Sodium secondary batteries and electrical devices
By introducing calcium and fluorocarbonate compounds from the electrolyte into the negative electrode film of a sodium secondary battery, and combining them with difluorooxalate borate, a stable SEI film is formed, which solves the gas generation problem in sodium secondary batteries during cycling and storage, and improves the battery's kinetic performance and cycle stability.
Patent Information
- Application Number
- CN202611550638.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-11-09
- Filing Date
- 2024-01-30
- Publication Date
- 2026-11-10
Smart Images

Figure CN123073181A_ABST
Abstract
Description
[0001] This application is a divisional application based on the invention with application number 202480071575.4, application date January 30, 2024, applicant CATL, and invention title "Sodium Secondary Battery and Power Consumption Device".
[0002] Cross-referencing This application incorporates Chinese Patent Application No. 202311486636.7, filed on November 9, 2023, entitled “Sodium Secondary Battery and Electrical Device,” which is incorporated herein by reference in its entirety. Technical Field
[0003] This application relates to the field of secondary battery technology, and in particular to a sodium secondary battery and an electrical device thereof. Background Technology
[0004] In recent years, rechargeable batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric cars, military equipment, aerospace, and many other fields. With the increasing application of rechargeable batteries, higher requirements have been placed on their cycle performance and service life.
[0005] In terms of resources and cost, sodium-ion batteries have a greater advantage than lithium-ion batteries. However, sodium-ion batteries produce gas more severely during cycling and storage, which limits their further application. Summary of the Invention
[0006] This application is made in view of the above-mentioned problems, and its purpose is to provide a sodium secondary battery for reducing gas production in sodium secondary batteries and improving the cycle stability of the battery.
[0007] The first aspect of this application provides a sodium secondary battery, the sodium secondary battery including a negative electrode sheet, the negative electrode sheet including a negative electrode film layer containing calcium element; and an electrolyte, the electrolyte including a first component, the first component being a fluorocarbonate compound.
[0008] Introducing calcium into the negative electrode film can induce sodium ion deposition, helping to suppress sodium dendrite formation and reduce the oxidation and gas generation of unstable components caused by sodium dendrites at the negative electrode. This reduces the amount of gas generated at the negative electrode during discharge and lowers the volume expansion rate of the battery after high-temperature storage. However, calcium easily forms calcium hydroxide during the negative electrode slurry mixing process, leading to high impedance and low initial efficiency, which in turn reduces the battery's kinetic performance, especially its charging capability at low temperatures. Introducing fluorocarbonate compounds into the electrolyte can react with calcium hydroxide during cycling to form stable CaF2, reducing the calcium hydroxide content and mitigating its negative impact on the negative electrode. Furthermore, it forms a stable solid electrolyte interphase (SEI) film on the negative electrode surface, reducing the generation of unstable components at the negative electrode while improving the battery's kinetic performance and initial efficiency, thus comprehensively enhancing the battery's cycle stability.
[0009] In any embodiment, based on the total mass of the electrolyte, the mass percentage of the fluorocarbonate compound is 'a', and based on the total mass of the negative electrode film, the mass percentage of calcium in the negative electrode film is 'b', and a and b satisfy: a / b≥1. In some embodiments, a and b satisfy: 10000≥a / b≥10.
[0010] When the a / b value is within a suitable range, through the synergistic effect of calcium and fluorinated carbonate compounds in the negative electrode, sodium secondary batteries can effectively suppress gas production in the negative electrode, reduce gas production during high-temperature storage, and improve battery dynamic performance, first-efficiency performance, and cycle stability.
[0011] In any embodiment, the mass percentage 'a' of the fluorocarbonate compound is 0.01% to 10% based on the total mass of the electrolyte. In some embodiments, the mass percentage 'a' of the fluorocarbonate compound is 0.2% to 10% based on the total mass of the electrolyte.
[0012] When the mass percentage 'a' of fluorinated carbonate compounds is within a suitable range, the fluorinated carbonate compounds can form a complex with calcium hydroxide, which can reduce the calcium hydroxide content in the negative electrode, improve the battery's dynamic performance and first-time efficiency, and also form stable organic and inorganic components in the SEI film of the negative electrode together with calcium hydroxide, reducing the gas generation of unstable components in the negative electrode, reducing the gas generation rate after the battery is stored at high temperature, and comprehensively improving the cycle stability of the battery.
[0013] In any embodiment, based on the total mass of the negative electrode film, the mass percentage b of calcium in the negative electrode film is 1 ppm to 3000 ppm. In any embodiment, based on the total mass of the negative electrode film, the mass percentage b of calcium in the negative electrode film is 50 ppm to 1000 ppm.
[0014] When the mass percentage (b) of calcium in the negative electrode film is within a suitable range, it can reduce the negative impact of excessive calcium content on the secondary battery impedance and initial efficiency, while fully leveraging the role of calcium in suppressing dendrite formation and reducing gas production. This reduces battery gas production while improving the battery's low-temperature charging performance, initial efficiency, and room-temperature cycle capacity retention. When the mass percentage (b) of calcium in the negative electrode film is between 50 ppm and 1000 ppm, the battery's gas production rate is reduced, while the battery's kinetic performance, initial efficiency, and cycle stability are further improved.
[0015] In any embodiment, the fluorocarbonate compound includes the compound shown in Formula I. Formula I Among them, R1, R2, R3, and R4 each independently include hydrogen atoms, halogen atoms, and carbon atoms. 1-6 hydrocarbon group, C 1-3 Haloalkyl, C 1-3 Alkoxy, C 1-3 At least one of haloalkoxy, ester, cyano, sulfonic acid, and isocyanate groups; and at least one of R1, R2, R3, and R4 is a fluorine atom.
[0016] Cyclic fluorocarbonates in which at least one of R1, R2, R3, and R4 is a fluorine atom are easy to open, forming an SEI film on the negative electrode surface, reducing battery gas production, and improving battery dynamic performance, first-efficiency performance, and cycle stability.
[0017] In any embodiment, the fluorocarbonate compound includes at least one of the following compounds: Formula II-1 Formula II-2 Formula II-3 Formula II-4 Formula II-5 Formula II-6 Formula II-7 Formula II-8 Formula II-9 Formula II-10.
[0018] In any embodiment, the electrolyte further includes a second component, which is difluorooxalate borate.
[0019] The SEI film formed at the negative electrode interface in sodium secondary batteries mainly consists of sodium alkyl carbonate (ROCO2Na) and sodium carbonate. However, sodium alkyl carbonate has a higher solubility in solvents than lithium alkyl carbonate, which makes the SEI film of sodium secondary batteries very unstable. Side reactions easily occur between the electrolyte and the negative electrode film, which is an important reason for the short lifespan of sodium secondary batteries.
[0020] Difluorooxalate borate has a high reduction potential, allowing it to preferentially reduce to form a film compared to the solvent. On the one hand, it effectively inhibits the formation of easily soluble substances such as sodium alkyl carbonate. On the other hand, difluorooxalate borate can form a thin and dense low-resistance SEI film containing a large number of inorganic components such as sodium fluoride and sodium borate. It works synergistically with the organic components generated by fluorinated carbonate compounds, taking into account both the flexibility and stability of the SEI film, thereby further suppressing gas production and improving the kinetic performance, first efficiency, and cycle life of sodium secondary batteries.
