A negative electrode sheet with a mesoporous material coating, its preparation method, and a lithium-ion battery.

By coating the negative electrode surface of a lithium-ion battery with a mesoporous material coating, the problems of high interfacial impedance and poor electrolyte wettability caused by ceramic coatings are solved, thereby improving the cycle stability and safety performance of the battery.

CN123073015APending Publication Date: 2026-11-10YANTAI LIHUA ELECTRIC POWER TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611151031.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-31
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing ceramic materials for lithium-ion battery anode coatings suffer from high interfacial impedance, poor electrolyte wettability, and insufficient cycle stability, leading to safety hazards and performance limitations.

Method used

A mesoporous material coating is used, which forms a coating with high specific surface area and abundant mesoporous channels by coating the surface of the negative electrode active material layer with mesoporous alumina or mesoporous silica. Combined with conductive carbon materials and binders, a stable SEI film and structural buffer layer are constructed.

Benefits of technology

It significantly improves the wetting rate and uniformity of the electrolyte, reduces interfacial impedance, improves the cycle performance and safety of the battery, and enhances the stability of the battery under high temperature and abuse conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073015A_ABST
    Figure CN123073015A_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of lithium-ion batteries, specifically relating to a negative electrode sheet with a mesoporous material coating, its preparation method, and a lithium-ion battery. The negative electrode sheet with a mesoporous material coating provided by this invention includes: a negative electrode current collector, a negative electrode active material layer, and a mesoporous material coating. The negative electrode active material layer is disposed on at least one surface of the negative electrode current collector, and the mesoporous material coating is disposed on the surface of the negative electrode active material layer away from the negative electrode current collector. The negative electrode sheet provided by this invention can reduce the interfacial impedance of the negative electrode sheet, improve electrolyte wettability, and enhance cycle performance. Simultaneously, due to the presence of the mesoporous material layer on the electrode sheet, micro-short circuits between the positive and negative electrodes can be avoided, reducing the cell's self-discharge rate and improving safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of lithium-ion batteries, specifically relating to a negative electrode sheet with a mesoporous material coating, its preparation method, and a lithium-ion battery. Background Technology

[0002] Lithium-ion batteries are widely used in portable electronic devices, electric vehicles, and energy storage systems due to their advantages such as high voltage, high specific energy, long cycle life, and good safety performance. The performance of lithium-ion batteries largely depends on factors such as electrode structure and the interface state between the electrolyte and the electrodes. Existing research shows that coating the negative electrode surface with an alumina ceramic coating can improve the battery's rate performance and cycle performance; for example, after coating the negative electrode surface with a ceramic coating, the capacity retention rate can reach 88.6% after 500 cycles. Furthermore, coating the separator surface with a nano-alumina film can also improve the safety of lithium-ion batteries.

[0003] However, the ceramic materials used for negative electrode coatings in existing technologies (such as boehmite, alumina, magnesium oxide, titanium dioxide, etc.) are mostly dense or ordinary porous structures, which still have the following shortcomings in improving battery performance: (i) High interfacial impedance: The introduction of inorganic ceramic anode coatings leads to an increase in interfacial impedance, which can easily cause lithium plating during later charge and discharge processes, posing a safety hazard. Ordinary ceramic coatings lack ordered ion transport channels, hindering the migration of lithium ions within the coating and significantly increasing the interfacial charge transfer impedance.

[0004] (ii) Poor electrolyte wettability: The introduction of inorganic ceramic anode coatings often results in poor electrolyte wettability on the anode, extending the required settling time after cell filling. Ordinary ceramic coatings have limited electrolyte retention capacity, making it difficult to form efficient ion conduction pathways, thus restricting the battery's rate performance.

[0005] (III) Cyclic stability needs to be improved: Although existing ceramic coatings can extend cycle life to a certain extent, the stability of the coating structure and its protective effect on the SEI film during long-term cycling are still not ideal, and the capacity decay accelerates in the later stage of cycling.

[0006] Therefore, it is necessary to provide a novel negative electrode coating structure that can effectively reduce interfacial impedance, improve electrolyte wettability, and significantly enhance cycle stability and safety performance, in order to overcome the aforementioned defects of the existing technology. Summary of the Invention

[0007] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, embodiments of this invention provide a negative electrode sheet with a mesoporous material coating, its preparation method, and its application.

