Seawater-based zinc-ion battery anode, its preparation method and battery

By using DMSO-modified MXene material to form an interfacial protective layer on the zinc substrate surface, the problem of easy failure of zinc anode in seawater environment is solved, and the long-term stability and high-efficiency energy storage performance of zinc-ion battery in seawater are achieved.

CN123073227APending Publication Date: 2026-11-10SANYA SCI & EDUCATION INNOVATION PARK WUHAN UNIV OF TECH
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
CN202611540091.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-10

Smart Images

  • Figure CN123073227A_ABST
    Figure CN123073227A_ABST
Patent Text Reader

Abstract

This invention discloses a seawater-based aqueous zinc-ion battery anode, its preparation method, and the battery itself, relating to the field of seawater-based aqueous zinc-ion battery technology. The anode comprises a zinc substrate and an interface protective layer loaded on the surface of the zinc substrate. The interface protective layer contains dimethyl sulfoxide (DMSO)-modified MXene material. DMSO adsorbs onto the MXene surface to form a hydrophobic barrier, which can inhibit the oxidation and degradation of MXene in seawater-based electrolytes, allowing the interface protective layer to maintain its structural integrity and conductivity over a long period, thereby inhibiting corrosion, hydrogen evolution, and dendrite growth of the zinc anode. Seawater-based aqueous zinc-ion batteries using this anode exhibit a long cycle life in seawater-based electrolytes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of seawater-based aqueous zinc-ion battery technology, and in particular to a seawater-based aqueous zinc-ion battery anode, its preparation method, and the battery itself. Background Technology

[0002] Seawater-based zinc-ion batteries directly utilize natural or simulated seawater as electrolytes, offering advantages such as intrinsic safety, low cost, and compatibility with marine environments. However, the zinc metal anode faces a stronger interface failure problem in seawater environments compared to conventional pure water zinc batteries, leading to rapid performance degradation.

[0003] Existing conventional Ti3C2T x MXene interface layers can improve zinc deposition behavior in pure aqueous zinc batteries due to their high conductivity, zinc-affinity end groups, and two-dimensional channels. However, in seawater systems, high concentrations of Cl... - SO4 2- The combined effects of dissolved oxygen and other factors can induce pitting corrosion of the zinc anode, hydrogen evolution side reactions, accumulation of basic salt byproducts, and dendrite growth. Simultaneously, unstabilized MXene is prone to water-induced oxidation in water-rich, oxygen-containing, and chlorine-containing environments, where surface or edge Ti atoms are oxidized to TiO2. This leads to conductive network degradation, lamellar structure collapse, sub-nanometer ion channel failure, and increased interfacial impedance, becoming a bottleneck restricting the long-term service life of seawater energy storage devices. Solving these problems to ensure that zinc-ion batteries maintain good performance in marine environments is a hot topic and a challenging area of ​​research in this field. Summary of the Invention

[0004] The purpose of this invention is to solve the problems of conventional Ti3C2T x To address the issues of easy oxidation of the MXene interface layer in seawater systems and the easy failure of the zinc anode, this invention provides a seawater-based zinc-ion battery anode. By loading highly antioxidant MXene, which is chemically modified on the surface of DMSO, onto the zinc substrate as an interface protective layer, the problem of easy oxidation and failure of the interface material is solved. The zinc anode has long-lasting anti-dendrite and anti-corrosion properties, and the prepared zinc-ion battery has good long-lasting stability and corrosion inhibition function in complex natural seawater systems at room temperature.

[0005] Previous studies have shown that MXene functional interfaces can effectively stabilize zinc anodes through physical barrier and ion regulation, significantly improving the cycle life of zinc batteries in pure aqueous electrolytes. However, the inventors discovered that directly coating conventionally prepared aqueous MXene onto zinc foil surfaces and applying it to natural seawater environments results in severe structural degradation and electrochemical failure. Specifically, although conventional MXene can initially provide some physical shielding, in complex, high-salt, and highly conductive seawater-based electrolyte environments, MXene nanosheets without antioxidant barriers are highly susceptible to intense nucleophilic attacks from free water molecules and dissolved oxygen. Unexpectedly, research revealed that DMSO-modified MXene materials can overcome the aforementioned defects of conventional MXene.

[0006] The first aspect of the present invention provides a seawater-based aqueous zinc-ion battery anode, the anode comprising a zinc substrate and an interface protective layer loaded on the surface of the zinc substrate, the interface protective layer comprising a dimethyl sulfoxide (DMSO) modified MXene material.

[0007] Preferably, the MXene material comprises Ti2CT x Ti3CNT x V2CT x Nb2CT x and Ti3C2T x At least one of them, more preferably Ti3C2T x Materials; the DMSO-modified MXene material has a layer thickness of 1~5nm and a layer spacing of 1.2~2.5nm after stacking.

[0008] The second aspect of the present invention provides a method for preparing a seawater-based aqueous zinc-ion battery anode, the method comprising: loading DMSO-modified MXene material onto the surface of a zinc substrate to form an interface protective layer, thereby obtaining a seawater-based aqueous zinc-ion battery anode.

[0009] Preferably, the loading method includes drop-coating an aqueous dispersion of the DMSO-modified MXene material onto the surface of the zinc substrate, allowing the DMSO-modified MXene material to electrostatically self-assemble on the zinc substrate surface to form the interface protective layer. Other loading methods include spraying, scraping, spin coating, and dip coating. The interface protective layer is suitable for both zinc foil electrodes and flexible negative electrodes.

[0010] Preferably, the MXene material is Ti3C2T. x Materials; the zinc substrate is zinc foil.

