Color conversion sheet and backlight unit including it
By using an antistatic layer and a bead coating formed from organic materials in the color conversion sheet, the problem of functional loss during the high-temperature drying process is solved, and the functional stability and reliability of the color conversion sheet at high temperatures are achieved, making it suitable for the backlight unit of LCD light guide plates.
Patent Information
- Application Number
- CN202580028137.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-24
- Filing Date
- 2025-04-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing color conversion sheets are prone to losing their function during high-temperature drying processes, and they exhibit numerous color variations and insufficient reliability.
The color conversion sheet, formed using organic materials, includes a substrate layer, a wavelength conversion section, an antistatic layer, and a bead coating layer. The antistatic layer is composed of organic adhesive resin, conductive polymer, and curing agent, while the bead coating layer is composed of organic adhesive resin and polymer beads, ensuring that the function is maintained at high temperatures.
It maintains functional stability during high-temperature drying processes, exhibits minimal color changes and excellent reliability, is easy to integrate with LCD light guide plates, and maintains low surface resistance.
Smart Images

Figure CN123125536A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a color conversion sheet and a backlight unit including the same, and more specifically, to a color conversion sheet with minimal color variation, excellent reliability, and the ability to maintain function even during high-temperature drying processes, and a backlight unit including the same. Background Technology
[0002] Currently, most display devices have evolved from the cathode ray tube (CRT) form factor displays, adopting the form of liquid crystal displays (LCDs). In particular, representative display devices such as TVs, smartphones, and monitors largely use LCDs. This type of LCD is essentially a light-receiving display device that cannot emit light itself to form an image, but instead receives light from an external source. Therefore, LCDs must have a backlight unit (BLU) on their back to emit light.
[0003] In particular, quantum dot technology has been extensively researched and applied recently in achieving high image quality for liquid crystal displays. Quantum dot technology offers the advantage of achieving various colors simply by adjusting the size of nano-inorganic particles, and it also exhibits excellent stability against UV and other light sources. However, existing cadmium (Cd)-based nano-inorganic particles suffer from environmental problems and are fragile to moisture, requiring the use of a barrier film, thus reducing their price competitiveness. Therefore, the development of organic phosphors that achieve high color reproduction and excellent brightness characteristics without using cadmium-based nano-inorganic particles has been actively pursued recently.
[0004] This color conversion sheet has a bead coating on the bottom back side to facilitate assembly with the LCD light guide plate, and has an additional antistatic function that can reduce surface resistance. However, it loses its function during the high-temperature drying process that forms the color conversion sheet. Summary of the Invention
[0005] The problem the invention aims to solve The present invention is proposed to solve the above-mentioned problems and meet existing needs. The technical problem to be solved by the present invention is to provide a color conversion sheet and a backlight unit including the color conversion sheet. The bead coating and antistatic layer on the bottom back of the color conversion sheet formed of organic material can not only maintain their function in the high temperature drying process, but also have less color change and excellent reliability.
[0006] The above and other objects and advantages of the present invention will become more apparent from the preferred embodiments described below.
[0007] means for solving problems The objective is achieved by a color conversion sheet comprising: a substrate layer; a wavelength conversion section located on one side of the substrate layer and comprising an organic phosphor and a matrix resin; an antistatic layer located on the other side of the substrate layer; and a bead coating layer formed by coating the antistatic layer.
[0008] Preferably, the antistatic composition forming the antistatic layer may include an organic adhesive resin, a conductive polymer, and a curing agent.
[0009] Preferably, the antistatic composition forming the antistatic layer may include 1 to 30 parts by weight of a conductive polymer relative to 100 parts by weight of the organic adhesive resin.
[0010] Preferably, the organic adhesive resin of the antistatic layer may include a mixture of one or more resins selected from acrylic resins, polyurethane resins and polyester resins or copolymers thereof.
[0011] Preferably, the conductive polymer may include one or more selected from polythiophene, polyaniline, polypyrrole, PEDOT, and PEDOT / PSS.
[0012] Preferably, the surface resistivity of the color conversion sheet measured on the bead-coated surface can be 1.0 × 10⁻⁶. 7 Ω / cm 2 the following.
[0013] Preferably, after the color conversion sheet undergoes a heat treatment at 170°C for 4 minutes, the surface resistivity measured on the bead coating surface can be 1.0 × 10⁻⁶. 7 Ω / cm 2 the following.
[0014] Preferably, the thickness of the antistatic layer can be 10 to 500 nm.
[0015] Preferably, the bead composition forming the bead coating may include an organic adhesive resin, polymer beads, and a curing agent.
[0016] Preferably, the bead composition forming the bead coating may include 0.1 to 0.3 parts by weight of polymer beads relative to 100 parts by weight of organic adhesive resin.
[0017] Preferably, the polymer beads may include one or a mixture of two or more selected from polyethylene terephthalate (PET), nylon, polystyrene (PS), polybutyl methacrylate (PBMA), polymethyl methacrylate (PMMA), and melamine.
[0018] Preferably, the organic adhesive resin for the bead coating may include a mixture of one or more selected from acrylic resins, polyurethane resins, and polyester resins, or copolymers thereof.
[0019] Preferably, the average particle size of the polymer beads can be 0.5 to 10 μm.
[0020] Preferably, the thickness of the bead coating can be 2 to 7 μm.
[0021] Preferably, it may also include a light diffusion layer, which is located on the wavelength conversion section and improves light diffusion and light efficiency.
[0022] Preferably, the wavelength conversion section may include a wavelength conversion layer located on one side of the substrate layer and comprising an organic phosphor and a matrix resin, and a transparent layer located on the wavelength conversion layer.
[0023] Preferably, the adhesion between the wavelength conversion layer and the transparent layer can be above 800 gf / inch.
[0024] Preferably, the wavelength conversion section may include a first wavelength conversion layer located on one side of the substrate layer and in which a first organic phosphor is dispersed in a first resin matrix, a transparent layer located on the first wavelength conversion layer, and a first wavelength conversion layer located on the transparent layer and in which a second organic phosphor is dispersed in a second resin matrix.
[0025] Preferably, the transparent layer may be a polymer film selected from one or more of polyethylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyetherimide, and polyimide.
[0026] Furthermore, the objective is achieved by a backlight unit equipped with the color conversion sheet.