[0021] In any embodiment, based on the total mass of the electrolyte, the mass percentage of difluorooxalate borate is c, the mass percentage of the fluorocarbonate compound is a, and c and a satisfy: c / a ≥ 0.001. In some embodiments, c and a satisfy: 2 ≥ c / a ≥ 0.1.
[0022] When the c / a value is within a suitable range, the synergistic effect of difluorooxalate borate and fluorocarbonate in the electrolyte can improve the stability, flexibility and sodium conductivity of the SEI film, reduce gas generation during high-temperature storage of the battery, improve battery dynamic performance and first-time efficiency, and comprehensively improve the cycle stability of the battery.
[0023] In any embodiment, the mass percentage c of the difluorooxalate borate is 0.01%-5% based on the total mass of the electrolyte. In some embodiments, the mass percentage c of the difluorooxalate borate is 0.1%-2% based on the total mass of the electrolyte.
[0024] When the mass percentage (c) of difluorooxalate borate is within a suitable range, difluorooxalate borate can form a complex with fluorinated carbonate compounds, which can improve the stability and flexibility of the SEI film, reduce the gas generation of unstable components at the negative electrode, and reduce the gas generation rate after high-temperature storage of the battery; it can also improve the sodium conductivity of the SEI film, improve the battery dynamic performance and first-time efficiency, and comprehensively improve the cycle stability of the battery.
[0025] In any embodiment, the difluorooxalate borate has the general chemical formula shown in Formula III. (F2C2O4B) y M-type III Wherein, M includes one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Fe, Ni, and Al, and y is 1, 2, or 3.
[0026] In any embodiment, the negative electrode film layer includes a negative electrode active material, which includes one or more of hard carbon, sodium metal, sodium-tin alloy, and metal oxide.
[0027] In any embodiment, the sodium secondary battery further comprises a positive electrode plate, the positive electrode plate comprises a positive electrode active material, and the positive electrode active material comprises a sodium transition metal oxide.
[0028] In any embodiment, based on the total mass of the positive electrode active material, the positive electrode active material further contains a copper element, and the mass proportion d of the copper element is 0.01% to 23%. In some embodiments, based on the total mass of the positive electrode active material, the mass proportion d of the copper element is 6.5% to 18%.
[0029] The positive electrode active material containing the copper element has a more stable structure, which can further improve the cycle stability of the battery. When the mass proportion of the copper element is within a suitable range, the cycle stability of the battery is improved while the copper element will not be converted into Cu at high voltage 3+ , which causes the electrolyte to accelerate decomposition under its high oxidizing property and sharply deteriorate the gas generation phenomenon of the battery. When the mass proportion of the copper element is in the range of 6.5% to 18%, the low gas generation amount, high kinetic performance, high initial efficiency and high cycle stability of the secondary battery can be further balanced.
[0030] In any embodiment, the sodium transition metal oxide comprises Na m Cu n X o Fe p Mn q O 2-s, wherein X comprises one or more of Li, Be, B, Mg, Al, K, Ca, Ti, Co, Ni, Zn, Ga, Sr, Y, Nb, Mo, In, Sn, Fe and Ba, 0≤m≤0.5, 0≤n≤0.5, 0≤o<0.5, 0≤p≤0.5, 0<q≤0.68, n+o+p+q=1, 0≤s<0.2. In some embodiments, the sodium transition metal oxide comprises Na[Cu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2, Na 7 / 9 [Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, Na 9 / 10 [Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2 of at least one.
[0031] Sodium transition metal oxide cathode active materials have high voltage. While the anionic oxygen contributes to capacity, it also generates a large amount of protonated hydrogen, accelerating the oxidation and gas production of unstable components in the negative electrode, resulting in severe gas generation on the negative electrode side. Through the combined action of calcium in the negative electrode film layer and fluorinated carbonate compounds in the electrolyte provided in this application embodiment, battery capacity and energy density can be improved while effectively reducing battery gas generation, enhancing battery kinetic performance, first-efficiency performance, and cycle stability.
[0032] In any embodiment, the electrolyte further includes a third component, which is one or more of the following: vinylene carbonate, ethylene ethylene carbonate, 1,3-propane sulfonyl lactone, 1,3-propene sulfonate lactone, vinyl sulfate, maleic anhydride, succinic anhydride, triallyl phosphate, sodium tetrafluorooxalate phosphate, sodium difluorobis(oxalate) phosphate, sodium difluorophosphate, and sodium fluorosulfonate.
[0033] The SEI film formed at the negative electrode interface in sodium-ion batteries mainly consists of sodium alkyl carbonate and sodium carbonate. However, sodium alkyl carbonate has a higher solubility in the electrolyte solvent than lithium alkyl carbonate, making the SEI film of sodium-ion batteries highly unstable. This leads to continuous side reactions between the electrolyte and the negative electrode, resulting in poor cycle performance. A second component containing unsaturated functional groups can preferentially reduce to form a film at the negative electrode compared to the solvent. It works in conjunction with fluorinated carbonate compounds and calcium elements at the negative electrode to inhibit the formation of easily soluble substances such as sodium alkyl carbonate, reducing battery gas production and improving the battery's kinetic performance, initial efficiency, and cycle stability.
[0034] In any embodiment, the third component accounts for 0.01% to 10% of the total mass of the electrolyte. In some embodiments, the third component accounts for 0.1% to 5% of the total mass of the electrolyte.
[0035] When the mass ratio of the third component is within the above-mentioned range, it can improve the gas generation phenomenon in the battery while controlling the thickness of the SEI film, thereby simultaneously achieving low impedance and low gas generation in the battery, and improving the battery's dynamic performance, first-efficiency performance, and cycle stability.
[0036] A second aspect of this application provides an electrical device including the sodium secondary battery of the first aspect. Attached Figure Description
[0037] Figure 1 This is a schematic diagram of a secondary battery according to one embodiment of this application; Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of this application is shown. Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application; Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application; Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown; Figure 6 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.
[0038] Explanation of reference numerals in the attached figures: 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Secondary battery; 51 Housing; 52 Electrode assembly; 53 Cover plate. Detailed Implementation
[0039] The embodiments of the sodium secondary battery and power-consuming device of this application are hereby disclosed in detail with appropriate reference to the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of actually identical structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0040] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0041] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0042] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0043] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0044] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0045] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0046] In existing technologies, it is generally believed that gas production in sodium-ion batteries mainly originates from the oxidation of the electrolyte by the positive electrode active material under high voltage. Therefore, existing technologies often employ methods such as coating the positive electrode active material and forming a film on the positive electrode surface to reduce gas production in secondary batteries. During the research process, the applicant discovered that another important factor contributing to gas production in sodium-ion batteries lies in the negative electrode. Unlike lithium-ion batteries, sodium-ion batteries often use hard carbon as their negative electrode active material. The capacity utilization of hard carbon mainly consists of two stages: the first stage is between 1.5V and 0.1V (vs Na / Na). + The capacity of ) comes from Na + The adsorption process at defects on the hard carbon surface, the second stage is at 0.1V (vs Na / Na) + The following capacity contribution comes from Na + The filling process within the micropores of hard carbon. To improve the negative electrode capacity, existing technologies often increase the porosity of hard carbon. However, Na... +The potential during the hard carbon micropore filling process is close to the potential for sodium deposition (0V), which easily leads to sodium deposition during charging. The deposited sodium dendrites are highly reactive and react rapidly with the electrolyte to produce a large amount of gas and unstable byproducts. These unstable byproducts are further oxidized and decomposed during discharge as the negative electrode potential increases and the film-forming driving force is insufficient. In addition, unstable organic byproducts are easily dissolved in the electrolyte, causing the solid electrolyte interphase (SEI) film to be in a constant cycle of dissolution and repair, exacerbating battery gas production and deteriorating cycle stability.
