A wide-temperature electrolyte, its preparation method and application
By designing a composite solvent system, a weak solvation shell structure was constructed by utilizing the synergistic effect of high-steric-barrier nitrile solvents and low-binding-energy linear solvents. This solved the problems of easy crystallization and slow desolvation of sodium-ion batteries at low temperatures, and achieved fast charging and long-cycle stability over a wide temperature range.
Patent Information
- Application Number
- CN202611362390.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-10
AI Technical Summary
Sodium-ion batteries are prone to crystallization failure in extreme low-temperature environments, resulting in a decline in kinetic performance and making it difficult to meet the requirements of wide-temperature-range applications. Furthermore, high-energy-density batteries exhibit slow desolvation kinetics at low temperatures, which limits their rate performance and safety.
A composite solvent system, including a high-steric-resistance nitrile solvent and a low-binding-energy linear solvent, is used to construct a weakly solvated shell structure through steric hindrance effect and binding energy difference design, which promotes rapid desolvation and interfacial reduction of sodium ions to form a low-impedance SEI film.
Maintaining electrolyte stability over a wide temperature range of -50℃ to 50℃ enables ultra-fast charging performance, low-temperature discharge capability, and long-cycle stability of sodium-ion batteries, while solving the problem of high-steric-resistance nitrile solvents easily freezing at low temperatures.
Smart Images

Figure CN123073170A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrolyte technology, and in particular to a wide-temperature electrolyte, its preparation method, and its application. Background Technology
[0002] Sodium-ion batteries have shown significant application potential in large-scale energy storage and power battery fields due to their abundant resources and low cost. However, the charge transfer kinetics of sodium ions at the electrode / electrolyte interface are sluggish, especially in fast charging and low-temperature applications. The excessively high desolvation energy barrier can easily induce the deposition of metallic sodium on the negative electrode side, which severely limits the battery's rate performance, low-temperature discharge capability, and operational safety.
[0003] Nitrile solvents (such as alkyl nitriles) typically possess high ionic conductivity, low viscosity, and excellent oxidation stability, effectively meeting the high-voltage cathode requirements of high-energy-density batteries. However, when pursuing extreme rate performance, the strong solvation effect of conventional nitriles becomes a kinetic bottleneck restricting the rapid insertion / extraction of ions from the electrode. To further improve fast-charging performance, constructing weakly solvated systems using branched or cyclic nitrile solvents with significant steric hindrance effects has become a research hotspot. These nitrile solvents utilize the steric hindrance effect generated by their large-volume branched or cyclic structures to not only weaken the steric hindrance of solvent molecules on Na+, but also... + It can enhance the binding force of the solvation shell, reduce the desolvation energy, and promote the reduction of anions at the interface by regulating the solvation shell structure, thereby generating a dense, stable solid electrolyte interphase (SEI) film with low interfacial impedance.
[0004] However, nitrile components also exhibit significant performance bottlenecks under extreme low-temperature environments. On the one hand, for nitrile components with extremely high steric hindrance (such as trimethylacetonitrile, TMAN), due to their highly symmetrical molecular structure and strong intermolecular forces, their melting points are usually high (e.g., TMAN's melting point is about 15~18℃), making them prone to phase transition crystallization at room temperature or low temperatures. On the other hand, for some nitrile components with low freezing points (such as isobutyronitrile), although they can remain liquid at low temperatures, their relatively weak steric hindrance and high solvation binding energy with sodium ions mean that, in extremely cold environments (such as -50℃), the solvation shell of a single component remains too stable, causing the interfacial desolvation kinetics to stagnate, making it difficult to meet the operating requirements of batteries in low-temperature environments.
[0005] Therefore, the key to realizing the practical application of sodium-ion batteries in a wide temperature range lies in how to break the physical phase transition of a single solvent component and reshape the solvation structure by altering the coordination synergy between solvent molecules while maintaining weak solvation characteristics. Furthermore, in the development of high-energy-density batteries, whether the electrolyte system can maintain high voltage compatibility and excellent oxidation stability with the cathode side while expanding and improving its operating temperature range and rate kinetics is also a crucial factor determining whether sodium-ion batteries can achieve full-scenario applications. Summary of the Invention
[0006] The purpose of this invention is to provide a wide-temperature electrolyte that utilizes the solvation difference effect between high-steric-resistance nitrile solvents and low-binding-energy linear solvents. This solves the problem of low-temperature crystallization in the electrolyte system and effectively reduces the difficulty of sodium ion desolvation at the interface, enabling sodium-ion batteries to have ultra-fast charging kinetics, low-temperature discharge capability, and long-cycle stability.
