and therefore cannot prevent the degradation of the solid electrolyte.
[0044] The first layer consists only of an oxide of a metal capable of alloying with lithium and a first binder. The second layer consists only of a carbon-based material and a second binder. If the second layer includes a metal typically used in deposited negative electrodes, such as Ag, alloying of lithium with the oxide of the lithium-alloying metal included in the first layer can be suppressed, which is undesirable. Furthermore, as cycling progresses, lithium deposition can occur between the second layer and the solid electrolyte layer, making it impossible to prevent direct contact between lithium and the solid electrolyte.
[0045] In one embodiment, the thickness ratio of the first layer to the second layer can be from 1:1 to 1:10, and can be from 1:1 to 1:7 or from 1:1 to 1:5. If the thickness ratio of the first layer and the second layer is included in the above range, the initial irreversible capacity can be minimized, and the long-term battery life characteristics can be stabilized more effectively.
[0046] The thickness of the first layer can be from 1 μm to 10 μm, and can be from 1 μm to 5 μm or from 1 μm to 3 μm. In addition, the thickness of the second layer can be from 1 μm to 10 μm, 2 μm to 7 μm or 3 μm to 5 μm.
[0047] If the thickness ratio of the first layer to the second layer meets the above range and the thicknesses of the first and second layers respectively meet the above range, the initial irreversible capacity can be minimized, lithium can be deposited in a more stable morphology, and the contact between lithium and the solid electrolyte layer can be minimized.
[0048] In one embodiment, based on 100% by weight of the total first layer, the amount of lithium-alloyable metal included in the first layer can be from 80% to 99% by weight, and can be from 85% to 99% by weight or from 90% to 99% by weight. If the amount of lithium-alloyable metal is included in the above range, the resistance caused by the first binder can be minimized, allowing the formation reaction of the alloy phase between the metal and lithium to be more smoothly induced within the first layer.
[0049] In one embodiment, based on 100% by weight of the total second layer, the amount of carbon-based material can be from 80% to 99% by weight, and can be from 85% to 99% by weight or from 90% to 99% by weight. If the amount of carbon-based material is included in the above range, the resistance caused by the second binder can be minimized, and the creep deformation of the lithium metal can be induced more fully, thereby minimizing direct contact between the solid electrolyte and lithium.
[0050] In one embodiment, the carbon-based material may be amorphous carbon.
[0051] Amorphous carbon may be, for example, carbon black, acetylene black, superconducting acetylene black, Ketjen black, furnace black, activated carbon, graphene, or combinations thereof. Carbon black may be Super P (available from Timcal, Ltd.). Amorphous carbon is not limited to this, and any material that can be classified as amorphous carbon in the art may be used.
[0052] In one embodiment, the amorphous carbon may be a single particle or an aggregated product in the form of secondary particles having primary particle agglomeration. If the amorphous carbon is a single particle, the size of the amorphous carbon may be a nanoscale with an average particle size of 100 nm or less, for example, 10 nm to 100 nm.
[0053] If the amorphous carbon is an agglomerate, the particle size of the primary particles can be from 20 nm to 100 nm, and the particle size of the secondary particles can be from 1 μm to 20 μm.
[0054] In one embodiment, the particle size of the primary particles can be 20 nm to 100 nm, 20 nm to 90 nm, 20 nm to 80 nm, or 30 nm to 70 nm.
[0055] In one embodiment, the particle size of the secondary particles can be from 1 μm to 20 μm, from 2 μm to 15 μm, or from 3 μm to 10 μm.
[0056] The shape of the primary particles can be spherical, elliptical, plate-shaped, or a combination thereof, and in one embodiment, the shape of the primary particles can be spherical, elliptical, or a combination thereof.
[0057] In one embodiment, the first adhesive and the second adhesive, respectively included in the first layer and the second layer, may be the same as or different from each other. The first adhesive and the second adhesive may be, for example, polyvinylidene fluoride, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, or combinations thereof. Carboxymethyl cellulose, hydroxypropyl cellulose, or diacetyl cellulose may be their alkali metal salts, and the alkali metal may be Na or Li. The first adhesive and the second adhesive are not limited thereto, and any adhesive used in the relevant technical field may be used.
[0058] Based on 100% by weight of the total first layer, the amount of the first binder may include 1% to 20% by weight, 1% to 15% by weight, or 1% to 10% by weight. Within the above ranges, the first binder can sufficiently exhibit adhesive ability without degrading battery performance.
[0059] Based on 100% by weight of the total second layer, the amount of the second binder may include 1% to 20% by weight, 1% to 15% by weight, or 1% to 10% by weight. Within the above ranges, the second binder can sufficiently exhibit adhesive ability without degrading battery performance.
[0060] The current collector can be, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or alloys thereof, and can be in foil or sheet shape. The thickness of the negative electrode current collector can be 1 μm to 20 μm, 5 μm to 15 μm, or 7 μm to 10 μm.
[0061] The current collector may include a metal as a substrate and may further include a thin film on the substrate. The thin film may include, but is not limited to, elements capable of forming alloys with lithium, such as gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, or combinations thereof, and any element known in the art may be used, as long as it forms an alloy with lithium. If the current collector further includes a thin film, a flatter lithium-containing layer may be formed if lithium is deposited during charging to form a lithium-containing layer, thereby further improving the cycle life characteristics of the all-solid-state battery.
