Secondary battery with non-aqueous electrolyte
By integrating a saturated cyclic hydrocarbon group into the positive electrode, the battery ensures timely power cut-off during overcharging, addressing the balance between gas generation and performance in non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- DE102015100122
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-01-08
- Filing Date
- 2015-01-07
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2035-01-07
AI Technical Summary
Conventional non-aqueous electrolyte secondary batteries face a challenge in balancing the generation of adequate gas for power cut-off mechanisms with maintaining battery performance, as increasing gas generators can cause resistance, while reducing them may delay mechanism activation.
Incorporating a compound with a saturated cyclic hydrocarbon group, such as cyclohexylbenzene, into the positive electrode active material layer of the battery, which functions as a gas generator when the voltage exceeds a threshold, ensuring timely power cut-off without compromising battery performance.
The solution allows for effective activation of the power cut-off mechanism during overcharging while maintaining high battery performance, including low resistance and superior stability.
Smart Images

Figure 00000011_0000 
Figure 00000012_0000 
Figure 00000013_0000
Abstract
Description
BACKGROUND OF THE INVENTION 1. Field of the Invention
[0001] The present invention relates to a secondary battery provided with a non-aqueous electrolyte (non-aqueous electrolyte secondary battery). 2. State of the art
[0002] Lithium-ion secondary batteries and other non-aqueous electrolyte secondary batteries are becoming increasingly important as vehicle-mounted power sources and power sources for personal computers, portable devices, and the like. In particular, lithium-ion secondary batteries are preferred as vehicle-mounted high-output power sources because of their lightweight nature and the ability to achieve high energy densities (see, for example, JP 2013-157139 A). When such non-aqueous electrolyte secondary batteries are overcharged, an excessive amount of charge carrier is released from the positive electrode, while an excessive amount of charge carrier is transferred to the negative electrode. As a result, the positive and negative electrodes become thermally unstable.When the positive electrode and the negative electrode become thermally unstable, the organic solvent of the electrolyte eventually decomposes, leading to the occurrence of an exothermic reaction that affects battery stability.
[0003] In response to this problem, a nonaqueous electrolyte secondary battery has been disclosed, which is provided with a current cutoff mechanism in the battery case that interrupts charging when, for example, the gas pressure in the battery case reaches a predetermined pressure or more. A gas generator is added that generates gas in the electrolyte when the battery reaches a predetermined overcharged state. For example, cyclohexylbenzene (CHB) or biphenyl (BP) are used as gas generators (see, for example, JP 2013-157139 A). CHB and BP generate hydrogen gas as a result of being activated by a polymerization reaction during overcharging. As a result, the pressure in the battery case rises, the current cutoff mechanism is activated, and the overcharge current is interrupted.
[0004] Furthermore, the documents US 6 156 459 A and DE 696 14 809 T2 disclose secondary batteries with non-aqueous electrolyte solutions from the prior art. List of cited documentsPatent literature Patent Literature 1: JP 2013-157139 A Patent Literature 2: US 6,156,459 A Patent literature 3: DE 696 14 809 T2 SUMMARY OF THE INVENTION
[0005] However, to enable the power cutoff mechanism to function efficiently, it is effective to increase the amount of the above-mentioned added gas generator. However, since the above-mentioned gas generator acts as a resistance component of the battery, increasing the amount of added gas generator may cause a decrease in battery performance. On the other hand, reducing the amount of added gas generator to maintain a high level of battery performance reduces the generation of gas during overcharging, potentially causing a delay in the activation of the power cutoff mechanism. With this type of conventional design, it was difficult to achieve both ensuring an adequate amount of generated gas and maintaining battery performance. The present invention solves the above-mentioned problems.
[0006] The nonaqueous electrolyte secondary battery provided by the present invention comprises: an electrode assembly provided with a positive electrode in which a positive electrode active material layer is held on a positive electrode current collector, a negative electrode in which a negative electrode active material layer is held on a negative electrode current collector, and a separator interposed between the positive electrode and the negative electrode; a battery case accommodating the electrode assembly together with a nonaqueous electrolyte; an external terminal provided in the battery case and connected to the electrode assembly; and a current cutoff mechanism that interrupts the electrical connection between the electrode assembly and the external terminal when the internal pressure of the battery case reaches a predetermined pressure or more.The above-mentioned positive electrode active material layer comprises at least one positive electrode active material and one conductive material. A compound comprising a saturated cyclic hydrocarbon group is retained (charged) in at least a portion of the above-mentioned conductive material, and the surface of the conductive material is chemically modified by the compound comprising a saturated hydrocarbon group. The content of the above-mentioned compound is 0.5% by mass or more based on a value of 100% by mass for the total solid content of the above-mentioned positive electrode active material layer. In a preferred mode thereof, the above-mentioned compound is composed such that protons are allowed to detach from the above-mentioned saturated cyclic hydrocarbon group when the voltage reaches a predetermined voltage or more.With this construction, a secondary battery can be provided that allows the power cut-off mechanism to function adequately during overcharging while maintaining favorable battery performance.
