All-dielectric structural color film
Through the design of structural color films alternately stacked with high and low refractive index dielectric layers, the problem that all-dielectric structural color films cannot appear black on a black substrate is solved, achieving color changes and high saturation at different viewing angles, and is suitable for a variety of applications Decorative and anti-counterfeiting applications.
Patent Information
- Application Number
- CN202420615266.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2034-03-27
AI Technical Summary
Existing all-dielectric structural color films cannot appear black on a black substrate, and cannot achieve low reflection and high transmission effects in the visible light band 400-700nm, which affects the display of the substrate color.
It adopts a structural color film design in which high and low refractive index dielectric layers are alternately stacked. The central wavelength of the dielectric layer is in the range of 700nm to 1000nm. The outer layer is a low refractive index dielectric layer. By adjusting the period number and thickness coefficient, the color can be achieved at different viewing angles. changes, using the electron beam evaporation process to improve the saturation of the film and the additive color mixing effect.
It achieves the appearance of black on a black base, turns to red when 60° oblique incidence, and appears purple on a blue base, which improves color quality and saturation, avoids the use of metal materials, and is suitable for decoration and anti-counterfeiting products.
Smart Images

Figure CN221883930U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of structural color films, in particular to a full-medium structural color film. Background Art
[0002] Structural color is achieved by constructing different micro-nano structures to achieve physical effects such as diffraction, scattering and interference, and ultimately achieve the regulation of visible light to show different colors. Its raw materials are widely available, environmentally friendly and have a long lifespan. It is widely used in anti-counterfeiting, display, solar panels and cosmetics. Among them, the research on structural color thin film devices based on the interference effect of multilayer thin films is hot. This solution does not require the use of more complex process technologies such as lithography, plasma etching or self-assembly, and is suitable for large-scale low-cost commercial production. There are currently two main technical solutions for achieving interference structural color with multilayer thin films. One is an optical interference structural color film based on the Fabry-Perot metal-medium structure, such as patent CN100482746C, which deposits metal layers, dielectric layers and absorption layers in sequence. Its reflective layer is generally composed of highly reflective metals such as aluminum, silver, gold, copper, platinum, titanium, chromium, nickel, cobalt, rhodium, niobium and their alloys. Due to the presence of the metal bottom reflective layer, this type of structural color thin film device is completely covered with the substrate, and the color of the substrate will not participate in the overall color development of the structural color film. The other type is a structural color film based on an all-dielectric multilayer film. This type of structure does not cover the substrate. For example, the all-dielectric optical interference pigment described in the patent application CN100475915C mainly constructs multiple reflection peaks in the visible light band to achieve different color displays in the visible light band. However, at a vertical observation angle, the color of the substrate will be superimposed on the color of the all-dielectric multilayer interference film, and the color of the substrate itself cannot be presented. This type of structure cannot be combined with a black substrate to present black, and the interference reflection color of the film is presented on the black substrate. For the currently available transparent all-dielectric structural color films, it is impossible to achieve a wide-band low reflection and high transmission effect in the visible light band of 400-700nm, thereby achieving the effect of not affecting the color of the substrate. Utility Model Content
[0003] In view of this, the purpose of the utility model is to propose an all-medium structural color film with a significant angle-dependent color effect. When the film is deposited on a black substrate, it appears black when observed vertically, and red when observed at an oblique incidence of 60°, with the effect that the color changes from black to red as the observation angle changes; and when the film is deposited on a blue substrate, it appears blue when observed vertically, and an additive color mixture of the substrate blue and the film red when observed at an oblique incidence of 60°, i.e., purple-red, with the effect that the color changes from black to red as the observation angle changes.
[0004] According to one aspect of the utility model, a full-dielectric structural color film is provided, wherein the structural color film is formed by stacking a plurality of high-refractive index dielectric layers and a plurality of low-refractive index dielectric layers in sequence, and the central wavelength of the dielectric layer varies in the range of 700nm to 1000nm. The outermost layer of the structural color film is a low-refractive index dielectric layer, and the basic thickness coefficient value of the low-refractive index dielectric layer is 0.4-0.6QWOT.
