A battery, an electric device

By setting a polymer adhesive layer on the lithium-ion battery separator and optimizing the composition of the non-aqueous electrolyte, the sealing failure problem of lithium-ion batteries under high-frequency vibration conditions is solved, thereby improving the cycle performance and safety of the battery.

CN123073133APending Publication Date: 2026-11-10ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611519069.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The sealing failure of lithium-ion batteries under high-frequency vibration conditions leads to electrolyte leakage, corrosion, and shortened battery life.

Method used

By setting a polymer adhesive layer on the diaphragm and optimizing the composition of the non-aqueous electrolyte, a matching relationship is formed, which improves the interface stability and buffer wear resistance, reduces the wear risk of the inner layer of the encapsulation, and improves the sealing reliability.

Benefits of technology

It effectively solves the problem of sealing failure of lithium-ion batteries under high-frequency vibration conditions, and improves the cycle performance and safety of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073133A_ABST
    Figure CN123073133A_ABST
Patent Text Reader

Abstract

The application provides a battery and an electric device. The battery comprises a package body and a battery core, the package body comprises a package cavity, and the battery core is packaged in the package cavity; the battery core comprises an electrode assembly and a nonaqueous electrolyte; the electrode assembly comprises a separator; the separator comprises a porous base film and a glue layer arranged on at least one side surface of the porous base film; the glue layer comprises a polymer; and the nonaqueous electrolyte comprises propylene carbonate and methyl ethyl carbonate; wherein K=M*T1, 12≤K≤165; M is the mass ratio of propylene carbonate to methyl ethyl carbonate, and T1 is the melting point of the polymer. The battery has excellent cycle performance and safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of secondary batteries, and more particularly to a battery and electrical device. Background Technology

[0002] Lithium-ion batteries may experience continuous or intermittent high-frequency vibrations during operation, such as the lateral shaking of a robotic vacuum cleaner rubbing against the ground or the severe vibrations of a power tool cutting or drilling. This vibration environment places stringent requirements on the battery's mechanical stability and sealing.

[0003] Currently, lithium-ion battery packaging relies on heat-sealing the polypropylene (PP) layer inside the aluminum-plastic film for sealing. However, the edge of the current collector inside the cell experiences long-term fretting friction and interference with the PP layer under vibration. Since the hardness of the metal current collector edge is much higher than that of the PP layer, this friction causes the PP layer to gradually thin or even completely wear through, exposing the intermediate aluminum foil layer. Once the aluminum foil layer is exposed, it not only damages the sealing structure leading to electrolyte micro-leakage but may also trigger electrochemical corrosion, ultimately causing battery bulging, increased internal resistance, and capacity drops, severely impacting battery life and equipment safety.

[0004] Therefore, developing an innovative technology that can effectively solve the sealing failure problem of soft-pack lithium-ion batteries under high-frequency vibration conditions is key to improving battery cycle performance and safety. Summary of the Invention

[0005] This invention provides a battery that effectively solves the problem of sealing failure of soft-pack lithium-ion batteries under high-frequency vibration conditions, and has excellent cycle performance and safety.

[0006] This invention provides an electrical device with excellent performance.

[0007] In a first aspect, the present invention provides a battery comprising a package body and a battery cell, wherein the package body includes a package cavity and the battery cell is packaged within the package cavity;

[0008] The battery cell includes an electrode assembly and a non-aqueous electrolyte;

[0009] The electrode assembly includes a diaphragm;

[0010] The diaphragm includes a porous base membrane and an adhesive layer disposed on at least one surface of the porous base membrane;

[0011] The adhesive layer comprises a polymer;

[0012] The non-aqueous electrolyte includes propylene carbonate and ethyl methyl carbonate;

[0013] Where K = M * T1, 12 ≤ K ≤ 165;

[0014] M is the mass ratio of propylene carbonate to methyl ethyl carbonate, and T1 is the melting point of the polymer.

[0015] For batteries as described above, 15 ≤ K ≤ 140.

[0016] For the battery as described above, 0.08 ≤ M ≤ 1.0;

[0017] And / or, 130℃≤T1≤175℃; preferably, 140℃≤T1≤165℃.

[0018] In the battery described above, the non-aqueous electrolyte satisfies at least one of the following conditions:

[0019] (1) Based on the total mass of the non-aqueous electrolyte, the mass percentage of propylene carbonate is 5% to 20%;

[0020] (2) Based on the total mass of the non-aqueous electrolyte, the mass percentage of methyl ethyl carbonate is 20% to 60%;

[0021] (3) The non-aqueous electrolyte also includes lithium salt, and the mass percentage of the lithium salt is 10% to 15% based on the total mass of the non-aqueous electrolyte;

[0022] (4) The non-aqueous electrolyte also includes at least one of ethylene carbonate, diethyl carbonate, dimethyl carbonate, and ethyl propyl carbonate.

[0023] As described above, the battery package includes an outer protective layer, a first adhesive layer, an aluminum foil layer, a second adhesive layer, and a heat-sealing layer stacked sequentially, with the heat-sealing layer close to the battery cell;

[0024] The package satisfies at least one of the following conditions:

[0025] (1) The thickness of the heat-sealing layer is 20~50μm;

[0026] (2) The surface roughness Ra of the heat-sealing layer on the side closest to the battery cell is ≤0.5μm;

[0027] (3) The heat-sealing layer comprises a modified polyolefin;

[0028] (4) The melting point of the heat-sealing layer is T2, 90℃≤T2≤150℃;

[0029] Preferably, 100℃≤T2≤140℃;

[0030] (5) The melting point of the heat-sealing layer is T2, 1.8 × 10⁻⁶. 3 ≤K×T2≤2.5×10 4 ;

[0031] Preferably, 3.6 × 10 3 ≤K×T2≤2.0×10 4 ;

[0032] (6) The melting point of the heat-sealing layer is T2, ΔT =|T2−T1|, and ΔT is 20℃~50℃.

[0033] The polymer in the battery described above includes at least one of polyvinylidene fluoride, polyvinylidene fluoride copolymer, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trifluorochloroethylene copolymer, polyvinylidene fluoride-tetrafluoroethylene copolymer, polymethyl methacrylate, polyethyl methacrylate, polyacrylate, polyvinyl acetate, and ethylene-vinyl acetate copolymer.

[0034] The weight-average molecular weight of the polymer is Mw; 300,000 ≤ Mw ≤ 1,200,000;

[0035] Preferably, 400,000 ≤ Mw ≤ 800,000.

[0036] As described above, the electrode assembly of the battery further includes a negative electrode.

[0037] The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on at least one side surface of the negative electrode current collector;

[0038] The porosity of the negative electrode active layer is P, where 25% ≤ P ≤ 45%;

[0039] Preferably, 30% ≤ P ≤ 40%.

[0040] As described above, the battery enclosure includes a bent section and a straight section, wherein the bent section is located on both sides of the width direction of the battery cell; and the straight section is located in the width direction of the battery cell.

[0041] The radius of curvature R of the bent segment satisfies: 1mm≤R≤5mm.

[0042] The electrode assembly of the battery described above further includes a positive electrode plate;

[0043] The separator is disposed between the positive electrode and the negative electrode;

[0044] The battery satisfies at least one of the following conditions:

[0045] (1) The peel strength between the separator and the positive electrode is F1, 3N / m≤F1≤50N / m;

[0046] Preferably, 5 N / m ≤ F1 ≤ 30 N / m;

[0047] (2) The peel strength between the diaphragm and the negative electrode sheet is F2, 3N / m≤F2≤50N / m; preferably, 5N / m≤F2≤30N / m;

[0048] (3) The peel strength between the battery cell and the package is F3, 3N / m≤F3≤30N / m.