[0047] Sodium secondary battery Based on this, this application proposes a sodium secondary battery, which includes a negative electrode sheet, the negative electrode sheet including a negative electrode film layer containing calcium; and an electrolyte, the electrolyte including a first component, the first component being a fluorocarbonate compound.
[0048] A sodium secondary battery is a type of secondary battery that mainly relies on the movement of sodium ions between the positive and negative electrodes to function.
[0049] It is understood that calcium can be introduced into the negative electrode film in any form. In some embodiments, calcium is introduced into the negative electrode film in the form of calcium oxide or calcium salt. In some embodiments, calcium is introduced into the negative electrode film in the form of CaO.
[0050] Fluorinated carbonate compounds are compounds containing a carbonate group (-OC(O)O-) in which at least one hydrogen atom is replaced by a fluorine atom. They can be linear or cyclic compounds.
[0051] Introducing calcium into the negative electrode film can induce sodium ion deposition, helping to suppress sodium dendrite formation and reduce the oxidation and gas generation of unstable components caused by sodium dendrites at the negative electrode. This reduces the amount of gas generated at the negative electrode during discharge and lowers the volume expansion rate of the battery after high-temperature storage. However, calcium easily forms calcium hydroxide during the negative electrode slurry mixing process, leading to high impedance and low initial efficiency, which in turn reduces the battery's kinetic performance, especially its charging capability at low temperatures. Introducing fluorocarbonate compounds into the electrolyte can react with calcium hydroxide during cycling to form stable CaF2, reducing the calcium hydroxide content and mitigating its negative impact on the negative electrode. Furthermore, it forms a stable solid electrolyte interphase (SEI) film on the negative electrode surface, reducing the generation of unstable components at the negative electrode while improving the battery's kinetic performance and initial efficiency, thus comprehensively enhancing the battery's cycle stability.
[0052] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the fluorocarbonate compound is 'a', and based on the total mass of the negative electrode film, the mass percentage of calcium in the negative electrode film is 'b', and a and b satisfy: a / b≥1. In some embodiments, a and b satisfy: 10000≥a / b≥10.
[0053] In some implementations, the value of a / b can be 1, 3.3, 5, 10, 20, 50, 100, 200, 500, 1000, 5000, 10000, or any value range between the two.
[0054] When the a / b value is within a suitable range, through the synergistic effect of calcium and fluorinated carbonate compounds in the negative electrode, sodium secondary batteries can effectively suppress gas production in the negative electrode, reduce gas production during high-temperature storage, and improve battery dynamic performance, first-efficiency performance, and cycle stability.
[0055] In some embodiments, the mass percentage 'a' of the fluorocarbonate compound is 0.01% to 10% based on the total mass of the electrolyte. In some embodiments, the mass percentage 'a' of the fluorocarbonate compound is 0.2% to 10% based on the total mass of the electrolyte.
[0056] In some embodiments, based on the total mass of the electrolyte, the mass percentage 'a' of the fluorocarbonate compound is 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any value between these values.
[0057] When the mass percentage 'a' of fluorinated carbonate compounds is within a suitable range, the fluorinated carbonate compounds can form a complex with calcium hydroxide, which can reduce the calcium hydroxide content in the negative electrode, improve the battery's dynamic performance and first-time efficiency, and also form stable organic and inorganic components together with calcium hydroxide in the negative electrode SEI film, reducing the gas generation of unstable components in the negative electrode, reducing the gas generation rate after the battery is stored at high temperature, and comprehensively improving the cycle stability of the battery.
[0058] In some embodiments, based on the total mass of the negative electrode film, the mass percentage b of calcium in the negative electrode film is 1 ppm to 3000 ppm. In some embodiments, based on the total mass of the negative electrode film, the mass percentage b of calcium in the negative electrode film is 50 ppm to 1000 ppm.
[0059] In some embodiments, based on the total mass of the negative electrode film, the mass percentage b of calcium in the negative electrode film is 1 ppm, 50 ppm, 100 ppm, 200 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 1500 ppm, 2000 ppm, 2500 ppm, 3000 ppm, or any value between these values.
[0060] In this article, ppm refers to parts per million.
[0061] When the mass percentage (b) of calcium in the negative electrode film is within a suitable range, it can reduce the negative impact of excessive calcium content on the secondary battery impedance and initial efficiency, while fully leveraging the role of calcium in suppressing dendrite formation and reducing gas production. This reduces battery gas production while improving the battery's low-temperature charging performance, initial efficiency, and room-temperature cycle capacity retention. When the mass percentage (b) of calcium in the negative electrode film is between 50 ppm and 1000 ppm, the battery's gas production rate is reduced, and the battery's kinetic performance, initial efficiency, and cycle stability are further improved.
[0062] In some embodiments, the fluorocarbonate compound includes compounds represented by Formula I. Formula I Among them, R1, R2, R3, and R4 each independently include hydrogen atoms, halogen atoms, and carbon atoms. 1-6 hydrocarbon group, C 1-3 Haloalkyl, C 1-3 Alkoxy, C 1-3 At least one of haloalkoxy, ester, cyano, sulfonic acid, and isocyanate groups; and at least one of R1, R2, R3, and R4 is a fluorine atom.
[0063] In this article, the term "halogen atom" refers to elements in Group VIIA of the periodic table, including but not limited to: F, Cl, Br, and I.
[0064] In this article, the term "C" 1-6 "Hydrocarbon group" refers to a group containing carbon and hydrogen atoms, comprising 1 to 6 carbon atoms. In some embodiments, C 1-6The hydrocarbon group does not include unsaturated bonds and is an alkyl group. Examples include, but are not limited to, methyl, ethyl, propyl, isopropyl, 2-methyl-1-propyl, 2-methyl-2-propyl, 2-methyl-1-butyl, 3-methyl-1-butyl, 2-methyl-3-butyl, 2,2-dimethyl-1-propyl, 2-methyl-1-pentyl, 3-methyl-1-pentyl, 4-methyl-1-pentyl, 2-methyl-2-pentyl, 3-methyl-2-pentyl, 4-methyl-2-pentyl, 2,2-dimethyl-1-butyl, 3,3-dimethyl-1-butyl, 2-ethyl-1-butyl, butyl, isobutyl, tert-butyl, pentyl, isopentyl, neopentyl, and hexyl. In some embodiments, C... 1-6 The hydrocarbon group includes unsaturated bonds, such as cycloalkyl, alkenyl, alkynyl, and aryl, and by way of example, includes but is not limited to cyclopropyl, cyclobutyl, vinyl, 1-propenyl or 2-propenyl, phenyl, and naphthyl.
[0065] In this article, the term "C" 1-3 "Halogenated alkyl" refers to a C-type alkyl group in which at least one hydrogen atom is replaced by a halogen atom. 1-3 Alkyl groups, for example including but not limited to: -CF3, -CF2CH2, -CF2CH2CH3.
[0066] In this article, the term "C" 1-3 "Alkoxy" refers to a carbon atom connected to the main carbon chain via an oxygen atom. 1-3 Alkyl groups, as examples, include, but are not limited to, methoxy (CH3O-), ethoxy (C2H5O-), and propoxy (C3H7O-).