[0027] Invention Effects The color conversion sheet and backlight unit including the present invention, by applying organic phosphor to the color conversion sheet, are not only environmentally safe but also have excellent color reproduction rate and brightness characteristics. They exhibit minimal color variation in various environments and excellent reliability. The bead coating and antistatic layer on the bottom back side do not lose their function even during high-temperature drying processes. Therefore, they are easy to integrate with LCD light guide plates and can maintain low surface resistance.
[0028] It should be noted that the effects of the present invention are not limited to those described above, and those skilled in the art can clearly understand other effects not described below based on the following description. Attached Figure Description
[0029] Figure 1 This is a structural diagram of a color conversion sheet according to an embodiment of the present invention.
[0030] Figure 2 This is a structural diagram of a color conversion sheet according to another embodiment of the present invention.
[0031] Figure 3 This is a schematic diagram of a backlight unit including a color conversion sheet according to an embodiment of the present invention. Detailed Implementation
[0032] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings, enabling those skilled in the art to readily implement the invention. The present invention can be implemented in various different forms and is not limited to the embodiments described herein.
[0033] To clearly illustrate the invention, parts unrelated to the description are omitted from the drawings. Throughout the specification, the same reference numerals are used in the drawings to refer to the same or similar constituent elements. Furthermore, in the drawings, the thickness of multiple layers and regions is enlarged to clearly show them. Additionally, in this specification, if a constituent element is described as being disposed "on" or "above" another constituent element, it means that the constituent element is directly disposed on the other constituent element, or that other constituent elements exist between the constituent elements. Conversely, if a constituent element is described as being directly disposed "on" or "above" another constituent element, it means that no other constituent elements are involved.
[0034] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as understood by those skilled in the art. In the event of conflict, the definitions used herein shall prevail. Furthermore, the same or equivalent methods and materials described herein may be used in the implementation or experimentation of the invention, and suitable methods and materials are described herein.
[0035] In this specification, "~ type resin", "~ type polymer" and / or "~ type copolymer" are broad concepts that include all "~ type resin", "~ type polymer", "~ type copolymer" and / or "~ type resin, polymer or copolymer derivatives". Additionally, in this specification, the term "polymer or copolymer crosslinked from these resins" means "polymer or copolymer crosslinked from the aforementioned resins".
[0036] In this specification, the term "compound" is used in a broad sense, including all "monoatomic molecules", "oligomers", and "polymeric compounds, including homopolymers and copolymers".
[0037] In this specification, unless otherwise expressly stated, the term "comprising" means that other constituent elements may be included, but are not excluded.
[0038] The term "these combinations" in this specification means a mixture or combination of one or more of the constituent elements described.
[0039] The term "and / or" in this specification means any and all combinations of more than one item described in connection with the description. The term "or" in this specification means "and / or". The use of "at least one" or "at least one" before a constituent element in this specification is to supplement the entire list of constituent elements, and not to supplement the individual constituent elements described.
[0040] Unless otherwise stated in this specification, all percentages, parts, and ratios are based on weight. Furthermore, when a quantity, concentration, or other value or parameter is given as any one of the categories of ranges, preferred ranges, or preferred upper and lower limits, it should be understood that, regardless of whether the range is disclosed individually, all ranges formed by any pair of any upper or preferred range limit and any lower or preferred range limit are specifically disclosed.
[0041] When a range of numerical values is mentioned in this specification, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range. The scope of this invention is not intended to be limited to the specific values mentioned when defining the range. In this specification, each constituent element includes both singular and plural concepts.
[0042] The constituent elements in this specification include the concepts of singular and plural.
[0043] Figure 1 This is a structural diagram of a color conversion sheet according to an embodiment of the present invention.
[0044] refer to Figure 1 According to one embodiment of the present invention, a color conversion sheet 100 may include a wavelength conversion section 10, a substrate layer 20, an antistatic layer 30, and a bead coating layer 40, and may also include a light diffusion layer 50. The wavelength conversion section 10 is located on one side of the substrate layer 20, the antistatic layer 30 is located on the other side of the substrate layer 20, and the bead coating layer 40 is formed by coating the antistatic layer 30. Furthermore, the light diffusion layer 50 may be located on the wavelength conversion section 10. The color conversion sheet 10 according to one embodiment of the present invention, having the above structure, can convert blue light into white light and emit it.
[0045] In addition, according to Figure 1The wavelength conversion section 10 shown in one example includes a wavelength conversion layer 11 and a transparent layer 12. In this case, the wavelength conversion layer 11 is located on one side of the substrate layer 20 and includes an organic phosphor and a matrix resin, while the transparent layer 12 is located on one side of the wavelength conversion layer 11 (the opposite side of the substrate layer 20). Each configuration will be described in detail below.
[0046] According to the present invention, the transparent layer 12 is a transparent and flexible polymer film, preferably comprising one or more resins selected from thermoplastic resins, thermosetting resins, and UV-curable resins with a visible light transmittance of 70% or more. More specifically, the transparent layer 12 is preferably a polymer film comprising one or more polymer films selected from polyethylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyetherimide, and polyimide.
[0047] Furthermore, the thickness of the transparent layer 12 is preferably 0.1 to 200 μm, more preferably 1 to 50 μm. This is because when the thickness of the transparent layer 12 is less than 0.1 μm, it is difficult to control the color changes that may occur due to the diffusion or mixing of the organic phosphors 13, 14 or the resin matrix 19 caused by temperature changes, while when it exceeds 200 μm, light transmission may be blocked.
[0048] According to one embodiment of the present invention, the wavelength conversion layer 11 of the color conversion sheet 100 is located between the transparent layer 12 and the substrate layer 20, and may simultaneously include a green organic phosphor 13 and a red organic phosphor 14 dispersed in the resin matrix 19. Furthermore, as described later... Figure 2 In the color conversion sheet 200 shown according to another embodiment of the present invention, the first organic phosphor 13, which is a green organic phosphor, and the second organic phosphor 14, which is a red organic phosphor, may also be included in separate first wavelength conversion layers 15 and second wavelength conversion layers 16, and thus be separated from each other.
[0049] The resin matrix 19 serves to fix the green organic phosphor 13 and the red organic phosphor 14 in the wavelength conversion layer 11, while preventing them from being exposed to moisture or oxygen, thereby preventing the decomposition of the green organic phosphor 13 and the red organic phosphor 14 dispersed in the resin matrix 19.