[0062] The thickness of the film can be 1 nm to 800 nm, 10 nm to 700 nm, 50 nm to 600 nm, or 100 nm to 500 nm. If the thickness of the film is within the range described above, the cycle life characteristics can be further enhanced.
[0063] According to one embodiment, the negative electrode may further include a lithium-containing layer formed between the current collector and the negative electrode coating after battery fabrication during initial charging. The thickness of the lithium-containing layer may be 1 μm to 1000 μm, 1 μm to 500 μm, 1 μm to 200 μm, 1 μm to 150 μm, 1 μm to 100 μm, or 1 μm to 50 μm. If the thickness of the lithium-containing layer falls within the aforementioned range, it can effectively function as a lithium reservoir, and the cycle life characteristics can be further enhanced.
[0064] A lithium-containing layer can be formed during charging after battery manufacturing when lithium ions are released from the positive electrode active material, pass through the solid electrolyte, and migrate toward the negative electrode, and thus lithium precipitates and deposits on the negative electrode current collector.
[0065] Charging can be a formation process, which can be carried out one to three times at about 25°C to 50°C at 0.05 C to 1 C. If lithium is precipitated and deposited to form a lithium-containing layer, the lithium in the lithium-containing layer is ionized during discharge and moves toward the positive electrode, and therefore, the lithium can be used as a negative electrode active material.
[0066] All-solid-state batteries
[0067] An all-solid-state battery according to one embodiment includes the negative electrode, the positive electrode, and a solid electrolyte layer located between the positive electrode and the negative electrode.
[0068] <Solid Electrolyte Layer>
[0069] In one embodiment, the solid electrolyte layer may include a solid electrolyte. This may be an inorganic solid electrolyte, such as a sulfide solid electrolyte, an oxide solid electrolyte, a halide solid electrolyte, etc., or it may be a solid polymer electrolyte. In one embodiment, the solid electrolyte may be a sulfide solid electrolyte. Sulfide solid electrolytes are suitable because they exhibit superior ionic conductivity compared to other solid electrolytes, such as oxide solid electrolytes, and demonstrate excellent cycle life characteristics over a wider operating range.
[0070] In one embodiment, the sulfide solid electrolyte may be Li2S-P2S5, Li2S-P2S5-LiX (where X is a halogen element such as I or Cl), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, or Li2S-P2S5-Z. m S n (where m and n are each an integer greater than 0 and less than 12, and Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p and q are each an integer greater than 0 and less than 12, and M is one of P, Si, Ge, B, Al, Ga, or In), Li a M b P c S d A e (Where a, b, c, d, and e are each an integer of 0 or greater and 12 or less, and M is Ge, Sn, Si, or a combination thereof, and A is one of F, Cl, Br, or I). Sulfide solid electrolytes can be, for example, Li. 7-x PS 6-x F x (0≤x≤2), Li 7-x PS 6-x Cl x (0≤x≤2), Li 7-x PS 6-x Br x (0≤x≤2) or Li 7- x PS 6-x I x (0≤x≤2). Furthermore, specifically, it can be Li3PS4 or Li7P3S.11 , Li7PS6, Li6PS5Cl, Li6PS5Cl, Li6PS5I, Li6PS5Br, Li 5.8 PS 4.8 Cl 1.2 Li 6.2 PS 5.2 Br 0.8 wait.
[0071] In one embodiment, the sulfide solid electrolyte may be a sulfide solid electrolyte of the argentite-germanium type. The sulfide solid electrolyte of the argentite-germanium type may be, for example, Li... a M b P c S d A e (where a, b, c, d, and e are each an integer of 0 or greater and 12 or less, and M is Ge, Sn, Si, or a combination thereof, and A is one of F, Cl, Br, or I).
[0072] Specific examples include Li3PS4 and Li7P3S. 11 , Li7PS6, Li6PS5Cl, Li6PS5Br, Li 5.8 PS 4.8 Cl 1.2 Li 6.2 PS 5.2 Br 0.8 Li6PS5I, Li 5.75 PS 4.75 Cl 1.25 、(Li 5.69 Cu 0.06 PS 4.75 Cl 1.25 、(Li 5.72 Cu 0.03 PS 4.75 Cl 1.25 、(Li 5.69 Cu 0.06 )P(S 4.70 (SO4) 0.05 )Cl 1.25 、(Li 5.69 Cu 0.06 )P(S 4.60 (SO4) 0.15 )Cl 1.25 、(Li 5.72 Cu 0.03 )P(S 4.725 (SO4) 0.025 )Cl 1.25 、(Li 5.72 Na 0.03 )P(S4.725 (SO4) 0.025 )Cl 1.25 Li 5.75 P(S 4.725 (SO4) 0.025 )Cl 1.25 Or combinations thereof, but not limited thereto. The solid electrolyte can be a β phase or an α phase. For example, it can be β-Li3PS4.