[0067] In this article, the term "C" 1-3 "Haloalkoxy" refers to a carbon atom in which at least one hydrogen atom is replaced by a halogen atom. 1-3 Alkyl group.
[0068] In this article, the term "ester group" refers to the -COO- group.
[0069] In this article, the term "cyano" refers to the -CN group.
[0070] In this paper, the term "sulfonic acid group" refers to the -SO3H group.
[0071] In this article, the term "isocyanate group" refers to the -NCO group.
[0072] Cyclic fluorocarbonates in which at least one of R1, R2, R3, and R4 is a fluorine atom are easy to open, forming an SEI film on the negative electrode surface, reducing battery gas production, and improving battery dynamic performance, first-efficiency performance, and cycle stability.
[0073] In some embodiments, the fluorocarbonate compound includes at least one of the following compounds: Formula II-1 Formula II-2 Formula II-3 Formula II-4 Formula II-5 Formula II-6 Formula II-7 Formula II-8 Formula II-9 Formula II-10.
[0074] In some embodiments, the electrolyte further includes a second component, which is difluorooxalate borate.
[0075] In this article, "difluorooxalate borate" is a borate with an anion of […]. Difluorooxalate borates include, but are not limited to, lithium difluorooxalate borate, sodium difluorooxalate borate, magnesium difluorooxalate borate, calcium difluorooxalate borate, barium difluorooxalate borate, aluminum difluorooxalate borate, and iron difluorooxalate borate.
[0076] In some embodiments, difluorooxalate borate includes sodium difluorooxalate borate.
[0077] In some embodiments, difluorooxalate borate includes calcium difluorooxalate borate.
[0078] The SEI film formed at the negative electrode interface in sodium secondary batteries mainly consists of sodium alkyl carbonate (ROCO2Na) and sodium carbonate. However, sodium alkyl carbonate has a higher solubility in solvents than lithium alkyl carbonate, which makes the SEI film of sodium secondary batteries very unstable. Side reactions easily occur between the electrolyte and the negative electrode film, which is an important reason for the short lifespan of sodium secondary batteries.
[0079] Difluorooxalate borate has a high reduction potential, allowing it to preferentially reduce to form a film compared to the solvent. On the one hand, it effectively inhibits the formation of easily soluble substances such as sodium alkyl carbonate. On the other hand, difluorooxalate borate can form a thin and dense low-resistance SEI film containing a large number of inorganic components such as sodium fluoride and sodium borate. It works synergistically with the organic components generated by fluorinated carbonate compounds, taking into account both the flexibility and stability of the SEI film, thereby further suppressing gas production and improving the kinetic performance, first efficiency, and cycle life of sodium secondary batteries.
[0080] In some embodiments, based on the total mass of the electrolyte, the mass percentage of difluorooxalate borate is c, and the mass percentage of the fluorocarbonate compound is a, where c and a satisfy: c / a ≥ 0.001. In some embodiments, c and a satisfy: 2 ≥ c / a ≥ 0.1.
[0081] In some implementations, the value of c / a can be 0.001, 0.1, 0.8, 1, 2, 3, 4, 5 or any value between them.
[0082] When the c / a value is within a suitable range, the synergistic effect of difluorooxalate borate and fluorocarbonate in the electrolyte can improve the stability and sodium conductivity of the SEI film, reduce gas generation during high-temperature storage of the battery, improve battery dynamic performance and first-time efficiency, and comprehensively enhance the cycle stability of the battery.
[0083] In some embodiments, the mass percentage c of difluorooxalate borate is 0.01%-5% based on the total mass of the electrolyte. In some embodiments, the mass percentage c of difluorooxalate borate is 0.1%-2% based on the total mass of the electrolyte.
[0084] In some embodiments, based on the total mass of the electrolyte, the mass percentage c of the difluorooxalate borate is 0.01%, 0.05%, 0.1%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, or any value between these values.
[0085] When the mass percentage (c) of difluorooxalate borate is within a suitable range, difluorooxalate borate can form a complex with fluorinated carbonate compounds, which can improve the stability of the SEI film, reduce the gas generation of unstable components at the negative electrode, and reduce the gas generation rate after high-temperature storage of the battery; it can also improve the sodium conductivity of the SEI film, improve the battery dynamic performance and first-time efficiency, and comprehensively improve the cycle stability of the battery.
[0086] In some embodiments, the difluorooxalate borate has the general chemical formula shown in Formula III. (F2C2O4B) y M-type III Wherein, M includes one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Fe, Ni, and Al, and y is 1, 2, or 3.
[0087] In some embodiments, the negative electrode film layer includes a negative electrode active material, which includes one or more of hard carbon, sodium metal, sodium-tin alloy, and metal oxides.
[0088] In some embodiments, the negative electrode active material includes hard carbon.
[0089] In some embodiments, the sodium secondary battery further includes a positive electrode sheet, which comprises a positive electrode active material.
[0090] In some embodiments, the positive electrode active material further contains a copper element, and based on the total mass of the positive electrode active material, the mass proportion d of the copper element is 0.01% to 23%. In some embodiments, based on the total mass of the positive electrode active material, the mass proportion d of the copper element is 6.5% to 18%. In some embodiments, based on the total mass of the positive electrode active material, the mass proportion d of the copper element is 0.01%, 4%, 6.5%, 10%, 13%, 15%, 18%, 20%, 23%, or a numerical range between any two of the foregoing values.
[0091] The positive electrode active material containing the copper element has a more stable structure, which can further improve the cycle stability of the battery. When the mass proportion of the copper element is within an appropriate range, while the cycle stability of the battery is improved, the copper element will not be converted into Cu at a high voltage 3+ , which causes the electrolyte to accelerate decomposition under its high oxidizing property and sharply deteriorate the gas generation phenomenon of the battery. When the mass proportion of the copper element is within the range of 6.5% to 18%, the low gas production, high kinetic performance, high initial efficiency and high cycle stability of the secondary battery can be further balanced.
[0092] In some embodiments, the positive electrode active material may employ a positive electrode active material well known in the art for batteries. As an example, the positive electrode active material may include at least one of the following materials: Prussian blue analogs, sodium-containing phosphates, sodium-containing transition metal oxides, and respective modified compounds thereof. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone, or two or more thereof may be used in combination. The Prussian blue analog is NaxP[R(CN)6] δ ·zH2O, wherein P and R are each independently selected from at least one of transition metal elements, 0<x≤2, 0<δ≤1 and 0≤z≤10; the sodium-containing phosphate is Na b Me c (PO4) d , wherein Me is one or more of Ti, Cr, Mn, Fe, Co, Ni, V, Cu and Zn, 0<b≤4, 0<c≤2, 1≤d≤3; the sodium-containing transition metal oxide is Na a M b N c Fe d Mn e O2, M and N include at least one of Sc, Ti, V, Cr, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W and Pb, 0.05≤b≤0.2, 0.2≤c≤0.3, 0.2≤d≤0.3, 0.3≤e≤0.4, 0.75≤a / (b+c+d+e)≤1.
[0093] In some embodiments, the positive electrode active material comprises a sodium transition metal oxide.
