A weakly solvated electrolyte, its preparation method and application

By using branched or cyclic sterically hindered ether solvents and weakly solvated electrolytes containing lithium salts, the kinetic and structural stability issues of lithium-ion batteries under ultra-fast charging and low-temperature environments were solved, achieving high-efficiency battery performance.

CN123073169APending Publication Date: 2026-11-10FUDAN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611362154.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing lithium-ion battery electrolytes exhibit insufficient kinetic performance under ultra-fast charging conditions, reduced ion conductivity at low temperatures, and traditional ether solvents are prone to co-intercalation with lithium ions into the graphite interlayer, leading to structural damage. Existing high-concentration strategies are costly and have insufficient performance.

Method used

An ether solvent with a branched or cyclic steric structure is used, combined with an appropriate amount of lithium salt and film-forming additives, to form a weakly solvated electrolyte. The solvent is blocked from entering the graphite interlayer by the steric hindrance effect, thus constructing a low-impedance SEI film.

Benefits of technology

It achieves efficient operation of lithium-ion batteries in ultra-fast charging and low-temperature environments, suppresses solvent co-intercalation, improves initial coulombic efficiency and cycle stability, and ensures high rate and long cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073169A_ABST
    Figure CN123073169A_ABST
Patent Text Reader

Abstract

This invention provides a weakly solvated electrolyte, its preparation method, and its application, belonging to the field of electrolyte technology. The weakly solvated electrolyte provided by this invention includes a lithium salt and a weakly solvated solvent; the weakly solvated solvent is an ether solvent with a branched or cyclic steric hindrance structure and 3-12 carbon atoms. The weakly solvated electrolyte provided by this invention uses an ether solvent with significant steric hindrance effect as the main solvent. Due to its special steric hindrance effect, when interacting with lithium ions, this ether solvent exhibits significant weak solvation energy, which can significantly increase the physical resistance of solvent molecules entering the graphite interlayer, completely suppressing solvent co-intercalation at the physical spatial level, thereby improving the cycle stability of commercial graphite anode systems in lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrolyte technology, specifically relating to a weakly solvated electrolyte, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries (LIBs), as the most successful rechargeable battery technology to date, have been widely used in portable electronic devices, electric vehicles, and large-scale energy storage systems. Currently, commercially available lithium-ion batteries generally use carbonate-based electrolytes (such as systems composed of EC, DMC, EMC, etc.). However, as the industry's requirements for fast-charging performance and wide-temperature adaptability become increasingly stringent, the limitations of traditional carbonate systems are becoming more and more prominent: on the one hand, carbonate molecules (especially EC) have extremely high binding energies with lithium ions, resulting in a huge desolvation energy barrier at the interface, which greatly limits the kinetic performance of the battery under ultra-fast charging conditions; on the other hand, the high melting point and high viscosity-temperature coefficient of carbonate solvents cause their ion conductivity to drop sharply at low temperatures, seriously affecting the battery's all-weather operation capability.

[0003] In contrast, ether solvents, with their extremely low viscosity, excellent ionic conductivity, and superior interfacial wettability, are considered ideal for constructing high-power, fast-charging lithium-ion batteries. However, the application of ether solvents in commercial graphite anode systems has long faced severe technical challenges. Traditional linear ether molecules (such as DME and DEM) have compact structures and high oxygen atom exposure, leading to difficulties in their interaction with lithium ions (Li). + There is a strong chelating coordination ability between these linear molecules and lithium ions. During charging, these linear molecules tend to combine with lithium ions to form stable "solvated lithium ion" complexes. Due to the layered structure of the graphite anode, its interlayer spacing (d002≈0.335 nm) allows small solvated ions to enter. Traditional linear ether-based solvated ions, lacking sufficient steric hindrance, are easily co-intercalated with lithium ions into the graphite interlayer. This co-intercalation behavior causes a dramatic expansion of the graphite lattice structure, leading to graphite layer peeling and pulverization, accompanied by continuous damage and repeated growth of the SEI film, ultimately resulting in a sharp increase in battery internal resistance and a rapid drop in cycle capacity.

[0004] To suppress solvent co-intercalation, existing technologies primarily rely on high-concentration electrolyte (HCE) or locally high-concentration electrolyte (LHCE) strategies. The HCE strategy significantly increases the amount of lithium salt, utilizing salt anions to occupy the lithium-ion solvation shell, thereby reducing the presence of free solvent molecules. However, the HCE strategy not only faces the problem of extremely high lithium salt costs but also suffers from drawbacks such as excessive viscosity, poor wettability, and a significant decrease in ionic conductivity. While the locally high-concentration strategy introduces fluorinated diluents to improve physical properties, these diluents are often complex to synthesize, expensive, and their high density and low chemical compatibility introduce additional difficulties to actual battery production.

