A lithium battery cathode slurry and its preparation method
By using microencapsulated flame retardants in the positive electrode slurry of lithium batteries, a composite material containing phosphazene flame retardants and boehmite is used to solve the risk of thermal runaway of lithium batteries under extreme conditions, thus improving safety while maintaining the electrochemical performance of the battery.
Patent Information
- Application Number
- CN202611158099.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-10
AI Technical Summary
Existing lithium battery cathode slurries pose a high risk of thermal runaway under extreme conditions, and existing flame retardants affect the battery's electrochemical performance and have not effectively solved battery safety issues.
Microencapsulated flame retardants are used, including phosphazene flame retardants, cage-type polysilsesquioxane and boehmite as core materials, which are encapsulated in a polymer shell. The resulting microencapsulated flame retardant is combined with ternary materials and lithium manganese iron phosphate. By controlling the release of the flame retardant, thermal runaway can be suppressed under extreme conditions.
Without affecting the normal electrochemical performance of the battery, it significantly improves the safety performance of lithium batteries, effectively suppresses thermal runaway, and enhances the flame retardant performance of the battery.
Smart Images

Figure CN123073016A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery technology, specifically to a lithium battery cathode slurry and its preparation method. Background Technology
[0002] Lithium-ion batteries are widely used in consumer electronics, electric vehicles, and energy storage power stations due to their advantages such as high energy density, high operating voltage, and long cycle life. With the rapid development of electric vehicles and energy storage systems, the safety issues of lithium-ion batteries are becoming increasingly prominent. In particular, batteries are prone to thermal runaway under extreme conditions such as puncture, impact, overcharging, and overheating, which can lead to combustion or even explosion accidents.
[0003] Currently, flame retardants are often added to the electrolyte to improve the safety of lithium-ion batteries. However, adding flame retardants to the electrolyte affects ionic conductivity and battery performance, thereby degrading the battery's rate performance and cycle stability. On the other hand, ternary materials such as lithium nickel cobalt manganese oxide have the advantage of high energy density, but their thermal stability is poor; lithium manganese iron phosphate has excellent thermal stability and safety performance, but its electronic conductivity is low. Combining ternary materials with lithium manganese iron phosphate can balance energy density and safety to a certain extent, but existing composite cathode slurries rely solely on the performance optimization of the active materials themselves and do not specifically address the flame retardancy and heat suppression issues under extreme operating conditions, leaving the risk of battery thermal runaway still relatively high. Furthermore, the current method of directly doping flame retardant components into the cathode system can easily cause side reactions between the flame retardant and the electrode and electrolyte, damaging the electrode conductive network and sacrificing the battery's electrochemical performance. Therefore, developing a cathode slurry that maintains good electrochemical performance and has efficient flame retardant properties, along with its preparation method, has significant practical significance and application value. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of the prior art by providing a lithium battery positive electrode slurry. This slurry exhibits excellent electrochemical and flame-retardant properties, contributing to improved battery safety. Furthermore, the preparation method of this lithium battery positive electrode slurry is convenient to control, highly efficient, and conducive to industrial production.
[0005] The objective of this invention is achieved through the following technical solution: a lithium battery positive electrode slurry, comprising the following raw materials in parts by weight: 60-100 parts of ternary material, 5-30 parts of lithium manganese iron phosphate, 0.5-5 parts of conductive carbon black, 0.5-5 parts of carbon nanotubes, 3-10 parts of microencapsulated flame retardant, and 0.5-5 parts of binder.
[0006] Furthermore, the microencapsulated flame retardant includes a core material and a shell material covering the surface of the core material. The core material contains phosphazene flame retardants, cage-type polysilsesquioxane, and boehmite, and the shell material is a high molecular polymer material.
[0007] Furthermore, the weight ratio of the core material to the shell material in the microencapsulated flame retardant is 1.5-3:1.
[0008] Furthermore, the weight ratio of the phosphazene flame retardant, the cage-type polysilsesquioxane, and the boehmite is 1-3:1:1-3.
[0009] Furthermore, the phosphazene flame retardant is at least one of ethoxy(pentafluoro)cyclotriphosphazene, (phenoxy)pentafluorocyclotriphosphazene, (trifluoroethoxy)pentafluorocyclotriphosphazene, hexachlorocyclotriphosphazene, hexaphenoxycyclotriphosphazene, and hexafluorocyclotriphosphazene.
