A monocrystalline lithium-ion battery and its preparation method
By employing a segmented baking and rapid cooling method, the problem of low oxalic acid retention in the baking process of lithium-ion batteries was solved, resulting in improved high-rate performance and long cycle life of lithium-ion batteries, especially enhanced stability under low and high temperature environments.
Patent Information
- Application Number
- CN202611252835.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-10
AI Technical Summary
The low retention rate of oxalic acid in the baking process of existing lithium-ion batteries prevents it from effectively fulfilling its potential interfacial modification function as a transition metal ion chelating agent, thus affecting the battery's wide temperature range, high rate capability, and long cycle performance.
A segmented baking process is adopted, including preheating and high-temperature short-time baking, combined with rapid cooling, to ensure that the chelating agent has a high retention rate distribution in the electrode coating and plays a chelating modification role during the formation stage, forming an insoluble chelate layer as the skeleton of the CEI membrane.
It significantly improves the retention rate of chelating agents, enhances the rate performance of batteries, strengthens low-temperature low-resistance, high-temperature stability and high-rate tolerance, extends the long cycle life at room temperature of 25℃ and slows down the degradation at -20℃/60℃.
Smart Images

Figure CN123073201A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery technology, and more specifically, to a single-crystal lithium-ion battery and its preparation method. Background Technology
[0002] With the rapid development of applications such as new energy vehicles, energy storage systems, and drones, the demand for comprehensive performance of lithium-ion batteries, including wide temperature range, high rate capability, and long cycle life, is becoming increasingly urgent. To optimize the interfacial stability between the cathode material and the electrolyte, the industry commonly adds oxalic acid as a functional additive during the electrode slurry homogenization stage. Its main functions include neutralizing the alkalinity of the slurry, inhibiting binder gelation, and chelating transition metal ions.
[0003] In current production processes, the baking process after electrode coating typically involves prolonged conveyor drying at temperatures ranging from 90℃ to 120℃ (usually lasting 3-12 minutes). However, the physicochemical properties of oxalic acid indicate that its sublimation initiation temperature is 100℃, with rapid sublimation occurring at 125℃. Under these conventional baking conditions, the actual retention rate of oxalic acid is typically below 40%, preventing it from effectively fulfilling its potential interfacial modification function as a transition metal ion chelating agent. Therefore, there is an urgent need to develop a new process that can effectively retain oxalic acid and enable it to fully participate in interfacial film formation during the formation stage, so as to achieve precise control of the cathode interface of single-crystal ternary materials, thereby comprehensively improving the wide temperature range, high rate and long cycle performance of lithium-ion batteries.
[0004] In view of this, the present invention is proposed. Summary of the Invention
[0005] The purpose of this invention is to provide a single-crystal lithium-ion battery and its preparation method to solve or improve the above-mentioned technical problems.
[0006] This invention is implemented as follows: In a first aspect, the present invention provides a method for preparing a single-crystal lithium-ion battery, comprising the following steps: The positive electrode slurry is coated and then baked to obtain the positive electrode sheet. A positive electrode, a negative electrode, an electrolyte, and a separator are assembled and subjected to formation treatment at 45℃-60℃ and 0.3MPa-1.0MPa to obtain a monocrystalline lithium-ion battery. The baking process includes: a first treatment at a temperature of 80℃-90℃ for 1.5min-2.5min; a second treatment at a temperature of 105℃-120℃ for 0.5min-1min; and then cooling the product after the second treatment to a temperature ≤60℃ within 30s.
[0007] In some embodiments, the raw materials of the cathode slurry, by mass percentage, consist of 94wt%-97wt% high-nickel ternary cathode material, 0.5wt%-3wt% first conductive agent, and 2wt%-4wt% first binder.
[0008] In some embodiments, the preparation of the cathode slurry also includes the addition of a chelating agent, the mass of which is 0.4%-0.7% of the total mass of the cathode slurry raw materials.
[0009] In some embodiments, the preparation of the positive electrode slurry also includes the addition of a first solvent, and the solid content of the positive electrode slurry is 70wt%-78wt%.
[0010] In an optional embodiment, the raw material for the positive electrode slurry has at least one of the following characteristics: Feature 1: The high-nickel ternary cathode material has D50 = 3μm-6μm, D10 = 1μm-3μm, and D90 = 9μm-11μm, with a specific surface area of 0.6m². 2 / g-0.8m 2 / g; Feature 2: The high-nickel ternary cathode material is selected from at least one of NCM811 and NCM622; Feature 3: The chelating agent is selected from at least one of oxalic acid, citric acid, and tartaric acid; Feature 4: By mass percentage, the first conductive agent comprises 1wt%-3wt% conductive carbon black and 0.5wt%-1wt% CNT; Feature 5: The first adhesive includes PVDF; Feature six: The first solvent includes NMP; when coating the positive electrode slurry, the areal density is 105 g / m³. 2 -120g / m 2 The compacted density is 3.0 g / cm³. 3 -3.8g / cm 3 .
[0011] In some embodiments, when preparing the negative electrode sheet, the raw materials of the negative electrode slurry are composed of 94wt%-96wt% dual-particle-size graphite, 1.5wt%-3wt% second conductive agent, 1wt%-3wt% second binder and 1wt%-2wt% thickener, by mass percentage. The dual-size graphite comprises 47wt%-49wt% primary graphite and 47wt%-49wt% secondary graphite.
[0012] In some embodiments, the preparation of the negative electrode slurry also includes the addition of a second solvent, and the solid content of the negative electrode slurry is 50wt%-58wt%.
[0013] In some embodiments, the raw materials for preparing the negative electrode slurry have at least one of the following characteristics: Feature 1: The first type of graphite has a D50 of 7μm-9μm and a specific surface area of 1.7m³. 2 / g-2.5m 2 / g; Second graphite D50 = 11μm-14μm, specific surface area is 1.5m². 2 / g-2.0m 2 / g; Feature 2: The second conductive agent is selected from at least one of conductive carbon black, carbon nanotubes, and graphene; Feature 3: The second binder is selected from at least one of SBR and polyacrylate; Feature 4: Thickeners include CMC; Feature 5: The second solvent is selected from at least one of pure water, ultrapure water, and distilled water; when coating the negative electrode slurry, the areal density is 55 g / m³. 2 -60g / m 2 The compacted density is 1.50 g / cm³. 3 -1.60g / cm 3 .
