Contact lens and silicone hydrogel contact lens
Silicone hydrogel contact lenses with a polyacrylic acid and/or sodium polyacrylate coating address the issue of low oxygen permeability in hydrogel lenses, enhancing hydrophilicity and wear comfort while enabling cost-effective mass production.
Patent Information
- Application Number
- JP2024015931
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-02-05
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional soft contact lenses made of hydrogel materials suffer from low oxygen permeability, leading to eye discomfort and redness due to oxygen deficiency, and existing surface treatments for silicone hydrogel lenses are complex and costly.
The development of silicone hydrogel contact lenses with a surface coating of polyacrylic acid and/or sodium polyacrylate, having a molecular weight exceeding 100 kDa, which enhances hydrophilicity and suitability for long-term wear while facilitating mass production.
The lenses achieve a contact angle of 60° or less, a water rupture time of 20 seconds or more, and a tear film breakage time of 8 to 10 hours, improving comfort and reducing production costs by simplifying the manufacturing process.
Smart Images

Figure 2024166068000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to contact lenses and silicone hydrogel contact lenses, and more particularly to surface-treated contact lenses and silicone hydrogel contact lenses. [Background technology]
[0002] Soft contact lens materials were introduced in the 1960s, and because the soft materials eliminated the discomfort that often occurred when wearing conventional hard contact lenses (RGP lenses), users who were not originally adapted to hard contact lenses were able to switch to using soft contact lenses. Therefore, soft contact lenses are the main choice for current contact lens wearers.
[0003] However, the conventional materials used in soft contact lenses (mainly HEMA, commonly known as hydrogel materials) have low oxygen permeability, generally with a Dk (oxygen permeability) of only 8-20. As a result, consumers (or users, contact lens wearers) often experience eye congestion and associated discomfort due to lack of oxygen at the end of the day of wearing contact lenses (after wearing them for more than 10 hours). Therefore, the main axis of development of contact lens materials evolved toward the search for high oxygen permeability materials. Around 2000, soft contact lens products containing silicone components began to appear on the market. These are contact lens products made from silicone hydrogel materials, commonly called silicone hydrogel contact lenses. Compared to conventional hydrogel materials, silicone hydrogel materials have a high oxygen permeability and are characterized by their ability to solve problems such as oxygen deficiency in the cornea.
[0004] The main technical hurdle in silicone hydrogel contact lenses is how to make the lens surface sufficiently hydrophilic to avoid discomfort caused by the hydrophobicity of the silicone component. The industry generally judges the hydrophilicity of the lens surface by the contact angle. The industry's first plasma technology for surface treatment of lenses was developed, which is related to patent documents US20030039748 and US5760100. However, this technology requires complicated processing, which increases the production cost of lenses. There is also a method of adding polyvinylpyrrolidone (PVP) as an internal wetting agent during compounding, which is related to patent documents US6367929, US6943203, US7052131, US7249848, US7473738, US7473738, and US7691916. This method avoids the complicated processing of plasma surface treatment, but has many limitations on the compounding of lenses. In addition to the above two techniques, researchers have developed a compounding technique that does not require plasma surface treatment and does not require the addition of separate PVP as an internal wetting agent, and is related to patent documents US7750079, US8129442, US8231218, US8476337, and EP195584. However, this compounding technique requires the combination of specific silicone-containing monomers, specific hydrophilic monomers, and specific diluents to achieve the desired lens properties, and also usually requires the combination of specific metal fitting materials to manufacture contact lenses. These constraints limit the optimization of the production cost of the product.
[0005] Therefore, there is a need to design a system that can easily mass produce high quality, cost-competitive contact lenses that meet consumer needs and are suitable for extended wear. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides contact lenses suitable for extended wear by consumers and facilitates mass production of contact lenses.
[0007] The present invention provides silicone hydrogel contact lenses suitable for extended wear by consumers and facilitates mass production of silicone hydrogel contact lenses. [Means for solving the problem]
[0008] To achieve the above advantages, one embodiment of the present invention provides a contact lens comprising at least one silicone-containing monomer, and the surface of the contact lens comprises polyacrylic acid and / or sodium polyacrylate, preferably having a molecular weight of more than 100 kDa, more preferably more than 200 kDa, and most preferably more than 450 kDa.
[0009] In order to achieve the above-mentioned advantages, another embodiment of the present invention provides a silicone hydrogel contact lens, comprising a first silicone-containing monomer, a second silicone-containing monomer, a first hydrophilic monomer, a second hydrophilic monomer, and a silicon-containing crosslinker, and the surface of the silicone hydrogel contact lens comprises polyacrylic acid and / or sodium polyacrylate. Specifically, the molecular weight of the polyacrylic acid and / or sodium polyacrylate is preferably greater than 100 kDa, more preferably greater than 200 kDa, and most preferably greater than 450 kDa.
[0010] The first silicone-containing monomer has the following structure:
[0011] [ka]
[0012] Of these, A has the following structure:
[0013] [ka]
[0014] or the following structure:
[0015] [ka]
[0016] R1 is H or CH3 or OSi(CH3)3, R2 is H or CH3 or OSi(CH3)3, and L1 is the following structures or combinations thereof:
[0017] [ka]
[0018] n1 is 1-5, m1 is 1-4, m2 is 0-1, m3 is 1-4, m4 is 0-1, m5 is 1-4, and m6 is 1-4.
[0019] The second silicone-containing monomer comprises a first structure or a second structure. The first structure:
[0020] [ka]
[0021] a is 0 to 20. R3 is H or CH3 or C2H5, R4 is H or CH3 or OSi(CH3)3, R5 is H or CH3 or OSi(CH3)3, and L2 is the following structure or a combination thereof:
[0022] [ka]
[0023] n6 is 1-5, n7 is 1-5, m7 is 1-4, m8 is 0-1, m9 is 1-4, m10 is 0-1, m11 is 1-4, m12 is 1-4, m13 is 0-1, m14 is 1-4, and m15 is 1-4.
[0024] The second structure:
[0025] [ka]
[0026] c is 0 to 20. 10 is H or CH3 or C2H5, and R 11 is H or CH3 or OSi(CH3)3, and R 12 is H or CH3 or OSi(CH3)3, L5 is the following structures or combinations thereof: O or NH; L6 is the following structures or combinations thereof:
[0027] [ka]
[0028] n20 is 1–5, m34 is 1–4, m35 is 0–1, m36 is 1–4, m37 is 0–1, m38 is 1–4, and m39 is 1–4.
[0029] The first hydrophilic monomer comprises an N-vinyl group, and the second hydrophilic monomer is different from the first hydrophilic monomer.
[0030] The first silicone-containing monomer comprises at least one of 3-[tris(trimethylsiloxy)silyl]propyl methacrylate, (3-methacryloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methylsilane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propyl carbamate, 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate.
