A battery and electronic device
By using a specific composition of negative electrode active materials and electrolyte additives, the problem of balancing battery energy density, cycle life, and safety is solved, forming an adaptive SEI film that optimizes interface stability and ion transport, thereby improving the battery's high-temperature cycling and safety performance.
Patent Information
- Application Number
- CN202611526368.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-10
AI Technical Summary
How to improve battery energy density while taking into account cycle life, high-temperature performance and safety, especially the volume expansion of silicon-based materials and interfacial side reactions of traditional carbonate electrolytes.
By employing a specific composition of negative electrode active material and electrolyte additives, including a combination of graphite materials, bulk silicon-based materials and spherical silicon-based materials, and combining them with a first additive of a specific structure, a differentiated SEI film is formed to improve interfacial stability, and ion transport and interfacial reactions are optimized by regulating the electrolyte composition.
It significantly improves the high-temperature cycle performance, charging performance and safety of batteries. By forming SEI films with different adaptability on the surfaces of graphite and silicon-based materials, it optimizes the interface impedance and ion transport dynamics, thereby achieving an overall performance improvement.
Smart Images

Figure SMS_8 
Figure QLYQS_1 
Figure QLYQS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery technology, specifically relating to a battery and an electronic device. Background Technology
[0002] With the development of technology and the increase in energy demand, high-energy-density batteries have become a research hotspot in the field of energy storage. In recent years, researchers have been continuously optimizing key materials such as positive and negative electrode materials and electrolytes to further improve the energy density and cycle life of batteries, thereby helping to promote the rapid development of the new energy industry.
[0003] On the one hand, the anode material has a significant impact on the energy density and cycle life of a battery. Graphite is widely used due to its good structural stability and ease of synthesis, but its theoretical capacity is relatively low. Silicon-based materials can provide more than three times the theoretical capacity of graphite, giving them an unparalleled advantage in future battery applications. However, silicon-based materials also face challenges such as volume expansion, short cycle life, and high cost. Currently, although volume expansion can be reduced by mixing with graphite, problems such as poor uniformity and difficulty in generating strong interaction forces exist, making it impossible to simultaneously achieve optimal battery performance at both room temperature and high temperatures.
[0004] On the other hand, as an ion transport medium between electrode materials, the composition and performance of the electrolyte can be controlled to improve the electrochemical performance and safety of the battery. However, traditional carbonate electrolytes are not suitable for high-voltage battery systems. At high temperatures, interfacial side reactions between the electrolyte and electrode materials intensify, ultimately leading to system degradation and capacity decay.
[0005] Therefore, how to improve battery energy density while also taking into account performance indicators such as cycle life, high-temperature performance, and safety is a problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a battery and electronic device. The present invention significantly improves the battery's cycle performance, charging performance, and high-temperature performance by comprehensively controlling the composition of the negative electrode active material and the electrolyte composition.
[0007] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides a battery, the battery comprising a negative electrode sheet and an electrolyte, the negative electrode sheet comprising a negative electrode active material, wherein the negative electrode active material comprises, based on the total mass of the negative electrode active material as 100%, a graphite material comprising 50% to 70% by mass, a bulk silicon-based material comprising 20% to 30% by mass, and a spherical silicon-based material comprising 10% to 20% by mass; The electrolyte comprises an electrolyte salt, a non-aqueous solvent, and an additive, wherein the additive comprises a first additive, which comprises a compound with the structure shown in Formula 1: Formula 1; R1 and R2 are each independently selected from -H, C2~C10 hydrocarbon group, C2~C10 carbonate group, sulfate group, phosphate group, silicate group or borate group, and R1 and R2 cannot be -H at the same time.
[0008] This invention significantly improves the high-temperature cycle performance, high-temperature storage performance, and safety of batteries through the synergistic effect of a specific composition of negative electrode active materials and electrolyte additives, as specifically demonstrated below: (1) By introducing a first additive with a specific structure into the electrolyte, a dense and uniform solid electrolyte film can be formed on the positive and negative electrode surfaces, effectively isolating the electrolyte from direct contact with the electrode active materials, reducing interfacial side reactions, and improving the cycle performance of the battery. In addition, the first additive has a differentiated mechanism of action for different types of negative electrode active materials, thereby producing synergistic effects. For example, for the graphite surface, since the reduction potential of the first additive on the graphite surface is higher than that of the electrolyte solvent, it can preferentially undergo reduction decomposition on the graphite negative electrode surface to form a thin and dense SEI film. This SEI film can passivate the active sites on the graphite surface and improve the gas generation phenomenon caused by the catalytic effect of the graphite layer. At the same time, the SEI film can also inhibit the co-intercalation of solvent molecules, prevent the graphite layer from peeling off, and effectively reduce the interfacial impedance, improving the transport path of metal ions at the graphite interface. For another example, for silicon-based materials, due to the severe volume expansion (up to 300% or more) of silicon-based materials during charging and discharging, conventional SEI films repeatedly rupture and regenerate, continuously consuming active metal ions and electrolyte, resulting in rapid capacity decay of the battery. The introduction of this first additive allows for the reduction and formation of a SEI film with improved elasticity and flexibility on the silicon-based surface, enabling it to withstand repeated volume expansion and contraction of the silicon-based material without cracking. Furthermore, the reduction potential of this first additive is lower than that of the main solvent in the electrolyte, allowing it to preferentially form a protective layer on the silicon-based surface. This prevents direct contact between the electrolyte and the silicon active material, thereby suppressing interfacial side reactions and significantly improving the battery's cycle performance, charge-discharge performance, high-temperature performance, and safety performance.