[0010] Furthermore, the cage-type polysilsesquioxane is at least one of epoxy-functionalized cage-type polysilsesquioxane, amino-functionalized cage-type polysilsesquioxane, and phenyl cage-type polysilsesquioxane.
[0011] This invention uses a microcapsule core material composed of phosphazene flame retardants, cage-like polysilsesquioxane, and boehmite, distributed within a shell formed of a polymer material. The well-coordinated composition of these raw materials contributes to improved flame retardant performance of the positive electrode slurry. Specifically, the cage-like polysilsesquioxane decomposes upon heating to form a dense protective layer, providing a barrier effect against heat and oxygen. Boehmite decomposes upon heating to release water vapor, which lowers the surface temperature of the material through an endothermic reaction, while the resulting alumina coating further isolates oxygen. Within the normal operating temperature range of the battery, the microcapsule shell structure remains intact, and the phosphazene flame retardants, cage-like polysilsesquioxane, and boehmite are encapsulated within the capsule, preventing interaction with the electrolyte, positive electrode active material, or conductive agent. The shell material, composed of melamine-urea-formaldehyde resin and polymethyl methacrylate, allows for timely release of the flame retardant in the event of thermal runaway, ensuring the microcapsule flame retardant maintains its flame-retardant function while minimizing its impact on battery cycle performance and rate performance.
[0012] Furthermore, the shell material is at least one of melamine-urea-formaldehyde resin, urea-formaldehyde resin, polyurea, polyurea-formaldehyde, and polymethyl methacrylate.
[0013] Preferably, the shell material is composed of melamine-urea-formaldehyde resin and polymethyl methacrylate in a weight ratio of 1-3:1.
[0014] In this invention, the shell material can be a composite of melamine-urea-formaldehyde resin and polymethyl methacrylate (PMMA). Melamine-urea-formaldehyde resin has high cross-linking density and rigidity, forming a dense protective shell layer on the core material surface to prevent premature leakage of the flame retardant under normal operating conditions. PMMA, as the flexible component of the shell material, effectively improves the interfacial compatibility between the shell material and the electrolyte. By using a composite of melamine-urea-formaldehyde resin and PMMA, the shell material can withstand the mechanical shearing during electrode processing without premature breakage, and can also soften and break in the early stages of thermal runaway, allowing for controlled release of the internal flame-retardant components. This ensures that the microencapsulated flame retardant has minimal impact on the battery's cycle performance and rate performance while maintaining its flame-retardant function.
[0015] Furthermore, the ternary material is lithium nickel cobalt manganese oxide, with the chemical formula LiNi. 1-x-y Co x Mn y O2, where 0 < x < 1, 0 < y < 1, x + y < 1.
[0016] Furthermore, the adhesive is polyvinylidene fluoride.
[0017] Furthermore, the preparation method of the microencapsulated flame retardant includes the following steps: A1. Add phosphazene flame retardant, cage-type polysilsesquioxane, boehmite, emulsifier and deionized water to the reaction vessel, and emulsify under stirring to form an emulsion; A2. Add shell material to the emulsion and stir to mix evenly; A3. Under stirring conditions, heat the reaction system to 55-65℃, add curing agent, and react for 3.5-4.5 hours to form a coating layer on the surface of the core material. A4. After the reaction is complete, the microencapsulated flame retardant is obtained by washing, filtering and vacuum drying.
[0018] Further, in step A1, by weight, 3-7 parts of phosphazene flame retardant, 2-3.5 parts of cage-type polysilsesquioxane, 3-5 parts of boehmite, 1-2 parts of emulsifier, and 50-60 parts of deionized water are added to the reaction vessel and emulsified under stirring to form an emulsion; the emulsifier may be sodium dodecyl sulfate.
[0019] Further, in step A3, the reaction system is heated to 55-65°C under stirring conditions, 0.1-1 parts of curing agent are added, and the reaction is carried out for 3.5-4.5 hours to form a coating layer on the surface of the core material using the shell material; the curing agent can be ammonium chloride.
[0020] This invention also provides a method for preparing a lithium battery cathode slurry, comprising the following steps: (1) Dissolve the adhesive in a solvent and stir until homogeneous to obtain an adhesive solution; (2) Add conductive carbon black and carbon nanotubes to the adhesive solution and stir evenly to obtain conductive slurry; (3) Add ternary materials and lithium manganese iron phosphate to the conductive slurry, stir evenly, and obtain a mixed slurry of active materials; (4) Add the flame retardant mixture formed by pre-mixing microencapsulated flame retardant and solvent to the active material mixture slurry, stir evenly, and obtain the positive electrode slurry.