[0031] The second silicone-containing monomer includes at least one of monomethacryloyloxypropyl-terminated polydimethylsiloxane, monomethacryloxypropyl-terminated carbamate polydimethylsiloxane, and mono-(3-methacryloxy-2-hydroxypropyloxy)propyl-terminated mono-butyl-terminated polydimethylsiloxane. The molecular weight of the second silicone-containing monomer is 350 to 2500, preferably 500 to 1500.
[0032] The silicone hydrogel contact lens further comprises a filler, and the combined content of the first silicone-containing monomer and the second silicone-containing monomer accounts for 15 to 60%, and preferably 25 to 45%, of the weight of the silicone hydrogel contact lens after the filler is removed.
[0033] The first hydrophilic monomer is N-vinylpyrrolidone or N-methyl-N-vinylacetamide.
[0034] The silicone hydrogel contact lens further contains a filler, and the content of the first hydrophilic monomer accounts for 30 to 65%, preferably 35 to 55%, of the weight of the silicone hydrogel contact lens after the filler is removed.
[0035] The second hydrophilic monomer comprises 2-hydroxyethyl methacrylate.
[0036] The silicon-containing crosslinker comprises the following structure:
[0037] [ka]
[0038] b is 0 to 20. R6 is H or CH3 or C2H5, R7 is H or CH3 or OSi(CH3)3, and L3 is the following structure or a combination thereof:
[0039] [ka]
[0040] n12 is 1 to 5, n13 is 1 to 5, m16 is 1 to 4, m17 is 0 to 1, m18 is 1 to 4, m19 is 0 to 1, m20 is 1 to 4, m21 is 1 to 4, m22 is 0 to 1, m23 is 1 to 4, and m24 is 1 to 4. R8 is the following structure or a combination thereof:
[0041] [ka]
[0042] R9 is H or CH3 or C2H5, and L4 is the following structures or combinations thereof:
[0043] [ka]
[0044] n18 is 1-5, n19 is 1-5, m25 is 1-4, m26 is 0-1, m27 is 1-4, m28 is 0-1, m29 is 1-4, m30 is 1-4, m31 is 0-1, m32 is 1-4, m33 is 1-4.
[0045] The silicon-containing crosslinker comprises the following structure:
[0046] [ka]
[0047] d is 0 to 20. 13 is H or CH3 or C2H5, and R 14 is H or CH3 or C2H5, L7 is the following structures or combinations thereof: O or NH; L8 is the following structures or combinations thereof:
[0048] [ka]
[0049] n25 is 1-5, m40 is 1-4, m41 is 0-1, m42 is 1-4, m43 is 0-1, m44 is 1-4, and m45 is 1-4. R 15 is the following structure or a combination thereof:
[0050] [ka]
[0051] R 16 is H or CH3 or C2H5, and L9 is the following structure or a combination thereof:
[0052] [ka]
[0053] n31 is 1-5, m46 is 1-4, m47 is 0-1, m48 is 1-4, m49 is 0-1, m50 is 1-4, and m51 is 1-4.
[0054] The silicon-containing crosslinking agent includes at least one of methacryloxypropyl-terminated polydimethylsiloxane, methacryloxypropyl-terminated carbamate polydimethylsiloxane, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification, 1,3-bis[4-(vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, and bis-3-methacryloxy-2-hydroxypropyloxypropyl polydimethylsiloxane. The molecular weight of the silicon-containing crosslinking agent is in the range of 500 to 3000.
[0055] The silicone hydrogel contact lens further comprises at least one non-silicon containing crosslinker, the at least one non-silicon containing crosslinker comprising at least one of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane trimethacrylate.
[0056] The contact lenses are silicone hydrogel contact lenses, with a contact angle of 60° or less, a water-breaking time (WBUT) of 20 seconds or more, and a tear film breakup time of more than 15 seconds after about 8 to 10 hours of wearing. Effect of the Invention
[0057] The contact lenses and silicone hydrogel contact lenses of the embodiments of the present invention contain at least one silicone-containing monomer, and the surfaces of the contact lenses and silicone hydrogel contact lenses contain polyacrylic acid and / or sodium polyacrylate having a molecular weight of more than 100 kDa, so that the contact lenses and silicone hydrogel contact lenses prepared have the advantages of excellent hydrophilicity and suitability for long-term wear by consumers.
[0058] In order to make the above and other objects, features and advantages of the present invention clearer and easier to understand, the following detailed description, particularly given by way of example and in conjunction with the accompanying drawings, will now be given. [Brief description of the drawings]
[0059] [Figure 1] FIG. 1 is a cross-sectional view of a contact lens according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a flow chart showing a method for manufacturing a contact lens according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0060] One embodiment of the present invention provides a contact lens 100, which is composed of a lens body 110 containing at least one silicone-containing monomer, and the surface of the contact lens 100 contains polyacrylic acid and / or sodium polyacrylate 120. FIG. 1 is a cross-sectional view of a contact lens according to one embodiment of the present invention. Referring to FIG. 1, specifically, polyacrylic acid and / or sodium polyacrylate 120 is a film covering the lens body 110, and this film is the surface of the contact lens 100. The surface of the contact lens 100 may include a convex surface, a concave surface, or a combination thereof, and since polyacrylic acid and sodium polyacrylate 120 are hydrophilic, the hydrophilicity of the contact lens 100 can be improved by using them as the surface of the contact lens 100. In addition, the surface of the contact lens 100 does not contain any polymer other than polyacrylic acid or sodium polyacrylate 120 that has an opposite charge to polyacrylic acid or sodium polyacrylate. That is, the contact lens 100 of this embodiment only has a film covering the lens body 110 formed by polyacrylic acid and / or sodium polyacrylate 120. The molecular weight of the polyacrylic acid and / or sodium polyacrylate 120 is preferably greater than 100 kDa, more preferably greater than 200 kDa, and most preferably greater than 450 kDa. Specifically, the contact lens 100 is a silicone hydrogel contact lens, and the lens body 110 of the contact lens 100 includes a first silicone-containing monomer, a second silicone-containing monomer, a first hydrophilic monomer, a second hydrophilic monomer, and a silicon-containing crosslinker.
[0061] The first silicone-containing monomer has the following structure:
[0062] [ka]
[0063] Of these, A has the following structure:
[0064] [ka]
[0065] or the following structure:
[0066] [ka]
[0067] R1 is H or CH3 or OSi(CH3)3, R2 is H or CH3 or OSi(CH3)3, and L1 is the following structures or combinations thereof:
[0068] [ka]
[0069] n1 is 1-5, m1 is 1-4, m2 is 0-1, m3 is 1-4, m4 is 0-1, m5 is 1-4, and m6 is 1-4.
