Process for preparing bimodal broad distribution mabs graft copolymer and transparent abs thermoplastic compositions
By using physical agglomeration technology to prepare large-particle-size polybutadiene latex with a bimodal wide distribution and constructing a double-grafted shell layer, the problems of long reaction cycle and insufficient light transmittance in the preparation of existing transparent ABS resins are solved, achieving high light transmittance and excellent mechanical properties.
Patent Information
- Application Number
- CN202611049168.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for preparing transparent ABS resin suffer from problems such as long reaction cycles or the introduction of impurities, resulting in light transmittance that cannot meet the requirements of high optical performance applications.
Large-particle-size polybutadiene latex with a bimodal broad distribution was prepared using physical agglomeration technology, and a double-grafted shell layer was formed on its surface. A transparent ABS thermoplastic composition was then prepared by melt extrusion.
The light transmittance and mechanical properties of transparent ABS resin have been improved, with a light transmittance of over 91% and a haze of less than 2.5%, achieving the best match between optical and mechanical properties.
Smart Images

Figure CN123107004A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of synthetic resin technology and relates to a method for preparing bimodal broad-distribution MABS graft copolymer and a transparent ABS thermoplastic composition. Background Technology
[0002] In recent years, with technological advancements and industrial development, the optical properties of materials have attracted increasing attention, leading to extensive research on transparent materials, with transparent ABS resin being one such example. Due to the excellent mechanical properties, chemical resistance, and processing fluidity of ABS resin, researchers have achieved transparency by controlling its refractive index.
[0003] Currently, there are two main technical routes for the industrialization of transparent ABS resin. One is the continuous bulk method, which has the advantage of producing relatively pure products, but the products are relatively limited. The other is the emulsion grafting method, in which the matrix resin phase and the rubber phase are prepared separately and then melt-plasticized to obtain transparent ABS resin. Its advantage is that there are many product grades, which can be used for different application requirements. Therefore, this method is the most widely used, but the products contain impurities such as emulsifiers, which affects its application in high-requirement scenarios such as medical treatment.
[0004] The preparation technology of the rubber phase (toughening modifier, usually a core-shell copolymer) for transparent ABS resin is one of the key technologies in the preparation of transparent ABS resin by emulsion grafting and blending, which is related to the stiffness and toughness balance of transparent ABS resin, especially in the preparation of large-particle-size polybutadiene latex. Large-particle-size polybutadiene latex can be prepared by one-step and two-step methods. The one-step method directly prepares large-particle-size polybutadiene latex, but the reaction time is long. The two-step method increases the size of small-particle-size polybutadiene latex through physical agglomeration and chemical agglomeration, ultimately achieving the preparation of large-particle-size polybutadiene latex.
[0005] Patent CN105008406B describes a one-step polymerization method for preparing large-particle-size polybutadiene latex with an average particle size of 2500–4000 Å and a reaction time of 18–20 hours. Subsequently, methyl methacrylate, styrene, and acrylonitrile monomers are grafted onto the latex to obtain a MABS resin modifier. After blending the MABS resin modifier with MSAN resin, a light transmittance of approximately 90.5% and an impact strength of 17 kJ / m² are obtained. 2Transparent ABS resin. Patent CN116162204B describes taking 100 parts of the prepared emulsion, adding 20 parts of a 5% acetic acid aqueous solution, and slowly stirring at room temperature and pressure. After reacting for 2 hours, a 5% KOH aqueous solution is added to adjust the pH of the reaction solution to approximately 11, obtaining an agglomerated latex emulsion with a particle size of 290-310 nm. From this large-particle-size polybutadiene latex, grafted latex emulsion, grafted powder, and transparent ABS resin are sequentially prepared. The transparent ABS resin has a light transmittance of approximately 90.0% and an impact strength of approximately 17 kJ / m².