[0007] To overcome the shortcomings of the prior art, the present invention provides a wide-temperature electrolyte, comprising: Sodium salt and composite solvent; the composite solvent is composed of a high-steric-barrier nitrile solvent and a low-binding-energy linear solvent; The high-stress nitrile solvent has a branched or cyclic structure and is selected from one or more nitrile compounds having an isopropyl, sec-butyl, tert-butyl, or neopentyl structure; The binding energy of the low-binding-energy linear solvent with sodium ions is lower than that of the high-steric-barrier nitrile solvent with sodium ions.
[0008] Preferably, the volume ratio of the high-stress nitrile solvent to the low-binding-energy linear solvent is 2:8 to 8:2.
[0009] Preferably, the high-sterile-barrier nitrile solvent includes one or more of isobutyronitrile, 2-methylbutyronitrile, trimethylacetonitrile, 2,2-dimethylbutyronitrile, 2,3-dimethylbutyronitrile, 3-methylpentanitrile, cyclopropylacetonitrile, cyclobutylnitrile, and cyclopentanitrile.
[0010] Preferably, the low binding energy linear solvent comprises linear carbonates and / or linear carboxylic acid esters.
[0011] Preferably, the linear carbonate includes one or more of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, and dipropyl carbonate.
[0012] Preferably, the linear carboxylic acid ester includes one or more of methyl acetate, ethyl acetate, ethyl propionate, and methyl propionate.
[0013] Preferably, the high-sterile-barrier nitrile solvent is trimethylacetonitrile, and the low-binding-energy linear solvent is diethyl carbonate.
[0014] Preferably, the sodium salt includes one or more of sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethyl)sulfonyl)imide, sodium hexafluorophosphate, and sodium perchlorate.
[0015] The present invention also provides a method for preparing the above-mentioned wide-temperature electrolyte, comprising the following steps: A composite solvent is obtained by mixing a high-resistance nitrile solvent and a low-binding-energy linear solvent in a certain ratio. The sodium salt is then dissolved in the composite solvent and stirred until completely dissolved to obtain the wide-temperature electrolyte.
[0016] The present invention also provides a sodium-ion battery, comprising a positive electrode, a negative electrode, a separator, and the above-mentioned wide-temperature electrolyte, wherein the sodium-ion battery is capable of operating in a wide temperature range of -50°C to 50°C.
[0017] Beneficial effects: This invention provides a wide-temperature-range electrolyte, comprising: a sodium salt and a composite solvent; the composite solvent is composed of a high-resistance nitrile solvent and a low-binding-energy linear solvent; the high-resistance nitrile solvent has a branched or cyclic structure, selected from one or more nitrile compounds having isopropyl, sec-butyl, tert-butyl, or neopentyl structures; the low-binding-energy linear solvent has a lower binding energy with sodium ions than the high-resistance nitrile solvent. In this invention, the high-resistance nitrile solvent, which exhibits excellent fast-charging performance, has its physical state greatly influenced by molecular symmetry: for example, trimethylacetonitrile has extremely high lattice energy due to its highly symmetrical spherical structure, resulting in a melting point above 15°C. This invention introduces a low-binding-energy linear solvent with a flexible long-chain structure, utilizing the asymmetry of the geometric configuration between components to generate a strong "intermolecular interference effect," disrupting the regularized stacking tendency of nitrile molecules and solving the problem of easy crystallization failure of highly symmetrical components under low-temperature conditions. For nitrile components with low freezing points, the introduction of linear solvents plays a crucial role in reducing viscosity and effectively suppresses metastable aggregation that occurs at low temperatures of -50°C, ensuring the stability of the electrolyte in low-temperature environments.
[0018] This invention constructs a metastable weak solvation shell structure based on steric hindrance. In a solvation system dominated by highly sterically hindered nitrile solvents, large-volume branches (such as isopropyl, tert-butyl, etc.) or cyclic groups in the molecular structure generate significant steric repulsion. This repulsion forces Na at the microscopic level... + The distance between the coordinating atoms of Na and the solvent is stretched, resulting in Na +-N coordination bonds are in a high-energy metastable state, which weakens the stability of the first solvation shell from a thermodynamic perspective. At the same time, the low-binding-energy linear solvent enters the solvation system as a weak coordination medium. Since its interaction with the central ion is weaker than that of the highly sterically hindered nitrile, it does not enhance the overall solvation intensity through competitive coordination. Instead, due to its lower coordination tendency, it generates a dual dilution effect of steric hindrance and binding energy difference in the solvation shell. This effect makes it easier for anions to overcome the repulsion of solvent molecules and enter the first solvation shell to form contact ion pairs or ion aggregates, thereby inducing anions to preferentially participate in electrochemical reduction film formation and construct a low-impedance SEI interface rich in inorganic components.