[0011] Preferably, the preparation method of the DMSO-modified MXene material includes: etching the Ti3AlC2MAX phase to obtain Ti3C2Tx ; Regarding the Ti3C2T x Intercalation, washing, and stripping processes were performed sequentially, with the intercalation occurring in a DMSO / H2O mixed solvent, to obtain the DMSO-modified MXene material.

[0012] Preferably, the etching method includes etching the Ti3AlC2MAX phase with an etchant to obtain the Ti3C2T phase. x The etching agent is an HF / HCl solution; The intercalation method includes: etching the obtained Ti3C2T x When mixed with the DMSO / H2O mixed solvent, 0.5~6g of Ti3C2T is added to every 30mL of the DMSO / H2O mixed solvent. x The lithium salt is added and stirred at room temperature for 12-24 hours for intercalation; the lithium salt is at least one of lithium chloride, lithium fluoride, and lithium hydroxide; preferably, the lithium salt is added simultaneously with the DMSO / H2O mixed solvent, that is, the lithium salt is first dissolved in the DMSO / H2O mixed solvent to prepare the intercalation solution, and then the etched Ti3C2T is added. x Intercalation is carried out by dispersing in the intercalation fluid, and the intercalation can be completed in one step; The stripping method includes: adding deionized water to the washed precipitate, and performing ultrasonic stripping under argon protection and ice-water bath conditions; centrifuging after ultrasonication, and taking the upper dispersion, which is the aqueous dispersion of DMSO-modified MXene material.

[0013] Preferably, in the DMSO / H2O mixed solvent, the volume percentage of DMSO is 50-90%; in the HF / HCl solution, the concentration of HF is 5-10 mol / L and the concentration of HCl is 2-6 mol / L.

[0014] The third aspect of the present invention provides a seawater-based aqueous zinc-ion battery anode prepared by the method described above.

[0015] A fourth aspect of the present invention provides a seawater-based aqueous zinc-ion battery, wherein the seawater-based aqueous zinc-ion battery comprises a seawater-based aqueous zinc-ion battery negative electrode as described above.

[0016] Preferably, the electrolyte of the seawater-based aqueous zinc-ion battery is an aqueous electrolyte obtained by dissolving zinc salts in seawater as a solvent; the seawater-based aqueous zinc-ion battery can be a Zn||Zn symmetric battery, a Zn||Cu asymmetric battery, or a full battery with manganese-based oxides as the positive electrode.

[0017] The battery can be prepared according to conventional methods in the art.

[0018] The seawater-based aqueous zinc-ion battery provided by this invention can be used in the following scenarios: Firstly, it enables on-site consumption of renewable energy in deep-sea areas and microgrid energy storage. Seawater-based zinc-ion batteries can directly utilize inexhaustible natural seawater as the electrolyte, effectively solving the problems of smooth output, peak-valley regulation, and on-site consumption of intermittent sea surface power such as offshore wind power, floating photovoltaic power, and marine biomass energy. Secondly, it addresses the independent power supply system for offshore exploration and island microgrids. For islands, coastal observation stations, deep-sea exploration buoys, and underwater unmanned equipment, traditional energy storage technologies face challenges such as difficulty in freshwater replenishment, susceptibility to salt spray corrosion, and high safety risks. The high-oxidation-resistant MXene interface-controlled energy storage device provided by this invention can significantly eliminate passive self-discharge and corrosion failure, ensuring long-term stable and safe operation of offshore or deep-sea off-grid equipment under harsh conditions without freshwater supply. Thirdly, it is an energy storage power source with high intrinsic safety for special scenarios. Compared with traditional consumer electronics or automotive lithium batteries, this technology eliminates the safety hazards of thermal runaway and flammability and explosion. It can maintain high intrinsic safety even in accident conditions such as immersion in water or impact, making it particularly suitable for special fields with the highest requirements for fire protection and explosion resistance in enclosed compartments, such as underwater equipment, marine engineering equipment, and offshore drilling platforms.

[0019] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: The present invention relates to a seawater-based zinc-ion battery anode, its preparation method, and the battery itself. DMSO-modified MXene material is used as the interface protective layer of the anode. The strong chemical adsorption and interaction between the strong polar bonds in the DMSO molecule and the active transition metal atoms on the MXene surface are utilized to construct a robust organic protection and hydrophobic barrier on its surface. This barrier, at the molecular scale, blocks nucleophilic attacks on the active transition metal sites by free water molecules, dissolved oxygen, and highly corrosive impurities in seawater. This solves the common problem of MXene's easy oxidation and deactivation in complex natural seawater and overcomes the interfacial compatibility challenge between the abundant end groups on the MXene surface and the zinc matrix. An anode interface protective layer based on the MXene framework is constructed in situ. The resulting zinc-ion battery exhibits good long-term stability and corrosion inhibition function in complex natural seawater systems at room temperature. Density functional theory calculations show that the adsorption energy of DMSO molecules on the MXene surface (-0.68 eV) is lower than that of H2O molecules (-0.33 eV). DMSO can preferentially adsorb onto the MXene surface in competitive adsorption with water molecules, providing a thermodynamic basis for the formation of the aforementioned barrier.