[0049] Secondly, the present invention provides an electrical device including the battery as described above.

[0050] This invention provides a battery that effectively solves the sealing failure problem of pouch lithium-ion batteries under high-frequency vibration conditions, exhibiting excellent cycle performance and safety. Specifically, by placing the battery cell within the encapsulation cavity of a package, and ensuring that the separator in the electrode assembly comprises a porous base film and a polymer-containing adhesive layer disposed on at least one surface, while simultaneously ensuring that the non-aqueous electrolyte comprises propylene carbonate and ethyl methyl carbonate, satisfying K=M*T1 and 12≤K≤165, a matching relationship can be established between the properties of the separator adhesive layer material and the electrolyte composition. This improves the interface stability and buffering wear resistance of the battery cell under vibration conditions, thereby reducing the risk of localized wear caused by fretting friction in the inner layer of the package, enhancing the sealing reliability of the pouch battery, and balancing battery space utilization and long-term electrochemical performance. Attached Figure Description

[0051] Figure 1 This is a partial structural diagram of the package provided in a specific embodiment of the present invention;

[0052] Figure 2 This is a partial structural diagram of the package provided in a specific embodiment of the present invention;

[0053] Figure 3 This is a partial structural diagram of the heat-sealing layer of a battery after cycling, provided in a specific embodiment of the present invention.

[0054] Explanation of reference numerals in the attached figures:

[0055] 01-Outer protective layer; 02-First adhesive layer; 03-Aluminum foil layer; 04-Second adhesive layer; 05-Heat-sealing layer; A-Straight section; B-Bent section. Detailed Implementation

[0056] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numerals in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples of apparatuses and methods consistent with some aspects of the invention as detailed in the appended claims.

[0057] Existing pouch batteries mostly use aluminum-plastic film to wrap the battery cell, and mechanically isolate the current collector edge from the inner packaging layer by means of insulating tape, adding buffer pads, or setting insulating spacers on the outside of the battery cell. The basic idea is to add an external barrier structure between the metal edge and the heat-sealing layer, and use additional materials to absorb some vibration energy and reduce direct friction.

[0058] However, under the combined effects of long-term vibration and charge-discharge cycles, the added tape or buffer is prone to compaction, displacement, aging, or performance degradation due to incompatibility with the electrolyte environment. The edge of the metal current collector may still generate high-frequency fretting friction on the inner layer of the aluminum-plastic film, causing local thinning and damage to the heat-sealing layer, thereby weakening the sealing performance. After the sealing barrier is damaged, the risks of electrolyte leakage, moisture intrusion, internal corrosion, and bulging failure increase.

[0059] Meanwhile, additional protective materials occupy internal packaging space, increasing battery assembly processes and material costs, which is detrimental to battery lightweighting and energy density improvement. Relying solely on external separators for protection makes it difficult to maintain a stable balance between vibration resistance, packaging reliability, and electrochemical performance.

[0060] Based on this, in a first aspect, the present invention provides a battery, including a package and a cell, wherein the package includes a package cavity and the cell is packaged in the package cavity;

[0061] The battery cell includes electrode components and non-aqueous electrolyte;

[0062] The electrode assembly includes a diaphragm;

[0063] The membrane includes a porous base membrane and an adhesive layer disposed on at least one surface of the porous base membrane;

[0064] The adhesive layer includes a polymer;

[0065] Non-aqueous electrolytes include propylene carbonate and ethyl methyl carbonate;

[0066] Where K = M * T1, 12 ≤ K ≤ 165;

[0067] M is the mass ratio of propylene carbonate to methyl ethyl carbonate, and T1 is the melting point of the polymer.

[0068] In this application, the battery may be an electrochemical device including a package and a cell, the package forming a package cavity, the cell being housed within the package cavity and together with the non-aqueous electrolyte forming a closed electrochemical system.

[0069] Electrode assemblies may include a diaphragm and an electrode sheet structure that mates with it.

[0070] The diaphragm provided by the present invention includes a porous base membrane and an adhesive layer disposed on at least one side surface of the porous base membrane.

[0071] The porous base membrane is used to provide ion transport channels and isolation support. The porous base membrane can be selected from common diaphragm base membrane materials. The adhesive layer is disposed on at least one surface of the porous base membrane, which can be exemplarily a single-sided coating or a double-sided coating structure. The adhesive layer serves to provide functions such as bonding the diaphragm and electrode sheet structure and thermal stability reinforcement, and also serves as a polymer source for subsequent in-situ precipitation to protect the interface.

[0072] The polymer in the adhesive layer is used to participate in the formation of the subsequent interface protective layer.

[0073] The melting point T1 of the polymer can be detected using methods commonly found in the art, for example, in some embodiments, by a method including the following steps:

[0074] Differential scanning calorimetry (DSC) was used. Approximately 3–5 mg of powdered sample was collected by gently scraping off the surface adhesive layer with a blade and placed in a sealed DSC aluminum crucible. Under a nitrogen atmosphere (flow rate 50 mL / min), the sample was heated from 25 °C to 200 °C at a heating rate of 10 °C / min. The melting endothermic curve was recorded, and the peak temperature of the endothermic peak was recorded as T1.

[0075] The non-aqueous electrolyte includes at least propylene carbonate and ethyl methyl carbonate. Propylene carbonate has high polarity and strong solvation ability, and has a swelling-inducing effect on the polymer chain segments of the gel layer. Ethyl methyl carbonate, as another carbonate component, regulates the solubility and diffusion kinetics of the overall solvent environment.

[0076] M is defined as the mass ratio of propylene carbonate to methyl ethyl carbonate. When M increases, the proportion of propylene carbonate in the system increases, and the polymer in the gel layer is more likely to swell and partially desorb. When M decreases, the proportion of methyl ethyl carbonate increases, the release of chain segments is inhibited, and both the driving force for precipitation and the amount of migration decrease.

[0077] The mass percentage of propylene carbonate and methyl ethyl carbonate in the electrolyte can be detected using methods commonly found in the art. For example, in some embodiments, the detection is performed using a method including the following steps:

[0078] First, the battery is disassembled in a glove box, and the electrolyte is completely extracted from the electrodes and separator using the diethyl carbonate (DEC) immersion method. After dilution with an organic solvent, the electrolyte is injected into a gas chromatograph or gas chromatography-mass spectrometry system. Using a carbonate-specific column or a weakly polar capillary column, separation and detection are performed under the set carrier gas flow rate, injection port temperature, and programmed temperature rise conditions. Subsequently, the target compound is qualitatively identified based on its retention time combined with a standard mass spectrum, and a peak area-concentration calibration curve is plotted using the external standard method or the internal standard method to calculate the mass percentage content of propylene carbonate and methyl ethyl carbonate.

[0079] In this invention, the gelation coefficient K is defined by the mass ratio M of propylene carbonate (PC) to ethyl methyl carbonate (EMC) in the electrolyte and the melting point T1 of the membrane adhesive layer (K=M×T1). This coefficient characterizes the thermodynamic equilibrium state of the adhesive layer dissolving and precipitating in the electrolyte during the hot pressing process.

[0080] It should be noted that the K value is calculated using only the numerical value, without units. For example, when M is 0.1 and T1 is 140℃, K = 0.1 × 140 = 14.

[0081] In detail, K includes, but is not limited to, a range of 12, 20, 40, 60, 80, 100, 120, 140, 160, 165, or any two of these ranges.