[0094] In some embodiments, the sodium transition metal oxide comprises Na m Cu n X o Fe p Mn q O 2-s, wherein X comprises one or more of Li, Be, B, Mg, Al, K, Ca, Ti, Co, Ni, Zn, Ga, Sr, Y, Nb, Mo, In, Sn, Fe, Ba, 0≤m≤0.5, 0≤n≤0.5, 0≤o<0.5, 0≤p≤0.5, 0<q≤0.68, n+o+p+q=1, 0≤s<0.2. In some embodiments, the sodium transition metal oxide comprises Na[Cu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2, Na 7 / 9 [Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, Na 9 / 10 [Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2 at least one of them.
[0095] The sodium transition metal oxide positive electrode active material has a high voltage, and the anionic oxygen therein will generate a large amount of proton hydrogen while contributing to the capacity, which accelerates the oxidation and gas production of unstable components in the negative electrode, resulting in severe gas production on the negative electrode side. Through the combined action of the calcium element in the negative electrode film layer in the negative electrode sheet provided by the embodiments of the present application and the fluorocarbonate compound in the electrolyte, the gas production of the battery can be effectively reduced while the battery capacity and energy density are improved, and the kinetic performance, initial efficiency and cycle stability of the battery are enhanced.
[0096] In some embodiments, the electrolyte further comprises a third component, and the third component is one or more of vinylene carbonate, vinylethylene carbonate, 1,3-propane sultone, 1,3-propene sultone, vinyl sulfate, maleic anhydride, succinic anhydride, triallyl phosphate, sodium tetrafluorooxalatophosphate, sodium difluorobis(oxalato)phosphate, sodium difluorophosphate, and sodium fluorosulfonate.
[0097] The SEI film formed at the negative electrode interface in sodium-ion batteries mainly consists of sodium alkyl carbonate and sodium carbonate. However, sodium alkyl carbonate has a higher solubility in the electrolyte solvent than lithium alkyl carbonate, making the SEI film of sodium-ion batteries highly unstable. This leads to continuous side reactions between the electrolyte and the negative electrode, resulting in poor cycle performance. A second component containing unsaturated functional groups can preferentially reduce to form a film at the negative electrode compared to the solvent. It works in conjunction with fluorinated carbonate compounds and calcium elements at the negative electrode to inhibit the formation of easily soluble substances such as sodium alkyl carbonate, reducing battery gas production and improving the battery's kinetic performance, initial efficiency, and cycle stability.
[0098] In some embodiments, the third component accounts for 0.01% to 10% of the total mass of the electrolyte. In some embodiments, the third component accounts for 0.1% to 5% of the total mass of the electrolyte.
[0099] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the third component is 0.01%, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any value between these values.
[0100] When the mass ratio of the third component is within the above-mentioned range, it can improve the gas generation phenomenon in the battery while controlling the thickness of the SEI film, thereby simultaneously achieving low impedance and low gas generation in the battery, and improving the battery's dynamic performance, first-efficiency performance, and cycle stability.
[0101] In some embodiments, the electrolyte includes an electrolyte salt selected from at least one of NaPF6, NaBF4, NaN(SO2F)2 (NaFSI), NaClO4, NaAsF6, NaB(C2O4)2 (NaBOB), NaBF2(C2O4) (NaDFOB), NaN(SO2RF)2, and NaN(SO2F)(SO2RF), wherein RF represents C x1 F 2x1+1 x1 is an integer from 1 to 10. In some embodiments, x1 can be an integer from 1 to 3. In some embodiments, the electrolyte salt is selected from one or more of NaPF6, NaClO4, NaN(SO2F)2, NaN(CF3SO2)2, NaB(C2O4)2, and NaBF2(C2O4). In some embodiments, the electrolyte salt is selected from one or more of NaPF6, NaN(SO2RF)2, and NaBF2(C2O4). In some embodiments, RF is -CF3, -C2F5, or -CF2CF2CF3.
[0102] In some embodiments, the electrolyte includes a solvent, which includes at least one selected from chain carbonates, chain carboxylic esters, cyclic carbonates, ether solvents, sulfone solvents, and nitrile solvents. In some embodiments, the chain carbonate includes at least one selected from dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), methyl propyl carbonate (MPC), methyl isopropyl carbonate (MIPC), methyl butyl carbonate, ethyl propyl carbonate, dipropyl carbonate, and dibutyl carbonate. In some embodiments, the chain carbonate includes at least one selected from dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), and methyl propyl carbonate (MPC). In some embodiments, the chain carboxylic ester includes at least one selected from methyl formate (MF), ethyl formate (EF), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), ethyl butyrate (EB), methyl acetate (MA), ethyl acetate (EA), and propyl acetate (PA). In some embodiments, the chain carboxylic acid ester includes at least one selected from methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl acetate (MA), ethyl acetate (EA), and propyl acetate (PA). In some embodiments, the ether solvent includes at least one selected from dioxolane (DOL), tetrahydrofuran (THF), 2-methyltetrahydrofuran (2Me-THF), tetrahydropyran (THP), 1,2-dimethoxyethane (DME), diethylene glycol dimethyl ether (DG), 1,2-diethoxyethane, and 1,2-dibutoxyethane.
[0103] [Positive electrode plate] A positive electrode typically includes a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector, the positive electrode film layer including a positive electrode active material.
[0104] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0105] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0106] In some embodiments, the positive electrode film layer includes a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0107] In some embodiments, the positive electrode film may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0108] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0109] [Negative electrode plate] The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer including a negative electrode active material.
[0110] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0111] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil or aluminum foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0112] In some embodiments, the negative electrode film layer includes an adhesive. As an example, the adhesive may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0113] In some embodiments, the negative electrode film layer includes a conductive agent. As an example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0114] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0115] In some embodiments, the negative electrode sheet can be prepared by dispersing the above-mentioned components for preparing the negative electrode sheet, such as negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto a negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.
[0116] [Isolation membrane] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0117] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0118] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0119] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.
[0120] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0121] In this application, the shape of the sodium secondary battery includes, but is not limited to, cylindrical, square, or other arbitrary shapes. For example, Figure 1 This is an example of a square-structured sodium secondary battery.
[0122] In some implementations, refer to Figure 2The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator may be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The sodium secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.
[0123] In some embodiments, sodium secondary batteries can be assembled into battery modules, and the number of sodium secondary batteries contained in a battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.
[0124] Figure 3 This is battery module 4, used as an example. (See reference...) Figure 3 In battery module 4, multiple sodium secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple sodium secondary batteries 5 can be fixed in place using fasteners.
[0125] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of sodium secondary batteries 5 are received.
[0126] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0127] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0128] In addition, this application also provides an electrical device, which includes at least one of the sodium secondary battery, battery module, or battery pack provided in this application. The sodium secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0129] As an electrical device, sodium secondary batteries, battery modules, or battery packs can be selected according to their usage requirements.
[0130] Figure 6 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of sodium-ion batteries for this device, a battery pack or battery module can be used.
[0131] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use sodium-ion batteries as their power source.
[0132] Example The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0133] Preparation method Example 1: 1) Electrolyte In an argon-atmospheric glove box (H2O content <10ppm, O2 content <1ppm), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed at a mass ratio of 30 / 70, and 1M NaPF6 sodium salt was dissolved. Then, fluoroethylene carbonate was added and stirred until homogeneous to prepare the electrolyte. Based on the total mass of the electrolyte, the mass percentage of fluoroethylene carbonate was 1%.