[0073] Sulfide solid electrolytes can be amorphous, crystalline, or a combination thereof. Sulfide solid electrolytes can be prepared, for example, by mixing Li₂S and P₂S₅ in a molar ratio of 50:50 to 90:10 or 50:50 to 80:20. Within these mixing ratios, sulfide solid electrolytes exhibiting excellent ionic conductivity can be prepared. Ionic conductivity can be further improved by additionally including other components such as SiS₂, GeS₂, B₂S₃, etc.
[0074] As a method for mixing sulfur-containing raw materials for preparing sulfide-based solid electrolytes, mechanical grinding or solution methods can be applied. Mechanical grinding involves placing the starting material and a ball mill, etc., into a reactor and vigorously stirring to pulverize the starting material into fine particles and then mixing them. Solution methods provide a solid electrolyte as a precipitate by mixing the starting material in a solvent. Furthermore, if heat treatment is performed after mixing, the crystals of the solid electrolyte can become more robust and the ionic conductivity can be improved. For example, sulfide-based solid electrolytes can be prepared by mixing sulfur-containing raw materials and performing heat treatment two or more times, and in this case, a robust sulfide-based solid electrolyte with high ionic conductivity can be prepared.
[0075] Sulfide solid electrolytes can also be commercially available solid electrolytes.
[0076] Oxide-based solid electrolytes can be, for example, Li 1+x Ti 2-x Al(PO4)3(LTAP) (0≤x≤4), Li 1+x+ y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2,0≤y<3)、BaTiO3、Pb(Zr,Ti)O3(PZT)、Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0≤x<1,0≤y<1), Pb(Mg3Nb 2 / 3)O3-PbTiO3 (PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0 ≤ x ≤ 1, 0 ≤ y ≤ 1), lanthanum lithium titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), Li2O, LiAlO2, Li2O - Al2O3 - SiO2 - P2O5 - TiO2 - GeO2 - based ceramics, garnet - based ceramics Li 3+ x La3M2O 12 (M = Te, Nb or Zr, and x is an integer from 1 to 10) or a mixture thereof.
[0077] The solid polymer electrolyte may include at least one selected from, for example, the following: polyethylene oxide, poly(trifluoromethanesulfonylimide)(diallyldimethylammonium) (polyTFSI(diallyldimethylammonium)), Cu3N, Li3N, LiPON, Li3PO 4· Li2S · SiS2, Li2S · GeS 2· Ga2S3, Li2O · 11Al2O3, Na2O · 11Al2O3, (Na, Li) 1+x Ti 2-x Al x (PO4)3 (0.1 ≤ x ≤ 0.9), Li[[ID=TiO3, Na5MSi4O 12 (where M is a rare earth element such as Nd, Gd, Dy, etc.), Li5ZrP3O 12 , Li5TiP3O 12 , Li3Fe2P3O 12 , Li4NbP, 12 , Li 1+x (M, Al, Ga) x (Ge 1-y Ti y ) 2-x (PO4)3 (0 ≤ x ≤ 0.8, 0 ≤ y ≤ 1.0, M is Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm or Yb), Li 1+x+y Q x Ti 2- x Si y P 3-y O 12 (0 < x ≤ 0.4, 0 < y ≤ 0.6, Q is Al or Ga), Li6BaLa2Ta2O 12 , Li7La3Zr2O 12 , Li5La3Nb2O 12 , Li5La, 12 (M is Nb, Ta) or Li 7+x A x La 3-x Zr2O 12 (0 < x < 3, A is Zn).
[0078] Halide solid electrolytes may include Li element, M element (where M is a metal other than Li) and X element (where X is a halogen). X may be, for example, F, Cl, Br and I. In particular, the halide solid electrolyte may include at least one of Br and Cl as X. In addition, M may be, for example, a metal element such as Sc, Y, B, Al, Ga, In, etc. <D
[0079] [[ID=SS]]The composition of the halide solid electrolyte is not limited, but the halide solid electrolyte may be composed of Li 6- 3a M a Br<00(0152>Cl c(where M is a metal other than Li, 0 < a < 2, 0 ≤ b ≤ 6, 0 ≤ c ≤ 6, and b + c = 6). Here, a can be 0.75 or greater or 1 or greater, and a can be 1.5 or less. b can be 1 or greater or 2 or greater. In addition, c can be 3 or greater or 4 or greater. Specific examples of the halide-based solid electrolyte can be Li3YBr6, Li3YCl6, or Li3YBr2Cl4.
[0080] The solid electrolyte can be in the form of particles. Here, the average particle size (D50) of the solid electrolyte can be 5.0 μm or less, and for example, can be 0.1 μm to 5.0 μm, 0.5 μm to 5.0 μm, 0.5 μm to 4.0 μm, 0.5 μm to 3.0 μm, 0.5 μm to 2.0 μm, or 0.5 μm to 1.0 μm.
[0081] The solid electrolyte layer can further include a binder. Here, the binder can be styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, an acrylate polymer, or a combination thereof, but the present disclosure is not limited thereto, and any material used as a binder in the relevant technical field can be used. The acrylate polymer can be butyl acrylate, polyacrylate, polymethacrylate, or a combination thereof.
[0082] The amount of the binder in the solid electrolyte layer can be appropriately adjusted and need not be limited.
