A flow battery with a solid-state energy storage mechanism

By introducing a lead and chromium ion system into the negative electrode of a vanadium redox flow battery, a solid-phase energy storage mechanism is constructed, which solves the problem of low energy density in vanadium redox flow batteries, improves system energy density and reduces cost, avoids electrode deposition and blockage, and improves battery charge and discharge performance.

CN122696728BActive Publication Date: 2026-11-10DALIAN RONGKE POWER
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202611178066.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-05
Publication Date
2026-11-10
Estimated Expiration
2046-08-05

AI Technical Summary

Technical Problem

Existing vanadium redox flow batteries suffer from high electrolyte costs, low energy density, and a lack of solid-phase energy storage mechanisms suitable for the negative electrode, which limits the improvement of the overall system energy density.

Method used

Solid-phase energy storage materials, including elemental lead and lead-containing precursor compounds, are introduced into the negative electrode system. Combined with total vanadium ions and total chromium ions as redox electron carriers, and using mixed anions to support the electrolyte, a solid-phase energy storage mechanism for the negative electrode is constructed. The chromium and vanadium dual carriers are responsible for the targeted redox cycle of charging and discharging.

Benefits of technology

It significantly improves the overall energy density of flow batteries, reduces the cost per kilowatt-hour, and avoids dendrite short circuits and flow channel blockage through stable solid-phase energy storage materials and specially designed supporting electrolyte, thereby improving the charge-discharge kinetics and lifespan of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of energy storage flow battery technology, specifically to a flow battery with a solid-phase energy storage mechanism. The negative electrode system of the flow battery includes a solid-phase energy storage material and a negative electrode electrolyte. The energy storage active material of the solid-phase energy storage material is selected from elemental lead and at least one lead-containing precursor compound capable of in-situ conversion in the negative electrode electrolyte to provide an active lead source; the negative electrode electrolyte contains vanadium ions and chromium ions as redox couples, and a supporting electrolyte solution composed of hydrogen ions and mixed anions, wherein the mixed anions are a combination of chloride ions and sulfate and / or hydrogen sulfate ions. This invention designs a flow battery with a solid-phase energy storage mechanism. 2+ ) and vanadium ions (V 3+ The solid-phase energy storage conversion process involving both the negative electrode and the battery system broadens the potential window of the redox reaction on the negative electrode side, improves the energy density of the battery system, and establishes a solid-phase energy storage mechanism based on the negative electrode for the first time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of energy storage flow battery technology, and more specifically to a flow battery with a solid-phase energy storage mechanism. Background Technology

[0002] Against the backdrop of global energy transition and the "dual carbon" goal, the development and utilization of renewable energy sources such as wind and solar power are becoming increasingly widespread. To address the intermittency and volatility of these new energy power generation methods, large-scale, long-duration energy storage technology has become crucial for maintaining grid stability. Vanadium redox flow batteries (VRFBs) are among the preferred technologies for large-scale, long-duration energy storage due to their outstanding advantages, including high intrinsic safety, long cycle life, and decoupled power and capacity configuration.

[0003] However, the large-scale commercial application of vanadium redox flow batteries has long been constrained by two major bottlenecks: first, the high initial investment cost, with the cost of vanadium electrolyte accounting for more than 40% to 50% of the total battery system cost; second, the low energy density of vanadium batteries (typically only 15 to 25 Wh / L) due to the solubility limit of pentavalent vanadium ions in room temperature acidic solutions (usually less than 2.0 mol / L) and thermal stability issues, resulting in a large system footprint.

[0004] To overcome the cost and energy density bottlenecks imposed by the aforementioned concentration limits, "Redox Targeting" has become a research hotspot in the flow battery field in recent years. Its core idea is to introduce low-cost, high-capacity solid-state energy storage materials into the electrolyte tank, utilizing redox-active ions dissolved in the liquid phase as "Nernst electron carriers (dielectrics)." These ions undergo chemical redox reactions with the solid-state material as the electrolyte flows through the tank, thereby storing the system's energy in the solid material. This mechanism significantly reduces the dependence on the concentration of expensive active ions.

[0005] In the prior art, some improvements to solid-phase energy storage in vanadium redox flow batteries have been disclosed. For example, Chinese patent application CN118645668A discloses a "vanadium redox flow battery based on solid energy storage materials and its preparation method," which introduces a Prussian blue analogue (PBA) as a solid energy storage material into the positive electrode storage tank. Another example is Chinese patent application CN118299630B, which discloses a "high-capacity vanadium redox flow battery positive electrode electrolyte," which also uses a targeted redox solid energy storage material containing ammonia-rich iron / copper ferrocyanide as the positive electrode energy storage medium. This material reacts with the positive electrode redox medium VOCs. 2+ / VO2 + With similar equilibrium potentials, high-capacity energy storage on the positive electrode side is achieved, thereby reducing the concentration requirement of pentavalent vanadium and the cost of electrolyte.

[0006] However, existing solid-phase energy storage solutions all focus on the "positive electrode side" of vanadium redox flow batteries, while solid-phase energy storage mechanisms for the "negative electrode side" are lacking. According to the "weakest link" principle in battery systems, the overall capacity of a flow battery is limited by the lower capacity of the positive or negative electrode. If high-capacity solid-phase energy storage is only achieved at the positive electrode, the system still requires a bulky and expensive conventional vanadium electrolyte storage tank for the negative electrode to maintain capacity matching. This means that existing single-sided (positive electrode) solid-phase energy storage solutions cannot truly achieve a leap in overall system energy density and a precipitous decrease in the cost per kilowatt-hour.

[0007] In summary, current vanadium redox flow battery technology urgently needs a solid-phase energy storage mechanism that can perfectly adapt to the negative electrode. Summary of the Invention

[0008] (a) Technical problems to be solved

[0009] This invention aims to address the technical problems of high cost, low energy density, and lack of a suitable solid-phase energy storage mechanism for the negative electrode in existing vanadium redox flow batteries. It provides a flow battery with a solid-phase energy storage mechanism. By constructing a novel negative electrode electrolyte and solid-phase energy storage material system, greater energy storage is achieved at the same cost, significantly reducing the overall levelized cost of electricity (LCOE) of flow batteries.