[0009] (2) Traditional silicon-based anode active materials are mostly bulk materials, characterized by low cost and good overall performance. They have shorter ion migration paths during charging and discharging, resulting in better fast charging performance. However, their voltage resistance is poor, and the material particles are easily crushed during battery manufacturing. Spherical silicon-based anode active materials perfectly compensate for this shortcoming. During battery cycling, their spherical shape reduces particle breakage and improves stability at high temperatures and high voltages. However, compared to graphite anode active materials, silicon-based anode active materials still have poor cycle stability, and the ion migration paths during charging and discharging are longer, resulting in relatively poor fast charging performance. In particular, after high-temperature storage, the SEI film on the material surface will be severely damaged, which is not conducive to improving the thermal shock performance of the battery. Based on this, the negative electrode active material provided by the present invention adopts a combination of graphite material, bulk silicon-based material and spherical silicon-based material in a specific mass ratio. Through differentiated but complementary effects, a rigid, low-resistance SEI film is formed on the graphite surface to ensure rapid lithium insertion and extraction, and a flexible, high-toughness SEI film is formed on the silicon-based surface to adapt to volume changes. This differentiated film formation behavior effectively improves the interfacial stability of different negative electrode active materials, and comprehensively optimizes the interfacial impedance, ion transport kinetics and structural integrity of the negative electrode hybrid system. This maximizes the performance advantages of each component material and optimizes the overall performance of the battery.
[0010] It should be noted that the C2~C10 hydrocarbon groups specifically refer to hydrocarbon groups with 2~10 carbon atoms, such as alkyl groups with 2~10 carbon atoms, alkenyl groups with 2~10 carbon atoms, or alkynyl groups with 2~10 carbon atoms.
[0011] As an example, the alkyl group having 2 to 10 carbon atoms includes, but is not limited to, at least one of ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, n-pentyl, isopentyl, tert-pentyl, neopentyl, n-hexyl, isohexyl, 2-hexyl, 3-hexyl, n-heptyl, 2-heptyl, 3-heptyl, isoheptyl, n-octyl, cyclooctyl, nonyl, or decyl.
[0012] As an example, the alkenyl group having 2 to 10 carbon atoms includes, but is not limited to, at least one of vinyl, n-propenyl, isopropenyl, n-butenyl, isobutenyl, sec-butenyl, tert-butenyl, cyclobutenyl, n-pentenyl, isopentenyl, tert-pentenyl, neopentenyl, n-hexenyl, isohexenyl, n-heptenyl, 2-heptenyl, 3-heptenyl, isoheptenyl, n-octenyl, nonenyl, or decenyl.
[0013] As an example, the alkyne group having 2 to 10 carbon atoms includes, but is not limited to, at least one of ethynyl, 1-propynyl, 2-propynyl, 1-n-butynyl, 2-n-butynyl, isobutynyl, 1-pentynyl, 1-hexynyl, 1-heptynyl, 1-octyynyl, 1-nonynyl, or 1-decynyl.
[0014] The C2~C10 carbonate group specifically refers to a carbonate group with 2~10 carbon atoms, such as 2, 3, 4, 5, 6, 7, 8, 9 or 10.
[0015] The sulfate ester group exemplarily includes a chain sulfate ester group or a cyclic sulfate ester group, the phosphate ester group exemplarily includes a chain phosphate ester group or a cyclic phosphate ester group, the silicate ester group exemplarily includes a chain silicate ester group or a cyclic silicate ester group, and the borate ester group exemplarily includes a chain borate ester group or a cyclic borate ester group.
[0016] Preferably, based on the total mass of the negative electrode active material as 100%, the mass percentage of the graphite material is 62% to 65%, for example, it can be 62%, 63%, 64% or 65%, etc., not limited to the listed values, and other unlisted values within this range are also applicable.