[0008] The negative electrode sheet with a mesoporous material coating according to an embodiment of the present invention includes: a negative electrode current collector, a negative electrode active material layer and a mesoporous material coating, wherein the negative electrode active material layer is disposed on at least one surface of the negative electrode current collector, and the mesoporous material coating is disposed on the surface of the negative electrode active material layer away from the negative electrode current collector.

[0009] The advantages and technical effects of the negative electrode sheet with mesoporous material coating in this invention are as follows: 1. In this invention, the high specific surface area and abundant mesoporous channels of the mesoporous material endow the coating with extremely strong capillary adsorption capacity, which can effectively adsorb and store electrolyte, forming a durable solid-liquid interface. This significantly improves the wetting speed and uniformity of the electrolyte on the negative electrode sheet, shortens the standing time after electrolyte injection, and reduces battery manufacturing costs; 2. In this invention, the electrolyte adsorbed by the mesoporous material coating can form a more uniform and stable SEI film, reducing the irreversible consumption of active lithium ions and alleviating the bulk density of the negative electrode active material during long-term cycling. The expansion of the material can damage the SEI film; in addition, the mesoporous material coating itself can act as a structural buffer layer, effectively dispersing and buffering the internal stress generated by the electrode during repeated charging and discharging, and improving the cycle performance of the battery; 3. In the embodiments of the present invention, the electrolyte loaded in the mesoporous material coating can form a more stable solid-liquid interface under abusive conditions such as high temperature or overcharging, inhibiting the thermal decomposition of the electrolyte and the occurrence of side reactions; the mesoporous material itself has good thermal stability and mechanical strength, and can still maintain good structural integrity under high temperature conditions, which can effectively prevent the occurrence of internal short circuits. After adopting the mesoporous material coating, the battery performs better in safety tests such as nail penetration and thermal abuse.

[0010] In some embodiments, the thickness of the negative electrode active material layer is 100~150 μm; the thickness of the mesoporous material coating is 0.5~5 μm.

[0011] In some embodiments, the mass fraction of the mesoporous material in the mesoporous material coating is 40-80 wt%.

[0012] In some embodiments, the mesoporous material includes at least one of mesoporous alumina or mesoporous silica, wherein the pore size of the mesoporous material is 2-50 nm; and the specific surface area of ​​the mesoporous alumina is 150-450 m² / g. 2 / g, wherein the specific surface area of ​​the mesoporous silica is 200~600m². 2 / g.

[0013] In some embodiments, the mesoporous material coating further comprises a conductive carbon material and a first binder. The conductive carbon material includes at least one of carbon nanotubes, conductive carbon black, or graphene, with a mass fraction of 3-10 wt%. The first binder includes at least one of vinylidene fluoride, polyvinylidene fluoride, a homopolymer of vinylidene fluoride, a copolymer of polyvinylidene fluoride, carboxymethyl cellulose, polyacrylic acid, polyacrylonitrile, polyacrylamide, styrene-butadiene rubber, or styrene-acrylic rubber, with a mass fraction of 40-50%.

[0014] In some embodiments, the negative electrode active material layer comprises a negative electrode active material, a conductive agent, and a second binder.

[0015] In some embodiments, the negative electrode active material includes at least one of graphite, silicon-carbon composite material, or silicon-oxygen composite material; And / or, the conductive agent includes at least one of carbon nanotubes, conductive carbon black, or graphene; And / or, the second adhesive comprises at least one of carboxymethyl cellulose, polyacrylic acid, polyacrylonitrile, polyacrylamide, styrene-butadiene rubber, or styrene-acrylic rubber.

[0016] In some embodiments, the negative current collector is selected from either copper foil or carbon-coated copper foil.

[0017] This invention also provides a method for preparing the above-mentioned negative electrode sheet with a mesoporous material coating, characterized by comprising the following steps: (1) The negative electrode active material, conductive agent, second binder and solvent are mixed evenly in proportion and coated on at least one surface of the negative electrode current collector. After drying, a negative electrode active material layer is obtained. (2) After the mesoporous material, the first binder, the conductive carbon material and the solvent are mixed evenly in proportion, they are coated on the surface of the negative electrode active material layer and dried to obtain the mesoporous material coating.

