Electrolyte additives, electrolytes, secondary batteries, electrical equipment and energy storage devices
By combining electrolyte additives with specific structures and low molecular weight nitrile substances, the problem of thickness expansion of the positive and negative electrodes in secondary batteries under high voltage is solved, forming stable SEI and CEI films, thereby improving the overall stability and safety of the battery.
Patent Information
- Application Number
- CN202510593560.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-10
AI Technical Summary
Existing secondary batteries exhibit strong surface oxidation of the positive electrode material under high charging cutoff voltage, leading to frequent electrolyte side reactions, causing battery gas generation and failure. Furthermore, the loss of nitriles at the negative electrode affects the cycle stability of the negative electrode, resulting in severe expansion of the battery thickness.
A combination of electrolyte additives with specific structures and low molecular weight nitrile substances is used. Tertiary nitrogen atoms are adsorbed on the surface of the negative electrode, and the steric hindrance effect of the six-membered ring structure is used to suppress the negative electrode side reaction. The additives also accumulate on the positive electrode side to form an SEI film rich in S and N elements, which inhibits the dissolution of positive electrode metal ions and the oxidation of electrolyte to produce gas.
It effectively suppresses the thickness expansion of the positive and negative electrode sides of the battery, improves the high-temperature storage and float charging performance of the battery, and enhances the overall stability and safety of the battery.
Smart Images

Figure CN123073176A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery electrolyte technology, specifically to an electrolyte additive, an electrolyte, a secondary battery, an electrical device, and an energy storage device. Background Technology
[0002] Rechargeable batteries have been widely used in portable electronic devices (mobile phones, tablets, etc.), electric vehicles, and other fields. With technological advancements, the energy density requirements for rechargeable batteries are increasing. Developing cathode materials with higher charging cut-off voltages is one common technique for improving the energy density of rechargeable batteries. However, higher charging cut-off voltages result in stronger oxidizability on the surface of the cathode material, which can easily lead to side reactions in the electrolyte, causing battery gas production or even failure.
[0003] Therefore, nitriles are commonly used as high-voltage additives in the electrolyte of secondary batteries to stabilize the positive electrode interface and reduce the probability of oxidative decomposition and gas generation of the electrolyte under high voltage and the catalytic effect of metal ions in the positive electrode material. However, nitriles are easily lost at the negative electrode during battery charging and discharging, affecting the cycle stability of the negative electrode. Simultaneously, they cannot effectively suppress electrolyte oxidation and gas generation on the positive electrode side, leading to significant thickness expansion of the battery during high-temperature storage and float charging. Therefore, it is necessary to provide an improved electrolyte solution to effectively reduce the thickness expansion problem of secondary batteries. Summary of the Invention
[0004] Therefore, embodiments of this application provide an electrolyte additive, an electrolyte, a secondary battery, and an electrical device. This electrolyte additive, through the combined use of a nitrile additive and another additive with a specific structure in a specific ratio, can simultaneously suppress battery thickness expansion on both the negative and positive electrode sides of the battery.
[0005] The first aspect of this application provides an electrolyte additive, comprising the substance shown in formula (I) and a nitrile substance with a molecular weight of less than 300:
[0006]
[0007] In formula (I), n is 0, 1 or 2, R1 is selected from alkenyl, haloalkenyl, alkynyl or haloalkynyl, m is an integer from 0 to 4, and R2 is selected independently each time from a halogen atom, substituted or unsubstituted alkyl, substituted or unsubstituted cycloalkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl or substituted or unsubstituted aryl; and the mass ratio of the nitrile substance to the substance shown in formula (I) is (10-100):1.
[0008] The aforementioned electrolyte additive combines the substance shown in Formula (I) with low-molecular-weight nitrile substances in an appropriate ratio. The appropriate amount of Formula (I) added can adsorb onto the negative electrode surface based on tertiary nitrogen atoms, and can suppress the adsorption of nitrile substances on the battery negative electrode surface and the resulting side reactions based on the steric hindrance effect of the six-membered ring structure. Simultaneously, during battery formation, the unsaturated bond R1 in Formula (I) can promote the reduction and decomposition of Formula (I) at the battery negative electrode, forming an SEI film rich in S and N elements, with good ionic conductivity and mechanical elasticity, thereby suppressing the increase in the thickness of the battery negative electrode. On the positive electrode side, nitrile substances are more likely to accumulate on the positive electrode surface due to the aforementioned negative electrode suppression effect, fully utilizing their adsorption, complexation / film-forming effects at the positive electrode, suppressing the dissolution of positive electrode metal ions and the continuous oxidation of the electrolyte, making it less prone to gas generation at high voltage, thus alleviating the battery thickness expansion problem caused by gas generation during high-temperature storage and float charging. Therefore, this electrolyte additive achieves bidirectional suppression of thickness expansion on both the negative and positive electrode sides of the battery, thereby effectively suppressing the overall thickness expansion of the battery.
[0009] In some embodiments of this application, the alkenyl, haloalkenyl, alkynyl, and haloalynyl groups have 2-10 carbon atoms; the substituted or unsubstituted alkyl groups have 1-10 carbon atoms; the substituted or unsubstituted cycloalkyl groups have 3-10 carbon atoms; the substituted or unsubstituted alkenyl groups have 2-10 carbon atoms; and the substituted or unsubstituted aryl groups have 6-30 carbon atoms. The appropriate number of carbon atoms in each group facilitates the preparation of the substance shown in formula (I) and enables good dispersion in battery electrolytes.
[0010] In some embodiments of this application, R1 is selected from one of C2-C5 alkenyl, halogenated C2-C5 alkenyl, C2-C5 ynyl, and halogenated C2-C5 ynyl. In this case, the substance represented by formula (Ⅰ) not only has high solubility in the battery electrolyte, but such R1 groups are also easily reduced at the battery negative electrode to obtain a negative electrode interface film with good ion conductivity and mechanical stability.
[0011] In some embodiments of this application, the substance represented by formula (I) includes one or more substances with structural formulas such as (I1)-(I15):
[0012]
[0013] In some embodiments of this application, the nitrile material includes compounds containing 2-3 cyano groups in their molecular structure. In this case, the nitrile material provides better stability to the battery positive electrode.
[0014] In some possible embodiments, the nitrile substance includes at least one selected from succinic anionyl nitrile, glutaronitrile, adiponitrile, 1,4-dicyano-2-butene, 1,3,5-pentanetrionitrile, 1,3,6-hexanetrionitrile, 1,2-bis(2-cyanoethoxy)ethane, and 1,2,3-tris(2-cyanoethoxy)propane.
[0015] In some embodiments of this application, the mass ratio of the nitrile substance to the substance shown in formula (I) is (20-30):1. In this case, the synergistic effect of the two additives is better, thereby suppressing battery thickness expansion on both the positive and negative electrode sides of the battery.
[0016] The second aspect of this application provides an electrolyte comprising an electrolyte salt, an organic solvent, and the electrolyte additives described in the first aspect of this application.
[0017] The electrolyte described above uses both the substance shown in formula (I) and nitrile substances as electrolyte additives. When the two meet a specific mass ratio, the substance shown in formula (I) can preferentially adsorb onto the negative electrode of the battery, suppressing the adsorption of nitrile substances at the negative electrode and the resulting side reactions. Benefiting from this, nitrile substances can effectively exert their adsorption effect at the positive electrode, suppressing the catalytic oxidation and gas production of the electrolyte by the high-voltage positive electrode. Simultaneously, the nitrogen- and sulfur-containing organic interface film generated by the reduction of the substance shown in formula (I) at the negative electrode can improve the stability of the negative electrode interface and suppress the volume expansion caused by negative electrode side reactions. Therefore, this electrolyte effectively suppresses battery thickness expansion on both the negative and positive electrode sides, inhibiting the hard expansion on the negative electrode side and the electrolyte gas production and expansion problems on the positive electrode side.
[0018] In some embodiments of this application, the mass percentage of the substance represented by formula (I) in the electrolyte is 0.04%-0.65%, and / or the mass percentage of the nitrile substance in the electrolyte is 2.5%-6.5%. When both the substance represented by formula (I) and the nitrile substance are used in the electrolyte at appropriate mass ratios, controlling the mass percentage of the substance represented by formula (I) and / or the nitrile substance itself in the electrolyte within a suitable range can also prevent the thickness of the SEI film on the negative electrode side and / or the CEI film on the positive electrode side from becoming excessively large, thus increasing the battery impedance.
[0019] In some possible implementations, the substance represented by formula (Ⅰ) is present in the electrolyte at a mass percentage of 0.05%-0.5%, and / or the nitrile substance is present in the electrolyte at a mass percentage of 3%-6%. In this case, the synergistic effect of the two additives is better, and the reduction in thickness expansion of the secondary battery using the above electrolyte is more significant.
[0020] In some embodiments of this application, the electrolyte additive further includes fluoroethylene carbonate (FEC). FEC can form a passivation interface film on the negative electrode surface during battery formation, suppressing continuous side reactions of the electrolyte at the negative electrode, and can also help suppress the adsorption and reduction consumption of nitriles at the negative electrode.
[0021] In some possible implementations, the fluoroethylene carbonate ester constitutes 5%-50% by mass in the electrolyte. This helps ensure that the negative electrode interface film formed with the participation of FEC has an appropriate thickness, preventing excessive negative electrode interface impedance.
[0022] In some possible embodiments of this application, the mass ratio of the substance represented by formula (I) to the fluoroethylene carbonate is 0.001-0.065. This ensures that the film-forming effect of FEC during battery formation is not excessively suppressed, thus affecting the cycle stability of the negative electrode, while also preventing an excessive increase in the interface impedance of the battery negative electrode. Furthermore, it effectively leverages the effect of the substance represented by formula (I) in improving the stability of the battery negative electrode side, ensuring that the battery thickness does not expand excessively.
[0023] In some possible embodiments of this application, the mass ratio of the nitrile material to the fluoroethylene carbonate is 0.0625-0.65. This ensures that the film-forming effect of FEC during battery formation is not excessively suppressed, thus affecting the cycle stability of the negative electrode, while also preventing an excessive increase in the interface impedance of the battery negative electrode. Furthermore, it ensures that the nitrile material effectively improves the stability of the battery positive electrode side and suppresses the thickness expansion of the battery caused by electrolyte gas generation.