[0010] (II) Technical Solution

[0011] To solve the above-mentioned technical problems, the present invention provides a flow battery with a solid-phase energy storage mechanism. The negative electrode system of the flow battery includes: a solid-phase energy storage material placed in an electrolyte circulation loop, and a flowable negative electrode electrolyte included in the circulation loop.

[0012] The solid-phase energy storage material comprises an energy storage active substance selected from elemental lead and at least one lead-containing precursor compound capable of in-situ transformation in the negative electrode electrolyte to provide an active lead source; the negative electrode electrolyte contains total vanadium ions as a redox electron carrier and total chromium ions as a targeting medium, as well as a supporting electrolyte solution composed of hydrogen ions and mixed anions.

[0013] When the flow battery is in operation with any charge-discharge depth or in its initial formulation state: in the negative electrode electrolyte, the total vanadium ions exist in the form of divalent vanadium ions, trivalent vanadium ions, or any mixture of the two in any proportion; in the negative electrode electrolyte, the total chromium ions exist in the form of divalent chromium ions, trivalent chromium ions, or any mixture of the two in any proportion; the mixed anions are a combination of chloride ions and sulfate and / or hydrogen sulfate ions.

[0014] According to a preferred embodiment of the present invention, the solid-phase energy storage material is a solid block, granular, or porous material with a spatial conductive network, which is a composite material obtained by mixing and molding an energy storage active substance, a conductive agent (such as a carbon-based material), and a binder.

[0015] Optionally, the mass percentage range of the energy storage active material, conductive agent, and binder is 60%-85%, 5%-30%, and 2%-15%, respectively. In one specific embodiment, the mass ratio of the three is 7:2:1.

[0016] Optionally, the conductive agent is selected from carbon-based conductive materials resistant to strong acid corrosion. The carbon-based conductive materials include, but are not limited to, one or more of the following: carbon powder, zero-dimensional conductive materials, one-dimensional conductive materials, two-dimensional conductive materials, and composite conductive materials.

[0017] Optionally, the adhesive may be a thermoplastic or thermosetting acid-resistant polymer resin, specifically including but not limited to: polyethylene resin (PE), polytetrafluoroethylene resin (PTFE), polyvinylidene fluoride resin (PVDF), perfluorosulfonic acid resin (Nafion resin), polypropylene resin (PP), and acid-resistant epoxy resin, or a mixture of several of these.

[0018] According to a preferred embodiment of the present invention, the energy storage active material in the solid-phase energy storage material is elemental lead and / or lead-based ionic compounds; the lead-based ionic compounds include lead sulfate, and lead-based compounds that can generate lead sulfate in situ through ion exchange or redox reactions; optionally, the lead-based compounds are selected from one or more of lead sulfite, lead chloride, lead bromide, lead carbonate, lead phosphate, and lead acetate.

[0019] According to a preferred embodiment of the present invention, when the energy storage active material is a lead salt other than lead sulfate or elemental lead, after the battery is assembled and the negative electrode electrolyte is injected into the negative electrode system, the energy storage active material in the solid phase energy storage material can undergo a chemical reaction with the negative electrode electrolyte, so that the main phase structure of the energy storage active material is partially or completely transformed into the lead sulfate phase, so as to participate in the solid phase energy storage cycle mechanism.

[0020] According to a preferred embodiment of the present invention, in the initial preparation state, the concentration range of each major component in the negative electrode electrolyte is as follows: the concentration of total vanadium ions is 0.5M-3.0M; the concentration of total chromium ions is 0.1M-1.5M; the concentration of chloride ions is 1.0M-3.0M; the sum of the concentrations of sulfate ions and bisulfate ions based on total sulfate groups is 1.0M-5.0M; and hydrogen ions are used to maintain electroneutrality and provide an acidic environment.

[0021] Optionally, in its initial preparation state, the negative electrode electrolyte comprises: 1.2M-1.8M trivalent vanadium ions, 0.3M-0.8M trivalent chromium ions, 2.5M-3.5M chloride ions, a collection of sulfate and bisulfate ions at a concentration of 2.5M-3.5M, and hydrogen ions to maintain electroneutrality. In the initial state of a specific embodiment, the negative electrode electrolyte contains 1.5M trivalent vanadium ions, 0.5M trivalent chromium ions, 3M chloride ions, and 3M sulfate ions (including incompletely ionized bisulfate ions), with the remainder being hydrogen ions.

[0022] According to a preferred embodiment of the present invention, the molar ratio of sulfate ions to chloride ions in the negative electrode electrolyte is 1-1.5:1.

[0023] According to a preferred embodiment of the present invention, the flow battery further includes a positive electrode system. The redox couple of the positive electrode system is not limited to tetravalent vanadium / pentavalent vanadium, but may also be selected from or include one or more available flow battery couples such as polyhalogen redox couples, iron ion redox couples, and chromium ion redox couples.

[0024] According to a preferred embodiment of the present invention, a positive electrode electrolyte circulates in the positive electrode system; in the initial preparation state, the positive electrode electrolyte comprises:

[0025] Vanadium tetravalent ions at concentrations of 1.0M-3.0M, chromium ions at concentrations of 0.05M-1.0M, chloride ions at concentrations of 1.0M-5.0M, sulfate ions and bisulfate ions at concentrations of 1.0M-5.0M, and hydrogen ions used to maintain electroneutrality and provide an acidic environment.

[0026] Further optionally, in the initial preparation state, the positive electrode electrolyte contains 2.0M tetravalent vanadium ions, 0.4M trivalent chromium ions, 2.2M chloride ions, sulfate ions and bisulfate ions with a total concentration of 3.0M, and hydrogen ions for maintaining electroneutrality.

[0027] In the positive electrode electrolyte, a certain amount of chromium ions are added to suppress the cross-diffusion of ions across the membrane caused by the concentration difference, thereby maintaining the capacity balance of the positive and negative electrodes during long-term cycling.