[0070] The second silicone-containing monomer comprises the first structure or the second structure. First structure:
[0071] [ka]
[0072] a is 0 to 20. R3 is H or CH3 or C2H5, R4 is H or CH3 or OSi(CH3)3, R5 is H or CH3 or OSi(CH3)3, and L2 is the following structure or a combination thereof:
[0073] [ka]
[0074] n6 is 1-5, n7 is 1-5, m7 is 1-4, m8 is 0-1, m9 is 1-4, m10 is 0-1, m11 is 1-4, m12 is 1-4, m13 is 0-1, m14 is 1-4, and m15 is 1-4. Second structure:
[0075] [ka]
[0076] c is 0 to 20. 10 is H or CH3 or C2H5, and R 11 is H or CH3 or OSi(CH3)3, and R 12 is H or CH3 or OSi(CH3)3, L5 is the following structures or combinations thereof: O or NH; L6 is the following structures or combinations thereof:
[0077] [ka]
[0078] n20 is 1–5, m34 is 1–4, m35 is 0–1, m36 is 1–4, m37 is 0–1, m38 is 1–4, and m39 is 1–4.
[0079] The first hydrophilic monomer comprises an N-vinyl group. The second hydrophilic monomer is different from the first hydrophilic monomer. The second hydrophilic monomer comprises 2-hydroxyethyl methacrylate (HEMA), which is an effective hydrophilic monomer.
[0080] The contact lens has a contact angle of 60° or less, a water-break time (WBUT) of 20 seconds or more, and a tear film breakup time of more than about 15 seconds after about 8 to 10 hours of wearing.
[0081] In this specification, contact lenses may refer to contact lenses that have been fully hydrated or contact lenses that have been fully hydrated and sterilized. In this specification, depending on the context, lenses may be interchangeable with contact lenses, while lenses may refer to lens bodies or dry lenses that have not been hydrated. In addition, lens formulations (hereinafter abbreviated as formulations) in this specification refer to formulations that consist of monomers, crosslinkers, and initiators, and may also include fillers, if necessary. The term "monomer" is used to refer to lens formulations that can undergo polymerization by free radical polymerization during the curing process to further form polymers, and monomers generally have a free radical double bond that is acceptable in their chemical structure.
[0082] The term "silicone monomer" refers to a monomer having at least one silicon-oxygen bond (-Si-O-). Examples of the silicone-containing monomer in this embodiment include 3-[tris(trimethylsiloxy)silyl]propyl methacrylate (abbreviated as TRIS) and monomethacryloxypropyl terminated polydimethylsiloxane (abbreviated as MPDMS). The CAS No. of the commonly used monomethacryloxypropyl terminated polydimethylsiloxane is 146632-07-7. Other silicone-containing monomers that can be used in this embodiment include 2-(trimethylsilyloxy)ethyl methacrylate (abbreviated as MPDMS). methacrylate), (3-(3-Methacryloxy-2-hydroxypropoxy)propylbis(trimethylsiloxy)methylsilane (SiGMA), (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane), methacryloxymethylphenethyltris(trimethylsiloxy)methylsilane Examples of suitable silanes include, but are not limited to, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate, and 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate.The silicone-containing monomers can be purchased commercially from chemical manufacturers such as Sigma-Aldrich, Gelest, JNC, Shin-Etsu, Pharnocia, Bimax, etc. Another example of the silicone-containing monomer used in this embodiment is mono-(3-methacryloxy-2-hydroxypropyloxy)propyl terminated, mono-butyl terminated polydimethylsiloxane, which can be synthesized by referring to the method described in US Patent US20030162862A1. Another example of the silicone-containing monomer used in this embodiment is a urethane ester of monocarbinol terminated polydimethylsiloxane (CAS No: 207308-30-3, abbreviated as MOHPMDS) and 2-isocyanatoethyl methacrylate (abbreviated as IEM), and the synthesis reaction of the urethane ester can be performed using 1,8-Diazabicyclo[5.4.0]undec-7-ene (abbreviated as DBU) as a catalyst.
[0083] The first silicone-containing monomer can include the following structure:
[0084] [ka]
[0085] Of these, A has the following structure:
[0086] [ka]
[0087] or the following structure:
[0088] [ka]
[0089] R1 is H or CH3 or OSi(CH3)3, R2 is H or CH3 or OSi(CH3)3, and L1 is the following structures or combinations thereof:
[0090] [ka]
[0091] n1 is 1-5, m1 is 1-4, m2 is 0-1, m3 is 1-4, m4 is 0-1, m5 is 1-4, and m6 is 1-4.
[0092] In this embodiment, the first silicone-containing monomer comprises at least one of 3-[tris(trimethylsiloxy)silyl]propyl methacrylate, (3-methacryloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methylsilane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propyl carbamate, and 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate.
[0093] The second silicone-containing monomer includes at least one of monomethacryloxypropyl-terminated polydimethylsiloxane, monomethacryloxypropyl-terminated carbamate polydimethylsiloxane, and mono-(3-methacryloxy-2-hydroxypropyloxy)propyl-terminated mono-butyl-terminated polydimethylsiloxane. In addition, the molecular weight of the second silicone-containing monomer is 350 to 2500, and preferably 500 to 1500.
[0094] The second silicone-containing monomer comprises the first structure or the second structure. First structure:
[0095] [ka]
[0096] a is 0 to 20. R3 is H or CH3 or C2H5, R4 is H or CH3 or OSi(CH3)3, R5 is H or CH3 or OSi(CH3)3, and L2 is the following structure or a combination thereof:
[0097] [ka]
[0098] n6 is 1-5, n7 is 1-5, m7 is 1-4, m8 is 0-1, m9 is 1-4, m10 is 0-1, m11 is 1-4, m12 is 1-4, m13 is 0-1, m14 is 1-4, and m15 is 1-4. Second structure:
[0099] [ka]
[0100] c is 0 to 20. 10 is H or CH3 or C2H5, and R 11 is H or CH3 or OSi(CH3)3, and R 12 is H or CH3 or OSi(CH3)3, L5 is the following structures or combinations thereof: O or NH; L6 is the following structures or combinations thereof:
[0101] [ka]
[0102] n20 is 1–5, m34 is 1–4, m35 is 0–1, m36 is 1–4, m37 is 0–1, m38 is 1–4, and m39 is 1–4.
[0103] The first hydrophilic monomer contains an N-vinyl group, for example N-vinylpyrrolidone or N-methyl-N-vinylacetamide.
[0104] The total content of the first silicone-containing monomer and the second silicone-containing monomer accounts for 15 to 60%, and preferably 25 to 45%, of the weight of the contact lens after the filler has been removed.