[0006] A comparison of existing publicly available technologies reveals that both one-step and chemical agglomeration methods can produce transparent ABS resin using emulsion grafting and blending. However, the one-step method for preparing large-particle-size polybutadiene latex has a long reaction cycle, while chemical agglomeration introduces agglomerating agents, reducing production efficiency (lower product solid content) and diminishing the reaction cycle advantage over the one-step method. Furthermore, the light transmittance of transparent ABS resin prepared by these methods is only around 90%, which fails to meet the requirements for high optical performance applications (light transmittance > 91.0%). Therefore, a process technology needs to be developed that can maintain the excellent light transmittance of transparent ABS resin while also ensuring the advantageous reaction cycle for large-particle-size polybutadiene latex. Summary of the Invention
[0007] In view of this, the present invention proposes a bimodal broad-distribution MABS graft copolymer and a transparent ABS thermoplastic composition, and a method for preparing the same. The present invention employs physical agglomeration-pressure agglomeration technology, preparing a large-particle-size polybutadiene latex with a bimodal broad-distribution by mixing primary and secondary pressure-agglomerated polybutadiene latex. Subsequently, a double-grafted shell layer is formed on its surface, and after coagulation, a bimodal broad-distribution MABS graft copolymer is obtained. This copolymer is then melt-extruded with MSAN resin to finally prepare a transparent ABS thermoplastic composition (transparent ABS resin). "Transparent ABS resin" and "transparent ABS thermoplastic composition" refer to the same substance; the term "thermoplastic composition" simply emphasizes that the material is thermoplastic and is a composition.
[0008] The present invention discloses a method for preparing a bimodal broad-distribution MABS graft copolymer, such as... Figure 4 As shown, the steps are as follows:
[0009] (1) Preparation of large-particle-size polybutadiene core latex with a bimodal wide distribution;
[0010] ① By mass, add 100-160 parts of pure water, 1.5-5 parts of emulsifier, 0.5-1.0 parts of electrolyte, 0.001-0.003 parts of reducing agent, 0.05-0.15 parts of co-reducing agent, and 0.1-0.3 parts of complexing agent to the polymerization reactor after nitrogen purging and mix thoroughly. Then add 0.08-0.25 parts of initiator, 100 parts of butadiene monomer, and 0.3-0.8 parts of chain transfer agent to the polymerization reactor and initiate the polymerization reaction at 50-70℃ for 8-12 hours. After terminating the reaction (the reaction is terminated when the monomer reaction is complete), a core layer latex of small particle size polybutadiene is obtained.
[0011] ② The small-particle-size polybutadiene core layer latex obtained in step ① is fed into a homogenizer with an operating pressure of 45~52 MPa for primary pressure agglomeration. Then, 10~30% of the mass of the core layer latex obtained from the primary pressure agglomeration is subjected to secondary pressure agglomeration at a pressure of 48~58 MPa. Finally, the remaining core layer latex obtained from the primary pressure agglomeration and the core layer latex obtained from the secondary pressure agglomeration are uniformly mixed to obtain a large-particle-size polybutadiene core layer latex with a bimodal wide distribution.
[0012] (2) Preparation of double-grafted shell MABS latex with bimodal width distribution;
[0013] ① Based on the total amount of large-particle-size polybutadiene core layer latex with bimodal wide distribution obtained in step (1) as 100 parts by mass, the total mass ratio of the dry base of the large-particle-size polybutadiene core layer with bimodal wide distribution to the total amount of grafted monomers is 1~2.5:1; the dry base of the large-particle-size polybutadiene core layer is the dry base material of polybutadiene core layer latex (excluding the water portion).
[0014] Take 260-600 parts of the large-particle-size polybutadiene core latex with bimodal wide distribution obtained in step (1) above into a grafting reactor, then add 70-150 parts of pure water, 0.5-2 parts of emulsifier, 0.1-0.2 parts of initiator, 0.0005-0.01 parts of reducing agent, 0.05-0.9 parts of co-reducing agent, and 0.005-0.15 parts of complexing agent, and mix evenly; then, at 50-65℃, continuously add 25-45 parts of the first grafted shell monomer, 0.1-1.2 parts of crosslinking agent, and 0.1-0.3 parts of initiator to the system, with a dropwise addition time of 20-40 minutes;
[0015] ② After the first grafted shell monomer is fed, continue the reaction for 10-20 minutes; then continuously add 55-75 parts of the second grafted shell monomer and 0.4-0.8 parts of initiator to the system over a period of 50-90 minutes; then raise the temperature of the system to 60-75℃, add 0.1-0.3 parts of initiator, maintain the temperature for 1-2 hours and then terminate the reaction (the reaction is terminated when the monomer reaction is complete), to obtain a double-grafted shell MABS latex with a bimodal broad distribution;
[0016] (3) The double-grafted shell MABS latex with bimodal width distribution obtained in step (2) is added to the coagulation liquid for coagulation and dehydration, and then dried to obtain the bimodal width distribution MABS graft copolymer.