[0082] The M value (PC / EMC mass ratio) determines the chemical affinity of the electrolyte system for the adhesive layer. PC, as a highly polar solvent (dielectric constant ε>3.6), has lone pair electrons on its carbonyl oxygen atoms that can form dipole-dipole interactions and weak hydrogen bonds with the polymer molecular chains. This is the core factor that disrupts the polymer lattice energy and causes the molecular chains to detach from the bulk. EMC, on the other hand, is a low-polarity solvent (dielectric constant ε between 2.8 and 3.6), providing only weak dispersion forces. When M is too small, there is a lack of sufficient free PC molecules in the system, and some PC is preferentially consumed by lithium salt coordination. The overall solubility parameter of the electrolyte deviates significantly from the soluble window of the polymer. The polymer crystal region cannot be effectively attacked thermodynamically, and the adhesive layer can only undergo surface wetting and cannot release free polymer chain segments into the liquid phase. At this time, it is necessary to select an adhesive layer with a higher melting point to take advantage of the stronger molecular chain rigidity and cohesive energy of the high melting point polymer. Under the condition of limited solvent solubility, it relies on its own high structural stability to maintain the integrity of the adhesive layer skeleton and prevent the adhesive layer from failing due to excessive swelling or dissolution, thereby ensuring the dimensional stability and mechanical strength of the separator in the electrolyte.

[0083] T1 characterizes the crystallinity and molecular chain rigidity of the polymer, essentially representing the macroscopic manifestation of the activation energy for chain segment de-entanglement. When T1 is too low, the molecular chain is highly flexible, the amorphous region accounts for a large proportion, and a large number of topological entanglements form between the molecular chains. The equilibrium concentration of free chain segments in the liquid phase is extremely low. After cooling, there is a lack of material basis required for heterogeneous nucleation, making it impossible to form a continuous interfacial layer on the surface of the encapsulated body. At this point, it is necessary to increase M, that is, increase the proportion of propylene carbonate. By utilizing the stronger polar solubility of PC, the topological entanglement between polymer chains can be effectively weakened, and the equilibrium concentration of free chain segments in the liquid phase can be significantly increased. This provides a sufficient material basis for heterogeneous nucleation of polymer chain segments on the surface of the encapsulated body and the construction of a continuous interfacial layer.

[0084] In summary, the K value, through the synergistic product of M and T1, defines the effective free polymer segment equilibrium concentration that the adhesive layer can release into the liquid phase within the safe formation temperature window. When 12 ≤ K ≤ 165, the concentration of free polymer segments in the liquid phase is precisely within the supersaturation critical range. After cooling, uniform heterogeneous nucleation can occur on the surface of the encapsulated body as a substrate, depositing a wear-resistant interface layer of suitable thickness, density, and strong adhesion. This effectively buffers the fretting friction between the current collector edge and the encapsulated body, solving the technical problems of seal failure and shortened cycle life under vibration conditions.

[0085] In some embodiments of the present invention, 15 ≤ K ≤ 140.

[0086] In detail, K includes, but is not limited to, a range of 15, 20, 40, 60, 80, 100, 120, 140, or any two of these.

[0087] By limiting K to between 15 and 140, insufficient solvent action and failure to form an effective protective interface can be avoided when K is too low, and excessive swelling of the adhesive layer can be avoided when K is too high, which would weaken the integrity of the film layer. This makes it easier for the adhesive polymer to migrate and deposit directionally on the inner surface of the package, forming a continuous buffer interface between the current collector edge and the inner layer of the package. This reduces the wear of the heat seal layer by fretting friction, improves the sealing stability of the package, and improves the battery life and safety under vibration and cycling conditions.

[0088] In some embodiments of the present invention, 0.08 ≤ M ≤ 1.0.

[0089] In detail, the mass ratio of propylene carbonate to methyl ethyl carbonate includes, but is not limited to, 0.08, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, 1.0, or any combination thereof.

[0090] By controlling M between 0.08 and 1.0, the non-aqueous electrolyte can possess both appropriate polarity and solvation capability, thereby acting more stably on the polymer in the separator layer during battery formation. This range avoids insufficient swelling driving force due to excessively low propylene carbonate content, and also prevents excessive softening or uncontrolled deposition of the separator layer due to excessively high content, thus enabling controlled migration and deposition of polymer segments on the inner surface of the encapsulation.

[0091] In some embodiments of the present invention, 130℃≤T1≤175℃; preferably, 140℃≤T1≤165℃.

[0092] In detail, the melting point T1 of the polymer includes, but is not limited to, a range of 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, or any combination thereof.

[0093] Preferably, 140℃≤T1≤165℃.

[0094] By limiting T1 to 130°C to 175°C, preferably 140°C to 165°C, it is possible to induce swelling and local untangling of the adhesive layer surface without causing instability of the diaphragm skeleton or the encapsulation heat seal layer.

[0095] In some embodiments of the present invention, based on a non-aqueous electrolyte, the mass percentage of propylene carbonate is 5% to 20%.

[0096] In detail, based on the non-aqueous electrolyte, the mass percentage of propylene carbonate includes, but is not limited to, 5%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, or any combination thereof.

[0097] When the mass percentage of propylene carbonate is 5% to 20%, it can enhance the wetting and penetration of the polymer layer without significantly increasing the viscosity of the system.

[0098] In some embodiments of the present invention, the mass percentage of ethyl methyl carbonate is 20% to 60% based on the non-aqueous electrolyte.

[0099] In detail, based on the non-aqueous electrolyte, the mass percentage of ethyl methyl carbonate includes, but is not limited to, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, or any combination thereof.

[0100] When the mass percentage of methyl ethyl carbonate is 20% to 60%, the solvent volatility and solubility parameters can be adjusted to promote the uniform deposition of the polymer layer during the formation process.

[0101] In some embodiments of the present invention, the non-aqueous electrolyte further includes lithium salt, and the mass percentage of lithium salt is 10% to 15% based on the total mass of the non-aqueous electrolyte.

[0102] Common lithium salts in the field can be selected, such as one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0103] In detail, based on the total mass of the non-aqueous electrolyte, the mass percentage of lithium salt includes, but is not limited to, 10%, 11%, 12%, 13%, 14%, 15%, or any combination thereof.

[0104] In some embodiments of the present invention, the non-aqueous electrolyte further includes at least one of ethylene carbonate, diethyl carbonate, dimethyl carbonate, and ethyl propyl carbonate.

[0105] When the non-aqueous electrolyte includes the above components, it can further balance the low-temperature fluidity, wettability and formation uniformity, making it easier for the non-aqueous electrolyte to fully wet the separator layer and electrode interface inside the battery cell.

[0106] In some embodiments of the present invention, such as Figure 1 As shown, the package includes an outer protective layer 01, a first adhesive layer 02, an aluminum foil layer 03, a second adhesive layer 04, and a heat-sealing layer 05 stacked in sequence, with the heat-sealing layer 05 close to the battery cell.

[0107] In one specific embodiment, the package adopts an aluminum-plastic film structure in which an outer protective layer, a first adhesive layer, an aluminum foil layer, a second adhesive layer and a heat-sealing layer are sequentially composited, wherein the heat-sealing layer is arranged on the innermost side and faces the battery cell so as to directly form a sealing interface during hot-pressing encapsulation.

[0108] The outer protective layer and aluminum foil layer provide puncture resistance and barrier properties, the adhesive layer ensures a strong bond between the layers, and the heat-sealing layer serves as a buffer and heat-sealing agent in the environment adjacent to the battery cell.