[0020] This invention utilizes an interfacial protective layer composed of DMSO-modified MXene material to achieve long-lasting anti-dendrying and anti-corrosion performance of the zinc anode through a triple synergistic mechanism of "electrostatic repulsion-electric field modulation-physical confinement". Thanks to the strong protection of the DMSO anti-oxidation barrier, MXene that has not undergone oxidative degradation can stably exert a multi-dimensional synergistic effect in seawater-based electrolytes for a long time: on the one hand, it utilizes the negatively charged polar functional groups on its surface to generate electrostatic repulsion, effectively shielding the highly corrosive Cl- in seawater. - With SO4 2- Anions are present, which simultaneously selectively attract and promote the activity of Zn. 2+ On the one hand, it facilitates rapid migration; on the other hand, it leverages the excellent conductivity of MXene to modulate the electric field, reconstructing and homogenizing the electric field distribution on the electrode surface, eliminating local high-field-strength hotspots, and inducing Zn... 2+ It achieves uniform flux and uniform deposition; furthermore, through the physical confinement effect of its two-dimensional layered structure, it suppresses the vertical penetration of dendrites at the physical source and effectively isolates free water at the interface to inhibit corrosion and hydrogen evolution side reactions. This multi-synergistic mechanism suppresses interfacial failure in complex seawater systems, prolongs the cycle life of the zinc anode in seawater-based electrolytes, and improves coulombic efficiency.

[0021] This invention confirms through systematic electrochemical testing and in-situ interface characterization that Zn in seawater-based electrolytes... 2+ Despite the drastic volume fluctuations caused by repeated deposition / stripping, the MXene interface protective layer not only maintained excellent structural integrity and mechanical self-adaptive properties but also significantly reduced electrode polarization impedance. The protected zinc anode significantly extended the stable cycle life of Zn‖Zn symmetric and Zn‖Cu asymmetric cells in natural seawater environments, maintaining high reversibility and extremely high coulombic efficiency during long cycles. Seawater-based full cells constructed under harsh real-world conditions with low N / P ratios and thin zinc foil also exhibited significantly improved long-term cycle stability.

[0022] The electrolyte in the battery of this invention does not require the use of organic solvents and lithium salts, nor does it require a complex seawater desalination system or a large freshwater reservoir, significantly reducing electrolyte costs and freshwater replenishment and maintenance costs. The modified interface greatly extends the service life of energy storage devices, improving the stable lifespan of symmetric batteries by more than 50 times, and the entire battery achieves a lifespan of 1.0 A·g. -1 Achieving 2000 long cycles under high current significantly reduces the frequency of replacement of offshore power grid facilities, which is conducive to reducing the levelized cost of energy storage throughout the entire life cycle of energy storage power stations. Attached Figure Description

[0023] Figure 1 This is a scanning electron microscope (SEM) image of the negative electrode (DM@Zn composite negative electrode) prepared in Example 1 of the present invention, wherein, Figure 1 a is a scanning electron microscope image of the negative electrode surface. Figure 1 b is a scanning electron microscope image of the negative electrode cross-section; Figure 2 The graph shows the characterization of the negative electrode prepared in Comparative Example 1 of this invention and its cycling performance in different electrolytes. Figure 2 a and Figure 2 b are scanning electron microscope images of the negative electrode before and after circulation in seawater-based electrolyte; Figure 2 c shows the Raman spectra of the negative electrode before and after cycling in seawater-based electrolyte. The blue area shows the appearance and enhancement of the characteristic peak of TiO2. Figure 2 d represents a zinc-symmetric cell, tested in deionized water-based and seawater-based electrolytes at 5 mA·cm⁻¹. -2 Current density and 1 mAh·cm -2 Constant current charge-discharge curves under constant current charge-discharge cycles at the areal capacity; Figure 2 e represents the X-ray diffraction patterns of the negative electrode before treatment and after treatment with deionized water-based electrolyte and seawater-based electrolyte, respectively. Figure 3 The graph shows the interface stability and electrochemical behavior of the negative electrode (DM@Zn composite negative electrode) prepared in Example 1 of this invention. Figure 3 a represents the initial state and the Ti 2p high-resolution X-ray photoelectron spectra of the negative electrode after aging in deionized water-based electrolyte DIW and seawater-based electrolyte NSW, respectively. Figure 3 b shows the X-ray diffraction patterns of the negative electrode in the initial state and after immersion in deionized water-based electrolyte DIW and seawater-based electrolyte NSW, respectively (the asterisks indicate the diffraction peaks on the zinc substrate, and the light blue shaded area shows the retention and evolution of the characteristic peaks of MXene (002)). Figure 3 c and 3d are the Tafel polarization curves and fitted corrosion current densities (i) of the negative electrodes prepared in Example 1, Comparative Example 1, and Comparative Example 2, respectively. corr Linear sweep voltammetry curves in 1 mol / L sodium sulfate solution (showing a significant extension of the overpotential of the hydrogen evolution reaction (HER)). Figure 3 e represents the electrochemical impedance spectroscopy of the zinc symmetric cells in Example 1, Comparative Example 1, and Comparative Example 2. Figure 3 f represents the current-time (it) curves of the negative electrode under constant potential in Example 1, Comparative Example 1, and Comparative Example 2, indicating that its nucleation and growth mode changes from infinite two-dimensional (2D) planar diffusion to confined and stable three-dimensional (3D) diffusion behavior. Figure 3 g is an Arrhenius-fitted linear relationship graph of the interface desolvation activation energy (Ea) calculated based on the temperature-dependent impedance of the negative electrode in Example 1, Comparative Example 1, and Comparative Example 2. Figure 3 h represents the zinc symmetric cells in Example 1, Comparative Example 1, and Comparative Example 2 at 5 mA·cm⁻¹. -2 High current density and 1mAh·cm-2 Long-cycle constant current charge-discharge cycle curves under harsh test conditions for areal capacity; Figure 4 The figures shown are of the zinc deposition behavior and reversibility test results of the negative electrodes prepared in Example 1 and the comparative example of the present invention. Figure 4 a represents the 3D white light interferometric laser surface profile and corresponding surface roughness (Sa) index of the negative electrode prepared in Comparative Example 2 and Example 1 before and after cycling. Figure 4 b represents the negative electrode prepared in Comparative Example 2, Comparative Example 1, and Example 1 at 5 mA·cm⁻¹. -2 Delayed in-situ cross-sectional optical microscopy image of the anode interface during 24 minutes of continuous deposition at high current density (the white dashed box marks the obvious protruding dendrite pillars on the bare zinc surface). Figure 4 c represents the Zn‖Cu asymmetric cells corresponding to Example 1 and Comparative Example 2 at 5 mA·cm⁻¹. -2 1mAh·cm -2 Coulomb efficiency diagram under the given conditions; Figure 4 d shows a comparison of the CV curves of the Zn‖Cu asymmetric cells corresponding to Example 1, Comparative Example 1, and Comparative Example 2 during the deposition / stripping cycle. Figure 4 e is a magnified comparison of the nucleation overpotentials of the negative electrodes of Example 1, Comparative Example 1, and Comparative Example 2 (the scale bar shows the differences in the initial nucleation energy barrier of each system). Figure 4 f、 Figure 4 g and Figure 4 h represents the in-situ relaxation time distribution (DRT) contour plots of the negative electrodes prepared in Comparative Example 2, Comparative Example 1 and Example 1, respectively, as they evolved over time during long-term electrochemical cycling tests. Figure 5 This invention serves as a verification of the electrochemical energy storage performance and commercial application conditions of the seawater-based aqueous full battery assembled with the negative electrode prepared in Example 1 and the comparative example of the present invention. Figure 5 a represents the concentrations in Example 1, Comparative Examples 1 and 2, ranging from 0.2 to 3.0 A·g. -1 Comparison of rate performance at different current densities; Figure 5 b is the constant current charge-discharge characteristic voltage-capacity curve of Comparative Example 1 under the corresponding rate gradient; Figure 5 c represents the constant current charge-discharge characteristic voltage-capacity curve of Comparative Example 2 under the corresponding rate gradient; Figure 5 d shows a comparison of the cyclic voltammetry (CV) characteristic curves of Example 1 and Comparative Example 2 (demonstrating higher response current and redox activation reversibility). Figure 5 e represents the Nyquist plots of electrochemical impedance spectroscopy (EIS) for Example 1 and Comparative Example 2; Figure 5 f is a comparison of the self-discharge and capacity retention rates of Example 1 and Comparative Example 2 after being completely left to stand for 24 hours under high charge. Figure 5g represents the concentration of Example 1 and Comparative Example 2 at 1.0 A·g. -1 Stability and coulombic efficiency of ultra-long constant current cycling under current density; Figure 5 h represents a comparison of the long-term cycling stability of Example 1 and Comparative Example 2 under harsh commercial zinc-poor operating conditions (8.6 μm ultrathin zinc foil, low N / P ratio, where N / P ratio is the capacity ratio of the negative electrode to the positive electrode). Detailed Implementation