[0017] Preferably, the emulsifier mentioned in steps (1) and (2) is potassium fatty acid, potassium stearate, potassium disproportionated rosinate, or C. 13 -C 15 One or more of allyl succinate dipotassium (including two, the same below); the initiator is one or more of cumene hydroperoxide, dicumene hydroperoxide, and tert-butyl dicumene hydroperoxide.
[0018] Preferably, the reducing agent mentioned in steps (1) and (2) is one or more of ferrous sulfate, sodium sulfite, sodium bisulfite, and sodium thiosulfate;
[0019] Preferably, the reducing agent mentioned in steps (1) and (2) is one or more of fructose, glucose, and sodium formaldehyde sulfoxylate.
[0020] Preferably, the complexing agent mentioned in steps (1) and (2) is one or both of sodium pyrophosphate and sodium ethylenediaminetetraacetate.
[0021] Preferably, the electrolyte mentioned in step (1) is one or more of potassium carbonate, sodium carbonate, and sodium bicarbonate;
[0022] Preferably, the chain transfer agent mentioned in step (1) is one or both of tert-dodecyl mercaptan and n-octyl mercaptan;
[0023] Preferably, the crosslinking agent mentioned in step (2) is one or a combination of two or more of allyl methacrylate (AMLA), ethylene glycol dimethacrylate (EGDMA), dicyclopentenyl acrylate (DCPA), triallyl isocyanurate (TAIC), divinylbenzene (DVB), and diallyl maleate (DAM).
[0024] Preferably, the first grafted shell monomer and the second grafted shell monomer mentioned in step (2) are one or more combinations of styrene, acrylonitrile, methyl methacrylate, methacrylic acid, and acrylic acid; the first grafted shell monomer and the second grafted shell monomer can be the same or different.
[0025] Preferably, the coagulation liquid in step (3) is composed of pure water and coagulant, with the mass ratio of coagulant to pure water being 2~10:1000, and the coagulant being one or more of concentrated sulfuric acid, magnesium sulfate, and calcium chloride.
[0026] The present invention also relates to a transparent ABS thermoplastic composition, which is obtained by melt plasticizing and extruding MSAN resin with a bimodal broad distribution MABS graft copolymer.
[0027] Furthermore, the transparent ABS thermoplastic composition is obtained by melt-plasticizing 200-300 g of bimodal broad-distribution MABS graft copolymer with 700-800 g of MSAN resin at 190-240°C, followed by extrusion granulation. This transparent ABS thermoplastic composition exhibits a notched impact strength of 150-185 J / m, light transmittance >91%, and haze <2.5%.
[0028] The melt plasticizing and extrusion granulation processes use a twin-screw extruder. The operating temperature and pressure parameters of each section are matched according to the specific machine to meet the actual needs.
[0029] The bimodal wide-distribution MABS graft copolymer described in this invention has a bimodal wide distribution and a double grafted shell structure, with a core-shell mass ratio of (50~70):(30~50).
[0030] The MSAN resin described in this invention is prepared by bulk polymerization, suspension polymerization or solution polymerization of methyl methacrylate, styrene and acrylonitrile, with a mass ratio of methyl methacrylate, styrene and acrylonitrile of (50~75):(10~30):(5~20); the MSAN resin can be prepared in-house or purchased.