[0014] In some embodiments, the conductivity of the electrolyte is 10.0 mS / cm to 15.0 mS / cm; The electrolyte comprises, by mass percentage, 10wt%-15wt% LiPF6, 0.8wt%-1.2wt% LiBF4, 0.5wt%-1.0wt% PS, 1.0wt%-1.5wt% VC, and the balance being organic solvents; wherein the organic solvents comprise EC, DEC, and EMC in a volume ratio of (1.8-2.1):(2.9-3.2):(4.8-5.2).
[0015] In some embodiments, the diaphragm includes a PP base film with a thickness of 10 μm-13 μm, an Al2O3 ceramic layer with a thickness of 2.5 μm-3.5 μm, and a PVDF adhesive layer with a thickness of 2.5 μm-3.5 μm; the Al2O3 ceramic layer is located between the PP base film and the PVDF adhesive layer; Along the thickness direction, after the battery cell is assembled, the PP base film contacts the negative active layer of the negative electrode sheet, and the surface of the PVDF adhesive layer contacts the positive active layer of the positive electrode sheet.
[0016] In some embodiments, the formation process includes a first stage to a third stage, wherein the first stage is performed for 8 min to 12 min at a temperature of 53°C-56°C, a pressure of 0.4 MPa-0.6 MPa, and a current of 0.01 C. The second stage involves constant current charging for 160-200 minutes under conditions of 53℃-56℃, 0.4MPa-0.6MPa, and 0.05C. The third stage involves charging the battery to 68%-72% of its rated capacity under conditions of 53℃-56℃, 0.4MPa-0.6MPa, and 0.5C, at which point the formation charging is stopped. And / or, after the formation treatment, it also includes aging treatment at a temperature of 43℃-48℃ for 22h-25h, followed by aging treatment at room temperature for 22h-25h.
[0017] In some embodiments, during the baking process, cooling is performed using an air-cooled mode, and the gas used is selected from at least one of air, nitrogen, and helium.
[0018] In some implementations, the pressure of the baking equipment is maintained at -50 Pa to -200 Pa during cooling.
[0019] Secondly, the present invention provides a single-crystal lithium-ion battery, which is prepared by any of the preparation methods described in the foregoing embodiments.
[0020] The present invention has the following beneficial effects: The method for preparing a single-crystal lithium-ion battery provided by this invention involves baking the positive electrode sheet through preheating, short-time high temperature, and rapid cooling. Compared with the traditional long-time baking process, the chelating agent retention rate is significantly improved. The residual chelating agent plays a chelating modification role during the formation process, forming an insoluble chelate layer in situ with trace ions dissolved from the positive electrode surface. The chelate layer serves as the framework of the CEI film, which facilitates the deposition of electrolyte decomposition products in its gaps to form a dense composite film. This effectively reduces cell interface polarization, improves rate performance, and balances low-temperature low resistance, high-temperature stability, and high-rate tolerance. In addition, it can effectively suppress the dissolution of transition metal ions in high-nickel ternary positive electrode materials, significantly improve the long cycle life at 25°C, greatly reduce the decay at -20°C / 60°C, and enhance the high-rate cycle stability. Attached Figure Description
[0021] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 The results of the cyclic tests of Example 1 and Comparative Examples 1-3 at 25°C and 10°C are shown. Figure 2The results of the cyclic tests of Example 1 and Comparative Examples 1-3 at 60°C and 10°C are shown. Figure 3 The DCR results for Example 1 and Comparative Example 7 at 25°C and 50% SOC are shown. Figure 4 This is a schematic diagram of the separator and electrode structure during battery cell assembly. Figure 5 This is a schematic diagram of the assembled battery cell structure.
[0023] Icons: 1-Separator; 11-PP base film; 12-Al2O3 ceramic layer; 13-PVDF adhesive layer; 3-Negative electrode sheet; 31-First negative electrode active layer; 32-Negative electrode current collector; 33-Second negative electrode active layer; 5-Positive electrode sheet; 51-First positive electrode active layer; 52-Positive electrode current collector; 53-Second positive electrode active layer. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0025] Existing technologies have the following limitations: First, although chelating agents (such as oxalic acid) are added as processing aids, the residual amount after baking is insufficient, and they cannot fully participate in the chelation reaction on the positive electrode surface. Second, traditional formation process parameters (such as temperature and voltage curves) are not optimized for the kinetic conditions required for the oxalic acid-transition metal chelation reaction, resulting in low oxalate content and high interfacial impedance in the solid electrolyte interfacial film (CEI film), which in turn leads to problems such as a sharp drop in battery discharge voltage at low temperatures and accelerated capacity decay at high temperatures. Finally, although the industry-standard pressurized formation process can improve interfacial contact, it is not synergistically optimized with upstream process parameters such as oxalic acid addition and baking retention rate, resulting in uneven electrolyte wetting and poor interfacial film consistency, causing significant polarization during high-current charge and discharge and accelerating cycle performance degradation. This invention proposes the following technical solution to address the above deficiencies: In a first aspect, the present invention provides a method for preparing a single-crystal lithium-ion battery, comprising the following steps: The positive electrode slurry is coated and then baked to obtain the positive electrode sheet 5. The positive electrode 5, the negative electrode 3, the electrolyte and the separator 1 are assembled and subjected to formation treatment at 45℃-60℃ and 0.3MPa-1.0MPa to obtain a single crystal lithium-ion battery. The baking process includes: a first treatment at a temperature of 80℃-90℃ for 1.5min-2.5min; a second treatment at a temperature of 105℃-120℃ for 0.5min-1min; and then cooling the product after the second treatment to a temperature ≤60℃ within 30s.
[0026] It should be noted that in this embodiment of the invention, the conveyor belt speed during the baking process is 15m / min-20m / min, and the effective drying length of the oven is 45m-60m. In other embodiments of the invention, the conveyor belt speed and the effective drying length of the oven are reasonably selected according to actual needs.
[0027] The baking process employs a phased approach involving short-duration high temperature and rapid cooling. The chelating agent is fixed in the electrode coating with a high retention rate in the form of molecules, anions, and a small amount of salt. It is evenly distributed around the high-nickel ternary cathode material particles without undergoing pyrolysis, forming a pre-coordinated layer to ensure that it plays a full chelating modification role during the formation stage.
[0028] Specifically, the coated positive electrode slurry is baked in a three-stage process. Unlike the conventional high-temperature exposure that lasts for several minutes, this invention significantly shortens the residence time of the electrode in the high-temperature zone (105℃-120℃) to only 0.5min-1.0min, and then performs rapid cooling.