[0024] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply; where the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0025] In this invention, MXene refers to a two-dimensional transition metal carbide, nitride, or carbonitride, such as Ti3C2T. x T in x The term "MXene" refers to surface end groups such as -O, -OH, -F, and -Cl. The DMSO-modified MXene material described in this invention refers to MXene material with DMSO molecules adsorbed on its surface, which can be obtained by introducing a DMSO / H2O mixed solvent during the etching, intercalation, washing, or stripping process of MXene. The S=O groups in the DMSO molecules interact with the transition metal sites on the MXene sheet surface (for Ti3C2T...). xCoordination or chemisorption occurs between Ti sites, causing DMSO molecules to adsorb onto the surface of MXene sheets, forming a stable hydrophobic barrier. After the DMSO-modified MXene material is loaded onto the zinc substrate to form an interfacial protective layer, the DMSO molecules adsorbed on the MXene sheet surface are distributed along with the MXene nanosheets on the negative electrode surface. The aforementioned hydrophobic barrier is located between the zinc substrate and the electrolyte. Seawater-based electrolyte refers to an aqueous electrolyte obtained by dissolving zinc salts in seawater as a solvent, while deionized water-based electrolyte refers to an aqueous electrolyte obtained by dissolving the same type and concentration of zinc salts in deionized water as a solvent; the only difference between the two is the solvent. The seawater used is natural seawater that has been filtered to remove suspended solids before use. In the text and accompanying figures, the negative electrode prepared in Example 1 is denoted as DM@Zn, the negative electrode prepared in Comparative Example 1 is denoted as MXene@Zn, and the negative electrode in Comparative Example 2 is denoted as Bare Zn. In some accompanying figures, DM@Zn is abbreviated as DM, and MXene@Zn is abbreviated as M@Zn or M. Seawater-based electrolyte is denoted as NSW, and deionized water-based electrolyte is denoted as DIW. The ambient temperature mentioned in this invention refers to 20~30℃. The zinc substrate mentioned in this invention refers to a zinc metal substrate used to support the interface protective layer, such as zinc foil. The sheet thickness of the DMSO-modified MXene material is obtained by measuring the height of the nanosheets using atomic force microscopy; the interlayer spacing refers to the interlayer spacing after the MXene nanosheets are stacked, calculated from the position of the (002) peak of its dried film according to the Bragg equation.

[0026] Example 1 A method for preparing a seawater-based aqueous zinc-ion battery includes the following steps: Step (1), Preparation of DMSO-modified MXene material: Using Ti3AlC2MAX phase as precursor, Ti3C2T is obtained by etching with HF / HCl mixed acid. x MXene; DMSO / H2O mixed solvent was introduced during the intercalation process to prepare DMSO-modified MXene materials. The specific steps are as follows: Etching: Weigh 1.0 g of Ti3AlC2MAX phase powder and place it in a polytetrafluoroethylene reaction flask. Slowly add 30 mL of etching solution, which consists of HF, HCl, and deionized water, with HF concentration of 7.5 mol / L and HCl concentration of 4 mol / L. Continue stirring and etching at 25 °C for 12 h. After the reaction, centrifuge, discard the supernatant, wash with deionized water until pH ≥ 6, then centrifuge again, collect the precipitate, and vacuum dry at room temperature for 24 h to obtain the etched product Ti3C2T. x .