[0109] Figure 3 This invention provides a partial structural diagram of the heat-sealing layer of a battery after cycling, according to a specific embodiment of the invention. Figure 3 It is evident that a wear-resistant interface layer formed by polymer is deposited on the surface of the heat-sealing layer.

[0110] In some embodiments, the thickness of the heat-sealing layer is 20 μm to 50 μm.

[0111] In detail, the thickness of the heat-sealing layer includes, but is not limited to, a range of 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, or any combination thereof.

[0112] The thickness of the heat seal layer is directly related to the allowance for wear resistance. When it is less than 20μm, even if an interface layer is formed, the heat seal layer of the substrate is too thin and is still easily worn through under long-term friction; when it is more than 50μm, it increases material cost and packaging difficulty, and is not conducive to heat dissipation.

[0113] In some embodiments of the present invention, the surface roughness Ra of the heat-sealing layer on the side closest to the battery cell is ≤0.5μm.

[0114] The surface roughness of the heat seal layer can be detected using methods commonly used in the art. For example, in some embodiments, the surface to be tested is first cleaned, and then the stylus method is selected for measurement based on the surface characteristics. The stylus method uses a diamond stylus to slide along the surface to record vertical displacement in order to calculate parameters such as Ra. Finally, the surface roughness parameter value is calculated and output based on the measurement data.

[0115] In detail, the surface roughness Ra of the heat-sealing layer on the side closest to the battery cell includes, but is not limited to, a range of 0.5 μm, 0.4 μm, 0.3 μm, 0.2 μm, 0.1 μm, 0 μm, or any two of these.

[0116] Lower surface roughness helps the precipitated interface layer to spread evenly, forming a continuous and strongly adherent protective film, avoiding local stress concentration or poor adhesion of the interface layer due to uneven surface.

[0117] In some embodiments of the present invention, the heat-sealing layer comprises a modified polyolefin.

[0118] When the heat-sealing layer uses modified polyolefin, its surface energy and wear resistance are more suitable for working in synergy with the deposits inside the battery cell, enabling it to maintain stable contact under vibration conditions.

[0119] In some embodiments of the present invention, the melting point of the heat-sealing layer is T2, in °C, where 90 °C ≤ T2 ≤ 150 °C;

[0120] Preferably, 100℃≤T2≤140℃.

[0121] The melting point T2 of the heat-sealing layer can be detected by methods commonly used in the art; for example, in some embodiments, it is performed by a method including the following steps:

[0122] The heat-sealing layer was placed inside a DSC aluminum crucible and sealed. Under a nitrogen atmosphere (flow rate 50 mL / min), the temperature was increased from 25 °C to 200 °C at a heating rate of 10 °C / min. The melting endothermic curve was recorded, and the peak temperature of the endothermic peak was recorded as T2.

[0123] In some embodiments of the present invention, the melting point of the heat-sealing layer is T2, in °C, 1.8 × 10⁻⁶. 3 ≤K×T2≤2.5×10 4 ;

[0124] Preferably, 3.6 × 10 3 ≤K×T2≤2.0×10 4 .

[0125] K×T2 represents the degree of matching between the tendency of the adhesive layer to precipitate and deposit on the surface of the heat seal layer during the formation process and the thermal stability of the heat seal layer.

[0126] In detail, K×T2 includes, but is not limited to, 1.8×10 3 2×10 3 4×10 3 6×10 3 8×10 3 1×10 4 2×10 4 2.5×104 Or a range consisting of any two of them.

[0127] Preferably, K×T2 includes, but is not limited to, 3.6×10 3 4×10 3 5×10 3 6×10 3 7×10 3 8×10 3 9×10 3 1×10 4 2×10 4 Or a range consisting of any two of them.

[0128] Low-melting-point heat-sealing layers facilitate rapid softening during abnormal battery heat generation, enhancing safety performance in conjunction with internal pressure release. However, there is also an interaction between the precipitated interface layer and the low-melting-point heat-sealing layer. If the product of K and T2 is too large, it means that more adhesive precipitates form in the heat-sealing layer during formation. An excessively thick precipitate layer can actually reduce the heat-sealing strength at the encapsulation point, affecting the long-term sealing reliability of the battery. Controlling the product of K and T2 within a reasonable range allows for the acquisition of an anti-wear interface layer without compromising, and may even enhance, the stability of the encapsulation structure.

[0129] In some embodiments of the present invention, the melting point of the heat-sealing layer is T2, in °C, ΔT=|T1−T2|, and ΔT is 20 °C~50 °C.

[0130] In detail, ΔT includes, but is not limited to, a range of 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, or any two of these ranges.

[0131] The absolute value ΔT of the melting point difference between T1 and T2 directly affects the deposition morphology and adhesion of polymer precipitates on the heat-sealing layer surface. When ΔT is controlled within the range of 20~50℃, the shrinkage behavior of polymer chain segments during the cooling process tends to be synchronized with the crystallization kinetics of the heat-sealing layer. The precipitated interface layer can undergo a certain degree of molecular chain interpenetration and physical anchoring with the heat-sealing layer, forming a "cold welding" effect, which significantly improves the bonding strength between the interface layer and the inner surface of the aluminum-plastic film, making it less prone to peeling off under long-term vibration conditions.

[0132] When ΔT is large, the precipitated polymer segments are highly rigid and well-crystallized, while the molecular chains on the heat-sealing layer surface are flexible and have low surface energy. During the cooling process, when the rigid polymer segments undergo heterogeneous nucleation on the soft heat-sealing layer surface, the mismatch in crystallization kinetics between the two leads to stress concentration at the interface layer. This can cause microcracks to propagate during long-term cycling, weakening the durable protective effect of the interface layer.

[0133] In some embodiments of the present invention, the polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride copolymer, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trifluorochloroethylene copolymer, polyvinylidene fluoride-tetrafluoroethylene copolymer, polymethyl methacrylate, polyethyl methacrylate, polyacrylate, polyvinyl acetate, and ethylene-vinyl acetate copolymer.

[0134] The weight-average molecular weight of the polymer is Mw; 300,000 ≤ Mw ≤ 1,200,000;

[0135] Preferably, 400,000 ≤ Mw ≤ 800,000.

[0136] Polymer type and weight-average molecular weight can be detected using methods commonly used in the art. For example, in some embodiments, detection is performed using a method comprising the following steps: First, the polymer sample is analyzed for composition and structure using Fourier transform infrared spectroscopy (FTIR) or nuclear magnetic resonance spectroscopy (NMR) to qualitatively identify the polymer type by recognizing characteristic functional groups or molecular structures; then, its weight-average molecular weight is determined using gel permeation chromatography (GPC). The polymer sample is dissolved in a suitable solvent and injected into the gel permeation chromatograph. Separation is performed according to molecular size based on the volume exclusion mechanism. The signal is recorded using a differential refractive index detector or light scattering detector, and a calibration curve is established using standard samples with known molecular weights to calculate the polymer's weight-average molecular weight Mw.

[0137] In detail, the weight-average molecular weight Mw of the polymer includes, but is not limited to, a range of 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000 or any two of these.

[0138] Preferably, the weight-average molecular weight Mw of the polymer includes, but is not limited to, a range of 400,000, 450,000, 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000 or any two thereof.