[0024] In some embodiments of this application, the electrolyte further includes thioesters. Thioesters are generally used as negative electrode film-forming additives to help improve the cycle performance of the battery.
[0025] In some possible implementations, the thioester material is present in the electrolyte at a mass percentage of 1%-5%. This helps ensure that the electrode interface film formed by the thioester material has an appropriate thickness.
[0026] In some possible embodiments, the thioesters include one or more of the following: 1,3-propanesulfonate lactone, 1,4-butanesulfonate lactone, 1,3-propenesulfonate lactone, methanedisulfonate, vinyl sulfate, vinyl sulfite, 4-methyl ethylene sulfate, dimethyl sulfite, diethyl sulfite, dimethyl sulfate, and diethyl sulfate.
[0027] In some embodiments of this application, the electrolyte further includes other additives; these other additives include one or more of biphenyl, fluorobenzene, trifluoromethyl ethylene carbonate, vinylene carbonate, ethylene ethylene carbonate, and flame retardants. Other additives may be selected according to the different performance requirements of the electrolyte.
[0028] In some embodiments of this application, the organic solvent includes one or more of carbonate solvents, carboxylic acid ester solvents, and ether solvents.
[0029] A third aspect of this application provides a secondary battery, which includes a positive electrode, a negative electrode, a separator and an electrolyte located between the positive electrode and the negative electrode, wherein the electrolyte includes the electrolyte described in the second aspect of this application.
[0030] This secondary battery uses an electrolyte containing the aforementioned specific additives, which can achieve good high and low temperature cycle capacity stability. It can also achieve a low battery thickness expansion rate under conditions such as high temperature storage, high temperature float charging, and normal temperature cycling. This battery has good stability and safety.
[0031] In some embodiments of this application, the secondary battery includes a lithium secondary battery, a sodium secondary battery, a potassium secondary battery, a magnesium secondary battery, a zinc secondary battery, or an aluminum secondary battery.
[0032] In some embodiments of this application, the negative electrode includes one or more of the following: lithium titanate negative electrode, carbon-based negative electrode, silicon-based negative electrode, tin-based negative electrode, phosphorus-based negative electrode, lithium negative electrode, sodium negative electrode, potassium negative electrode, magnesium negative electrode, zinc negative electrode, and aluminum negative electrode.
[0033] In some embodiments of this application, the carbon-based anode includes one or more of graphite, hard carbon, soft carbon, porous carbon, mesophase carbon microspheres, and graphene; the silicon-based anode includes one or more of elemental silicon, silicon-carbon materials, silicon oxides, and silicon compounds; the tin-based anode includes one or more of elemental tin, tin-carbon materials, tin oxides, and tin compounds; the phosphorus-based anode includes one or more of red phosphorus, black phosphorus, and phosphorus compounds; the lithium anode includes elemental lithium or a lithium alloy; the sodium anode includes elemental sodium or a sodium alloy; the potassium anode includes elemental potassium or a potassium alloy; the magnesium anode includes elemental magnesium or a magnesium alloy; the zinc anode includes elemental zinc or a zinc alloy; and the aluminum anode includes elemental aluminum or an aluminum alloy.
[0034] In some embodiments of this application, the positive electrode includes one or more of layered transition metal oxide positive electrode materials and polyanionic positive electrode materials. Among them, layered transition metal oxides have a higher charging cut-off voltage and are particularly suitable for use with the above-mentioned electrolytes using nitrile substances as additives.
[0035] The fourth aspect of this application provides an electrical device, including a housing and a battery housed within the housing, the battery including the secondary battery described in the third aspect of this application.
[0036] The electrical equipment is powered by the secondary battery described in this application, and the equipment has a long service life and outstanding market competitiveness.
[0037] A fifth aspect of this application provides an energy storage device, which includes the secondary battery described in the embodiments of this application. The secondary battery in this embodiment stores electrical energy in the energy storage device, thereby improving the performance of the energy storage device and enhancing its product competitiveness. Attached Figure Description
[0038] Figure 1 This is a schematic diagram of a secondary battery provided in an embodiment of this application.
[0039] Figure 2 This is a schematic diagram of the structure of an electrical device provided in an embodiment of this application.
[0040] Figure 3 This is a schematic diagram of the structure of an energy storage device provided in an embodiment of this application.
[0041] Figure 4 The room temperature cycle capacity curves of the lithium secondary batteries of Examples 2, 4, and 7 and Comparative Examples 1 and 4 of this application are summarized. Detailed Implementation
[0042] The embodiments of this application will now be described in conjunction with the accompanying drawings.
[0043] like Figure 1 As shown, the main components of the secondary battery 100 (taking a lithium secondary battery as an example) include a positive electrode 10, a negative electrode 20, a separator 30, and an electrolyte 40. The separator 30 is disposed between the positive electrode 10 and the negative electrode 20, and the electrolyte 40 fills the space between the positive electrode 10 and the negative electrode 20 and wets the separator 30. The electrolyte 40 is lithium-ion (Li₂O₃) electrolyte. + The medium that transports energy between the positive electrode 10 and the negative electrode 20. During charging, Li... + The Li is extracted from the positive electrode active material 102 of the positive electrode 10, passes through the electrolyte 40, and is then embedded into the negative electrode active material 202 of the negative electrode 20; during discharge, Li + It is extracted from the negative electrode active material 202, passes through the electrolyte 40, and then inserts into the crystal lattice of the positive electrode active material 102.
[0044] During the initial charging (formation) of the battery, the electrolyte reacts on both the positive and negative electrode sides to form corresponding electrolyte interface films. The electrolyte interface film formed on the surface of the negative electrode 20 is generally called the solid electrolyte interface (SEI) film, while the electrolyte interface film formed on the surface of the positive electrode 10 is usually called the cathode electrolyte interphase (CEI) film. When the stability of the generated SEI film is insufficient, the electrolyte will continuously undergo side reactions with the negative electrode 20, deteriorating the negative electrode performance and increasing its thickness. When the stability of the generated CEI film is insufficient or the positive electrode cannot be effectively stabilized by adsorption of specific species, the positive electrode active material 102 will catalyze the oxidation of the electrolyte 40, leading to gas production. Simultaneously, metal ions in the positive electrode active material will dissolve, affecting battery performance. Therefore, it is necessary to develop suitable electrolytes to form good SEI and CEI films, effectively stabilize the positive and negative electrode materials, suppress battery expansion due to side reactions, and improve overall battery performance.
[0045] Currently, in pursuit of higher energy density, secondary batteries are developing cathode materials with higher charging cut-off voltages. However, high-voltage cathode materials (e.g., charging cut-off voltages above 4.5V) experience more severe side reactions with the electrolyte. This significantly increases the probability of battery gas production caused by electrolyte side reactions, and makes it easier for metal elements in the cathode material to dissolve, thus affecting the battery's cycle performance. To address these issues in high-voltage battery systems, high-voltage additives are typically added to the electrolyte. For example, in lithium secondary batteries using lithium cobalt oxide cathode materials and silicon-carbon anode materials, nitrile substances are used as high-voltage cathode additives in the electrolyte. The aim is for nitrile substances to play an adsorption, complexation, / film-forming role at the cathode, inhibiting the dissolution of cathode metal ions and the continuous oxidation and gas production catalyzed by the high-voltage cathode. However, in practical applications, nitrile substances do not always accumulate in large quantities on the positive electrode surface to form a stable CEI film, effectively suppressing electrolyte oxidation and gas generation, as well as the dissolution of positive electrode metal ions. This leads to severe battery thickness expansion problems caused by gas generation during high-temperature storage and float charging. Nitriles are actually more easily adsorbed at the negative electrode and consumed through reduction reactions, which further hinders their stability at the positive electrode and degrades the stability of the SEI film on the negative electrode side. Consequently, the SEI film cannot suppress the volume expansion of the negative electrode material, resulting in increased negative electrode thickness. Therefore, to address the battery thickness expansion problem in high-voltage battery systems, this application provides an electrolyte additive, an electrolyte, a secondary battery, and an electrical device.
[0046] Specifically, the electrolyte additives provided in this application include: the substance represented by formula (Ⅰ) and nitrile substances with a molecular weight of less than 300:
[0047]
[0048] In formula (I), n is 0, 1 or 2, R1 is selected from alkenyl, haloalkenyl, alkynyl or haloalkynyl, m is an integer from 0 to 4, and R2 is selected independently each time from a halogen atom, substituted or unsubstituted alkyl, substituted or unsubstituted cycloalkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl or substituted or unsubstituted aryl; and the mass ratio of the nitrile substance to the substance shown in formula (I) is (10-100):1.
[0049] When n = 0, the above -S (= O) n Specifically, -S-; when n=1, -S(=O) n Specifically, it is a sulfoxide group (-S(=O)-); when n=2, -S(=O) n - Specifically, it is a sulfone group (-S(=O)2-). When m=0, it means that there is no substituent R2 on the four carbon atoms of the six-membered ring in formula (Ⅰ). R2 represents the substituent on the ring in formula (Ⅰ) when m is a non-zero integer. When m is not 0, it means that at least one of the four carbon atoms of the six-membered ring in formula (Ⅰ) has a substituent R2.
[0050] When the substance shown in Formula (I) is combined with low molecular weight nitrile substances in an appropriate ratio, on the one hand, the appropriate amount of the added substance of Formula (I) can be adsorbed on the surface of the negative electrode based on the tertiary nitrogen atom. The six-membered ring structure of the substance of Formula (I) exerts a steric hindrance effect, which can suppress the adsorption of nitrile substances on the surface of the battery negative electrode and the side reactions that occur thereafter. As a result, nitrile substances are more likely to accumulate on the surface of the positive electrode, giving full play to their adsorption complexation / film formation effect on the positive electrode, suppressing the dissolution of positive electrode metal ions and the continuous oxidation and gas production of the electrolyte, so that the positive electrode side of the battery is less likely to produce gas under high voltage, thereby alleviating the problem of battery thickness expansion caused by gas production during high-temperature storage and float charging. On the other hand, during battery formation, the substance of formula (Ⅰ) adsorbed on the negative electrode can promote its reduction and decomposition at the negative electrode through the unsaturated bond R1 in its structure. The free radicals formed by R1 can polymerize, and simultaneously, the ring structure on the right side undergoes ring-opening and breaking, participating in the formation of an SEI component rich in S and N elements. This helps improve the ionic conductivity, mechanical elasticity, and stability of the SEI film, thereby suppressing the increase in negative electrode thickness. This SEI film can also suppress the side reactions of nitriles at the negative electrode and the resulting increase in negative electrode thickness. Therefore, the above-mentioned electrolyte additives exert an effect of suppressing battery thickness expansion on both the negative and positive electrode sides of the battery.