[0017] Preferably, based on the total mass of the negative electrode active material as 100%, the mass percentage of the bulk silicon-based material is 20% to 23%, for example, it can be 20%, 21%, 22% or 23%, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0018] Preferably, based on the total mass of the negative electrode active material as 100%, the mass percentage of the spherical silicon-based material is 12% to 18%, for example, it can be 12%, 13%, 14%, 15%, 16%, 17% or 18%, etc., not limited to the listed values, and other unlisted values within this range are also applicable.
[0019] This invention further adjusts the mass ratio of graphite material, bulk silicon-based material, and spherical silicon-based material, so that graphite material provides framework stability and fast ion insertion / extraction channels, spherical silicon-based material plays an isotropic expansion buffer role, and bulk silicon-based material provides high capacity supplementation. The three work together to achieve a balance between energy density and cycle life, thereby significantly improving the cycle performance, charging performance, and safety performance of the battery.
[0020] Preferably, the D of the graphite material v The particle size of 50 is 15μm to 16μm, for example, it can be 15μm, 15.2μm, 15.5μm, 15.8μm or 16μm, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0021] Preferably, the D of the bulk silicon-based material v The particle size is 7μm to 9μm, for example, it can be 7μm, 7.5μm, 8μm, 8.5μm or 9μm, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0022] Preferably, the D of the spherical silicon-based material v The particle size is 7μm to 9μm, for example, it can be 7μm, 7.5μm, 8μm, 8.5μm or 9μm, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0023] In this invention, the silicon-based material exemplary includes silicon-carbon materials and / or silicon-oxygen materials.
[0024] More preferably, the specific capacity of the silicon-based material is 1400mAh / g to 1950mAh / g.
[0025] More preferably, R1 and R2 are each independently selected from C3 to C8 carbonate groups, sulfate groups, phosphate groups, silicate groups or borate groups, and R1 and R2 cannot both be -H.
[0026] Preferably, based on the total mass of the electrolyte as 100%, the mass percentage of the first additive is 0.1% to 3%, for example, it can be 0.1%, 0.5%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8% or 3%, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0027] This invention significantly improves the cycle performance, charging performance, and safety performance of batteries by adjusting the mass ratio of the first additive.
[0028] More preferably, the first additive is selected from at least one of the following compounds: .
[0029] Preferably, the non-aqueous solvent includes a primary solvent and a secondary solvent.
[0030] Preferably, the main solvent comprises a carboxylic acid ester compound.
[0031] As an example, the carboxylic acid ester compounds include, but are not limited to, at least one of methyl formate, ethyl formate, propyl formate, butyl formate, methyl acetate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl acetate, or propyl propionate.
[0032] Preferably, the secondary solvent comprises carbonate compounds.
[0033] As an example, the carbonate solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, or methyl ethyl carbonate.
[0034] In this invention, the above-mentioned carboxylic acid ester compounds and the first additive have a synergistic effect, which further improves the cycle performance, charging performance and safety performance of the battery.
[0035] Preferably, based on the total mass of the non-aqueous solvent as 100%, the mass percentage of the carboxylic acid ester compound is 35% to 80%, for example, it can be 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or 80%, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable. If the mass percentage of the carboxylic acid ester compound is low, the ion transport performance cannot be effectively improved; if the mass percentage of the carboxylic acid ester compound is high, it is easy to lead to the aggravation of high-voltage oxidation side reactions and low concentration of film-forming additives, thereby deteriorating the long-cycle performance and rate performance of the battery.
[0036] Preferably, the electrolyte further includes a second additive.
[0037] Preferably, the second additive comprises a nitrile compound.
[0038] As an example, the nitrile compounds include, but are not limited to, at least one of malononitrile, succinic anionyl nitrile, glutaronitrile, isoprene, ethyl succinic anionyl nitrile, 1,3,6-hexanetrionitrile, ethylene glycol bis(propionitrile) ether, 2-propylmalononitrile, or adiponitrile.
[0039] Preferably, based on the total mass of the electrolyte as 100%, the mass percentage of the second additive is 1% to 5%, for example, it can be 1%, 2%, 3%, 4% or 5%, etc., not limited to the listed values, and other unlisted values within this range are also applicable.
[0040] Preferably, the electrolyte further includes a third additive.
[0041] Preferably, the third additive includes cyclic film-forming ester additives.
[0042] As an example, the cyclic film-forming ester additives include, but are not limited to, at least one of fluoroethylene carbonate, ethylene sulfate, vinylene carbonate, or propanesulfonate lactone.