[0139] Molecular weight directly affects the crystallization behavior and dissolution kinetics of polymers. When the molecular weight is too low, the cohesive force of the adhesive layer is insufficient, and it dissolves too quickly during the formation process, making it difficult to control the amount of precipitate. When the molecular weight is too high, the molecular chains are severely entangled, dissolving slowly, and the precipitate particles after formation are large and uneven. A suitable molecular weight ensures that the adhesive layer swells and dissolves appropriately during the formation process, ultimately forming a uniform, dense interface layer that is firmly bonded to the surface of the encapsulated body. At the same time, it ensures that the membrane base film is not excessively damaged, maintaining the mechanical strength and ion permeability of the membrane.

[0140] In some embodiments of the present invention, the electrode assembly further includes a negative electrode sheet;

[0141] The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on at least one side surface of the negative electrode current collector;

[0142] The porosity of the negative electrode active layer is P, where 25% ≤ P ≤ 45%;

[0143] Preferably, 30% ≤ P ≤ 40%.

[0144] In this invention, the porosity P of the negative electrode active layer can be obtained by density calculation based on the apparent density and true density of the negative electrode active layer, wherein the true density of the negative electrode active layer is obtained by helium true density meter.

[0145] In this invention, the porosity of the negative electrode active layer can be controlled by adjusting the solid content of the negative electrode slurry and the linear pressure of the hot rolling during the preparation of the negative electrode sheet.

[0146] For example, if the solid content of the negative electrode slurry increases, P decreases, and vice versa, while if the solid content of the negative electrode slurry increases, P decreases; or, if the linear pressure of the hot roller press increases, P decreases, and vice versa, while if the solid content of the negative electrode slurry increases, P decreases.

[0147] In detail, the porosity of the negative electrode active layer includes, but is not limited to, a range of 25%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 45%, or any two of these.

[0148] Preferably, 30% ≤ P ≤ 40%.

[0149] During hot-pressing formation, some dissolved sol material may seep into the negative electrode pores. If the negative electrode porosity is too low, the sol can easily clog the pores, hindering the lithium-ion insertion / extraction channels, increasing battery polarization, and deteriorating rate performance and low-temperature performance. If the porosity is too high, although it is less likely to clog the pores, the contact resistance between the active material and the current collector increases, and excessively high porosity means that the distribution of binder and conductive agent may be uneven, affecting cycle stability. Controlling the porosity within this range allows for the tolerance of a small amount of sol infiltration while ensuring lithium-ion transport efficiency and electrode structural integrity.

[0150] In some embodiments of the present invention, the package can be pre-formed by punching before housing the battery cell, such as... Figure 2 As shown, the encapsulation cavity includes a bent section B and a straight section A. The bent section B is located on both sides of the width direction of the battery cell; the straight section A extends along the width direction of the battery cell.

[0151] The radius of curvature R of the bent segment B satisfies: 1mm≤R≤5mm.

[0152] The radius of curvature R of the bend can be detected using methods commonly used in the art, for example, in some embodiments, by a method including the following steps:

[0153] First, obtain cross-sectional images or three-dimensional topographic data of the bent section of the encapsulation cavity. Then, use a two-dimensional image measuring instrument, optical profilometer, or coordinate measuring machine to perform non-contact scanning or point sampling on the arc profile of the bent section. The measurement software automatically extracts multiple coordinate points on the arc profile and performs arc fitting to calculate the radius of curvature R of the bent section.

[0154] In detail, the radius of curvature R of the bend is including, but is not limited to, a range of 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, or any two of these ranges.

[0155] During the stamping and encapsulation process of the package, the bending section experiences the most severe material deformation. If the radius of curvature of the bending section is too small (<1mm), the package will be excessively stretched and thinned at this point, and the molten adhesive layer will easily accumulate at the corners during encapsulation, forming localized stress concentration points, making it more susceptible to puncture by the current collector edge under vibration. If the radius of curvature is too large (>5mm), the battery space utilization will decrease. A suitable radius of curvature can improve the flow distribution of the adhesive layer at the corners, reduce accumulation, ensure uniform package thickness at the corners, and thus improve overall wear resistance.

[0156] In some embodiments of the present invention, the electrode assembly further includes a positive electrode sheet;

[0157] A separator is placed between the positive electrode and the negative electrode.

[0158] The electrode assembly is further composed of a positive electrode, a negative electrode, and a separator disposed between the two. The separator serves as an ion conduction channel on the one hand and inhibits direct contact between the positive and negative electrodes on the other hand, thus ensuring the basic safety of the battery cell after assembly.

[0159] In some embodiments of the present invention, the peel strength between the separator and the positive electrode is F1, 3N / m≤F1≤50N / m;

[0160] Preferably, 5N / m≤F1≤30N / m.

[0161] In some embodiments, the peel strength F1 between the separator and the positive electrode is tested by a method including the following steps: Referring to GB / T 2790-1995 or a similar standard, the formed battery is disassembled, and the composite containing the separator and electrode is removed and cut into strips 25 mm wide. A short section is pre-separated at one end of the separator and the electrode, and each section is clamped in the upper and lower clamps of a tensile testing machine. A 180° peel is performed at a speed of 100 mm / min, and the average force value during the stable peeling stage is recorded.

[0162] In detail, the peel strength F1 between the separator and the positive electrode includes, but is not limited to, 3 N / m, 10 N / m, 15 N / m, 20 N / m, 25 N / m, 30 N / m, 35 N / m, 40 N / m, 45 N / m, 50 N / m or any combination thereof.

[0163] Preferably, 5N / m≤F1≤30N / m.

[0164] This adhesive strength reflects the bonding state between the diaphragm and the electrode interface. A peel strength that is too low (<3 N / m) indicates poor bonding between the interface layer and the electrode, making the interface prone to detachment during charging and discharging, increasing interfacial impedance, and accelerating capacity decay. A peel strength that is too high (>50 N / m), while indicating strong bonding, may mean that the adhesive layer has excessively penetrated to the electrode surface, blocking the surface of the active material and affecting ion exchange. This range ensures good interfacial contact while avoiding over-coverage.

[0165] In some embodiments of the present invention, the peel strength between the separator and the negative electrode sheet is F2, 3N / m≤F2≤50N / m; preferably, 5N / m≤F2≤30N / m.

[0166] In detail, the peel strength F2 between the separator and the negative electrode includes, but is not limited to, a range of 3 N / m, 10 N / m, 15 N / m, 20 N / m, 25 N / m, 30 N / m, 35 N / m, 40 N / m, 45 N / m, 50 N / m, or any combination thereof.

[0167] Preferably, 5N / m≤F2≤30N / m.

[0168] This peel strength reflects the bonding state between the separator and the electrode interface. A peel strength that is too low (<3 N / m) indicates poor bonding between the interface layer and the electrode, making the interface prone to detachment during charging and discharging, increasing interfacial impedance, and accelerating capacity decay. A peel strength that is too high (>50 N / m), while indicating strong bonding, may mean that the adhesive layer has excessively penetrated to the electrode surface, blocking the surface of the active material and affecting ion exchange. This range ensures good interfacial contact while avoiding over-coverage.

[0169] In some embodiments of the present invention, the peel strength between the battery cell and the package is F3, where 3N / m≤F3≤30N / m.

[0170] The peel strength between the battery cell and the package can be tested using a method that includes the following steps:

[0171] (1) Sample preparation: Take the finished battery that has been hot-pressed and fully discharged. Cut a sample with a width of 25 mm and a length of at least 120 mm along the length of the large surface of the battery (non-sealed area). Carefully separate the cell from the inner surface of the aluminum-plastic film at one end of the sample by about 20-30 mm to form two free ends.

[0172] (2) Test conditions: ambient temperature 23±2℃, relative humidity ≤65%.

