A sodium-ion battery electrolyte, its preparation method, and a sodium-ion battery.
By using sodium-based aromatic nitrogen-containing additives to form a tight N-organic double layer structure in sodium-ion batteries, the incompatibility problem between the electrolyte and the hard carbon anode interface is solved, resulting in higher battery performance and stability.
Patent Information
- Application Number
- CN202510579592.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-10
AI Technical Summary
In sodium-ion batteries, the electrolyte and hard carbon anode interface are incompatible, leading to interface instability and affecting battery performance and safety.
Sodium-based aromatic nitrogen-containing additives, such as sodium-based aromatic azoles, idines, and azines, are used to form a tight N-organic double layer structure, constructing an ultra-thin and dense solid electrolyte interface film, thereby reducing the contact area between the electrode material and the electrolyte.
It improves the rate performance and cycle stability of sodium-ion batteries, reduces gas generation, and enhances the charge-discharge efficiency and long-term stability of the batteries.
Smart Images

Figure CN123073175A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion batteries, specifically to a sodium-ion battery electrolyte, its preparation method, and a sodium-ion battery. Background Technology
[0002] Sodium-ion batteries are considered one of the most promising next-generation high-energy storage systems due to the abundance of sodium resources, low cost, relative safety, and good low-temperature performance. To improve the overall performance of sodium-ion batteries, numerous researchers have conducted extensive research and optimization on key electrode materials over the past decade, and some important positive and negative electrode materials with large-scale application potential have already entered the industrialization process. In sodium-ion batteries, the electrolyte acts as a carrier for Na+. + And the key components for constructing the electrode-electrolyte interface layer largely determine its performance ceiling.
[0003] However, side reactions occurring at the electrolyte interface, and incompatibility between the electrolyte and its additives and the positive or negative electrode materials, prevent the formation of a stable solid electrolyte interface film during battery charge and discharge, leading to rapid performance degradation of sodium-ion batteries. Furthermore, this instability causes the electrolyte to continuously react with the electrode materials in subsequent charge and discharge cycles, generating gases that could compromise battery safety.
[0004] A well-designed interfacial reaction between the electrode and the electrolyte can construct a stable and robust solid electrolyte interfacial film, effectively preventing continuous electrolyte decomposition, suppressing gas generation, and contributing to the high electrochemical reversibility of sodium-ion battery systems. Therefore, the electrolyte is crucial for regulating electrochemical behavior and phase structure. Although some progress has been made in the regulation of the solid electrolyte interfacial film at the hard carbon anode interface in ether-based electrolytes, the problems at the hard carbon anode interface remain a significant challenge hindering the practical application of sodium-ion batteries. Summary of the Invention
[0005] To address the problem that conventional electrolytes for sodium-ion batteries struggle to achieve a stable and robust solid-state electrolyte interface film on a hard carbon anode, this invention provides an electrolyte for sodium-ion batteries. This electrolyte facilitates the formation of a thinner, more uniform, and denser interface layer, promoting the sodium-ion desolvation process and increasing the ion transport rate across the interface layer, thereby achieving superior rate performance and cycle stability in sodium-ion batteries.
[0006] To achieve the above objectives, the technical solution of the present invention is implemented as follows: The present invention provides a sodium-ion battery electrolyte, comprising a base electrolyte and an additive, wherein the additive is a sodium-based aromatic nitrogen-containing additive.
[0007] Preferably, the sodium-modified aromatic nitrogen-containing additive is any one or a mixture of two or more of the following: sodium-modified aromatic azole compounds, sodium-modified aromatic pyridine compounds, and sodium-modified aromatic azine compounds.
[0008] Furthermore, the aromatic azole compound is any of the compounds shown in the following structural formulas. The aromatic pyridine compound is any one of the compounds shown in the following structural formulas. The aromatic azine compound is any one of the compounds shown in the following structural formulas. .
[0009] It should be noted that not all derivatives of the above-mentioned compounds are listed in this article.
[0010] Furthermore, the basic electrolyte is composed of sodium salt and ether solvent, with the sodium salt concentration in the basic electrolyte being 0.5-2.0 mol / L and the additive concentration in the electrolyte being 0.01-0.10 mol / L.
[0011] Furthermore, the sodium salt is any one or a mixture of any two or more of sodium hexafluoroborate, sodium tetrafluoroborate, sodium trifluoromethanesulfonate, sodium difluorosulfonamide, sodium difluoromethanesulfonamide, sodium difluorooxalate borate, sodium dioxalate borate, sodium difluorobis(oxalate) phosphate, sodium tetrafluorooxalate phosphate, and sodium fluorosulfonate; the ether solvent is any one or a mixture of any two or more of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, 1,2-dimethoxypropane, and dimethoxymethane.