[0029] The first treatment, which takes place at a temperature of 80℃-90℃, is a preheating stage. The residence time in this stage is 1.5min-2.5min, which causes the positive electrode 5 to slowly heat up and evaporate most of the first solvent, thus preventing the chelating agent from sublimating in large quantities due to rapid heating.
[0030] The second treatment, conducted at a temperature of 105℃-120℃, is a high-temperature baking stage with a residence time of 0.5min-1.0min. At this temperature, the first solvent can evaporate rapidly, and the extremely short residence time significantly limits the sublimation loss of the chelating agent.
[0031] Air cooling was used to cool the product after the second treatment to ≤60℃ within 30 seconds, quickly terminating the continuous sublimation of the chelating agent. A slight negative pressure (-50Pa to -200Pa) was maintained throughout the oven to facilitate the removal of solvent vapors and reduce the residual time of oxalic acid in the high-temperature zone.
[0032] In some embodiments, the raw materials of the cathode slurry, by mass percentage, consist of 94wt%-97wt% high-nickel ternary cathode material, 0.5wt%-3wt% first conductive agent, and 2wt%-4wt% first binder.
[0033] In some embodiments, the preparation of the cathode slurry also includes the addition of a chelating agent, the mass of which is 0.4%-0.7% of the total mass of the cathode slurry raw materials.
[0034] It should be noted that oxalic acid is used as an example of a chelating agent. Oxalic acid partially dissociates into HC2O4 in the first solvent. - (Hydrooxate ion) and C2O4 2- (Oxalate ions) neutralize residual alkalis (such as LiOH, Li2CO3) on the surface of high-nickel ternary cathode materials, purifying the cathode surface, reducing the pH of the cathode slurry, and inhibiting the gelation of the first binder; at the same time, some oxalate ions are adsorbed on the surface of high-nickel ternary cathode materials to form a pre-coordinated layer.
[0035] Adding the chelating agent during the homogenization stage of the positive electrode slurry helps to neutralize the residual alkali in the positive electrode slurry and purify the surface of the positive electrode sheet 5.
[0036] Oxalate ions react with trace amounts of ions (such as Ni) dissolved from the surface of the positive electrode 5 during the initial formation process. 2+ Co 2+ Mn 2+ An insoluble oxalate chelate layer is generated in situ, which serves as the framework of the CEI film. Electrolyte decomposition products (such as LiF) are deposited in the gaps to form a dense composite film, which can effectively reduce cell interface polarization, improve rate performance, and take into account low temperature and low resistance, high temperature stability and high rate tolerance.
[0037] In addition, the oxalate chelate layer forms a physical barrier layer by covering the surface of the positive electrode 5; the in-situ fixation of dissolved ions promotes the coordination balance of the chelating agent; the interfacial chemical environment regulation helps to reduce HF corrosion. The three mechanisms work synergistically to effectively inhibit the dissolution of transition metal ions in the high-nickel ternary positive electrode material, thereby significantly improving the long cycle life at room temperature of 25℃, greatly slowing down the decay at -20℃ / 60℃, and enhancing the high-rate cycle stability.
[0038] For example, the mass ratio of the chelating agent to the total mass of the cathode slurry raw materials can be selected from any one of 0.4%, 0.5%, 0.6% and 0.7%, or other values in the range of 0.4% to 0.7%.
[0039] In some embodiments, the preparation of the positive electrode slurry also includes the addition of a first solvent, and the solid content of the positive electrode slurry is 70wt%-78wt%.
[0040] It should be noted that the embodiments of the present invention do not impose a particular limitation on the solid content of the cathode slurry, and can be reasonably adjusted within a set range according to different equipment and processes. For example, the solid content of the cathode slurry can be selected from any one of 70wt%, 72wt%, 73wt%, 75wt%, 76wt%, and 78wt%, or other values within the range of 70wt%-78wt%.
[0041] The solid content of the cathode slurry is adjusted according to different processes. The formula for calculating the solid content is: Cathode slurry solid content (%) = total weight of first dry powder / total weight of cathode slurry × 100% composition; the first dry powder includes: high-nickel ternary cathode material, first conductive agent, first binder and chelating agent; total weight of cathode slurry = mass of first dry powder + mass of first solvent.
[0042] In an optional embodiment, the raw material for the positive electrode slurry has at least one of the following characteristics: Feature 1: The high-nickel ternary cathode material has D50 = 3μm-6μm, D10 = 1μm-3μm, and D90 = 9μm-11μm, with a specific surface area of 0.6m². 2 / g-0.8m 2 / g; High-nickel ternary cathode materials have the characteristics of single crystal structure, high crystallinity, and layered order.
[0043] Feature 2: The high-nickel ternary cathode material is selected from at least one of NCM811 and NCM622; it belongs to the high-nickel active material category. The chemical formula of NCM811 is LiNi. 0.8 Co 0.1 Mn 0.1 O2, NCM622 has the chemical formula LiNi 0.6 Co 0.2 Mn 0.2 O2.
[0044] Feature 3: The chelating agent is selected from at least one of oxalic acid, citric acid and tartaric acid; when other chelating agents (such as citric acid and tartaric acid) are added, the chelating effect is weak, the high temperature stability is poor, and the wide temperature range performance is not as good as that of oxalic acid.
[0045] Feature 4: By mass percentage, the first conductive agent comprises 1wt%-3wt% conductive carbon black and 0.5wt%-1wt% CNT; Feature 5: The first adhesive includes PVDF; Feature six: The first solvent includes NMP; when coating the positive electrode slurry, the areal density is 105 g / m³. 2 -120g / m 2 The compacted density is 3.0 g / cm³. 3 -3.8g / cm 3 .
[0046] In some embodiments, when preparing the negative electrode sheet 3, the raw materials of the negative electrode slurry are composed of 94wt%-96wt% dual-particle-size graphite, 1.5wt%-3wt% second conductive agent, 1wt%-3wt% second binder and 1wt%-2wt% thickener, by mass percentage. The dual-size graphite comprises 47wt%-49wt% primary graphite and 47wt%-49wt% secondary graphite.
[0047] The dual-particle-size graphite used in the embodiments of the present invention is compounded to form a multi-level stacked structure, which takes into account both high-rate ion channels and structural stability, and is beneficial to improving low-temperature discharge at -20℃, high-rate charge and discharge and cycle stability.