[0005] In summary, how to block the pathway of solvent molecules into the graphite interlayer while maintaining a low salt concentration is a key scientific problem that urgently needs to be solved in the field of lithium-ion battery electrolytes. Summary of the Invention

[0006] In view of this, the present invention provides a weakly solvated electrolyte, its preparation method, and its application. The weakly solvated electrolyte provided by the present invention introduces ether solvents with branched or cyclic steric structures exhibiting significant steric hindrance effects. Utilizing the geometrical repulsion effect of these solvents' molecular structures, the pathways for solvent molecules to enter the graphite interlayer are completely blocked without relying on expensive additives or extremely high salt concentrations, thereby achieving long-term stable operation of the graphite anode system in the ether-based electrolyte.

[0007] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a weakly solvated electrolyte, comprising the following components: Lithium salts and weakly solvating solvents; The weak solvating solvent is an ether solvent with a branched structure or a cyclic sterically hindered structure and a carbon number of 3 to 12.

[0008] Preferably, the weak solvating solvent includes one or more of the following: triethyl orthoformate, trimethyl orthoformate, triisopropyl orthoformate, triethyl orthoacetate, trimethyl orthoacetate, tripropyl orthoacetate, triethyl orthopropionate, isopropyl ether, diisopentyl ether, methyl tert-butyl ether, ethyl tert-butyl ether, 1,3-dioxopentane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, and their heteroatom-substituted derivatives.

[0009] Preferably, the lithium salt comprises one or more of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, and lithium difluorooxalate borate.

[0010] Preferably, the molar concentration of the lithium salt in the weakly solvated electrolyte is 0.5~3.0 mol / L.

[0011] Preferably, the weakly solvated electrolyte further includes a co-solvent; The cosolvent includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl acetate, ethyl acetate, ethyl propionate, methyl propionate, propyl propionate, fluoroethylene carbonate, and fluorocarboxylic acid esters.

[0012] Preferably, the volume ratio of the weakly solvating solvent to the co-solvent is 10:90~100:0.

[0013] Preferably, the weakly solvated electrolyte further includes film-forming additives; The film-forming additives include one or more of the following: vinylene carbonate, ethylene vinylene carbonate, vinyl sulfate, 1,3,6-hexanetrionitrile, phenyltrivinylsilane, lithium bis(oxalato)borate, lithium difluorophosphate, 1,3-propanesulfonyl lactone, lithium nitrate, lithium difluorobis(oxalato)phosphate, lithium tetrafluorooxalato)phosphate, triallyl phosphite, methylene disulfonate, pyridine, difluorodiphenylsilane, and tri(trimethylsilyl) phosphite.

[0014] Preferably, the mass of the film-forming additive is 0 to 5% of the total mass of the weakly solvated electrolyte.

[0015] This invention also provides a method for preparing the weakly solvated electrolyte described in the above technical solution, comprising the following steps: The lithium salt is mixed with the weak solvating solvent under anhydrous and oxygen-free conditions to obtain the weak solvating electrolyte.

[0016] The present invention also provides the application of the weakly solvated electrolyte described in the above technical solution or the weakly solvated electrolyte prepared by the preparation method described in the above technical solution in a lithium-ion battery, wherein the lithium-ion battery comprises: a positive electrode, a graphite-based negative electrode, a separator and the weakly solvated electrolyte.

[0017] This invention provides a weakly solvated electrolyte, comprising a lithium salt and a weakly solvated solvent; the weakly solvated solvent is an ether solvent with a branched or cyclic sterically hindered structure and 3-12 carbon atoms. The weakly solvated electrolyte provided by this invention uses an ether solvent with a significant steric hindrance effect as the main solvent. Due to its special steric hindrance effect, this ether solvent exhibits a significant weak solvation energy when interacting with lithium ions. This can significantly increase the physical resistance of solvent molecules entering the graphite interlayer, completely suppressing solvent co-intercalation at the physical steric level. Therefore, when the weakly solvated electrolyte of this invention is applied to a graphite anode lithium-ion battery, it exhibits excellent initial coulombic efficiency and cycle stability.

[0018] Furthermore, the weakly solvated electrolyte provided by this invention not only features low desolvation energy but also induces the formation of a highly stable SEI film with low impedance. When applied to lithium-ion battery systems using graphite-based materials as the negative electrode, lithium ions can be rapidly desolvated and embedded into the negative electrode, exhibiting excellent fast-charging characteristics. Simultaneously, the weakly solvated branched solvent promotes the participation of more anions in the solvation shell, thereby generating a high-strength SEI film rich in inorganic components such as LiF. The weakly solvated electrolyte of this invention effectively ensures that lithium-ion batteries exhibit high rate capability, long cycle life, and large capacity. Attached Figure Description