[0012] This invention also discloses a method for preparing a sodium-ion battery electrolyte, the steps of which are as follows: (1) Add any one or more of aromatic azole compounds, aromatic pyridine compounds, and aromatic azin compounds to an ether solvent to obtain solution A; add metallic sodium to solution A and let it stand to obtain a precursor solution; (2) Dissolve sodium salt in an ether solvent to obtain the basic electrolyte for sodium-ion batteries; (3) Add precursor solution to sodium-ion battery base electrolyte to obtain sodium-ion battery electrolyte.
[0013] Preferably, in step (1), the volume concentration of aromatic azole compounds, aromatic pyridine compounds, and aromatic azin compounds in solution A is 0.1-1.0 mol / L, the molar ratio of metallic sodium to aromatic azole compounds, aromatic pyridine compounds, or aromatic azin compounds is 1-1.2:1, and the standing time is 20-28 h.
[0014] Preferably, the sodium salt concentration in the basic electrolyte in step (2) is 0.5-2.0 mol / L; and the volume concentration of the sodium-modified aromatic nitrogen-containing additive in step (3) is 0.01-0.10 mol / L.
[0015] The present invention also discloses a sodium-ion battery, comprising a positive electrode, a negative electrode, and an electrolyte containing a sodium-containing aromatic nitrogen-containing additive disclosed in the present invention.
[0016] The negative electrode is a hard carbon negative electrode; the positive electrode is a layered oxide positive electrode or a polyanionic positive electrode.
[0017] The present invention has the following beneficial effects: This invention provides an electrolyte for sodium-ion batteries, comprising a sodium salt, an ether solvent, and a sodium-based aromatic nitrogen-containing additive. Due to the localized electronic enhancement structure of aromatic N-organic molecules, N-organic and Na+... + / Na 0 The two layers exhibit close interactions, thereby modulating the electrical bilayer structure through the Coulomb force of the N-Na-O (hard carbon anode). Under strong interactions, the compacted sodium-based N-organic double layer subsequently transforms into an ultrathin, dense N-organic-rich solid electrolyte interfacial film. Simultaneously, it effectively coats the material surface, reducing the contact area between the electrode material and the electrolyte and the exposure of surface defects, thus minimizing excessive electrolyte consumption and corresponding irreversible capacity loss, and suppressing gas generation. Furthermore, the formation of this interfacial film is further optimized during the subsequent sodium insertion / extraction process, constructing a thin and uniform interfacial film. The unique interfacial film composition accelerates the sodium ion desolvation polarization process and the interfacial transport process, thereby improving the rate performance and cycle stability of the sodium-ion battery. Attached Figure Description
[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 Cycling curve of a half-cell assembled with the electrolyte prepared in Example 1 of this invention; Figure 2 Cycling curve of a half-cell assembled with the electrolyte prepared in Example 2 of this invention; Figure 3 Cycling curve of a half-cell assembled with the electrolyte prepared in Example 3 of this invention; Figure 4 Cycling curve of a half-cell assembled with the electrolyte prepared in Example 4 of this invention; Figure 5 Cycling curve of a half-cell assembled with the electrolyte prepared in Example 5 of this invention; Figure 6 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Example 6 of the present invention; Figure 7 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Example 7 of the present invention; Figure 8 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Example 8 of the present invention; Figure 9 Cycling curve of a half-cell assembled with the electrolyte prepared in Example 9 of this invention; Figure 10 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Example 10 of the present invention; Figure 11 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Example 11 of the present invention; Figure 12 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Example 12 of the present invention; Figure 13 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Example 13 of the present invention; Figure 14 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Example 14 of this invention; Figure 15 The first-cycle charge-discharge curve and cycle curve of the half-cell assembled with the electrolyte prepared in Comparative Example 1 of the present invention. Figure 16 This is a comparison of the first-cycle charge-discharge curves and cycle curves of full cells assembled with the electrolytes prepared in Example 6 and Comparative Example 1 of the present invention, wherein the positive electrode is Na 0.72 Ni 0.32 Mn 0.68 O2; Figure 17The first-cycle charge-discharge curve and cycle curve of the full battery assembled with the electrolyte prepared in Example 6 and Comparative Example 1 are compared, wherein the positive electrode is Na4Fe3(PO4)2P2O7. Figure 18 This is the interface of Embodiment 6 and Comparative Example 1 of the present invention; Figure 19 The first-cycle discharge curve and gas production of the half-cell assembled with the electrolyte prepared in Comparative Example 1 of this invention. Detailed Implementation
[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] All raw materials used in the embodiments of the present invention are commercially available products.
[0022] Example 1 0.20 g of 1-methylimidazolium was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a 0.5 mol / L sodium 1-methylimidazolium solution. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium 1-methylimidazolium additive.
[0023] Example 2 0.17 g of triazole was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a 0.5 mol / L sodium triazole solution. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium triazole additive.
[0024] Example 3 0.18 g of tetrazolium was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a sodium tetrazolium solution with a volume concentration of 0.5 mol / L. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium tetrazolium additive.
[0025] Example 4 0.30 g of indazole was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a sodium indazole solution with a volume concentration of 0.5 mol / L. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium indazole additive.