[0083] The solid electrolyte layer can be prepared by placing the solid electrolyte in a mold and pressing it, or can be prepared by adding the solid electrolyte to a binder solution, coating it on a substrate film, and drying it. The binder solution can include isobutyl isobutyrate, xylene, toluene, benzene, hexane, or a combination thereof as a solvent. The pressing process can be carried out by applying a pressure of 10 MPa to 500 MPa or a pressure of 100 MPa to 400 MPa. Since the process for preparing the solid electrolyte layer is widely known in the relevant field, its detailed description will be omitted in this specification.
[0084] The thickness of the solid electrolyte layer can be, for example, 10 μm to 150 μm.
[0085] The solid electrolyte layer can further include an alkali metal salt and / or an ionic liquid and / or a conductive polymer.
[0086] The alkali metal salt can be, for example, a lithium salt. In the solid electrolyte layer, the amount of the lithium salt can be 1 M or greater, for example, 1 M to 4 M. In this case, the lithium salt can improve the lithium ion mobility of the solid electrolyte layer, thereby improving the ionic conductivity.
[0087] The lithium salt may be, for example, LiSCN, LiN(CN)2, Li(CF3SO2)3C, LiC4F9SO3, LiN(SO2CF2CF3)2, LiCl, LiF, LiBr, LiI, LiB(C2O4)2, LiBF4, LiBF3(C2F5), lithium bis(oxalate)borate (LiBOB), lithium oxaloyl difluoroborate (LIODFB), lithium difluoro(oxalate)borate (LiDFOB), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI, LiN(SO2F)2), LiCF3SO3, LiAsF6, LiSbF6, LiClO4, or mixtures thereof.
[0088] Furthermore, lithium salts can be imide-based, for example, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2) or lithium bis(fluorosulfonyl)imide (LiFSI, LiN(SO2F)2). Lithium salts can suitably retain their chemical reactivity with ionic liquids, and therefore, can maintain or improve ionic conductivity.
[0089] Ionic liquids are salts or molten salts composed solely of ions that have a melting point at or below room temperature and are liquid at room temperature.
[0090] Ionic liquids may be compounds including: a) at least one cation selected from: ammonium-based, pyrrolidine Based on pyrrolidine ), pyridine pyridine-based ), pyrimidine basal (based on pyrimidine) (of) imidazole base (based on imidazole) piperidine) Based on piperidine ), pyrazole pyrazole-based of), azole base (based on) azole (and pyridazine) (Based on pyridazine) of), base (based on) ), sulfonyl (sulfonyl-based), triazole triazole-based a) or a mixture thereof, and b) selected from at least one anion selected from BF4 - PF6 - AsF6- SbF6 - AlCl4 - HSO4 - ClO4 - CH3SO3 - CF3CO2 - Cl - ,Br - I - BF4 - SO4 - CF3SO3 - (FSO2)2N - (C2F5SO2)2N - (C2F5SO2)(CF3SO2)N - Or (CF3SO2)2N - .
[0091] The ionic liquid may be, for example, selected from at least one of the following: bis(trifluoromethanesulfonyl)imide N-methyl-N-propylpyrrolidine bis(3-trifluoromethanesulfonyl)imine N-butyl-N-methylpyrrolidine bis(trifluoromethanesulfonyl)amine 1-butyl-3-methylimidazolium Or bis(trifluoromethanesulfonyl)amine 1-ethyl-3-methylimidazolium .
[0092] In the solid electrolyte layer, the weight ratio between the solid electrolyte and the ionic liquid can range from 0.1:99.9 to 90:10, for example, 10:90 to 90:10, 20:80 to 90:10, 30:70 to 90:10, 40:60 to 90:10, or 50:50 to 90:10. Solid electrolyte layers within these ranges can have improved electrochemical contact area with the electrodes, and therefore, can maintain or improve ionic conductivity. Consequently, the energy density, discharge capacity, rate performance, etc., of all-solid-state rechargeable batteries can be improved.
[0093] <Positive electrode>
[0094] According to one embodiment, the positive electrode for an all-solid-state battery includes a positive electrode current collector and a layer of positive electrode active material on one surface of the positive electrode current collector.
[0095] The positive electrode active material layer may include a positive electrode active material. This positive electrode active material may be a positive electrode active material capable of reversibly inserting and deintercalating lithium ions. For example, the positive electrode active material may include one or more composite oxides of lithium and metals selected from cobalt, manganese, nickel, and combinations thereof. An example of a positive electrode active material may be Li. a A 1-b B1 b D 1 2 (0.90≤a≤1.8,0≤b≤0.5);Li a HAVE BEEN 1-b B 1 b O 2-c D 1 c (0.90≤a≤1.8, 0≤b≤0.5,0≤c≤0.5);Li a HAVE BEEN 2-b B 1 b O 4- c D 1 c (0.90≤a≤1.8,0≤b≤0.5,0≤c≤05);Li a Ni 1-b-c Co b B 1 c D 1 α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α≤2);Li a Ni 1-b-c Co b B 1 c O 2-α F 1 α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Co b B 1 c O 2-α F 1 2 (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b- c Mr b B 1 c D 1 α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α≤2);Li a Ni 1-b-c Mr b B 1 c O 2-α F 1α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 2 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b E c G d O2 (0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1); Li a Ni b Co c L 1 d G e O2 (0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a MnG b O2 (0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4 (0.90≤a≤1.8, 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiI 1 O2; LiNiVO4; Li (3-f) J2(PO4)3 (0≤f≤2); Li (3-f) Fe2(PO4)3 (0≤f≤2); or LiFePO4.