[0005] In the above technical solution, the basic structure is (HL)^n(0.4-0.6L), wherein the (HL) periodic unit can adjust the peak value of the reflection peak in the near-infrared 700-1000nm band. As the number of periods n increases, the peak reflectivity will be effectively improved and affect the additive color mixing effect at an inclined angle (45-60 degrees). The structure takes a certain value λ in the 700-1000nm band as the central wavelength, and the thickness of a single H or L is one-fourth of λ. The purpose of the last layer of 0.4-0.6L is to reduce the sideband reflection peak in the visible light band so as not to affect the base color and to improve the saturation of the film structural color at normal incidence.
[0006] In some embodiments, the refractive index difference between the high refractive index medium layer and the low refractive index medium layer should be ≥ 0.2.
[0007] In the above technical solution, the purpose is to achieve alternating superposition of high and low refractive index materials.
[0008] In some embodiments, the basic structure of the structural color film is as follows:
[0009] (aHbL)^n aH cL
[0010] Wherein, a, b, c represent thickness coefficients in the range of one quarter optical thickness, the coefficient variation range is a: 0.8~1.2, b: 0.8~1.2, c: 0.4~0.6, and n is the number of repetition periods of the (HL) periodic unit, n: 1-20.
[0011] In the above technical solution, the basic structure is (aHbL)^n aH cL, which takes a certain value λ in the 700nm~1000nm band as the central wavelength, the thickness of a single H or L is one-quarter of the optical thickness of λ, 1H or 1L represents one-quarter of the optical thickness of 1 λ, a, b, c represent thickness coefficients with a range of one-quarter optical thickness, the coefficient variation range is a: 0.8~1.2, b: 0.8~1.2, c: 0.4~0.6, n is the number of repetition periods of the (HL) periodic unit, n: 1-20, the central wavelength λ is located in the near-infrared 700nm~1000nm band, with the increase of the period number n, the peak reflectivity in the infrared 700nm~1000nm band will be effectively improved, and affect the additive color mixing effect under the tilt angle (45-60 degrees). The purpose of the last layer cL is to reduce the sideband reflection peak in the visible light band, so as not to affect the base color, and to improve the saturation of the film structural color at normal incidence. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the embodiments of the utility model or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0013] Figure 1 This is a schematic diagram of the structure of a full dielectric structural color film according to an embodiment of the utility model.
[0014] Figure 2 This is a comparison of the reflection spectra of a quarter-wavelength regular film system and an optimized film system of an embodiment of an all-dielectric structural color film of the utility model.
[0015] Figure 3 This is a specific example of an embodiment of an all-dielectric structural color film of the utility model. Spectral comparison at normal incidence and 60° oblique incidence
[0016] Figure 4 This is a specific example of an embodiment of an all-medium structural color film of the utility model. The chromaticity coordinates at normal incidence and 60° oblique incidence
[0017] Figure 5 This is a specific example 2 of an embodiment of an all-dielectric structural color film of the utility model. Spectral comparison at normal incidence and 60° oblique incidence
[0018] Figure 6 The chromaticity coordinates of the second embodiment of the all-medium structural color film of the utility model at normal incidence and 60° oblique incidence are
[0019] Figure 7 This is a specific example of an embodiment of an all-dielectric structural color film of the utility model. Spectral comparison at normal incidence and 60° oblique incidence
[0020] Figure 8 The chromaticity coordinates of the three normal incidence and 60° oblique incidence of a specific example of an embodiment of an all-medium structural color film of the utility model are as follows: DETAILED DESCRIPTION
[0021] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It is particularly noted that the following embodiments are only used to illustrate the present invention, but do not limit the scope of the present invention. Similarly, the following embodiments are only partial embodiments of the present invention rather than all embodiments. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The utility model provides a full-medium structural color film with a significant angle-dependent color effect. When the film is deposited on a black substrate, it appears black when observed vertically, and red when observed at an oblique incidence of 60 degrees, with the effect that the color changes from black to red as the observation angle changes; and when the film is deposited on a blue substrate, it appears blue when observed vertically, and an additive mixed color of the substrate blue and the film red when observed at an oblique incidence of 60 degrees, that is, purple-red, with the effect that the color changes from black to red as the observation angle changes.