[0019] Figure 1 The graphite-lithium half-cells assembled using the electrolytes obtained in Examples 1 and 4 and Comparative Examples 1 and 2 are shown as the first charge-discharge curves at a rate of 0.1 C (1 C = 372 mA / g). Figure 2 The graph shows the relationship between the reversible specific capacity, coulombic efficiency and cycle number of graphite||lithium half-cells assembled using the electrolytes obtained in Example 1 and Comparative Examples 1 and 2, respectively, at 0.5C (1 C = 372 mA / g). Figure 3 The graph shows the relationship between reversible specific capacity, coulombic efficiency and cycle number of graphite||NCM811 full cells assembled using the electrolytes obtained in Example 1 and Comparative Example 3 at room temperature under charge and discharge at a rate of 0.5 C (1 C = 200 mA / g). Figure 4 The graph shows the relationship between reversible specific capacity, coulombic efficiency and cycle number of graphite||NCM811 full cells assembled using the electrolytes obtained in Example 1 and Comparative Example 3, when charged and discharged at a rate of 0.1 C at a low temperature of -20°C. Detailed Implementation

[0020] This invention provides a weakly solvated electrolyte, comprising the following components: Lithium salts and weakly solvating solvents; The weak solvating solvent is an ether solvent with a branched structure or a cyclic sterically hindered structure and a carbon number of 3 to 12.

[0021] Unless otherwise specified, all raw materials used in this invention are commercially available products in the art.

[0022] In this invention, the weak solvating solvent is an ether solvent with a branched structure or a cyclic steric structure and a carbon number of 3 to 12. In this invention, the number of carbon atoms is preferably 3-7; the weak solvating solvent preferably includes one or more of the following: triethyl orthoformate, trimethyl orthoformate, triisopropyl orthoformate, triethyl orthoacetate, trimethyl orthoacetate, tripropyl orthoacetate, triethyl orthopropionate, isopropyl ether, diisopentyl ether, methyl tert-butyl ether, ethyl tert-butyl ether, 1,3-dioxopentane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, and their heteroatom-substituted derivatives. The structural formulas of triethyl orthoformate, trimethyl orthoformate, triisopropyl orthoformate, triethyl orthoacetate, trimethyl orthoacetate, tripropyl orthoacetate, triethyl orthopropionate, isopropyl ether, diisopentyl ether, methyl tert-butyl ether, ethyl tert-butyl ether, 1,3-dioxopentane, 2-methyltetrahydrofuran, and 2,5-dimethyltetrahydrofuran are preferably as shown in formulas (1) to (14):

[0023] The weak solvation solvent used in this invention has the characteristics of low viscosity and good interfacial wettability. Through the steric hindrance effect, the solvation sheath structure can be controlled and the solvent coordination strength can be reduced. This can promote the derivatization of anion-low impedance SEI film and accelerate the desolvation of lithium ions, thereby achieving excellent rate performance, fast charging characteristics and high cycle stability of the battery under different negative electrode interfaces.

[0024] In this invention, the lithium salt preferably includes one or more of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium hexafluorophosphate (LiPF6), and lithium difluorooxalate borate (LiDFOB), more preferably lithium bis(fluorosulfonyl)imide or lithium bis(trifluoromethanesulfonyl)imide. In this invention, the molar concentration of the lithium salt in the weakly solvated electrolyte is preferably 0.5~3.0 mol / L, more preferably 1.0 mol / L or 2.0 mol / L.

[0025] In this invention, the weakly solvated electrolyte preferably further includes a co-solvent; the co-solvent preferably includes one or more of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl acetate (MA), ethyl acetate (EA), ethyl propionate (EP), methyl propionate (MP), propyl propionate (PP), fluoroethylene carbonate (FEC), and fluorocarboxylic acid esters, more preferably fluoroethylene carbonate. The co-solvent is intended to adjust the viscosity, polarity, and interfacial wettability of the electrolyte to further optimize the ionic conductivity, low-temperature conductivity, or thermal stability of the system.

[0026] In this invention, the volume ratio of the weak solvating solvent to the co-solvent is preferably 10:90 to 100:0, more preferably 90:10 or 100:0.

[0027] In this invention, the weakly solvated electrolyte preferably further includes a film-forming additive; the film-forming additive preferably includes one or more of the following: vinylene carbonate (VC), ethylene vinyl carbonate (VEC), vinyl sulfate (DTD), 1,3,6-hexanetrionitrile (HTN), phenyltrivinylsilane (PTVS), lithium bis(oxalato)borate (LiBOB), lithium difluorophosphate (LiDFP), 1,3-propanesulfonyl lactone (PS), lithium nitrate (LiNO3), lithium difluorobis(oxalato)phosphate (LiDODFP), lithium tetrafluorooxalato)phosphate (LiOTFP), triallyl phosphite, methylene disulfonate (MMDS), pyridine (Py), difluorodiphenylsilane, and tri(trimethylsilyl) phosphite, more preferably lithium nitrate. The film-forming additive preferentially decomposes at the electrode interface, inducing the formation of a stable and low-resistance solid electrolyte interphase (SEI / CEI) film, effectively suppressing the continuous decomposition of solvent molecules and improving the cycle stability of the battery.

[0028] In this invention, the mass of the film-forming additive is preferably 0 to 5% of the total mass of the weakly solvated electrolyte, and more preferably 2%.

[0029] This invention also provides a method for preparing the weakly solvated electrolyte described in the above technical solution, comprising the following steps: The lithium salt is mixed with the weak solvating solvent under anhydrous and oxygen-free conditions to obtain the weak solvating electrolyte.