[0028] This invention does not limit the materials and forms of the electrodes and proton separators, and can refer to existing technologies.

[0029] In this application:

[0030] The negative electrode electrolyte is an electrolyte that operates on the negative electrode side, which includes redox electron carriers (divalent and / or trivalent vanadium ions), a targeting medium (trivalent and / or divalent chromium ions), and a supporting electrolyte solution.

[0031] The supporting electrolyte solution consists of hydrogen ions and a mixture of anions; the mixed anions are a combination of chloride ions and sulfate and / or hydrogen sulfate ions. The supporting electrolyte solution is a conductive solution used to support the electrochemical reactions of the vanadium ion redox pair and chromium ions.

[0032] The positive electrode electrolyte is the electrolyte operating on the positive electrode side. It contains redox electron carriers (tetravalent and / or pentavalent vanadium ions) and a supporting electrolyte solution, which consists of hydrogen ions and anions. In the positive electrode electrolyte, chromium ions are optional, not mandatory; their valence state can be divalent or trivalent. The main purpose of adding chromium ions to the positive electrode is to suppress cross-diffusion of ions across the proton exchange membrane caused by the concentration gradient, thus maintaining the capacity balance between the positive and negative electrodes during long-term cycling.

[0033] In the positive electrode electrolyte, the supporting anions in the electrolyte solution can be a single type of anion or a mixture of the same type of anion as the negative electrode side.

[0034] (III) Beneficial Effects

[0035] Compared with the prior art, the present invention has achieved the following unexpected technical effects:

[0036] 1. This invention creatively designs a process using chromium ions (Cr...) 2+ ) and vanadium ions (V 3+ The solid-phase energy storage conversion process of the negative electrode, which involves the participation of both vanadium ions, breaks through the limitations of the thermodynamic potential of a single vanadium ion system and greatly broadens the potential window of the redox reaction on the negative electrode side. The supporting electrolyte system containing mixed anions is adapted to the lead sulfate / lead system for high-capacity targeted energy storage, breaking the low energy density bottleneck caused by the traditional all-vanadium redox flow battery negative electrode relying solely on liquid phase energy storage. This achieves a significant improvement in the overall energy density of the system and also establishes a solid-phase energy storage mechanism based on the negative electrode for the first time.

[0037] 2. This invention constructs a highly original charge-discharge targeted redox cycle mechanism:

[0038] (1) During the charging stage: Trivalent chromium ions in the negative electrode electrolyte are reduced to divalent chromium ions on the electrode surface. After contacting the solid-phase energy storage material, the divalent chromium ions, with their extremely low reduction potential, precisely target and reduce solid lead sulfate to elemental lead (a two-electron transfer process). During this process, the divalent chromium ions themselves are re-oxidized to trivalent chromium ions, and the regenerated trivalent chromium ions can continue to gain electrons, forming an efficient charging medium cycle.

[0039] (2) During the discharge stage: solid elemental lead is oxidized to lead sulfate by trivalent vanadium ions flowing through the liquid phase, and the trivalent vanadium ions themselves are transformed into divalent vanadium; the generated divalent vanadium has the ability to continue to release electrons and can flow back to the electrode surface for discharge, thus forming an efficient discharge medium cycle.

[0040] This "relay" mechanism, in which chromium and vanadium are the dual carriers responsible for charging and discharging, reduces the polarization overpotential of solid-phase conversion, endows solid-phase materials with excellent charge-discharge kinetics, and improves the energy density of the battery.

[0041] 3. For this dual-medium system, the present invention has specially designed a mixed acid support electrolyte of "chloride ion + sulfate / hydrosulfate ion", which overcomes the technical bias of existing low-potential deposition batteries that are prone to failure due to dendrite short circuits or precipitation blockage.

[0042] Experiments show that if pure chloride ions are used as the single anion in the electrolyte, the high concentration of free chloride ions will strongly attack lead-based solid compounds, undergoing coordination / chelation to form soluble complex ions [PbCl4]. 2- This leads to uncontrolled free dissolution of lead ions, which then randomly redeposit in the pipeline or single-cell flow field, ultimately causing system blockage and failure.

[0043] This invention maintains a high concentration of sulfate ions and rationally controls the chloride ion concentration in the negative electrode electrolyte. On the one hand, it utilizes the common-ion effect to stabilize the PbSO4 lattice; on the other hand, it suppresses the attack of chloride ions on lead-based anionic compounds from both thermodynamic and kinetic perspectives. This mixed-acid supporting electrolyte ensures that the highly active lead source is firmly confined within the solid-phase energy storage material framework during charge-discharge solid-phase conversion (PbSO4 and Pb interconversion), achieving structural stability and long lifetime of the solid-phase energy storage material during charge-discharge cycles, and avoiding the risks of loss of energy storage active material and channel blockage. Detailed Implementation

[0044] To better explain and facilitate understanding of the present invention, the present invention will be described in detail below through specific embodiments.

[0045] The present invention provides a flow battery with a solid-phase energy storage mechanism. The negative electrode system of the flow battery includes: a solid-phase energy storage material placed in an electrolyte circulation loop, and a flowable negative electrode electrolyte included in the circulation loop.

[0046] The solid-phase energy storage material comprises an energy storage active substance selected from elemental lead and at least one lead-containing precursor compound capable of in-situ transformation in the negative electrode electrolyte to provide an active lead source; the negative electrode electrolyte contains total vanadium ions as a redox electron carrier and total chromium ions as a targeting medium, as well as a supporting electrolyte solution composed of hydrogen ions and mixed anions.

[0047] When the flow battery is in operation with any charge-discharge depth or in its initial formulation state: in the negative electrode electrolyte, the total vanadium ions exist in the form of divalent vanadium ions, trivalent vanadium ions, or a mixture of both in any proportion; in the negative electrode electrolyte, the total chromium ions exist in the form of divalent chromium ions, trivalent chromium ions, or a mixture of both in any proportion; the mixed anions are a combination of chloride ions and sulfate and / or hydrogen sulfate ions.