[0096] In the chemical formula, A is selected from Ni, Co, Mn, or combinations thereof; B 1 Selected from Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements or combinations thereof; D 1 Selected from O, F, S, P or combinations thereof; E selected from Co, Mn or combinations thereof; F 1Selected from F, S, P or a combination thereof; G is selected from Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is selected from Ti, Mo, Mn or a combination thereof; I 1 Selected from Cr, V, Fe, Sc, Y or a combination thereof; J is selected from V, Cr, Mn, Co, Ni, Cu or a combination thereof; L 1 Selected from Mn, Al or a combination thereof.
[0097] According to one embodiment, the positive electrode active material can be a ternary lithium transition metal oxide, such as LiNi x Co y Al z O2 (NCA), LiNi x Co y Mn z O2 (NCM) (where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1), etc.
[0098] The compound may have a coating layer on its surface, or may be mixed with another compound having a coating layer. The coating layer may include at least one coating element compound selected from the following: oxides of coating elements, hydroxides of coating elements, hydroxyoxides of coating elements, carbonate oxides of coating elements, and hydroxycarbonates of coating elements. The compound for the coating layer can be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or a mixture thereof. The coating layer can be formed by any coating method such as spraying, dip coating, etc., as long as the elements are applied to the compound in a manner that does not adversely affect the properties of the positive electrode active material, and no detailed description is given thereof, because such methods will be readily understood by those of ordinary skill in the art.
[0099] In addition, the coating layer can be any coating material known as a coating layer for a positive electrode active material in a all-solid-state battery. For example, it can be a buffer layer for reducing the interfacial resistance between the positive electrode active material and the solid electrolyte. For example, the buffer layer can include lithium-metal-oxides and the metal can be one or more elements selected from Al, B, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ta, V, W or Zr. Specific examples of the buffer layer can be Li2O-ZrO2 (LZO), LiNbO2, etc.
[0100] Furthermore, if the positive electrode active material is a ternary material including nickel, cobalt, and manganese, or nickel, cobalt, and aluminum, the capacity density of the all-solid-state battery can be further improved, and the metal leaching from the positive electrode active material during charging can be further reduced. As a result, the long-term reliability and cycle characteristics of the all-solid-state battery during charging can be further improved.
[0101] The average particle size of the positive electrode active material can be from 1 μm to 25 μm, for example, 3 μm to 25 μm, 1 μm to 20 μm, 1 μm to 18 μm, 3 μm to 15 μm, or 5 μm to 15 μm. For example, the positive electrode active material may include small particles with an average particle size D50 of 1 μm to 9 μm and large particles with an average particle size D50 of 10 μm to 25 μm. Positive electrode active materials with such particle size ranges can be harmoniously mixed with other components in the positive electrode active material layer, and high capacity and high energy density can be achieved.
[0102] The positive electrode active material can be a secondary particle formed by the agglomeration of multiple primary particles or a single crystal. In addition, the shape of the positive electrode active material can be spherical or nearly spherical, or it can be polyhedral or irregular.
[0103] In the positive electrode active material layer, there is no limitation on the amount of positive electrode active material, and it can be within any range applicable to the positive electrode layer of conventional rechargeable all-solid-state batteries. For example, based on 100% by weight of the total positive electrode active material layer, the positive electrode active material can be included in amounts of 55% to 99.5% by weight, such as 65% to 95% by weight or 75% to 91% by weight.
[0104] The positive electrode active material layer may further include a binder and / or a conductive material.
[0105] The adhesive may be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but is not limited to these.
[0106] Based on 100% by weight of the total positive electrode active material layer, a binder may be included in an amount from 0.1% by weight to 5% by weight or from 0.1% by weight to 3% by weight. Within these amounts, the binder can exhibit sufficient adhesion without degrading battery performance.
[0107] This includes conductive materials to impart conductivity to the electrodes, and any material that has electronic conductivity can be used without causing chemical changes in the battery. Examples of conductive materials may include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, carbon nanotubes, etc.; metal-based materials, including metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0108] Based on 100% by weight of the total positive electrode active material layer, conductive material may be included in an amount of 0.1% to 5% by weight or 0.1% to 3% by weight. Conductive material within these ranges can improve electrical conductivity without degrading battery performance.
[0109] The positive electrode active material layer may further include a solid electrolyte. The solid electrolyte included in the positive electrode active material layer may be an inorganic solid electrolyte, such as a sulfide solid electrolyte, an oxide solid electrolyte, a halide solid electrolyte, or a solid polymer electrolyte. The solid electrolyte is the same as described in the preceding section on solid electrolytes and may be the same as or different from the solid electrolyte included in the solid electrolyte layer.