[0134] 2) Preparation of positive electrode active materials Na 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3O2 preparation: 0.39 mol Na2CO3, 0.22 mol CuO, 0.06 mol Fe2O3 and 0.67 mol MnO2 precursors were ball-milled in a ball mill for 12 h with ethanol as the dispersant. After drying, the uniformly mixed powder was pressed into tablets at 20 MPa and sintered at 900 °C for 12 h to obtain the O2. The sintered powder needs to be quickly transferred to a glove box for storage.
[0135] 3) Preparation of positive electrode sheet Na, the positive electrode active material 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were thoroughly mixed in an N-methylpyrrolidone solvent system at a weight ratio of 90:5:5 to obtain a positive electrode slurry; the positive electrode slurry was then mixed at a rate of 0.28 g (dry weight) / 1540.25 mm. 2 The density is uniformly coated on a 13μm thick positive electrode current collector aluminum foil; after the aluminum foil is dried at room temperature, it is transferred to a 120℃ oven to dry for 1 hour, and then cold-pressed and slit to obtain the positive electrode sheet.
[0136] 4) Preparation of negative electrode sheet The negative electrode active material (hard carbon), conductive agent (acetylene black), binder (styrene-butadiene rubber (SBR), and thickener (sodium carboxymethyl cellulose (CMC-Na)) were thoroughly mixed in a deionized water solvent system at a weight ratio of 90:4:4:2. A certain amount of CaO was added to ensure that the calcium content in the dry slurry (i.e., the total mass of the negative electrode active material (hard carbon), conductive agent (acetylene black), binder (styrene-butadiene rubber (SBR), thickener (sodium carboxymethyl cellulose (CMC-Na), and CaO)) was 100 ppm, thus obtaining the negative electrode slurry. The negative electrode slurry was then prepared at a concentration of 0.14 g (dry weight) / 1540.25 mm. 2 The amount of coating is uniformly coated on a 13μm thick negative electrode current collector copper foil; after the copper foil is dried at room temperature, it is transferred to a 120℃ oven to dry for 1 hour, and then cold-pressed and slit to obtain the negative electrode sheet.
[0137] 5) Separating membrane A 9μm porous polyethylene (PE) polymer film was used as the separator.
[0138] 6) Battery manufacturing The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to isolate them. The cells are then wound to obtain a bare cell. The tabs are welded on, and the bare cell is placed in an outer package. The electrolyte prepared above is injected into the dried cell. After processes such as encapsulation, settling, formation, shaping, and capacity testing, the sodium secondary battery product of Example 1 is obtained.
[0139] The preparation methods of sodium secondary batteries in Examples 2-4 are basically the same as those in Example 1, except that the types of fluorocarbonate compounds are adjusted. Specific parameters are shown in Table 1.
[0140] The preparation methods of sodium secondary batteries in Examples 5-8 are basically the same as those in Example 1, except that the mass ratio of fluorinated carbonate compound based on electrolyte is adjusted. Specific parameters are shown in Table 1.
[0141] The preparation methods of sodium secondary batteries in Examples 9-12 are basically the same as those in Example 1. The difference is that the mass ratio of calcium in the negative electrode film is adjusted by adding different amounts of CaO to the negative electrode slurry. The specific parameters are shown in Table 2.
[0142] The preparation methods of sodium secondary batteries in Examples 13-18 are basically the same as those in Example 1, except that a second component, sodium difluorooxalate borate, is added to the electrolyte, and the mass ratio of sodium difluorooxalate borate and / or fluorocarbonate compounds is adjusted. Specific parameters are shown in Table 1.
[0143] The preparation method of the sodium secondary battery in Example 19 is basically the same as that in Example 14, except that the type of the second component is adjusted. The specific parameters are shown in Table 1.
[0144] The preparation methods of sodium secondary batteries in Examples 20-23 are basically the same as those in Example 1, except that the preparation processes of the positive electrode active material and the positive electrode sheet are adjusted to adjust the mass ratio of copper in the positive electrode active material. Specific parameters are shown in Table 2, and the preparation process is as follows: In Example 20, the copper content of the positive electrode active material in the positive electrode sheet is 0%, and the preparation method is as follows: Na 1 / 2 Fe 1 / 2 Mn 1 / 2 Preparation of O2: 0.25 mol Na2CO3, 0.25 mol Fe2O3 and 0.5 mol MnO2 precursors were ball-milled in a ball mill for 12 h with ethanol as the dispersant. After drying, the uniformly mixed powder was pressed into tablets at 20 MPa and sintered at 900 °C for 12 h to obtain O2. The sintered powder needs to be quickly transferred to a glove box for storage.
[0145] Na, the positive electrode active material 1 / 2 Fe 1 / 2 Mn 1 / 2 O2, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were thoroughly mixed in an N-methylpyrrolidone solvent system at a weight ratio of 90:5:5 to obtain a positive electrode slurry; the positive electrode slurry was then mixed at a rate of 0.28 g (dry weight) / 1540.25 mm. 2The amount of material is evenly coated onto a 13μm thick positive current collector aluminum foil; after the aluminum foil is dried at room temperature, it is transferred to a 120℃ oven to dry for 1 hour, and then cold-pressed and slit to obtain the positive electrode sheet.
[0146] In Example 21, the copper element in the positive electrode active material of the positive electrode sheet accounts for 6.5% by mass, and the preparation method is as follows: The positive electrode active material (50wt% Na) 1 / 2 Fe 1 / 2 Mn 1 / 2 O2 and 50wt% Na 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2), conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were thoroughly mixed in an N-methylpyrrolidone solvent system at a weight ratio of 90:5:5 to obtain a positive electrode slurry; the positive electrode slurry was then mixed at a rate of 0.28 g (dry weight) / 1540.25 mm. 2 The amount of material is evenly coated onto a 13μm thick positive current collector aluminum foil; after the aluminum foil is dried at room temperature, it is transferred to a 120℃ oven to dry for 1 hour, and then cold-pressed and slit to obtain the positive electrode sheet.
[0147] In Example 22, the copper element in the positive electrode active material of the positive electrode sheet accounts for 23% by mass, and the preparation method is as follows: Na 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2 preparation: 0.45 mol Na2CO3, 0.4 mol CuO, 0.05 mol Fe2O3 and 0.5 mol MnO2 precursor were ball-milled in a ball mill for 12 h with ethanol as the dispersant. After drying, the uniformly mixed powder was pressed into tablets at 20 MPa and sintered at 900 °C for 12 h to obtain the O2. The sintered powder needs to be quickly transferred to a glove box for storage.
[0148] Na, the positive electrode active material 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were thoroughly mixed in an N-methylpyrrolidone solvent system at a weight ratio of 90:5:5 to obtain a positive electrode slurry; the positive electrode slurry was then mixed at a rate of 0.28 g (dry weight) / 1540.25 mm. 2 The amount of material is evenly coated onto a 13μm thick positive current collector aluminum foil; after the aluminum foil is dried at room temperature, it is transferred to a 120℃ oven to dry for 1 hour, and then cold-pressed and slit to obtain the positive electrode sheet.
[0149] In Example 23, the copper element in the positive electrode active material of the positive electrode sheet accounts for 18% by mass, and the preparation method is as follows: The positive electrode active material (50wt% Na) 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2 and 50wt% Na 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2), conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were thoroughly mixed in an N-methylpyrrolidone solvent system at a weight ratio of 90:5:5 to obtain a positive electrode slurry; the positive electrode slurry was then mixed at a rate of 0.28 g (dry weight) / 1540.25 mm. 2 The amount of material is evenly coated onto a 13μm thick positive current collector aluminum foil; after the aluminum foil is dried at room temperature, it is transferred to a 120℃ oven to dry for 1 hour, and then cold-pressed and slit to obtain the positive electrode sheet.