[0031] Compared with the prior art, the beneficial effects of the present invention are:
[0032] This invention employs pressure agglomeration technology to prepare large-particle-size polybutadiene latex. By mixing polybutadiene latex obtained through primary pressure agglomeration with polybutadiene latex obtained through secondary pressure agglomeration, a large-particle-size polybutadiene latex with a bimodal broad distribution is prepared. Then, this invention constructs a double-grafted shell layer on the surface of the bimodal broad-distribution polybutadiene. The advantages are: the first grafted shell layer has a cross-linked structure, which can greatly suppress the collapse of the polybutadiene rubber phase, thereby avoiding the resulting diffuse reflection of light and improving the light transmittance of transparent ABS resin; the second grafted shell layer does not have a cross-linked structure, ensuring the mobility of the molecular chains in the grafted shell layer and avoiding the decrease in fluidity caused by the cross-linking of the molecular chains in the first grafted shell layer. Because the MABS graft copolymer in this invention has a bimodal broad distribution, when it is dispersed in MSAN resin by extrusion blending, the relatively small particle size MABS graft copolymer in the bimodal broad distribution can ensure the optical properties of the material, while the relatively large particle size MABS graft copolymer in the bimodal broad distribution, although it hinders the propagation of light, can improve the toughness of the material. This invention achieves the best match between optical and mechanical properties of transparent ABS resin thermoplastic composition through the bimodal broad distribution. Attached Figure Description
[0033] Figure 1 This is a particle size distribution diagram of the large-particle-size polybutadiene latex with a bimodal wide distribution in Example 1;
[0034] Figure 2 This is a particle size distribution diagram of the large-particle-size polybutadiene latex in Comparative Example 1.
[0035] Figure 3 This is a particle size distribution diagram of the large-particle-size polybutadiene latex in Comparative Example 2;
[0036] Figure 4 This is a flowchart of the method for preparing the bimodal broad-distribution MABS graft copolymer described in this invention. Detailed Implementation
[0037] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0038] Example 1
[0039] Add 15 kg of pure water, 0.15 kg of potassium fatty acid, 0.05 kg of potassium disproportionated rosinate, 0.08 kg of potassium carbonate, 0.0002 kg of ferrous sulfate, 0.012 kg of fructose, and 0.025 kg of sodium pyrophosphate to the nitrogen-purified polymerization reactor and mix thoroughly. Then add 0.013 kg of cumene hydroperoxide, 10 kg of butadiene monomer, and 0.05 kg of tert-dodecyl mercaptan to the polymerization reactor. Initiate the polymerization reaction at 65°C for 10 hours. After terminating the reaction (after the monomer has completely reacted),... (That is, terminating the reaction) yields a small-particle-size polybutadiene core-layer latex with a conversion rate of 98.5%. This small-particle-size core-layer latex is then subjected to primary pressure polymerization in a homogenizer operating at 50 MPa. Subsequently, 20% (by mass) of the core-layer latex obtained from the primary pressure polymerization is subjected to secondary pressure polymerization at 55 MPa. The remaining core-layer latex obtained from the primary and secondary pressure polymerizations is then uniformly mixed to obtain a large-particle-size polybutadiene core-layer latex with a bimodal broad distribution. Figure 1 As shown.
[0040] Take 375g of the above core layer latex into a grafting reactor, then add 125g of pure water, 0.8g of potassium oleate, 0.1g of cumene hydroperoxide, 0.001g of ferrous sulfate, 0.07g of fructose, and 0.01g of sodium pyrophosphate, and mix well. At 55°C, continuously add 21g of styrene, 9g of acrylonitrile, 0.4g of divinylbenzene, and 0.28g of cumene hydroperoxide to the system over a period of 25 minutes. After the first grafted shell layer monomer is added, continue the reaction for 10 minutes. Then, continuously add 66g of methyl methacrylate, 4g of methacrylic acid, and 0.72g of cumene hydroperoxide to the system over a period of 70 minutes. Then, raise the temperature of the reaction system to 65°C, add 0.23g of cumene hydroperoxide, and maintain the temperature for 1 hour to terminate the reaction (the reaction is terminated when the monomer reaction is complete). This yields a double-grafted shell layer MABS latex with a bimodal broad distribution. MABS latex was coagulated and dehydrated using a coagulation solution (4g of 98% sulfuric acid + 1000g of pure water), and dried at 60°C to obtain a bimodal broad-distribution MABS graft copolymer.