[0021] The beneficial effects of this invention are as follows: The positive electrode slurry of this invention combines ternary materials, lithium manganese iron phosphate, conductive carbon black, carbon nanotubes, binders, and other raw materials, and adds a microencapsulated flame retardant. This results in a positive electrode slurry with excellent electrochemical and flame-retardant properties. During normal battery operation, the flame retardant is encapsulated within the capsule, minimizing its impact on electrochemical performance. In cases of puncture or overheating, the capsule ruptures, releasing the flame retardant to prevent electrolyte combustion, thereby effectively improving battery safety. The preparation method of the lithium battery positive electrode slurry is convenient to control, highly efficient in production, and conducive to industrial production. Attached Figure Description
[0022] Figure 1 This is a comparison chart of the discharge specific capacity of Embodiment 1 and Comparative Example 1 at different rates.
[0023] Figure 2 This is a graph comparing the capacity retention rates of lithium-ion batteries from Example 1 and Comparative Example 1 during 500 charge-discharge cycles.
[0024] Figure 3 This is a comparison of the temperature-time curves of lithium-ion batteries in Example 1 and Comparative Examples 2-3 of the present invention during the nail penetration test. Detailed Implementation
[0025] To facilitate understanding by those skilled in the art, the present invention will be further described below with reference to embodiments. The content mentioned in the embodiments is not intended to limit the present invention.
[0026] In some embodiments of the present invention, a lithium battery cathode slurry comprises the following raw materials in parts by weight: 60-100 parts of ternary material, 5-30 parts of lithium manganese iron phosphate, 0.5-5 parts of conductive carbon black, 0.5-5 parts of carbon nanotubes, 3-10 parts of microencapsulated flame retardant, and 0.5-5 parts of binder.
[0027] In some embodiments of the present invention, the microencapsulated flame retardant includes a core material and a shell material covering the surface of the core material. The core material contains a phosphazene flame retardant, cage-type polysilsesquioxane, and boehmite (AlOOH), and the shell material is a polymer material.
[0028] In some embodiments of the present invention, the weight ratio of the core material to the shell material in the microencapsulated flame retardant is 1.5-3:1.
[0029] In some embodiments of the present invention, the weight ratio of the phosphazene flame retardant, the cage-like polysilsesquioxane, and boehmite is 1-3:1:1-3. The particle size of the boehmite is 0.1-0.5 μm.
[0030] In some embodiments of the present invention, the phosphazene flame retardant is at least one selected from ethoxy(pentafluoro)cyclotriphosphazene, (phenoxy)pentafluorocyclotriphosphazene, (trifluoroethoxy)pentafluorocyclotriphosphazene, hexachlorocyclotriphosphazene, hexaphenoxycyclotriphosphazene, and hexafluorocyclotriphosphazene.
[0031] In some embodiments of the present invention, the cage-like polysilsesquioxane is at least one of epoxy-functionalized cage-like polysilsesquioxane, amino-functionalized cage-like polysilsesquioxane, and phenyl cage-like polysilsesquioxane.
[0032] In some embodiments of the present invention, the shell material is at least one selected from melamine-urea-formaldehyde resin (MUF), urea-formaldehyde resin, polyurea, polyurea-formaldehyde, and polymethyl methacrylate.
[0033] In some embodiments of the present invention, the shell material is composed of melamine-urea-formaldehyde resin and polymethyl methacrylate in a weight ratio of 1-3:1.
[0034] In some embodiments of the present invention, the melamine-urea-formaldehyde cocondensation resin is made of melamine, urea and formaldehyde in a molar ratio of 1:1-3:4-8.
[0035] In some embodiments of the present invention, the preparation method of the melamine-urea-formaldehyde cocondensation resin includes the following steps: mixing melamine, urea and formaldehyde in a molar ratio, adjusting the pH to 7.5-8, and reacting at 70-80°C for 1-2 hours to obtain the melamine-urea-formaldehyde cocondensation resin.
[0036] In some embodiments of the present invention, the polymethyl methacrylate is prepared from methyl methacrylate monomers and has a weight-average molecular weight of 50,000 to 500,000.