[0019] Finally, this invention achieves a synergistic enhancement of both room-temperature kinetics and low-temperature performance. The composite solvent, designed based on the difference in binding energy, exhibits an extremely low desolvation energy barrier, enabling rapid desolvation of sodium ions at the interface. Experimental results show that, due to the significant reduction in overall viscosity and optimized conductivity of the linear component, the composite system exhibits superior rate performance at room temperature compared to pure nitrile systems with stronger binding energy. Furthermore, even in extreme cold environments of -50°C, the low-melting-point linear component optimizes ionic conductivity and significantly lowers the desolvation energy barrier, ensuring rapid migration and efficient desolvation of sodium ions at low temperatures. This guarantees a high proportion of battery capacity release and completely solves the problem of "easy freezing and kinetic paralysis" in high-steric-resistance nitrile electrolyte systems at low temperatures. Attached Figure Description
[0020] Figure 1 The first charge-discharge curves of HC || NFM full cells assembled using the electrolytes obtained in Example 1 and Comparative Example 1 are shown. Figure 2 The rate performance graphs show the HC || NFM full cells assembled using the electrolytes obtained in Example 1 and Comparative Example 1, respectively. Figure 3 The graph shows the 1C cycle performance of HC || NFM full cells assembled using the electrolytes obtained in Example 1 and Comparative Example 1, respectively. Figure 4 The graph shows the low-temperature discharge performance of the HC || NFM full cell assembled using the electrolyte obtained in Example 1. Detailed Implementation
[0021] Unless otherwise specified, the present invention does not have special requirements regarding the source of raw materials used, and commercially available products well known to those skilled in the art can be used.
[0022] This invention provides a wide-temperature electrolyte, comprising: Sodium salt and composite solvent; the composite solvent is composed of a high-steric-barrier nitrile solvent and a low-binding-energy linear solvent; The high-stress nitrile solvent has a branched or cyclic structure and is selected from one or more nitrile compounds having an isopropyl, sec-butyl, tert-butyl, or neopentyl structure; The binding energy of the low-binding-energy linear solvent with sodium ions is lower than that of the high-steric-barrier nitrile solvent with sodium ions.
[0023] The wide-temperature electrolyte of this invention includes sterically hindered nitrile compounds with branched or cyclic structures. This invention utilizes the steric hindrance effect generated by the large-volume branched chains (such as isopropyl, sec-butyl, tert-butyl, or neopentyl) or cyclic groups in the nitrile compounds to construct a weak solvation structure that is easy to desorb, thereby weakening the solvation intensity.
[0024] In this invention, the highly sterically hindering nitrile solvent having a branched or cyclic structure is preferably a nitrile compound solvent with 4 to 10 carbon atoms; in this invention, the branched structure is preferably one or more of isopropyl, sec-butyl, tert-butyl, or neopentyl. In a specific embodiment of this invention, the highly sterically hindering nitrile solvent includes one or more of isobutyronitrile, 2-methylbutyronitrile, trimethylacetonitrile, 2,2-dimethylbutyronitrile, 2,3-dimethylbutyronitrile, 3-methylpentanitrile, cyclopropylacetonitrile, cyclobutyl nitrile, or cyclopropionitrile (CPN), as shown in formulas (1) to (9):
[0025] In this invention, the high-stress nitrile solvent is further preferably trimethylacetonitrile.
[0026] In this invention, the low-binding-energy linear solvent is a linear component with a low melting point and low binding energy. The binding energy between the low-binding-energy linear solvent and sodium ions is lower than that between the high-steric-barrier nitrile solvent and sodium ions. Furthermore, the low-binding-energy linear solvent has a low dielectric constant and an extremely low freezing point. On the one hand, it effectively disrupts the symmetric stacking of high-steric-barrier nitrile molecules through intermolecular spatial interference effects, thereby suppressing the phase transition crystallization behavior of the system at low temperatures and keeping the electrolyte in a liquid state below -50°C. On the other hand, it utilizes its low binding energy characteristics to construct weak coordination sites within the solvation shell, significantly reducing the sodium ion desolvation energy barrier at low temperatures.
[0027] In this invention, the volume ratio of the high-stress nitrile solvent to the low-binding-energy linear solvent is 2:8 to 8:2, more preferably 4:6 to 6:4. Within this ratio range, the electrolyte can significantly suppress the crystallization behavior of the system at low temperatures while maintaining the advantage of weak solvation kinetics, thus extending the lower limit of the electrolyte's liquid window to -50°C.
[0028] In this invention, the low binding energy linear solvent preferably includes linear carbonates and / or linear carboxylic acid esters.