[0105] The term "hydrophilic monomer" refers to a monomer that is relatively hydrophilic in chemical structure. Examples of hydrophilic monomers used in the present embodiment include N-vinyl pyrrolidone (NVP), N-methyl-N-vinylacetamide (MVA), N,N-dimethyl acrylamide (DMA), N,N-diethylacrylamide, N-(hydroxymethyl)acrylamide, N-hydroxyethyl acrylamide, 2-hydroxyethyl methacrylate (HEMA), ethylene glycol vinyl ether (EGVE), 1,4-butanediol vinyl ether (1,4-butanediol vinyl ether (BVE), Di(ethylene glycol) vinyl ether, Hydroxypropyl methacrylate and / or Hydroxyisopropyl methacrylate, Hydroxybutyl methacrylate (HOBMA), Poly(propylene ethylene glycol) methacrylate, Poly(ethpropylene glycol) acrylate, Glyceryl methacrylate, Glycidyl methacrylate, 2-Hydroxyethyl acrylate, Hydroxypropyl acrylate and / or Hydroxyisopropyl acrylate, 4-Hydroxybutyl acrylate, Glyceryl acrylate acrylate), N-[Tris(hydroxymethyl)methyl]acrylamide, Methacrylamide, 2-Hydroxypropyl methacrylamide, N-Isopropylacrylamide, N,N-DiethylacrylamideThe hydrophilic monomers include, but are not limited to, N-Diethylacrylamide, N-Ethylacrylamide, 2-Ethoxyethyl methacrylate (EOEMA), Polyethylene glycol dimethacrylate (PEGDMA), 2-Methacryloyloxyethyl phosphorylcholine, etc. In this embodiment, the preferred hydrophilic monomer is N-vinylpyrrolidone or N-methyl-N-vinylacetamide (MVA). More preferred is a combination of N-vinylpyrrolidone (NVP) and 2-hydroxyethyl methacrylate (HEMA), or a combination of N-methyl-N-vinylacetamide (MVA) and 2-hydroxyethyl methacrylate (HEMA). The hydrophilic monomers are generally commercially available from chemical manufacturers, such as Sigma-Aldrich, Tokyo Chemical Industry Co., Ltd. (TCI), and Alfa Aesar. In addition to the hydrophilic monomers, hydrophobic monomers can be selectively added to the formulation. This is usually done to adjust the mechanical properties of the lens, for example, methyl methacrylate (MMA) is added in some embodiments of the present invention.
[0106] In one embodiment of the present invention, the first hydrophilic monomer is N-vinylpyrrolidone or N-methyl-N-vinylacetamide (MVA), and the content of the first hydrophilic monomer accounts for 30-65% of the weight of the contact lens after the filler is removed.
[0107] In one embodiment of the present invention, the first hydrophilic monomer is N-vinylpyrrolidone or N-methyl-N-vinylacetamide (MVA), and the content of the first hydrophilic monomer accounts for 35-55% of the weight of the contact lens after the filler is removed.
[0108] In one embodiment of the present invention, the second hydrophilic monomer comprises at least one of 2-hydroxyethyl methacrylate (HEMA), ethylene glycol vinyl ether, and 1,4-butanediol vinyl ether. In particular, 2-hydroxyethyl methacrylate (HEMA) has the most excellent effect. At this point, there is no detailed theoretical framework, and the inventor does not want to limit the invention to a specific theoretical framework. However, the unexpected discovery of the present invention is that 2-hydroxyethyl methacrylate (HEMA) may have a hydroxyl group in its structure, and can form a silicon-containing polymer structure in combination with the first hydrophilic monomer containing an N-vinyl group, which can form a suitable hydrogen bond or van der Waals force with polyacrylic acid and / or sodium polyacrylate, so that the polyacrylic acid and / or sodium polyacrylate can be more stably adsorbed on the lens surface, and can also promote the formation of entanglement with the polymer structure on the lens surface after adsorption on the lens surface. Therefore, polyacrylic acid and / or sodium polyacrylate can be more stably adsorbed onto the lens surface, improving the quality of the contact lens and making it more suitable for wearing.
[0109] The term "UV blocker" refers to a component that is added to a lens and has the property of blocking UV wavelength light. Generally, the blockers used in contact lenses also belong to the category of monomers because they have a double bond of a free radical that is acceptable in the chemical structure. The UV blockers used in this embodiment include, but are not limited to, 2-[3-(2H-Benzotriazol-2-yl)-4-hydroxyphenyl]ethyl methacrylate (abbreviated as HMEPB) and 2-(4-Benzoyl-3-hydroxyphenoxy)ethyl acrylate. The UV blockers can generally be purchased commercially from chemical manufacturers such as Sigma-Aldrich, Tokyo Chemical Industry Co., Ltd. (TCI), and Alfa Aesar.
[0110] In this embodiment, the contact lens further comprises at least one non-silicon containing crosslinker.
[0111] The term "crosslinking agent" refers to a substance that can cause a crosslinking reaction when a monomer undergoes a polymerization reaction, can provide a polymer produced by a polymerization reaction with a required crosslinking density, and can generate and react two polymer chains to bond them into a network polymer. The crosslinking agent can be classified into non-silicon-containing crosslinking agents and silicon-containing crosslinking agents depending on whether it has a silicon-oxygen bond chemical structure (-Si-O-). The non-silicon crosslinking agents used in this example include ethylene glycol dimethacrylate (EGDMA), di(ethylene glycol) dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate (TEGDMA), ethylene glycol diacrylate, di(ethylene glycol) diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diacrylate), N,N'-Methylenebis(acrylamide), N,N'-Ethylenebis(acrylamide), N,N'-(1,2-dihydroxyethylene)bisacrylamide, trimethylolpropanetrimethacrylate (abbreviated as TEPTMA), N,N'-hexamethylenebis(methacrylamide)Examples of the vinyl ether include, but are not limited to, N'-Hexamethylenebis(methacrylamide), glycerol trimethacrylate, polyethylene glycol dimethacrylate, polyethylene glycol diacrylate, mono-2-(methacryloyloxy)ethyl maleate, diurethanedimethacrylate, 3-isopropenyl-α,α-dimethylbenzylisocyanate, diethylene glycol monovinyl ether (abbreviated as DEGVE), and tri(ethylene glycol) divinyl ether (abbreviated as TEGDVE). The non-silicon-containing crosslinkers are generally commercially available from chemical manufacturers such as Sigma-Aldrich, Tokyo Chemical Industry Co., Ltd. (TCI), and Alfa Aesar.
[0112] In this embodiment, the at least one non-silicon containing crosslinker comprises at least one of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane trimethacrylate.
[0113] "Silicon-containing crosslinking agent" refers to a chemical structure (-Si-O-) that belongs to the scope of crosslinking agents and has at least one silicon-oxygen bond. Examples of silicon-containing crosslinking agents used in this embodiment include, but are not limited to, the following examples. For example, there is methacryloxypropyl terminated polydimethylsiloxane (abbreviated as DMPDMS), and the CAS No. of commonly used methacryloxypropyl terminated polydimethylsiloxane is 58130-03-3. Another example is methacryloxypropyl terminated polydimethylsiloxane with polyethylene glycol modification, which has the following structure:
[0114] [ka]
[0115] Silicon-containing crosslinking agent is used in combination with other crosslinking agents to form suitable lens properties. In this embodiment, the silicon-containing crosslinking agent can be purchased commercially from chemical manufacturers such as Sigma-Aldrich, Gelest, JNC, Shin-Etsu, Pharnocia, Bimax, etc. The silicon-containing crosslinking agent used in this embodiment can be, for example, 1,3-bis[4-(vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, which can be obtained by synthesis with reference to the method in US Patent US5070215A. Another example of the silicon-containing crosslinking agent used in this embodiment is bis-3-methacryloxy-2-hydroxypropyloxypropyl polydimethylsiloxane, which can be synthesized by referring to the method described in U.S. Patent US20030162862A1, and can be obtained by replacing mono-(2,3-epoxy)propylether terminated polydimethylsiloxane with epoxypropoxypropyl terminated polydimethylsiloxane. Another example of the silicon-containing crosslinking agent used in this embodiment is a urethane ester of carbinol (hydroxyl) terminated polydimethylsiloxane (DOHPDMS; CAS No: 156327-07-0) and 2-isocyanatoethyl methacrylate (IEM), and the synthesis reaction of the urethane ester can be performed using 1,8-Diazabicyclo[5.4.0]undec-7-ene (DBU) as a catalyst.