[0051] Furthermore, if the mass ratio of the nitrile to the substance shown in formula (I) is less than 10, on the one hand, insufficient nitrile cannot stabilize the positive electrode, and on the other hand, excessive substances of formula (I) will decompose at the negative electrode interface, increasing the negative electrode interface impedance, affecting the rate performance and cycle performance of the battery, and affecting the reaction of other film-forming additives that may exist in the electrolyte, thus degrading the cycle stability of the negative electrode. If the mass ratio of the nitrile to the substance shown in formula (I) is greater than 100, insufficient substances of formula (I) cannot effectively suppress the decomposition loss of the nitrile on the negative electrode side. If the molecular weight of the nitrile is too high, the nitrile may surround the substance of formula (I), affecting the barrier adsorption effect of the substance of formula (I) on the nitrile at the negative electrode.
[0052] Therefore, by combining nitrile substances of appropriate molecular weight with the substances shown in formula (Ⅰ) in an appropriate mass ratio, the side reaction problem caused by using nitrile additives alone at the negative electrode of the battery can be solved, the instability of the negative electrode SEI film and the expansion of the negative electrode thickness caused by the side reaction can be suppressed, and the beneficial effect of nitrile additives on the positive electrode side of the battery can be enhanced, so as to better suppress the expansion caused by the oxidation of electrolyte gas at the positive electrode of the battery. Thus, the above electrolyte additives play a role in suppressing the thickness expansion of the battery on both the positive and negative electrode sides of the battery, thereby effectively suppressing the overall thickness expansion of the battery.
[0053] It should be further noted that in the ring structure of formula (Ⅰ), the tertiary nitrogen atom interacts with S (=O). n - The groups are indirectly connected by substituted or unsubstituted ethylenes, which can avoid the weakening of the electron-donating ability of the tertiary nitrogen atom caused by direct connection between the two, which is not conducive to the adsorption of the substance of formula (Ⅰ) at the negative electrode.
[0054] For example, the mass ratio of the nitrile substance to the substance shown in formula (I) can be 10, 15, 18, 20, 22, 25, 28, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100. For another example, the mass ratio can be between 10 and 30, or between 20 and 50, or between 40 and 80, or between 70 and 100. In some embodiments, the mass ratio of the nitrile substance to the substance shown in formula (I) can be in the range of (20-30):1. In this case, the synergistic effect of the two additives is better, and they can better suppress battery thickness expansion on both the positive and negative electrode sides of the battery. Therefore, the battery has a lower thickness expansion rate under conditions such as high-temperature storage, high-temperature float charging, and normal-temperature cycling, and better cycle performance.
[0055] In this embodiment, the number of carbon atoms in R1 of the alkenyl, haloalkenyl, alkynyl, and haloalkynyl groups can be 2-10. For example, the number of carbon atoms in the alkenyl, alkynyl, haloalkenyl, and haloalkynyl groups can be independently selected from 2, 3, 4, 5, 6, 7, 8, 9, or 10. The halogenated or unhalogenated alkenyl and alkynyl groups have suitable numbers of carbon atoms, and the substances shown in formula (I) are relatively easy to prepare and can achieve good dispersion in battery electrolytes, avoiding the negative impact of uneven dispersion. The alkenyl, haloalkenyl, alkynyl, and haloalkynyl groups can be straight-chain or branched-chain structures. In some embodiments, R1 can be selected from one of C2-C5 alkenyl, haloC2-C5 alkenyl, C2-C5 alkynyl, and haloC2-C5 alkynyl groups. In this case, the substance shown in formula (Ⅰ) not only has high solubility in the organic solvent of the battery electrolyte, but also the R1 group is easily reduced at the negative electrode of the battery to obtain an SEI film with good ion conductivity and mechanical stability. For example, R1 can be selected from vinyl, propenyl, ethynyl, propynyl, n-butenyl, n-pentenyl, n-butynyl, n-pentynyl, etc.
[0056] In R1 above, the halogen in the halogenated alkenyl or halogenated alkynyl groups can include one or more of fluorine (F), chlorine (Cl), bromine (Br), and iodine (I). "Halogenated..." means that any one or more hydrogen atoms in a group are replaced by a halogen atom. This halogenation can be full halogenation or partial halogenation. "Full halogenation" means that all hydrogen atoms in the above group are replaced by halogen atoms. "Partial halogenation" means that some hydrogen atoms in the above group are replaced by halogen atoms. For example, a halogenated alkenyl group can be either a full halogenated alkenyl group or a partial halogenated alkenyl group.
[0057] In this application, in formula (I) above, R2 is independently selected from one of the following: halogen atom, substituted or unsubstituted alkyl group, substituted or unsubstituted cycloalkyl group, substituted or unsubstituted alkenyl group, substituted or unsubstituted alkynyl group, and substituted or unsubstituted aryl group. As a substituent on the cyclic structure of the substance of formula (I) above, different types of R2 can enrich the variety of substances of formula (I) and slightly differ some properties.
[0058] In some embodiments of this application, the number of carbon atoms in the substituted or unsubstituted alkyl group can be 1-10, specifically 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10. The number of carbon atoms in the substituted or unsubstituted cycloalkyl group can be 3-10, specifically 3, 4, 5, 6, 7, 8, 9, or 10. The number of carbon atoms in the substituted or unsubstituted alkenyl group or the substituted or unsubstituted alkynyl group can independently be in the range of 2-10, specifically 2, 3, 4, 5, 6, 7, 8, 9, or 10. The number of carbon atoms in the substituted or unsubstituted aryl group can be in the range of 6-30, specifically 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30. The fact that each of the above groups has a suitable number of carbon atoms is beneficial to ensuring that substances of formula (Ⅰ) selected from these groups are more readily available, have higher solubility in the organic solvent of the electrolyte, and ensure that the viscosity of the electrolyte is within a suitable range.
[0059] Furthermore, the substituents in the aforementioned substituted alkyl, substituted cycloalkyl, substituted alkenyl, substituted alkynyl, and substituted aryl groups may include one or more of the following: halogen atom, halogenated or unsubstituted alkyl, halogenated or unsubstituted cycloalkyl, halogenated or unsubstituted alkoxy, halogenated or unsubstituted alkenyl, halogenated or unsubstituted alkenyloxy, halogenated or unsubstituted alkynyl, and halogenated or unsubstituted alkynoxy. Introducing various different substituents onto substituent R2 can enrich the variety of additives in formula (I) and obtain products with slightly different properties. In some embodiments, the substituted alkyl group in R2 is a halogenated C1-C... 10 Alkyl group. The substituted alkenyl group is a halogenated C2-C group. 10 Alkenyl group. The substituted alkynyl group is a halogenated C2-C group. 10 Alkyne group. The substituents in the substituted aryl group include at least one of halogen atoms, alkyl groups, and haloalkyl groups.
[0060] In some embodiments of this application, R2 is independently selected each time it appears from a halogen atom, a halogenated or unsubstituted C1-C atom. 10 One of the alkyl groups. The haloalkyl group may be a partially haloalkyl group or a fully haloalkyl group. The halogen atom in the haloalkyl group may be one or more of fluorine, chlorine, bromine, and iodine, for example, fluorine. Exemplarily, the halogenated or unsubstituted C1-C... 10 Alkyl groups can be fluorinated or unsubstituted C1-C6 alkyl groups, such as methyl, fluoromethyl, ethyl, fluoroethyl, etc.
[0061] In some other embodiments of this application, m = 0 in formula (I) above. That is, there is no substituent R2 in formula (I). In this case, formula (I) can be simplified to the following structure:
[0062]
[0063] In some embodiments of this application, in formula (Ⅰ), m = 0, n = 1 or 2, and R1 is vinyl, propenyl, ethynyl, or propynyl.
[0064] For example, the substance represented by formula (I) above may include one or more of the substances with the structural formulas shown in formulas (I1) to (I15) below.
[0065]
[0066] In the embodiments of this application, the substance represented by formula (I) above can be commercially available or synthesized by the applicant. This application does not limit the method of synthesizing the substance of formula (I).
[0067] It is understood that in this application, the electrolyte additive may include a substance represented by formula (I) as an additive, or it may include a variety of substances with different structures conforming to the general formula (I) as additives. Similarly, the electrolyte additive may include one or more nitrile substances.
[0068] In this application, nitrile substances refer to substances whose molecular structure contains at least one cyano (-CN) group. In some embodiments of this application, the nitrile substances include compounds whose molecular structure contains 2-3 cyano groups. In this case, the nitrile substances have a better stabilizing effect on the battery positive electrode and can form a more stable complex protective layer on the battery positive electrode.
[0069] For example, the nitrile substances may include at least one of butadiene nitrile (SN), glutaronitrile (ADN), adiponitrile (ADN), 1,4-dicyano-2-butene (DCB), 1,3,5-pentanetricarbonitrile (PTCN), 1,3,6-hexanetrionitrile (HTCN), 1,2-bis(2-cyanoethoxy)ethane (DENE, also known as ethylene glycol bis(propionitrile) ether), and 1,2,3-tris(2-cyanoethoxy)propane (TCP), but are not limited thereto.
[0070] The structural formula of SN is CN-CH2-CH2-CN, and its molecular weight is 80. The structural formula of ADN is CN-CH2-CH2-CH2-CN, and its molecular weight is 94. The structural formula of ADN is CN-CH2-CH2-CH2-CH2-CN, and its molecular weight is 108. The structural formula of DCB is CN-CH2-CH=CH-CH2-CN, and its molecular weight is 106.
[0071] The structural formulas of PTCN, HTCN, DENE, and TCP are shown below. The molecular weight of PTCN is 147. The molecular weight of HTCN is 161. The molecular weight of DENE is 168. The molecular weight of TCP is 251.
[0072] PTCN: HTCN:
[0073] DENE: TCP:
[0074] In some embodiments of this application, the electrolyte additives may further include additives other than nitriles and substances shown in formula (I). This will be described in detail in the electrolyte section below.