[0018] This invention also provides a lithium-ion battery, comprising the above-described negative electrode sheet and the negative electrode sheet, positive electrode sheet, separator, and electrolyte prepared by the above-described preparation method. Attached Figure Description

[0019] Figure 1 This is a schematic diagram of the negative electrode sheet according to an embodiment of the present invention; Among them, 1-negative electrode current collector, 2-negative electrode active material layer, 3-mesoporous material coating. Detailed Implementation

[0020] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0021] like Figure 1 As shown, the negative electrode sheet with a mesoporous material coating according to an embodiment of the present invention includes: a negative electrode current collector, a negative electrode active material layer and a mesoporous material coating, wherein the negative electrode active material layer is disposed on at least one surface of the negative electrode current collector, and the mesoporous material coating is disposed on the surface of the negative electrode active material layer away from the negative electrode current collector.

[0022] The advantages and technical effects of the negative electrode sheet with mesoporous material coating in this invention are as follows: 1. In this invention, the high specific surface area and abundant mesoporous channels of the mesoporous material endow the coating with extremely strong capillary adsorption capacity, which can effectively adsorb and store electrolyte, forming a durable solid-liquid interface. This significantly improves the wetting speed and uniformity of the electrolyte on the negative electrode sheet, shortens the standing time after electrolyte injection, and reduces battery manufacturing costs; 2. In this invention, the electrolyte adsorbed by the mesoporous material coating can form a more uniform and stable SEI film, reducing the irreversible consumption of active lithium ions and alleviating the bulk density of the negative electrode active material during long-term cycling. The expansion of the material can damage the SEI film; in addition, the mesoporous material coating itself can act as a structural buffer layer, effectively dispersing and buffering the internal stress generated by the electrode during repeated charging and discharging, and improving the cycle performance of the battery; 3. In the embodiments of the present invention, the electrolyte loaded in the mesoporous material coating can form a more stable solid-liquid interface under abusive conditions such as high temperature or overcharging, inhibiting the thermal decomposition of the electrolyte and the occurrence of side reactions; the mesoporous material itself has good thermal stability and mechanical strength, and can still maintain good structural integrity under high temperature conditions, which can effectively prevent the occurrence of internal short circuits. After adopting the mesoporous material coating, the battery performs better in safety tests such as nail penetration and thermal abuse.

[0023] In some embodiments, preferably, the thickness of the negative electrode active material layer is 100~150 μm, such as 100μm, 120μm, 130μm, 140μm or 150μm; the thickness of the mesoporous material coating is 0.5~5μm, such as 0.5μm, 1μm, 2μm, 3μm, 4μm or 5μm.

[0024] In this embodiment of the invention, the thickness of the mesoporous material coating is preferred. If the mesoporous material coating is too thin, it cannot form a complete and uniform coverage on the surface of the negative electrode active material, causing some active areas to be directly exposed to the electrolyte, making it difficult to effectively suppress the occurrence of side reactions. At the same time, an excessively thin coating is very easy to crack due to the volume expansion of the active material during charging and discharging, and cannot play a continuous physical isolation and protection role, so the effect of improving wetting and enhancing safety performance is not obvious. If the mesoporous material coating is too thick, it will significantly increase the diffusion resistance of lithium ions, hindering the normal insertion and extraction of lithium ions at the interface of the active material, resulting in increased battery polarization and decreased rate performance. At the same time, an excessively thick ceramic layer will occupy the limited internal space of the electrode, reducing the overall volumetric energy density of the cell, and is more prone to cracking or peeling off due to excessive internal stress during the drying process.

[0025] In some embodiments, preferably, the mass fraction of the mesoporous material in the mesoporous material coating is 40-80 wt%, such as 40 wt%, 50 wt%, 60 wt%, 70 wt%, or 80 wt%.