[0050] The resin matrix 19 preferably includes one or more resins selected from ester, olefin, acrylic, ether, urethane, carbonate and imide.
[0051] Furthermore, the resin included in the resin matrix 19 preferably has a number average molecular weight (Mn) of 1000-50000 g / mol or a weight average molecular weight (Mw) of 50000-2000000 g / mol. This is because when the number average molecular weight of the resin included in the resin matrix 19 is less than 1000 g / mol or the weight average molecular weight is less than 50000 g / mol, the resin matrix 19 becomes sticky, which may result in poor winding of the film when the color conversion sheet 100 is wound into a roll. When the number average molecular weight exceeds 50000 g / mol or the weight average molecular weight exceeds 2000000 g / mol, the poor solubility of the resin matrix 19 in the solvent may make it difficult to form the wavelength conversion layer 11.
[0052] Furthermore, the acid value of the resin included in the resin matrix 19 is preferably 0 to 20 mg KOH / g, and the hydroxyl value of the resin included in the resin matrix 19 is preferably 0 to 30 mg KOH / g, more preferably 0 to 20 mg KOH / g. This is because ester-based, olefin-based, acrylic-based, ether-based, urethane-based, carbonate-based, and imide-based resins, which are commonly used as resin matrices for wavelength conversion layers in color conversion sheets, can accelerate the decomposition of organic phosphors dispersed in the resin matrix due to the presence of functional groups such as hydroxyl or carboxylic acid groups within the resin, potentially reducing the reliability of the organic phosphor. Therefore, the above-mentioned ranges are preferred.
[0053] As an example, an ester-based resin that can be used as one of the resins in the resin matrix 19 preferably includes an ester-based resin polymerized from an aliphatic polyol and an aliphatic or aromatic polyacid. The aliphatic polyol is an aliphatic compound having two or more hydroxyl groups and having 2 to 10 carbon atoms, for example, it may include at least one selected from ethylene glycol, propylene glycol, butanediol, neopentyl glycol, and trimethylolpropane. Furthermore, the aliphatic polyacid is an aliphatic compound having two or more carboxylic acid groups and having 2 to 12 carbon atoms, for example, it may include at least one selected from malonic acid, succinic acid, adipic acid, and sebacic acid; the aromatic polyacid is an aromatic compound having two or more carboxylic acid groups and having 1 to 4 aromatic rings, for example, it may include at least one selected from isophthalic acid, phthalic acid, terephthalic acid, and cyclohexanedicarboxylic acid.
[0054] The resin matrix 19 preferably includes at least one of polyester, modified polyester, polyethylene, polycyclic olefin, poly(methyl)methacrylate, polyethylene glycol, polyurethane, polycarbonate, polyimide, and their block copolymers.
[0055] In addition, the resin matrix 19 may, as needed, include a crosslinking agent for chemical crosslinking of the resin matrix 19. As a crosslinking agent, it may include isocyanate-based, amine-based, anhydride-based, thiol-based, epoxy-based crosslinking agents, etc., but is not limited to these; various crosslinking agents may be included as needed.
[0056] The green organic phosphor 13 dispersed in the resin matrix 19 of the wavelength conversion layer 11 according to the present invention can absorb blue light and emit green light. The green organic fluorescent agent 13 preferably includes compounds or derivatives thereof with fused aromatic rings selected from naphthalene, anthracene, phenanthrene, pyrene, thionylene, triphenylene, perylene, fluoranthene, fluorene, indene, etc. (e.g., 2-(benzothiazol-2-yl)-9,10-diphenylanthracene or 5,6,11,12-tetraphenyltetraphenyl, etc.), furan, pyrrole, thiophene, silylopadiene, 9-silylfluorene, 9,9'-spirodisilylfluorene, benzothiophene, benzofuran, indole, dibenzothiophene, dibenzofuran, imidazopyridine, phenanthrene, pyridine, pyrazine, naphthidine, quinoxaline, pyrrolopyridine, thioxanthium, etc., with heteroaromatic rings, borane derivatives, stilbeneylbenzene derivatives, 4,4'-bis(2-(4-diphenylaminophenyl)ethyl The following are included in the list of at least one of the following: aminostyryl derivatives of alkenyl)biphenyl, 4,4'-bis(N-(zir-4-yl)-N-phenylamino)zir, aromatic acetylene derivatives, tetraphenylbutadiene derivatives, zir derivatives, aldehyde azide derivatives, pyrrole methylene derivatives, diketopyrrolo[3,4-c]pyrrole derivatives, 2,3,5,6-1H,4H-tetrahydro-9-(2'-benzothiazolyl)quinolorizizo[9,9a,1-gh]coumarin and other coumarin derivatives, imidazole, thiazole, thiadiazole, carbazole, oxazole, oxadiazole, triazole and other azole derivatives and their metal complexes, and aromatic amine derivatives represented by N,N'-diphenyl-N,N'-di(3-methylphenyl)biphenyl-4,4'-diamine.
[0057] In addition, the green organic phosphor 13 may include compounds of the following chemical formula 1.
[0058] (Chemical Formula 1)
[0059] Furthermore, the green organic phosphor 13 preferably comprises 0.1 to 5 parts by weight, more preferably 0.1 to 2 parts by weight, relative to 100 parts by weight of the solid component of the resin matrix 19. This is because when the green organic phosphor 13 is included in an amount of less than 0.1 parts by weight, the effect of converting the color to the desired color by the color conversion sheet 100 may be weak, while when it is included in an amount of more than 5 parts by weight, extinction may occur due to the aggregation and other interactions of the green organic phosphor 13.
[0060] The wavelength conversion layer 11 according to the present invention may include a red organic phosphor 14 dispersed in a resin matrix 19. The red organic phosphor 14 dispersed in the resin matrix 19 of the wavelength conversion layer 11 absorbs blue or green light and emits red light.