[0150] The preparation methods of sodium secondary batteries in Examples 24-26 are basically the same as those in Example 1, except that a third component is added to the electrolyte. The specific parameters are shown in Table 1.
[0151] Comparative Example 1 Compared to Example 1, the electrolyte of Comparative Example 1 does not contain fluorocarbonate compounds. Specific parameters are shown in Table 1.
[0152] Comparative Example 2 Compared to Example 5, the negative electrode film of Comparative Example 2 does not contain calcium. Specific parameters are shown in Table 1.
[0153] Comparative Example 3 Compared to Example 1, the electrolyte of Comparative Example 3 does not contain fluorinated carbonate compounds, and the negative electrode film does not contain calcium. Specific parameters are shown in Table 1.
[0154] II. Battery Performance Testing 1. High-temperature storage volume change rate At 25°C, the sodium secondary batteries prepared in the examples and comparative examples were left to stand for 5 minutes, then charged at a constant current rate of 1C to 4.0V, and then charged at a constant voltage rate until the current was less than or equal to 0.05C. After that, they were left to stand for 5 minutes, and then discharged at a constant current rate of 1C to 1.5V. The volume V1 of the battery was tested by the water displacement method. Then the battery was placed in a 60°C oven and stored for 2 months. After that, the battery was taken out and the volume was tested as V2. The volume change rate of the battery was = (V2-V1) / V1×100%.
[0155] 2. Low-temperature charging performance at -10℃ A three-electrode battery with a reference electrode, sodium vanadium phosphate, was prepared. The battery was charged at 25°C with a constant current of 0.1C to a voltage of 4.0V, then charged at a constant voltage until the current was less than or equal to 0.05C. After resting for 5 minutes, it was discharged at a constant current of 1C to 1.5V, and the discharge capacity was recorded as C1. The battery was then placed at -10°C for 2 hours and charged at a constant current of 0.1C to a voltage of 4.0V. The charging capacity at the negative electrode potential before the reference potential reached -3.377V was obtained as C2. The charging capability of the battery at -10°C was calculated as C2 / C1 × 100%.
[0156] 3. Determination of the mass percentage of calcium in the negative electrode film layer The mass percentage of calcium in the negative electrode film can be determined according to the general rule EPA 6010D-2014, using inductively coupled plasma atomic emission spectrometry. The mass percentage of calcium in the negative electrode film is calculated by dividing the mass of the negative electrode film sample by the mass of the negative electrode film sample itself.
[0157] 4. Determination of the mass percentage of copper in the positive electrode active material The mass percentage of Cu in the positive electrode active material can be determined according to the general rule EPA 6010D-2014, using inductively coupled plasma atomic emission spectrometry. The mass percentage of Cu in the positive electrode active material is calculated by dividing the mass of Cu in the positive electrode active material sample by the mass of the positive electrode active material sample.
[0158] 5. First Coulomb Efficiency (First-Effect) Test After the battery is filled with electrolyte, it is charged to 4.0V at a constant current of 0.1C at 25℃, and then charged at a constant voltage of 4.0V until the current drops to 0.05C. This is recorded as the first charge capacity of the battery, C1. After standing for 5 minutes, it is discharged to 1.5V at a constant current of 0.1C. This is the first discharge capacity of the battery (C2). The first efficiency of the battery is = C2 / C1×100%.
[0159] 6. Battery cycle capacity retention rate At 25°C, the prepared battery was charged to 4.0V with a constant current of 1C, and then charged to 0.05C with a constant voltage of 4.0V. After standing for 5 minutes, it was discharged to 1.5V with a constant current of 1C. This is the first charge / discharge cycle of the battery, and the discharge capacity of this cycle is recorded as the discharge capacity of the battery in the first cycle (C0). The above steps were repeated for the same battery. The discharge capacity of the battery after 400 cycles (C1) was recorded. The capacity retention rate after 400 cycles is calculated as C1 / C0 × 100%.
[0160] III. Analysis of Test Results for Each Embodiment and Comparative Example Batteries for each embodiment and comparative example were prepared according to the above method, and various performance parameters were measured. The results are shown in the table below.
[0161] Table 1
[0162] Table 2
[0163] Table 3
[0164] Based on the above results, it can be seen that the sodium secondary batteries in Examples 1-26 all include a negative electrode sheet and an electrolyte. The negative electrode sheet includes a negative electrode film layer containing calcium. The electrolyte includes a first component, which is a fluorocarbonate compound.
[0165] As can be seen from the comparison between Examples 1-26 and Comparative Examples 1-3, sodium secondary batteries with a negative electrode film containing calcium and an electrolyte containing fluorinated carbonate compounds exhibit excellent cycle stability, low-temperature charging performance and first-time efficiency, as well as low volume expansion rate after high-temperature storage.
[0166] As can be seen from Examples 1 and 5-8, based on the total mass of the electrolyte, when the mass percentage (a) of the fluorocarbonate compound is 0.01%-10%, the sodium secondary battery exhibits low battery volume expansion rate after high-temperature storage, excellent low-temperature charging performance, first-efficiency performance, and cycle stability. When the mass percentage (a) of the fluorocarbonate compound is 0.2%-10%, the battery volume expansion rate after high-temperature storage, low-temperature charging performance, first-efficiency performance, and cycle stability of the sodium secondary battery can be further optimized.
[0167] As seen in Examples 1 and 9-12, based on the total mass of the negative electrode film, when the mass percentage (b) of calcium in the negative electrode film is 1ppm-3000ppm, the sodium secondary battery exhibits low battery volume expansion rate after high-temperature storage, excellent low-temperature charging performance, first-efficiency rating, and cycle stability. When the mass percentage (b) of calcium in the negative electrode film is 50ppm-1000ppm, the sodium secondary battery balances low battery volume expansion rate after high-temperature storage with even better low-temperature charging performance, first-efficiency rating, and cycle stability. As seen in Examples 1, 5-12, and 17, when a / b satisfies a / b≥1, the sodium secondary battery exhibits low battery volume expansion rate after high-temperature storage, excellent low-temperature charging performance, first-efficiency rating, and cycle stability. When a / b satisfies 10000≥a / b≥10, the sodium secondary battery balances low battery volume expansion rate after high-temperature storage with excellent low-temperature charging performance, first-efficiency rating, and cycle stability.
[0168] A comparison of Examples 1, 5, and 13-19 shows that, based on the total mass of the electrolyte, a mass percentage (c) of 0.01%-5% for difluorooxalate borate can reduce the battery volume expansion rate after high-temperature storage and improve the battery's low-temperature charging performance, first-efficiency performance, and cycle stability. A mass percentage (c) of 0.1%-2% for difluorooxalate borate can further reduce the battery volume expansion rate of sodium secondary batteries after high-temperature storage and improve the battery's low-temperature charging performance, first-efficiency performance, and cycle stability.