[0048] Solid-phase energy storage materials are composites formed by mixing and molding energy storage active materials, conductive agents (such as carbon-based materials) and binders. They are solid block, granular, or porous materials with a spatial conductive network. Their shape can be processed into geometric shapes such as blocks, cylinders, and porous honeycomb structures with high specific surface area, which are flowable and do not cause blockage of the flow battery circulation channel, according to the internal spatial structure requirements of the negative electrode storage tank.

[0049] The mass percentage range of the energy storage active material, conductive agent, and binder in solid-phase energy storage materials is 60%-85%, 5%-30%, and 2%-15%, respectively. Within this ratio range, both solid-phase energy storage (high targeted active capacity) and excellent electronic conduction network can be achieved. In one specific embodiment, the mass ratio of the three is 7:2:1.

[0050] Optionally, in order to make solid-phase targeted electron transfer more efficient, especially to keep the internal electron channels open when the target material is converted into lead ion state, the conductive agent is selected from carbon-based conductive materials that are resistant to strong acid corrosion; in addition to conventional carbon powder, carbon-based conductive materials may also include, but are not limited to, one or more of the following combinations: zero-dimensional conductive materials, one-dimensional conductive materials, two-dimensional conductive materials and composite conductive materials.

[0051] Zero-dimensional conductive materials include: conductive carbon black (such as acetylene black, Ketjen black, SuperP, etc.) and nano-graphite powder; one-dimensional conductive materials include: carbon nanotubes (CNTs), carbon fibers (CF), and vapor-grown carbon fibers (VGCF); two-dimensional conductive materials include: graphene and expanded graphite; composite conductive materials include: such as a three-dimensional interconnected conductive framework constructed by combining the above-mentioned multi-dimensional carbon materials (for example, mixing particulate carbon black with one-dimensional carbon nanotubes in a certain proportion to establish a conductive network that combines long and short ranges).

[0052] Optionally, the adhesive can be a thermoplastic or thermosetting acid-resistant polymer resin, specifically including but not limited to: polyethylene resin (PE), polytetrafluoroethylene resin (PTFE), polyvinylidene fluoride resin (PVDF), perfluorosulfonic acid resin (Nafion resin), polypropylene resin (PP), acid-resistant epoxy resin, or a mixture thereof. These adhesives possess both extremely high acid corrosion resistance and electrochemical reduction resistance, and can withstand the highly corrosive support electrolyte solutions of hydrochloric acid and sulfuric acid, as well as the corrosion of divalent chromium with an extremely low redox potential.

[0053] Alternatively, solid-phase energy storage materials can be prepared by the following method:

[0054] Step A (Mixing and Dispersion): The above-mentioned energy storage active material (i.e., elemental lead or lead-based ionic compounds), conductive material, and binder are uniformly mixed according to a set ratio. Optionally, ball milling can be used for mixing, with the milling time controlled between 2h and 48h. For example, in a preferred embodiment, ball milling is used for 24h, so that the components are not only uniformly distributed macroscopically, but also that the carbon-based material can be fully coated on the surface of the lead active particles at the microscopic level, enhancing the targeted reaction sites.

[0055] Step B (Cure and Molding): The uniformly mixed powder is placed in a molding die for hot pressing and curing. Considering the softening point and glass transition temperature of different adhesives, the hot pressing temperature range is controlled between 80℃ and 300℃, the hot pressing pressure range is 0.5MPa to 20MPa, and the holding time is 0.5h to 24h. Through hot pressing, the adhesives cross-link / fuse with each other, firmly locking the lead active material and the carbon conductive network, preventing them from pulverizing or detaching under long-term scouring of acidic electrolyte.

[0056] The energy storage active material is elemental lead and / or lead-based ionic compounds; the lead-based ionic compounds include lead sulfate, and lead-based compounds that can generate lead sulfate in situ through ion exchange or redox reactions; optionally, the lead-based compounds are selected from one or more of lead sulfite, lead chloride, lead bromide, lead carbonate, lead phosphate, and lead acetate.

[0057] In one specific embodiment, if polyethylene resin is used as the adhesive, the preparation method of the solid phase energy storage material is as follows: lead-based ionic compound / lead powder / lead-containing precursor compound, carbon powder and polyethylene resin are spheroidized at a mass ratio of 7:2:1 for 24 hours, and the solid phase material is fixed by hot pressing at 150°C and 1 MPa for 10 hours through a mold. The mold can be selected according to the shape of the solid phase energy storage material to be prepared, such as square cavity, cylindrical cavity, honeycomb cavity, etc.

[0058] Optionally, after the flow battery is assembled and the negative electrode electrolyte is injected into the negative electrode system, the non-lead sulfate energy storage active substances such as lead sulfite, lead chloride, lead bromide, lead carbonate, lead phosphate, or lead acetate contained in the solid-phase energy storage material undergo a chemical reaction with the negative electrode electrolyte. Partially or completely, its main phase structure is transformed into the lead sulfate phase to participate in the solid-phase energy storage cycle mechanism. For example, in the battery, some large particles may not have fully reacted internally, resulting in the core material remaining "lead carbonate" while the outer shell becomes "lead sulfate."

[0059] Understandably, to achieve excellent solid-phase energy storage performance, the core active component of this invention during charge-discharge cycling is primarily lead sulfate and its derivatives. However, those skilled in the art should understand that during the initial assembly, preparation, or formation stages of the battery, the solid-phase material does not necessarily have to be limited to pure lead sulfate from the outset. In fact, any lead salt added to the negative electrode side of the flow battery is acceptable, as long as it ultimately transforms into the functional "lead sulfate". Therefore, any one or more lead-based ionic compounds can be introduced into the system as lead-containing precursors. Specifically, the lead-containing precursors include, but are not limited to, one or more mixtures of lead sulfate, lead sulfite, lead chloride, lead bromide, lead carbonate, lead phosphate, and lead acetate. Regardless of the lead-containing precursor (or elemental lead) used, when it is immobilized and exposed to the initial environment of the supporting electrolyte solution containing sulfuric acid and hydrochloric acid as described in this invention, or under electrochemical formation / charge-discharge redox drive after the initial injection of electrolyte, the aforementioned precursor material will be completely or partially converted in situ into the desired "lead sulfate" or its similar lead active component through spontaneous ion exchange reactions (e.g., lead carbonate is converted into lead sulfate in acid) or through redox electrochemical processes. This allows for the construction of the targeted energy storage cycle mechanism of this invention. Therefore, any technical solution that can be added as a lead-containing precursor and, when the flow battery is in operation or in the electrolyte-wetting state, ultimately generates or evolves into the lead sulfate component described in this invention, thereby performing solid-phase energy storage, falls within the essential technical concept and protection scope of this invention.