[0041] A transparent ABS thermoplastic composition with bimodal broad distribution structure can be obtained by melting and plasticizing 250g of bimodal broad distribution MABS graft copolymer and 750g of MSAN resin prepared by bulk method at 220℃ and then extruding and granulating.
[0042] Example 2
[0043] The amount of crosslinking agent used in the first grafted shell layer in Example 1 was adjusted from 0.4g to 0.8g, and the rest was the same as in Example 1.
[0044] Example 3
[0045] The large-particle-size polybutadiene core latex with a bimodal wide distribution is the same as in Example 1.
[0046] Take 375g of the above-mentioned core layer latex into a grafting reactor, then add 125g of pure water, 0.8g of potassium oleate, 0.1g of cumene hydroperoxide, 0.001g of ferrous sulfate, 0.07g of fructose, and 0.01g of sodium pyrophosphate, and mix thoroughly. At 55℃, continuously add dropwise 21g of methyl methacrylate, 6.3g of styrene, 2.7g of acrylonitrile, 0.4g of divinylbenzene, and 0.28g of cumene hydroperoxide to the system, with the addition time being... After the first grafted shell monomer is fed for 25 minutes, the reaction continues for another 10 minutes. Then, 49g of methyl methacrylate, 14.7g of styrene, 6.3g of acrylonitrile, and 0.72g of cumene hydroperoxide are continuously added dropwise to the system for 70 minutes. The temperature of the reaction system is then increased to 65°C, and 0.23g of cumene hydroperoxide is added. The reaction is terminated after maintaining the temperature for 1 hour, yielding a double-grafted shell MABS latex with a bimodal broad distribution. The MABS latex is coagulated using a coagulation solution (4g of 98% concentrated sulfuric acid + 1000g of pure water) and dried at 60°C to obtain a bimodal broad distribution MABS graft copolymer.
[0047] By melting and plasticizing 250g of bimodal broad-distribution MABS graft copolymer and 750g of MSAN resin prepared by bulk method at 220℃ and then extruding and granulating, a transparent ABS thermoplastic composition with bimodal broad-distribution structural characteristics can be obtained.
[0048] Example 4
[0049] The large-particle-size polybutadiene core latex with a bimodal wide distribution is the same as in Example 1.
[0050] Take 465g of the above core layer latex into a grafting reactor, then add 123g of pure water, 0.8g of potassium oleate, 0.1g of cumene hydroperoxide, 0.001g of ferrous sulfate, 0.07g of fructose, and 0.01g of sodium pyrophosphate, and mix well. At 55°C, continuously add 21g of styrene, 9g of acrylonitrile, 0.4g of divinylbenzene, and 0.28g of cumene hydroperoxide to the system for 25 minutes. After the first grafted shell layer monomer is fed, continue the reaction for 10 minutes, then continuously add 66g of methyl methacrylate, 4g of methacrylic acid, and 0.72g of cumene hydroperoxide to the system for 70 minutes. Then raise the temperature of the reaction system to 65°C, add 0.23g of cumene hydroperoxide, maintain the temperature for 1 hour, and terminate the reaction to obtain a double-grafted shell layer MABS latex with a bimodal broad distribution. The MABS latex is coagulated using a coagulation solution (4g concentrated sulfuric acid + 1000g pure water) and dried at 60°C to obtain a bimodal broad-distribution MABS graft copolymer.
[0051] By melting and plasticizing 250g of bimodal broad-distribution MABS graft copolymer and 750g of MSAN resin prepared by bulk method at 220℃ and then extruding and granulating, a transparent ABS thermoplastic composition with bimodal broad-distribution structural characteristics can be obtained.
[0052] Comparative Example 1
[0053] Add 15 kg of pure water, 0.15 kg of potassium fatty acid, 0.05 kg of potassium disproportionated rosinate, 0.08 kg of potassium carbonate, 0.0002 kg of ferrous sulfate, 0.012 kg of fructose reducing agent, and 0.025 kg of sodium pyrophosphate to a nitrogen-purified polymerization reactor and mix thoroughly. Then add 0.013 kg of cumene hydroperoxide, 10 kg of butadiene monomer, and 0.05 kg of tert-dodecyl mercaptan to the polymerization reactor. Initiate the polymerization reaction at 65°C for 10 hours. After terminating the reaction, a core-layer latex of small-particle-size polybutadiene is obtained with a conversion rate of 98.6%. The small-particle-size core-layer latex is then fed into a homogenizer operating at 50 MPa for pressure agglomeration to obtain a large-particle-size polybutadiene core-layer latex. Figure 2 As shown.