[0116] In one embodiment of the present invention, the silicon-containing crosslinker comprises the following structure:
[0117] [ka]
[0118] b is 0 to 20. R6 is H or CH3 or C2H5, R7 is H or CH3 or OSi(CH3)3, and L3 is the following structure or a combination thereof:
[0119] [ka]
[0120] n12 is 1 to 5, n13 is 1 to 5, m16 is 1 to 4, m17 is 0 to 1, m18 is 1 to 4, m19 is 0 to 1, m20 is 1 to 4, m21 is 1 to 4, m22 is 0 to 1, m23 is 1 to 4, and m24 is 1 to 4. R8 is the following structure or a combination thereof:
[0121] [ka]
[0122] R9 is H or CH3 or C2H5, and L4 is the following structures or combinations thereof:
[0123] [ka]
[0124] n18 is 1-5, n19 is 1-5, m25 is 1-4, m26 is 0-1, m27 is 1-4, m28 is 0-1, m29 is 1-4, m30 is 1-4, m31 is 0-1, m32 is 1-4, m33 is 1-4.
[0125] In one embodiment of the present invention, the silicon-containing crosslinker comprises the following structure:
[0126] [ka]
[0127] d is 0 to 20. 13 is H or CH3 or C2H5, and R 14 is H or CH3 or C2H5, L7 is the following structures or combinations thereof: O or NH; L8 is the following structures or combinations thereof:
[0128] [ka]
[0129] n25 is 1-5, m40 is 1-4, m41 is 0-1, m42 is 1-4, m43 is 0-1, m44 is 1-4, and m45 is 1-4. R 15 is the following structure or a combination thereof:
[0130] [ka]
[0131] R 16 is H or CH3 or C2H5, and L9 is the following structure or a combination thereof:
[0132] [ka]
[0133] n31 is 1-5, m46 is 1-4, m47 is 0-1, m48 is 1-4, m49 is 0-1, m50 is 1-4, and m51 is 1-4.
[0134] In one embodiment of the present invention, the silicon-containing crosslinker comprises at least one of methacryloxypropyl-terminated polydimethylsiloxane, methacryloxypropyl-terminated carbamate polydimethylsiloxane, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification, 1,3-bis[4-(vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, and bis-3-methacryloxy-2-hydroxypropyloxypropylpolydimethylsiloxane.
[0135] In one embodiment of the present invention, it has been confirmed that the degree of haze of the lens is reduced by combining the compounded composition containing a silicon-containing crosslinking agent with a hydrating liquid containing polyacrylic acid and / or sodium polyacrylate.This may be due to the fact that in the lens body containing a silicon-containing crosslinking agent, the degree of polymerization between silicone-containing monomers (first silicone-containing monomer and second silicone-containing monomer) is high and the degree of polymerization between non-silicon-containing monomers is low, so that the entire structure of the lens formed is such that polyacrylic acid and / or sodium polyacrylate do not penetrate excessively into the internal structure of the lens, but remain only on the lens surface, thereby reducing the phenomenon of lens haze. Therefore, by combining the molecular weight of polyacrylic acid and / or sodium polyacrylate, the concentration of polyacrylic acid and / or sodium polyacrylate in an aqueous solution, a suitable silicon-containing crosslinker, and a suitable molecular weight of the silicon-containing crosslinker, the contact lens can effectively meet the following conditions: a contact angle of 60° or less, a water-breaking time (WBUT) of 20 seconds or more, a tear film breakup time of more than about 15 seconds after about 8 to 10 hours of wearing, and at the same time, an acceptable degree of fogging of the contact lens.
[0136] The molecular weight of the silicon crosslinking agent is preferably in the range of 500 to 5,000, more preferably in the range of 700 to 3,000, and even more preferably in the range of 900 to 2,000.
[0137] The content of the silicon crosslinking agent is 0.1 to 6.0% of the weight of the contact lens after removing the filler, and preferably 0.1 to 3.0%.
[0138] An "initiator" is used as a free radical required to generate free radical polymerization, and can generally be classified into thermal initiators and photoinitiators according to the various methods by which it can be initiated to generate free radicals. An initiator capable of generating free radicals by thermal initiation is a thermal initiator, and an initiator capable of generating free radicals by photoinitiation is a photoinitiator. Photoinitiators used in this embodiment include, but are not limited to, 2-hydroxy-2-methylpropiophenone (abbreviated as 1173) and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (abbreviated as 819). In other embodiments, for example, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and 2,2-dimethoxy-2-phenylacetophenone are used. The thermal initiators used in this example include azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), acid), 1,1'-Azobis(cyclohexanecarbonitrile), 2,2'-Azobis(2-methylpropionamidine), 2,2'-Azobis(2-methylpropionamidine) dihydrochloride, 2,2'-Azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2,2'-Azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, 2,2'-Azobis(1-imino-1-pyrrolidino-2-ethylpropane)dihydrochloride, 2,2'-Azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-methyl]propane}dihydrochloride Examples of initiators include, but are not limited to, 2,2'-Azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-Azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-Azobis(4-methoxy-2,4-dimethyl valeronitrile), and benzoyl peroxide. The initiators are generally commercially available from chemical manufacturers such as Sigma-Aldrich, Tokyo Chemical Industry Co., Ltd. (TCI), and Alfa Aesar.
[0139] A "diluent" refers to a component added to a lens formulation that does not have an acceptable free radical double bond to produce free radical polymerization. It is therefore a chemical that cannot polymerize with a monomer or crosslinker or initiator to form a further polymer. Some fillers may act as chain transfer agents and may extend to some free radical polymerization processes, but the effect of such chain transfer is generally much less than that of true chain transfer agents such as thiols, and therefore the function of the fillers as chain transfer agents is not considered in this embodiment. Fillers are usually used to aid in the compatibility of the components of a lens formulation, and solvent-type compounds may be an option for the filler.Examples of the filler used in this embodiment include alcohols such as ethanol, isopropyl alcohol (IPA), n-butanol, n-hexanol (Hexanol), and tert-amyl alcohol; esters such as ethyl acetate, butyl acetate, and ethyl lactate; organic acids such as oleic acid; ethyl cellosolve, 2-propoxyethanol, ethylene glycol monobutyl ether, hexyl cellosolve, ethylene glycol monophenyl ether, propylene glycol monomethyl ether, and propylene glycol phenyl ether. Examples of alcohol ethers include, but are not limited to, 2-(2-methoxyethoxy)ethanol, 2-(2-ethoxyethoxy)ethanol, diethylene glycol monobutyl ether, diethylene glycol hexyl ether, dipropylene glycol monomethyl ether, dipropylene glycol propyl ether, and dipropylene glycol n-butyl ether.The fillers are generally commercially available from chemical manufacturers such as, for example, Sigma-Aldrich, Tokyo Chemical Industry Co., Ltd. (TCI), Alfa Aesar, and the like.