[0110] Based on 100% by weight of the total positive electrode active material layer, a solid electrolyte may be included in amounts ranging from 0.1% to 35% by weight, for example, 1% to 35% by weight, 5% to 30% by weight, 8% to 25% by weight, or 10% to 20% by weight. Including a solid electrolyte in the positive electrode in amounts within these ranges can improve the efficiency and cycle life characteristics of the all-solid-state battery without capacity degradation.
[0111] The positive electrode current collector includes, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or alloys thereof, and may be in foil or sheet form.
[0112] <Elastic Layer>
[0113] An all-solid-state battery according to one embodiment may further include an elastic layer that buffers thickness variations that occur during charging and discharging. The elastic layer may be located between the negative electrode and the casing.
[0114] The elastic layer may include materials with insulating properties and an elastic recovery rate of 50% or greater, and specifically may include silicone rubber, acrylic rubber, fluorinated rubber, nylon, synthetic rubber, or combinations thereof. The cushioning material may be in the form of a polymer sheet (sheet).
[0115] Manufacturing of all-solid-state batteries
[0116] According to one embodiment, an all-solid-state battery can be manufactured by the following process.
[0117] A first layer composition is prepared by adding an oxide of a metal capable of alloying with lithium and a first binder to a first solvent. A second layer composition is prepared by adding a carbon-based material and a second binder to a second solvent.
[0118] The first solvent may be N-methylpyrrolidone, octyl acetate, isobutyl isobutyrate, toluene, xylene, water, or a combination thereof, and the second solvent may be N-methylpyrrolidone, octyl acetate, isobutyl isobutyrate, toluene, xylene, water, or a combination thereof.
[0119] A first structure comprising a first layer is formed by coating a first layer composition onto a first substrate and drying it. A second structure comprising a second layer is formed by coating a second layer composition onto a second substrate and drying it. The second substrate may be stainless steel, but is not limited thereto. The first substrate may be a current collector.
[0120] The coating process can be performed by spraying, slurry casting, or sputtering. Depending on the coating process, the thicknesses of the first and second layers can be adjusted, and for example, the process can be performed such that the thickness ratio of the first layer to the second layer is in the range of 1:10 to 1:3.
[0121] A second structure is disposed such that the second layer contacts one surface of the solid electrolyte layer, and after the initial pressing, the second substrate is removed to transfer the second layer to the solid electrolyte layer. The initial pressing process can be performed at 1 MPa to 500 MPa, 10 MPa to 400 MPa, or 100 MPa to 400 MPa.
[0122] Subsequently, the first structure is placed so that the first layer contacts the second layer, and a secondary pressing is performed to form the first layer on the second layer. The secondary pressing process can be carried out at pressures ranging from 1 MPa to 500 MPa, 10 MPa to 400 MPa, or 100 MPa to 400 MPa. However, the secondary pressing process can also be carried out at lower pressures than the primary pressing process.
[0123] Through the above process, a negative electrode comprising a second layer, a first layer, and a current collector can be formed on the solid electrolyte layer.
[0124] Subsequently, the positive electrode is placed on the surface of the solid electrolyte layer opposite to the surface that contacts the second layer to prepare a laminate. The all-solid-state battery is then fabricated by pressing the laminate.
[0125] The pressing process can be carried out at temperatures ranging from 25°C to 90°C. Alternatively, the pressing process can be performed at pressures of 550 MPa or less, for example 500 MPa or less, or for example, within the range of 1 MPa to 500 MPa. The pressing time can vary depending on the temperature and pressure, and can be, for example, less than 30 minutes. The pressing process can be, for example, an isostatic press, a roller press, a plate press, or a warm isostatic press.
[0126] All-solid-state secondary batteries can be unit cells with a structure including a positive electrode / solid electrolyte layer / negative electrode, dual-cell cells (dual cells) with a structure including a positive electrode / solid electrolyte layer / negative electrode / solid electrolyte layer / positive electrode, or stacked cells of repeated unit cells.
[0127] There are no limitations on the shape of all-solid-state rechargeable batteries, but they can be, for example, coin-shaped, button-shaped, sheet-shaped, stacked, cylindrical, or flat. Furthermore, all-solid-state rechargeable batteries can be used in large batteries used in electric vehicles, etc. For example, all-solid-state rechargeable batteries can also be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, all-solid-state rechargeable batteries can be used in a variety of applications requiring large-capacity energy storage, such as in electric bicycles or power tools. Moreover, all-solid-state rechargeable batteries can be used in various fields, such as portable electronic devices.
[0128] Figure 2 This is a cross-sectional view showing an all-solid-state battery according to one embodiment. (Refer to...) Figure 2 The all-solid-state battery 100 may have the following structure: an electrode assembly is housed in a casing, such as a bag, and the electrode assembly includes: a negative electrode 400 comprising a negative electrode current collector 401, a first layer 403, and a second layer 405; a solid electrolyte layer 300; and a positive electrode 200 comprising a positive electrode active material layer 203 and a positive electrode current collector 201. The all-solid-state battery 100 may further include an elastic layer 500 located on the outer side of at least one of the positive electrode 200 and the negative electrode 400.