[0060] Optionally, in the initial preparation state (before battery charging), the concentration range of each major component in the negative electrode electrolyte is as follows: total vanadium ions (V... 2+ With V 3+ The total concentration of chromium ions (Cr) is 0.5M-3.0M; 2+ With Cr 3+The total concentration of sulfate ions is 0.1M-1.5M; the concentration of chloride ions is 1.0M-3.0M; the total concentration of sulfate ions and bisulfate ions is 1.0M-5.0M; the remaining ions are hydrogen ions that maintain electroneutrality and provide an acidic environment.

[0061] Further optionally, in the initial preparation state (before battery charging), the negative electrode electrolyte composition includes: 1.2M-1.8M trivalent vanadium ions, 0.3M-0.8M trivalent chromium ions, 2.5M-3.5M chloride ions, and a collection of sulfate and bisulfate ions at a concentration of 2.5M-3.5M, with the remainder being hydrogen ions to maintain electroneutrality and provide an acidic environment. In a specific embodiment, in the initial state, the negative electrode electrolyte contains 1.5M trivalent vanadium ions, 0.5M trivalent chromium ions, 3M chloride ions, and 3M sulfate ions (including incompletely ionized bisulfate ions), with the remainder being hydrogen ions.

[0062] Optionally, the molar ratio of sulfate ions to chloride ions in the negative electrode electrolyte is 1-1.5:1, so that sulfate ions are as dominant as possible compared to chloride ions, thereby better suppressing the attack of chloride ions on lead-based anionic compounds and keeping the solid-phase energy storage material stable during charge-discharge cycles.

[0063] The aforementioned flow battery also includes a positive electrode system in which a positive electrode electrolyte circulates; the redox couple of the positive electrode system is not limited to tetravalent / pentavalent vanadium, but may also include one or more of the following available flow battery couples: polyhalogen redox couple, iron ion redox couple, chromium ion redox couple, etc.

[0064] Optionally, for vanadium-based flow batteries, in the initial formulation, the concentration range of the main components of the positive electrode electrolyte is as follows: the total vanadium ion concentration is 1.0M-3.0M, wherein the initial state of the total vanadium ions is tetravalent vanadium ions; the concentration of chromium ions (trivalent and / or divalent) is 0.05M-1.0M; the concentration of chloride ions is 1.0M-5.0M; the sum of the concentrations of sulfate ions and bisulfate ions based on the total sulfate groups is 1.0M-5.0M; and the remaining ions are hydrogen ions, which maintain electroneutrality and provide an acidic environment. Chromium ions (divalent and / or trivalent) are also added to the positive electrode electrolyte, which not only provides a redox couple but also suppresses cross-diffusion of ions across the proton exchange membrane caused by the concentration difference, thus maintaining the capacity balance of the positive and negative electrodes during long-term cycling.

[0065] In a preferred embodiment, in the initial state, the positive electrode electrolyte contains 2.0M tetravalent vanadium ions, 0.4M trivalent chromium ions, 2.2M chloride ions and 3M sulfate ions (including incompletely ionized bisulfate ions), with the remaining components being hydrogen ions.

[0066] This invention constructs a highly original charge-discharge targeted redox cycle mechanism:

[0067] (1) During the charging stage: Trivalent chromium ions in the negative electrode electrolyte are reduced to divalent chromium ions on the electrode surface. After contacting the solid-phase energy storage material, the divalent chromium ions, with their extremely low reduction potential, precisely target and reduce solid lead sulfate to elemental lead (a two-electron transfer process). During this process, the divalent chromium ions themselves are re-oxidized to trivalent chromium ions, and the regenerated trivalent chromium ions can continue to gain electrons, forming an efficient charging medium cycle.

[0068] (2) During the discharge stage: solid elemental lead is oxidized to lead sulfate by trivalent vanadium ions flowing through the liquid phase, and the trivalent vanadium ions themselves are transformed into divalent vanadium; the generated divalent vanadium has the ability to continue to release electrons and can flow back to the electrode surface for discharge, thus forming an efficient discharge medium cycle.

[0069] Please refer to the following reaction formula for details:

[0070] Negative side charging process:

[0071] Cr 3+ +e-→Cr 2+ (Electrochemical conversion);

[0072] 2Cr 2+ +PbSO4→2Cr 3+ +Pb+SO4 2- (Chemical transformation);

[0073] Discharge process on the negative side:

[0074] 2V 3+ +Pb+SO4 2- →2V 2+ +PbSO4 (chemical transformation);

[0075] V 2+ -e - →V 3+ (Electrochemical conversion).

[0076] The aforementioned "relay" mechanism, in which chromium and vanadium are responsible for charging and discharging, greatly reduces the polarization overpotential of solid-phase conversion, endows solid-phase materials with excellent charge-discharge kinetics, and improves the energy density of the battery.

[0077] The following description is based on specific embodiments and comparative examples of the present invention.

[0078] Example 1:

[0079] The solid-phase energy storage material and positive and negative electrode electrolyte configurations of the flow battery in this embodiment are as follows:

[0080] Solid-phase energy storage material: Lead sulfate, carbon powder and polyethylene resin were ball-milled at a mass ratio of 7:2:1 for 24 hours, and then hot-pressed at 150℃ and 1 MPa for 10 hours to form a block solid energy storage material with a diameter of 10 mm and a thickness of 4 mm.