[0030] In this invention, the mixing method is preferably dissolution. This invention does not impose any particular limitation on the dissolution method; any dissolution method well-known to those skilled in the art can be used.

[0031] The present invention also provides the application of the weakly solvated electrolyte described above in a lithium-ion battery, wherein the lithium-ion battery comprises: a positive electrode, a graphite-based negative electrode, a separator, and the weakly solvated electrolyte.

[0032] In this invention, the active material of the positive electrode preferably includes one or more of layered oxide, spinel oxide and polyanionic compound, more preferably one or more of lithium cobalt oxide, lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA), lithium manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate and lithium-rich manganese-based materials, and most preferably lithium nickel cobalt manganese oxide (NCM).

[0033] In this invention, the graphite-based anode preferably includes one or more of graphite-type anodes and graphite-based composite anodes, more preferably graphite-type anodes; the graphite-type anode preferably includes one or more of natural graphite, artificial graphite, modified graphite, mesophase carbon microspheres (MCMB), expanded graphite, graphene, and carbon nanotubes, more preferably artificial graphite; the graphite-based composite anode preferably includes one or more of silicon / graphite composite anodes, silicon suboxide / graphite composite anodes, tin / graphite composite anodes, hard carbon / graphite composite anodes, and metal / graphite composite anodes. In some preferred embodiments, the graphite-based anode is preferably a graphite-type anode with a layered structure. When the weakly solvated electrolyte is applied to a graphite anode lithium-ion battery, the weakly solvated electrolyte can significantly suppress the co-intercalation of solvent molecules in the layered graphite-type anode.

[0034] In this invention, the diaphragm preferably comprises one or more of polyethylene, polypropylene, porous vinylidene fluoride-hexafluoropropylene, polyimide, aramid fiber and glass fiber, more preferably polypropylene and / or glass fiber.

[0035] The weakly solvated electrolyte of this invention has a low desolvation energy, which can form a highly stable solid electrolyte interface film with low impedance. When applied to a lithium-ion battery system with graphite as the negative electrode, it can effectively suppress the co-intercalation phenomenon of traditional ether solvents in the graphite negative electrode, exhibiting good fast charging characteristics and low-temperature performance. The weakly solvated electrolyte of this invention can effectively ensure that the lithium-ion battery exhibits the characteristics of high power, large capacity, and extreme environment application.

[0036] Furthermore, the weakly solvated electrolyte of this invention not only effectively solves the problem of solvent co-intercalation in graphite anodes, but also has a significant optimization effect on other anode systems. For example, for high-capacity anodes such as silicon-based and tin-based anodes, this type of electrolyte can induce the formation of a stable SEI film rich in inorganic components through the weakly solvated structure, effectively buffering the interface damage caused by volume expansion; while for high-power anodes such as hard carbon and lithium titanate, its low desolvation energy barrier can significantly improve the ion exchange rate at the interface.

[0037] The following detailed description of the weakly solvated electrolyte, its preparation method, and its application, with reference to specific embodiments, should not be construed as limiting the scope of protection of this invention.

[0038] Example 1

[0039] Under anhydrous and oxygen-free conditions, lithium bisfluorosulfonyl imide (LiFSI) was dissolved in triethyl orthoformate (TOF, structural formula 1) at a molar concentration of 1 mol / L to prepare a weakly solvated electrolyte of 1 mol / L LiFSI in TOF.

[0040] Example 2

[0041] Under anhydrous and oxygen-free conditions, a weakly solvated electrolyte of 1 mol / L LiFSI in TOF / FEC (9:1, v / v) was prepared by dissolving lithium bisfluorosulfonylimide (LiFSI) in TOF / FEC at a molar concentration of 1 mol / L using TOF and FEC as solvents, wherein TOF:FEC = 9:1 (volume ratio).

[0042] Example 3

[0043] Under anhydrous and oxygen-free conditions, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was dissolved in 1,3-dioxopentane (DOL, structural formula 2) at a molar concentration of 1 mol / L to prepare a weakly solvated electrolyte of 1 mol / L LiTFSI in DOL.

[0044] Example 4

[0045] Under anhydrous and oxygen-free conditions, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was dissolved in DOL and fluoroethylene carbonate (FEC) as solvents, with DOL:FEC = 9:1 (volume ratio), at a molar concentration of 2 mol / L. 2 wt.% lithium nitrate (LiNO3) was added to prepare a weakly solvated electrolyte of DOL / FEC (9:1, v / v) + 2 wt.% LiNO3 containing 2 mol / L LiTFSI.

[0046] Example 5

[0047] Under anhydrous and oxygen-free conditions, lithium bisfluorosulfonyl imide (LiFSI) was dissolved in isopropyl ether (IPE, structural formula 8) at a molar concentration of 1 mol / L to prepare a weakly solvated electrolyte of 1 mol / L LiFSI in IPE.