[0129] Figure 2 The diagram shows an electrode assembly including a negative electrode 400, a solid electrolyte layer 300, and a positive electrode 200, but an all-solid-state battery can also be fabricated by stacking at least two electrode assemblies. For example, electrode assemblies can be stacked in numbers such as 2 to 100, 3 to 50, 4 to 20, etc.
[0130] Mode for carrying out the present invention
[0131] Embodiments and comparative examples of the invention are described below. However, these embodiments are not to be construed as limiting the scope of the invention in any way.
[0132] (Example 1)
[0133] 90 mg of β-Li3PS4 (available from NEI corporation) was placed in a mold with an inner diameter of 10 mm and pressed at 200 MPa to prepare a solid electrolyte layer with a thickness of 100 μm.
[0134] The first layer composition was prepared by mixing ZnO (average particle size: 500 nm) and polyvinylidene fluoride in an N-methylpyrrolidone solvent at a weight ratio of 9:1.
[0135] The first layer composition is applied to stainless steel by a slurry casting method and dried to prepare a first structure in which a first layer with a thickness of 1 μm is formed.
[0136] The second layer composition was prepared by mixing carbon black (SC65, available from MTI) and polyvinylidene fluoride in an N-methylpyrrolidone solvent at a weight ratio of 9:1.
[0137] The second layer composition is applied to a stainless steel current collector by a slurry casting method and dried to prepare a second structure in which a second layer with a thickness of 3 μm is formed.
[0138] A first structure is placed such that the first layer is in contact with the solid electrolyte layer, and then pressed at 300 MPa. The stainless steel is then removed to transfer the first layer onto the solid electrolyte layer. A second structure is placed such that the second layer is in contact with the first layer, and then pressed at 380 MPa to fabricate a negative electrode comprising the first layer, the second layer, and a current collector.
[0139] Subsequently, a lithium metal foil (thickness: 400 μm, available from Honjo) was placed on the surface of the solid electrolyte layer opposite to the surface on which the negative electrode is formed, and then pressed at 5 MPa to manufacture a half-cell. In the manufactured all-solid-state half-cell, the thickness of the first layer is 1 μm, the thickness of the second layer is 3 μm, and therefore the thickness ratio of the first layer to the second layer is 1:3.
[0140] (Example 2)
[0141] The half-cell was manufactured in the same manner as in Example 1, except that the negative electrode was prepared by changing the thickness of the first layer to 3 μm, so that the thickness ratio of the first layer to the second layer was 1:1.
[0142] (Example 3)
[0143] The half-cell was manufactured in the same manner as in Example 1, except that SnO(II) was used instead of ZnO.
[0144] (Example 4)
[0145] The half-cell was manufactured in the same manner as in Example 3, except that the negative electrode was prepared by changing the thickness of the first layer to 3 μm, so that the thickness ratio of the first layer to the second layer was 1:1.
[0146] (Comparative Example 1)
[0147] A carbon layer composition was prepared by mixing carbon black (SC65, available from MTI) and polyvinylidene fluoride in an N-methylpyrrolidone solvent at a weight ratio of 9:1.
[0148] The carbon layer composition was applied to a stainless steel current collector by a slurry casting method and dried to prepare a structure in which a carbon layer with a thickness of 3 μm is formed.
[0149] The structure was positioned such that the carbon layer was in contact with the solid electrolyte layer of Example 1, and then pressed at 300 MPa to prepare a negative electrode comprising a carbon layer and a current collector on the solid electrolyte layer.
[0150] Subsequently, a lithium metal foil (thickness: 400 μm, available from Honjo) was placed on the surface of the solid electrolyte layer opposite to the surface on which the negative electrode is formed. The resulting assembly was then pressed at 5 MPa to fabricate a single half-cell. In the fabricated all-solid-state half-cell, the carbon layer was 3 μm thick.
[0151] (Comparative Example 2)
[0152] A ZnO composition was prepared by mixing ZnO (average particle size: 500 nm) and polyvinylidene fluoride in an N-methylpyrrolidone solvent at a weight ratio of 9:1.
[0153] The ZnO layer composition was applied to a stainless steel current collector by a slurry casting method and dried to prepare a structure in which a ZnO layer with a thickness of 1 μm is formed.
[0154] The structure was arranged so that the ZnO layer was in contact with the solid electrolyte layer of Example 1, and then pressed at 300 MPa to prepare a negative electrode comprising a ZnO layer and a current collector on the solid electrolyte layer.
[0155] Subsequently, a lithium metal foil (thickness: 400 μm, available from Honjo) was placed on the surface of the solid electrolyte layer opposite to the surface on which the negative electrode is formed, and then pressed at 5 MPa to fabricate a half-cell. In the fabricated all-solid-state half-cell, the carbon layer thickness was 3 μm.
[0156] (Comparative Example 3)
[0157] The first layer composition was prepared by mixing ZnO (average particle size: 500 nm), carbon black (SC65, available from MTI) and polyvinylidene fluoride in an N-methylpyrrolidone solvent at a weight ratio of 3:9:1.
[0158] The first layer composition is applied to stainless steel by a slurry casting method and dried to prepare a first structure in which a first layer with a thickness of 4 μm is formed.