[0027] Intercalation: Add 30 mL of DMSO / H2O mixed solvent with a volume percentage of 60% to 1 g of etching product, and add 1 g of lithium chloride. Stir at 25 °C for 12 h to perform intercalation treatment and obtain intercalated product.

[0028] Ultrasonic exfoliation: The intercalated product was repeatedly centrifuged and washed with deionized water until the supernatant turned black. Then, it was exfoliated by ultrasonication at 200W for 20 min under argon protection and ice-water bath conditions. After ultrasonication, the upper dispersion was collected by centrifugation, which is the aqueous dispersion of DMSO-modified MXene material. A portion of this dispersion was filtered, vacuum dried at 50℃ for 12 h, and weighed. The monolayer yield of DMSO-modified MXene material was found to be 95.4%. The layer thickness was measured to be 1.35 nm by atomic force microscopy. The interlayer spacing after stacking was calculated to be 1.47 nm by X-ray diffraction and Bragg equation.

[0029] Step (2), Preparation of zinc anode: Take the aqueous dispersion of DMSO-modified MXene material obtained in step (1), determine its concentration by weighing, and adjust its concentration to 10 mg / mL to obtain the aqueous dispersion of DMSO-modified MXene.

[0030] A 100 μm thick zinc foil with dimensions of 2 cm × 2 cm was ultrasonically cleaned for 5 min each with anhydrous ethanol and deionized water, and then dried. At room temperature, the DMSO-modified MXene aqueous dispersion was uniformly drop-coated onto the zinc foil surface, with the drop-coating amount determined to be approximately 9 μm thick for the interface protective layer after drying. The foil was then allowed to stand at 25 °C for 30 min under argon protection. The Zn dissolved from the zinc foil surface... 2+ Electrostatic bridging was achieved between the negatively charged MXene nanosheets and the zinc foil, allowing the MXene nanosheets to self-assemble in situ on the zinc foil surface to form an interfacial protective layer. This layer was then vacuum-dried at 40°C for 12 hours to obtain the negative electrode for a seawater-based zinc-ion battery, denoted as DM@Zn. The interfacial protective layer continuously covered the zinc foil surface with a thickness of approximately 9 μm. Figure 1 ).

[0031] Step (3), Preparation of seawater-based zinc-ion batteries: Zinc symmetric batteries, Zn||Cu asymmetric batteries, full batteries, and zinc-poor full batteries were prepared respectively, as follows: 1) Zinc symmetric battery The positive and negative electrodes of the zinc symmetric battery are the same, with a diameter of 12 mm, which is the DM@Zn electrode prepared according to step (2).

[0032] Separator: Glass fiber diaphragm, 16mm in diameter and 0.68mm in thickness.

[0033] Electrolyte: 2 mol / L ZnSO4 aqueous solution, using natural seawater as solvent, i.e., seawater-based electrolyte (NSW).

[0034] Battery assembly: Under air atmosphere, CR2032 coin cells were assembled in the following order: positive electrode shell, gasket, DM@Zn electrode, separator, DM@Zn electrode, gasket, spring, and negative electrode shell. The electrolyte volume was 100μL. The cells were sealed and allowed to stand for 12 hours to allow the electrolyte to fully impregnate them, thus preparing a zinc symmetric cell.

[0035] 2) Zn‖Cu asymmetric cell The positive electrode of the Zn‖Cu asymmetric battery is a copper foil with a thickness of 20μm. Before use, it is ultrasonically cleaned for 5 minutes each with acetone, 0.1mol / L dilute hydrochloric acid and deionized water and then dried.

[0036] Diaphragm: The same glass fiber diaphragm as in 1).

[0037] Electrolyte: Seawater-based electrolyte NSW.

[0038] Battery assembly: Using the DM@Zn electrode prepared in step (2) as the negative electrode and the copper foil as the positive electrode, the cells were assembled in the order of CR2032 coin cells under an air atmosphere. The liquid volume was 100 μL, and the cells were left to stand for 12 h to prepare a Zn‖Cu asymmetric cell.

[0039] 3) Full battery The positive electrode of the full cell was prepared as follows: α-MnO2, conductive carbon black, and polyvinylidene fluoride were mixed in N-methylpyrrolidone at a mass ratio of 7:2:1 to form a slurry. This slurry was coated onto a titanium foil current collector, vacuum dried at 80°C for 12 hours, and then cut into 12mm diameter discs. The active material loading was 1.0~2.0 mg / cm³. 2 .

[0040] Diaphragm: The same glass fiber diaphragm as in 1).

[0041] Electrolyte: 2 mol / L ZnSO4 aqueous solution and 0.1 mol / L MnSO4 aqueous solution, with natural seawater as the solvent.

[0042] Battery assembly: Take the DM@Zn negative electrode prepared in step (2) and assemble it with the above positive electrode, separator and electrolyte according to the assembly sequence of CR2032 coin cell. The liquid injection volume is 100μL. Let it stand for 12h to prepare a full cell.

[0043] 4) Zinc-poor full cells The process was carried out according to the full cell method in 3), except that the zinc foil was replaced with an 8.6 μm ultrathin zinc foil, and the loading of the positive electrode active material was increased accordingly, so that the capacity ratio (N / P ratio) of the negative electrode to the positive electrode was 3.0, and a zinc-poor full cell was prepared.