[0173] (3) Test procedure: Clamp the separated aluminum-plastic film end and the battery cell end in the upper and lower clamps of the universal tensile testing machine, and perform a 180° peel test at a tensile speed of 100 mm / min. Record the peel force value as a function of displacement curve, and take the average peel force when the peel curve enters the stable platform area (usually the peel 50 mm range), which is F, in N / m.

[0174] (4) Effective sample size: at least 5 samples should be tested and the arithmetic mean should be taken.

[0175] In detail, the peel strength between the cell and the package includes, but is not limited to, a range of 3 N / m, 5 N / m, 10 N / m, 15 N / m, 20 N / m, 25 N / m, 30 N / m, or any two of these ranges.

[0176] This peel strength characterizes the ability of the precipitated interface layer to "anchor" the cell to the package. Moderate peel strength effectively constrains the lateral movement of the cell within the casing, significantly reducing the relative displacement between the cell and the aluminum-plastic film under vibration conditions. This fundamentally reduces frictional wear on the package layer from the current collector edge and prevents short circuits caused by tearing of the aluminum foil during abnormal battery impacts, thus avoiding the risk of fire failure due to excessive binding.

[0177] In some embodiments, the battery provided by the present invention is prepared by a method comprising the following steps:

[0178] The electrode assembly is encapsulated in a membrane housing, then injected with a non-aqueous electrolyte, and hot-pressed to form the battery; the hot-pressing temperature is T3, in °C.

[0179] In some embodiments, T3 ≤ T1 - 35℃;

[0180] In detail, the difference (T1-T3) between the melting point T1 of the polymer and the temperature T3 of hot pressing includes, but is not limited to, 35°C, 40°C, 45°C, 50°C or other ranges greater than or equal to 35°C.

[0181] T3 is much lower than the melting point T1 of the diaphragm adhesive layer to suppress thermal macro-melting of the adhesive layer. It only allows the adhesive layer to undergo controllable solvation, surface swelling and partial dissolution under the action of the electrolyte. This temperature difference ensures that the heat of formation is insufficient to destroy the crystalline structure of the polymer in the diaphragm adhesive layer, so that the main skeleton of the adhesive layer can be preserved and the strength of the diaphragm base membrane is prevented from dropping sharply due to excessive loss of the adhesive layer.

[0182] In some embodiments of the present invention, T3 ≤ T2 - 25℃.

[0183] In detail, the difference (T2-T3) between the melting point T2 of the heat-sealing layer and the temperature T3 of hot pressing includes, but is not limited to, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C or other ranges greater than or equal to 25°C.

[0184] T3 is significantly lower than the melting point T2 of the heat seal layer, preventing the PP layer from softening and deforming during hot pressing, which could lead to creep or deterioration of the seal.

[0185] In some embodiments of the present invention, 75℃≤T3≤95℃.

[0186] In detail, the hot pressing temperature includes, but is not limited to, 75°C, 80°C, 85°C, 90°C, 95°C, or any combination thereof.

[0187] When the hot-pressing temperature is within the above-mentioned range, a balance can be achieved between practical production operability and electrolyte activity. Within this preferred temperature range, although the temperature is much lower than T1, the highly polar, small-molecule solvent PC in the electrolyte possesses sufficient penetration kinetic energy to efficiently weaken the van der Waals forces between polymer molecular chains and localized crystallization regions, inducing selective swelling of the adhesive layer surface and releasing an appropriate amount of free polymer segments. The amount of polymer precipitated is mainly determined by the thermodynamic swelling balance characterized by the precipitation coefficient K (=M×T1). The higher the K value, the stronger the tendency for dissolution and precipitation per unit time, while T3 can regulate the dissolution rate. By controlling T3 within a lower window of 75~95℃, it is ensured that the precipitation reaction is completed within a reasonable time, and the driving force of supersaturated polymer precipitation on the surface of the encapsulated body during the cooling stage can be utilized to spontaneously form a uniformly thick and firmly adhered interface layer.

[0188] Secondly, the present invention provides an electrical device including the battery as described above.

[0189] It is understood that the electrical device of this application includes the aforementioned battery, and therefore has the same technical effect as the battery of this application, which will not be described again here.

[0190] Specifically, the electrical device can be a consumer electronics product, an energy storage device, an electric vehicle, etc. Examples include, but are not limited to, mobile phones, tablets, laptops, Bluetooth headsets, smartwatches, portable power banks, energy storage battery packs, drones, electric toys, electric bicycles, electric cars, and electric boats.

[0191] The present invention will now be described in detail through specific embodiments.

[0192] Example 1

[0193] The battery preparation method provided by the present invention includes the following steps:

[0194] 1. Preparation of the positive electrode:

[0195] Lithium cobalt oxide (LiCoO2), conductive agent Super P, and binder PVDF are mixed in a mass ratio of 96:2:2. N-methylpyrrolidone is added, and the mixture is stirred at high speed to obtain a uniformly dispersed mixture containing the positive electrode active material, i.e., positive electrode active slurry. The above positive electrode slurry is uniformly coated on both sides of aluminum foil, and after drying, rolling, and slitting, a positive electrode sheet is obtained.

[0196] 2. Preparation of the negative electrode:

[0197] Artificial graphite (anode active material), Super P (conductive agent), sodium carboxymethyl cellulose (CMC) (thickener), and styrene-butadiene rubber (SBR) (binder) are mixed in a mass ratio of 95:1.5:1.5:2. Deionized water is added, and the mixture is thoroughly mixed under vacuum until a uniform and fluid anode slurry is formed. The anode slurry is then uniformly coated on both sides of a copper foil, and after drying, rolling, and slitting, the anode sheet is obtained.

[0198] 3. Diaphragm preparation

[0199] Using 5μm polyethylene (PE) as a porous base membrane, a 1μm thick coating of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) with a weight-average molecular weight Mw of 600,000 was coated on both sides of the porous base membrane facing the positive and negative electrodes. The coated membrane was dried in an oven at 70℃ to remove the solvent, and the melting point T1 of the adhesive layer was measured to be 140℃ by differential scanning calorimetry (DSC).

[0200] 4. Electrolyte preparation

[0201] The electrolyte was prepared in a glove box filled with high-purity argon (water and oxygen content both <1 ppm). Lithium hexafluorophosphate (LiPF6) was dissolved as the lithium salt in a non-aqueous organic solvent, with the lithium salt comprising 12% of the total electrolyte mass. The remaining 88% was a non-aqueous organic solvent, with the following mass ratios of propylene carbonate (PC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and diethyl carbonate (DEC) being 15:50:25:10. The calculated mass percentages of each solvent based on the total electrolyte mass were: propylene carbonate 13.2%, ethyl methyl carbonate 44%, ethylene carbonate 22%, and diethyl carbonate 8.8%. The mass ratio of PC to EMC, M = PC / EMC = 15 / 50 = 0.30.

[0202] Based on the melting point of the diaphragm adhesive layer T1=140℃, the gelation coefficient K=M×T1=0.30×140=42.

[0203] After mixing the above solvents evenly, slowly add LiPF6 and stir until completely dissolved to obtain a non-aqueous electrolyte.

[0204] 5. Package and encapsulation

[0205] A laminated aluminum-plastic film was selected, consisting of, from the outside in, an outer protective layer (nylon layer), a first adhesive layer, an aluminum foil layer, a second adhesive layer, and a heat-sealing layer (modified polypropylene PP layer). The melting point T2 of the heat-sealing layer, determined by DSC, is 110 °C, the heat-sealing layer thickness is 40 μm, and its surface roughness Ra is 0.3 μm (measured using a stylus roughness tester). Based on the melting point T1 of the diaphragm adhesive layer (140 °C) and the separation coefficient K (42), K × T2 = 42 × 110 = 4.62 * 10⁻⁶ 3 The casing is formed by stamping with a die to create a recess to accommodate the battery cell, with the radius of curvature R of the bent section controlled to be 3 mm. The stamped package is then cut to the required size for later use.