[0037] In some embodiments of the present invention, the ternary material is lithium nickel cobalt manganese oxide, with the chemical formula LiNi. 1-x- y Co x Mn y O2, where 0 < x < 1, 0 < y < 1, x + y < 1.
[0038] In some embodiments of the present invention, the adhesive is polyvinylidene fluoride (PVDF).
[0039] In some embodiments of the present invention, the preparation method of the microencapsulated flame retardant includes the following steps: A1. By weight, add 3-7 parts of phosphazene flame retardant, 2-3.5 parts of cage-type polysilsesquioxane, 3-5 parts of boehmite, 1-2 parts of emulsifier, and 50-60 parts of deionized water to a reaction vessel, and emulsify under stirring to form an emulsion; the emulsifier can be sodium dodecyl sulfate. A2. Add 4-10 parts of shell material to the emulsion and stir to mix evenly; A3. Under stirring conditions, heat the reaction system to 55-65℃, add 0.1-1 parts of curing agent, and react for 3.5-4.5 hours to form a coating layer on the surface of the core material using the shell material; the curing agent can be ammonium chloride. A4. After the reaction is complete, the product is washed with deionized water, filtered, and vacuum dried to obtain the microencapsulated flame retardant.
[0040] The microencapsulated flame retardant prepared by this invention has moderate mechanical strength and can withstand the preparation processes such as stirring and coating of positive electrode slurry without premature cracking and failure. At the same time, the shell material has excellent solvent resistance after cross-linking and curing, and has good stability in N-methylpyrrolidone solvent and battery working environment, maintaining the core-shell structure relatively intact.
[0041] In some embodiments of the present invention, a method for preparing a lithium battery cathode slurry includes the following steps: (1) Dissolve the adhesive in a solvent and stir until homogeneous to obtain an adhesive solution; (2) Add conductive carbon black and carbon nanotubes to the adhesive solution and stir evenly to obtain conductive slurry; (3) Add ternary materials and lithium manganese iron phosphate to the conductive slurry, stir evenly, and obtain a mixed slurry of active materials; (4) Add a flame retardant mixture, which is a pre-mixed solution of microencapsulated flame retardant and solvent at a weight ratio of 1-3:1, to the active material mixture slurry, and stir evenly to obtain a positive electrode slurry. The solvent may be N-methylpyrrolidone.
[0042] Further, in step (4), a flame retardant mixture formed by pre-mixing microencapsulated flame retardant and solvent at a weight ratio of 2:1 is added to the active material mixture slurry, and stirred evenly to obtain the positive electrode slurry.
[0043] Example 1
[0044] In this embodiment, a lithium battery cathode slurry comprises the following raw materials in parts by weight: 80 parts LiNi0.8Co0.1Mn0.1O2, 18 parts LiMn0.6Fe0.4PO4, 2 parts conductive carbon black, 3 parts carbon nanotubes, 7 parts microencapsulated flame retardant, and 4 parts binder. The carbon nanotubes are multi-walled carbon nanotubes.
[0045] Furthermore, the microencapsulated flame retardant comprises a core material and a shell material covering the surface of the core material. The core material contains a phosphazene flame retardant, cage-type polysilsesquioxane, and boehmite. The shell material is composed of melamine-urea-formaldehyde resin and polymethyl methacrylate in a weight ratio of 2:1. The polymethyl methacrylate has a weight-average molecular weight of 350,000.
[0046] In this embodiment, the preparation method of the melamine-urea-formaldehyde resin includes the following steps: melamine, urea and formaldehyde are mixed in a molar ratio of 1:2:6, the pH is adjusted to 8.0, and the mixture is reacted at 70°C for 1.5 h to obtain melamine-urea-formaldehyde resin.
[0047] Furthermore, the weight ratio of the phosphazene flame retardant, the cage-type polysilsesquioxane, and the boehmite is 2:1:2.
[0048] Furthermore, the phosphazene flame retardant is ethoxy(pentafluoro)cyclotriphosphazene. The cage-like polysilsesquioxane is aminopropylheptyl-cage-like polysilsesquioxane.
[0049] Furthermore, the adhesive is polyvinylidene fluoride, specifically Arkema Kynar® HSV 900.