[0075] This application also provides an electrolyte comprising an electrolyte salt, an organic solvent, and the electrolyte additives described in this application.
[0076] To address the issue of battery thickness expansion caused by side reactions at the positive and negative electrode interfaces in secondary batteries, and the ineffective suppression of electrolyte gas generation on the positive electrode side by commonly used nitrile additives due to side reactions at the negative electrode, the electrolyte provided in this application uses both the substance shown in formula (I) and nitrile substances as electrolyte additives. When the two meet a specific mass ratio, the substance shown in formula (I) can preferentially adsorb onto the negative electrode of the battery, suppressing the adsorption of nitrile substances at the negative electrode and the resulting side reactions. As a result, nitrile substances can better exert their adsorption effect at the positive electrode, suppressing the catalytic oxidation of the electrolyte by the high-voltage positive electrode. Simultaneously, the nitrogen- and sulfur-containing organic interface film generated by the reduction of the substance shown in formula (I) at the negative electrode can improve the stability of the negative electrode interface and suppress the volume expansion caused by negative electrode side reactions. Therefore, this electrolyte effectively suppresses battery thickness expansion on both the negative and positive electrode sides, inhibiting hard expansion on the negative electrode side and electrolyte gas generation expansion on the positive electrode side.
[0077] In some embodiments of this application, the mass percentage of the substance shown in formula (I) in the electrolyte can be 0.04%-0.65%. Here, the mass percentage refers to the sum of the mass percentages of all substances conforming to the general structural formula (I). When both the substance shown in formula (I) and nitrile substances are used in the electrolyte at appropriate mass ratios, controlling the mass percentage of the substance shown in formula (I) in the electrolyte within a suitable range ensures that it is sufficient to suppress the adsorption and decomposition consumption of nitrile substances at the negative electrode, without increasing the negative electrode interface impedance due to excessive decomposition of the substance in formula (I) at the negative electrode, thus affecting the rate performance of the battery, and ensuring a good synergistic effect between the substance in formula (I) and the nitrile substances.
[0078] For example, the mass percentage of the substance shown in formula (I) in the electrolyte can be 0.05%, 0.06%, 0.08%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.58%, etc. In some possible embodiments of this application, the mass percentage of the substance shown in formula (I) in the electrolyte is 0.05%-0.5%. In this case, the synergistic effect of the substance in formula (I) and the nitrile substance is better, and the reduction in thickness expansion of the secondary battery using the above electrolyte is more significant.
[0079] In some embodiments of this application, the mass percentage of the aforementioned nitrile material in the electrolyte can be 2.5%-6.5%. When both the substance shown in formula (I) and the nitrile material are used in the electrolyte at an appropriate mass ratio, the mass percentage of the nitrile material itself in the electrolyte is controlled within a suitable range, which is sufficient to stabilize the positive electrode, form a complex protective layer of appropriate thickness on the surface of the positive electrode, and prevent the CEI film on the positive electrode side from becoming too thick, thereby increasing the positive electrode interface impedance and affecting the rate performance of the battery, and ensuring a good synergistic effect between the substance of formula (I) and the nitrile material.
[0080] For example, the mass percentage of nitrile substances in the electrolyte can be specifically 2.6%, 2.8%, 3.0%, 3.2%, 3.5%, 3.8%, 4.0%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.5%, 5.8%, 6.0%, 6.2%, etc. In some possible embodiments of this application, the mass percentage of nitrile substances in the electrolyte can be 3%-6%. In this case, the synergistic effect of the substance of formula (I) and the nitrile substances is better, and the reduction in thickness expansion of the secondary battery using the above electrolyte is more significant.
[0081] It is understood that the mass percentage of nitrile substances or substances shown in formula (Ⅰ) in the electrolyte and the mass ratio of the two mentioned in the embodiments of this application may have a certain measurement system error during actual testing operations. The values within the system error range can be understood as the range defined by the embodiments of this application.
[0082] In some embodiments of this application, the electrolyte further includes fluoroethylene carbonate (FEC). FEC can form a passivation interface film on the negative electrode surface during battery formation, suppressing continuous side reactions of the electrolyte at the negative electrode, and also helping to suppress the adsorption and reduction consumption of nitriles at the negative electrode. In some possible embodiments, the mass percentage of FEC in the electrolyte can be 5%-50%, specifically 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, or 50%. This is beneficial for effective FEC film formation and also helps ensure that the negative electrode interface film formed by FEC has a suitable thickness, preventing excessive negative electrode interface impedance.
[0083] In some embodiments of this application, the mass ratio of the substance shown in formula (I) to FEC is 0.001-0.065. This ensures that the film-forming effect of FEC during battery formation is not excessively suppressed, thus affecting the cycle stability of the negative electrode, while also preventing excessive increase in battery impedance. Furthermore, it effectively leverages the effect of the substance shown in formula (I) in improving the stability of the negative electrode side of the battery, ensuring that the battery thickness does not expand excessively.
[0084] For example, the mass ratio of the substance shown in formula (I) to FEC can be 0.002, 0.005, 0.01, 0.015, 0.02, 0.025, 0.03, 0.035, 0.04, 0.045, 0.05, 0.055, 0.06, or 0.062, etc. In some embodiments, the mass ratio can be any value between 0.001 and 0.02, any value between 0.01 and 0.03, a value between 0.02 and 0.035, or a value between 0.035 and 0.065, etc.
[0085] In some embodiments of this application, the mass ratio of nitrile material to FEC can be 0.0625-0.65. In this case, the film-forming effect of FEC during battery formation will not be excessively suppressed, thus affecting the cycle stability of the negative electrode. At the same time, the battery impedance will not increase excessively due to excessive FEC content. Furthermore, the nitrile material can effectively improve the stability of the positive electrode side of the battery and suppress the thickness expansion of the battery caused by electrolyte gas generation.
[0086] For example, the mass ratio of nitrile to FEC can be 0.07, 0.08, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, etc. In some embodiments, this mass ratio can be any value between 0.0625 and 0.2, any value between 0.1 and 0.3, any value between 0.3 and 0.5, or any value between 0.45 and 0.65, etc.
[0087] In some embodiments of this application, the electrolyte further includes thioesters. Thioesters may refer to substances whose molecular structure contains at least one -OS (=O). 1~2 -or -OS (=O) 1~2 Linear or cyclic substances with -O- groups. Thioesters are generally used as negative electrode film-forming additives to help improve battery cycle performance.
[0088] For example, the thioesters may include one or more of the following: 1,3-propanesulfonate lactone (PS), 1,4-butanesulfonate lactone (BS), 1,3-propenesulfonate lactone (PST), methanedisulfonate methylene ester (MMDS), vinyl sulfate (DTD), vinyl sulfite (ES), 4-methyl ethylene sulfate, dimethyl sulfite, diethyl sulfite, dimethyl sulfate, and diethyl sulfate.
[0089] In some possible implementations, the mass percentage of the aforementioned thioesters in the electrolyte can be 1%-5%, for example, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.
[0090] In some embodiments of this application, the electrolyte simultaneously includes the substance shown in formula (I), nitrile substances, FEC, and thioester substances. In other embodiments of this application, in addition to adding the substance shown in formula (I), nitrile substances, FEC, thioester substances, etc., as electrolyte additive components, other additives may be added according to different performance requirements of the electrolyte. Other additives may include one or more of other film-forming additives, overcharge prevention additives, wetting agents, flame retardants, etc.
[0091] Exemplary examples include other film-forming additives such as VEC analogs, such as trifluoromethyl ethylene carbonate (TFEC), vinylene carbonate (VC), and ethylene ethylene carbonate (VEC). Exemplary overcharge protection additives may include biphenyl (BP), etc. Biphenyl also has the function of improving the high-voltage performance of the battery. Wetting agents can improve the wettability of the electrolyte to the electrodes; exemplary wetting agents may include fluorobenzene, etc. Exemplary flame retardants may include one or more of the following: phosphate esters (such as trimethyl phosphate, triethyl phosphate, tri(trimethylsilyl) phosphate), phosphites (such as trimethyl phosphite, triethyl phosphite), and cyclotriphosphazenes (such as (ethoxy)pentafluorocyclotriphosphazene, hexafluorocyclotriphosphazene).
[0092] In some embodiments of this application, the other additives mentioned above may include one or more of biphenyl, fluorobenzene, vinylene carbonate (VC), ethylene ethylene carbonate (VEC), and flame retardants, but are not limited thereto. Biphenyl can help prevent battery overcharging. Fluorobenzene can help improve the wettability of the electrolyte to the positive and negative electrodes. TFEC, VC, and VEC can form a film on the surface of the battery negative electrode.
[0093] In some embodiments of this application, the organic solvent in the electrolyte may include one or more of carbonate solvents, carboxylic acid ester solvents, and ether solvents. When there are multiple organic solvents, they can be mixed in any proportion. The carbonate solvents may include linear carbonate solvents and / or cyclic carbonate solvents.
[0094] For example, linear carbonate solvents may include, but are not limited to, one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), bis(2,2,2-trifluoroethyl) carbonate, and (2,2,2-trifluoroethyl)methyl carbonate. Cyclic carbonate solvents may include, but are not limited to, one or more of ethylene carbonate (EC) and propylene carbonate (PC). Carboxylic acid ester solvents may include, but are not limited to, one or more of methyl formate, ethyl formate, ethyl acetate, propyl acetate, ethyl propionate, propyl propionate, methyl difluoroacetate, and methyl trifluoroacetate. Ether solvents may include, but are not limited to, one or more of tetrahydrofuran (THF), 2-methyltetrahydrofuran, 1,3-dioxolane, dimethoxymethane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and bis(2,2,2-trifluoroethyl) ether.
[0095] In some embodiments of this application, the organic solvent includes cyclic carbonate solvents and linear carbonate solvents. Cyclic carbonate solvents generally have a high dielectric constant, and using them as an organic solvent component helps to improve the ionic conductivity of the electrolyte. The introduction of linear carbonate solvents helps to reduce the viscosity of the electrolyte, and they have high compatibility with cyclic carbonate solvents.