[0048] In some embodiments, the preparation of the negative electrode slurry also includes the addition of a second solvent, and the solid content of the negative electrode slurry is 50wt%-58wt%.
[0049] It should be noted that the embodiments of the present invention do not impose a particular limitation on the solid content of the negative electrode slurry, and can be reasonably adjusted within a set range according to different equipment and processes. For example, the solid content of the negative electrode slurry can be selected from any one of 50wt%, 52wt%, 54wt%, 55wt%, 56wt%, and 58wt%, or other values within the range of 50wt%-58wt%.
[0050] The solid content of the negative electrode slurry is adjusted according to different processes: solid content of negative electrode slurry (%) = total weight of second dry powder / total weight of negative electrode slurry × 100% composition; the second dry powder includes: dual-particle-size graphite, second conductive agent, second binder and thickener; total weight of negative electrode slurry = mass of second dry powder + mass of second solvent.
[0051] In some embodiments, the raw materials for preparing the negative electrode slurry have at least one of the following characteristics: Feature 1: The first type of graphite has a D50 of 7μm-9μm and a specific surface area of 1.7m³. 2 / g-2.5m 2 / g; Second graphite D50 = 11μm-14μm, specific surface area is 1.5m². 2 / g-2.0m 2 / g; Feature 2: The second conductive agent is selected from at least one of conductive carbon black, carbon nanotubes, and graphene; Feature 3: The second binder is selected from at least one of SBR and polyacrylate; Feature 4: Thickeners include CMC; Feature 5: The second solvent is selected from at least one of pure water, ultrapure water, and distilled water; when coating the negative electrode slurry, the areal density is 55 g / m³.2 -60g / m 2 The compacted density is 1.50 g / cm³. 3 -1.60g / cm 3 The second solvent is water, and the negative electrode slurry belongs to an aqueous system, which is beneficial for enhancing interfacial wettability.
[0052] In some embodiments, the conductivity of the electrolyte is 10.0 mS / cm to 15.0 mS / cm; The electrolyte comprises, by mass percentage, 10wt%-15wt% LiPF6, 0.8wt%-1.2wt% LiBF4, 0.5wt%-1.0wt% PS, 1.0wt%-1.5wt% VC, and the balance being organic solvents; wherein the organic solvents comprise EC, DEC, and EMC in a volume ratio of (1.8-2.1):(2.9-3.2):(4.8-5.2).
[0053] It should be noted that the mass percentage of each substance in the electrolyte and the volume ratio of the organic solvent should be set reasonably according to actual needs.
[0054] In some embodiments, the diaphragm 1 includes a PP base film 11 with a thickness of 10 μm-13 μm, an Al2O3 ceramic layer 12 with a thickness of 2.5 μm-3.5 μm, and a PVDF adhesive layer 13 with a thickness of 2.5 μm-3.5 μm; the Al2O3 ceramic layer 12 is located between the PP base film 11 and the PVDF adhesive layer 13. Along the thickness direction, after assembly, the PP base film 11 contacts the negative active layer of the negative electrode 3, and the surface of the PVDF adhesive layer 13 contacts the positive active layer of the positive electrode 5. A schematic diagram of the assembled cell structure is shown below. Figure 5 .
[0055] Specifically, the schematic diagram of the assembled battery cell only shows a portion of it to illustrate its positional relationship. Along the thickness direction, the structure consists of the negative electrode, which includes a first negative electrode active layer 31, a negative electrode current collector 32, and a second negative electrode active layer 33; the separator 1, which includes a PP base film 11, an Al2O3 ceramic layer 12, and a PVDF adhesive layer 13; and the positive electrode, which includes a first positive electrode active layer 51, a positive electrode current collector 52, and a second positive electrode active layer 53.
[0056] It should be noted that the orientation or positional relationship indicated by "first" and "second" above is based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship that the product is usually placed in during use. It is only for the purpose of facilitating the description of the embodiments of the present invention and simplifying the description, and is not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, it should not be construed as a limitation on the product.
[0057] In some embodiments, the formation process includes a first stage to a third stage, wherein the first stage is performed for 8 min to 12 min at a temperature of 53°C-56°C, a pressure of 0.4 MPa-0.6 MPa, and a current of 0.01 C. The second stage involves constant current charging for 160-200 minutes under conditions of 53℃-56℃, 0.4MPa-0.6MPa, and 0.05C. The third stage involves charging the battery to 68%-72% of its rated capacity under conditions of 53℃-56℃, 0.4MPa-0.6MPa, and 0.5C, at which point the formation charging is stopped. And / or, after the formation treatment, it also includes aging treatment at a temperature of 43℃-48℃ for 22h-25h, followed by aging treatment at room temperature for 22h-25h.
[0058] It should be noted that the formation process is carried out in stages. In the initial stage, a small current is beneficial for the full dissociation of oxalic acid and the smooth completion of the chelation reaction. In the later stage, the current is increased to carry out the conventional formation film-forming process. This avoids excessive current in the initial stage, which could cause violent interfacial reactions and rapid consumption of oxalic acid, thus ensuring the integrity and uniformity of the film.
[0059] In the formation process, chelating agents are explained using oxalic acid as an example: After the electrolyte is injected, it is placed in an environment of 45°C for immersion and settling. After settling, it enters the formation treatment. During the formation treatment, oxalic acid rapidly dissociates into C2O4 under the action of an electric field. 2- Under the influence of an electric field, negatively charged C2O4... 2- Migrating towards the positive electrode surface, and reacting with trace ions dissolved from the positive electrode surface, such as Ni. 2+ Co 2+ Mn 2+ When a bidentate chelation coordination reaction occurs, an insoluble oxalate chelate layer (such as NiC2O4, CoC2O4, MnC2O4) is generated in situ. This layer is chemically bonded to the positive electrode surface and serves as the inner framework of the CEI film. At the same time, electrolyte decomposition products (LiF, Li2CO3, etc.) fill the gaps in the framework, forming a low-impedance, wide-temperature-range stable composite CEI film. This can effectively reduce cell interface polarization, which is beneficial to improving rate performance and takes into account low resistance at low temperatures, high temperature stability, and high rate tolerance.
[0060] In some embodiments, during the baking process, cooling is performed using an air-cooled mode, and the gas used is selected from at least one of air, nitrogen, and helium.
[0061] In some implementations, the pressure of the baking equipment is maintained at -50 Pa to -200 Pa during cooling.