[0048] Example 6

[0049] Under anhydrous and oxygen-free conditions, lithium bis(fluorosulfonyl)imide (LiFSI) was dissolved in diisopentyl ether (DIAE, structural formula 9) at a molar concentration of 1 mol / L to prepare a weakly solvated electrolyte of 1 mol / L LiFSI in DIAE.

[0050] Example 7

[0051] Under anhydrous and oxygen-free conditions, lithium bisfluorosulfonyl imide (LiFSI) was dissolved in tripropyl orthoacetate (TPOA, structural formula 6) at a molar concentration of 1 mol / L to prepare a weakly solvated electrolyte of TPOA containing 1 mol / L LiFSI.

[0052] Comparative Example 1

[0053] Under anhydrous and oxygen-free conditions, lithium bisfluorosulfonyl imide (LiFSI) was dissolved in ethylene glycol dimethyl ether (DME) at a molar concentration of 1 mol / L to prepare an electrolyte of 1 mol / L LiFSI in DME.

[0054] Comparative Example 2

[0055] Under anhydrous and oxygen-free conditions, lithium bisfluorosulfonyl imide (LiFSI) was dissolved in diethoxymethane (DEM) at a molar concentration of 1 mol / L to prepare an electrolyte of 1 mol / L LiFSI in DEM.

[0056] Comparative Example 3

[0057] Under anhydrous and oxygen-free conditions, lithium hexafluorophosphate (LiPF6) was dissolved in ethylene carbonate (EC) and dimethyl carbonate (DMC) as solvents, with EC:DMC = 1:1 (volume ratio), to obtain an electrolyte of 1 mol / L LiPF6 in EC / DMC (1:1, v / v).

[0058] Comparative Example 4

[0059] Under anhydrous and oxygen-free conditions, lithium bisfluorosulfonyl imide (LiFSI) was dissolved in triisobutyl orthoacetate (TIBA, carbon 14) at a molar concentration of 1 mol / L to prepare a weakly solvated electrolyte of TIBA with 1 mol / L LiFSI.

[0060] Performance testing

[0061] (1) A coin cell (CR2032) was assembled in an argon atmosphere glove box using a graphite electrode as the working electrode and a lithium metal sheet as the counter and reference electrodes. At room temperature, it was first tested at a 0.1 C rate from 0.005 V to 2 V (vs. Li / Li). + Charge-discharge tests were conducted within the specified voltage range, where 1 C = 372 mA / g. The resulting first-cycle charge-discharge curves are shown below. Figure 1 As shown in the figure. Subsequently, within the same voltage range, cyclic charge-discharge tests were conducted at a rate of 0.5 C, and the relationship between its reversible discharge specific capacity, coulombic efficiency, and number of cycles was recorded. The results are shown in the figure. Figure 2 As shown. Similarly, the graphite-lithium half-cell assembled using this method was charged and discharged sequentially at rates of 0.2 C, 0.5 C, 1 C, 2 C, 3 C, and 5 C, with each rate being repeated 5 times. The rate performance results are summarized in Table 1.

[0062] (2) Using high-nickel ternary material NCM811 as the positive electrode active material and graphite as the negative electrode active material, a full cell was assembled with a positive / negative electrode capacity matching ratio (N / P ratio) of 1.1~1.2. At room temperature, the battery was subjected to charge-discharge cycle tests at a rate of 0.5 C within a voltage range of 2.65 V-4.25 V. The current density was calculated based on the mass of the positive electrode active material, with 1 C = 200 mA / g. The room temperature cycle performance curves of the obtained full cell are shown below. Figure 3 As shown. Subsequently, to investigate the low-temperature performance of the electrolyte, the assembled NCM811||graphite full cell was placed in a -20℃ low-temperature test chamber and kept at a constant temperature for 2 hours. Charge-discharge cycle tests were then conducted at a 0.1 C rate. The obtained low-temperature cycle specific capacity and coulombic efficiency curves are summarized in... Figure 4 .

[0063] Table 1 shows the rate performance of the graphite (Gr) half-cells assembled in Examples 1, 2, 3, 4, 5, 6, 7 and Comparative Examples 3 and 4.

[0064]

[0065] from Figure 1 Comparing Example 1 and Comparative Example 1, it is evident that triethyl orthoformate (TOF), compared to the traditional linear ether solvent dimethoxyethane (DME), exhibits a strong steric hindrance effect due to its unique three-branched spatial configuration. As shown in the attached figures, Comparative Example 1 exhibits a broad and extremely flat voltage plateau near 1.0V during the initial discharge, followed by rapid capacity depletion. This is a typical characteristic of solvent molecules co-intercalating with lithium ions into the graphite interlayer and then decomposing, rendering effective lithium ion intercalation and deintercalation virtually impossible. In contrast, Example 1 demonstrates a clear and stable graphite lithium intercalation plateau (0.01V~0.2V), with no co-intercalation characteristic plateaus appearing. Its initial discharge specific capacity exceeds 350 mAh / g, and its coulombic efficiency is over 85%. This proves that the branched structure of TOF significantly increases the kinetic diameter of solvated ions, making it geometrically difficult for them to enter the graphite interlayer, thereby completely suppressing co-intercalation.