[0050] In this embodiment, the preparation method of the microencapsulated flame retardant includes the following steps: A1. By weight, 7 parts of ethoxy(pentafluoro)cyclotriphosphazene, 3.5 parts of aminopropylheptyl-cage polysilsesquioxane, 3.5 parts of boehmite, 1.5 parts of emulsifier, and 55 parts of deionized water are added to a reaction vessel and emulsified under stirring to form an emulsion; the emulsifier is sodium dodecyl sulfate. A2. Add 4 parts of melamine-urea-formaldehyde resin and 2 parts of polymethyl methacrylate to the emulsion and stir to mix evenly; A3. Under stirring conditions, the reaction system is heated to 60°C, 0.5 parts of curing agent are added, and the reaction is carried out for 4 hours to form a coating layer on the surface of the core material; the curing agent is ammonium chloride. A4. After the reaction is complete, the microencapsulated flame retardant is obtained by washing, filtering and vacuum drying.
[0051] In this embodiment, a method for preparing a lithium battery cathode slurry includes the following steps: (1) Dissolve the adhesive in a solvent and stir until homogeneous to obtain an adhesive solution; the solvent is N-methylpyrrolidone, and the weight ratio of the adhesive to the solvent is 1:5; (2) Add conductive carbon black and carbon nanotubes to the adhesive solution and stir evenly to obtain conductive slurry; (3) Add ternary materials and lithium manganese iron phosphate to the conductive slurry, stir evenly, and obtain a mixed slurry of active materials; (4) Add the flame retardant mixture formed by pre-mixing microencapsulated flame retardant and solvent at a weight ratio of 2:1 to the active material mixture slurry, stir evenly, and obtain the positive electrode slurry.
[0052] Example 2
[0053] In this embodiment, a lithium battery cathode slurry comprises the following raw materials in parts by weight: 75 parts of LiNi0.8Co0.1Mn0.1O2, 20 parts of LiMn0.6Fe0.4PO4, 3 parts of conductive carbon black, 2 parts of carbon nanotubes, 5 parts of microencapsulated flame retardant, and 5 parts of binder.
[0054] Furthermore, the microencapsulated flame retardant includes a core material and a shell material covering the surface of the core material. The core material contains phosphazene flame retardants, cage-type polysilsesquioxane, and boehmite. The shell material is composed of melamine-urea-formaldehyde resin and polymethyl methacrylate in a weight ratio of 3:2.
[0055] Furthermore, the weight ratio of the phosphazene flame retardant, the cage-type polysilsesquioxane, and the boehmite is 2.5:1:1.5.
[0056] Furthermore, the phosphazene flame retardant is (phenoxy)pentafluorocyclotriphosphazene. The cage-like polysilsesquioxane is aminopropylheptyl-cage-like polysilsesquioxane.
[0057] Furthermore, the preparation method of the microencapsulated flame retardant includes the following steps: A1. By weight, 5 parts of (phenoxy)pentafluorocyclotriphosphazene, 2 parts of aminopropylheptyl-cage polysilsesquioxane, 3 parts of boehmite, 1.5 parts of emulsifier, and 55 parts of deionized water are added to a reaction vessel and emulsified under stirring to form an emulsion; the emulsifier may be sodium dodecyl sulfate. A2. Add 3 parts of melamine-urea-formaldehyde resin and 2 parts of polymethyl methacrylate to the emulsion and stir to mix evenly; A3. Under stirring conditions, heat the reaction system to 60°C, add 0.5 parts of curing agent, and react for 4 hours to form a coating layer on the surface of the core material; the curing agent can be ammonium chloride; A4. After the reaction is complete, the microencapsulated flame retardant is obtained by washing, filtering and vacuum drying.
[0058] In this embodiment, a method for preparing a lithium battery cathode slurry includes the following steps: (1) Dissolve the adhesive in a solvent and stir until homogeneous to obtain an adhesive solution; the solvent is N-methylpyrrolidone, and the weight ratio of the adhesive to the solvent is 1:5; (2) Add conductive carbon black and carbon nanotubes to the adhesive solution and stir evenly to obtain conductive slurry; (3) Add ternary materials and lithium manganese iron phosphate to the conductive slurry, stir evenly, and obtain a mixed slurry of active materials; (4) Add the flame retardant mixture formed by pre-mixing microencapsulated flame retardant and solvent at a weight ratio of 2:1 to the active material mixture slurry, stir evenly, and obtain the positive electrode slurry.