[0206] 6. Winding and Assembly

[0207] The positive electrode sheet prepared in step (1), the separator prepared in step (3), and the negative electrode sheet prepared in step (2) are stacked in order to ensure that the separator is between the positive and negative electrodes and plays a role in isolation. Then, the bare battery is obtained by winding. The bare battery cell is placed in the outer packaging aluminum-plastic film, and the electrolyte prepared in step (4) is injected into the aluminum-plastic film. After injection, it is left to stand for 48 hours to allow the electrolyte to fully wet the electrode sheet and the separator.

[0208] 7. Hot pressing formation

[0209] The pre-sealed battery is placed in a hot-pressing formation fixture, the hot-pressing formation temperature T3 is set to 85℃, and the hot-pressing formation pressure is 1.1 MPa.

[0210] A stepped charging regime was used for formation: first, constant current charging at 0.05C to 10% of the rated capacity, then constant current charging at 0.1C to 30% of the rated capacity, and finally constant current charging at 0.2C to 90% of the rated capacity. During formation, the highly polar small-molecule PC in the electrolyte solubilized and penetrated the PVDF adhesive layer surface at 85°C, inducing controlled surface swelling and partial dissolution of the adhesive layer, releasing an appropriate amount of free polymer segments. In the subsequent cooling stage, the dissolved PVDF segments precipitated from the electrolyte due to reduced solubility, and uniformly deposited on the PP layer on the inner surface of the aluminum-plastic film, forming a wear-resistant interface layer of suitable thickness, density, and strong adhesion. After formation, the battery was vacuum-sealed, degassed, and the excess material of the tabs was trimmed to obtain the final soft-pack lithium-ion battery.

[0211] According to the test, the peel strength F1 between the separator adhesive layer and the positive electrode of the battery obtained in this embodiment is 15 N / m, the peel strength F2 between the separator adhesive layer and the negative electrode is 18 N / m, and the peel strength F3 between the cell (including the stack of electrode and separator) and the inner surface of the aluminum-plastic film is 10 N / m.

[0212] Examples 2 to 27 and Comparative Examples 1 to 2 provide battery preparation methods that are basically the same as those in Example 1, except that the mass percentage of various substances in the electrolyte, the type of polymer in the separator layer, the weight-average molecular weight, the thickness and roughness of the heat-sealing layer, and the melting point are adjusted.

[0213] See Table 1-1 and Table 1-2 for details.

[0214] Table 1-1

[0215]

[0216] Table 1-2

[0217]

[0218] Test case

[0219] 1. Polymer melting point T1 test

[0220] Differential scanning calorimetry (DSC) was used. Approximately 3–5 mg of powdered sample was collected by gently scraping off the surface adhesive layer with a blade and placed in a sealed DSC aluminum crucible. Under a nitrogen atmosphere (flow rate 50 mL / min), the sample was heated from 25 °C to 200 °C at a heating rate of 10 °C / min. The melting endothermic curve was recorded, and the peak temperature of the endothermic peak was recorded as T1.

[0221] 2. Melting point T2 test of heat seal layer

[0222] The heat-sealing layer was placed inside a DSC aluminum crucible and sealed. Under a nitrogen atmosphere (flow rate 50 mL / min), the temperature was increased from 25 °C to 200 °C at a heating rate of 10 °C / min. The melting endothermic curve was recorded, and the peak temperature of the endothermic peak was recorded as T2.

[0223] 3. Separation strength test between the separator and the positive and negative electrode plates

[0224] Referring to GB / T 2790-1995, the formed battery was disassembled, and the composite containing the separator and electrode was removed and cut into strips 25 mm wide. A small section was pre-separated from one end of the separator and electrode, and clamped in the upper and lower clamps of a tensile testing machine. The separator was peeled 180° at a speed of 100 mm / min, and the average force value during the stable peeling stage was recorded.

[0225] 4. Peel strength test between battery cell and package

[0226] (1) Sample preparation: Take the finished battery that has been hot-pressed and fully discharged. Cut a sample with a width of 25 mm and a length of at least 120 mm along the length of the large surface of the battery (non-sealed area). Carefully separate the cell from the inner surface of the aluminum-plastic film at one end of the sample by about 20-30 mm to form two free ends.

[0227] (2) Test conditions: ambient temperature 23±2℃, relative humidity ≤65%.

[0228] (3) Test procedure: Clamp the separated aluminum-plastic film end and the battery cell end in the upper and lower clamps of the universal tensile testing machine, and perform a 180° peel test at a tensile speed of 100 mm / min. Record the peel force value as a function of displacement curve, and take the average peel force when the peel curve enters the stable platform area (usually the peel 50 mm range), which is F, in N / m.

[0229] (4) Effective sample size: at least 5 samples should be tested and the arithmetic mean should be taken.

[0230] 5. Determination of the mass percentage of propylene carbonate (PC) and ethyl methyl carbonate (EMC) in the electrolyte.

[0231] The detection was performed using gas chromatography-mass spectrometry. The specific steps are as follows:

[0232] (1) Sample pretreatment: Disassemble the battery in a glove box, take 0.5g of electrolyte, add anhydrous acetone to make up to 5mL, add 0.05g of n-butanol internal standard, mix well, filter through a 0.22μm organic phase membrane, and wait for testing.

[0233] (2) Preparation of standard solutions: Weigh ethylene carbonate standard and dimethyl carbonate standard, and prepare standard solutions with concentrations of 0.1 mg / mL, 0.5 mg / mL, 1.0 mg / mL, 2.0 mg / mL and 5.0 mg / mL with anhydrous acetone. Add 0.05 g of n-butanol internal standard to each standard solution.

[0234] (3) Chromatographic conditions: The column was DB-5MS, with a size of 30m×0.25mm×0.25μm; the injection port temperature was 250℃; the carrier gas was high-purity helium, with a flow rate of 1.0mL / min; the split ratio was 20:1; the column temperature was initially 50℃ and held for 3min, then increased to 220℃ at 10℃ / min and held for 5min; the mass spectrometer detector was an EI source, and the scanning m / z range was 20 to 300.

[0235] (4) Qualitative and quantitative analysis: qualitative analysis is performed based on the retention time and mass spectrometry characteristic ions of ethylene carbonate and dimethyl carbonate standards; standard curves are plotted based on the peak area ratio of the target analyte to the internal standard, and the concentrations of ethylene carbonate and dimethyl carbonate are calculated.

[0236] (5) Calculation of results: Ethylene carbonate mass percentage = (C×V / m)×100%, where C is the ethylene carbonate concentration calculated from the standard curve, V is the volume of the liquid to be tested, and m is the mass of the electrolyte sample. Dimethyl carbonate mass percentage is calculated using the same formula.

[0237] 6. Radius of curvature detection

[0238] (1) Sample preparation: Take the sample of the bent section of the encapsulation cavity and cut it along the direction perpendicular to the extension of the bent section to obtain a cross section containing the arc contour of the bent section. Grind with 2000-grit sandpaper and polish with diamond polishing paste.

[0239] (2) Image acquisition: A two-dimensional image measuring instrument with a magnification of 100 times was used to scan the arc contour of the bending section, with a sampling point spacing of 0.02 mm.