[0066] Comparing Example 1 and Comparative Example 2, it can be seen that although diethoxymethane (DEM) and triethyl orthoformate (TOF) have similar structures, TOF has one more ethoxy branch than DEM. As shown in the accompanying figures, while Comparative Example 2 exhibits some charge-discharge capability, its charging curve (delithiation process) shows significant instability and polarization, and its reversible capacity is significantly lower than that of Example 1. This indicates that the steric hindrance provided by the dioxyacetal structure (DEM) alone is insufficient to completely block the co-intercalation tendency of solvent molecules; some solvent molecules still enter the graphite interlayer along with lithium ions, causing structural damage. In contrast, Example 1, through the synergistic steric hindrance effect generated by the third branch, further weakens the coordination strength between the solvent and lithium ions, allowing more anions to enter the first solvation layer. This promotes the formation of a denser and lower impedance inorganic SEI film on the graphite surface, exhibiting superior voltage curve flatness and electrochemical stability.

[0067] Depend on Figure 2 Comparing Example 1 with Comparative Examples 1 and 2, it is evident that the branched ether structure exhibits superior cycling stability. Within a 40-cycle range, its reversible specific capacity remained stable around 340 mAh / g, with a flat curve and no significant capacity decay. This indicates that the TOF molecule, thanks to its strong three-branched steric hindrance, effectively protects the graphite layered structure throughout the long-term lithium intercalation / deintercalation process. In contrast, the capacities of Comparative Examples 1 and 2 showed a significant decrease in the early stages of cycling. The specific capacity of commonly used short-chain ethers dropped rapidly within a few cycles, eventually stabilizing at a low level of around 100 mAh / g, with significant curve fluctuations. This result demonstrates that, due to the lack of sufficient steric hindrance, linear ether solvent molecules undergo significant co-intercalation behavior, causing local collapse of the graphite layered structure and loss of some active sites, leading to a substantial reduction in reversible capacity. The significant difference between Example 1 and Comparative Example 2 further confirms that the additional branch in the TOF is of decisive technical significance for achieving complete non-co-intercalation of graphite.

[0068] In summary, Figure 2 The cycling data strongly demonstrates the core inventiveness of this invention: the steric hindrance effect generated by the branched structure design of solvent molecules not only solves the first-cycle compatibility problem but also ensures the structural integrity of the graphite anode during long-term cycling. Example 1 achieves comprehensive performance suppression over traditional linear ether systems (DME, DEM) in terms of cycling stability and interfacial efficiency, demonstrating extremely high practical value.

[0069] Comparing Example 4 with Comparative Examples 1 and 2, it can be seen that cyclic ether solvents also exhibit a significant steric hindrance-induced suppression of co-intercalation effects. (From the appendix...) Figure 1As can be seen, the charge-discharge curves of Example 2 are highly similar to those of Example 1 (TOF), exhibiting standard and stable graphite lithium intercalation / deintercalation behavior, with a reversible specific capacity remaining above 320 mAh / g. This demonstrates that, compared to the linear structure (DME / DEM), the cyclic structure (DOL) significantly increases the spatial rigidity and apparent volume of the lithium-ion solvation shell due to ring strain and spatial configuration constraints, thereby generating an effective physical shielding effect and preventing solvent molecules from penetrating into the graphite interlayer. This comparative result strongly proves that, regardless of whether it is a branched or cyclic design, constructing a weakly solvation sheath with significant steric hindrance can effectively solve the compatibility problem between ether solvents and graphite anodes.

[0070] By comparing the rate data of Examples 1, 2, 3, 4, and 5 with Comparative Example 3 in Table 1, it can be seen that the weakly solvated electrolyte provided by the present invention not only solves the compatibility problem between ethers and graphite, but also exhibits excellent high-rate fast charging performance.

[0071] First, Example 1 exhibits excellent kinetic stability. At 0.5 C, its specific capacity is 339.2 mAh / g; when the rate is further increased to 5 C, its specific capacity remains at 270.4 mAh / g, with a capacity retention (5 C / 0.2 C) of 78.2%. In contrast, the specific capacity of the commercial carbonate system in Comparative Example 3 drops rapidly to 105.5 mAh / g at 5 C, with a retention rate of only 30.3%. Example 1's specific capacity at 5 C is more than 2.5 times that of Comparative Example 3. This significant technical effect demonstrates that the weakly solvated sheath layer constructed using the steric hindrance effect of the triple-branched branched ether molecules can significantly reduce the desolvation energy barrier of lithium ions at the negative electrode interface, thereby maintaining extremely low polarization and a high lithium-ion insertion rate even under extremely fast charging conditions.