[0007] The content of the above-mentioned compound is approximately 0.5% by mass or more (and preferably 1% by mass or more) based on a value of 100% by mass for the total solid content of the above-mentioned positive electrode active material layer. If the content of the above-mentioned compound is excessively low, the amount of gas generated during overcharging will be insufficient, which may cause a delay in the function of the current cut-off mechanism. On the other hand, if the content of the above-mentioned material is excessively high, the function of a conductive material 58 through the compound will be impaired, thereby causing a possible decrease in battery performance (e.g., in terms of battery capacity). From the standpoint of enabling the function of the conductive material to be adequately achieved, the content of the above-mentioned compound is approximately 4% by mass or less (and preferably 2% by mass or less).
[0008] In a preferred mode of the non-aqueous electrolyte secondary battery disclosed herein, the aforementioned saturated cyclic hydrocarbon group is a cyclohexyl group. Since a cyclohexyl group promotes the release of protons (H + ) when the voltage reaches a predetermined voltage or more, it can be preferably used as a compound that meets the object of the present invention. An example of a compound containing a cyclohexyl group here is cyclohexylbenzene (CHB).
[0009] In a preferred mode of the non-aqueous electrolyte secondary battery disclosed herein, the above-mentioned non-aqueous electrolyte does not contain a gas generator that generates gas when the voltage reaches a predetermined voltage or higher. When a gas generator is contained in the electrolyte, the gas generator inhibits the phoretic diffusion of the charge carrier (lithium ions in the case of a lithium-ion secondary battery) and the anions present in the electrolyte, potentially causing a decrease in battery performance. However, with the structure of the present invention, an appropriate amount of gas can be ensured during overcharging even when no gas generator is contained in the electrolyte, since the above-mentioned compound functioning as a gas generator is adhered to a conductive material.Thus, the power cut-off mechanism can be enabled to function properly during overcharging without causing a decrease in battery performance. SHORT DESCRIPTION OF THE CHARACTERS Fig. 1 is a drawing illustrating an example of the structure of a lithium ion secondary battery according to an embodiment; Fig. 2 is a drawing illustrating a wound electrode assembly according to an embodiment; Fig. 3 is a cross-sectional view showing a section taken along the line III-III in Fig. 2 represents the cross-section taken; Fig. 4 is a schematic diagram illustrating a portion of a cross section obtained by dicing a wound electrode assembly in the radial direction; Fig. 5 is a drawing showing an example of a conductive material that holds CHB; and Fig.Figure 6 is a drawing showing an example of a conductive material that holds CHB. DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following provides an explanation of preferred embodiments of the present invention. In addition, matters necessary for carrying out the present invention, which are not specifically mentioned in the present description, can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents described in the present description and common general technical knowledge in the relevant field. In addition, in the present description, the term "secondary battery" refers to any electrically chargeable device that can be repeatedly charged and discharged, and it includes both so-called storage batteries such as lithium-ion secondary batteries and electrical storage elements such as electric double-layer capacitors.Furthermore, "lithium-ion secondary battery" refers to a secondary battery that uses lithium ions as the electrolyte ions and is charged and discharged by the migration of lithium ions between positive and negative electrodes. Furthermore, "electrode active material" refers to a material capable of reversibly absorbing and releasing chemical species (lithium ions in the case of a lithium-ion secondary battery).
[0011] The following provides an explanation of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention based on the figures. In addition, the same reference numerals are appropriately used to denote those elements and locations that exhibit the same function. Furthermore, the figures are intended as schematic illustrations and do not necessarily reflect actual objects. The figures are also intended as examples and do not limit the present invention unless expressly stated otherwise. Although the following provides an explanation of the embodiments of the present invention by using the case of applying the present invention to a lithium ion battery as an example, this is not intended to limit the scope of the present invention.