[0061] The aforementioned red organic phosphor 14 preferably includes compounds or derivatives thereof with fused aromatic rings, such as naphthalene, anthracene, phenanthrene, pyrene, thionylene, triphenylene, perylene, fluoranthene, fluorene, and indene (e.g., 2-(benzothiazol-2-yl)-9,10-diphenylanthracene or 5,6,11,12-tetraphenylbenzotetraphenyl), furan, pyrrole, thiophene, siliconecyclopentadiene, 9-siliconefluorene, 9,9'-spirodisilylfluorene, benzothiophene, benzofuran, indole, dibenzothiophene, dibenzofuran, imidazopyridine, phenanthrene, pyridine, pyrazine, naphthidine, quinoxaline, pyrrolopyridine, thioxanthium, etc., as well as borane derivatives, stilbeneylbenzene derivatives, and 4,4'-bis(2-(4-diphenylaminophenyl)). The following are included in the list of aminostyryl derivatives such as vinyl)biphenyl, 4,4'-bis(N-(zir-4-yl)-N-phenylamino)zir, aromatic acetylene derivatives, tetraphenylbutadiene derivatives, zir derivatives, aldehyde azide derivatives, pyrrole methylene derivatives, diketopyrrolo[3,4-c]pyrrole derivatives, 2,3,5,6-1H,4H-tetrahydro-9-(2'-benzothiazolyl)quinolorizizo[9,9a,1-gh]coumarin and other coumarin derivatives, imidazole, thiazole, thiadiazole, carbazole, oxazole, oxadiazole, triazole and other azole derivatives and their metal complexes, and aromatic amine derivatives represented by N,N'-diphenyl-N,N'-di(3-methylphenyl)biphenyl-4,4'-diamine.
[0062] Furthermore, the red organic fluorescent agent 14 preferably comprises a compound of the following chemical formula 2.
[0063] (Chemical Formula 2)
[0064] Furthermore, the red organic phosphor 14 preferably comprises 0.1 to 1 part by weight, more preferably 0.1 to 0.6 parts by weight, relative to 100 parts by weight of the solid component of the resin matrix 19. This is because when the red organic phosphor 14 is included in an amount less than 0.1 parts by weight, the effect of converting the color to the desired color by the color conversion sheet 100 may be weak, while when it is included in an amount greater than 1 part by weight, extinction may occur due to the aggregation and other interactions of the red organic phosphor 14.
[0065] The thickness of the wavelength conversion layer 11 according to the present invention is preferably 1 to 150 μm, more preferably 5 to 100 μm.
[0066] In a color conversion sheet 100 according to an embodiment of the present invention, the adhesive force between the transparent layer 12 and the wavelength conversion layer 11 is preferably 800 gf / inch or more. This is because when the adhesive force between the transparent layer 12 and the wavelength conversion layer 11 is less than 800 gf / inch, it is difficult to use the color conversion sheet 100 to fix it to the backlight unit.
[0067] Furthermore, the wavelength conversion layer 11 and the transparent layer 12 preferably have different refractive indices. Preferably, the refractive index is lower at the point where the incident light finally exits (at a greater distance from the light source). For example, preferably, when the incident light finally exits through the wavelength conversion layer 11, the refractive index of the transparent layer 12 is greater than that of the wavelength conversion layer 11; conversely, when the incident light finally exits through the transparent layer 12, the refractive index of the transparent layer 12 is less than that of the wavelength conversion layer 11. That is, as... Figure 3 As shown, in a color conversion sheet 100 according to an embodiment of the present invention, since the light source 70 is located in the direction of the wavelength conversion layer 11, the refractive index of the transparent layer 12 is preferably less than that of the wavelength conversion layer 11. This is because it increases the light reflectivity of the transparent layer 12, thereby effectively emitting the color-converted light to the outside.
[0068] The substrate layer 20 according to the present invention can be a transparent and flexible polymer film, such as polyethylene terephthalate, polyethylene naphtholate, polyacrylate, polycarbonate, polyetherimide, polyimide, etc., but is not limited thereto; various polymer films can be used. Furthermore, the substrate layer 20 can be an optical film such as a diffuser sheet or prism sheet, but is not limited thereto; sheets with various functions can be used.
[0069] According to the present invention, the light diffusion layer 50 can be located on the wavelength conversion section 10. That is, the light diffusion layer 50 is located on the transparent layer 12 in the wavelength conversion section 10, and plays a role in improving light diffusion and light efficiency. The light diffusion layer 50 is preferably a transparent and flexible polymer film, preferably including one or more selected from polyethylene terephthalate, polyethylene naphtalate, polyacrylate, polycarbonate, polyetherimide, and polyimide. In addition, the light diffusion layer 50 can be an optical film such as a diffusion sheet or a prism sheet, but is not limited to this, and sheets with various functions can be used. Furthermore, the light diffusion layer 50 can be formed of the same material as the substrate layer 20, or it can be composed of different materials.
[0070] According to the present invention, the antistatic layer 30 is located on the other side of the substrate layer 20 (the opposite side of the side where the wavelength conversion section 10 is located). The antistatic layer 30 is formed by coating an antistatic composition comprising an organic adhesive resin, a conductive polymer, and a curing agent onto the other side of the substrate layer 20. More specifically, the antistatic layer 30 is formed by coating an antistatic composition obtained by dispersing the organic adhesive resin, conductive polymer, and curing agent in an organic solvent onto the other side (lower part) of the substrate layer 20, drying it, and then curing it by heat or UV. In this case, the stacking order of the antistatic layer 30 can be before or after the formation of other functional layers.
[0071] In this invention, the antistatic composition forming the antistatic layer 30 preferably comprises 1 to 30 parts by weight of a conductive polymer and 0.2 to 2.0 parts by weight of a curing agent relative to 100 parts by weight of the organic adhesive resin. Specifically, the antistatic composition acquires antistatic properties through a mixture of the organic adhesive resin and the conductive polymer, preferably comprising 1 to 30 parts by weight of the conductive polymer relative to 100 parts by weight of the organic adhesive resin. In the antistatic composition, when the conductive polymer is included in an amount less than 1 part by weight relative to 100 parts by weight of the organic adhesive resin, the antistatic properties are weak. While an excessive amount exceeding 30 parts by weight improves the antistatic effect, it is uneconomical to use expensive conductive polymers. Therefore, it is preferable to control the content within the above-mentioned range to achieve the desired level of surface resistance.
[0072] Furthermore, the organic adhesive resin included in the antistatic composition preferably comprises a mixture of resins or copolymers thereof whose polymer backbone is selected from one or more of acrylic resins, polyurethane resins, and polyester resins. In the embodiments described later, a polyurethane resin with fluorinated hydrocarbon side chains was used at a solids content of 15% by weight, but this is not a limitation.