[0023] See also Figure 1 , a full-dielectric structural color film, which is formed by alternating a plurality of high-refractive index medium layers and a plurality of low-refractive index medium layers on a substrate, and the central wavelength variation range of the medium layer is 700nm-1000nm; wherein the outermost layer of the structural color film is a low-refractive index medium layer, and the basic thickness coefficient value of the low-refractive index medium layer is 0.5QWOT.
[0024] In this embodiment, a non-absorbing dielectric material with a high (H) and low (L) refractive index is stacked on a substrate material, including two parts: a substrate of different colors and a multilayer film that is transparent to visible light (400-700nm) and highly reflective to near infrared (700-100nm), such as Figure 1The schematic diagram of the film structure is shown. The high and low refractive index dielectric materials in the structure can be selected from one or more of titanium oxide, tantalum oxide, niobium oxide, hafnium oxide, zirconium oxide, yttrium oxide, lanthanum titanate, silicon dioxide, aluminum oxide, and metal fluoride, with a refractive index range of 1.2-3.0, and the refractive index difference between the two should be greater than or equal to 0.2. The substrate materials of different colors can be highly polished glass, polished stainless steel, and polished mirror aluminum. According to needs, the substrate can also be one of the optical plastic substrates such as polyethylene terephthalate (PET), triacetyl cellulose (TAC), polymethyl methacrylate (PMMA), polycarbonate / polymethyl methacrylate composites (PC / PMMA), polyimide (PI), polypropylene (PP), polyvinyl chloride (PVC), polyvinyl butyral (PVB), ethylene vinyl acetate copolymer (EVA) or polyurethane elastomer (TPU), polytetrafluoroethylene (PTFE), fluoroethyl propylene (FEP), polyvinyl difluoride (PVDF), etc.
[0025] In this embodiment, the basic structure is (aHbL)^n aH(cL), which takes a certain value λ in the 700-1000nm band as the central wavelength, the thickness of a single H or L is one-quarter optical thickness of λ, 1H or 1L represents one-quarter optical thickness of 1 λ, a, b, c represent thickness coefficients in units of one-quarter optical thickness, the coefficients vary in the range of a: 0.8-1.2, b: 0.8-1.2, c: 0.4-0.6, n is the number of repetition periods of the (HL) period unit, n: 1-20; the central wavelength λ is located in the near-infrared 700-1000nm band, and as the number of periods n increases, the peak reflectivity in the infrared 700-1000nm band will be effectively improved, and affect the additive color mixing effect at an inclined angle (45-60 degrees). The purpose of the last layer c0.5L is to reduce the sideband reflection peak in the visible light band so as not to affect the base color and improve the saturation of the film structural color at normal incidence.
[0026] In order to achieve high transparency in the visible light range of 400-700nm, the thickness of the above-mentioned basic structure needs to be fine-tuned. The coefficient range of thickness fine-tuning is a: 0.8~1.2, b: 0.8~1.2, c: 0.4~0.6, such as Figure 2 As shown in the comparison of the reflection spectra of the same film system with a regular quarter film thickness and after fine-tuning and optimization of the film thickness, the regular quarter film system has two higher reflection peaks in the visible light region (the highest value is 28%), while the highest reflection of the film after fine-tuning and optimization does not exceed 5%.
[0027] In this embodiment, the structural color multilayer thin film device is deposited using an ion-assisted electron beam evaporation process. Electron beam evaporation allows the film material to obtain energy and deposits it on the substrate. Since the electron beam has extremely high energy, various high-melting-point film materials can be completely melted and vaporized in a short time to grow a high-purity film layer. Moreover, during vapor deposition, bombarding the deposited film material with ions with a certain amount of energy can significantly improve the bonding strength between the film and the substrate.