[0012] Fig.1 shows a lithium-ion secondary battery 100 according to an embodiment of the present invention. As shown in Fig. 1, this lithium-ion secondary battery 100 is provided with a wound electrode assembly 20 and a battery case 30. Fig. 2 is a drawing illustrating the wound electrode assembly 20. Fig. 3 is a cross-sectional view taken along the line III-III in Fig. 2. In the lithium-ion secondary battery 100 according to an embodiment of the present invention, as shown in Fig. 1 and Fig. 2, the flat-shaped wound electrode assembly 20 is housed in the flat rectangular battery case 30 (namely, an outer case) together with a liquid electrolyte (electrolytic solution) not shown.
[0013] The battery case 30 is formed by a box-shaped (namely, the shape of a rectangular parallelepiped with a bottom) case body 32 having an opening in one end thereof (corresponding to the upper end when the battery is in the normal use state) and a sealing plate (cover) 34 attached to the opening, which is formed from a rectangular plate member that covers the opening. An example of the material of the battery case 30 is aluminum. As shown in Fig. As shown in Figure 1, a positive electrode terminal 42 and a negative electrode terminal 44 for establishing external connections are formed in the sealing plate 34. A thin-walled safety valve 36 is formed between the two terminals 42 and 44 of the sealing plate 34, which is configured to release the pressure in the battery case 30 if it has risen to a predetermined level or more.
[0014] The wound electrode assembly 20 is provided with a long sheet-shaped positive electrode (positive electrode sheet 50), a long sheet-shaped negative electrode (negative electrode sheet 60) similar to the positive electrode sheet 50, and a total of two long sheet-shaped separators (separators 70 and 72).
[0015] The positive electrode sheet 50 is provided with a belt-shaped positive electrode current collector 52 and a positive electrode active material layer 54. For example, a belt-shaped aluminum foil with a thickness of 15 μm is used as the positive electrode current collector 52. An uncoated region 52a is provided along one edge in the width direction of the positive electrode current collector 52. In the example shown in the figure, the positive electrode active material layer 54 is adhered to both sides of the positive electrode current collector 52 except for the uncoated region 52a provided on the positive electrode current collector 52. The positive electrode active material layer 54 includes a positive electrode active material, a conductive material, and a binder.
[0016] A substance used as the positive electrode active material of a lithium-ion secondary battery can be used for the positive electrode active material. Examples of positive electrode active materials include lithium transition metal oxides such as lithium nickel cobalt manganese oxide (LiNiCoMnO2). For example, a conductive material can be mixed into the positive electrode active material. The conductive material is described below.
[0017] Furthermore, a binder such as polyvinylidene fluoride (PVdF), styrene-butadiene rubber (SBR), or carboxymethyl cellulose (CMC) may be added in addition to the positive electrode active material and the conductive material. A composition for forming the positive electrode active material layer (paste) can be prepared by dispersing it in a suitable dispersion medium and kneading it. The positive electrode active material layer 54 is formed by coating this composition for forming the positive electrode active material layer on the positive electrode current collector 52, followed by drying and pressing it to a predetermined thickness.
[0018] As in Fig.As shown in Figure 2, the negative electrode sheet 60 is provided with a belt-shaped negative electrode current collector 62 and a negative electrode active material layer 64. A belt-shaped copper foil with a thickness of approximately 10 μm is used as the negative electrode current collector 62. An uncoated region 62a is provided along one edge in the width direction of the negative electrode current collector 62. The negative electrode active material layer 64 is held on both sides of the negative electrode current collector 62, except for the uncoated region 62a provided on the negative electrode current collector 62. The negative electrode active material layer 64 contains, for example, a negative electrode active material, a thickener, and a binder.
[0019] One or two or more substances conventionally used in lithium-ion secondary batteries can be used as the negative electrode active material without any particular restrictions. Preferred examples thereof include carbon-based materials such as graphite carbon. Similar to the positive electrode, a negative electrode mixture (paste) can be prepared by dispersing the negative electrode active material in a suitable dispersion medium together with a binder such as PVDF, SBR, PTFE, or CMC and kneading. The negative electrode active material layer 64 is coated on the negative electrode current collector 62, followed by drying and pressing to a predetermined thickness.