[0059] The rest of the content of this embodiment is the same as that of Embodiment 1, and will not be repeated here.
[0060] Example 3
[0061] In this embodiment, a lithium battery positive electrode slurry comprises the following raw materials in parts by weight: 85 parts of LiNi0.8Co0.1Mn0.1O2, 15 parts of LiMn0.6Fe0.4PO4, 2 parts of conductive carbon black, 2 parts of carbon nanotubes, 9 parts of microencapsulated flame retardant, and 3 parts of binder.
[0062] Furthermore, the microencapsulated flame retardant includes a core material and a shell material covering the surface of the core material. The core material contains phosphazene flame retardants, cage-type polysilsesquioxane, and boehmite. The shell material is composed of melamine-urea-formaldehyde resin and polymethyl methacrylate in a weight ratio of 2:1.
[0063] Furthermore, the weight ratio of the phosphazene flame retardant, cage-type polysilsesquioxane, and boehmite is 1.5:1:2.5.
[0064] Furthermore, the phosphazene flame retardant is ethoxy(pentafluoro)cyclotriphosphazene. The cage-type polysilsesquioxane is octaphenyl cage-type polysilsesquioxane.
[0065] In this embodiment, the preparation method of the microencapsulated flame retardant includes the following steps: A1. By weight, 7 parts of ethoxy(pentafluoro)cyclotriphosphazene, 3.5 parts of octaphenyl cage-type polysilsesquioxane, 3.5 parts of boehmite, 1.5 parts of emulsifier, and 55 parts of deionized water are added to a reaction vessel and emulsified under stirring to form an emulsion; the emulsifier is sodium dodecyl sulfate. A2. Add 4 parts of melamine-urea-formaldehyde resin and 2 parts of polymethyl methacrylate to the emulsion and stir to mix evenly; A3. Under stirring conditions, the reaction system is heated to 60°C, 0.5 parts of curing agent are added, and the reaction is carried out for 4 hours to form a coating layer on the surface of the core material; the curing agent is ammonium chloride. A4. After the reaction is complete, the microencapsulated flame retardant is obtained by washing, filtering and vacuum drying.
[0066] In this embodiment, a method for preparing a lithium battery cathode slurry includes the following steps: (1) Dissolve the adhesive in a solvent and stir until homogeneous to obtain an adhesive solution; the solvent is N-methylpyrrolidone, and the weight ratio of the adhesive to the solvent is 1:5; (2) Add conductive carbon black and carbon nanotubes to the adhesive solution and stir evenly to obtain conductive slurry; (3) Add ternary materials and lithium manganese iron phosphate to the conductive slurry, stir evenly, and obtain a mixed slurry of active materials; (4) Add the flame retardant mixture formed by pre-mixing microencapsulated flame retardant and solvent at a weight ratio of 2:1 to the active material mixture slurry, stir evenly, and obtain the positive electrode slurry.
[0067] The rest of the content of this embodiment is the same as that of Embodiment 1, and will not be repeated here.
[0068] Comparative Example 1 The difference between this comparative example and Example 1 is that no microencapsulated flame retardant is added to the lithium battery positive electrode slurry in this comparative example. The remaining components and preparation methods of this comparative example are the same as in Example 1.
[0069] Comparative Example 2 The difference between this comparative example and Example 1 is that the microcapsule core material in this comparative example contains only ethoxy(pentafluoro)cyclotriphosphazene and does not contain cage-like polysilsesquioxane or boehmite; the weight of ethoxy(pentafluoro)cyclotriphosphazene added to the core material is the same as the total weight of phosphazene flame retardants, cage-like polysilsesquioxane, and boehmite in Example 1. The remaining components and preparation methods of this comparative example are the same as in Example 1.
[0070] Comparative Example 3 The difference between this comparative example and Example 1 is that: in this comparative example, an unmicroencapsulated composite flame retardant is added to the positive electrode slurry. This composite flame retardant is composed of a phosphazene flame retardant, cage-type polysilsesquioxane, and boehmite in a weight ratio of 2:1:2, and the total weight of the composite flame retardant is equal to the total weight of the core material in Example 1; no microencapsulated flame retardant is added in this comparative example. The remaining components and preparation methods of this comparative example are the same as in Example 1.