[0026] In this embodiment of the invention, the content of mesoporous material in the mesoporous material coating is preferred. If the content of mesoporous material is too low, the proportion of functional mesoporous components in the coating is insufficient, making it difficult to form a continuous and effective three-dimensional porous network structure. This results in limited improvement in electrolyte retention capacity and ion conduction capacity, and the effect of improving wetting and cycle performance is not significant. At the same time, a low content means that the proportion of auxiliary materials such as binders or conductive agents is relatively increased. These auxiliary materials may block some mesoporous channels or increase the risk of interfacial side reactions, which weakens the original advantages of mesoporous materials. If the content of mesoporous material is too high, the content of binder in the coating is relatively insufficient, resulting in a significant decrease in the bonding force between the ceramic layer and the negative electrode active material layer. During charging and discharging, the coating is prone to cracking, powdering, or even falling off due to the volume expansion of the active material. At the same time, an excessively high proportion of ceramic will increase the brittleness of the coating, and powder shedding and edge damage are easy to occur during processing (such as rolling and slitting), which seriously deteriorates the cycle life and safety performance of the battery.

[0027] In some embodiments, preferably, the mesoporous material comprises at least one of mesoporous alumina or mesoporous silica; the pore size of the mesoporous material is 2-50 nm, and the specific surface area of ​​the mesoporous alumina is 150-450 m² / g. 2 / g, wherein the specific surface area of ​​the mesoporous silica is 200~600m². 2 / g.

[0028] In this embodiment of the invention, the mesoporous alumina and mesoporous silica used possess ordered pore structures and high specific surface areas, with pore sizes ranging from 2 to 50 nm, providing a fast and unobstructed transport channel for lithium ions. The diffusion path of lithium ions in the mesoporous coating is more ordered and exhibits less resistance, significantly reducing interfacial charge transfer impedance, thereby effectively improving rate performance and low-temperature performance. In contrast, existing nano-dense alumina coatings, due to the lack of ordered pores, often result in a significant increase in internal resistance.

[0029] In some embodiments, preferably, the mesoporous material coating further comprises a conductive carbon material, the conductive carbon material including at least one of carbon nanotubes, conductive carbon black or graphene, with a mass fraction of 3 to 10 wt%.

[0030] In this embodiment of the invention, conductive carbon material is added to the mesoporous material coating to construct a conductive network, improve the electronic conductivity of the electrode, reduce polarization, and improve rate performance. The preferred content of the conductive carbon material is 3-10 wt%, which achieves the best balance between electronic conductivity, ion conductivity, and coating structural stability. If the content of the conductive carbon material is too low, it will be detrimental to forming a continuous and effective conductive pathway in the mesoporous coating, and the effect of improving conductivity will not be significant. If the content of the conductive carbon material is too high, excessive conductive carbon material will block the mesoporous channels, hinder lithium-ion transport, weaken the function of the mesoporous material in improving wetting and stabilizing the interface, and may deteriorate the mechanical properties of the coating.

[0031] In some embodiments, preferably, the mesoporous material coating further comprises a first binder, the first binder comprising at least one of vinylidene fluoride, polyvinylidene fluoride, a homopolymer of vinylidene fluoride, a copolymer of polyvinylidene fluoride, carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyacrylonitrile (PAN), polyacrylamide (PAM), styrene-butadiene rubber (SBR), or styrene-acrylic rubber (commonly referred to as styrene-acrylic SBR), with a mass fraction of 40-50%.

[0032] In some embodiments, preferably, the negative electrode active material layer comprises a negative electrode active material, a conductive agent, and a second binder.

[0033] In some embodiments, preferably, the negative electrode active material includes at least one of graphite, silicon-carbon composite material, or silicon-oxygen composite material; And / or, the conductive agent includes at least one of carbon nanotubes, conductive carbon black, or graphene; And / or, the second adhesive comprises at least one of carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyacrylonitrile (PAN), polyacrylamide (PAM), styrene-butadiene rubber (SBR), or styrene-acrylic rubber.

[0034] In some embodiments, preferably, the negative current collector is selected from either copper foil or carbon-coated copper foil.