[0020] The separators 70 and 72 are components that separate the positive electrode sheet 50 and the negative electrode sheet 60. In this example, the separators 70 and 72 are formed from a belt-like base material of a predetermined width having a plurality of small holes. A sheet material with a single-layer structure formed from a porous polyolefin-based resin (such as a single-layer polyethylene structure) or a sheet material with a laminated structure (such as a three-layer structure consisting of polypropylene, polyethylene, and polypropylene) can be used as the base material, for example. As shown in Fig. 2 and Fig. 3, a width b1 of the negative electrode active material layer 64 is wider than a width a1 of the positive electrode active material layer 54. In addition, the widths c1 and c2 of the separators 70 and 72 are wider than the width b1 of the negative electrode active material layer 64 (c1, c2>b1>a1).
[0021] The wound electrode assembly 20 is obtained by superimposing the positive electrode sheet 50 and the negative electrode sheet 60 with the separators 70 and 72 interposed therebetween, so that the positive electrode active material layer 54 and the negative electrode active material layer 64 are in mutual opposition. Furthermore, the negative electrode current collector 62 and the positive electrode current collector 52 are superimposed so that their both-side uncoated regions 52a and 62a protrude to the opposite side in the width direction of the wound electrode assembly 20. The superimposed sheet materials (such as the positive electrode sheet 50) are wound around a winding line WL oriented in the width direction.
[0022] The wound electrode assembly 20 is fixed to the electrode terminals 42 and 44, which are fixed to the battery case 30 (in this example, to the cover 34). The wound electrode assembly 20 is housed in the battery case 30 in a state where it is pressed and bent into a flat shape in a direction perpendicular to the winding line. Furthermore, the wound electrode assembly is configured such that the uncoated portion 52a of the positive electrode sheet 40 and the uncoated portion 62a of the negative electrode sheet 60 protrude on mutually opposite sides in the width direction of the separators 70 and 72. One of the electrode terminals 42 is fixed to the uncoated portion 52a of the positive electrode current collector 52, while the other electrode terminal 44 is fixed to the uncoated portion 62a of the negative electrode current collector 62.The wound electrode assembly 20 is housed in a shallow space within the housing body 32. The housing body 32 is closed with the cover 34 after the wound electrode assembly 20 has been housed therein.
[0023] A non-aqueous electrolyte similar to a non-aqueous electrolyte conventionally used in lithium-ion secondary batteries can be used as the electrolyte (non-aqueous electrolyte) without any particular restrictions. The non-aqueous electrolyte typically has a composition obtained by dissolving a conductive salt in a suitable non-aqueous solvent. Examples of the above-mentioned non-aqueous solvent that can be used include one or more non-aqueous solvents selected from the group consisting of, for example, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, and 1,3-dioxolane. In addition, examples of the above-mentioned carrier salt that can be used include lithium salts such as LiPF6, LiBF4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2 or LiC(CF3SO2)3.An example of this is a non-aqueous electrolyte obtained by dissolving LiPF6 at a concentration of approximately 1 mol / L in a mixed solvent of ethylene carbonate and diethyl carbonate (in a mass ratio of, for example, 1:1). In this embodiment, the non-aqueous electrolyte does not contain a gas generator (such as cyclohexylbenzene (CHB) or biphenyl (BP)) that generates gas when the voltage reaches a predetermined voltage or higher.
[0024] In addition, this lithium-ion secondary battery is provided with a current cutoff mechanism 90. The current cutoff mechanism 90 is a mechanism that interrupts the current path if the pressure in the battery case has become abnormally high. In this embodiment, the current cutoff mechanism is formed on the inside of the positive electrode terminal 42 so that it interrupts the conductive path of the battery current in the positive electrode, as shown in Fig. 1 shown.
[0025] The following provides a detailed explanation of this lithium ion secondary battery 100. Fig. 4 schematically illustrates a cross section obtained by dividing the positive electrode sheet 50 and the separator 70 superimposed in the wound electrode assembly 20 in the direction of the winding line (as well as in the direction of the width of the positive electrode sheet 50).
[0026] As in Fig.As shown in Figure 2, the positive electrode sheet 50 is provided with the positive electrode current collector 52 and the positive electrode active material layer 54 adhered to the positive electrode current collector 52. The positive electrode active material layer 54 includes a positive electrode active material 56, the conductive material 58, and a binder (not shown). As described above, the conductive material 58 is formed from a powdered carbon material (such as AB). A compound comprising a saturated cyclic hydrocarbon group is adhered (chemically immobilized) to at least a portion of the conductive material 58. In other words, the surface of the conductive material 58 is chemically modified by the compound comprising a saturated hydrocarbon group.