[0062] The air-cooling mode can rapidly lower the temperature and stop the continuous sublimation of the chelating agent. During the baking process, a slight negative pressure is maintained throughout the oven to facilitate the discharge of the first and second solvent vapors and reduce the residual time of the chelating agent in the high-temperature zone.
[0063] In some embodiments, the current collectors of the positive electrode 5 and the negative electrode 3 of the present invention are independently selected from any one of aluminum foil, copper foil, carbon-coated aluminum foil and carbon-coated copper foil, respectively, according to actual needs.
[0064] Secondly, the present invention provides a single-crystal lithium-ion battery, which is prepared by any of the preparation methods described in the foregoing embodiments.
[0065] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0066] Example 1 This embodiment provides a monocrystalline lithium-ion battery, the preparation method of which includes the following steps: 1.1 Preparation of positive electrode sheet 5 The positive electrode paste is coated onto the surface of the aluminum foil current collector, and then baked to obtain the positive electrode sheet 5. The cathode slurry raw materials, by mass percentage, include: high-nickel ternary cathode material NCM622 (D50=4.5μm, specific surface area of 0.7m²). 2 95wt% ( / g), first conductive agent (2wt% conductive carbon black and 0.5wt% CNT) and first binder (2.5wt% PVDF); The chelating agent (oxalic acid) is added during the homogenization stage, and its dosage is 0.5% of the total amount of the positive electrode slurry raw materials.
[0067] The cathode slurry was prepared using the first solvent (NMP), resulting in a solid content of 75 wt% and an areal density of 110 g / m³. 2 The compacted density is 3.4 g / cm³. 3 A 2mm wide hydrated alumina insulating layer is coated on the edge of the electrode.
[0068] The baking process includes: a first treatment at 83°C for 2 minutes; a second treatment at 110°C for 1 minute; and then, cooling the product after the second treatment to ≤60°C within 30 seconds using a dry air cooling mode.
[0069] 1.2 Preparation of negative electrode sheet 3 By mass percentage, the raw material for the negative electrode slurry consists of dual-particle-size graphite (first graphite (D50=8μm, specific surface area 2.2m²)). 2 / g) 47.9wt%, second graphite (D50=12μm, specific surface area of 1.8m) 2 It consists of 47.9 wt% (g), a second conductive agent (1.7 wt% conductive carbon black), a second binder (1.5 wt% SBR), and a thickener (1.0 wt% CMC).
[0070] The negative electrode slurry is prepared using a second solvent (deionized water) and then coated with an aqueous coating. The solid content of the negative electrode slurry is 55 wt%, and the surface density of the single-sided coating is 58 g / m². 2 The compacted density is 1.55 g / cm³. 3 .
[0071] 1.3 Preparation of the diaphragm 1 The diaphragm 1 includes a 12μm PP base film 11, a 3μm PVDF adhesive layer 13 and a 3μm Al2O3 ceramic layer 12, wherein the Al2O3 ceramic layer 12 is located between the PP base film 11 and the PVDF adhesive layer 13.
[0072] 1.4 Preparation of electrolyte The electrolyte comprises, by mass percentage, 12 wt% LiPF6, 1 wt% LiBF4, 0.8 wt% PS, 1.2 wt% VC and the balance organic solvent (EC / DEC / EMC volume ratio of 2:3:5); the conductivity of the electrolyte is 12.0 mS / cm.
[0073] 1.5 Assembly and Formation Treatment (1) Assembly Assembly includes the following steps: The cell lamination process involves stacking the positive electrode 5, negative electrode 3 (cut to the designed dimensions), and composite separator 1 in a Z-shaped staggered arrangement. During stacking, the orientation of the separator 1 is strictly controlled: the PP base film 11 side adheres to the surface of the negative electrode 3, the PVDF adhesive layer 13 side adheres to the surface of the positive electrode 5, and the Al2O3 ceramic layer 12 is positioned between the PP base film 11 and the PVDF adhesive layer 13 as an insulating barrier layer. After stacking to the designed number of layers, a high-temperature terminating adhesive is used to fix the sides of the cell body, resulting in a neat bare cell. A schematic diagram of the separator 1 and electrode structure during cell assembly is shown below. Figure 4 A schematic diagram of the assembled battery cell structure can be found here. Figure 5 .
[0074] It should be noted that when assembling the battery cell, the separator 1 is continuously folded along the thickness direction to form multiple U-shaped bends and multiple parallel segments; electrode sheets are placed between adjacent parallel segments. The electrode sheets include multiple positive electrode sheets 5 and multiple negative electrode sheets 3, which are arranged alternately along the thickness direction, and the two outermost electrode sheets are both negative electrode sheets 3.
[0075] For electrode welding and insulation protection, the positive current collector electrode and aluminum lead electrode of the bare cell prepared above are connected by ultrasonic welding process, and the negative current collector electrode and nickel-plated copper lead electrode are connected by ultrasonic welding process. After welding, insulating tape is pasted at the root of the electrode and the edge of the package to isolate the electrode burrs from the aluminum layer of the aluminum-plastic film and avoid the risk of short circuit.
[0076] For aluminum-plastic film encapsulation, the aluminum-plastic film is first processed into a cavity that matches the size of the bare cell through a punching process. Then, the welded bare cell is placed inside the cavity, and the tab position is aligned with the encapsulation edge. The top edge and side edge are then heat-pressed and encapsulated in sequence using a heat-sealing mold, leaving only the liquid injection edge opening, to obtain a sealed semi-finished cell.
[0077] High-temperature vacuum baking removes moisture. The packaged semi-finished battery cells are placed in a vacuum oven and vacuum baked for 24 hours at a temperature of 85℃ and an absolute pressure of -95kPa to fully remove the trace amounts of moisture remaining in the electrodes and separator 1, ensuring the high-temperature cycling stability of the battery cells.
[0078] The packaged product was baked at 85°C and under a vacuum of -95 kPa for 24 hours; then it was injected with liquid at a liquid injection coefficient of 3.2 g / Ah.
[0079] Immediately after the electrolyte injection is completed, the injection port is pre-sealed once. Then, the cell is left to stand and soak at 45°C for 24 hours to ensure that the electrolyte fully wets the electrode plates and diaphragm pores.
[0080] (2) Chemical treatment The formation process includes three stages, with the first stage being a 10-minute treatment at a temperature of 55°C, a pressure of 0.5 MPa, and a current of 0.01 C. The second stage involves constant current charging for 180 minutes at a temperature of 55℃, a pressure of 0.5MPa, and a current of 0.05C. The third stage involves charging the battery to 70% of its rated capacity under conditions of 55℃, 0.5MPa, and 0.5C, at which point the formation charging process is stopped.