[0096] In this embodiment of the application, depending on the different systems of the secondary battery, the electrolyte salt in the electrolyte can be lithium salt, sodium salt, potassium salt, magnesium salt, zinc salt, or aluminum salt, etc. For example, lithium salt, sodium salt, and potassium salt may include MClO4, MBF4, MPF6, MAsF6, MPF2O2, MCF3SO3, MTDI (TDI), etc. - It is 4,5-dicyano-2-trifluoromethylimidazolium), MB(C2O4)2 (abbreviated as MBOB), MBF2C2O4 (abbreviated as MDFOB), M[(CF3SO2)2N] (abbreviated as MTFSI), M[(FSO2)2N] (abbreviated as MFSI) and M[(C x F 2x+1 SO2)(C y F 2y+1 Lithium salts can be one or more of the following: [(C(SO2)N], where M is Li, Na, or K, and x and y are natural numbers. For example, lithium salts can be, but are not limited to, LiClO4, LiBF4, LiPF6, LiAsF6, LiPF2O2, LiCF3SO3, LiTDI, LiB(C2O4)2, LiBF2C2O4, Li[(CF3SO2)2N], Li[(FSO2)2N], and Li[(C(C(SO2)N))N]. x F 2x+1 SO2)(C y F 2y+1 One or more of [SO2)N]. Similarly, magnesium salts, zinc salts, and aluminum salts can also be salts formed by magnesium ions, zinc ions, and aluminum ions with anions from the lithium salts, sodium salts, and potassium salts mentioned above.
[0097] This application does not impose special requirements on the content of electrolyte salts in the electrolyte, which can be adjusted according to actual needs. In the embodiments of this application, the molar concentration of electrolyte salts in the electrolyte can be 0.01 mol / L-2 mol / L, specifically 0.01 mol / L, 0.02 mol / L, 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, etc.
[0098] The content, concentration, and ratio of each substance mentioned above in this application refer to their values in the battery electrolyte before formation, or they can refer to their values in the battery electrolyte after formation. It is understood that after actual battery formation, capacity testing, or cycling, the formation of the electrolyte interface film will have a certain impact on the testing of parameters such as the content, concentration, and ratio of each substance in the electrolyte. A certain degree of measurement error is permissible. Values within the error range can be understood as being within the range defined in the embodiments of this application. Alternatively, if the values of the aforementioned parameters measured after actual battery formation, capacity testing, or cycling are still within the aforementioned range, they can be understood as being within the range defined in the embodiments of this application.
[0099] This application does not limit the preparation method of the electrolyte described above; generally, it involves mixing the components constituting the electrolyte. Exemplarily, in some embodiments, the preparation method of the electrolyte may include: in an inert or sealed environment (such as a glove box filled with argon), adding a thoroughly dried electrolyte salt and the electrolyte additive described in this application embodiment to an organic solvent, stirring and mixing thoroughly to obtain the electrolyte of this application embodiment. The electrolyte salt and the electrolyte additive may be added to the organic solvent simultaneously; or the electrolyte additive may be added to the organic solvent first, followed by the electrolyte salt; or the electrolyte salt may be added first, followed by the electrolyte additive. Furthermore, the components included in the electrolyte additive may be mixed before being added, or they may be added separately to the organic solvent.
[0100] Each operation in the above preparation method can be implemented according to the existing conventional battery electrolyte preparation process. The specific selection of raw materials such as electrolyte salts, organic solvents, and battery electrolyte additives is as described above and will not be repeated here.
[0101] This application also provides a secondary battery 100, the structural schematic diagram of which is shown below. Figure 1 As shown, the secondary battery 100 includes a positive electrode 10, a negative electrode 20, a separator 30, and an electrolyte 40, wherein the electrolyte 40 includes the electrolyte described in the embodiments of this application. The specific structure of the secondary battery is as described above in this application and will not be repeated here.
[0102] The secondary battery 100 provided in this application embodiment uses an electrolyte containing specific additives, which enables the secondary battery to achieve good high and low temperature cycle capacity stability. It can also achieve a low battery thickness expansion rate under operating conditions such as room temperature cycling, high temperature storage, and high temperature float charging. The battery has good stability and safety.
[0103] In this embodiment of the application, the secondary battery can be a lithium secondary battery, a sodium secondary battery, a potassium secondary battery, a magnesium secondary battery, a zinc secondary battery, or an aluminum secondary battery, etc. Figure 1(The secondary battery in this example is a lithium secondary battery). The secondary battery provided in this application can be used in consumer products, such as mobile phones, tablets, power banks, laptops, and other wearable or portable electronic devices; it can also be used in vehicles, energy storage devices, base stations, and other products to improve the long-term reliability and safety of the products.
[0104] The following is a detailed introduction to the positive electrode 10, negative electrode 20, separator 30, etc. of the secondary battery 100.
[0105] like Figure 1 As shown, the positive electrode 10 includes a positive electrode current collector 11 and a positive electrode material layer 12 disposed on the surface of the positive electrode current collector 11. The positive electrode material layer 12 includes a positive electrode active material 120. The positive electrode current collector 11 may include metal foil (e.g., aluminum foil, gold foil, platinum foil, etc.) or carbon-coated metal foil, etc.
[0106] The positive electrode active material 120 is a material capable of reversibly inserting and extracting active metal ions (in the case of lithium secondary batteries, these active metal ions are lithium ions). This application does not impose any special limitations on the selection of the positive electrode active material; any positive electrode active material conventionally used in existing secondary batteries can be used. In some embodiments of this application, the positive electrode active material 120 may include one or more of layered M-based transition metal oxides and polyanionic M-containing positive electrode materials; wherein M is Li, Na, K, Mg, Zn, or Al. Generally, layered M-based transition metal oxides have a higher charging cut-off voltage than polyanionic M-containing positive electrode materials and are commonly used in high-voltage battery systems. Taking a lithium secondary battery as an example, exemplary positive electrode active materials may be lithium iron phosphate (LiFePO4, abbreviated as LFP), lithium cobalt oxide (LiCoO2, abbreviated as LCO), or lithium nickel cobalt manganese oxide (NCM, chemical formula may be LiNi). a Co b Mn c One or more of O2, a+b+c=1). Among them, LCO and NCM belong to layered lithium-based transition metal oxides. LFP belongs to polyanionic cathode materials.
[0107] In addition to the positive electrode active material 120, the positive electrode material layer 12 may also include a certain amount of binder, conductive agent, and other components. Specifically, the binder for the positive electrode 10 may include, but is not limited to, one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), polyacrylate, polyacrylamide (PAM), polyacrylonitrile (PAN), and polyimide (PI). The conductive agent for the positive electrode 10 may include one or more of acetylene black, Ketjen black, Super P, amorphous carbon, carbon nanotubes, carbon fibers, and graphene. The above-mentioned binders and conductive agents are merely illustrative examples and are not specifically limited herein.
[0108] In this embodiment, the negative electrode 20 may include one or more of the following: carbon-based negative electrode, silicon-based negative electrode, tin-based negative electrode, phosphorus-based negative electrode, lithium titanate negative electrode, lithium negative electrode, sodium negative electrode, potassium negative electrode, magnesium negative electrode, zinc negative electrode, and aluminum negative electrode. The carbon-based negative electrode may include, but is not limited to, one or more of the following: graphite (e.g., artificial graphite, natural graphite), hard carbon, soft carbon, porous carbon, mesophase carbon microspheres, and graphene. The silicon-based negative electrode may include, but is not limited to, one or more of the following: elemental silicon, silicon-carbon materials, silicon oxides, and silicon metal compounds. The tin-based negative electrode may include, but is not limited to, one or more of the following: elemental tin, tin-carbon materials, tin oxides, and tin metal compounds. The phosphorus-based negative electrode may include, but is not limited to, one or more of the following: red phosphorus, black phosphorus, and phosphorus-containing compounds. The lithium titanate negative electrode includes lithium titanate materials, and an exemplary chemical formula may be Li4Ti5O. 12 The lithium, sodium, potassium, magnesium, zinc, and aluminum anodes can each comprise elemental lithium, sodium, potassium, magnesium, zinc, or aluminum, or alloys thereof, or can be the aforementioned metals or alloys thereof with a current collector. Specifically, the lithium anode may comprise elemental lithium or lithium alloys (e.g., at least one of lithium-silicon alloys, lithium-sodium alloys, lithium-potassium alloys, lithium-aluminum alloys, lithium-tin alloys, lithium-indium alloys, etc.). The sodium anode may comprise elemental sodium or sodium alloys. The potassium anode may comprise elemental potassium or potassium alloys. The magnesium anode may comprise elemental magnesium or magnesium alloys. The zinc anode may comprise elemental zinc or zinc alloys. The aluminum anode may comprise elemental aluminum or aluminum alloys. It is understood that the lithium, sodium, potassium, magnesium, zinc, and aluminum anodes are respectively used in lithium secondary batteries, sodium secondary batteries, potassium secondary batteries, magnesium secondary batteries, zinc secondary batteries, or aluminum secondary batteries.
[0109] In some embodiments of this application, such as Figure 1 As shown, the negative electrode 20 includes a negative electrode current collector 21 and a negative electrode material layer 22 disposed on the surface of the negative electrode current collector 21. The negative electrode material layer 22 includes a negative electrode active material 220. The negative electrode current collector 21 may include metal foil (e.g., copper foil, aluminum foil, gold foil, platinum foil, etc.), carbon-coated metal foil, etc. For example, in a lithium secondary battery, the positive electrode current collector 11 may be aluminum foil, and the negative electrode current collector 21 may be copper foil. In a sodium secondary battery, both the positive electrode current collector 11 and the negative electrode current collector 21 may be aluminum foil.
[0110] The negative electrode active material 220 is a material capable of reversibly accepting and releasing metal ions (such as lithium ions, sodium ions, potassium ions, magnesium ions, zinc ions, aluminum ions, etc.; for lithium secondary batteries, the metal ion is lithium ions). In this application, the negative electrode active material 220 may include the aforementioned carbon-based negative electrode materials, silicon-based negative electrode materials, tin-based negative electrode materials, phosphorus-based negative electrode materials, and lithium titanate (Li4Ti5O4). 12The negative electrode material can be one or more of elemental lithium or its alloy, elemental sodium or its alloy, elemental potassium or its alloy, elemental magnesium or its alloy, elemental zinc or its alloy, elemental aluminum or its alloy, etc. In some embodiments of this application, the negative electrode active material 220 for a lithium secondary battery may include lithium titanate (Li4Ti5O4). 12 ( ), carbon-based anode materials, silicon-based anode materials, tin-based anode materials, phosphorus-based anode materials, elemental lithium or its alloys, at least one of the following:
[0111] In some embodiments, the negative electrode material layer 22 may include, in addition to the negative electrode active material 220, a certain amount of binder, conductive agent, and other components. For example, the binder for the negative electrode 20 may include, but is not limited to, one or more of carboxymethyl cellulose (CMC), sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), lithium polyacrylate (LiPAA), sodium polyacrylate, sodium alginate, etc. The conductive agent for the negative electrode 20 may include, but is not limited to, one or more of acetylene black, Ketjen black, Super P, amorphous carbon, carbon nanotubes, carbon fibers, graphene, etc. The above-mentioned binders and conductive agents are merely illustrative examples and are not specifically limited herein.