[0081] The initial negative electrode electrolyte consists of 1.5M trivalent vanadium ions, 0.5M trivalent chromium ions, 3M chloride ions, and 3M sulfate ions (including incompletely ionized bisulfate ions), with the remaining components being hydrogen ions to maintain charge balance.

[0082] The initial positive electrode electrolyte consists of 2.0M tetravalent vanadium ions, 0.4M trivalent chromium ions, 2.2M chloride ions, and 3M sulfate ions (including incompletely ionized bisulfate ions), with the remaining components being hydrogen ions to maintain charge balance.

[0083] Example 2:

[0084] The negative and positive electrolytes of the flow battery in this embodiment are the same as those in Example 1, except that the lead sulfate in the solid-phase energy storage material is replaced with an equal mass of lead sulfite.

[0085] Example 3:

[0086] The negative and positive electrolytes of the flow battery in this embodiment are the same as those in Example 1, except that the lead sulfate in the solid-phase energy storage material is replaced with an equal mass of lead chloride.

[0087] Example 4:

[0088] The negative and positive electrolytes of the flow battery in this embodiment are the same as those in Example 1, except that the lead sulfate in the solid-phase energy storage material is replaced with an equal mass of lead bromide.

[0089] Example 5:

[0090] The negative and positive electrolytes of the flow battery in this embodiment are the same as those in Example 1, except that the lead sulfate in the solid-phase energy storage material is replaced with an equal mass of lead carbonate.

[0091] Example 6:

[0092] The negative and positive electrolytes of the flow battery in this embodiment are the same as those in Example 1, except that the lead sulfate in the solid-phase energy storage material is replaced with an equal mass of lead phosphate.

[0093] Example 7:

[0094] The negative and positive electrolytes of the flow battery in this embodiment are the same as those in Example 1, except that the lead sulfate in the solid-phase energy storage material is replaced with an equal mass of lead acetate.

[0095] Example 8:

[0096] The negative and positive electrolytes of the flow battery in this embodiment are the same as those in Example 1, except that the lead sulfate in the solid-phase energy storage material is replaced with an equal mass of lead powder (micron-sized lead powder with D50=5μm).

[0097] Example 9:

[0098] This embodiment relates to a flow battery with a solid-phase energy storage mechanism, and the preparation process of its solid-phase energy storage material is the same as in Embodiment 1. The only difference is that a lower concentration of electrolyte is used.

[0099] The initial negative electrode electrolyte consists of 0.8M trivalent vanadium ions, 0.2M trivalent chromium ions, 1.5M chloride ions, and 1.5M sulfate ions (including incompletely ionized bisulfate ions), with the remaining components being hydrogen ions to maintain charge balance.

[0100] The initial positive electrode electrolyte consists of 1.2M tetravalent vanadium ions, 0.1M trivalent chromium ions, 1.5M chloride ions, and 1.5M sulfate ions (including incompletely ionized bisulfate ions), with the remaining components being hydrogen ions to maintain charge balance.

[0101] Example 10:

[0102] The preparation method of the solid-phase energy storage material in this embodiment is the same as in Example 1. The only difference is in verifying the tolerance of the mixed acid system to high-concentration liquid-phase targeted ions:

[0103] The initial negative electrode electrolyte consists of 2.5M trivalent vanadium ions, 1.0M trivalent chromium ions, 4.5M chloride ions, and 4.5M sulfate ions (including incompletely ionized bisulfate ions), with the remaining components being hydrogen ions to maintain charge balance.

[0104] The initial positive electrode electrolyte consists of 2.5M tetravalent vanadium ions, 0.8M trivalent chromium ions, 4.0M chloride ions, and 4.5M sulfate ions (including incompletely ionized bisulfate ions), with the remaining components being hydrogen ions to maintain charge balance.

[0105] Example 11:

[0106] The preparation method of the solid-phase energy storage material in this embodiment is the same as in Embodiment 1. The only difference is that during the initial assembly of the flow battery, the negative electrode electrolyte is Cr. 3+ / Cr 2+ The assembly of mixed valence states verifies the self-initiation capability of the targeted electron transfer mechanism under homologous mixed valence states:

[0107] The initial negative electrode electrolyte consists of 1.5M trivalent vanadium ions, 0.25M trivalent chromium ions and 0.25M divalent chromium ions (a mixture with a total chromium concentration of 0.5M), 3M chloride ions and 3M sulfate ions (containing incompletely ionized bisulfate ions), with the remaining components being hydrogen ions to maintain charge balance.

[0108] The initial positive electrolyte was the same as in Example 1.

[0109] Example 12:

[0110] The preparation method of the solid-phase energy storage material in this embodiment is the same as in Embodiment 1. The only difference is that during the initial assembly of the flow battery, the negative electrode electrolyte is prepared at a concentration of V... 3+ / V 2+ With Cr 3+ / Cr 2+ Mixed valence state assembly:

[0111] The initial negative electrode electrolyte contains 1.0M trivalent vanadium ions and 0.5M divalent vanadium ions (total vanadium concentration 1.5M), as well as 0.3M trivalent chromium ions and 0.2M divalent chromium ions (total chromium concentration 0.5M), along with 2.8M chloride ions and 3.2M sulfate ions (including bisulfate ions), with the remainder being hydrogen ions.

[0112] The initial positive electrode electrolyte contains 1.5M tetravalent vanadium ions and 0.5M pentavalent vanadium ions (total vanadium 2.0M), 0.4M trivalent chromium ions, combined with 2.2M chloride ions and 3.0M sulfate ions (including incompletely ionized bisulfate ions), and the remaining components are hydrogen ions to maintain charge balance.

[0113] Example 13:

[0114] The electrolyte composition of this embodiment is the same as that in Example 1, except that: the solid-phase energy storage material lead sulfate, carbon powder and polyethylene resin are ball-milled at a mass ratio of 85:5:15 for 24 hours, and then hot-pressed at 150°C and 2 MPa for 20 hours to form a block solid energy storage material with a diameter of 10 mm and a thickness of 4 mm.