[0072] Secondly, Example 2 demonstrates the optimal room-temperature rate performance of this invention: its specific capacity reaches 365.2 mAh / g at 0.2 C and 356.5 mAh / g at 0.5 C, maintaining extremely high capacity retention even at high rates, with a capacity of 295.6 mAh / g at 5 C. This fully demonstrates the excellent synergistic effect between the spatial shielding effect of the TOF solvent and the dense SEI film formed by FEC: TOF molecules completely block the co-intercalation path of solvent molecules at the physical spatial level through intrinsic steric hindrance, while the ultrathin SEI film rich in LiF formed by FEC further optimizes the interfacial ion conductivity. The combination of the two significantly reduces interfacial impedance and desolventizing energy barrier while completely suppressing co-intercalation, thereby endowing the battery with extremely fast charging kinetics.

[0073] Furthermore, data from Example 3 shows that while the pure DOL system can be adapted to graphite anodes at low salt concentrations, its performance at high rates is mediocre due to its relatively high desolvation barrier. Its capacity at 5 C is only 120.4 mAh / g, significantly lower than Examples 1 and 2 of this application. This fully demonstrates the unique technical value of orthoformate ester (TOF) weak solvation solvents in improving fast-charging performance: TOF solvents not only solve the solvent co-intercalation problem through physical blocking, but their constructed extreme weak solvation sheath layer also significantly reduces the lithium-ion desolvation barrier, resulting in excellent kinetic stability in Examples 1 and 2.

[0074] Example 4 exhibited the highest capacity performance at low rates. Its specific capacity reached 358.2 mAh / g at 0.2 C, demonstrating that the synergistic effect of increasing salt concentration, film-forming aids (FEC, LiNO3), and cyclic ether solvents effectively induced the formation of a dense and stable SEI film, completely suppressing the co-intercalation of DOL molecules. Although the capacity of Example 4 at 5 C (198.5 mAh / g) was slightly lower than that of Examples 1 and 2, it was still far superior to Comparative Example 3. This further verifies that the synergistic effect of molecular configurational steric hindrance, film-forming co-solvents, and additives can also effectively improve the rate performance of the battery.

[0075] Comparing the data from Example 5 with those from Examples 1 and 2, it can be seen that using isopropyl ether (IPE) as the branched ether solvent, at a low salt concentration of 1 mol / L, the discharge specific capacity at 0.2 C is 342.1 mAh / g, without significant graphite layer stripping. This further demonstrates the universality of the principle of suppressing co-intercalation through steric hindrance, indicating that even without additives, the branched ether system can be initially adapted to commercial graphite anodes. However, as the discharge rate increases to 5 C, the capacity decay in Example 5 is significant, which again demonstrates that the unique three-branched structure in the TOF molecule has a more thorough steric shielding effect and a more intrinsic weak solvation capability compared to the two-branched structure.

[0076] Further analysis of the data from Examples 1, 6, and 7, as well as Comparative Example 4, reveals that the present invention's limitation of the carbon number of the weakly solvable ether solvent to 3-12 has a clear technical basis. Data from Examples 6 (C10) and 7 (C11) show that in the high carbon number range near the upper limit, the steric hindrance caused by the branching can still effectively suppress graphite co-intercalation, ensuring the utilization of the basic capacity. However, the results of Comparative Example 4 (C14) show that once the carbon number exceeds 12, although the steric hindrance effect still exists, the dramatic increase in viscosity due to the excessively large molecular weight severely deteriorates the ion conduction kinetics, leading to a precipitous drop in rate performance. Therefore, the present invention defines the range as 3-12, which represents the optimal balance between physical steric hindrance and transport kinetics.

[0077] In summary, the weakly solvated electrolyte designed in this invention uses TOF solvent as its core component, and achieves protection of the graphite anode through its intrinsic steric hindrance effect. At the same time, with the synergistic effect of additives such as FEC, the interfacial ion conductivity is further optimized, thereby enabling Example 2 to exhibit extreme specific capacity and rate retention at room temperature.

[0078] Since full cells represent the final application of electrolytes in practical applications, graphite||NCM811 full cells were assembled using Example 1 and Comparative Example 3 with commercial carbonate-based electrolytes, respectively, for cycle testing. The room temperature cycle performance is as follows: Figure 3 As shown, the low-temperature performance is as follows Figure 4 As shown.

[0079] Compare Figure 3 As can be seen, the full cell assembled using the electrolyte of Example 1 of this invention exhibits excellent cycle stability at room temperature (25°C). Looking at the corresponding left-axis discharge specific capacity curve in the figure, its initial discharge specific capacity is approximately 173.2 mAh / g, followed by a significant capacity ramp-up activation process, reaching a peak specific capacity of approximately 176.6 mAh / g after about 40 cycles. In subsequent cycles, the specific capacity of Example 1 is extremely stable, maintaining around 170.7 mAh / g after 100 cycles, demonstrating a very high capacity retention rate. In contrast, Comparative Example 3, using a conventional commercial electrolyte, although having an initial capacity similar to Example 1, exhibits a continuous and significant capacity decay trend from the initial stage of cycling, with its specific capacity decreasing to approximately 156.4 mAh / g by the end of 100 cycles, showing significantly inferior cycle stability compared to Example 1. The comparative results strongly demonstrate that the weakly solvated electrolyte described in this invention has excellent electrochemical stability when adapted to a full battery system with a high-nickel cathode and a graphite anode, ensuring that the capacity of the high-energy-density battery remains stable during long-cycle operation at room temperature.