[0054] The rest is the same as in Example 1.
[0055] Comparative Example 2
[0056] Add 15 kg of pure water, 0.15 kg of potassium fatty acid, 0.05 kg of potassium disproportionated rosinate, 0.08 kg of potassium carbonate, 0.0002 kg of ferrous sulfate, 0.012 kg of fructose reducing agent, and 0.025 kg of sodium pyrophosphate to the nitrogen-purified polymerization reactor and mix thoroughly. Then add 0.013 kg of cumene hydroperoxide, 10 kg of butadiene monomer, and 0.05 kg of tert-dodecyl mercaptan to the polymerization reactor, and initiate the polymerization reaction at 65°C for 10 hours, then terminate the reaction. After the reaction, a core-layer latex of small-particle-size polybutadiene is obtained with a conversion rate of 98.5%. This small-particle-size core-layer latex is then fed into a homogenizer at an operating pressure of 50 MPa for primary pressure polymerization. Subsequently, 40% (by mass) of the primary pressure-polymerized core-layer latex is subjected to secondary pressure polymerization at an operating pressure of 55 MPa. The remaining core-layer latex obtained from the primary and secondary pressure polymerizations is then uniformly mixed to obtain a large-particle-size polybutadiene core-layer latex with a bimodal broad distribution. Figure 3 As shown.
[0057] The rest is the same as in Example 1.
[0058] The particle size and distribution of polybutadiene latex were characterized using a nanoparticle size analyzer. Figure 1 This indicates that the preparation method of this invention can successfully prepare large-particle-size polybutadiene latex with a bimodal broad distribution, while... Figure 2 Therefore, without using the method described in this invention, large-particle-size polybutadiene latex with a bimodal wide distribution was not prepared. Figure 3 This indicates that the secondary homogenized polybutadiene latex exceeds the scope of the claims, providing evidence that the performance of the subsequent transparent ABS resin cannot meet expectations.
[0059] Comparative Example 3
[0060] The amount of crosslinking agent in the first grafted shell layer in Example 1 was adjusted from 0.4g to 0g, and the rest was the same as in Example 1.
[0061] Comparative Example 4
[0062] The large-particle-size polybutadiene core latex with a bimodal wide distribution is the same as in Example 1.
[0063] Take 375g of the core layer latex mentioned above into a grafting reactor, then add 125g of pure water, 0.8g of potassium oleate, 0.1g of cumene hydroperoxide, 0.001g of ferrous sulfate, 0.07g of fructose, and 0.01g of sodium pyrophosphate. Mix well. At 55°C, continuously add dropwise 21g of styrene, 9g of acrylonitrile, 0.4g of divinylbenzene, and 0.28g of cumene hydroperoxide to the system for 25 minutes. After the first grafted shell layer monomer is fed, continue the reaction for 10 minutes, and continuously add dropwise 66g of methyl... Methyl acrylate, 4g methacrylic acid, 0.4g divinylbenzene (compared to Example 1, a crosslinking agent was used in the preparation of the second grafted shell; to illustrate, the transparent ABS thermoplastic composition has optimal optical properties and flowability only when the first grafted layer is crosslinked), 0.72g cumene hydroperoxide were added. The reaction was carried out for 70 minutes, then the temperature of the reaction system was increased to 65°C, 0.23g cumene hydroperoxide was added, and the reaction was terminated after maintaining the temperature for 1 hour. This yielded a double-grafted shell MABS latex with a bimodal broad distribution. The MABS latex was coagulated with a coagulating solution (4g of 98% concentrated sulfuric acid + 1000g of pure water) and dried at 60°C to obtain a bimodal broad distribution MABS graft copolymer.
[0064] By melting and plasticizing 250g of bimodal broad-distribution MABS graft copolymer and 750g of MSAN resin prepared by bulk method at 220℃ and then extruding and granulating, a transparent ABS thermoplastic composition with bimodal broad-distribution structural characteristics can be obtained.