[0029] In this invention, the linear carbonate preferably includes one or more of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, and dipropyl carbonate, as shown in formulas (10) to (14):
[0030] The present invention selects linear carbonates, which can, on the one hand, disrupt the crystal regularity of high-sterile-barrier nitrile solvents through molecular stacking intervention and suppress low-temperature phase transitions; on the other hand, through their low binding energy characteristics, effectively reduce the desolvation energy barrier of sodium ions at the interface, thereby maintaining efficient interfacial ion dynamics at low temperatures.
[0031] In this invention, the linear carbonate is further preferably diethyl carbonate.
[0032] In this invention, the linear carboxylic acid ester preferably includes one or more of methyl acetate, ethyl acetate, ethyl propionate and methyl propionate.
[0033] In this invention, the high-sterile-barrier nitrile solvent is preferably trimethylacetonitrile, and the low-binding-energy linear solvent is preferably diethyl carbonate; the volume ratio of trimethylacetonitrile to diethyl carbonate is preferably 5:5. In a specific embodiment of this invention, the high-sterile-barrier nitrile solvent is preferably trimethylacetonitrile (TMAN). Trimethylacetonitrile (TMAN) has extremely high lattice energy due to its highly symmetrical spherical structure, and its melting point is usually above 15°C. As a main solvent, it utilizes the steric hindrance effect of its tert-butyl group to provide kinetic support. The low-binding-energy linear solvent is preferably diethyl carbonate (DEC) with a flexible long-chain structure as a weakly co-solvent. It utilizes the asymmetry of the geometric configuration between components to generate a strong "intermolecular interference effect," which disrupts the regularized stacking tendency of nitrile molecules, solves the problem of easy crystallization failure of highly symmetric components, and can adjust the solvation structure and suppress crystallization.
[0034] In this invention, the sodium salt preferably includes one or more of sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium hexafluorophosphate, and sodium perchlorate; in this invention, the concentration of sodium salt in the electrolyte is preferably 0.5 to 2.5 mol / L, more preferably 0.8 to 1.5 mol / L.
[0035] In this invention, the wide-temperature electrolyte further includes a film-forming additive; the film-forming additive includes one or more of fluoroethylene carbonate, ethylene sulfate, sodium difluorophosphate, sodium difluorooxalate borate, and sodium dioxoborate. In this invention, the mass of the film-forming additive accounts for 0.5% to 5% of the total mass of the electrolyte, more preferably 1% to 4%.
[0036] The wide-temperature electrolyte provided by this invention utilizes the synergistic regulation of "steric hindrance" and "binding energy difference." Although the selected high-steric-hindrance nitrile solvent has a relatively high initial binding energy with sodium ions, its large molecular structure creates a metastable structure in the solvation layer that is easily dissociated. Based on this, this invention introduces a linear solvent with lower binding energy and a lower melting point, which not only breaks the phase transition crystallization path of nitrile molecules but also utilizes the low viscosity and weak coordination properties of the linear component at low temperatures to ensure that sodium ions still maintain a high interfacial desolvation rate even in the extreme environment of -50℃.
[0037] The present invention further provides a method for preparing the above-mentioned wide-temperature electrolyte, comprising the following steps: A composite solvent is obtained by mixing a high-resistance nitrile solvent and a low-binding-energy linear solvent in a certain ratio. The sodium salt is then dissolved in the composite solvent and stirred until completely dissolved to obtain the wide-temperature electrolyte.
[0038] The present invention also provides the application of the above-mentioned wide-temperature electrolyte in sodium-ion batteries, and provides a sodium-ion battery including a positive electrode, a negative electrode, a separator and the above-mentioned wide-temperature electrolyte, wherein the sodium-ion battery can operate in a wide temperature range of -50°C to 50°C.
[0039] In this invention, the positive electrode material includes one or more of the following: sodium transition metal phosphate, layered transition metal oxide, Prussian blue analogues, polyanionic compounds, and tunnel oxides; more preferably, layered transition metal oxide or sodium transition metal phosphate; in this invention, the sodium transition metal phosphate includes sodium vanadium phosphate (Na3V2(PO4)3) and / or sodium vanadium fluorophosphate (Na3V2(PO4)2F3); the layered transition metal oxide has the chemical formula Na x MO2, wherein M is one or more transition metal elements; the transition metal elements include one or more of Mn, Fe, Co, Ni, Ti, Cr, Cu and V, and are more preferably NaNi. 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 (NFM).
[0040] In this invention, the negative electrode material is preferably one or more of carbon-based materials, alloy materials, and titanium-based oxide materials, and more preferably carbon-based materials; the carbon-based materials include hard carbon materials (HC) or soft carbon materials, and more preferably hard carbon materials; the alloy materials include one or more of tin-based alloy materials, antimony-based alloy materials, and phosphorus-based composite materials; the titanium-based oxide materials include sodium titanium phosphate (Na3Ti2(PO4)3) and / or sodium titanate (Na2Ti3O7).