[0043] Preferably, based on the total mass of the electrolyte as 100%, the mass percentage of the third additive is 13% to 17%, for example, it can be 13%, 14%, 15%, 16% or 17%, etc., not limited to the listed values, and other unlisted values within this range are also applicable.
[0044] The present invention further introduces nitrile compound additives and cyclic film-forming ester additives, which can synergistically work with the first additive to improve the cycle and storage stability of the battery at high temperatures.
[0045] Preferably, the electrolyte salt includes a lithium salt, and the lithium salt includes a first lithium salt and a second lithium salt.
[0046] Preferably, the first lithium salt comprises lithium hexafluorophosphate (LiPF6).
[0047] Preferably, based on the total mass of the electrolyte as 100%, the mass percentage of the first lithium salt is 12.5% to 16%, for example, it can be 12.5%, 13%, 14%, 15% or 16%, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0048] Preferably, the second lithium salt comprises at least one of lithium difluorophosphate (LiDFP), lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiODFB), lithium difluorooxalate phosphate (LiODFP), lithium tetrafluorooxalate phosphate (LiOTFP), lithium bis(trifluoromethyl)sulfonylimide (LiFSI), lithium bis(trifluoromethyl)sulfonylimide (LiTFSI), or lithium 4,5-dicyano-2-trifluoromethyl-imidazolium (LiTDI).
[0049] Preferably, based on the total mass of the electrolyte as 100%, the mass percentage of the second lithium salt is 0.1% to 5%, for example, it can be 0.1%, 0.5%, 1%, 2%, 3%, 4% or 5%, etc., and is not limited to the listed values. Other unlisted values within this range are also applicable.
[0050] This invention improves the ion conductivity and interfacial properties of the electrolyte by adjusting the specific composition of the lithium salt.
[0051] In a second aspect, the present invention provides a method for preparing a battery according to the first aspect, the method comprising the following steps: The positive electrode active material, positive electrode conductive agent, and positive electrode binder are mixed for the first time to obtain a positive electrode slurry; the positive electrode slurry is then used to prepare a positive electrode sheet. The negative electrode active material, negative electrode conductive agent, and negative electrode binder are mixed for the second time to obtain a negative electrode slurry; the negative electrode slurry is then used to prepare a negative electrode sheet; wherein, based on the total mass of the negative electrode active material as 100%, the negative electrode active material includes: graphite material with a mass ratio of 50% to 70%, bulk silicon-based material with a mass ratio of 20% to 30%, and spherical silicon-based material with a mass ratio of 10% to 20%; The electrolyte salt, non-aqueous solvent, and additives are mixed for the third time to obtain the electrolyte, wherein the additives include the first additive. The positive electrode, negative electrode, separator, and electrolyte are assembled to obtain the battery.
[0052] Thirdly, the present invention provides an electronic device comprising the battery according to the first aspect.
[0053] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0054] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a battery that, through the synergistic effect of a negative electrode active material with a specific composition and electrolyte additives, can significantly improve the battery's high-temperature cycle performance, high-temperature storage performance, and safety, as specifically demonstrated below: (1) By introducing a first additive with a specific structure into the electrolyte, a dense and uniform solid electrolyte film can be formed on the positive and negative electrode surfaces, reducing interfacial side reactions and improving the cycle performance of the battery. In addition, the first additive has different effects on different types of negative electrode active materials. For example, for graphite materials, since the reduction potential of the first additive on the graphite surface is higher than that of the electrolyte solvent, it can preferentially undergo reduction decomposition on the graphite negative electrode surface to form a thin and dense SEI film. This SEI film can passivate the active sites on the graphite surface and improve the gas generation phenomenon caused by the catalytic effect of the graphite layer. At the same time, the SEI film can also inhibit the co-intercalation of solvent molecules, prevent the graphite layer from peeling off, and effectively reduce the interfacial impedance and improve the transport path of metal ions at the graphite interface. For example, for silicon-based materials, due to the severe volume expansion (up to 300% or more) of silicon-based materials during charging and discharging, conventional SEI films repeatedly break and regenerate, continuously consuming metal ions and electrolyte, resulting in rapid capacity decay of the battery. The introduction of this first additive allows for the reduction and formation of a SEI film with improved elasticity and flexibility on the silicon-based surface, enabling it to withstand repeated volume expansion and contraction of the silicon-based material without cracking. Furthermore, the reduction potential of this first additive is lower than that of the main solvent in the electrolyte, allowing it to preferentially form a protective layer on the silicon-based surface. This prevents direct contact between the electrolyte and the silicon active material, thereby suppressing interfacial side reactions and significantly improving the battery's cycle performance, charge-discharge performance, high-temperature performance, and safety performance.