[0028] In this embodiment, when the structural color film is observed vertically, since its reflection peak is in the near infrared (700-1000nm), rather than in the visible light band that can be perceived by the human eye, and the visible light (400-700nm) is fully transparent and low-reflective, the film as a whole will directly present the color of the substrate without the influence of additional reflection peaks, that is, if the substrate is black, the entire film will appear black, and if the substrate is blue, the entire film will appear blue, with high color quality. At an inclined observation angle (45-60 degrees), due to the inherent effect of the medium film spectrum moving toward the short wave with the incident angle, the reflection peak in the near infrared band moves toward the short wave into the red band 600nm-700nm, forming a high reflection in the red region and superimposing with the reflection peak of the substrate color, from the perspective of human vision, a significant color change will occur, that is, if the film is deposited on a black substrate, the color presentation is the effect of black turning into red. If the film is deposited on a blue substrate, it will turn from blue to purple-red (additive mixing of the substrate blue and the film red).
[0029] This embodiment optimizes the material selection of traditional structural color films, avoids the use of organic materials and heavy metals, and avoids the phenomenon that the color of the previous all-medium structural color film substrate material is limited to black. It achieves one color at normal incidence and another color at 60-degree oblique incidence, such as black turning red on a black substrate and blue turning purple on a blue substrate. It has a significant angle-dependent color effect and is expected to be applied to various decorative objects and anti-counterfeiting products.
[0030] One of the specific examples
[0031] As shown in the table below, a multilayer all-dielectric structural color film consists of a substrate Sub (BK7), a high refractive index material H (TiO2), and a low refractive index material (MgF2), and the high refractive index material and the low refractive index material are stacked alternately.
[0032]
[0033] The total number of layers in this specific example is 14, the quarter optical thickness coefficients of each layer are as shown in the table, and the central wavelength λ is 850 nm. Figure 3 The following are the reflection spectra of the structural color film at 0° and 60° incidence. When sunlight is incident directly on the film, the reflection spectrum is as follows: Figure 3 As shown by the solid line in the middle, it has a high reflectivity (about 99%) only in the 750-1050nm band, and has a low reflectivity (the average value is less than 1%) in the visible light band of 400-700nm. The sunlight is completely transmitted and reflected back as the light of the base color (black if the base is black, blue if it is blue); when the sunlight is incident on the film at 60°, the reflection spectrum is as follows Figure 3 As shown by the middle dotted line, the multilayer film has a lower reflectivity in the 430-585nm band with an average value of less than 10%, and a higher reflectivity (97%) in the 650-800nm band. At this time, the object exhibits additive mixing of the base color and the film color (red if the base is black, and purple if the base is blue). Figure 4 The chromaticity coordinate diagram of Example 1 at 0° and 60° is shown. The light source used is D65. When the incident light is 0°, the chromaticity coordinates of the reflected light are (0.3275, 0.3171); when the incident light is 60°, the chromaticity coordinates of the reflected light are (0.4156, 0.2267).
[0034] Specific example two
[0035] As shown in the table below, a multilayer all-dielectric structural color film consists of a substrate Sub (BK7), a high refractive index material H (Y2O3), and a low refractive index material (MgF2), and the high refractive index material and the low refractive index material are stacked alternately.
[0036]
[0037] The total number of layers in this specific example is 18, the quarter optical thickness coefficients of each layer are as shown in the table, and the central wavelength λ is 850 nm. Figure 5 The following are the reflection spectra of the structural color film at 0° and 60° incidence. When sunlight is incident directly on the film, the reflection spectrum is as follows: Figure 5 As shown by the solid line in the middle, it has a high reflectivity (about 95%) only in the 775-925nm band, and has a low reflectivity (the average value is less than 1%) in the visible light band of 400-725nm. The sunlight is completely transmitted and reflected back as the light of the base color (black if the base is black, blue if it is blue); when the sunlight is incident on the film at 60°, the reflection spectrum is as follows Figure 5 As shown by the middle dotted line, the multilayer film has a lower reflectivity in the 400-600nm band with an average reflectivity of less than 2.5%, and a higher reflectivity in the 625-750nm band (up to 83%). At this time, the object exhibits additive mixing of the base color and the film color (red if the base is black, and purple if the base is blue). Figure 6The chromaticity coordinate diagram of Example 1 at 0° and 60° is shown. The light source used is D65. When the incident light is 0°, the chromaticity coordinates of the reflected light are (0.2951, 0.2640); when the incident light is 60°, the chromaticity coordinates of the reflected light are (0.5798, 0.3029).