[0140] There are several methods for evaluating the hydrophilicity of a contact lens surface. First, there is a method for evaluating the hydrophilicity of a contact lens surface by measuring the contact angle. The contact angle can be measured using the sessile drop method or the captive bubble method. In the examples of the present invention, the contact angle was measured using the sessile drop method.
[0141] Next, the contact lens is removed from water, an aqueous solution containing buffer salts, an aqueous solution containing surfactants (such as Poloxamer 407 or Tween-80), or an aqueous solution containing both buffer salts and surfactants (such as Poloxamer 407 or Tween-80). The excess water on the lens surface is then gently shaken off, and the time it takes for the water layer on the lens surface to break is observed and recorded. The time from the start of this test until the water layer on the lens surface breaks is called the Water Break-up Time (WBUT).
[0142] Furthermore, an evaluation method that is more in line with the needs of contact lens users is to have a subject wear sterilized contact lenses, and have a qualified optometrist observe the subject's eyes wearing the contact lenses using a slit lamp to observe how long it takes for the tear film to break up after blinking. The time it takes to observe the tear film break up on the surface of the lens on the eye after blinking begins is called the "tear break-up time (TBUT)." In general, the lower the contact angle of a contact lens, the longer the tear film break up time it corresponds to, and at the same time, the longer the tear film break up time it corresponds to, and the more hydrophilic the contact lens surface is.
[0143] The present invention provides a method for preparing a contact lens, which includes the steps of producing a lens body (dried lens), treating the lens body with a hydrating liquid, and then washing the lens body with an aqueous solution containing water or a buffer solution or an aqueous solution containing a small amount of surfactant. The hydrating liquid is an organic solution containing polyacrylic acid and / or sodium polyacrylate, which results in a contact lens having a lens body coated with polyacrylic acid and / or sodium polyacrylate. The contact lens can be sterilized and disinfected by sterilization (autoclave), and the sterilized contact lens can be provided for wearing. The lens body is composed of a silicon-containing unit, a silicon-free unit, a crosslinking agent, and an initiator, and may contain a filler as required. The preparation of the lens body includes the steps of providing a composition containing a silicon-containing unit, a silicon-free unit, a crosslinking agent, an initiator, etc., mixing and stirring a composition containing a filler as required to form a uniform blend, injecting the blend into a mold for controlling the shape and size of the lens to form a blend-mold complex, and then polymerizing and crosslinking the polymerized units in the blend by a photocuring or heat-curing method, thereby curing and forming the lens body.
[0144] FIG. 2 is a flow chart showing a method for manufacturing a contact lens according to an embodiment of the present invention. Referring to FIG. 2, in an embodiment of the present invention, the method for manufacturing a contact lens includes the following steps: Step S100: Provide a lens body. Step S200: Provide a hydration liquid, the hydration liquid being an organic solution containing polyacrylic acid and / or sodium polyacrylate, the polyacrylic acid and / or sodium polyacrylate occupying 0.01-10 wt% of the weight of the hydration liquid. Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. Step S400: Immerse the lens body in water or an aqueous solution for at least 15 minutes. The aqueous solution contains buffer salts and / or surfactants. As described below, the order of steps S100 and S200 is not particularly limited in this embodiment, and steps S100 and S200 may be performed simultaneously in another embodiment.
[0145] That is, the method for manufacturing contact lenses is composed of two parts. In the first part, a hydration liquid containing a homogeneously mixed polyacrylic acid and / or sodium polyacrylate, an organic solvent, and water is used to soak the lens body. That is, the process of step S200 and step S300. The soaking temperature is room temperature, for example, 20 to 30°C. In the embodiment of the present invention, by providing sufficient adsorption power (hydrogen bonds and van der Waals forces, etc.) by polyacrylic acid and / or sodium polyacrylate and a specific lens formulation, and further selecting polyacrylic acid and / or sodium polyacrylate with a sufficient high molecular weight, the polyacrylic acid and / or sodium polyacrylate can form stable entanglement with the crosslinked polymer structure on the lens surface, so that a sufficient and stable amount remains on the lens surface and is not washed away in the subsequent production process. Therefore, since there is no need to chemically react polyacrylic acid and / or sodium polyacrylate to form a covalent bond with the lens body, heating is not necessarily required in step S300. If the temperature needs to be controlled for other production and manufacturing purposes, the temperature of the hydration liquid can be controlled at 10-80°C. Using an aqueous solution containing polyacrylic acid and / or sodium polyacrylate as the hydration liquid can effectively reduce the hydrophobicity of the surface of the lens body of the well-known silicone hydrogel contact lens (reducing the contact angle, increasing the water break time (WBUT), and increasing the tear film break time when wearing the contact lens). In addition, the first part of hydration can help simultaneously improve the hydrophobicity problem of the lens surface when the lens body transitions from a dry lens to a wet lens. The immersion time can vary from, for example, 30 minutes to 12 hours, which can improve the hydrophobic effect of the lens surface to different degrees, obviously improve the wearing comfort of the lens, and solve the hydrophobic problem of the lens surface.
[0146] The polymer can be selected from poly(acrylic acid) or poly(acrylic acid sodium salt) of different molecular weights, and can be used alone or in combination. In general, to obtain suitable performance, it is preferable that the molecular weight is within a specific range. Specifically, the molecular weight range is preferably 100 kDa or more, more preferably 200 kDa or more, and even more preferably 450 kDa or more. The preferred ratio of the polymer in the hydration solution is 0.01 to 10 wt%, more preferably 0.05 to 5 wt%, and even more preferably 0.1 to 1.5 wt%. The ratio of the polymer in the hydration solution is determined by comprehensively considering the quality requirements of the lens surface (contact angle, water breaking time (WBUT), tear film breakup time when wearing contact lenses, etc.), the molecular weight of the polymer, and the units that make up the lens body.
[0147] In many of the examples of the present invention, the contact lenses before and after sterilization were stained with Toluidine Blue O. This proves that the contact lenses and the manufacturing method thereof according to the examples of the present invention can leave polymers such as polyacrylic acid and / or sodium polyacrylate on the surface of the contact lenses, thereby improving the hydrophilicity of the lens surface.