[0071] The positive electrode slurries of Examples 1-3 and Comparative Examples 1-3 were uniformly coated on the surface of the aluminum foil current collector, and the coating surface density was controlled to be 200 g / m² on a dry weight basis.2 The material was vacuum dried at 120℃ for 12 hours, then compacted by roller pressing and cut to obtain the positive electrode sheet. Using the above positive electrode sheet as the positive electrode, an artificial graphite negative electrode sheet as the negative electrode, a polyethylene microporous membrane as the separator, and a solution of 1 mol / L LiPF6 dissolved in ethylene carbonate (EC) / dimethyl carbonate (DMC) / ethyl methyl carbonate (EMC) as the electrolyte, a lithium-ion battery was assembled; the volume ratio of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate was 1:1:1.
[0072] Cyclic performance tests were performed on Example 1 and Comparative Example 1, and the test data are shown in Table 1 below:
[0073] The cycle performance was tested as follows: At 25°C, the batteries of Example 1 and Comparative Example 1 were subjected to charge-discharge cycle tests at a current density of 0.5C / 0.5C, and the capacity retention rate was recorded. The test results showed that after 500 cycles, the capacity retention rate of the battery in Example 1 was 91.2%, and that of the battery in Comparative Example 1 was 91.6%. The cycle performance of Example 1 was essentially equivalent to that of Comparative Example 1, indicating that the addition of the microencapsulated flame retardant did not significantly degrade the cycle performance, while significantly improving flame retardant safety.
[0074] The rate performance of Example 1 and Comparative Example 1 was tested, and the test data are shown in Table 2 below:
[0075] The rate performance tests were conducted as follows: At 25°C, the batteries of Example 1 and Comparative Example 1 were charged and discharged at current densities of 0.2C, 0.5C, 1C, 2C, and 3C, respectively. The test results showed that at a rate of 0.2C, the discharge specific capacity of Example 1 was 183.1 mAh / g, while that of Comparative Example 1 was 186.1 mAh / g, representing a decrease of approximately 1.6% compared to Comparative Example 1. At each rate, the capacity retention rates of Example 1 and Comparative Example 1 were essentially equivalent. These results indicate that the addition of the microencapsulated flame retardant in this invention did not have a significant adverse effect on the rate performance of the batteries. Furthermore, the electrochemical performance of Examples 2 and 3 maintained the same trend as that of Example 1, and the addition of the microencapsulated flame retardant did not have a significant negative impact on battery cycle life or rate performance.
[0076] The lithium battery positive electrode sheets and lithium-ion batteries of Examples 1-3 and Comparative Examples 1-3 were subjected to nail penetration performance tests. The test results are shown in Table 3 below:
[0077] In this case, the lithium-ion batteries of Examples 1-3 and Comparative Examples 1-3 were subjected to nail penetration tests in accordance with GB / T 31485-2015. The batteries were all fully charged (SOC=100%), and a steel needle with a diameter of 3 mm was used. The penetration rate was 20 mm / s, and the occurrence of fire, explosion and the highest temperature during the test were recorded. Figure 3 This is a comparison of the temperature-time curves of lithium-ion batteries from Example 1 and Comparative Examples 2-3 in the nail penetration test. It can be seen that: the battery in Comparative Example 3, due to the lack of microencapsulation of the flame retardant, is prone to premature failure due to side reactions with the electrolyte, exhibits poor dispersion uniformity, reaches a peak temperature of 187℃, and cools down slowly after heat release; the battery cell material in Comparative Example 2 contains only phosphazene flame retardant components, lacking the synergistic effect of cage-like polysilsesquioxane and boehmite, and has a peak temperature of 159℃; while the battery in Example 1, after nail penetration, showed effective temperature suppression, with a peak temperature of 137℃, and no fire or explosion occurred. These results indicate that the present invention, through the synergistic effect of phosphazene flame retardants, cage-like polysilsesquioxane, and boehmite, as well as the microencapsulation protective structure, can effectively block the thermal runaway chain reaction, and its flame retardant and temperature suppression effects are significantly better than those of the flame retardant system in Comparative Example 2 and the unmicroencapsulated flame retardant system in Comparative Example 3.