[0115] Example 14:

[0116] The electrolyte composition of this embodiment is the same as that in Example 1, except that: the solid-phase energy storage material lead sulfate, carbon powder and polyethylene resin are ball-milled for 24 hours at a mass ratio of 65:25:10, and then hot-pressed for 10 hours at 150°C and 1.5 MPa using a mold to form a block solid energy storage material with a diameter of 10 mm and a thickness of 4 mm.

[0117] Comparative Example 1:

[0118] The only difference between this comparative example and Example 1 is that no solid-phase energy storage material is prepared, and no solid-phase energy storage material is added to the negative electrode of the assembled battery.

[0119] Comparative Example 2:

[0120] The preparation method of the solid-phase energy storage material in this comparative example is the same as that in Example 1. The only difference is:

[0121] Initial negative electrode electrolyte: 1.5M trivalent vanadium ions, 0.5M trivalent chromium ions, 8M chloride ions, and the remaining components are hydrogen ions to maintain charge balance.

[0122] The initial positive electrode electrolyte consists of 2.0M tetravalent vanadium ions, 0.4M trivalent chromium ions, 8M chloride ions, and the remaining components are hydrogen ions to maintain charge balance.

[0123] Comparative Example 3:

[0124] The preparation method of the solid-phase energy storage material in this comparative example is the same as that in Example 3. The composition of the initial negative electrode electrolyte and the initial positive electrode electrolyte is the same as that in Comparative Example 2.

[0125] Single-cell tests were conducted on the solid-state energy storage materials and electrolyte configurations of the above embodiments and comparative examples. The test methods are as follows: using a 48cm... 2 A single cell was used as the power unit for charging and discharging. The positive and negative current collectors were hard graphite plates, the electrode material was carbon cloth, and the proton exchange membrane was Nafion 212. During single-cell testing, the initial positive electrode volume was set to 125 mL, the negative electrode volume to 100 mL, and 10 g of solid-phase material was added. The specific charge-discharge strategy was as follows: first, charging at 5A for 30 min, followed by charging at 1A to a cutoff voltage of 1.7V; then discharging at 5A for 30 min, followed by discharging at 1A to a cutoff voltage of 1V. The test results are shown in Table 1.

[0126] Table 1: Single-cell discharge capacity and operating status of the examples and comparative examples

[0127] Test results and mechanism analysis of the examples and comparative examples:

[0128] 1. The successful establishment of solid-state energy storage mechanisms and the widespread applicability of precursor materials

[0129] A comprehensive comparison of Examples 1-8 with Comparative Example 1 shows that, under the condition that the initial positive and negative electrode electrolyte compositions are exactly the same, the introduction of the solid-phase energy storage material prepared by this invention on the negative electrode side significantly improves the system discharge capacity (Ah) of the flow battery. Furthermore, the single cell operates stably during long-term cycling, completely overcoming the traditional bias that solid-phase materials are prone to dissolution and failure. Simultaneously, the internal horizontal comparison of Examples 1-8 further confirms that the negative electrode-targeted solid-phase reaction mechanism designed in this invention has excellent universality for various lead sources. Whether using lead-containing precursor compounds such as lead sulfate, lead sulfite, lead chloride, lead bromide, lead acetate, lead carbonate, or lead phosphate, or directly using micron-sized lead powder, the assembled single cells can successfully activate the dual-medium relay transfer mechanism and obtain high capacity values. Among them, Example 1, which uses lead sulfate precursor to prepare the solid-target material, exhibits the best performance, achieving an additional absolute capacity increase of 0.242 Ah in its single-cell test, making it the optimal solution of this invention.

[0130] 2. The innovative "mixed acid anion effect" mechanism for inhibiting the dissolution of solid materials and flow field blockage.

[0131] A detailed comparison of Examples 1-8 with Comparative Examples 2-3 highlights the irreplaceable crucial role of the specially formulated "sulfate-chloride ion" support electrolyte in this invention. In Comparative Examples 2 and 3, because the negative electrode electrolyte uses only chloride ions as the single anion, excessively high concentrations of free chloride ions strongly attack and etch the crystal lattice microstructure of the lead-based solid-phase energy storage material, causing the lead to exist as a soluble complex ion [PbCl4]. 2 - In its liquid phase, lead is released into the liquid. This "uncontrollable dissolution" not only causes the active lead to be lost with the flow of the negative electrode electrolyte, but the free lead is also very easy to re-precipitate and precipitate disorderly under specific conditions in the pipeline flow field or on the electrode surface, eventually leading to pipeline blockage and single cell failure.

[0132] Conversely, this embodiment of the invention introduces a high concentration of sulfate ions into the system to form a mixed anion system. Utilizing like-ion interactions and coordination competition, it not only thermodynamically suppresses the attack of chloride ions on the solid-phase lead framework but also strictly confines the originally free lead within the solid-state energy storage region. The supporting electrolyte of this mixed acid system ensures that the lead-based targeted energy storage material does not collapse or leak during multiple charge-discharge cycles, guaranteeing the long-term unobstructed flow of the circulating liquid channel and the absolute stability of the system operation.

[0133] 3. Extremely wide operating window: robustness with both concentration adaptability and coexistence of multiple valence states.

[0134] Further reference to the test results of Examples 9-12 and Example 13 reveals that the targeting mechanism disclosed in this invention is not limited to a specific concentration, but exhibits an extremely broad operating window. Tests show that the discharge capacity of the solid-phase system exhibits a highly positively correlated response with the gradient change in the total vanadium ion concentration in the negative electrode electrolyte, demonstrating that the system can flexibly customize its energy density by changing the ion concentration of the electrolyte according to actual application requirements.

[0135] Furthermore, the system of this invention exhibits extremely high tolerance for the redox valence states of the initial carrier ions (i.e., chromium ions in the negative electrode electrolyte): in the negative electrode electrolyte, regardless of whether pure trivalent chromium, divalent chromium, or a mixture of both is initially used, the targeting mechanism can be spontaneously activated (for example, when divalent chromium is initially present, some divalent chromium will immediately and preferentially reduce the lead-containing precursor, transforming itself into trivalent chromium and smoothly entering the liquid phase circulation track); similarly, for vanadium ions (V... 2+ V 3+ The same applies to batteries (or mixtures of both), which means that batteries can be assembled while charged or replenished midway through any state of charge (SOC).