[0055] (2) The negative electrode active material provided by the present invention adopts a combination of graphite material + bulk silicon-based material + spherical silicon-based material in a specific mass ratio, with differentiated but complementary effects: a rigid, low-resistance SEI film is formed on the graphite surface to ensure rapid lithium insertion and extraction, and a flexible, high-toughness SEI film is formed on the silicon-based surface to adapt to volume changes. This differentiated film formation behavior effectively improves the interfacial stability of different negative electrode active materials, and comprehensively optimizes the interfacial impedance, ion transport kinetics and structural integrity of the negative electrode hybrid system, thereby maximizing the performance advantages of each component material and achieving the best overall performance of the battery. Detailed Implementation
[0056] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0057] Example 1 This embodiment provides a lithium-ion battery and its preparation method, the preparation method including the following steps: (1) Preparation of positive electrode sheet The positive electrode sheet comprises an aluminum foil and a positive electrode active material layer disposed on one side of the aluminum foil. The specific preparation method includes uniformly mixing lithium cobalt oxide (LiCoO2) positive electrode active material, conductive agent Super P, and binder polyvinylidene fluoride (PVDF) in a mass ratio of LiCoO2:Super P:PVDF = 97.5%:1%:1.5%, then adding them to N-methylpyrrolidone (NMP) solvent and mixing uniformly to obtain a positive electrode slurry. The positive electrode slurry is coated onto the current collector side of the aluminum foil, dried at 85°C, cold-pressed, then trimmed, cut, and slit, and finally dried under vacuum at 85°C for 4 hours. Aluminum tabs are then welded to obtain the positive electrode sheet.
[0058] (2) Preparation of negative electrode The negative electrode sheet includes a copper foil and a negative electrode active material layer disposed on one side of the copper foil. Specifically, it is prepared by mixing graphite material, bulk silicon-carbon material, and spherical silicon-carbon material in a mass ratio of 6.5:2:1.5 to obtain the negative electrode active material. Among them, the D of the graphite material... v 50 bulk silicon-carbon materials with a particle size of 15.5 μm. v 50 particles with a diameter of 8 μm, and D of spherical silicon-carbon materials v 50 particles have a diameter of 8 μm.
[0059] The aforementioned negative electrode active material, conductive agent carbon nanotubes (CNTs), thickener sodium carboxymethyl cellulose (CMC), and binder polyacrylic acid (PAA) were added to deionized water in a mass ratio of 97.6%:0.5%:0.7%:1.2% to obtain a negative electrode slurry. The negative electrode slurry was coated onto one side of a copper foil current collector, dried at 85°C, and then cold-pressed. After edge trimming, cutting, and slitting, it was dried again under vacuum at 85°C for 12 hours. Copper-plated nickel tabs were then welded on to obtain the negative electrode sheet.
[0060] (3) Preparation of electrolyte In an argon-filled glove box, ethylene carbonate (EC), propylene carbonate (PC), ethyl propionate (EP), and propyl propionate (PP) were mixed in a mass ratio of EC:PC:EP:PP = 10%:10%:15%:65%, with the total non-aqueous solvent mass being 100%. Lithium hexafluorophosphate (LiPF6) and lithium difluorooxalate borate (LiODFB) were then slowly added to the mixture. Finally, the first additive, succinate, and fluoroethylene carbonate were added, and the mixture was stirred until homogeneous to obtain the electrolyte. With the total electrolyte mass being 100%, LiPF6 accounted for 14% of the mass, LiODFB accounted for 0.5% of the mass, and the first additive was the compound shown in T02 (…). The corresponding mass percentages are 2%, succinic anionyl ester 5%, and fluoroethylene carbonate 15%.
[0061] (4) Preparation of lithium-ion batteries The prepared positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes, and wound to obtain a bare battery. The bare battery is placed in an aluminum-plastic film outer packaging, and the electrolyte prepared above is injected into the dried battery. After encapsulation, settling, formation, shaping, and capacity testing, a lithium-ion battery is obtained.
[0062] Example 2 The difference between this embodiment and Embodiment 1 is that: Preparation of negative electrode The negative electrode sheet includes a copper foil and a negative electrode active material layer disposed on one side of the copper foil. Specifically, it is prepared by mixing graphite material, bulk silicon-carbon material, and spherical silicon-carbon material in a mass ratio of 5:3:2 to obtain the negative electrode active material. Among these, the D... v 50 bulk silicon-carbon materials with a particle size of 15μm v 50 particles with a diameter of 7 μm, and D of spherical silicon-carbon materials v The particle size of 50 is 7μm.