[0081] After the formation and charging process is completed, a negative pressure vacuum sealing process (secondary encapsulation) is performed to remove the side reaction gases generated inside the cell during the formation process, thus completing the final sealing of the aluminum-plastic film.
[0082] After final sealing, two aging treatments are performed sequentially: aging at 45℃ for 24 hours, and then aging at room temperature for 24 hours.
[0083] After the aging process is completed, the product undergoes testing, volume separation, and screening.
[0084] Example 2 This embodiment provides a single-crystal lithium-ion battery, the preparation method of which is the same as that in Embodiment 1, the only difference being: In step 1.1, the amount of chelating agent oxalic acid used in the preparation of positive electrode sheet 5 is 0.4% of the total amount of positive electrode slurry raw materials.
[0085] Example 3 This embodiment provides a single-crystal lithium-ion battery, the preparation method of which is the same as that in Embodiment 1, the only difference being: In step 1.1, the amount of chelating agent oxalic acid used in the preparation of the positive electrode sheet 5 is 0.7% of the total amount of the positive electrode slurry raw materials.
[0086] Example 4 This embodiment provides a single-crystal lithium-ion battery, the preparation method of which is the same as that in Embodiment 1, the only difference being: In step 1.1, in the preparation of the positive electrode sheet 5, after the first treatment, the baking treatment is carried out at a temperature of 115℃ for a time of 0.6min for the second treatment.
[0087] Example 5 This embodiment provides a single-crystal lithium-ion battery, the preparation method of which is the same as that in Embodiment 1, the only difference being: In step 1.1, after the first baking treatment in the preparation of the positive electrode sheet 5, the second treatment is carried out at a temperature of 105℃ for 1 min.
[0088] Example 6 This embodiment provides a single-crystal lithium-ion battery, the preparation method of which is the same as that in Embodiment 1, the only difference being: In step 1.5 assembly and formation treatment, the temperature of the first to third stages of formation treatment is 60℃.
[0089] Comparative Example 1 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.1, the preparation of the positive electrode sheet 5, the baking process adopts a continuous multi-temperature zone baking process with a conventional conveyor belt speed (15m / min-20m / min). The oven is set with 6 gradient temperature zones, with temperatures of 90℃, 100℃, 115℃, 120℃, 110℃, and 90℃ respectively. The total residence time in the temperature zone of 100℃ and above is about 1.5min-2min. The oven outlet adopts natural circulating air for slow cooling. It takes more than 90s to cool the electrode sheet to below 60℃.
[0090] It should be noted that the dwell time in the temperature range of 100℃ and above is related to the belt speed and should be adjusted reasonably according to the actual belt speed.
[0091] Comparative Example 2 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.5 assembly and formation treatment, the temperature of the first to third stages of formation treatment is 45℃.
[0092] Comparative Example 3 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.1, during the preparation of the positive electrode sheet 5, no chelating agent oxalic acid was added during the homogenization stage.
[0093] Comparative Example 4 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.1, the amount of chelating agent oxalic acid used in the preparation of the positive electrode sheet 5 is 0.2% of the total amount of the positive electrode slurry raw materials.
[0094] Comparative Example 5 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.1, the amount of chelating agent oxalic acid used in the preparation of the positive electrode sheet 5 is 1.0% of the total amount of the positive electrode slurry raw materials.
[0095] Comparative Example 6 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.1, the preparation of the positive electrode sheet 5 involves baking after the first treatment, followed by a second treatment at a temperature of 110°C for 3 minutes.
[0096] Comparative Example 7 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.1, the preparation of the positive electrode sheet 5 involves baking after the first treatment, followed by a second treatment at a temperature of 95°C for 1 minute.
[0097] Comparative Example 8 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.1, in the preparation of the positive electrode sheet 5, after the first treatment, the baking treatment is carried out at a temperature of 130℃ for a time of 0.5 min for the second treatment.
[0098] Comparative Example 9 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.1, the preparation of the positive electrode sheet 5 involves baking the product after the second treatment to cool naturally to a temperature ≤60℃.
[0099] Comparative Example 10 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.5 assembly and formation treatment, the pressure in the first to third stages of formation treatment is 0 Pa.
[0100] Comparative Example 11 This comparative example provides a single-crystal lithium-ion battery, whose preparation method is the same as that in Example 1, except that: In step 1.2, the graphite in the raw material of the negative electrode slurry has a single particle size, D50=10μm.
[0101] Test Example 1 This test example performs performance tests on the monocrystalline lithium-ion batteries prepared in Examples 1-6 and Comparative Examples 1-11, respectively. The test items are as follows: (1) Oxalic acid retention rate In the same batch of coating, a blank control slurry without oxalic acid was set up, and control electrode sheets were prepared under the same coating and baking conditions. Samples from both the experimental and blank control electrode sheets were taken using a wafer punching machine and weighed on a balance for calculation. Oxalic acid retention rate (%) = [(m1–m0) / m2]×100% (Equation 1); In Equation 1, m1 represents the mass of the electrode sampled from the experimental group (with added oxalic acid) after baking, in g; m0 represents the mass of the electrode sampled from the blank control group (without oxalic acid) after baking, in g; and m2 represents the total mass of the added oxalic acid, in g. Three cells were tested in parallel for each sample, and the arithmetic mean was taken. The relevant results are shown in Table 1.
[0102] Table 1 Oxalic acid retention rate and rate performance
[0103] Note: " / " in the table indicates that oxalic acid was not added.
[0104] (2) Rate charging performance test (5C charging retention rate) The test was conducted under constant temperature conditions of 25℃±2℃. First, the battery was charged at a constant current and constant voltage of 0.5C to 4.2V, with the 0.05C cutoff point, and allowed to stand for 10 minutes. Then, it was discharged at a constant current of 0.5C to 3V, and the 0.5C discharge capacity was recorded (as the baseline capacity). Next, the battery was charged at a constant current and constant voltage of 0.5C to 4.2V, with the 0.05C cutoff point, and allowed to stand for 10 minutes. Then, it was charged at a constant current of 5C to 4.2V, and the 5C charge capacity was recorded. The 5C charge retention rate was calculated using Equation-2. 5C charge retention rate (%) = (5C charge capacity / 0.5C discharge capacity) × 100% (Equation 2); where, 3 cells were tested in parallel for each sample, and the arithmetic mean was taken. The relevant results are shown in Table 1.