[0136] More innovatively, this invention simultaneously incorporates a specific concentration of divalent / trivalent chromium into the positive electrode electrolyte (whether containing tetravalent vanadium, pentavalent vanadium, or a combination of both). This helps to counteract the parasitic osmotic pressure difference driven by the concentration difference of chromium ions on both sides of the proton exchange membrane, greatly suppressing the cross-permeation of active ions. This ensures capacity balance of the positive and negative electrolytes over an ultra-long lifespan at the physical membrane level. Furthermore, the proportions of the energy storage active material, conductive agent, and binder in the solid-phase energy storage material can be flexibly set. As long as appropriate pressing parameters are used, it can be ensured that the prepared solid-phase energy storage material does not disintegrate into fine particles or powder within the battery.

[0137] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features. These modifications or substitutions, or combinations of technical features in the above embodiments that do not conflict with each other, can be made in accordance with the manner described in the embodiments. These modifications, substitutions or combinations do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A flow battery with a solid-phase energy storage mechanism, characterized in that, The negative electrode system of the flow battery includes: a solid-phase energy storage material placed in an electrolyte circulation loop, and a flowable negative electrode electrolyte included in the circulation loop; Wherein: the solid-phase energy storage material contains an energy storage active substance, which is elemental lead and / or lead-based ionic compounds; the lead-based ionic compounds include lead sulfate, and lead-based compounds that can generate lead sulfate in situ through ion exchange or redox reactions, wherein the lead-based compounds are selected from one or more of lead sulfite, lead chloride, lead bromide, lead carbonate, lead phosphate, and lead acetate; when the energy storage active substance is a lead salt or elemental lead other than lead sulfate, after the battery is assembled and the negative electrode electrolyte is injected into the negative electrode system, the energy storage active substance in the solid-phase energy storage material can chemically react with the negative electrode electrolyte, causing the main phase structure of the energy storage active substance to be partially or completely converted into the lead sulfate phase; The negative electrode electrolyte contains total vanadium ions as redox electron carriers and total chromium ions as a targeting medium, as well as a supporting electrolyte solution composed of hydrogen ions and mixed anions. When the flow battery is in operation with any charge-discharge depth or in its initial formulation state: in the negative electrode electrolyte, the total vanadium ions exist in the form of divalent vanadium ions, trivalent vanadium ions, or any mixture of the two in any proportion; in the negative electrode electrolyte, the total chromium ions exist in the form of divalent chromium ions, trivalent chromium ions, or any mixture of the two in any proportion; the mixed anions are a combination of chloride ions and sulfate and / or hydrogen sulfate ions.

2. The flow battery with a solid-phase energy storage mechanism according to claim 1, characterized in that, The solid-phase energy storage material is a solid block, granular, or porous material with a spatial conductive network. It is a composite material obtained by mixing and molding energy storage active substances, conductive agents, and binders.

3. The flow battery with a solid-phase energy storage mechanism according to claim 1, characterized in that, The mass percentage range of the energy storage active material, conductive agent, and binder is: 60%–85%, 5%–30%, and 2%–15%, respectively; the conductive agent is a carbon-based conductive material; the binder is a thermoplastic or thermosetting acid-resistant polymer resin, including one or a mixture of several of polyethylene resin, polytetrafluoroethylene resin, polyvinylidene fluoride resin, Nafion resin, polypropylene resin, and acid-resistant epoxy resin.

4. The flow battery with a solid-phase energy storage mechanism according to claim 1, characterized in that, In the initial preparation state, the concentration range of each major component in the negative electrode electrolyte is as follows: the concentration of total vanadium ions is 0.5M-3.0M; the concentration of total chromium ions is 0.1M-1.5M; the concentration of chloride ions is 1.0M-3.0M; the sum of the concentrations of sulfate ions and bisulfate ions based on total sulfate groups is 1.0M-5.0M; and hydrogen ions are used to maintain electroneutrality and provide an acidic environment.

5. The flow battery with a solid-phase energy storage mechanism according to claim 4, characterized in that, The negative electrode electrolyte components in the initial preparation state include: trivalent vanadium ions at a concentration of 1.2M-1.8M, trivalent chromium ions at a concentration of 0.3M-0.8M, chloride ions at a concentration of 2.5M-3.5M, a collection of sulfate and bisulfate ions at a concentration of 2.5M-3.5M, and hydrogen ions for maintaining electroneutrality.

6. The flow battery with a solid-phase energy storage mechanism according to claim 4 or 5, characterized in that, The molar ratio of sulfate ions to chloride ions in the negative electrode electrolyte is 1-1.5:

1.

7. The flow battery with a solid-phase energy storage mechanism according to claim 1, characterized in that, The flow battery also includes a positive electrode system in which a positive electrode electrolyte is circulated. In the initial preparation state, the positive electrode electrolyte contains: 1.0M-3.0M tetravalent vanadium ions, 0.05M-1.0M chromium ions, 1.0M-5.0M chloride ions, sulfate ions and bisulfate ions with a total concentration of 1.0M-5.0M, and hydrogen ions to maintain electroneutrality and provide an acidic environment.

8. The flow battery with a solid-phase energy storage mechanism according to claim 7, characterized in that, In its initial preparation state, the positive electrode electrolyte contains 2.0 M tetravalent vanadium ions, 0.4 M trivalent chromium ions, 2.2 M chloride ions, sulfate ions and bisulfate ions with a total concentration of 3.0 M, and hydrogen ions to maintain electroneutrality.

Citation Information

Patent Citations

  • A high-capacity cathode electrolyte for all-vanadium redox flow batteries

    CN118299630B

  • Vanadium redox flow battery based on solid energy storage material and preparation method of vanadium redox flow battery

    CN118645668A

  • Multi-active material electrolyte and flow battery comprising same

    CN118016948A

  • Solid compatibilization material for negative electrode of vanadium redox flow battery and preparation method of solid compatibilization material

    CN122455806A

  • Redox flow battery

    JP2011233372A