[0073] Furthermore, the conductive polymer included in the antistatic composition is preferably one or more of polythiophene, polyaniline, polypyrrole, poly(3,4-ethylenedioxythiophene) (PEDOT), and poly(3,4-ethylenedioxythiophene) / polystyrene sulfonic acid (PEDOT / PSS) or a mixture thereof.
[0074] Furthermore, the curing agent used in the antistatic composition is an additive for forming the antistatic layer, and can generally be selected from curing agents applicable to acrylic resins, polyurethane resins, and polyester resins. In this case, the antistatic composition preferably includes 0.2 to 2.0 parts by weight of curing agent relative to 100 parts by weight of organic adhesive resin. When the content of curing agent is less than 0.2 parts by weight, the adhesion between the substrate layer 20 and the antistatic layer 30 decreases; when it exceeds 2.0 parts by weight, a problem arises where the miscibility between the constituent substances of the antistatic composition decreases, i.e., the constituent substances cannot be uniformly mixed.
[0075] Furthermore, any solvent used in the antistatic composition can be a solvent capable of uniformly dissolving or dispersing the mixed resin of the organic adhesive resin and the conductive polymer. It is preferred to use a variety of mixed solvents, and most preferably a mixed solvent composed of water, ethanol, isopropanol and butanol.
[0076] Furthermore, the thickness of the antistatic layer 30 is preferably between 10 and 500 nm. When the thickness of the antistatic layer 30 is less than 10 nm, there is a problem that the antistatic function cannot be fully provided; when it exceeds 500 nm, there is a problem that the surface of the antistatic layer will crack.
[0077] The bead coating 40 according to the present invention is located on one side of the antistatic layer 30 (the side opposite to the side where the substrate layer 20 is formed) and comprises an organic adhesive resin and polymer beads. More specifically, the bead coating 40 is formed by applying a bead composition obtained by dispersing polymer beads, organic adhesive resin, and any curing agent in an organic solvent to the lower part of the antistatic layer 30 (the side opposite to the side where the substrate layer of the antistatic layer is formed), drying it, and then curing it by heat or UV. In this case, the stacking order of the bead coating 40 can be before or after the formation of other functional layers.
[0078] In this invention, the bead composition constituting the bead coating 40 may include 0.1 to 0.3 parts by weight of polymer beads and 0.01 to 0.2 parts by weight of curing agent relative to 100 parts by weight of organic adhesive resin. In particular, the bead composition, through the mixing of the organic adhesive resin and polymer beads, facilitates bonding with the light guide plate, thereby imparting a processability characteristic. It is preferable to include 0.1 to 0.3 parts by weight of polymer beads relative to 100 parts by weight of organic adhesive resin. At this point, when the bead composition includes polymer beads in an amount less than 0.1 parts by weight relative to 100 parts by weight of organic adhesive resin, the ease of assembly with the light guide plate decreases. When it includes an excessive amount exceeding 0.3 parts by weight, the particles are difficult to disperse, and the organic adhesive resin cannot adequately cover the polymer beads to achieve a single-layer coating, resulting in poor appearance. Therefore, the above-mentioned range is preferred.
[0079] Furthermore, the organic adhesive resin included in the bead composition preferably comprises a mixture of one or more of acrylic resins, polyurethane resins and polyester resins or copolymers thereof, whose polymer backbone is selected from acrylic resins, polyurethane resins and polyester resins.
[0080] Furthermore, the polymer beads included in the bead composition preferably comprise at least one or a mixture of two or more selected from polyethylene terephthalate (PET), nylon, polystyrene (PS), polybutyl methacrylate (PBMA), polymethyl methacrylate (PMMA), and melamine.
[0081] Furthermore, the curing agent included in the bead composition is an additive used to form the bead coating 40, and is generally preferably selected from curing agents applicable to acrylic resins, polyurethane resins, and polyester resins. Additionally, the bead composition preferably includes 0.01 to 0.2 parts by weight of curing agent relative to 100 parts by weight of the organic adhesive resin. In the bead composition, when the content of curing agent is less than 0.01 parts by weight, the organic adhesive resin cannot cure sufficiently, and the adhesion between the bead coating 40 and the antistatic layer 30 decreases; while when it exceeds 0.2 parts by weight, there is a problem of decreased miscibility of the bead composition.
[0082] Furthermore, the average particle size of the polymer beads included in the bead composition is preferably 0.5 to 10 μm, more preferably 4 to 8 μm. When the average particle size of the polymer beads is less than 0.5 μm, the polymer beads are not easily dispersed in the bead composition, while when the average particle size exceeds 10 μm, the polymer beads protrude outward from the bead coating 40 and fall off.
[0083] Furthermore, the thickness of the bead coating 40 is preferably 2 to 7 μm, more preferably 3 to 5 μm. When the bead coating thickness is less than 2 μm, the polymer beads cannot be sufficiently covered by the organic adhesive resin, which may result in particle protrusion or uneven coating. When the thickness exceeds 7 μm, it is not conducive to sheet film formation. In particular, since the bead coating 40 is formed in this invention to solve the problem of difficulty in separating the finished color conversion sheets due to static electricity, thereby improving process ease, the disadvantage of the bead coating 40 being unfavorable for sheet film formation outweighs the advantage of improved process ease when the thickness exceeds 7 μm.
[0084] Furthermore, the solvent used in the bead composition forming the bead coating 40 can be freely used as long as it is capable of uniformly dissolving or dispersing the mixed resin of the organic binder resin and the polymer beads included in the bead composition. For example, the solvent used for the bead composition can be water, alcohol, or ether-based solvents, but is not limited to these; various solvents can be used.
[0085] The surface resistance of the color conversion sheet according to an embodiment of the present invention, specifically the surface resistance measured on the surface of the bead coating 40, is preferably 1.0 × 10⁻⁶. 7 Ω / cm 2 The following applies when the surface resistivity exceeds 1.0 × 10⁻⁶. 7 Ω / cm 2 At that time, due to the high surface resistance, the antistatic effect is weak.
[0086] Furthermore, according to an embodiment of the present invention, after the color conversion sheet is heat-treated at 170°C for 4 minutes, the surface resistivity measured on the bead coating 40 is preferably 1.0 × 10⁻⁶. 7 Ω / cm 2 The following applies when the surface resistivity after heat treatment exceeds 1.0 × 10⁻⁶. 7 Ω / cm 2 During the manufacturing process of the color conversion sheet 100 or the subsequent manufacturing process of the backlight unit, the antistatic properties of the antistatic layer 30 decrease.