[0148] In many examples of the present invention, when the molecular weight of the polyacrylic acid and / or sodium polyacrylate selected as the hydrating liquid is 200 kDa or more, it was confirmed that the TBUT was 15 seconds or more within 10 minutes after the subject first put on the contact lens (after putting the contact lens on the eye) and after 8 to 10 hours or more of wearing. In some examples, when the molecular weight of the polyacrylic acid and / or sodium polyacrylate selected as the hydrating liquid is 25 kDa or less, it was found that some subjects had a TBUT of less than 15 seconds at the stage of first wearing the contact lens, even though the contact angle measured on the surface of the contact lens was less than 50 degrees. In some examples, it was found that when the molecular weight of the polyacrylic acid and / or sodium polyacrylate is about 100 kDa, the TBUT exceeded 15 seconds when the subject first put on the contact lens, even though the contact angle measured on the surface of the contact lens was less than 20 to 30 degrees, but some subjects had a TBUT of less than 15 seconds after wearing the contact lens for 8 to 10 hours or more.
[0149] The ratio of the organic solvent in the hydration liquid is 1 to 90 wt %, and preferably 20 to 60 wt %. Commonly used organic solvents include tripropylene glycol methyl ether, dipropylene glycol methyl ether, ethylene glycol n-butyl ether, ketones (acetone, methyl ethyl ketone, etc.), diethylene glycol n-butyl ether, diethylene glycol methyl ether, ethylene glycol phenyl ether, propylene glycol methyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol n-propyl ether, dipropylene glycol n-propyl ether, tripropylene glycol n-butyl ether, ether), propylene glycol n-butyl ether, dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, propylene glycol phenyl ether, dipropylene glycol dimethyl etherglycol dimethyl ether, polyethylene glycols, polypropylene glycols, ethyl acetate, butyl acetate, amyl acetate, methyl lactate, ethyl lactate, isopropyl acetate, monohydric alcohols (1-butanol, 2-butanol, 1-propanol, 2-propanol, etc.) panol, methanol, ethanol, cyclohexanol, cyclopentanol, exo-Norborneol, 1-pentanol, 2-pentanol, 3-pentanol, 1-hexanol, 2-hexanol, 3-hexanol, 3-methyl-2-butanol l-2-butanol, 1-heptanol, 2-heptanol, 1-octanol, 2-octanol, 1-nonanol, 2-nonanol, 1-decanol, 2-decanol, 3-octanol, norborneol, tert-butanol, tert-amyl alcoholalcohol), 2-methyl-2-pentanol, 2,3-dimethyl-2-butanol, 3-methyl-3-pentanol, 1-methylcyclohexanol, 2-methyl-2-hexanol, 3,7-dimethyl-3-octanol, 1-chloro-2-methyl-2-propanol, 2-propano, 2-methyl-2-heptanol, 2-methyl-2-octanol, 2-methyl-2-nonanol, 2-methyl-2-decanol, 3-methyl-3-hexanol (3-methyl-3-hexanol), 3-methyl-3-heptanol, 4-methyl-4-heptanol, 3-methyl-3-octanol, 4-methyl-4-octanol, 3-methyl-3-nonanol, 4-methyl-4-nonanol, 3-methyl-3-octanol, 3-ethyl-3-hexanol 3-hexanol, 3-methyl-3-heptanol, 4-ethyl-4-heptanol, 4-propyl-4-heptanol, 4-isopropyl-4-heptanol, 2,4-dimethyl-2-pentanol, 1-methylcyclopentanol(1-methylcyclopentanol), 1-ethylcyclopentanol, 3-hydroxy-3-methyl-1-butene, 4-hydroxy-4-methyl-1-cyclopentanol, 2-phenyl-2-propanol, 2-methoxy-2-methyl-2-propanol, 2,3,4-trimethyl-3-pentanol, 3,7-dimethyl 3,7-dimethyl-3-octanol, 2-phenyl-2-butanol, 2-methyl-1-phenyl-2-propanol, 3-ethyl-3-pentanol, 1-ethoxy-2-propanol, 3-ethyl-3-pentanol, 1-ethoxy-2-propanol, 1-methyl-2-propanol, t-amyl alcohol alcohol, isopropanol, 1-methyl-2-pyrrolidone, N,N-dimethylpropionamide, dimethyl formamide, dimethyl acetamide, dimethyl propionamide, N-methylpyrrolidinone, polyethylene glycol with a molecular weight of 200 Da or less, tetrahydrofuran, methylene chlorideChloride) and mixtures thereof.
[0150] The second part of the method for manufacturing contact lenses is carried out following the first part, i.e., step S400. Water (RO water or pure water) can be used, an aqueous solution containing buffer salts can be used, an aqueous solution containing a small amount of surfactant (e.g., Poloxamer 407 or Tween-80) can be used, or an aqueous solution containing both buffer salts and a small amount of surfactant can be used. That is, after the lens body is immersed in the hydration liquid for a certain time, it is immersed in water or an aqueous solution to wash away the organic solvent remaining on the surface and inside of the contact lens. The time for immersing the lens body in the water or aqueous solution is preferably at least 15 to 30 minutes, to ensure that cleaning and replacement are performed. The immersion temperature can be constant, or can be alternating between cold and warm temperatures. For example, the lens is immersed in water or an aqueous solution at a constant temperature within a temperature range from room temperature to 60°C, or the lens is immersed alternately in water or an aqueous solution at two temperatures, cold and warm. The temperature range is set so as not to cause any undesirable effect on the lens material. The temperature change promotes thermal expansion and cold contraction of the lens body, washing away the organic solvent. The choice of temperature and whether to use a constant or variable temperature depends on the type of organic solvent used.
[0151] Preferably, the water or the aqueous solution containing buffer salts used in the second part (i.e., step S400) contains a trace amount of surfactant. The amount of surfactant is adjusted in proportion to the number of lens bodies to be treated. For example, when 5 to 100 mL of water is used per lens body to wash 100 lens bodies at one time, 500 mL to 10 L of water is used. The more the amount of water used, the fewer the number of washes, and conversely, the less the amount of water used, the more the number of washes. During or after the process of step S400 is performed, the remaining state of the organic solvent in the lens body can be inspected by any known method. The immersion in step S400 can be repeated several times, for example, the water can be replaced and the lens can be immersed again, and at least one water exchange and a total of two immersions are preferable. The number of immersions can be adjusted according to the type of organic solvent and the remaining state of the organic solvent. For example, the amount of organic solvent measured from the water or aqueous solution after immersion is preferably less than 1 ppm. If it exceeds 1 ppm, the water or aqueous solution can be further replaced and the immersion can be continued.
[0152] The second part of the contact lens manufacturing method is a step of immersing the lens body in water or an aqueous solution, which can further change the expansion rate of the wet lens in the first part, i.e., after the treatment of the second part, the diameter of the lens body can be changed again to reach the desired diameter of the contact lens. The following shows the conditions and results of the lens body manufacturing method in Examples 1 to 3. The compounds used in the following examples include:
[0153] [Table 1]
[0154] [Table 2]
[0155] [Table 3]
[0156] [Table 4]
[0157] The compounds used in the examples will be explained using common abbreviations.