[0080] Compare Figure 4It can be seen that Example 1, using the weakly solvated electrolyte of the present invention, exhibits excellent low-temperature cycling stability. Its initial discharge specific capacity is approximately 156 mAh / g. During the initial stage of cycling, it undergoes a typical electrochemical interface activation process, with the specific capacity steadily increasing and stabilizing at approximately 161 mAh / g. Furthermore, the capacity curve remains smooth and flat throughout the subsequent 50 cycles, with virtually no capacity decay. In contrast, Comparative Example 3, using a conventional commercial electrolyte, has a lower initial capacity at -20°C (approximately 146 mAh / g), and exhibits a continuous and significant capacity decay trend with increasing cycle number. These comparative results fully demonstrate that the weakly solvated electrolyte of the present invention can significantly reduce the desolvation energy barrier of lithium ions at the graphite anode interface, effectively overcoming the drawbacks of traditional carbonate electrolytes, such as slow kinetics and rapid capacity depletion caused by the difficult interface desolvation process at low temperatures. This allows lithium-ion batteries to maintain superior electrochemical activity and long cycle life even under extremely low temperature conditions.

[0081] In summary, through in-depth research on ether solvents with different structures, this invention has discovered that the key to suppressing solvent co-intercalation lies in constructing a weakly solvated structure to form a physical shield or reduce the binding energy. As shown in Examples 3, 4, and 5, even under conventional low salt concentrations, the weakly solvated design provided by this invention has already preliminarily solved the industry problem of graphite exfoliation, demonstrating the universality and reliability of the technical solution of this invention. Triethyl orthoformate (TOF), as a preferred embodiment, with its unique three-branched spatial configuration, further achieves excellent fast charging and wide temperature range characteristics while being compatible with graphite anodes. Therefore, the weakly solvated electrolyte system covered by this invention provides diversified technical path options for lithium-ion batteries with different application requirements.

[0082] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A weakly solvated electrolyte, characterized in that, Includes the following components: Lithium salts and weakly solvating solvents; The weak solvating solvent is an ether solvent with a branched structure or a cyclic sterically hindered structure and a carbon number of 3 to 12.

2. The weakly solvated electrolyte according to claim 1, characterized in that, The weak solvating solvent includes one or more of the following: triethyl orthoformate, trimethyl orthoformate, triisopropyl orthoformate, triethyl orthoacetate, trimethyl orthoacetate, tripropyl orthoacetate, triethyl orthopropionate, isopropyl ether, diisopentyl ether, methyl tert-butyl ether, ethyl tert-butyl ether, 1,3-dioxopentane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, and their heteroatom-substituted derivatives.

3. The weakly solvated electrolyte according to claim 1, characterized in that, The lithium salt includes one or more of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, and lithium difluorooxalate borate.

4. The weakly solvated electrolyte according to claim 1 or 3, characterized in that, The molar concentration of the lithium salt in the weakly solvated electrolyte is 0.5~3.0 mol / L.

5. The weakly solvated electrolyte according to claim 1, characterized in that, The weakly solvated electrolyte also includes a co-solvent; The cosolvent includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl acetate, ethyl acetate, ethyl propionate, methyl propionate, propyl propionate, fluorobenzene, fluoroethylene carbonate, and fluorocarboxylic acid esters.

6. The weakly solvated electrolyte according to claim 5, characterized in that, The volume ratio of the weakly solvating solvent to the co-solvent is 10:90~100:

0.

7. The weakly solvated electrolyte according to claim 1, characterized in that, The weakly solvated electrolyte also includes film-forming additives; The film-forming additives include one or more of the following: vinylene carbonate, ethylene vinylene carbonate, vinyl sulfate, 1,3,6-hexanetrionitrile, phenyltrivinylsilane, lithium bis(oxalato)borate, lithium difluorophosphate, 1,3-propanesulfonyl lactone, lithium nitrate, lithium difluorobis(oxalato)phosphate, lithium tetrafluorooxalato)phosphate, triallyl phosphite, methylene disulfonate, pyridine, difluorodiphenylsilane, and tri(trimethylsilyl) phosphite.

8. The weakly solvated electrolyte according to claim 7, characterized in that, The mass of the film-forming additive is 0-5% of the total mass of the weakly solvated electrolyte.

9. The method for preparing the weakly solvated electrolyte according to any one of claims 1 to 8, characterized in that, Includes the following steps: The lithium salt is mixed with the weak solvating solvent under anhydrous and oxygen-free conditions to obtain the weak solvating electrolyte.

10. The weakly solvated electrolyte according to any one of claims 1 to 8 or the weakly solvated electrolyte prepared by the preparation method according to claim 9 is used in a lithium-ion battery, characterized in that, The lithium-ion battery includes: a positive electrode, a graphite-based negative electrode, a separator, and the weakly solvated electrolyte.