[0105] (3) Rate discharge performance test (10C discharge retention rate) The test was conducted under constant temperature conditions of 25℃±2℃. First, the battery was charged at a constant current and constant voltage of 0.5C to 4.2V, with the 0.05C cutoff point, and allowed to stand for 10 minutes. Then, it was discharged at a constant current of 0.5C to 3V, and the 0.5C discharge capacity was recorded (as the baseline capacity). Next, the battery was charged at a constant current and constant voltage of 0.5C to 4.2V, with the 0.05C cutoff point, and allowed to stand for 10 minutes. Then, it was discharged at a constant current of 10C to 3V, and the 10C discharge capacity was recorded. The 10C discharge retention rate was calculated using Equation-3. 10C discharge retention rate (%) = (10C discharge capacity / 0.5C discharge capacity) × 100% (Equation 3); 3 cells were tested in parallel for each sample, and the arithmetic mean was taken. The relevant results are shown in Table 1.
[0106] (4) Low temperature discharge The test was conducted under constant temperature conditions of -20℃±2℃. First, the battery was charged at a constant current and constant voltage of 0.5C to 4.2V, with the 0.05C cutoff point, and allowed to stand for 10 minutes. Then, it was discharged at a constant current of 0.5C to 3V, and the 0.5C discharge capacity was recorded (as the baseline capacity). Next, the battery was charged at a constant current and constant voltage of 0.5C to 4.2V, with the 0.05C cutoff point, and allowed to stand for 10 minutes. Then, it was discharged at a constant current of 5C to 3V, and the 5C discharge capacity was recorded. The low-temperature 5C discharge retention rate was calculated using Equation-4. Low-temperature 5C discharge retention rate (%) = (5C discharge capacity / 0.5C discharge capacity) × 100% (Equation 4); Three batteries were tested in parallel for each sample, and the arithmetic mean was taken. The relevant results are shown in Table 1.
[0107] (5) Cyclic test at room temperature (25℃) Charge the capacitor to 4.2 V using a constant current and constant voltage of 10C, cut off at 0.05C, and let it rest for 10 min. Then discharge it to 3 V using a constant current of 10C and let it rest for 10 min. This constitutes one cycle. Record the discharge capacity (C0) of the first cycle, and repeat the above charge-discharge process. After 500 cycles, record the remaining capacity (C0) after 500 cycles. 500 ). Calculate the capacity retention rate after 500 cycles using Equation-5: Capacity retention rate (%) = (C 500 / C0)×100% (Formula-5).
[0108] In Equation 5, C0 is the discharge capacity of the first cycle, C 500 The remaining capacity after 500 cycles is shown in Table 2; the relevant results of capacity retention are shown in Table 2; the cycle test results of Example 1 and Comparative Examples 1-3 at 25°C and 10°C are shown in Table 2. Figure 1 .
[0109] (6) High temperature 10C cycle test (60℃, 500 cycles capacity retention rate) The test was conducted in a constant temperature chamber at 60℃±2℃. The capacitor was charged at a constant current and constant voltage of 10C to 4.2V, cut off at 0.05C, and allowed to stand for 10 min. Then it was discharged at a constant current of 10C to 3V and allowed to stand for 10 min. This constituted one cycle, and the discharge capacity (C0) of the first cycle was recorded. The above charge-discharge process was repeated. After 500 cycles, the remaining capacity (C0) after 500 cycles was recorded. 500 ). Calculate the capacity retention rate after 500 cycles using Equation-6: Capacity retention rate (%) after 500 cycles at 60℃ (10°C) = (C) 500 _60 / C0_60)×100% (Equation-6); In Equation 6, C0_60 is the first cycle discharge capacity at 60℃; C 500 _60 represents the remaining capacity after 500 cycles at 60℃; 3 cells were tested in parallel for each sample, and the arithmetic mean was taken.
[0110] The results of capacity retention are shown in Table 2; the cycling test results of Example 1 and Comparative Examples 1-3 at 60°C and 10°C are shown in Table 2. Figure 2 .
[0111] Table 2 Cyclic Performance
[0112] (7) DC internal resistance (DCR) test The test was conducted in a constant temperature chamber at 25℃±2℃. Taking Example 1 and Comparative Example 7 as examples, the battery cell was first activated by one standard charge-discharge cycle, and then adjusted to 50% SOC. After that, it was left to stand for 60 minutes until the open circuit voltage of the battery cell stabilized, and the open circuit voltage V0 before the test was recorded. A constant current of 1C was discharged for 10 seconds, and the discharge current was recorded as I. The battery cell voltage V1 at the 10th second was recorded. The battery cell was left to stand for at least 30 minutes to allow the voltage to return to the open circuit state. The discharge DC internal resistance DCR was calculated according to Equation-7: DCR = (V0 - V1) / I (Equation 7); In Equation 7, V0 is the open-circuit voltage, V1 is the cell voltage at time 10s, and I is the discharge current; 3 cells were tested in parallel for each sample, and the arithmetic mean was taken. The DCR results of Example 1 and Comparative Example 7 under 25℃ and 50% SOC conditions are shown in [reference needed]. Figure 3 .
[0113] As can be seen from the above, combining the data in Tables 1 and 2, and... Figure 1-3 It can be seen that Example 1 performs excellently at three temperatures: 25℃, 60℃, and -20℃. Detailed analysis is as follows: Among them, when comparing Examples 1-3 with Comparative Examples 4-5, the product performance was excellent when the oxalic acid addition was in the range of 0.4%-0.7%, with 0.5% being the optimal value.
[0114] Compared with Comparative Examples 6-9, Examples 1 and 4-5, with a high temperature of 105℃-120℃, a dwell time of 0.5min-1.0min, and rapid cooling, can achieve an oxalic acid retention rate of 65%-78%, which is significantly better than traditional long-time baking (Comparative Example 1, 41.01%).
[0115] In Comparative Example 7, the temperature in the high-temperature region was reduced to 95°C, which led to insufficient evaporation of NMP solvent, increased interfacial impedance, and decreased rate and cycle performance. The oxalic acid retention rate was improved, but the cell performance was relatively reduced. In addition, when the DCR was tested at 25°C and 50% SOC, the cell DCR was significantly higher than that of Example 1, further verifying that insufficient baking led to increased interfacial degradation.
[0116] Compared with Example 6 and Comparative Example 2, Example 1 showed similar formation performance at 55℃-60℃, and all were significantly better than Comparative Example 2.