[0063] The aforementioned negative electrode active material, conductive agent carbon nanotubes (CNTs), thickener sodium carboxymethyl cellulose (CMC), and binder polyacrylic acid (PAA) were added to deionized water in a mass ratio of 97.6%:0.5%:0.7%:1.2% to obtain a negative electrode slurry. The negative electrode slurry was coated onto one side of a copper foil current collector, dried at 85°C, and then cold-pressed. After edge trimming, cutting, and slitting, it was dried again under vacuum at 85°C for 12 hours. Copper-plated nickel tabs were then welded on to obtain the negative electrode sheet.
[0064] Preparation of electrolyte In an argon-filled glove box, ethylene carbonate (EC), propylene carbonate (PC), ethyl propionate (EP), and propyl propionate (PP) were mixed in a mass ratio of EC:PC:EP:PP = 10%:10%:35%:45%, with the total non-aqueous solvent mass being 100%. Lithium hexafluorophosphate (LiPF6) and lithium difluorooxalate borate (LiODFB) were then slowly added to the mixture. Finally, the first additive, succinate, and fluoroethylene carbonate were added, and the mixture was stirred until homogeneous to obtain the electrolyte. With the total electrolyte mass being 100%, LiPF6 accounted for 12.5% of the mass, LiODFB accounted for 0.1% of the mass, and the first additive was the compound shown in T02 (…). The corresponding mass percentages are 3%, succinic anionyl ester 5%, and fluoroethylene carbonate 17%.
[0065] Example 3 The difference between this embodiment and Embodiment 1 is that: Preparation of negative electrode The negative electrode sheet includes a copper foil and a negative electrode active material layer disposed on one side of the copper foil. The negative electrode active material is obtained by mixing graphite material, bulk silicon-carbon material, and spherical silicon-carbon material in a mass ratio of 7:2:1. Among them, the D of the graphite material... v 50 bulk silicon-carbon materials with a particle size of 16μm v 50 particles with a diameter of 9 μm, and D of spherical silicon-carbon materials v 50 particles have a diameter of 9 μm.
[0066] The aforementioned negative electrode active material, conductive agent carbon nanotubes (CNTs), thickener sodium carboxymethyl cellulose (CMC), and binder polyacrylic acid (PAA) were added to deionized water in a mass ratio of 97.6%:0.5%:0.7%:1.2% to obtain a negative electrode slurry. The negative electrode slurry was coated onto one side of a copper foil current collector, dried at 85°C, and then cold-pressed. After edge trimming, cutting, and slitting, it was dried again under vacuum at 85°C for 12 hours. Copper-plated nickel tabs were then welded on to obtain the negative electrode sheet.
[0067] Preparation of electrolyte In an argon-filled glove box, ethylene carbonate (EC), propylene carbonate (PC), ethyl propionate (EP), and propyl propionate (PP) were mixed in a mass ratio of EC:PC:EP:PP = 15%:10%:15%:60%, with the total mass of non-aqueous solvents being 100%. Lithium hexafluorophosphate (LiPF6) and lithium difluorooxalate borate (LiODFB) were then slowly added to the mixture. Finally, the first additive, succinate, and fluoroethylene carbonate were added, and the mixture was stirred until homogeneous to obtain the electrolyte. With the total mass of the electrolyte being 100%, LiPF6 accounted for 16% of the mass, LiODFB accounted for 5% of the mass, and the first additive was the compound shown in T02. The corresponding mass percentages are 0.1% for succinic acid, 1% for succinic acid, and 13% for fluoroethylene carbonate.
[0068] Example 4 The difference between this embodiment and Embodiment 1 is that, in the preparation process of the electrolyte, the first additive is replaced with an equal mass proportion of T04, while everything else is the same as in Embodiment 1.
[0069] Example 5 The difference between this embodiment and Embodiment 1 is that, in the preparation process of the electrolyte, the first additive is replaced with T05 in an equal mass ratio, while all other aspects are the same as in Embodiment 1.
[0070] Example 6 The difference between this embodiment and Example 1 is that, in the preparation process of the electrolyte, the first additive is replaced with an equal mass proportion of the compound shown in T01 ( Everything else is the same as in Example 1.
[0071] Example 7 The difference between this embodiment and Example 1 is that, in the preparation process of the electrolyte, the first additive is replaced with an equal mass proportion of the compound shown in T03 ( Everything else is the same as in Example 1.
[0072] Example 8 The difference between this embodiment and Embodiment 1 is that, taking the total mass of the negative electrode active material as 100%, the mass ratio of graphite material is 40%, the mass ratio of bulk silicon carbide material is 40%, and the mass ratio of spherical silicon carbide material is 20%, while all other aspects are the same as in Embodiment 1.