[0027] Within the range over which the effects of the present invention can be exhibited, there are no particular restrictions on the compound containing the saturated cyclic hydrocarbon group introduced into the surface of the conductive material 58 and other molecular structures thereof, as long as it is a compound having at least one saturated cyclic hydrocarbon group and which may have any functional groups, bonding sites, halogen atoms or metal atoms, and the like. Furthermore, the compound is preferably structured to allow a proton to detach from the saturated cyclic hydrocarbon group when it is oxidized when the voltage reaches a predetermined voltage or more. Examples of such saturated cyclic hydrocarbon groups include:Cyclic hydrocarbon groups include cycloalkyl groups having, for example, a monocyclic, bicyclic, tricyclic, or tetracyclic structure consisting of 5 to 10 (preferably 6 to 8) carbon atoms. Examples of monocycloalkyl groups include, for example, a cyclopentyl group, a cyclohexyl group, a cycloheptanyl group, a cyclooctanyl group, a cyclononanyl group, and a cyclodecanyl group. Furthermore, compounds in which one or two or more of these cyclic hydrocarbon groups are directly or indirectly bonded to an aromatic ring (including a heteroaromatic ring) are preferred.The compound may also be a compound in which hydrogen atoms in the aromatic ring (and typically a benzene ring) bonded to atoms forming the aromatic ring (such as carbon atoms) are each and independently exchanged with, for example, an aliphatic alkyl group (linear or branched having 1 to 10 carbon atoms), an alicyclic alkyl group (saturated or unsaturated having 1 to 10 carbon atoms), an oxygen atom (which may also be a hydroxyl group (OH)) or a halogen atom (such as F, Cl or Br).
[0028] A specific example of a more preferred compound having a saturated cyclic hydrocarbon group in the technology disclosed herein is a compound in which the above-mentioned cycloalkyl group is directly bonded to a benzene ring (cycloalkylbenzene). This cycloalkylbenzene has a monocyclic cycloalkyl group with 5 to 10 (preferably 6 to 8) carbon atoms. Particularly preferred examples include cyclohexolbenzene (CHB), cycloheptanylbenzene, and cyclooctanylbenzene. Of these, CHB is preferably used. Fig. 5 schematically shows the conductive material 58, as CHB holds (is loaded with). In the Fig. In the example shown in Figure 5, the surface of the conductive material 58 is chemically modified by CHB.
[0029] In the lithium-ion secondary battery 100 employing this construction, a compound containing a saturated cyclic hydrocarbon group (such as CHB) is retained (charged) on the conductive material 58 as described above. According to this construction, since the compound containing the saturated cyclic hydrocarbon group is normally retained on the conductive material (namely, during the time the battery is used within the normal charge and discharge range), problems that may occur with the compound dispersed in the electrolyte (such as a decrease in power output characteristics due to the compound inhibiting the theoretical diffusion of lithium ions and anions in the electrolyte) can be avoided.In addition, the pressure in the battery case rises rapidly due to the generation of gas from the above-mentioned compound when the battery is overcharged. As a result, the power cutoff mechanism 19 can be triggered at the right time. According to the present design, the lithium-ion secondary battery 100 can be provided that exhibits high performance (e.g., in terms of low resistance) and superior stability.
[0030] Furthermore, according to the present construction, when the voltage reaches a predetermined voltage or more (overcharged state), even if gas can be generated derived from the above-mentioned compound comprising a saturated cyclic hydrocarbon group, this effect is considered to be related to the release of a proton (H +) is realized by the saturated cyclic hydrocarbon group included in the compound. As an example, when the above-mentioned compound is cyclohexylbenzene (CHB), as in Fig. 6, even if CHB is normally held on the conductive material 58, when the voltage reaches a predetermined voltage or more (overcharged state) electrons are extracted from the CHB by the conductive material 58 and thus H + from the CHB, resulting in the formation of a double bond. The H +, which are released from the CHB, migrate to the negative electrode, where they are reduced, and this is believed to result in the generation of hydrogen gas at the negative electrode. However, the present invention can be easily carried out based on the information disclosed herein (as well as the structure of the compound comprising a saturated cyclic hydrocarbon group or the conductive material). Thus, the mechanism of action of the compound of the present invention comprising a cyclic hydrocarbon group, as it relates to the generation of gas during overcharging, does not need to be understood in order to carry out the present invention. The description concerning the above-mentioned mechanism of action is merely intended to provide an example thereof and is not intended to limit the present invention to the mechanism of action explained herein.