[0087] As described above, the color conversion sheet 100 according to an embodiment of the present invention has an antistatic layer 30 that maintains antistatic function even at high temperatures disposed on the lowermost back side, and a bead coating 40 is stacked on the surface of the antistatic layer 30, thereby ensuring ease of assembly with the light guide plate and antistatic function.
[0088] Figure 2 This is a structural diagram of a color conversion sheet according to another embodiment of the present invention.
[0089] refer to Figure 2 In another embodiment of the color conversion sheet 200 according to the present invention, the wavelength conversion section 17 includes a first wavelength conversion layer 15, a transparent layer 12 and a second wavelength conversion layer 16. Figure 1 The color conversion sheet 100 shown has a structure in which a wavelength conversion layer 11 encompasses both a green organic phosphor 13 and a red organic phosphor 14. Figure 2 The color conversion sheet 200 shown has a structure in which a first organic phosphor 13, serving as a green organic phosphor, and a second organic phosphor 14, serving as a red organic phosphor, are separated and located in separate first wavelength conversion layers 15 and second wavelength conversion layers 16, respectively. The detailed structure of the color conversion sheet 200 will be described below. However, for... Figure 1 The repeated description of the same composition and structure as the color conversion sheet 100 will be omitted.
[0090] exist Figure 2In the color conversion sheet 200 shown, a wavelength conversion section 17, on a substrate layer 20, is sequentially stacked with a first wavelength conversion layer 15, a transparent layer 12, and a second wavelength conversion layer 16, and a light diffusion layer 50 is located on the second wavelength conversion layer 16 of the wavelength conversion section 17. That is, multiple layers are formed, including a first wavelength conversion layer 15 comprising a first resin matrix 19a (containing a first organic phosphor 13) and a second wavelength conversion layer 16 comprising a second resin matrix 19b (containing a second organic phosphor 14).
[0091] At this point, the closer the second organic phosphor 14, which is a red organic phosphor, is to the first organic phosphor 13, which is a green organic phosphor, the easier it is for the green light to be absorbed, thereby increasing the luminous efficiency of the red light. Therefore, in a color conversion sheet containing the same amount of organic phosphors 13 and 14, various white lights can be achieved by adjusting the distance between these organic phosphors 13 and 14. However, when the green organic phosphor 13 and the red organic phosphor 14 are included together in a resin matrix composed of a single layer, the distance between them may change significantly due to the influence of the surrounding environment (e.g., high temperature or high humidity). This can alter the luminous efficiency of the red organic phosphor 14, and ultimately may change the color coordinates of the white light that can be converted by the color conversion sheet or reduce reliability. On the other hand, when a resin matrix layer including a green organic phosphor 13 and a resin matrix layer including a red organic phosphor 14 are in contact with each other to form multiple layers, over time, the green or red organic phosphors present at the interface of each layer may diffuse to the interface of another layer. As a result, the distance between the red organic phosphor 14 and the green organic phosphor 13 becomes closer, changing the luminous efficiency of the red organic phosphor 14, which may change the color coordinates of white light or reduce reliability.
[0092] Therefore, in this invention, as Figure 2 As shown, the color conversion sheet 200, by distributing a transparent layer 12 between a first wavelength conversion layer 15 including a green (first) organic phosphor 13 and a second wavelength conversion layer 16 including a red (second) organic phosphor 14, completely separates the first and second wavelength conversion layers 15 and 16, thereby maintaining a certain distance between the green organic phosphor 13 and the red organic phosphor 14. This allows the luminous efficiency of the red organic phosphor 14 to be maintained at a certain level, thereby preventing changes in the color coordinates of the white light emitted by the color conversion sheet 200 and a decrease in reliability.
[0093] That is, according to another embodiment of the present invention, the color conversion sheet 200 prevents the green and red organic phosphors 13 and 14 included in the first and second wavelength conversion layers 15 and 16 from diffusing or mixing with the first resin matrix 19a and the second resin matrix 19b by distributing a transparent layer 12 between the first wavelength conversion layer 15 and the second wavelength conversion layer 16, thereby achieving the technical effect of high color uniformity and uniform brightness even in high temperature and high humidity environments.
[0094] The thicknesses of the first wavelength conversion layer 15 and the second wavelength conversion layer 16 according to the present invention are preferably 1 to 150 μm, more preferably 5 to 100 μm.
[0095] Furthermore, in the wavelength conversion section 17, preferably, the refractive index of the wavelength conversion layer (the wavelength conversion layer furthest from the light source) at the location where the incident light finally exits is less than that of the transparent layer 12. For example, preferably, when the incident light finally exits through the first wavelength conversion layer 15, the refractive index of the transparent layer 12 is greater than that of the first wavelength conversion layer 15; conversely, when the incident light finally exits through the second wavelength conversion layer 16, the refractive index of the transparent layer 12 is greater than that of the second wavelength conversion layer 16. That is, Figure 2 The color conversion chip 200 shown is applied to Figure 3 When the backlight unit is in use, light is emitted through the second wavelength conversion layer 16. Therefore, the refractive index of the second wavelength conversion layer 16 can be less than that of the transparent layer 12. This is because it can improve the light reflectivity of the transparent layer 12, thus effectively emitting the color-converted light to the outside.
[0096] Next, referring to a schematic diagram of a backlight unit including a color conversion sheet as an embodiment of the present invention... Figure 3 A backlight unit 900 including a color conversion sheet according to an embodiment of the present invention will be described.
[0097] According to an embodiment of the present invention, a backlight unit 900 may include a light source 700, a reflector 500 which can improve light efficiency by reflecting light emitted from the light source 700, a light guide plate 300 located on the upper part of the reflector 500 and serving to uniformly diffuse the light emitted from the light source 700, and color conversion sheets 100 and 200 located on the upper part of the light guide plate 300.
[0098] Among them, color conversion sheets 100 and 200 are applicable to the above. Figure 1 or Figure 2The same color conversion sheet described in the illustrated embodiments will be omitted from repeated descriptions. In addition, the upper part of the color conversion sheet 100 may include more than one optical sheet, such as a diffuser sheet, a prism sheet, a dual brightness enhancement film (DBEF), etc.
[0099] The structure of the present invention and its effects will now be described in more detail through embodiments and comparative examples. However, these embodiments are only used to illustrate the purpose of the present invention more specifically, and the scope of the present invention is not limited to these embodiments.