[0041] In this invention, the diaphragm is preferably one or more of glass fiber, polypropylene, and polyethylene.
[0042] The sodium-ion battery wide-temperature electrolyte provided by this invention not only has the characteristics of low desolvation energy barrier, but also, due to its special weak coordination environment, can effectively promote the reduction of anions on the negative electrode surface to form an inorganic solid electrolyte interphase (SEI) film with low impedance and high mechanical strength. When applied to a sodium-ion battery system with hard carbon as the negative electrode, sodium ions can achieve rapid desorption and shuttle at the interface, exhibiting excellent fast-charging kinetic performance and long-cycle stability.
[0043] This invention utilizes a composite solvent of a high-steric-resistance nitrile solvent and a low-binding-energy linear component, leveraging the synergistic effect of binding energy differences and steric hindrance, to successfully suppress phase transition crystallization of solvent molecules at low temperatures. This electrolyte system not only solves the industry problem of conventional high-steric-resistance systems being prone to failure below room temperature, but also significantly expands the lower limit of the operating temperature range of sodium-ion batteries to -50°C. The electrolyte of this invention effectively ensures that sodium-ion batteries retain their advantages of high power density, long cycle life, and high capacity retention even in extremely cold environments.
[0044] The following examples, along with several other embodiments, will make the technical content clearer and easier to understand. This invention can be embodied in many different forms of embodiments, and the scope of protection of this invention is not limited to the embodiments mentioned herein.
[0045] Example 1
[0046] Under anhydrous and oxygen-free conditions, a 1.5 mol / L NaFSI electrolyte was prepared by dissolving sodium bis(fluorosulfonyl)imide (NaFSI) in TMAN / DEC (5:5, v / v) under trimethylacetonitrile (TMAN, structural formula 3) and diethyl carbonate (DEC, structural formula 11) in a volume ratio of 5:5.
[0047] Example 2
[0048] Under anhydrous and oxygen-free conditions, a 1.5 mol / L NaFSI electrolyte was prepared by dissolving sodium bis(fluorosulfonyl)imide (NaFSI) in TMAN / DEC (4:6, v / v) at a molar concentration of 1.5 mol / L in the solvents, using trimethylacetonitrile (TMAN, structural formula 3) and diethyl carbonate (DEC, structural formula 11) in a volume ratio of 4:6.
[0049] Example 3
[0050] Under anhydrous and oxygen-free conditions, a 1.5 mol / L NaFSI electrolyte was prepared by dissolving sodium bis(fluorosulfonyl)imide (NaFSI) in TMAN / DEC (6:4, v / v) at a molar concentration of 1.5 mol / L in the solvents, using trimethylacetonitrile (TMAN, structural formula 3) and diethyl carbonate (DEC, structural formula 11) in a volume ratio of 6:4.
[0051] Example 4
[0052] Under anhydrous and oxygen-free conditions, an electrolyte was prepared using 2,2-dimethylbutyronitrile (Structural Formula 4) and diethyl carbonate (DEC, Structural Formula 11) in a volume ratio of 5:5. Sodium difluorosulfonyl imide (NaFSI) was dissolved in the electrolyte at a molar concentration of 1.2 mol / L.
[0053] Example 5
[0054] Under anhydrous and oxygen-free conditions, an electrolyte was prepared using trimethylacetonitrile (TMAN, structural formula 3) and ethyl methyl carbonate (EMC, structural formula 10) in a volume ratio of 5:5. Sodium bis(fluorosulfonyl)imide (NaFSI) was dissolved in the electrolyte at a molar concentration of 1.2 mol / L.
[0055] Example 6
[0056] Under anhydrous and oxygen-free conditions, an electrolyte was prepared using isobutyronitrile (Structural Formula 1) and diethyl carbonate (DEC, Structural Formula 11) in a volume ratio of 5:5. Sodium difluorosulfonyl imide (NaFSI) was dissolved in the solvent at a molar concentration of 1.2 mol / L, and 1% sodium difluorooxalate borate (NaDFOB) was added.
[0057] Example 7
[0058] Under anhydrous and oxygen-free conditions, an electrolyte was prepared using trimethylacetonitrile (TMAN, structural formula 3) and dipropyl carbonate (structural formula 12) in a volume ratio of 5:5. Sodium bis(fluorosulfonyl)imide (NaFSI) was dissolved in the electrolyte at a molar concentration of 0.8 mol / L. This example demonstrates the wide-temperature performance under low-concentration salt systems.
[0059] Example 8
[0060] Under anhydrous and oxygen-free conditions, a dual-salt electrolyte was prepared by dissolving sodium bis(fluorosulfonyl)imide (NaFSI) and sodium hexafluorophosphate (NaPF6) in the electrolyte at a total concentration of 1.2 mol / L (molar ratio 1:1) under an anhydrous and oxygen-free environment.