[0073] Example 9 The difference between this embodiment and Embodiment 1 is that, taking the total mass of the negative electrode active material as 100%, the mass ratio of graphite material is 80%, the mass ratio of bulk silicon carbide material is 10%, and the mass ratio of spherical silicon carbide material is 10%, while all other aspects are the same as in Embodiment 1.
[0074] Example 10 The difference between this embodiment and Example 1 is that ethyl propionate and propyl propionate are replaced with an equal amount of diethyl carbonate solvent. Specifically, in the preparation of the electrolyte, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) are mixed in a mass ratio of EC:PC:DEC = 10%:10%:80%, while all other aspects are the same as in Example 1.
[0075] Comparative Example 1 The difference between this comparative example and Example 1 is that the first additive (T01) is replaced with an equal mass proportion of 1,3-propanesulfonic acid lactone; otherwise, they are the same as in Example 1.
[0076] Comparative Example 2 The difference between this comparative example and Example 1 is that the blocky silicon-carbon material is replaced with spherical silicon-carbon material of equal mass proportion; otherwise, they are the same as in Example 1.
[0077] Comparative Example 3 The difference between this comparative example and Example 1 is that the spherical silicon-carbon material is replaced with blocky silicon-carbon material of equal mass proportion; otherwise, they are the same as in Example 1.
[0078] Test conditions The lithium-ion batteries provided in the above embodiments and comparative examples were subjected to performance tests, as detailed below: (1) Capacity The lithium-ion batteries provided in the above embodiments and comparative examples were charged to 4.55V with a constant current of 2C and a cutoff rate of 0.02C; then discharged to the set lower limit voltage with a constant current of 1C. This step was repeated 3 times, and the average value was taken. This discharge capacity was recorded as the average capacity.
[0079] (2) Cyclic performance test at room temperature (25℃) At 25°C, the lithium-ion batteries provided in the above embodiments and comparative examples were charged to 4.55V at a 2C stage with a cutoff rate of 0.09C; then discharged at a constant current of 1C to the set lower limit voltage. This cycle was repeated 500 times, and the discharge capacity of the first week and the discharge capacity of the 500th week were recorded. The capacity retention rate was calculated using the following formula: Capacity retention rate = (Discharge capacity at week 500 / Discharge capacity at week 1) × 100%; Thickness expansion rate = (full charge thickness in week 500 - full charge thickness in week 1) / full charge thickness in week 1 × 100%.
[0080] (3) High temperature (45℃) cycle performance test At 45°C, the lithium-ion batteries provided in the above embodiments and comparative examples were charged to 4.55V at a 2C stage with a cutoff rate of 0.09C; then discharged at a constant current of 1C to the set lower limit voltage. This cycle was repeated 500 times, and the discharge capacity in the first week and the discharge capacity in the 500th week were recorded. The capacity retention rate was calculated using the following formula: Capacity retention rate = (Discharge capacity at week 500 / Discharge capacity at week 1) × 100%; Thickness expansion rate = (full charge thickness in week 500 - full charge thickness in week 1) / full charge thickness in week 1 × 100%.
[0081] (4) High temperature (60℃) storage performance test The lithium-ion batteries provided in the above embodiments and comparative examples were charged to 4.55V at 2C level and stored at 60°C for 21 days to observe whether the batteries swelled.
[0082] The test results are shown in Table 1.
[0083] Table 1 As can be seen from Table 1, comparing the test results of Examples 1 to 10 and Comparative Examples 1 to 3, it can be seen that under the electrolyte formulation with specific additives, the lithium-ion battery assembled with the specific ratio of composite silicon-based materials provided in this application has better overall performance than a single silicon-based material system. It has excellent high-temperature cycle performance, room-temperature cycle performance and long-term high-temperature storage performance, while the battery does not swell.
[0084] Furthermore, comparing Examples 1 and 4 to 7, it can be seen that by comparing the effects of different additives, the additive with the TO2 structure has a better effect on improving the long-term cycle performance of the battery. This is mainly due to its special structural characteristics, which can achieve rapid interface repair when the SEI film is damaged, preventing more side reactions from causing rapid capacity decay. At the same time, because it contains two sulfate ester groups, the impedance increase brought by the additive is controlled overall. Therefore, the battery exhibits excellent long-term cycle stability during long-term cycling.
[0085] Comparing Examples 1 and 8-9, it can be seen that by adjusting the mass ratio of graphite material, bulk silicon-based material and spherical silicon-based material to a reasonable range, the three work together to achieve a balance between energy density and cycle life, thereby significantly improving the cycle performance, charging performance and safety performance of the battery.