[0078] The hot box test was conducted as follows: Batteries from Examples 1-3 and Comparative Examples 1-3 were placed in a hot box and heated from 25°C to 200°C at a heating rate of 5°C / min, and the battery status was observed. The test results showed that: after the batteries of Examples 1-3 were heated to the shell cracking temperature (approximately 100-120°C), the microcapsules released the flame retardant, and the batteries did not experience thermal runaway; the battery of Comparative Example 1 experienced thermal runaway and ignited when heated to approximately 150°C; the battery of Comparative Example 2 contained only phosphazene in its core material, and although it did not ignite after the phosphazene was released when heated to approximately 120°C, it failed to effectively suppress heat accumulation due to the lack of synergistic flame retardant effects from cage-like polysilsesquioxane and boehmite, and the battery temperature continued to rise with the increase in the hot box temperature; the battery of Comparative Example 3 had a significantly lower flame retardant effect than Example 1 because the flame retardant was not microencapsulated, resulting in uneven distribution in the slurry and premature partial deactivation.
[0079] The positive electrode slurry of this invention combines ternary materials, lithium manganese iron phosphate, conductive carbon black, carbon nanotubes, binders, and other raw materials, and adds microencapsulated flame retardants. This results in a positive electrode slurry with good electrochemical and flame retardant properties. When the battery is operating normally, the flame retardant is encapsulated in capsules and has little impact on the electrochemical performance. When the battery is subjected to conditions such as puncture or overheating, the capsules rupture and release the flame retardant to prevent the electrolyte from burning, thereby effectively improving the safety performance of the battery.
[0080] The above embodiments are preferred implementations of the present invention. In addition, the present invention can be implemented in other ways. Any obvious substitutions without departing from the concept of the present invention are within the protection scope of the present invention.
Claims
1. A lithium battery positive electrode slurry, characterized in that: The raw materials include the following parts by weight: 60-100 parts of ternary material, 5-30 parts of lithium manganese iron phosphate, 0.5-5 parts of conductive carbon black, 0.5-5 parts of carbon nanotubes, 3-10 parts of microencapsulated flame retardant, and 0.5-5 parts of binder.
2. The lithium battery positive electrode slurry according to claim 1, characterized in that: The microencapsulated flame retardant includes a core material and a shell material covering the surface of the core material. The core material contains phosphazene flame retardants, cage-type polysilsesquioxane, and boehmite.
3. The lithium battery positive electrode slurry according to claim 2, characterized in that: The weight ratio of the core material to the shell material in the microencapsulated flame retardant is 1.5-3:
1.
4. The lithium battery positive electrode slurry according to claim 2, characterized in that: The weight ratio of the phosphazene flame retardant, cage-type polysilsesquioxane, and boehmite is 1-3:1:1-3.
5. The lithium battery positive electrode slurry according to claim 2, characterized in that: The phosphazene flame retardant is at least one of ethoxy(pentafluoro)cyclotriphosphazene, (phenoxy)pentafluorocyclotriphosphazene, (trifluoroethoxy)pentafluorocyclotriphosphazene, hexachlorocyclotriphosphazene, hexaphenoxycyclotriphosphazene, and hexafluorocyclotriphosphazene.
6. The lithium battery positive electrode slurry according to claim 2, characterized in that: The cage-type polysilsesquioxane is at least one of epoxy-functionalized cage-type polysilsesquioxane, amino-functionalized cage-type polysilsesquioxane, and phenyl cage-type polysilsesquioxane.
7. The lithium battery positive electrode slurry according to claim 2, characterized in that: The shell material is at least one of melamine-urea-formaldehyde resin, urea-formaldehyde resin, polyurea, polyurea-formaldehyde, and polymethyl methacrylate.
8. The lithium battery positive electrode slurry according to claim 1, characterized in that: The ternary material is lithium nickel cobalt manganese oxide, with the chemical formula LiNi. 1-x-y CoxMn y O2, where 0 < x < 1, 0 < y < 1, x + y < 1.
9. The lithium battery positive electrode slurry according to claim 1, characterized in that: The adhesive is polyvinylidene fluoride.
10. A method for preparing the positive electrode slurry as described in any one of claims 1-9, comprising the following steps: (1) Dissolve the adhesive in a solvent and stir until homogeneous to obtain an adhesive solution; (2) Add conductive carbon black and carbon nanotubes to the adhesive solution and stir evenly to obtain conductive slurry; (3) Add ternary materials and lithium manganese iron phosphate to the conductive slurry, stir evenly, and obtain a mixed slurry of active materials; (4) Add the flame retardant mixture formed by pre-mixing microencapsulated flame retardant and solvent to the active material mixture slurry, stir evenly, and obtain the positive electrode slurry.