[0100] [Example] [Example 1] (Step 1) Formation of antistatic layer and bead coating An antistatic composition was prepared by dispersing 1g of PEDOT / PSS (Baytron PH, manufacturer: Bayer), 133.3g of polyurethane resin with fluorinated hydrocarbon side chains (manufacturer: Daihsei Kagaku Co., Ltd.) with a solid content of 15% by weight, and 0.4g of aziridine curing agent (manufacturer: DOORICHEM) in 100g of a mixed solvent including water, ethanol, isopropanol and butanol (in a weight ratio of 20 / 55 / 20 / 5). The antistatic composition was then coated onto the underside of a 100μm thick polyester film (TAK Corporation, XG7PH8) and dried to form a 50nm thick antistatic layer.
[0101] Next, 0.1 g of PBMA particles with an average particle size of 6 μm and 80 g of acrylic resin (Mihara Co., AT-2100) including 0.024 g of curing agent (Sanwa Co., SC70I) were dispersed in 100 g of ethyl acetate solvent to prepare a bead composition. This bead composition was then coated onto an antistatic layer and dried to form a bead coating with a thickness of 5 μm. Subsequently, a wavelength conversion section was formed on the opposite side of the antistatic layer where the polyester film was formed.
[0102] (Step 2) Formation of the wavelength conversion layer An organic phosphor solution was prepared by dissolving a green organic phosphor according to Formula 1 and a red organic phosphor according to Formula 2 in ethyl acetate at equal weights. A polyester resin (Toyobo Co., Ltd., Vylon 630) was then mixed into the organic phosphor solution, and ethyl acetate was added to adjust the viscosity to 150 cps. The mixture was then stirred at 150 rpm for 30 minutes to prepare the wavelength conversion layer composition. At this point, the total content of the organic phosphors (red and green organic phosphors) was 0.72 parts by weight relative to 100 parts by weight of the solid content of the polyester resin.
[0103] Next, the prepared wavelength conversion layer composition is applied to the opposite side of the antistatic layer on which the polyester film is formed, and then dried at 170°C for 4 minutes to form a wavelength conversion layer with a thickness of 10 μm.
[0104] (Step 3) Formation of the transparent layer Next, 80 parts by weight of toluene were added relative to 100 parts by weight of silicone resin (Dow, 7904), and after stirring for 2 hours, 0.05 parts by weight of platinum catalyst (Dow, SYL-OFF 4000 CATALYST) were added, and then stirred for another 30 minutes to prepare a transparent layer composition. The prepared transparent layer composition was coated on the opposite side of the diffusion layer of a diffusion film (TFN, TDV10F), and then dried at 170°C for 2 minutes to form a transparent layer with a thickness of 24 μm.
[0105] (Step 4) Preparation of color conversion film Next, the wavelength conversion layer and transparent layer prepared as described above are laminated in a contact manner, and a color conversion sheet is manufactured using a roll-to-roll laminator (GMP, EXCELAM Ⅱ-355Q).
[0106] [Example 2] The color conversion sheet was manufactured in the same manner as in Example 1, except that 6g of PEDOT / PSS (Baytron PH, manufacturer: Bayer) was used in the antistatic layer.
[0107] [Example 3] The color conversion sheet was manufactured in the same manner as in Example 1, except that 0.2 g of PEDOT / PSS (Baytron PH, manufacturer: Bayer) was used in the antistatic layer and 0.24 g of PBMA particles was used in the bead coating.
[0108] [Comparative Example 1] Except for the absence of an antistatic layer, the color conversion sheet was manufactured in the same manner as in Example 1.
[0109] [Comparative Example 2] The color conversion sheet was manufactured in the same manner as in Example 1, except that 7g of PEDOT / PSS (Baytron PH, manufacturer: Bayer) was used.
[0110] [Comparative Example 3] The color conversion sheet was manufactured in the same manner as in Example 1, except that 0.1g of PEDOT / PSS (Baytron PH, manufacturer: Bayer) was used.
[0111] [Comparative Example 4] The color conversion sheet was manufactured in the same manner as in Example 1, except that 0.3g of PBMA particles were used in the bead coating.
[0112] [Comparative Example 5] The color conversion sheet was manufactured in the same manner as in Example 1, except that 0.07g of PBMA particles were used in the bead coating.
[0113] Using the color conversion sheets according to Examples 1 to 3 and Comparative Examples 1 to 5, the physical properties were measured through the following experimental examples, and the results are shown in Table 1 below.
[0114] [Experimental Example] (1) Measurement of color coordinates The color coordinates (x, y) of the color conversion sheets according to the embodiments and comparative examples were measured using a spectroradiometer (KONICA MINOLTA, CA-S20W).
[0115] (2) Measurement of adhesive strength To measure the adhesive force between the transparent layer and the wavelength conversion layer, for the embodiments and comparative examples, without the formation of the antistatic layer and the bead coating, one side of the polyester film laminated on the wavelength conversion layer was attached to the SUS plate and fixed. Then, a tensile testing machine (LLOYD, L / F Plus) was used to peel the diffusion film laminated on the transparent layer at room temperature (25°C) at a peeling speed of 300 mm / min and 180 degrees relative to the polyester film, thereby measuring the adhesive force between the transparent layer and the wavelength conversion layer.
[0116] (3) Measurement of surface resistance For the embodiments and comparative examples, the surface resistance was measured on the bead coating surface in step 2 using a surface resistance meter (Advantest, R8340A). At this time, the surface resistance measured immediately after the formation of the antistatic layer and bead coating in step 1 was taken as the surface resistance before heat treatment (initial surface resistance), and the surface resistance (final surface resistance) was measured after the final color conversion sheet was manufactured through the coating, drying, and bonding process in step 2. For reference, it was confirmed that the formation of the transparent layer in step 3 did not affect the surface resistance.
[0117] (4) Confirmation of sheet appearance For the embodiments and comparative examples, the appearance of the color conversion sheet was evaluated by visual inspection. When no particles or stains were visible to the naked eye, it was marked as "O"; when aggregated particles were visible or surface stains appeared, it was marked as "X".