[0169] As seen in Examples 13-19, when c / a ≥ 0.001, the sodium secondary battery exhibits low battery volume expansion rate after high-temperature storage, excellent low-temperature charging performance, first-efficiency rating, and cycle stability. When c / a ≥ 2 ≥ c / a ≥ 0.1, the sodium secondary battery balances low battery volume expansion rate after high-temperature storage with even better low-temperature charging performance, first-efficiency rating, and cycle stability. As seen in Examples 1 and 20-23, based on the total mass of the positive electrode active material, when the mass percentage d of copper is 0%~23%, the sodium secondary battery exhibits low battery volume expansion rate after high-temperature storage, excellent low-temperature charging performance, first-efficiency rating, and cycle stability. When the mass percentage d of copper is 6.5%~18%, the sodium secondary battery balances low battery volume expansion rate after high-temperature storage with excellent low-temperature charging performance, first-efficiency rating, and cycle stability.
[0170] As can be seen from the comparison between Example 1 and Examples 24-26, the presence of a third component in the electrolyte can further optimize the battery volume expansion rate after high-temperature storage, low-temperature charging performance, first-efficiency performance, and cycle stability of sodium secondary batteries.
[0171] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A sodium secondary battery, comprising: The negative electrode sheet includes a negative electrode film layer containing calcium; and An electrolyte comprising a third component, the third component comprising one or more of sodium fluorosulfonate, maleic anhydride, and triallyl phosphate.
2. The sodium secondary battery according to claim 1, wherein, Based on the total mass of the negative electrode film, the mass percentage b of calcium in the negative electrode film is 1ppm to 3000ppm, and can be selected as 1000ppm to 3000ppm or 50ppm to 1000ppm.
3. The sodium secondary battery according to claim 1 or 2, wherein, Based on the total mass of the electrolyte, the mass percentage of the third component is 0.01% to 10%, and can be selected as 0.1% to 5%.
4. The sodium secondary battery according to any one of claims 1 to 3, wherein, The electrolyte includes a first component, which is a fluorocarbonate compound.
5. The sodium secondary battery according to claim 4, wherein, Based on the total mass of the electrolyte, the mass percentage a of the fluorocarbonate compound is 0.01% to 10%, and can be selected as 0.2% to 10%.
6. The sodium secondary battery according to claim 5, wherein, a is 0.2% to 5%, or optionally, a is 0.2% to 1%.
7. The sodium secondary battery according to any one of claims 4 to 6, wherein, Based on the total mass of the electrolyte, the mass percentage of the fluorocarbonate compound is a, and based on the total mass of the negative electrode film, the mass percentage of calcium in the negative electrode film is b, and a and b satisfy: a / b≥1; optionally, a and b satisfy: 10000≥a / b≥1; further optionally, a and b satisfy: 10000≥a / b≥10.
8. The sodium secondary battery according to any one of claims 4 to 7, wherein, The fluorocarbonate compounds include those shown in Formula I. Formula I Among them, R1, R2, R3, and R4 each independently include hydrogen atoms, halogen atoms, and carbon atoms. 1-6 hydrocarbon group, C 1-3 Haloalkyl, C 1-3 Alkoxy, C 1-3 At least one of haloalkoxy, ester, cyano, sulfonic acid, and isocyanate groups; and at least one of R1, R2, R3, and R4 is a fluorine atom.
9. The sodium secondary battery according to any one of claims 4 to 8, wherein, The fluorocarbonate compound includes at least one of the following compounds. Formula II-1 Formula II-2 Formula II-3 Formula II-4 Formula II-5 Formula II-6 Formula II-7 Formula II-8 Formula II-9 Formula II-10.
10. The sodium secondary battery according to claim 9, wherein, The fluorocarbonate compound includes at least one of formulas II-1, II-2, II-5, and II-10; Optionally, the fluorocarbonate compound includes formula II-1.
11. The sodium secondary battery according to any one of claims 4 to 10, wherein, The electrolyte further includes a second component, which is difluorooxalate borate, and the difluorooxalate borate satisfies at least one of the following conditions: Based on the total mass of the electrolyte, the mass percentage of difluorooxalate borate is c, and the mass percentage of the fluorocarbonate compound is a, where c and a satisfy: c / a ≥ 0.001; alternatively, 2 ≥ c / a ≥ 0.
1. Based on the total mass of the electrolyte, the mass percentage (c) of the difluorooxalate borate is 0.01%-5%; The option is 0.1%-2%; Optionally, the second component is sodium difluorooxalate borate.
12. The sodium secondary battery according to claim 11, wherein, The general chemical formula of the difluorooxalate borate is shown in Formula III. (F2C2O4B) y M-type III Wherein, M includes one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Fe, Ni, and Al, and y is 1, 2, or 3.
13. The sodium secondary battery according to any one of claims 1 to 12, wherein, The negative electrode film layer includes a negative electrode active material, which includes one or more of hard carbon, sodium metal, sodium-tin alloy, and metal oxide; optionally, the negative electrode active material includes hard carbon.
14. The sodium secondary battery according to any one of claims 1 to 13, wherein, The sodium secondary battery also includes a positive electrode sheet, which comprises a positive electrode active material, and the positive electrode active material comprises a sodium transition metal oxide.
15. The sodium secondary battery according to claim 14, wherein, The sodium transition metal oxide includes Na. m Cu n X o Fe p Mn q O 2-s, Where X includes one or more of Li, Be, B, Mg, Al, K, Ca, Ti, Co, Ni, Zn, Ga, Sr, Y, Nb, Mo, In, Sn, Fe, and Ba, 0≤m≤0.5, 0≤n≤0.5, 0≤o<0.5, 0≤p≤0.5, 0 <q≤0.68,n+o+p+q=1,0≤s<0.2; Optionally, the sodium transition metal oxide includes Na[Cu] 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2, Na 7 / 9 [Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, Na 9 / 10 [Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 At least one of O2.
16. The sodium secondary battery according to claim 14 or 15, wherein, The positive electrode active material also contains copper, and the mass percentage of copper, based on the total mass of the positive electrode active material, is 0.01% to 23%; optionally, it is 6.5% to 18%.
17. The sodium secondary battery according to any one of claims 1 to 16, wherein, The electrolyte includes a solvent, which includes one or more of the following: chain carbonates, chain carboxylic esters, cyclic carbonates, ether solvents, sulfone solvents, and nitrile solvents. Optionally, the chain carbonate includes one or more of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, methyl butyl carbonate, ethyl propyl carbonate, dipropyl carbonate, and dibutyl carbonate.
18. The sodium secondary battery according to claim 17, wherein, The solvent includes at least one of methyl ethyl carbonate and ethylene carbonate.
19. The sodium secondary battery according to any one of claims 1 to 18, wherein, The electrolyte comprises an electrolyte salt selected from one or more of NaPF6, NaBF4, NaN(SO2F)2 (NaFSI), NaClO4, NaAsF6, NaB(C2O4)2, NaBF2(C2O4), NaN(SO2RF)2, and NaN(SO2F)(SO2RF), wherein RF represents C x1 F 2x1+1 x1 is an integer between 1 and 10; optionally, RF is -CF3, -C2F5 or -CF2CF2CF3.
20. The sodium secondary battery according to claim 19, wherein, The electrolyte salt is selected from one or more of NaPF6, NaClO4, NaN(SO2F)2, NaN(CF3SO2)2, NaB(C2O4)2, and NaBF2(C2O4); optionally, the electrolyte salt is NaPF6.
21. An electrical device comprising a sodium secondary battery according to any one of claims 1 to 20.
Citation Information
Patent Citations
Pickerstick for use in weaving machines
EP0001563A1
Semiconductor device for resistance structures in high-density integrated circuits and method for making it