[0035] This invention also provides a method for preparing the above-mentioned negative electrode sheet with a mesoporous material coating, characterized by comprising the following steps: (1) The negative electrode active material, conductive agent, second binder and solvent are mixed evenly in proportion and coated on at least one surface of the negative electrode current collector. After drying, a negative electrode active material layer is obtained. (2) After the mesoporous material, the first binder, the conductive carbon material and the solvent are mixed evenly in proportion, they are coated on the surface of the negative electrode active material layer and dried to obtain the mesoporous material coating.

[0036] This invention also provides a lithium-ion battery, comprising the above-described negative electrode sheet and the negative electrode sheet, positive electrode sheet, separator, and electrolyte prepared by the above-described preparation method.

[0037] The technical solution of the present invention will now be described in detail with reference to specific embodiments and accompanying drawings.

[0038] Example 1 (1) A slurry with a solid content of 46% was prepared by mixing graphite anode active material (94.5% by mass), conductive carbon black (2.0% by mass), CMC binder (1.5% by mass), SBR binder (2% by mass) and deionized water as solvent. After being mixed evenly, the slurry was coated on the surface of a copper foil anode current collector with a thickness of 6 μm. After drying, a layer of anode active material with a thickness of 115 μm was obtained. (2) Mesoporous alumina powder (pore size distribution range of 3~10 nm, average pore size of 6 nm, BET specific surface area of ​​260 m² / g, mass fraction of 40%), SBR binder (mass fraction of 45%) and conductive carbon black (mass fraction of 5%) were dispersed in deionized H2O (mass fraction of 10%) solvent and coated on the surface of the negative electrode active material layer. After drying, a mesoporous material coating with a thickness of 2.0 μm was obtained.

[0039] Example 2 The preparation method of this embodiment is the same as that of Example 1, except that in step (2), the mesoporous material is composed of mesoporous alumina and mesoporous silica in a mass ratio of 1:1, wherein the pore size of the mesoporous alumina is 3~8nm and the BET specific surface area is 230m² / g; the pore size of the mesoporous silica is 5~12nm and the BET specific surface area is 350m² / g, and the thickness of the mesoporous material coating is 2.5μm.

[0040] Example 3 The preparation method of this embodiment is the same as that of Example 1, except that: in step (2), conductive carbon black is not added, and the mass fraction of mesoporous alumina powder is 45%; the mass fraction of SBR binder is 40%; and the mass fraction of deionized H2O is 15%.

[0041] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is that the negative electrode sheet is not coated with a mesoporous material coating, while the other conditions are exactly the same as in Example 1.

[0042] Comparative Example 2 A slurry with a solid content of 46% was prepared by mixing graphite anode active material (92.5% by mass), conductive carbon black (2.0% by mass), CMC binder (1.5% by mass), SBR binder (2% by mass), and 2% by mass of mesoporous alumina powder (pore size distribution range of 3~10 nm, average pore size of 6 nm, BET specific surface area of ​​260 m² / g) and deionized water. After uniform mixing, the slurry was coated on the surface of a copper foil anode current collector with a thickness of 6 μm. After drying, a layer of anode active material with a thickness of 115 μm was obtained.

[0043] The negative electrode sheets prepared in Examples 1-3 and Comparative Examples 1-2 were assembled with lithium iron phosphate positive electrode sheets, PE separators, and LiPF6 / EC+DEC electrolytes to form soft-pack lithium-ion batteries, and their electrochemical performance was tested. A 1000-cycle test was conducted at 1.0 C rate, and the results are shown in Table 1.