[0118] (5) Evaluation of anti-adhesion properties After overlapping the two color conversion sheets from the examples and comparative examples, at 1 kg / cm² 2The plates were placed under pressure for 24 hours, and then evaluated to see if adhesion occurred when the two plates were separated. If the two plates separated immediately due to their own weight, it was marked as "O"; if they did not separate immediately due to their own weight, it was marked as "X".
[0119] The experimental results of the color conversion film based on the experimental example are shown in Table 1.
[0120] Table 1
[0121] As shown in Table 1, in Examples 1 to 3, the surface resistivity of the bead coating at the bottom edge remained well maintained at 1.0 × 10⁻⁶ after both the initial application and the completion of the color conversion sheet. 7 Ω / cm 2 In particular, even when subjected to a heat treatment at 170°C for 4 minutes during the manufacturing process, the surface resistivity required by the present invention was maintained. Furthermore, in Examples 1 to 3, it was confirmed that the adhesion between the wavelength conversion layer and the transparent layer was above 800 gf / inch, the color conversion sheet was manufactured stably, and it was also confirmed that there were no problems with the ease of assembly with the light guide plate.
[0122] Conversely, as can be seen in Comparative Example 1, the surface resistance value significantly exceeds 1.0 × 10⁻⁶ from the initial stage. 7 Ω / cm 2 Furthermore, after a high-temperature (170°C) drying process, it exhibits a density of 1.0 × 10⁻⁶. 13 Ω / cm 2 The above surface resistance values completely negate the antistatic function.
[0123] Furthermore, as shown in Comparative Example 2, poor appearance occurred due to excessive conductive polymer content; and as shown in Comparative Example 3, due to insufficient conductive polymer content, the surface resistivity exceeded 1.0 × 10⁻⁶ after heat treatment at 170°C for 4 minutes. 7 Ω / cm 2 This reduces the antistatic function.
[0124] Furthermore, as seen in Comparative Example 4, which excessively includes polymer beads, the polymer beads are difficult to disperse, resulting in poor appearance.
[0125] Furthermore, it was confirmed that in Comparative Example 5, where the content of polymer beads was insufficient, the ease of assembly with the light guide plate decreased. More specifically, as in Comparative Example 5, when the content of polymer beads was less than 0.1 parts by weight, when different color conversion sheets came into contact with each other, due to insufficient particles, no air layer was formed between the different color conversion sheets, resulting in decreased anti-adhesion. The sheets adhered to each other due to static electricity generated between them, making it difficult to separate them easily by their own weight, thus causing difficulties in the assembly operation.
[0126] While the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto. Various modifications and improvements made by those skilled in the art using the basic concepts of the present invention as defined in the claims also fall within the scope of the present invention.
Claims
1. A color conversion chip, characterized in that, include: Substrate layer; A wavelength conversion section is located on one side of the substrate layer and includes an organic phosphor and a matrix resin; An antistatic layer is located on the other side of the substrate layer; A bead coating is formed by applying it onto the antistatic layer.
2. The color conversion sheet according to claim 1, characterized in that, The antistatic composition forming the antistatic layer includes an organic adhesive resin, a conductive polymer, and a curing agent.
3. The color conversion sheet according to claim 2, characterized in that, The antistatic composition forming the antistatic layer comprises 1 to 30 parts by weight of a conductive polymer relative to 100 parts by weight of organic adhesive resin.
4. The color conversion sheet according to claim 2, characterized in that, The organic adhesive resin of the antistatic layer includes a mixture of one or more resins selected from acrylic resins, polyurethane resins and polyester resins or copolymers thereof.
5. The color conversion sheet according to claim 2, characterized in that, The conductive polymer includes one or more selected from polythiophene, polyaniline, polypyrrole, PEDOT, and PEDOT / PSS.
6. The color conversion sheet according to claim 1, characterized in that, Regarding the color conversion sheet, the surface resistivity measured on the bead-coated surface is 1.0 × 10⁻⁶. 7 Ω / cm 2 the following.
7. The color conversion sheet according to claim 1, characterized in that, Regarding the color conversion sheet, after a heat treatment at 170°C for 4 minutes, the surface resistivity measured on the bead coating surface was 1.0 × 10⁻⁶. 7 Ω / cm 2 the following.
8. The color conversion sheet according to claim 1, characterized in that, The thickness of the antistatic layer is 10 to 500 nm.
9. The color conversion sheet according to claim 1, characterized in that, The bead composition forming the bead coating includes an organic adhesive resin, polymer beads, and a curing agent.
10. The color conversion sheet according to claim 9, characterized in that, The bead composition forming the bead coating comprises 0.1 to 0.3 parts by weight of polymer beads relative to 100 parts by weight of organic adhesive resin.
11. The color conversion sheet according to claim 9, characterized in that, The polymer beads comprise one or a mixture of two or more selected from polyethylene terephthalate, nylon, polystyrene, polybutyl methacrylate, polymethyl methacrylate, and melamine.
12. The color conversion sheet according to claim 9, characterized in that, The organic adhesive resin of the bead coating comprises a mixture of one or more selected from acrylic resins, polyurethane resins, and polyester resins, or copolymers thereof.
13. The color conversion sheet according to claim 9, characterized in that, The average particle size of the polymer beads is 0.5 to 10 μm.
14. The color conversion sheet according to claim 1, characterized in that, The thickness of the bead coating is 2 to 7 μm.
15. The color conversion sheet according to claim 1, characterized in that, Also includes: A light diffusion layer is located on the wavelength conversion section and improves light diffusion and light efficiency.
16. The color conversion sheet according to claim 1, characterized in that, The wavelength conversion unit includes: A wavelength conversion layer, located on one side of the substrate layer, includes an organic phosphor and a matrix resin; and A transparent layer is located on the wavelength conversion layer.
17. The color conversion sheet according to claim 16, characterized in that, The adhesion between the wavelength conversion layer and the transparent layer is greater than 800 gf / inch.
18. The color conversion sheet according to claim 1, characterized in that, The wavelength conversion unit includes: A first wavelength conversion layer is located on one side of the substrate layer, and a first organic phosphor is dispersed in a first resin matrix. A transparent layer is located on the first wavelength conversion layer. A first wavelength conversion layer is located on the transparent layer, and a second organic phosphor is dispersed in a second resin matrix.
19. The color conversion sheet according to claim 16 or 18, characterized in that, The transparent layer is a polymer film selected from one or more of polyethylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyetherimide and polyimide.
20. A backlight unit equipped with a color conversion sheet according to claim 1.