[0061] Comparative Example 1
[0062] Under anhydrous and oxygen-free conditions, sodium difluorosulfonamide (NaFSI) was dissolved in trimethylacetonitrile (TMAN, structural formula 3) as a single solvent to prepare an electrolyte.
[0063] Comparative Example 2
[0064] Under anhydrous and oxygen-free conditions, sodium bis(fluorosulfonyl)imide (NaFSI) was dissolved in diethyl carbonate (DEC, structural formula 11) as a single solvent to prepare an electrolyte.
[0065] Comparative Example 3
[0066] Under anhydrous and oxygen-free conditions, an electrolyte was prepared by dissolving sodium bis(fluorosulfonyl)imide (NaFSI) at a molar concentration of 1.5 mol / L in ethylene carbonate (EC) and diethyl carbonate (DEC, structural formula 11) in a volume ratio of 5:5.
[0067] Comparative Example 4
[0068] Under anhydrous and oxygen-free conditions, an electrolyte was prepared by dissolving sodium bis(fluorosulfonyl)imide (NaFSI) at a molar concentration of 1.5 mol / L in trimethylacetonitrile (TMAN, structural formula 3) and ethylene carbonate (EC) in a volume ratio of 5:5.
[0069] Comparative Example 5
[0070] Under anhydrous and oxygen-free conditions, an electrolyte was prepared by dissolving sodium bis(fluorosulfonyl)imide (NaFSI) at a molar concentration of 1.5 mol / L in a solvent of n-butyronitrile (unbranched) and diethyl carbonate (DEC, structural formula 11) in a volume ratio of 5:5.
[0071] Comparative Example 6
[0072] Under anhydrous and oxygen-free conditions, an electrolyte was prepared by dissolving sodium bis(fluorosulfonyl)imide (NaFSI) at a molar concentration of 1.5 mol / L in trimethylacetonitrile (TMAN, structural formula 3) and dimethyl ethylene glycol (DME) in a volume ratio of 5:5.
[0073] Comparative Example 7
[0074] Under anhydrous and oxygen-free conditions, using cyclopropionitrile (CPN, structural formula 9) and diethyl carbonate (DEC, structural formula 11) as a composite solvent in a volume ratio of 5:5, sodium bis(fluorosulfonyl)imide (NaFSI) was dissolved in it at a molar concentration of 1.5 mol / L to prepare a 1.5 mol / L NaFSI in CPN / DEC (5:5, v / v) electrolyte.
[0075] Performance testing
[0076] With NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 Using O2 as the positive electrode, hard carbon as the negative electrode, and glass fiber as the separator, an HC || NFM button cell was assembled. The areal capacity of the NFM electrode at 0.2C was 0.945 mAh / cm³. 2 With an N / P ratio of 1.1, the cells were charged and discharged sequentially at 0.2C, 0.5C, 1C, 2C, 3C, 4C, and 5C, where 1C = 120 mA / g. The resulting electrochemical performance is summarized in Table 1. Figure 1 The first charge-discharge curves of HC || NFM button cells assembled using the electrolytes prepared in Example 1 and Comparative Example 1 are shown. Figure 2 The rate performance graphs show the HC || NFM button cells assembled using the electrolytes prepared in Example 1 and Comparative Example 1, respectively.
[0077] Table 1 shows the rate performance of the HC || NFM full cells assembled in each embodiment and comparative example.
[0078] As shown in Table 1, comparing Example 1 and Comparative Example 1, the TMAN (trimethylacetonitrile) system exhibits a slightly higher specific capacity at low rates (0.2C, 0.5C). However, when the rate increases to 1C and above, the capacity of Example 1 begins to significantly surpass that of Comparative Example 1, maintaining a high reversible capacity at a high rate of 5C. Conventionally, introducing a low-binding-energy and low-polarity linear solvent, DEC (diethyl carbonate), might lead to a decrease in the system's ability to dissociate sodium salts due to dilution, potentially causing battery capacity degradation. However, the experimental results of this invention show a significant "paradoxical" gain effect: as the rate increases to 1C and above, the capacity of Example 1 exhibits strong kinetic support, maintaining a reversible capacity of 82.8 mAh / g at a high rate of 5C, far exceeding the 68.2 mAh / g of Comparative Example 1. This anomaly can be attributed to the introduction of a binding energy gradient: although TMAN and Na... +The original binding energy of Na is higher than that of DEC, but the large tert-butyl group of TMAN generates a strong steric repulsion force, making Na... + The system is in a metastable state where it is prone to desorption. At this time, the introduction of DEC, which has a lower binding energy and extremely low viscosity, as an auxiliary medium significantly accelerates liquid phase transport and further reduces the interfacial desolvation energy barrier. This endows the composite system with excellent room temperature fast charging dynamics, enabling sodium ions to have rapid dissociation dynamics in complex shell environments. While completely breaking the bottleneck of low temperature phase transition of high steric components, it also greatly expands the battery's rate charge and discharge window and capacity release capability under extreme cold environments.