[0031] Although this is already clear from the above-mentioned mechanism of action, the modified conductive material 58 disclosed herein makes it possible to ensure an appropriate amount of gas during overcharging, even when no gas generator such as CHB or PB is contained in the electrolyte. Consequently, during the time the battery is used in the normal charging and discharging range, adverse effects attributable to the inclusion of a gas generator such as CHB or PB in the electrolyte (such as a reduction in power output characteristics due to inhibition of the phoretic diffusion of lithium ions or anions in the electrolyte) are avoided, while enabling proper operation of the current cutoff mechanism 90 during overcharging.The content of the above-mentioned compound having a saturated cyclic hydrocarbon group used in the positive electrode active material layer of the lithium-ion secondary battery disclosed herein is suitably about 0.5% by mass or more, preferably 0.8% by mass or more, and particularly preferably 1% by mass or more, based on a value of 100% by mass for the total solid content of the positive electrode active material layer. If the content of the above-mentioned compound is excessively low, the amount of gas generated during overcharging will be insufficient, resulting in a delay in the operation of the current cutoff mechanism 90 (Fig. Fig.1). On the other hand, if the content of the above-mentioned compound is excessively high, the function of the conductive material will be hindered by the compound, potentially causing a decrease in battery performance (e.g., in terms of battery capacity). From the viewpoint of allowing the function of the conductive material to adequately exhibit itself, the content of the above-mentioned compound is suitably about 8% by mass or less, preferably 4% by mass or less, and particularly preferably 2% by mass or less.
[0032] Various types of materials that are conventionally known to be used as conductive materials of lithium-ion secondary batteries and that can be modified by the above-mentioned compound containing a saturated cyclic hydrocarbon group can be used as the conductive material (and typically in particulate form) used in the lithium-ion secondary battery disclosed herein without any particular limitations. Examples of conductive materials that can be used include carbon black, such as acetylene black (AB), Ketjen Black, furnace black, or crack black, and other powdered carbon materials (such as graphite). AB is preferably used. Although there are no particular limitations, the average particle diameter of the conductive material is approximately 100 nm to 1000 nm.Although there are also no particular restrictions on the proportion of the conductive material present throughout the positive electrode active material layer (apart from the mass of the above-mentioned compound adhered to the conductive material), it is usually about 0.5% by mass to 15% by mass (and preferably 1% by mass to 10% by mass, and particularly preferably 2% by mass to 5% by mass).
[0033] Although there are no particular restrictions on the method (chemical modification treatment) used to adhere the above-mentioned compound to the surface of the above-mentioned conductive material, a method consisting, for example, of mixing an unmodified conductive material with a raw material of the above-mentioned compound, followed by heating and stirring, may be preferably used. For example, in the case of obtaining a conductive material by modifying its surface with CHB, the conductive material is placed in a reaction vessel equipped with a Liebig condenser and a stirrer, and the oxygen inside the oxidation vessel is removed and replaced with argon, followed by the addition of O-dichloromethane, tetrahydrofuran (THF), and p-cyclohexylaniline, and stirring at room temperature.After allowing it to cool by standing, filtering, and washing the filtrate with acetone, the filtrate is dried to obtain a modified conductive material whose surface is modified with the above-mentioned CHB. In this manufacturing process, the chemical modification of a conductive material using CHB can be carried out simply and efficiently, and the conductive material chemically modified by CHB can be formed with advantageous productivity. Furthermore, the amount of the above-mentioned compound (such as CHB) retained on the conductive material is determined by thermal analysis.The above-mentioned amount can be determined, for example, by the weight change when an unmodified conductive material and a modified conductive material are scanned from 100 °C to 500 °C in the presence of flowing nitrogen using a thermogravimetric differential thermal analysis (TG-DTA). In other words, the amount of weight increase of the modified conductive material can be considered the amount of the above-mentioned compound. Experimental examples
[0034] In the experimental examples, evaluation cells (lithium-ion secondary batteries) were fabricated using a modified conductive material chemically modified with CHB, followed by conducting an overcharge test on the batteries and evaluating their discharge characteristics. The following provides a detailed description of the method used.
[0035] The modified conductive material of the evaluation cell was prepared as described below. First, a conductive material in the form of acetylene black (DENKI KAGAKU KOGYO KABUSHIKI KAISHA.) was placed in a reaction vessel equipped with a Liebig condenser and a stirrer. After removing oxygen and replacing the atmosphere in the reaction vessel with argon, O-dichloromethane, tetrahydrofuran (THF, Aldrich INC.), and p-cyclohexylaniline (Wako Pure Chemical Industries, Ltd.) were added and stirred at room temperature. Isoamyl nitride was added to the reaction product with a syringe and heated. After allowing it to cool, the reaction product was filtered, and the filtrate was washed with acetone, followed by drying to obtain a modified conductive material with CHB attached thereto.