[0065] The transparent ABS thermoplastic composition prepared above was injection molded. The thickness of the test samples was 3.2 mm. The test data are shown in the table below. Light transmittance and haze were tested according to ASTM D1003, and cantilever beam notched impact strength was tested according to ASTM D256. Melt flow rate was tested under the conditions of 220℃ and 10 kg.
[0066] Impact strength / J / m Melt flow rate (g / 10min) transmittance / % Haze / % Example 1 171 23.1 91.7 1.8 Example 2 163 22.7 91.3 2.2 Example 3 172 23.3 91.6 1.7 Example 4 183 22.6 91.8 1.9 Comparative Example 1 152 23.0 90.6 2.6 Comparative Example 2 179 24.1 89.3 3.3 Comparative Example 3 168 23.0 90.9 2.9 Comparative Example 4 156 20.2 91.5 2.1
[0067] The test results above show that the process technology provided in this invention can produce a transparent ABS resin composition with a bimodal broad distribution structure. The rubber phase in this transparent ABS resin exhibits a bimodal broad distribution structure. However, the transparent ABS resin in Comparative Example 1 did not construct the characteristic rubber phase structure described in this invention, and the proportion of secondary pressure-aggregated latex in Comparative Example 2 exceeded the range; therefore, its optical properties could not achieve optimal results. Furthermore, the data from the examples and Comparative Examples 3 and 4 indicate that when the first grafted shell layer lacks a cross-linked structure, the haze of the transparent ABS resin cannot achieve optimal results, while when both the first and second grafted shell layers have cross-linked structures, the flowability of the transparent ABS resin will decrease.
[0068] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Two or more combinations of modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a bimodal broad-distribution MABS graft copolymer, characterized in that, Includes the following steps: (1) Preparation of large-particle-size polybutadiene core latex with a bimodal wide distribution; ① By mass, add 100-160 parts of pure water, 1.5-5 parts of emulsifier, 0.5-1.0 parts of electrolyte, 0.001-0.003 parts of reducing agent, 0.05-0.15 parts of co-reducing agent, and 0.1-0.3 parts of complexing agent to the polymerization reactor after nitrogen purging and mix thoroughly. Then add 0.08-0.25 parts of initiator, 100 parts of butadiene monomer, and 0.3-0.8 parts of chain transfer agent to the polymerization reactor and initiate the polymerization reaction at 50-70℃ for 8-12 hours. After terminating the reaction, a core layer latex of small-particle-size polybutadiene is obtained. ② The small-particle-size polybutadiene core layer latex obtained in step ① is fed into a homogenizer with an operating pressure of 45~52 MPa for primary pressure agglomeration. Then, 10~30% of the mass of the core layer latex obtained from the primary pressure agglomeration is subjected to secondary pressure agglomeration at a pressure of 48~58 MPa. Finally, the remaining core layer latex obtained from the primary pressure agglomeration and the core layer latex obtained from the secondary pressure agglomeration are uniformly mixed to obtain a large-particle-size polybutadiene core layer latex with a bimodal wide distribution. (2) Preparation of double-grafted shell MABS latex with bimodal width distribution; ① Based on the total amount of large-particle-size polybutadiene core layer latex with bimodal wide distribution obtained in step (1) as 100 parts by mass, the total mass ratio of the dry base of the large-particle-size polybutadiene core layer with bimodal wide distribution to the total amount of grafted monomers is 1~2.5:1; Take 260-600 parts of the large-particle-size polybutadiene core latex with bimodal wide distribution obtained in step (1) above into a grafting reactor, then add 70-150 parts of pure water, 0.5-2 parts of emulsifier, 0.1-0.2 parts of initiator, 0.0005-0.01 parts of reducing agent, 0.05-0.9 parts of co-reducing agent, and 0.005-0.15 parts of complexing agent, and mix evenly; then add 25-45 parts of the first grafted shell monomer, 0.1-1.2 parts of crosslinking agent, and 0.1-0.3 parts of initiator continuously at 50-65℃, with a dropwise addition time of 20-40 minutes; ② After the first grafted shell monomer is fed, continue the reaction for 10-20 minutes; then continuously add 55-75 parts of the second grafted shell monomer and 0.4-0.8 parts of initiator over a period of 50-90 minutes; then raise the temperature to 60-75°C, add 0.1-0.3 parts of initiator, maintain the temperature for 1-2 hours, and terminate the reaction to obtain a double-grafted shell MABS latex with a bimodal wide distribution. (3) The double-grafted shell MABS latex with bimodal width distribution obtained in step (2) is added to the coagulation liquid for coagulation and dehydration, and then dried to obtain the bimodal width distribution MABS graft copolymer.