[0079] Based on the comparison of the effects of Example 1 and Comparative Example 3, it can be seen that the capacity of conventional ester electrolytes at 5C is only 42.4mAh / g, and the polarization is extremely severe. This further confirms that conventional ethylene carbonate EC has an excessively strong solvation binding energy with sodium ions, making it extremely difficult for desolvation to occur at the interface. In contrast, the "double weak" coordination environment constructed in this invention has an extremely low dissociation barrier, which is the core guarantee for high-rate fast charging.
[0080] Based on the comparison of the effects of Example 1 and Comparative Example 5, it can be seen that when the main solvent is replaced with a straight-chain nitrile lacking steric hindrance, the specific capacity at 5C drops significantly to 58.2 mAh / g. This strongly demonstrates that the presence of sterically hindered branched groups (such as tert-butyl groups) in the molecular structure is a necessary condition for weakening the coordination bond strength, promoting the entry of anions into the first solvation layer, and generating a low-resistance SEI film.
[0081] Based on the comparison of the effects of Examples 1, 2, and 3, it can be seen that in the composite solvent of TMAN and DEC, there is a significant synergistic boundary for the improvement of rate performance by the solvent ratio. Experimental results show that when the volume ratio of TMAN to DEC is 5:5, the full cell achieves optimal capacity performance at all rates, especially exhibiting the highest reversible capacity at a high rate of 5C. The experimental results indicate that the 5:5 volume ratio achieves a perfect balance between the advantages of high steric kinetics and bulk transport characteristics: on the one hand, TMAN provides sufficient steric hindrance to maintain a low desolvation energy barrier; on the other hand, DEC effectively neutralizes the viscosity of the nitrile components. In contrast, when the proportion of DEC is further increased (Example 2, 4:6), although the system viscosity decreases, the sterically hindered TMAN component is over-diluted, leading to a weakened weak coordination characteristic of the solvation shell, resulting in a less effective interfacial kinetic response under high current charge and discharge compared to Example 1. When the proportion of TMAN was increased (Example 3, 6:4), although the weak solvation effect was enhanced, the increase in the overall viscosity of the system limited the bulk migration rate of sodium ions, thereby inhibiting capacity release at high rates. Therefore, a solvent ratio of 5:5 is the optimal ratio for activating the synergistic potential of the "steric hindrance-weak coordination" mechanism and the "physical viscosity reduction" effect, and can construct an electrolyte system with the fastest kinetic response and the best rate performance.
[0082] Comparing Example 1 and Example 6, it can be seen that the appropriate introduction of film-forming additives (such as 1% NaDFOB) can assist FSI. - Anions are preferentially reduced on the surface of the hard carbon anode to construct a boron / fluorine-containing inorganic SEI film with both high mechanical strength and high Young's modulus, thereby further improving the first-cycle coulombic efficiency of the full cell to 88.54%.
[0083] Comparing Example 1 and Comparative Example 7, it can be seen that although the cyclopropionitrile (CPN) composite system performs reasonably well at 0.2C, it exhibits severe polarization in the high-rate range of 3C to 5C, with a specific capacity of only 45.3 mAh / g at 5C, significantly lower than the 82.8 mAh / g of Example 1. This strongly confirms the irreplaceable advantage of the tert-butyl steric hindrance effect unique to trimethylacetonitrile (TMAN) in reshaping the metastable weak solvation shell. Compared to the cyclopropionitrile structure, the tert-butyl group in Example 1 can more significantly elongate the Na... + The -N coordination bond length, combined with the desolvation leader site constructed by DEC, significantly reduces the desorption resistance of ions under extreme environments.
[0084] like Figure 3As shown, HC || NFM button cells were assembled using the electrolytes prepared in Example 1 and Comparative Example 1, respectively, and subjected to long-cycle charge-discharge tests at 1C. The battery using the electrolyte in Comparative Example 1 (TMAN) experienced a precipitous drop in capacity during the early stages of cycling, falling to approximately 65 mAh / g in less than 200 cycles. This was mainly attributed to the difficulty of interfacial desolvation in pure nitrile solvents at high rates, leading to severe sodium deposition on the negative electrode surface and damage to the SEI film. In contrast, the battery using the electrolyte in Example 1 of this invention maintained a specific capacity of approximately 90 mAh / g after 1000 stable cycles at 1C, exhibiting a capacity retention of up to 90%. This clearly demonstrates that the introduction of DEC reshapes the solvated shell, effectively suppresses the fast-charging sodium deposition side reaction, and endows the battery with excellent long cycle life.