[0036] The positive electrode of the evaluation cells was prepared as described below. First, a positive electrode active material in the form of LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 powder, the above-mentioned modified conductive material, and a binder in the form of PVDF in NMP were mixed in a mass ratio of 93:4:3 to prepare a composition for a positive electrode active material layer. This composition for a positive electrode active material layer was coated in tape form on both sides of a long sheet-shaped aluminum foil (positive electrode current collector) and dried to prepare a positive electrode sheet with a positive electrode active material layer provided on both sides of a positive electrode current collector.
[0037] The negative electrode of the evaluation cells was prepared as described below. First, a negative electrode active material in the form of amorphous coated graphite, a binder in the form of SBR, and a thickener in the form of CMC were mixed in water at a mass ratio of 98:1:1 to prepare a negative electrode active material layer composition. This negative electrode active material layer composition was coated on both sides of a long sheet-shaped copper foil (negative electrode current collector) to prepare a negative electrode sheet having a negative electrode active material layer provided on both sides of a negative electrode current collector.
[0038] A porous polyethylene (PE) sheet was used for the separators of the evaluation cells. A non-aqueous electrolyte obtained by dissolving a conductive salt in the form of LiPF6 at a concentration of approximately 1 mol / liter in a mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 3:3:4 was used as the non-aqueous electrolyte for the evaluation cells.
[0039] A wound electrode assembly was fabricated by winding the positive electrode sheet and the negative electrode sheet with two separator sheets sandwiched between them. The resulting wound electrode assembly was then housed in a cylindrical battery case along with the nonaqueous electrolyte, followed by sealing the opening of the battery case to achieve leakage closure. The evaluation cells (lithium-ion secondary batteries) were assembled in this way. The evaluation cells were equipped with a current cutoff mechanism that interrupts the current flowing to the electrode assembly when the pressure in the battery case reaches a predetermined pressure or higher. Samples 1 to 11
[0040] In Samples 1 to 10, evaluation batteries were fabricated while varying the CHB content based on a value of 100% by mass for the total solid content of the positive electrode active material layer. Specifically, in Samples 1 to 10, the CHB content throughout the entire positive electrode active material layer was varied in the range of 1% by mass to 8% by mass. The other conditions were the same. In addition, in Sample 11, a conventional conductive material that did not retain CHB was used instead of the aforementioned conductive material that retained CHB. Furthermore, CHB was added to the nonaqueous electrolyte at 4% by mass. The other conditions were the same as those of Samples 1 to 10. Measuring battery capacity
[0041] Each of the resulting evaluation cells of the above-mentioned Samples 1 to 11 was charged to a battery voltage of 4.1 V at a constant current of 1 C in an atmosphere of 25 °C, followed by charging at a constant voltage of 4.1 V to a charging current of 1 / 10 C. Subsequently, the samples were charged to a voltage of 3.0 V at a constant current of 1 C, and the discharge capacity at this time of constant current discharge was defined as the battery capacity. The results are shown in Table 1. The values here are presented as relative values based on a value of 100 for the battery capacity of the Sample 11 battery. Discharge property test
[0042] Each of the resulting evaluation cells of the above-mentioned Samples 1 to 11 was charged to a battery voltage of 3.7 V at a constant current of 1 C in an atmosphere at 25 °C, followed by charging at a constant voltage of 3.7 V to a charging current of 1 / 10 C. The cells were then allowed to discharge for 10 seconds at a constant current of 10 C. The discharge resistance was then calculated as (voltage immediately before discharge - voltage after discharge for 10 seconds) / discharge current. The results are presented in the corresponding columns of Table 1. The values here are presented as relative values based on a value of 100 for the discharge resistance of the battery of Sample 11. Overload test
[0043] Each of the resulting evaluation cells of the above-mentioned problems 1 to 11 was charged with a constant current of 1 C and in an atmosphere at 25 °C to a battery voltage of 4.1 V, followed by charging with a constant voltage of 4.1 V to a charging current of 1 / 10 C (state of charge: 100%). Subsequently, the batteries were charged with a constant current of 1 C to an overcharged state at a state of charge of 160%, followed by designating the batteries in which the current cut-off mechanism functioned with an "O" and those in which the current cut-off mechanism did not function with an "X." The results are shown in the corresponding columns of Table 1. [Table 1] sample CHB content (wt%) Discharge resistance Battery capacity Overload test rating Positive electrode active material layer electrolyte 1 0,1 - 81 100 × 2 0,2 - 79 99 × 3 0,3 - 80 101 × 4 0,4 - 81 100 × 5 0,5 - 82 101 O 6 0,6 - 81 100 O 7 1 - 80 99 O 8 2 - 79 97 O 9 4 - 81 96 O 10 8 - 82 93 O 11 - 4 100 100 O