[0112] In some other embodiments of this application, the negative electrode 20 is a metal negative electrode that does not include a current collector. For example, the negative electrode 20 is the aforementioned lithium negative electrode, sodium negative electrode, potassium negative electrode, magnesium negative electrode, zinc negative electrode, or aluminum negative electrode that does not have a current collector.
[0113] In the secondary battery 100, the separator 30 can block the passage of electrons while allowing the passage of ions. The separator 30 can be any separator material in existing secondary batteries. Exemplarily, the separator 30 can be, but is not limited to, single-layer PP (polypropylene), single-layer PE (polyethylene), double-layer PP / PE, double-layer PP / PP, triple-layer PP / PE / PP, ceramic-coated PE, solid electrolyte-coated PE, non-woven fabric, etc.
[0114] This application does not impose any particular restrictions on the shape of the secondary battery 100, which can be cylindrical, button-shaped (coin-shaped), flat, square, or other irregular shapes.
[0115] The specific shape or type of the secondary battery 100 in this application embodiment is not limited, and it can be a square battery, button battery, cylindrical battery, pouch battery, etc.; it can be a wound battery or a stacked battery. The secondary battery can be in rigid packaging, such as a hard plastic shell, aluminum shell, steel shell, etc., or in flexible packaging, such as a pouch-type flexible packaging. The material of the flexible packaging can be plastic, such as polypropylene (PP), polybutylene terephthalate (PBT), etc.
[0116] The secondary battery provided in this application embodiment can be used in terminal devices, such as consumer electronic products, such as mobile phones, tablets, power banks, laptops, and other wearable or mobile electronic devices, as well as vehicles, energy storage devices, base stations, and other equipment products.
[0117] This application also provides an electrical device that includes the secondary battery described in this application. The device is powered by the aforementioned sodium-ion battery.
[0118] Figure 2 This is a schematic diagram of the structure of an electrical device provided in an embodiment of this application. Figure 2 As shown, the electrical equipment 200 includes a housing 201 and a battery 202 and electronic components housed within the housing 201. Figure 2 (Not shown in the image). Battery 202 includes the secondary battery 100 provided in the embodiments of this application. Battery 202 can supply power to electronic components, thereby supplying power to electrical device 200. Electronic components are electrical components within electrical device 200, such as circuit boards.
[0119] The electrical device 200 can be any device that can use electricity, including consumer electronics such as mobile phones, tablets, laptops, portable computers, power banks, wearable devices (such as glasses, watches, wristbands, headphones, etc.), augmented reality (AR) devices, virtual reality (VR) devices, etc.; it can also be mobile devices such as drones, vehicles (such as electric cars, electric bicycles, electric buses, electric trucks, electric trains, etc.), ships, aerospace equipment, etc., or even base stations. In some embodiments, the housing 201 may include a front cover assembled on the front side of the electrical device and a rear housing assembled on the rear side, with the battery 202 fixed inside the rear housing. Figure 2 The electrical device 200 shown may be, for example, a mobile phone.
[0120] Because the electrolyte used in the secondary battery 100 can simultaneously improve the problems of hard expansion and gas expansion on the positive and negative electrode sides of the battery, the secondary battery is less likely to cause excessive expansion or deformation of the casing of the electrical device 200 that houses it. The electrical device 200 has high reliability, stable performance, and strong product competitiveness.
[0121] This application also provides an energy storage device, including a receiving cavity and a battery housed in the receiving cavity, wherein the battery stores electrical energy for the energy storage device. The energy storage device generally includes multiple of the aforementioned secondary batteries 100.
[0122] See Figure 3 , Figure 3This is a schematic diagram of a structure of an energy storage device 300 provided in an embodiment of this application. The energy storage device 300 includes a receiving cavity 31 and a battery pack 32. The battery pack 32 is housed within the receiving cavity 31. The battery pack 32 can be a module formed by connecting multiple secondary batteries 320 in series, parallel, or a combination thereof. Any two secondary batteries 320 are connected in series or parallel. At least some of the multiple secondary batteries 320 include the secondary battery 100 described in the embodiments of this application. In one embodiment, Figure 3 The energy storage device shown may be, for example, a battery pack. The battery pack may include one or more battery cells 32.
[0123] In some embodiments, the energy storage device 300 may further include a battery management system (BMS) 33, which may be electrically connected to the battery pack 32. The BMS 33 may be used to monitor the status information of each secondary battery 320 in the battery pack 32, such as temperature, voltage, current, internal resistance, etc., and to control the charging / discharging status of each secondary battery 100.
[0124] This application also provides an energy storage system, which includes a power converter electrically connected to the energy storage device described in this application. The number of energy storage devices or power converters can be one or more. The power converter is used to convert the voltage and / or current output from the energy storage device and output it to the power grid or electrical load, and / or to convert the voltage and / or current output from an external power source and input it to the energy storage device.
[0125] The embodiments of this application will be further described below with reference to several examples. Unless otherwise specified, all materials used in the following embodiments are commercially available products.
[0126] Example 1
[0127] The preparation of an electrolyte for a lithium secondary battery includes: mixing propylene carbonate (PC), diethyl carbonate (DEC), and propyl propionate (PP) in a mass ratio of 20:22.5:30 in an argon-filled glove box to form an organic solvent; then sequentially adding fluoroethylene carbonate (FEC) and fully dried lithium hexafluorophosphate (LiPF6) to the organic solvent and stirring until homogeneous to obtain a solution; then adding the additive shown in formula (I1), a nitrile substance (specifically additive B1: glutaronitrile), and 1,3-propanesulfonic acid lactone (PS) to the solution and stirring until homogeneous to obtain the desired electrolyte. The molar concentration of LiPF6 in the electrolyte is 1 mol / L, and the mass percentages of FEC, the additive of formula (I1), glutaronitrile, and PS are 15%, 0.5%, 5%, and 3%, respectively.
[0128] I1: B1:
[0129] The preparation of a lithium secondary battery includes:
[0130] 1) The binder polyvinylidene fluoride (PVDF), the conductive agent super P, and the positive electrode active material lithium cobalt oxide (LiCoO2) are mixed in the solvent N-methylpyrrolidone (NMP) at a mass ratio of 2:2:96 and stirred until uniform to obtain a positive electrode slurry; the positive electrode slurry is coated on an aluminum foil current collector, dried, cold-pressed, and slit to obtain a positive electrode sheet;
[0131] 2) The binder carboxymethyl cellulose (CMC), the binder styrene-butadiene rubber (SBR), the conductive agent Super P, and the negative electrode active material (a mixture of silicon carbon material and graphite material in equal mass ratio) are mixed in deionized water at a mass ratio of 1.5:2.5:1:95 and stirred thoroughly to obtain a negative electrode slurry. The negative electrode slurry is coated on a copper foil current collector, dried, cold-pressed, and slit to obtain a negative electrode sheet.
[0132] 3) The positive electrode sheet, commercial PE separator, and negative electrode sheet prepared above are stacked in sequence to form a battery cell; the battery cell is packaged with polymer, filled with the lithium secondary battery electrolyte prepared in Example 1 of this application, and after formation and other processes, a soft-pack lithium secondary battery with a rated capacity of 4Ah is obtained.
[0133] Example 2
[0134] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.05%, 5% and 3%, respectively.
[0135] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 2 was used to prepare a soft-pack lithium secondary battery.
[0136] Example 3
[0137] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.2%, 4% and 3%, respectively.
[0138] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 3 was used to prepare a soft-pack lithium secondary battery.
[0139] Example 4
[0140] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.2%, 6% and 3%, respectively.
[0141] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 4 was used to prepare a soft-pack lithium secondary battery.
[0142] Example 5
[0143] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.05%, 3% and 3%, respectively.
[0144] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 5 was used to prepare a soft-pack lithium secondary battery.
[0145] Example 6
[0146] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.1%, 6% and 3%, respectively.
[0147] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 6 was used to prepare a soft-pack lithium secondary battery.
[0148] Example 7
[0149] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.04%, 2.5% and 3%, respectively.
[0150] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 7 was used to prepare a soft-pack lithium secondary battery.
[0151] Example 8
[0152] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.65%, 6.5% and 3%, respectively.
[0153] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 8 was used to prepare a soft-pack lithium secondary battery.
[0154] Example 9
[0155] A lithium secondary battery electrolyte, the preparation method of which differs from that of Example 1, is that the nitrile substances in the electrolyte simultaneously employ additives B1-glutaronitrile and B3-1,2-bis(2-cyanoethoxy)ethane (DENE). In the electrolyte of Example 9, the mass percentages of FEC, additive of formula (I1), glutaronitrile, DENE, and PS are 15%, 0.2%, 4%, 1%, and 3%, respectively.
[0156] I1: B1: B3:
[0157] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 9 was used to prepare a soft-pack lithium secondary battery.
[0158] Example 10
[0159] The preparation of a lithium secondary battery electrolyte includes: mixing PC, DEC, and PP in a mass ratio of 20:22.5:30 in an argon-filled glove box to form an organic solvent; then adding FEC and fully dried lithium hexafluorophosphate (LiPF6) to the organic solvent and stirring until homogeneous to obtain a solution; then adding the additive shown in formula (I1), nitrile substances (specifically additive B2-1,3,6-hexanetrionitrile (HTCN) and additive B4-butadionitrile), and 1,3-propanesulfonic acid lactone (PS) to the solution and stirring until homogeneous to obtain the desired electrolyte. The molar concentration of LiPF6 in the electrolyte is 1 mol / L, and the mass percentages of FEC, the additive of formula (I1), HTCN, butadionitrile, and PS in the electrolyte are 15%, 0.2%, 2%, 2%, and 3%, respectively.