[0044] Table 1

[0045] As can be seen from the data in Table 1, compared with Comparative Example 1, the mesoporous material coatings provided in Examples 1 and 2 of the present invention significantly reduced the DCR of the battery cell from 4.23 mΩ to 2.91 mΩ and 2.85 mΩ, respectively, representing reductions of 31% and 32.6%. The contact angle of the electrolyte decreased from 36.5° to 18.2° and 17.6°, respectively, greatly improving electrolyte wettability. The cycle life was increased by approximately 11 percentage points, and the growth rate of DCR during cycling was significantly reduced. The needle penetration safety performance was also significantly enhanced. In Example 3, because the mesoporous material coating lacks conductive carbon material, the cell's DCR (Displacement Rate) slightly increases compared to Examples 1 and 2. However, compared to Comparative Example 1, the DCR is still 19.6% lower, and the electrolyte contact angle is reduced, indicating a positive improvement in wetting and needle penetration resistance. Compared to Comparative Example 1, Example 3's insufficient DCR reduction leads to accelerated cycle performance degradation, demonstrating that adding a conductive agent to the mesoporous material significantly improves conductivity and cycle performance. Comparative Example 2 adds the mesoporous material to the negative electrode active layer. Compared to Example 1, the contact angle and DCR increase, with the contact angle increasing by 85.7% and the DCR by 29%, while needle penetration performance remains largely unchanged. In contrast, the solution of this invention significantly improves both electrical performance and safety performance.

[0046] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0047] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.

Claims

1. A negative electrode sheet with a mesoporous material coating, characterized in that, include: The present invention comprises a negative electrode current collector, a negative electrode active material layer, and a mesoporous material coating, wherein the negative electrode active material layer is disposed on at least one surface of the negative electrode current collector, and the mesoporous material coating is disposed on the surface of the negative electrode active material layer away from the negative electrode current collector.

2. The negative electrode sheet with a mesoporous material coating according to claim 1, characterized in that, The thickness of the negative electrode active material layer is 100~150 μm; the thickness of the mesoporous material coating is 0.5~5 μm.

3. The negative electrode sheet with a mesoporous material coating according to claim 1, characterized in that, The mass fraction of the mesoporous material in the mesoporous material coating is 40~80wt%.

4. The negative electrode sheet with a mesoporous material coating according to claim 3, characterized in that, The mesoporous material includes at least one of mesoporous alumina or mesoporous silica, wherein the pore size of the mesoporous material is 2-50 nm; and the specific surface area of ​​the mesoporous alumina is 150-450 m². 2 / g, wherein the specific surface area of ​​the mesoporous silica is 200~600m². 2 / g.

5. The negative electrode sheet with a mesoporous material coating according to claim 1, characterized in that, The mesoporous material coating also includes conductive carbon material and a first binder; The conductive carbon material includes at least one of carbon nanotubes, conductive carbon black, or graphene, with a mass fraction of 3-10 wt%. The first adhesive comprises at least one of vinylidene fluoride, polyvinylidene fluoride, a homopolymer of vinylidene fluoride, a copolymer of polyvinylidene fluoride, carboxymethyl cellulose, polyacrylic acid, polyacrylonitrile, polyacrylamide, styrene-butadiene rubber, or styrene-acrylic rubber, with a mass fraction of 40-50%.

6. The negative electrode sheet with a mesoporous material coating according to claim 1, characterized in that, The negative electrode active material layer includes a negative electrode active material, a conductive agent, and a second binder.

7. The negative electrode sheet with a mesoporous material coating according to claim 6, characterized in that, The negative electrode active material includes at least one of graphite, silicon-carbon composite material, or silicon-oxygen composite material; And / or, the conductive agent includes at least one of carbon nanotubes, conductive carbon black, or graphene; And / or, the second adhesive comprises at least one of carboxymethyl cellulose, polyacrylic acid, polyacrylonitrile, polyacrylamide, styrene-butadiene rubber, or styrene-acrylic rubber.

8. The negative electrode sheet with a mesoporous material coating according to claim 1, characterized in that, The negative electrode current collector is selected from either copper foil or carbon-coated copper foil.

9. A method for preparing a negative electrode sheet with a mesoporous material coating according to any one of claims 1 to 8, characterized in that, Includes the following steps: (1) The negative electrode active material, conductive agent, second binder and solvent are mixed evenly in proportion and coated on at least one surface of the negative electrode current collector. After drying, a negative electrode active material layer is obtained. (2) After the mesoporous material, the first binder, the conductive carbon material and the solvent are mixed evenly in proportion, they are coated on the surface of the negative electrode active material layer and dried to obtain the mesoporous material coating.

10. A lithium-ion battery, characterized in that, Includes the negative electrode sheet according to any one of claims 1 to 8 or the negative electrode sheet, positive electrode sheet, separator and electrolyte prepared by the preparation method according to claim 9.