[0117] Further comparison of Comparative Examples 1-3 shows that the traditional long-time segmented baking process and the 45℃ low-temperature formation process result in reduced performance, and the performance without oxalic acid addition is significantly reduced. Figure 1 ).
[0118] Compared with Comparative Example 11, the pressurized formation improved the 5C charge retention rate from 81.29% to 89.53% and the 10C discharge rate from 74.05% to 84.8%.
[0119] Compared with Comparative Example 3, Example 1 showed a decreasing trend in retention rates after 500 cycles at 10C / 10C and 60°C without oxalic acid.
[0120] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing a single-crystal lithium-ion battery, characterized in that, Includes the following steps: The positive electrode slurry is coated and then baked to obtain the positive electrode sheet. The positive electrode, negative electrode, electrolyte, and separator are assembled and subjected to formation treatment at 45℃-60℃ and 0.3MPa-1.0MPa to obtain a monocrystalline lithium-ion battery. The baking process includes: a first treatment at a temperature of 80℃-90℃ for 1.5min-2.5min; a second treatment at a temperature of 105℃-120℃ for 0.5min-1min after the first treatment; and then cooling the product after the second treatment to a temperature ≤60℃ within 30s.
2. The preparation method according to claim 1, characterized in that, The raw materials of the cathode slurry, by mass percentage, consist of 94wt%-97wt% high-nickel ternary cathode material, 0.5wt%-3wt% first conductive agent and 2wt%-4wt% first binder; And / or, when preparing the positive electrode slurry, a chelating agent is further added, wherein the mass of the chelating agent is 0.4%-0.7% of the total mass of the positive electrode slurry raw materials; And / or, when preparing the positive electrode slurry, the addition of a first solvent is also included, wherein the solid content of the positive electrode slurry is 70wt%-78wt%.
3. The preparation method according to claim 2, characterized in that, The raw materials of the positive electrode slurry have at least one of the following characteristics: Feature 1: The high-nickel ternary cathode material has D50 = 3μm-6μm, D10 = 1μm-3μm, and D90 = 9μm-11μm, with a specific surface area of 0.6m². 2 / g-0.8m 2 / g; Feature 2: The high-nickel ternary cathode material is selected from at least one of NCM811 and NCM622; Feature 3, the chelating agent is selected from at least one of oxalic acid, citric acid and tartaric acid; Feature 4: By mass percentage, the first conductive agent comprises 1wt%-3wt% conductive carbon black and 0.5wt%-1wt% CNT (carbon nanotubes). Feature 5: The first adhesive comprises PVDF; Feature six: the first solvent includes NMP; when coating the positive electrode slurry, the areal density is 105 g / m³. 2 -120g / m 2 The compacted density is 3.0 g / cm³. 3 -3.8g / cm 3 .
4. The preparation method according to claim 1, characterized in that, By mass percentage, when preparing the negative electrode sheet, the raw materials of the negative electrode slurry consist of 94wt%-96wt% dual-particle-size graphite, 1.5wt%-3wt% second conductive agent, 1wt%-3wt% second binder and 1wt%-2wt% thickener; Among them, the dual-grain size graphite includes 47wt%-49wt% first graphite and 47wt%-49wt% second graphite; And / or, when preparing the negative electrode slurry, a second solvent is also added, and the solid content of the negative electrode slurry is 50wt%-58wt%.
5. The preparation method according to claim 4, characterized in that, The raw materials for preparing the negative electrode slurry have at least one of the following characteristics: Feature one: The first graphite has a D50 of 7μm-9μm and a specific surface area of 1.7m³. 2 / g-2.5m 2 / g; the second graphite has a D50 of 11μm-14μm and a specific surface area of 1.5m². 2 / g-2.0m 2 / g; Feature 2, the second conductive agent is selected from at least one of conductive carbon black, carbon nanotubes and graphene; Feature 3, the second adhesive is selected from at least one of SBR and polyacrylate; Feature 4: The thickener includes CMC; Feature five: the second solvent is selected from at least one of pure water, ultrapure water, and distilled water; when the negative electrode slurry is coated, the areal density is 55 g / m³. 2 -60g / m 2 The compacted density is 1.50 g / cm³. 3 -1.60g / cm 3 .
6. The preparation method according to claim 1, characterized in that, The conductivity of the electrolyte is 10.0 mS / cm - 15.0 mS / cm; The electrolyte comprises, by mass percentage, 10wt%-15wt% LiPF6, 0.8wt%-1.2wt% LiBF4, 0.5wt%-1.0wt% PS, 1.0wt%-1.5wt% VC, and the balance being organic solvent; wherein the organic solvent comprises EC, DEC, and EMC in a volume ratio of (1.8-2.1):(2.9-3.2):(4.8-5.2).
7. The preparation method according to claim 1, characterized in that, The diaphragm comprises a PP base film with a thickness of 10μm-13μm, an Al2O3 ceramic layer with a thickness of 2.5μm-3.5μm, and a PVDF adhesive layer with a thickness of 2.5μm-3.5μm; the Al2O3 ceramic layer is located between the PP base film and the PVDF adhesive layer; Along the thickness direction, after the battery cell is assembled, the PP base film is in contact with the negative active layer of the negative electrode sheet, and the surface of the PVDF adhesive layer is in contact with the positive active layer of the positive electrode sheet.
8. The preparation method according to claim 1, characterized in that, The formation process includes three stages, wherein the first stage is performed for 8 min to 12 min under the conditions of a temperature of 53℃-56℃, a pressure of 0.4MPa-0.6MPa, and a current of 0.01C. The second stage involves constant current charging for 160-200 minutes under conditions of 53℃-56℃, 0.4MPa-0.6MPa, and 0.05C. The third stage involves charging the battery to 68%-72% of its rated capacity under conditions of 53℃-56℃, 0.4MPa-0.6MPa, and 0.5C, at which point the formation charging is stopped. And / or, after the formation treatment, the process further includes aging at a temperature of 43℃-48℃ for 22h-25h, followed by aging at room temperature for 22h-25h.
9. The preparation method according to claim 1, characterized in that, During the baking process, cooling is performed using an air-cooling mode, and the gas used is selected from at least one of air, nitrogen, and helium. And / or, during cooling, maintain the pressure of the baking equipment at -50 Pa to -200 Pa.
10. A monocrystalline lithium-ion battery, characterized in that, It is prepared by the preparation method described in any one of claims 1-9.