[0240] (3) Circular arc fitting: Import the collected contour coordinate points into the measurement software, select 10 coordinate points in the curved arc area, and perform least squares circular arc fitting.

[0241] (4) Result reading: The radius of curvature R of the bent segment obtained by fitting is the radius of curvature R of the bent segment, in mm. Five samples were tested and the arithmetic mean was taken.

[0242] 7. Roughness Inspection

[0243] (1) Sample preparation: Take the surface of the heat-sealed layer of the package that is close to the cell as the test surface. Clean the surface with anhydrous ethanol and let it air dry.

[0244] (2) Measuring instrument: A stylus-type surface roughness tester was used, with a diamond stylus tip radius of 2μm and a measuring force of 0.75mN.

[0245] (3) Measurement conditions: The sampling length is 0.8 mm, the evaluation length is 4 mm, and the measurement direction is perpendicular to the processing texture direction of the heat seal layer surface. Five positions are measured for each sample.

[0246] (4) Result calculation: The instrument automatically records the profile curve and calculates the arithmetic mean deviation Ra, in μm. The arithmetic mean of Ra at 5 locations is taken as the surface roughness Ra of the heat seal layer of the sample.

[0247] 8. Heat seal layer wear rate test

[0248] Referring to GB / T 2423.10, the frequency was 10-55Hz, the amplitude was 0.35mm, and the vibration duration was 50h in each of the XYZ directions. After testing, the package was disassembled, and the heat-sealing layer was separated. The degree of damage to the heat-sealing layer was tested using a 3D microscope, a 3D profilometer, and a CP (contrast plate oscillator) (measuring the remaining thickness of the worn heat-sealing layer after vibration), and the wear rate of the heat-sealing layer was calculated using the following formula:

[0249] Heat seal wear rate = (original thickness of heat seal - thickness of heat seal after wear) / original thickness of heat seal × 100%.

[0250] The test calculation results are shown in Table 2.

[0251] 9. Cyclic performance testing

[0252] The batteries prepared in the examples and comparative examples were subjected to a 45°C cycling test. The specific test method is as follows:

[0253] S1. Place the prepared battery in a constant temperature environment of 45℃, charge it to 4.3V with constant current and constant voltage at 1C, cut off current at 0.05C, let it stand for 10 minutes after it is fully charged, and discharge it to the cutoff voltage of 2.5V with constant current at 5C; perform 3 complete charge and discharge cycles and take the discharge capacity of the 3rd cycle as the initial capacity C1.

[0254] S2. Continue to cycle according to the charge and discharge regime (1C charge / 5C discharge) of step S1; when the number of cycles reaches 800, stop the test and record the discharge capacity of the 800th cycle as C2; then the capacity retention rate (%) = C2 / C1×100%.

[0255] The test calculation results are shown in Table 2.

[0256] Table 2

[0257]

[0258] As shown in Table 2, the wear rate of the heat seal layer of the battery provided in the embodiment of the present invention is no higher than 43.4%, and the capacity retention rate of 800T is no less than 68.3%. It can be seen that the battery provided by the present invention has excellent cycle performance and safety.

[0259] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.

Claims

1. A battery, characterized in that, The package includes a package body and a battery cell, wherein the package body includes a package cavity and the battery cell is packaged within the package cavity; The battery cell includes an electrode assembly and a non-aqueous electrolyte; The electrode assembly includes a diaphragm; The diaphragm includes a porous base membrane and an adhesive layer disposed on at least one surface of the porous base membrane; The adhesive layer comprises a polymer; The non-aqueous electrolyte includes propylene carbonate and ethyl methyl carbonate; Where K = M * T1, 12 ≤ K ≤ 165; M is the mass ratio of propylene carbonate to methyl ethyl carbonate, and T1 is the melting point of the polymer, in °C.

2. The battery according to claim 1, characterized in that, 15≤K≤140。 3. The battery according to claim 1, characterized in that, 0.08≤M≤1.0; And / or, 130℃≤T1≤175℃; preferably, 140℃≤T1≤165℃.

4. The battery according to claim 1, characterized in that, The non-aqueous electrolyte meets at least one of the following conditions: (1) Based on the total mass of the non-aqueous electrolyte, the mass percentage of propylene carbonate is 5% to 20%; (2) Based on the total mass of the non-aqueous electrolyte, the mass percentage of methyl ethyl carbonate is 20% to 60%; (3) The non-aqueous electrolyte also includes lithium salt, and the mass percentage of the lithium salt is 10% to 15% based on the total mass of the non-aqueous electrolyte; (4) The non-aqueous electrolyte also includes at least one of ethylene carbonate, diethyl carbonate, dimethyl carbonate, and ethyl propyl carbonate.

5. The battery according to any one of claims 1-4, characterized in that, The package includes an outer protective layer, a first adhesive layer, an aluminum foil layer, a second adhesive layer, and a heat-sealing layer stacked in sequence, with the heat-sealing layer close to the battery cell; The package satisfies at least one of the following conditions: (1) The thickness of the heat-sealing layer is 20μm~50μm; (2) The surface roughness Ra of the heat-sealing layer on the side closest to the battery cell is ≤0.5μm; (3) The heat-sealing layer comprises a modified polyolefin; (4) The melting point of the heat-sealing layer is T2, in °C, and 90 °C ≤ T2 ≤ 150 °C; Preferably, 100℃≤T2≤140℃; (5) The melting point of the heat-sealing layer is T2, in °C, 1.8 × 10⁻⁶. 3 ≤K×T2≤2.5×10 4 ; Preferably, 3.6 × 10 3 ≤K×T2≤2.0×10 4 ; (6) The melting point of the heat-sealing layer is T2, in °C, ΔT=|T2−T1|, and ΔT is 20℃~50℃.

6. The battery according to any one of claims 1-4, characterized in that, The polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride copolymer, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-trifluorochloroethylene copolymer, polyvinylidene fluoride-tetrafluoroethylene copolymer, polymethyl methacrylate, polyethyl methacrylate, polyacrylate, polyvinyl acetate, and ethylene-vinyl acetate copolymer. The weight-average molecular weight of the polymer is Mw; 300,000 ≤ Mw ≤ 1,200,000; Preferably, 400,000 ≤ Mw ≤ 800,000.

7. The battery according to any one of claims 1-4, characterized in that, The electrode assembly also includes a negative electrode sheet; The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on at least one side surface of the negative electrode current collector; The porosity of the negative electrode active layer is P, where 25% ≤ P ≤ 45%; Preferably, 30% ≤ P ≤ 40%.

8. The battery according to any one of claims 1-4, characterized in that, The encapsulation cavity includes a bent section and a straight section. The bent section is located on both sides of the width direction of the battery cell; the straight section is located in the width direction of the battery cell. The radius of curvature R of the bent segment satisfies: 1mm≤R≤5mm.

9. The battery according to claim 7, characterized in that, The electrode assembly also includes a positive electrode sheet; The separator is disposed between the positive electrode and the negative electrode; The battery satisfies at least one of the following conditions: (1) The peel strength between the separator and the positive electrode is F1, 3N / m≤F1≤50N / m; Preferably, 5 N / m ≤ F1 ≤ 30 N / m; (2) The peel strength between the diaphragm and the negative electrode sheet is F2, 3N / m≤F2≤50N / m; preferably, 5N / m≤F2≤30N / m; (3) The peel strength between the battery cell and the package is F3, 3N / m≤F3≤30N / m.

10. An electrical appliance, characterized in that, Includes the battery as described in any one of claims 1-9.