[0086] Comparing Examples 1 and 10, it is evident that the choice of main solvent and the combination with the negative electrode active material in the electrolyte formulation are of paramount importance. The use of carboxylic acid esters as the main solvent, compared to using carbonates, significantly highlights the importance of carboxylic acid esters, while DEC exhibits noticeable gas expansion during long-term storage. Furthermore, using non-aqueous solvents mixed with different solvent ratios can balance the kinetic differences between bulk and spherical silicon-based materials. Simultaneously, using a higher content of carboxylic acid esters as the main solvent results in lower polarization and higher melting and boiling points, thus making the prepared electrolyte more stable at high temperatures. This reduces the risk of gas generation during long-term high-temperature cycling and the risk of introducing additional side reactions that could damage the interfacial film during long-term battery performance testing. Therefore, the combination of a higher content of carboxylic acid esters with the composite silicon-carbon negative electrode demonstrates superior performance.
[0087] Therefore, this application significantly improves the cycle performance, charging performance and high-temperature performance of the battery by regulating the composition of the negative electrode active material and the electrolyte composition. In particular, the preferred electrolyte with carboxylic acid ester compounds as the main solvent, combined with additives with specific structures, has a good compatibility with composite silicon-based systems.
[0088] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A battery, said battery comprising a negative electrode and an electrolyte, characterized in that, The negative electrode sheet includes a negative electrode active material. Based on the total mass of the negative electrode active material as 100%, the negative electrode active material includes: graphite material with a mass ratio of 50% to 70%, bulk silicon-based material with a mass ratio of 20% to 30%, and spherical silicon-based material with a mass ratio of 10% to 20%. The electrolyte comprises an electrolyte salt, a non-aqueous solvent, and an additive, wherein the additive comprises a first additive, which comprises a compound with the structure shown in Formula 1: Formula 1; R1 and R2 are each independently selected from -H, C2~C10 hydrocarbon group, C2~C10 carbonate group, sulfate group, phosphate group, silicate group or borate group, and R1 and R2 cannot be -H at the same time.
2. The battery according to claim 1, characterized in that, Based on the total mass of the negative electrode active material being 100%, the mass percentage of the graphite material is 62% to 65%. And / or, based on the total mass of the negative electrode active material being 100%, the mass percentage of the bulk silicon-based material is 20% to 23%; And / or, based on the total mass of the negative electrode active material being 100%, the mass percentage of the spherical silicon-based material is 12% to 18%.
3. The battery according to claim 1 or 2, characterized in that, The graphite material D v 50 particles have a diameter of 15μm~16μm; And / or, the D of the bulk silicon-based material v 50 particles have a diameter of 7μm~9μm; And / or, the D of the spherical silicon-based material v The particle size of 50 particles is 7μm~9μm.
4. The battery according to claim 1, characterized in that, R1 and R2 are each independently selected from C3 to C8 carbonate, sulfate, phosphate, silicate, or borate groups, and R1 and R2 cannot both be -H. And / or, based on the total mass of the electrolyte being 100%, the mass percentage of the first additive is 0.1% to 3%.
5. The battery according to claim 4, characterized in that, The first additive is selected from at least one of the following compounds: 。 6. The battery according to claim 1, characterized in that, The non-aqueous solvent includes a primary solvent and a secondary solvent; The main solvent includes carboxylic acid ester compounds; The secondary solvent includes carbonate compounds; Based on the total mass of the non-aqueous solvent being 100%, the mass percentage of the carboxylic acid ester compound is 35% to 80%.
7. The battery according to claim 1, characterized in that, The electrolyte also includes a second additive; The second additive includes nitrile compounds; Based on the total mass of the electrolyte being 100%, the mass percentage of the second additive is 1% to 5%.
8. The battery according to claim 1, characterized in that, The electrolyte also includes a third additive; The third additive includes cyclic film-forming ester additives; Based on the total mass of the electrolyte being 100%, the mass percentage of the third additive is 13% to 17%.
9. The battery according to claim 1, characterized in that, The electrolyte salt includes a lithium salt, and the lithium salt includes a first lithium salt and a second lithium salt; And / or, the first lithium salt comprises lithium hexafluorophosphate; And / or, based on the total mass of the electrolyte being 100%, the mass percentage of the first lithium salt is 12.5% to 16%; And / or, the second lithium salt comprises at least one of lithium difluorophosphate, lithium tetrafluoroborate, lithium difluorooxalate borate, lithium difluorooxalate phosphate, lithium tetrafluorooxalate phosphate, lithium bis(trifluoromethyl)sulfonylimide, lithium bis(trifluoromethyl)sulfonylimide, or lithium 4,5-dicyano-2-trifluoromethyl-imidazolium. And / or, based on the total mass of the electrolyte being 100%, the mass percentage of the second lithium salt is 0.1% to 5%.