[0044] Comparative Example 1 This comparative example is used to illustrate seawater-based aqueous zinc-ion batteries prepared using conventional aqueous MXene.

[0045] The operation was carried out according to the method described in Example 1, except that ordinary MXene prepared in a conventional aqueous phase was used instead of the DMSO-modified MXene material prepared in step (1) of Example 1. The difference between the preparation method of ordinary MXene and the preparation method of MXene material in Example 1 is that DMSO / H2O was replaced with deionized water to prepare a seawater-based aqueous zinc-ion battery, denoted as MXene@Zn battery, and its negative electrode is denoted as MXene@Zn negative electrode.

[0046] Comparative Example 2 This comparative example is used to illustrate seawater-based aqueous zinc-ion batteries prepared from bare zinc.

[0047] The method described in Example 1 was followed, except that bare zinc foil was used instead of the DM@Zn prepared in step (2) of Example 1 to prepare a seawater-based aqueous zinc-ion battery, denoted as Bare Zn battery.

[0048] The following performance tests were performed on Example 1, Comparative Example 1, and Comparative Example 2.

[0049] The surface and cross-sectional morphology of the negative electrode prepared in Example 1 were characterized by scanning electron microscopy (SEM), and the results are shown in the figure. Figure 1 .

[0050] Depend on Figure 1 As can be seen from this, the surface of the DM@Zn anode is composed of overlapping, wrinkled MXene nanosheets. These nanosheets continuously and uniformly cover the zinc foil surface, without any obvious cracks. Figure 1 As shown in b (the bright area at the bottom of the figure represents the zinc foil substrate), the interfacial protective layer exhibits a layered stacked structure parallel to the zinc foil surface, with a thickness of approximately 9 μm. It is tightly bonded to the zinc foil substrate, with a continuous interface and no obvious peeling gaps. These results indicate that DMSO-modified MXene nanosheets, after drop-coating, electrostatically self-assemble on the zinc foil surface, forming a continuous and dense layered interfacial protective layer. This layer effectively blocks free water molecules and corrosive anions in seawater and provides a protective layer for Zn. 2+ Providing a two-dimensional interlayer transmission channel provides the structural foundation.

[0051] The negative electrode and zinc symmetric battery prepared in Comparative Example 1 were subjected to SEM morphology testing, Raman spectroscopy testing, XRD testing, and constant current charge-discharge testing. The results are shown in the figure. Figure 2 .

[0052] Experiments have shown that although ordinary MXene can provide some physical shielding in the early stages, in complex high-salt, high-conductivity seawater-based electrolyte environments, MXene nanosheets without antioxidant barriers are extremely susceptible to severe nucleophilic attacks from free water molecules and dissolved oxygen.

[0053] Depend on Figure 2 It is known that after immersion in seawater and charge-discharge cycles, the surface of ordinary MXene interface protective layer changes from flat and dense to extremely rough and porous, and a large number of nanoscale insulating oxide crystals grow. Raman spectroscopy and XRD characterization revealed the nature of its physicochemical failure: Raman spectroscopy confirmed that ordinary MXene spontaneously oxidizes in the seawater system and produces obvious titanium dioxide (TiO2) characteristic vibrational peaks on the surface; while the insulating anatase TiO2 crystal phase generated in situ between the nanosheet layers not only disorderly exfoliates and destroys the two-dimensional stacking channels, but also causes the intrinsic (002) characteristic diffraction peak of MXene to shift significantly to the high-angle direction on a large scale, and the characteristic peak intensity is greatly reduced.

[0054] Due to severe damage to the two-dimensional lattice and the breakage of metallic conductive channels, the zinc anode protected by ordinary MXene exhibits rapidly deteriorating interfacial kinetic impedance in long-term electrochemical cycling tests in a seawater-based electrolyte system. Because of localized high-field polarization and the rapid accumulation of dead zinc, the electrode experiences a polarization surge and sudden short-circuit failure within a very short cycling time. This stark contrast between physicochemical and electrochemical properties indicates that traditional ordinary MXene materials are at a bottleneck in natural seawater environments, characterized by "spontaneous oxidation deactivation, channel blockage, and dendrite failure."

[0055] To further elucidate the mechanism by which DMSO inhibits MXene oxidation, density functional theory (DFT) was used to calculate the adsorption energies of DMSO and H2O molecules on the MXene surface. The calculation results show that the adsorption energy of DMSO molecules on the MXene surface is -0.68 eV, lower than that of H2O molecules (-0.33 eV) (lower adsorption energy indicates more stable adsorption). This indicates that the adsorption of DMSO on the MXene surface is thermodynamically more favorable, allowing it to preferentially occupy the MXene surface and repel free water molecules in the competitive adsorption process. The DMSO molecular layer adsorbed on the MXene nanosheet surface isolates free water molecules and dissolved oxygen from seawater through steric hindrance, blocking their nucleophilic attack on Ti atoms on the MXene surface.

[0056] The negative electrodes and batteries prepared in the examples and comparative examples were subjected to performance tests to determine their antioxidant stability and interfacial electrochemical reaction kinetics mechanism. The results are shown in [Figure number missing]. Figure 3 .