2. The method for preparing a bimodal broad-distribution MABS graft copolymer according to claim 1, characterized in that: The bimodal wide-distribution MABS graft copolymer has a bimodal wide distribution and a double grafted shell structure, with a core-shell mass ratio of (50~70):(30~50).
3. The method for preparing a bimodal broad-distribution MABS graft copolymer according to claim 1, characterized in that: The emulsifier is one or a combination of more than two of potassium fatty acid, potassium stearate, potassium disulfated rosin acid, C 13 -C 15 one or a combination of more than two of dipotassium alkenylsuccinate The initiator is one or a combination of two or more of cumene hydroperoxide, dicumene hydroperoxide, and tert-butyl dicumene hydroperoxide.
4. The method for preparing a bimodal broad-distribution MABS graft copolymer according to claim 1, characterized in that: The reducing agent is one or a combination of two or more of ferrous sulfate, sodium sulfite, sodium bisulfite, and sodium thiosulfate; The reducing agent is one or a combination of two or more of fructose, glucose, and sodium formaldehyde sulfoxylate.
5. The method for preparing a bimodal broad-distribution MABS graft copolymer according to claim 1, characterized in that: The complexing agent is one or both of sodium pyrophosphate and sodium ethylenediaminetetraacetate; The electrolyte is one or a combination of two or more of potassium carbonate, sodium carbonate, and sodium bicarbonate; The chain transfer agent is one or both of tert-dodecyl mercaptan and n-octyl mercaptan; The coagulated liquid is composed of pure water and a coagulant, with a mass ratio of coagulant to pure water of 2~10:1000. The coagulant is one or more of concentrated sulfuric acid, magnesium sulfate, and calcium chloride.
6. The method for preparing a bimodal broad-distribution MABS graft copolymer according to claim 1, characterized in that: The crosslinking agent is one or a combination of two or more of allyl methacrylate (AMLA), ethylene glycol dimethacrylate (EGDMA), dicyclopentenyl acrylate (DCPA), triallyl isocyanurate (TAIC), divinylbenzene (DVB), and diallyl maleate (DAM).
7. The method for preparing a bimodal broad-distribution MABS graft copolymer according to claim 1, characterized in that: The first grafted shell monomer and the second grafted shell monomer are one or more combinations of styrene, acrylonitrile, methyl methacrylate, methacrylic acid, and acrylic acid.
8. A transparent ABS thermoplastic composition, characterized in that: The bimodal broad-distribution MABS graft copolymer prepared by any one of claims 1 to 7 is obtained by melt plasticizing and extruding granulation with MSAN resin.
9. A transparent ABS thermoplastic composition according to claim 8, characterized in that: The transparent ABS thermoplastic composition is obtained by melt plasticizing 200-300 g of bimodal broad-distribution MABS graft copolymer with 700-800 g of MSAN resin at 190-240°C and then extruding and granulating.
10. A transparent ABS thermoplastic composition according to claim 9, characterized in that: The MSAN resin is prepared by bulk polymerization, suspension polymerization or solution polymerization of methyl methacrylate, styrene and acrylonitrile, with the mass ratio of methyl methacrylate, styrene and acrylonitrile being (50~75):(10~30):(5~20). The transparent ABS thermoplastic composition has a notched impact strength of 150~185 J / m, a light transmittance of >91%, and a haze of <2.5%.
Citation Information
Patent Citations
Transparent ABS resin and transparent ABS resin composition
CN105008406B
A preparation method of polybutadiene latex and transparent ABS resin
CN116162204B