[0159] A first structure is placed such that the first layer contacts the solid electrolyte layer of Example 1, and after pressing at 300 MPa, the stainless steel is removed to transfer the first layer to the solid electrolyte layer, thereby preparing a negative electrode comprising the first layer and a current collector on the solid electrolyte layer.
[0160] Subsequently, a lithium metal foil (thickness: 400 μm, available from Honjo) was placed on the surface of the solid electrolyte layer opposite to the surface on which the negative electrode is formed, and then pressed at 5 MPa to manufacture a half-cell. In the manufactured all-solid-state half-cell, the thickness of the first layer is 4 μm.
[0161] Example 1) Evaluation of SEM
[0162] Cross-sectional SEM images of the negative electrode and solid electrolyte layer in Example 1 and Comparative Examples 1 and 2 are shown in the figures. Figure 3 , 4 and 5 in. exist Figures 3 to 5 In this context, SE represents the solid electrolyte layer, carbon represents the layer containing carbon black, and ZnO represents the layer containing ZnO.
[0163] like Figure 3 As shown in Example 1, a columnar lithium deposition between the second and first layers can be confirmed.
[0164] like Figure 4 As shown in Comparative Example 1, lithium is deposited on the current collector in a wave (undulating) shape, and as... Figure 5 As shown in Comparative Example 2, although lithium is deposited in a columnar shape, the lithium deposition occurs at the interface in contact with the solid electrolyte.
[0165] Example 2) Evaluation of Coulomb efficiency
[0166] The half-cells manufactured according to Example 1 and Comparative Examples 1 and 2 were subjected to a temperature of 0.5 mA / cm at 60°C. 2 Current density, 2 mAh / cm 2 The battery was subjected to 90 charge-discharge cycles at a capacity of [capacity] and a rate of 0.25 C. The ratio of charge capacity to discharge capacity in each cycle was calculated. The results are presented as @coulomb efficiency. Figure 6 middle.
[0167] like Figure 6 As shown, Example 1 exhibits a coulombic efficiency of approximately 95% even after 90 charge and discharge cycles, while in Comparative Example 1, a short circuit occurs at approximately 22 cycles and in Comparative Example 2, at approximately 32 cycles, making subsequent charge and discharge impossible.
[0168] While the invention has been described with respect to exemplary embodiments which are now considered practical, it will be understood that the invention is not limited to the disclosed embodiments. Rather, it is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.
Claims
1. A negative electrode for all-solid-state batteries, comprising: current collector; A first layer located on the current collector and consisting of an oxide of a metal capable of alloying with lithium and a first binder; as well as A second layer located on top of the first layer and composed of a carbon-based material and a second binder.
2. The negative electrode for an all-solid-state battery according to claim 1, wherein the oxide of the metal capable of alloying with lithium is ZnO, SnO2(IV), SnO(II), Bi2O3, or a combination thereof.
3. The negative electrode for an all-solid-state battery according to claim 1, wherein the thickness ratio of the first layer to the second layer is 1:1 to 1:
10.
4. The negative electrode for an all-solid-state battery according to claim 1, wherein the thickness ratio of the first layer to the second layer is 1:1 to 1:
7.
5. The negative electrode for an all-solid-state battery according to claim 1, wherein the first layer has a thickness of 1 μm to 10 μm.
6. The negative electrode for an all-solid-state battery according to claim 1, wherein the first layer has a thickness of 1 μm to 5 μm.
7. The negative electrode for an all-solid-state battery according to claim 1, wherein the second layer has a thickness of 1 μm to 10 μm.
8. The negative electrode for an all-solid-state battery according to claim 1, wherein the second layer has a thickness of 2 μm to 7 μm.
9. The negative electrode for an all-solid-state battery according to claim 1, wherein the carbon-based material is amorphous carbon.
10. The negative electrode for an all-solid-state battery according to claim 9, wherein the amorphous carbon is carbon black, acetylene black, superconducting acetylene black, Ketjen black, furnace black, activated carbon, graphene, or a combination thereof.
11. The negative electrode for an all-solid-state battery according to claim 1, wherein the first binder and the second binder are polyvinylidene fluoride, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, or a combination thereof.
12. The negative electrode for an all-solid-state battery according to claim 1, wherein the amount of the oxide of the metal capable of alloying with lithium is from 80% to 99% by weight, based on 100% by weight of the total first layer.
13. The negative electrode for an all-solid-state battery according to claim 1, wherein the amount of the first binder is from 1% to 20% by weight based on 100% by weight of the total first layer.
14. The negative electrode for an all-solid-state battery according to claim 1, wherein the amount of the carbon-based material is from 80% to 99% by weight, based on 100% by weight of the total second layer.
15. The negative electrode for an all-solid-state battery according to claim 1, wherein the amount of the second binder is from 1% to 20% by weight, based on 100% by weight of the total second layer.
16. The negative electrode for an all-solid-state battery according to claim 1, wherein the current collector is, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
17. All-solid-state batteries, including: The negative electrode according to any one of claims 1 to 16; Positive electrode; as well as A solid electrolyte layer located between the positive electrode and the negative electrode.