[0057] Depend on Figure 3 The XPS Ti 2p high-resolution spectrum of a shows that after DIW and NSW aging treatment, the proportion of Ti-O oxidation characteristics in the DM@Zn anode remains low, with the intrinsic Ti-C characteristic peak near 455.0 eV consistently dominating. Meanwhile, XRD phase analysis in natural seawater indicates that unprotected MXene undergoes severe water-induced oxidation, generating an insulating titanium dioxide phase between the nanosheet layers. This not only disrupts the interlayer stacking order but also causes a significant shift of the intrinsic (002) characteristic diffraction peak of MXene towards higher angles and a sharp decrease in peak intensity. Figure 2 e); while the DM@Zn electrode only showed slight TiO2 oxidation diffraction characteristics ( Figure 3 b), its (002) characteristic diffraction main peak is still sharp and has not shifted significantly at a large angle. The above spectral and diffraction data show that the DMSO molecules adsorbed on the surface of MXene nanosheets can resist the strong oxidation and corrosion of seawater at the microscale and maintain the intrinsic interlayer spacing and lattice integrity of MXene for a long time.

[0058] Because the DMSO barrier provides long-term protection against oxidation failure of the MXene interface protective layer, it remains in a state of extremely high conductivity and retains dense surface polar groups, thus robustly exhibiting a triple synergistic mechanism of "electrostatic repulsion-electric field modulation-physical confinement" in complex seawater. In linear sweep voltammetry (LSV) testing, DM@Zn significantly postpones the hydrogen evolution reaction (HER) limiting overpotential in 1 mol / L Na2SO4, while Tafel polarization curves reveal that its corrosion current density increases from that of bare zinc. corr =2.22mA·cm -2 And MXene@Zn 1.73mA·cm -2 Reduced to 1.68 mA·cm -2 These electrochemical parameters indicate that the negatively charged surface and tightly layered structure of MXene create a strong electrostatic barrier and physical barrier, successfully blocking highly corrosive Cl- from seawater. - With SO4 2- It keeps anions and free water molecules out, inhibiting pitting corrosion and parasitic side reactions, and effectively improving its corrosion resistance. Figure 3Electrochemical impedance spectroscopy (EIS) showed that the real part span of the impedance spectrum of the DM@Zn symmetric cell was significantly smaller than that of the MXene@Zn symmetric cell, indicating that the DMSO-modified interfacial protective layer had a lower interfacial impedance. Meanwhile, Arrhenius curves obtained by temperature-dependent electrochemical impedance spectroscopy (EIS) confirmed that the interfacial desolvation activation energies (Ea) of bare zinc, MXene@Zn, and DM@Zn were 33.2 kJ·mol⁻¹. -1 24.4 kJ·mol -1 and 28.8 kJ·mol -1 The MXene interface protective layer reduces the interface desolvation activation energy to below that of bare zinc, indicating that the zinc-loving active groups on the MXene surface are beneficial to Zn. 2+ The desolvation of MXene@Zn was observed. In the chronoamperometry (IT) curves, the bare zinc electrode exhibited an uncontrolled, tip-aggregated two-dimensional (2D) planar diffusion failure mode for approximately 60 seconds, while the DM@Zn anode rapidly and smoothly transitioned to a three-dimensional (3D) uniform diffusion response within approximately 20 seconds. Simultaneously, due to the excellent equipotential flow field homogenization effect, the zinc deposition nucleation overpotential decreased from 20.6 mV for bare zinc and 16.0 mV for MXene@Zn to 15.8 mV, fully demonstrating that unoxidized MXene has the ability to induce Zn deposition. 2+ It has the advantage of flux isotropication and guiding planar parallel and uniform nucleation.

[0059] The interfacial deposition behavior of the negative electrodes prepared in the examples and comparative examples was studied, and the results are shown in [the table below]. Figure 4 .

[0060] Figure 4 Mid-in-situ cross-sectional optical microscopy showed that at 5 mA·cm -2 During continuous deposition at high current density for 24 minutes, the bare zinc surface showed obvious protrusions and dendrite pillars that could easily pierce the separator after several minutes. In contrast, the DM@Zn composite electrode interface remained smooth and flat under over-deposition, without any obvious dendrite protrusions. Quantitative characterization using 3D white light interferometry profilers after multiple cycles confirmed that the surface roughness (Sa) of the bare zinc deteriorated from an initial 0.15 μm to 1.35 μm, including giant corrosion pits and moss-like dead zinc. In contrast, the DM@Zn anode, after prolonged high-salt immersion and charge-discharge cycles, had a surface roughness of 0.86 μm, indicating that the interface protective layer could suppress surface stress distortion and improve the deposition morphology. In extreme load life tests of the battery, facing 5 mA·cm... -2 Ultra-high current density and 1mAh·cm -2 Under the harsh operating conditions of surface capacity, bare zinc symmetric cells experienced localized puncture short circuits after only about 40 hours of cycling, while DM@Zn symmetric cells operated stably for over 2000 hours, maintaining a small charge / discharge polarization overpotential of about 40mV without fluctuation, achieving a cycle life leap of more than 50 times. Figure 3 h); In the Zn‖Cu asymmetric cell deposition / stripping experiment, the cell with DM@Zn as the counter electrode maintained an average coulombic efficiency (CE) of up to 98.97% for a long time. Combined with the time-resolved in-situ relaxation time distribution (DRT) spectrum, it can be seen that its polarization impedance distribution remains stable during the long charge-discharge cycle, indicating that the interface protective layer remains stable during long-term cycling. Figure 4 The cyclic voltammetry curves of d show that the deposition / stripping peaks of the Zn‖Cu asymmetric cells corresponding to DM@Zn and MXene@Zn are similar and the peak currents are relatively small, while the cathode current and stripping peak current of the cells corresponding to bare zinc are significantly larger.

[0061] The performance of the full cells prepared in the examples and comparative examples was tested, and the results are shown in the figure. Figure 5 .