[0038] Specific example three
[0039] As shown in the table below, a multilayer all-dielectric structural color film is composed of a substrate Sub (BK7), a high refractive index material H (SiO2), and a low refractive index material (Al2O3), and the high refractive index material and the low refractive index material are stacked alternately.
[0040]
[0041]
[0042] In this specific example, the total number of layers is 18, and the quarter optical thickness coefficient of each layer is shown in the table. The central wavelength λ is 800nm. Since the refractive index difference between the two materials is small (0.2), the optical thickness of the film layer of this film system can directly use one quarter of the central wavelength to achieve the effect of low reflection and high transmission of visible light. Figure 7 The following are the reflection spectra of the structural color film at 0° and 60° incidence. When sunlight is incident directly on the film, the reflection spectrum is as follows: Figure 7 As shown by the solid line in the middle, it has a high reflectivity only in the 775-875nm band (Gaussian line shape, up to 70%), and has a low reflectivity in the visible light band of 400-750nm (average value is 3%). The sunlight is completely transmitted and reflected back as the light of the base color (black if the base is black, blue if the base is blue); when the sunlight is incident on the film at 60°, the reflection spectrum is as follows Figure 7 As shown by the middle dotted line, the multilayer film has a lower reflectivity in the 400-600nm band with an average value of less than 6%, and a higher reflectivity (60%) in the 625-725nm band. At this time, the object exhibits additive mixing of the base and the film color (red if the base is black, and purple if the base is blue). Figure 8 The chromaticity coordinate diagram of Example 1 at 0° and 60° is shown. The light source used is D65. When the incident light is 0°, the chromaticity coordinates of the reflected light are (0.2956, 0.3157); when the incident light is 60°, the chromaticity coordinates of the reflected light are (0.4547, 0.3036).
[0043] The above descriptions are only some embodiments of the present invention, and do not limit the protection scope of the present invention. Any equivalent device or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. An all-dielectric structural color film, characterized in that: The structural color film is formed by alternately stacking a plurality of high-refractive index medium layers and a plurality of low-refractive index medium layers on a substrate, and the central wavelength of the medium layer is 700nm-1000nm; wherein, the outermost layer of the structural color film is a low-refractive index medium layer, and the thickness coefficient value of the low-refractive index medium layer is 0.4-0.6QWOT.
2. The all-dielectric structural color film according to claim 1, characterized in that: The refractive index difference between the high refractive index medium layer and the low refractive index medium layer is ≥0.
2.
3. The all-dielectric structural color film according to claim 1, characterized in that: The basic structure of the structural color film is as follows: (aHbL)^n aH cL Wherein, a, b, c represent thickness coefficients in the range of one quarter optical thickness, the coefficient variation range is a: 0.8~1.2, b: 0.8~1.2, c: 0.4~0.6, and n is the number of repetition periods of the (HL) periodic unit, n: 1-20.
4. The all-dielectric structural color film according to claim 1, characterized in that: The substrate material is one of polyethylene terephthalate, cellulose triacetate, polymethyl methacrylate, polycarbonate / polymethyl methacrylate composite material, polyimide, polypropylene, polyvinyl chloride, polyvinyl butyral, ethylene vinyl acetate copolymer, polyurethane elastomer, polytetrafluoroethylene, fluoroethyl propylene, and polyvinylidene fluoride.
5. The all-dielectric structural color film according to claim 1, characterized in that: The dielectric layer is made of one or more of titanium oxide, tantalum oxide, niobium oxide, hafnium oxide, zirconium oxide, yttrium oxide, lanthanum titanate, silicon dioxide, aluminum oxide, and metal fluoride, and has a refractive index ranging from 1.2 to 3.0.