[0085] like Figure 4 As shown, the battery assembled using the electrolyte of Example 1 of this invention was evaluated for its discharge capability over an ultra-wide temperature range of 20°C to -50°C. As the temperature decreased sequentially from 20°C to -20°C, -30°C, and -40°C, the battery's discharge voltage plateau and capacity showed a smooth transition without any impedance abrupt change due to phase transition. Even at the extreme low temperature of -50°C, the battery could still smoothly release approximately 0.4 mAh of reversible capacity. This low-temperature performance solves the problem of single TMAN solvent crystallizing and solidifying at 15°C. The underlying mechanism is that the intervention of the asymmetric molecule DEC generates strong eutectic interference, significantly lowering the system's solidification temperature. Simultaneously, at -50°C, the weaker binding energy of DEC acts as a kinetic "lubricating medium" for sodium ions to cross the interface, freeing ion desorption from the limitation of insufficient low-temperature thermal excitation energy.
[0086] In summary, the wide-temperature electrolyte proposed in this invention cleverly utilizes the asymmetric synergistic effect of the steric hindrance repulsion of nitrile molecules and the difference in binding energy gradient between the two types of solvents. This solves the fatal defect that high-steric-hindrance nitrile solvents are prone to solidification and crystallization at low temperatures. Furthermore, without increasing the system cost, it achieves 5C fast charging at room temperature, stable cycling at a high rate of 1000 cycles, and effective discharge operation at a low temperature of -50℃.
[0087] Although the above embodiments have provided a detailed description of the present invention, they are merely some, not all, embodiments of the present invention. Those skilled in the art can obtain other embodiments without inventive step, and these embodiments all fall within the protection scope of the present invention. It should be understood that any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention, utilizing the spatial steric hindrance effect and binding energy gradient control mechanism described in the present invention, should be included within the protection scope of the present invention.
Claims
1. A wide-temperature-range electrolyte, comprising: Sodium salt and composite solvent; the composite solvent is composed of a high-steric-barrier nitrile solvent and a low-binding-energy linear solvent; The high-stress nitrile solvent has a branched or cyclic structure and is selected from one or more nitrile compounds having an isopropyl, sec-butyl, tert-butyl, or neopentyl structure; The binding energy of the low-binding-energy linear solvent with sodium ions is lower than that of the high-steric-barrier nitrile solvent with sodium ions.
2. The wide-temperature electrolyte as described in claim 1, characterized in that, The volume ratio of the high-position-barrier nitrile solvent to the low-binding-energy linear solvent is 2:8 to 8:
2.
3. The wide-temperature electrolyte as described in claim 1 or 2, characterized in that, The high-position-barrier nitrile solvents include one or more of isobutyronitrile, 2-methylbutyronitrile, trimethylacetonitrile, 2,2-dimethylbutyronitrile, 2,3-dimethylbutyronitrile, 3-methylpentanitrile, cyclopropylacetonitrile, cyclobutylnitrile, and cyclopentanitrile.
4. The wide-temperature electrolyte as described in claim 1 or 2, characterized in that, The low binding energy linear solvents include linear carbonates and / or linear carboxylic acid esters.
5. The wide-temperature electrolyte as described in claim 4, characterized in that, The linear carbonate includes one or more of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, and dipropyl carbonate.
6. The wide-temperature electrolyte as described in claim 4, characterized in that, The linear carboxylic acid esters include one or more of methyl acetate, ethyl acetate, ethyl propionate, and methyl propionate.
7. The wide-temperature electrolyte as described in claim 1 or 2, characterized in that, The high-stress nitrile solvent is trimethylacetonitrile, and the low-binding-energy linear solvent is diethyl carbonate.
8. The wide-temperature electrolyte as described in claim 1, characterized in that, The sodium salt includes one or more of sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethyl)sulfonyl)imide, sodium hexafluorophosphate, and sodium perchlorate.
9. A method for preparing a wide-temperature electrolyte as described in any one of claims 1 to 8, comprising the following steps: A composite solvent is obtained by mixing a high-resistance nitrile solvent and a low-binding-energy linear solvent in a certain ratio. The sodium salt is then dissolved in the composite solvent and stirred until completely dissolved to obtain the wide-temperature electrolyte.
10. A sodium-ion battery, comprising a positive electrode, a negative electrode, a separator, and a wide-temperature electrolyte according to any one of claims 1 to 8 or a wide-temperature electrolyte prepared by the method of claim 9, wherein the sodium-ion battery is capable of operating in a wide temperature range of -50°C to 50°C.