[0062] Depend on Figure 5 It can be seen that when a large-capacity cathode is assembled into a complete energy storage cell, the cyclic voltammetry (CV) curve shows that the DM@Zn cell has a sharper and more reversible redox characteristic peak and a higher response current than bare zinc, indicating that the interface protective layer improves the charge transfer kinetics. Figure 5 Electrochemical impedance spectroscopy (E) shows that the semicircular diameter of the DM@Zn full cell in the high-frequency region is smaller than that of the bare zinc full cell, further indicating its lower charge transfer impedance; in the range of 0.2 to 3.0 A·g -1 Under extremely wide current gradient loads, DM@Zn exhibits higher specific capacitance at all current densities than the comparative example; at 1.0 A·g -1 During ultra-long-life cycling, the bare zinc full cell rapidly decayed to near zero capacity after approximately 400 cycles due to dendrite piercing the separator and depletion of free water, while the DM@Zn full cell successfully completed 2000 charge-discharge cycles. Simultaneously, 24-hour static charge-discharge tests under high charge conditions showed that DM@Zn maintained a charge capacity retention rate as high as 93.2%, while bare zinc only retained 90.1%, indicating that the DMSO-modified MXene interface protective layer suppressed the self-discharge corrosion of the zinc anode in the seawater system. Finally, to verify the system's resilience near the limits of commercial energy storage, a rigorous commercial zinc-poor system was constructed. The anode used was an 8.6 μm thick zinc foil with an N / P ratio of 3.0. Experiments demonstrated that the DM@Zn zinc-poor full cell performed well in seawater-based electrolyte at 1.0 A·g -1 Under heavy workloads, it can maintain stable operation for 200 cycles without short circuits. These results demonstrate that the DMSO-modified MXene interface protective layer can effectively extend the cycle life of seawater-based zinc-ion batteries.

[0063] The above results indicate that the symmetrical cell of Example 1 operates at 5 mA·cm⁻¹. -2 With 1mAh·cm -2Under certain conditions, it can be stably cycled for more than 2000 hours, which is significantly better than the less than 100 hours of Comparative Example 1 and the approximately 40 hours of Comparative Example 2.

[0064] In summary, the seawater-based zinc-ion battery anode, its preparation method, and the battery of the present invention utilize DMSO-modified MXene material as the interface protection layer of the anode, constructing a robust organic protection and hydrophobic barrier on its surface. This overcomes the interface compatibility challenge between the abundant end groups on the MXene surface and the zinc matrix, and constructs an anode interface protection layer based on the MXene framework in situ. The resulting zinc-ion battery exhibits good long-term stability and corrosion inhibition function in complex natural seawater systems at room temperature.

[0065] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various specific technical features in any suitable manner. To avoid unnecessary repetition, the present invention will not describe the various possible combinations separately. However, these simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A seawater-based aqueous zinc-ion battery negative electrode, characterized in that, The negative electrode includes a zinc substrate and an interface protective layer loaded on the surface of the zinc substrate, the interface protective layer comprising MXene material modified with dimethyl sulfoxide (DMSO).

2. The negative electrode of a seawater-based zinc-ion battery according to claim 1, characterized in that, The MXene material contains Ti2CT x Ti3CNT x V2CT x Nb2CT x and Ti3C2T x At least one of the following: the DMSO-modified MXene material has a sheet thickness of 1-5 nm and a layer spacing of 1.2-2.5 nm after stacking.

3. A method for preparing a negative electrode for a seawater-based aqueous zinc-ion battery, characterized in that, The method includes loading a dimethyl sulfoxide (DMSO) modified MXene material onto the surface of a zinc substrate to form an interfacial protective layer, thereby obtaining a seawater-based aqueous zinc-ion battery anode.

4. The method for preparing the negative electrode of a seawater-based aqueous zinc-ion battery according to claim 3, characterized in that, The loading method includes drop-coating an aqueous dispersion of the DMSO-modified MXene material onto the surface of the zinc substrate, allowing the DMSO-modified MXene material to electrostatically self-assemble on the zinc substrate to form the interface protective layer.

5. The method for preparing the negative electrode of a seawater-based aqueous zinc-ion battery according to claim 3, characterized in that, The MXene material is Ti3C2T. x The material, wherein the zinc substrate is zinc foil.

6. The method for preparing the negative electrode of a seawater-based aqueous zinc-ion battery according to claim 5, characterized in that, The preparation method of the DMSO-modified MXene material includes: etching the Ti3AlC2MAX phase to obtain Ti3C2T x ; Regarding the Ti3C2T x Intercalation, washing, and stripping processes were performed sequentially, with the intercalation occurring in a DMSO / H2O mixed solvent, to obtain the DMSO-modified MXene material.

7. The method for preparing the negative electrode of a seawater-based aqueous zinc-ion battery according to claim 6, characterized in that, The etching process includes etching the Ti3AlC2MAX phase with an etchant to obtain the Ti3C2T phase. x The etching agent is an HF / HCl solution; The intercalation method includes: etching the obtained Ti3C2T x When mixed with the DMSO / H2O mixed solvent, 0.5~6g of Ti3C2T is added to every 30mL of the DMSO / H2O mixed solvent. x Lithium salt was added, and the mixture was stirred at room temperature for 12-24 hours to induce intercalation.

8. The method for preparing the negative electrode of a seawater-based aqueous zinc-ion battery according to claim 7, characterized in that, In the DMSO / H2O mixed solvent, the volume percentage of DMSO is 50-90%; in the HF / HCl solution, the concentration of HF is 5-10 mol / L and the concentration of HCl is 2-6 mol / L.

9. A seawater-based aqueous zinc-ion battery anode prepared by the preparation method of any one of claims 3-8.

10. A seawater-based aqueous zinc-ion battery, characterized in that, The seawater-based aqueous zinc-ion battery comprises the seawater-based aqueous zinc-ion battery negative electrode as described in claim 1 or 2.