[0026] Example 5 0.30 g of benzotriazole was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution and allowed to stand for 24 h to obtain a 0.5 mol / L sodium benzotriazole solution. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium benzotriazole additive.
[0027] Example 6 0.39 g of 2,2'-bipyridine was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a 0.5 mol / L sodium 2,2'-bipyridine solution. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium 2,2'-bipyridine additive.
[0028] Example 7 0.32 g of 1,5'-naphthidine was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a 0.5 mol / L sodium 1,5'-naphthidine solution. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium 1,5'-naphthidine additive.
[0029] Example 8 0.64 g of 2,2'-biquinoline was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a 0.5 mol / L sodium 2,2'-biquinoline solution. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium 2,2'-biquinoline additive.
[0030] Example 9 0.20 g of pyrazine was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a sodium pyrazine solution with a volume concentration of 0.5 mol / L. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium pyrazine additive.
[0031] Example 10 0.20 g of pyridazine was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a 0.5 mol / L sodium pyridazine solution. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium pyridazine additive.
[0032] Example 11 0.21 g of triazine was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a sodium phenazine solution with a volume concentration of 0.5 mol / L. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L of sodium triazine additive.
[0033] Example 12 0.32 g of phthalazine was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a sodium phenolate solution with a volume concentration of 0.5 mol / L. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.98 mL of the 1.0 mol / L base electrolyte was mixed with 0.02 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.01 mol / L sodium phenolate additive.
[0034] Example 13 0.21 g of triazine was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a sodium phenazine solution with a volume concentration of 0.5 mol / L. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.90 mL of the 1.0 mol / L base electrolyte was mixed with 0.10 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.05 mol / L sodium triazine additive.
[0035] Example 14 0.21 g of triazine was dissolved in 5 mL of diethylene glycol dimethyl ether to obtain a 0.5 mol / L precursor solution. 0.058 g of metallic sodium was added to the precursor solution, and the mixture was allowed to stand for 24 h to obtain a sodium phenolate solution with a volume concentration of 0.5 mol / L. 1.78 g of NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain a 1.0 mol / L base electrolyte. 0.80 mL of the 1.0 mol / L base electrolyte was mixed with 0.20 mL of the 0.5 mol / L precursor solution to obtain a sodium-ion battery electrolyte containing 0.10 mol / L sodium triazine additive.
[0036] Comparative Example 1 1.78 g NaPF6 was dissolved in 10 mL of diethylene glycol dimethyl ether and stirred for 12 h to obtain an electrolyte of 1.0 mol / L.
[0037] Performance tests were conducted on the products obtained in Examples 1-12 and Comparative Example 1. The specific test methods and results are as follows: Na4Fe3(PO4)2P2O7 or Na 0.72 Ni 0.32 Mn 0.68O2 is used as the positive electrode active material, and hard carbon is used as the negative electrode active material; Preparation of the positive electrode sheet: A sodium-ion battery positive electrode slurry was prepared by uniformly mixing the positive electrode active material, conductive agent Super P Li, and binder PVDF at a mass ratio of 8:1:1, using N-methylpyrrolidone as the solvent. The uniformly mixed slurry was coated onto aluminum foil, dried, rolled, and punched into discs with a diameter of 13 mm, yielding a loading of 9 mg / cm². 2 Positive electrode film.
[0038] Preparation of negative electrode sheet: A sodium-ion battery negative electrode slurry was prepared by uniformly mixing the negative electrode active material, conductive agent, and binder in a mass ratio of 8:1:1. The binder consisted of sodium chondroitin sulfate A (CS-A) and polyethylene oxide (PEO) in a mass ratio of 9:1. Deionized water was used as the solvent. The uniformly mixed slurry was coated onto copper foil, dried, rolled, and punched into 13 mm diameter discs, yielding a loading of 2.5 mg / cm². 2 Negative electrode plate.
[0039] Preparation of button sodium-ion batteries: Using hard carbon as the cathode and sodium metal foil as the anode, the electrodes, separator, electrolyte, sodium sheet, spring, and gasket are encapsulated in an argon-filled glove box using positive and negative electrode shells to obtain a 2025 coin cell. The electrolyte is then used in a coin half-cell. Hard carbon is used as the negative electrode, along with Na4Fe3(PO4)2P2O7 or Na... 0.72 Ni 0.32 Mn 0.68 Using O2 as the positive electrode, the electrode, separator, electrolyte, sodium sheet, spring sheet, and gasket are encapsulated in a glove box filled with argon gas using positive and negative electrode shells to obtain a 2025 coin cell.
[0040] By analyzing the data in Table 1-2 and... Figure 1-12 Analysis shows that in Examples 1-12, the sodium-ion half-cells using the electrolyte of this invention exhibited extremely outstanding cycle stability, with the capacity retention rate increasing from 95.8% to 100% after 50 cycles. In Examples 1-5, the electrolyte additives were aromatic azole compounds, which slightly improved the coulombic efficiency in the first week, with Example 5 showing a reversible specific capacity increase of approximately 10 mAh / g.