[0160] I1: B2: B4:
[0161] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 10 was used to prepare a soft-pack lithium secondary battery.
[0162] Example 11
[0163] The preparation of a lithium secondary battery electrolyte includes: mixing PC, DEC, and PP in a mass ratio of 20:22.5:30 in an argon-filled glove box to form an organic solvent; then adding FEC and fully dried lithium hexafluorophosphate (LiPF6) to the organic solvent and stirring until homogeneous to obtain a solution; then adding the additive shown in formula (I3), a nitrile substance (specifically additive B4-butadionitrile), and 1,3-propanesulfonic acid lactone (PS) to the solution and stirring until homogeneous to obtain the desired electrolyte. The molar concentration of LiPF6 in the electrolyte is 1 mol / L, and the mass percentages of FEC, the additive of formula (I3), butadionitrile, and PS are 15%, 0.65%, 6.5%, and 3%, respectively.
[0164] I3: B4:
[0165] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 11 was used to prepare a soft-pack lithium secondary battery.
[0166] Example 12
[0167] A lithium secondary battery electrolyte differs from Example 1 in that: PC, DEC, and PP are mixed in a mass ratio of 5:12.5:15; and the mass percentages of FEC, additive of formula (I1), glutaronitrile, and PS in the electrolyte are 55%, 0.05%, 3%, and 3%, respectively.
[0168] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 12 was used to prepare a soft-pack lithium secondary battery.
[0169] Example 13
[0170] A lithium secondary battery electrolyte differs from that of Example 1 in that: PC, DEC, and PP are mixed in a mass ratio of 30:22.5:30; and the mass percentages of FEC, additive of formula (I1), glutaronitrile, and PS in the electrolyte are 5%, 0.5%, 5%, and 3%, respectively.
[0171] Following the method described in Example 1, the lithium secondary battery electrolyte of Example 13 was used to prepare a soft-pack lithium secondary battery.
[0172] To highlight the beneficial effects of the embodiments of this application, the following comparative examples are provided.
[0173] Comparative Example 1
[0174] The preparation of a lithium secondary battery electrolyte includes: mixing PC, DEC, and PP in an argon-filled glove box to form an organic solvent; then adding FEC and fully dried lithium hexafluorophosphate (LiPF6) to the organic solvent and stirring until homogeneous to obtain a solution; then adding the additive shown in formula (I1), a nitrile substance (specifically additive B5-1,2,3,4,5-penta(2-cyanoethoxy)pentane, with a molecular weight of 417), and 1,3-propanesulfonic acid lactone (PS) to the solution and stirring until homogeneous to obtain the desired electrolyte. The mass percentage of LiPF6 in the electrolyte is 12.5%, the mass percentages of PC, DEC, and PP are 20%, 22.5%, and 30%, respectively, and the mass percentages of FEC, the additive of formula (I1), TCP, and PS are 15%, 0.2%, 5%, and 3%, respectively.
[0175] Following the method described in Example 1, the lithium secondary battery electrolyte of Comparative Example 1 was used to prepare a soft-pack lithium secondary battery.
[0176] Comparative Example 2
[0177] A lithium secondary battery electrolyte differs from that of Example 1 mainly in that the electrolyte does not contain nitriles or the substances shown in the aforementioned formula (I).
[0178] Following the method described in Example 1, the lithium secondary battery electrolyte of Comparative Example 2 was used to prepare a soft-pack lithium secondary battery.
[0179] Comparative Example 3
[0180] A lithium secondary battery electrolyte differs from that of Example 1 mainly in that it contains the substance shown in formula (I1) but does not contain nitrile substances. In the electrolyte of Comparative Example 3, the mass percentages of FEC, additive of formula (I1), and PS are 15%, 0.2%, and 3%, respectively.
[0181] Following the method described in Example 1, the lithium secondary battery electrolyte of Comparative Example 3 was used to prepare a soft-pack lithium secondary battery.
[0182] Comparative Example 4
[0183] A lithium secondary battery electrolyte differs from that of Example 1 mainly in that it contains additive B1—glutaronitrile, but does not contain any substance satisfying formula (I). In the electrolyte of Comparative Example 4, the mass percentages of FEC, glutaronitrile, and PS are 15%, 3%, and 3%, respectively.
[0184] Following the method described in Example 1, the lithium secondary battery electrolyte of Comparative Example 4 was used to prepare a soft-pack lithium secondary battery.
[0185] Comparative Example 5
[0186] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.5%, 3% and 3%, respectively.
[0187] Following the method described in Example 1, the lithium secondary battery electrolyte of Comparative Example 5 was used to prepare a soft-pack lithium secondary battery.
[0188] Comparative Example 6
[0189] A lithium secondary battery electrolyte is prepared in the same way as in Example 1, except that the mass percentages of FEC, additive of formula (I1), glutaronitrile and PS in the electrolyte are 15%, 0.05%, 6% and 3%, respectively.
[0190] Following the method described in Example 1, the lithium secondary battery electrolyte of Comparative Example 6 was used to prepare a pouch lithium secondary battery.
[0191] To strongly support the beneficial effects of the embodiments of this application, the soft-pack lithium secondary batteries of the above embodiments and comparative examples were subjected to the following performance tests.
[0192] 1) Room temperature cycling capacity retention test: Each lithium secondary battery was placed in a constant temperature oven at 25±3℃ and charged at a constant current of 3C to 4.2V, then charged at a constant current of 1C to 4.53V, and then charged at a constant voltage of 4.53V until the current dropped to 0.025C, and allowed to stand for 10 minutes; then discharged at a constant current of 1C to 3.0V, and this cycle was repeated 500 times. The discharge capacity of the first and nth cycles was recorded, and the percentage of the discharge capacity of the nth cycle to the discharge capacity of the first cycle was taken as the capacity retention rate after n cycles. The capacity retention rate results of room temperature cycling are summarized in Table 1 below. Figure 4 The room temperature cycle capacity curves of the lithium secondary batteries of Examples 2, 4, and 7 and Comparative Examples 1 and 4 of this application are also summarized.
[0193] 2) Room temperature cycling battery thickness expansion rate test: Each lithium secondary battery was placed in a constant temperature oven at 25±3℃ and charged at a constant current of 0.2C to 4.53V, then charged at a constant voltage of 4.53V until the current dropped to 0.025C, and allowed to stand for 5 minutes; then discharged at a constant current of 0.2C to 3.0V, allowed to stand for 5 minutes, and then charged at a current of 0.5C for 1 hour. The battery thickness was measured and recorded as the initial battery thickness. Subsequently, the battery was discharged at 0.2C to 3.0V and allowed to stand for 5 minutes. The battery was then charged at a constant current of 3C to 4.2V, then at a constant current of 1C to 4.53V, and then at a constant voltage of 4.53V until the current dropped to 0.025C. After resting for 10 minutes, it was discharged at a constant current of 1C to 3.0V. This cycle was repeated 500 times. Every 100 cycles, the full-charge thickness of the battery was measured, and the battery thickness expansion rate was calculated using the following formula: Thickness Expansion Rate = (Battery Full-Charge Thickness at Cycle n / Initial Battery Thickness - 1) × 100%. The relevant results are summarized in Table 1 below.
[0194] 3) Battery thickness expansion rate test after 18 hours of storage at 85℃: Under an ambient temperature of 25±3℃, each lithium secondary battery was charged at a constant current and constant voltage of 0.2C to 4.53V, then charged at a constant voltage until the current dropped to 0.025C, and left to stand for 5 minutes; then discharged at a constant current of 0.2C to 3.0V, and left to stand for 5 minutes; afterwards, the battery was charged at a constant current of 0.2C to 4.53V, then charged at a constant voltage until the current dropped to 0.025C, and the battery thickness at this point was measured and recorded as a1. The charged battery was left to stand at 85℃ for 18 hours, and then left to stand in an open circuit at room temperature for 2 hours, and the battery thickness was measured and recorded as a2. (a2 / a1-1)×100% was taken as the thickness expansion rate of the battery after 18 hours of storage at 85℃. The relevant results are summarized in Table 1 below.
[0195] 4) Battery thickness expansion rate test after 28 days of float charging at 45℃: Under an ambient temperature of 25±3℃, each lithium secondary battery was charged at a constant current and constant voltage of 0.2C to 4.53V, then charged at a constant voltage until the current dropped to 0.025C, and left to stand for 5 minutes; then discharged at a constant current of 0.2C to 3.0V, and left to stand for 5 minutes; then charged at a constant current of 0.5C for 1 hour, and the battery thickness was measured and recorded as b1. Subsequently, the battery was discharged at 0.5C to 3.0V. The discharged battery was transferred to a constant temperature chamber at 45±2℃, left to stand for 2 hours, and then charged at a constant current of 0.5C to 4.53V. This voltage was maintained at 4.53V for 28 days, and then transferred to an environment of 25±3℃ and left to stand for 2 hours. The battery thickness at this time was measured and recorded as b2. (b2 / b1-1)×100% is taken as the thickness expansion rate of the battery after 28 days of float charging at 4℃. The relevant results are summarized in Table 1 below.
[0196] Table 1
[0197]
[0198]
[0199] A comparison of Examples 1-8 and Comparative Examples 2-6 in Table 1 shows that when the electrolyte simultaneously uses additive of formula (I) of this application (hereinafter referred to as Additive I) and a nitrile additive with a molecular weight of less than 300, and the mass ratio of the two is within an appropriate range of 10-100, the thickness expansion of the battery under various operating conditions can be effectively suppressed. Specifically, the thickness expansion rate of the batteries in Examples 1-8 after storage at 85°C for 18 hours is below 17.12%, the thickness expansion rate after float charging at 45°C for 28 days is below 15.59%, and the thickness expansion rate after 200 cycles at room temperature is below 50.32%, while the battery's capacity retention rate at room temperature is above 82.89%. In contrast, Comparative Examples 2-4 did not simultaneously add nitrile additives and Class I additives to their battery electrolytes. Although Comparative Examples 5-6 added both nitrile additives and Class I additives to their battery electrolytes, the mass ratio of nitrile additives to Class I additives was not within the appropriate range of 10-100. Comparative Examples 2-6 exhibited higher 85°C storage thickness expansion rate (18.49-25.42%), higher 45°C float charge thickness expansion rate (16.33%-30.69%), higher room temperature cycling thickness expansion rate (51.11-55.61%), and poorer room temperature cycling capacity retention rate (80.29%-82.51%). This may be because when the two additives are used in an appropriate ratio, the adsorption of additive I at the negative electrode and the electrochemical reduction reaction inhibit the aggregation of nitrile additives at the negative electrode and the subsequent reduction side reaction, allowing the nitrile additives to play a better positive role on the positive electrode side, forming a complex protective layer on the positive electrode surface, suppressing the oxidation and gas generation side reaction of the electrolyte. Additive I also forms an organic oligomeric SEI film rich in sulfur and nitrogen elements at the negative electrode, which has good ion conduction, mechanical elasticity and high stability, thereby effectively suppressing the volume expansion of the battery negative electrode and improving cycle stability.