[0044] As shown in Table 1, in the battery case corresponding to Sample 11, CHB was added to the electrolyte without being bound to the conductive material. In this Sample 11, the discharge resistance tended to increase compared to Samples 1 to 11, even though the current cutoff mechanism functioned in the overcharge test. In contrast, in the batteries corresponding to Samples 5 to 10, the conductive materials held the CHB in place, and the CHB content throughout the entire positive electrode active material layer was 0.5% by mass or more. In these Samples 5 to 10, the current cutoff mechanism functioned adequately in the overcharge test, and a reasonable amount of gas was generated. Furthermore, compared to Sample 11, in which CHB was added to the electrolyte without being held by the conductive material, the discharge resistance was lower and the power output characteristics were superior.Based on these results, it was confirmed that a battery with high performance (low resistance) and superior stability was obtained by using a conductive material with CHB adhered to it and by adjusting the content throughout the positive electrode active material layer to 0.5% by mass or more. Furthermore, in comparison with Samples 5 to 10, the battery capacity tended to decrease as the CHB content increased throughout the positive electrode active material layer. In the case of the batteries used in this experiment, an extremely high battery capacity of 96% or more was achieved compared with Sample 11 by adjusting the CHB content throughout the positive electrode active material layer to 4% by mass or less.Based on this result, the content of CHB throughout the entire positive electrode active material layer is preferably about 4% by mass or less, and more preferably about 2% by mass or less.
[0045] Although the above has provided an explanation of a lithium ion secondary battery according to one embodiment of the present invention, the secondary battery according to the present invention is not limited to the above-mentioned embodiment.
Claims
[1] A non-aqueous electrolyte secondary battery (100) comprising: an electrode assembly (20) provided with a positive electrode (50) in which a positive electrode active material layer (54) is held on a positive electrode current collector (52), a negative electrode (60) in which a negative electrode active material layer (64) is held on a negative electrode current collector (62), and a separator (70, 72) interposed between the positive electrode (50) and the negative electrode (60); a battery case (30) accommodating the electrode assembly (20) together with a non-aqueous electrolyte; an external terminal provided in the battery case (30) and connected to the electrode assembly (20); and, a power cut-off mechanism that interrupts the electrical connection between the electrode assembly (20) and the external terminal when the internal pressure of the battery case (30) reaches a predetermined pressure or more, wherein the positive electrode active material layer (54) comprises a positive electrode active material and a conductive material (58), a compound comprising a saturated cyclic hydrocarbon group is retained in at least a portion of the conductive material (58), wherein the surface of the conductive material (58) is chemically modified by the compound comprising a saturated hydrocarbon group, and the content of the compound is 0.5% by mass or more based on a value of 100% by mass for the total solid content of the positive electrode active material layer (54). [2] The non-aqueous electrolyte secondary battery (100) according to claim 1, wherein the content of the compound is 4% by mass or less based on a value of 100% by mass for the total solid content of the positive electrode active material layer (54). [3] The non-aqueous electrolyte secondary battery (100) according to claim 1 or 2, wherein the compound is constructed so that protons are allowed to detach from the saturated cyclic hydrocarbon group when the voltage reaches a predetermined voltage or more. [4] The non-aqueous electrolyte secondary battery (100) according to any one of claims 1 to 3, wherein the saturated cyclic hydrocarbon group is a cyclohexyl group. [5] The non-aqueous electrolyte secondary battery (100) according to any one of claims 1 to 4, wherein the compound is cyclohexylbenzene. [6] The non-aqueous electrolyte secondary battery (100) according to any one of claims 1 to 5, wherein the non-aqueous electrolyte does not contain a gas generator that generates gas when the voltage reaches a predetermined voltage or more.
Citation Information
Patent Citations
aromatic monomer degassing agents for overcharge protection in nonaqueous lithium batteries
DE69614809T2
Sealed battery and manufacturing method therefor
JP2013157139A
Nonaqueous-electrolytic solution secondary battery
US6156459A