[0200] Furthermore, a comparison of Comparative Example 1 and Examples 1-8 of this application (e.g., Examples 3, 4, 9, 10) reveals that when the molecular weight of the nitrile additive is less than a certain value (e.g., less than 300), the nitrile additive and the additive of formula (I) must be used in combination in an appropriate ratio to achieve the effects claimed above in this application. This is because when the molecular weight of the nitrile additive is too high, it may surround additive I, causing additive I to fail to block the adsorption of nitrile substances on the negative electrode, thereby significantly reducing the electrochemical performance of the battery, especially the capacity retention rate and the suppression of thickness expansion during long-cycle operation at room temperature.
[0201] Specifically, in the electrolytes of the batteries of Examples 2, 4, and 7, the mass ratios of nitrile additives to additive I were 100, 30, and 62.5, respectively, falling within the suitable range of 10-100. Furthermore, the molecular weight of the nitrile additives was less than 300, while the molecular weight of nitrile additive B5 in Comparative Example 1 was greater than 300. In contrast, the electrolyte of Comparative Example 4 used only nitrile additives and not additive I. Therefore, the thickness expansion rates at 85°C storage, 45°C float charge, and room temperature cycling of the batteries of Examples 2, 4, and 7 were all lower than those of Comparative Examples 1 and 4. The long-cycle capacity retention rates at room temperature of the batteries of Examples 2, 4, and 7 were all higher than those of Comparative Examples 1 and 4 (see [link to relevant documentation]). Figure 4 (and Table 1).
[0202] Furthermore, a comparison between Examples 3-4 and 9-10 and Examples 1-2 and 5-6 reveals that when the mass ratio of nitrile additives to additive I is in the range of 20-30, it is more conducive to reducing the thickness expansion rate of the battery under 85°C storage, 45°C float charging, and room temperature cycling, and improving the room temperature cycling capacity retention rate.
[0203] Comparing the performance test results of the batteries in Examples 1-6 and Examples 7-8, it can be seen that when the mass ratio of nitrile additives to additive I is 10-100, the mass percentage of additive I in the electrolyte is in the range of 0.05%-0.5%, and the mass percentage of nitrile additives in the electrolyte is in the range of 3-6%, which is more conducive to reducing the thickness expansion rate of the battery under various operating conditions and improving the capacity retention rate during room temperature cycling.
[0204] Comparing Example 13 with Example 1 and Comparing Example 12 with Example 5, it can be seen that when the electrolyte contains FEC and appropriate mass ratios of nitrile additives and additive I, the mass ratio of additive I to FEC is in the range of 0.001-0.065, and the mass ratio of nitrile additives to FEC is in the range of 0.0625-0.65. The improvement effect of battery thickness expansion under various operating conditions is more obvious, and the capacity retention rate at room temperature is also higher.
[0205] The above description merely illustrates exemplary embodiments of this application, and while the description is specific and detailed, it should not be construed as limiting the scope of this patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
[0206] In this application, "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone, where A and B can be singular or plural. The character " / " generally indicates that the related objects before and after it are in an "or" relationship.
[0207] In the description of this application, unless otherwise stated, "multiple" means two or more. "At least one" means one or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0208] Furthermore, the numerical range indicated by "-" in this application refers to the range including the values before and after "-" as the minimum and maximum values, respectively. Expressions of parameter ranges in this application, such as "greater than or equal to (≥)", "less than or equal to (≤)", "above", and "below", all include the stated number. The numerical values and ranges involved in the embodiments of this application are approximate values and may have a certain range of errors due to the influence of manufacturing processes / testing methods, etc. These errors are negligible to those skilled in the art.
Claims
1. An electrolyte additive, characterized in that, The electrolyte additive includes the substance shown in formula (Ⅰ) and nitrile substances with a molecular weight of less than 300: In formula (Ⅰ), n is 0, 1 or 2, R1 is selected from alkenyl, haloalkenyl, alkynyl or haloalkynyl, m is an integer from 0 to 4, and R2 is selected independently each time from a halogen atom, substituted or unsubstituted alkyl, substituted or unsubstituted cycloalkyl, substituted or unsubstituted alkenyl, substituted or unsubstituted alkynyl or substituted or unsubstituted aryl. Furthermore, the mass ratio of the nitrile substance to the substance represented by formula (Ⅰ) is (10-100):
1.
2. The electrolyte additive as described in claim 1, characterized in that, The alkenyl, haloalkenyl, alkynyl, and haloalkynyl groups have 2-10 carbon atoms; the substituted or unsubstituted alkyl groups have 1-10 carbon atoms; the substituted or unsubstituted cycloalkyl groups have 3-10 carbon atoms; the substituted or unsubstituted alkenyl groups have 2-10 carbon atoms; and the substituted or unsubstituted aryl groups have 6-30 carbon atoms.
3. The electrolyte additive as described in claim 1 or 2, characterized in that, R1 is selected from one of C2-C5 alkenyl, halogenated C2-C5 alkenyl, C2-C5 ynyl, and halogenated C2-C5 ynyl.
4. The electrolyte additive according to any one of claims 1-3, characterized in that, The substance represented by formula (Ⅰ) includes one or more of the substances with structural formulas as shown in formulas (I1)-(I15):
5. The electrolyte additive according to any one of claims 1-4, characterized in that, The nitrile substances include compounds whose molecular structure contains 2-3 cyano groups.
6. The electrolyte additive as described in claim 5, characterized in that, The nitrile substances include at least one of succinic anion, glutaronitrile, adiponitrile, 1,4-dicyano-2-butene, 1,3,5-pentanetrionitrile, 1,3,6-hexanetrionitrile, 1,2-bis(2-cyanoethoxy)ethane, and 1,2,3-tris(2-cyanoethoxy)propane.
7. The electrolyte additive according to any one of claims 1-6, characterized in that, The mass ratio of the nitrile substance to the substance represented by formula (Ⅰ) is (20-30):
1.
8. An electrolyte, characterized in that, The electrolyte comprises an electrolyte salt, an organic solvent, and an electrolyte additive as described in any one of claims 1-7.
9. The electrolyte as described in claim 8, characterized in that, The mass percentage of the substance represented by formula (Ⅰ) in the electrolyte is 0.04%-0.65%, and / or the mass percentage of the nitrile substance in the electrolyte is 2.5%-6.5%.
10. The electrolyte as described in claim 9, characterized in that, The mass percentage of the substance represented by formula (Ⅰ) in the electrolyte is 0.05%-0.5%, and / or the mass percentage of the nitrile substance in the electrolyte is 3%-6%.
11. The electrolyte according to any one of claims 8-10, characterized in that, The electrolyte also includes fluoroethylene carbonate.
12. The electrolyte as described in claim 11, characterized in that, The fluoroethylene carbonate ester is present in the electrolyte at a mass percentage of 5%-50%.
13. The electrolyte as described in claim 11 or 12, characterized in that, The mass ratio of the substance represented by formula (Ⅰ) to the fluoroethylene carbonate is (0.001-0.065):
1.
14. The electrolyte according to any one of claims 11-13, characterized in that, The mass ratio of the nitrile substance to the fluoroethylene carbonate is (0.0625-0.65):
1.
15. The electrolyte according to any one of claims 8-14, characterized in that, The electrolyte also includes thioesters.
16. The electrolyte as described in claim 15, characterized in that, The thioesters in the electrolyte account for 1%-5% by mass.
17. The electrolyte as described in claim 15 or 16, characterized in that, The thioesters include one or more of the following: 1,3-propanesulfonate lactone, 1,4-butanesulfonate lactone, 1,3-propenesulfonate lactone, methylene disulfonate, vinyl sulfate, vinyl sulfite, 4-methyl ethylene sulfate, dimethyl sulfite, diethyl sulfite, dimethyl sulfate, and diethyl sulfate.
18. The electrolyte according to any one of claims 8-17, characterized in that, The electrolyte also includes other additives; the other additives include one or more of biphenyl, fluorobenzene, trifluoromethyl ethylene carbonate, vinylene carbonate, ethylene ethylene carbonate, and flame retardants.
19. The battery electrolyte according to any one of claims 8-18, characterized in that, The organic solvent includes one or more of carbonate solvents, carboxylic acid ester solvents, and ether solvents.
20. A secondary battery, characterized in that, The secondary battery includes a positive electrode, a negative electrode, a separator and an electrolyte located between the positive electrode and the negative electrode, wherein the electrolyte includes the electrolyte according to any one of claims 8-19.
21. The secondary battery as described in claim 20, characterized in that, The secondary battery includes lithium secondary batteries, sodium secondary batteries, potassium secondary batteries, magnesium secondary batteries, zinc secondary batteries, or aluminum secondary batteries.
22. The secondary battery as described in claim 20 or 21, characterized in that, The negative electrode includes one or more of the following: lithium titanate negative electrode, carbon-based negative electrode, silicon-based negative electrode, tin-based negative electrode, phosphorus-based negative electrode, lithium negative electrode, sodium negative electrode, potassium negative electrode, magnesium negative electrode, zinc negative electrode, and aluminum negative electrode.
23. The secondary battery according to any one of claims 20-22, characterized in that, The positive electrode uses one or more of the following active materials: layered transition metal oxides and polyanionic positive electrode materials.
24. An electrical appliance, characterized in that, It includes a housing and a battery housed within the housing, the battery including a secondary battery as described in any one of claims 20-23.
25. An energy storage device, characterized in that, The energy storage device includes a plurality of secondary batteries as described in any one of claims 20-23.