[0158] Example 1:
[0159] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the first formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratios: SIGMA 12.70%, MPDMS (molecular weight about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 819 0.58%, HMEPB 0.57%, the total amount of the above is 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight %, and 9.53% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0160] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0161] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0162] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0163] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 81.24° for the five experimental lenses in this example.
[0164] Example 2:
[0165] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the second formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 15.17%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP 61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount of the above as the denominator of weight %, and 10.17% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0166] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0167] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0168] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0169] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 83.07° for the five experimental lenses in this example.
[0170] Example 3:
[0171] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the third formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 16.11%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP 54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is calculated by using the total amount as the denominator of the weight percent, and 11.33% hexanol and 11.33% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0172] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0173] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0174] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0175] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 68.91° for the five experimental lenses in this example.
[0176] Example 4:
[0177] Step S100: provide a lens body. The lens body of this embodiment is used in the preparation of the fourth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% TPME separately, with the total amount above as the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex at this time is a dry lens (a lens that has not yet been hydrated).
[0178] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0179] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0180] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0181] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 69.03° for the five experimental lenses in this example.
[0182] Example 5:
[0183] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the fifth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, methacryloxypropyl terminated polydimethylsiloxane with polyethylene glycol modification 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% ethyl lactate separately to the total amount above as the weight percent denominator. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. The blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0184] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0185] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0186] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0187] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 70.14° for the five experimental lenses in this example.
[0188] Example 6:
[0189] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the sixth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification 0.58%, TEGDMA 1.26%, 819 0.60%, HMEPB 0.60%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 10.00% hexanol and 10.00% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0190] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0191] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0192] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0193] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 73.89° for the five experimental lenses in this example.
[0194] Example 7:
[0195] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the seventh formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 17.26%, MPDMS 16.15%, HEMA 16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above being 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 12.10% hexanol and 12.10% tAA are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0196] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0197] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0198] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0199] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 79.61° for the five experimental lenses in this example.
[0200] Example 8:
[0201] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the eighth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 17.25%, methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is the denominator of the total amount of the above in weight %, and 11.44% IPA and 11.44% hexanol are added separately. The mixed formulation is stirred for more than 4 hours while flowing nitrogen to ensure that the mixed formulation is completely and uniformly mixed. The mixed compound is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed compound exists in the space between the male mold and the female mold. This mixed mold complex is light-cured, with the ambient temperature maintained between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens mixed complex after the curing process, and the lens in the lens mixed complex is a dry lens (a lens that has not yet been hydrated).
[0202] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0203] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0204] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0205] As a result of observation or measurement and calculation, it was found that the average value of the contact angle of the contact lenses produced in this example was 80.72° for the five experimental lenses in this example.
[0206] Example 9:
[0207] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the ninth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 5.70%, 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 11.11%, MPDMS 12.00%, NVP 34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 11.33% butyl acetate and 11.33% hexanol are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0208] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0209] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0210] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0211] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 85.96° for the five experimental lenses in this example.
[0212] Example 10:
[0213] Step S100: provide a lens body. The lens body of this embodiment is used during the preparation of the tenth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 13.15%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP 32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.44% ethyl lactate and 12.44% hexanol separately, with the total amount above being the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0214] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 2 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0215] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0216] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0217] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 91.86° for the five experimental lenses in this example.
[0218] Example 11:
[0219] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the first formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 12.70%, MPDMS (molecular weight about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 819 0.58%, HMEPB 0.57%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount as the denominator of the weight %, and 9.53% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0220] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0221] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0222] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0223] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 70.94° for the five experimental lenses in this example.
[0224] Example 12:
[0225] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the second formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 15.17%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP 61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount of the above as the denominator of weight %, and 10.17% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0226] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0227] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0228] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0229] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 68.49° for the five experimental lenses in this example.
[0230] Example 13:
[0231] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the third formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 16.11%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP 54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is calculated by using the total amount as the denominator of the weight percent, and 11.33% hexanol and 11.33% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0232] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0233] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0234] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0235] As a result of observation or measurement and calculation, it was found that the average value of the contact angle of the contact lenses produced in this example was 40.12° for the five experimental lenses in this example.
[0236] Example 14:
[0237] Step S100: provide a lens body. The lens body of this embodiment is used in the preparation of the fourth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% TPME separately, with the total amount above as the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex at this time is a dry lens (a lens that has not yet been hydrated).
[0238] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0239] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0240] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0241] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 37.59° for the five experimental lenses in this example.
[0242] Example 15:
[0243] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the fifth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, methacryloxypropyl terminated polydimethylsiloxane with polyethylene glycol modification 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% ethyl lactate separately to the total amount above as the weight percent denominator. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. The blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0244] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0245] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0246] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0247] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 66.52° for the five experimental lenses in this example.
[0248] Example 16:
[0249] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the sixth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification 0.58%, TEGDMA 1.26%, 819 0.60%, HMEPB 0.60%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 10.00% hexanol and 10.00% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0250] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0251] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0252] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0253] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 68.07° for the five experimental lenses in this example.
[0254] Example 17:
[0255] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the seventh formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 17.26%, MPDMS 16.15%, HEMA 16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above being 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 12.10% hexanol and 12.10% tAA are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0256] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0257] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0258] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0259] As a result of observation or measurement and calculation, it was found that the average value of the contact angle of the contact lenses produced in this example was 74.84° for the five experimental lenses in this example.
[0260] Example 18:
[0261] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the eighth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 17.25%, methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is the denominator of the total amount of the above in weight %, and 11.44% IPA and 11.44% hexanol are added separately. The mixed formulation is stirred for more than 4 hours while flowing nitrogen to ensure that the mixed formulation is completely and uniformly mixed. The mixed compound is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed compound exists in the space between the male mold and the female mold. This mixed mold complex is light-cured, with the ambient temperature maintained between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens mixed complex after the curing process, and the lens in the lens mixed complex is a dry lens (a lens that has not yet been hydrated).
[0262] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0263] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0264] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0265] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 84.21° for the five experimental lenses in this example.
[0266] Example 19:
[0267] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the ninth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 5.70%, 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 11.11%, MPDMS 12.00%, NVP 34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 11.33% butyl acetate and 11.33% hexanol are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0268] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0269] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0270] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0271] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 81.98° for the five experimental lenses in this example.
[0272] Example 20:
[0273] Step S100: provide a lens body. The lens body of this embodiment is used during the preparation of the tenth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 13.15%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP 32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.44% ethyl lactate and 12.44% hexanol separately, with the total amount above being the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0274] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 3 to 5 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0275] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0276] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0277] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 87.61° for the five experimental lenses in this example.
[0278] Example 21:
[0279] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the first formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratios: SIGMA 12.70%, MPDMS (molecular weight about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 819 0.58%, HMEPB 0.57%, the total amount of the above is 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight %, and 9.53% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0280] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0281] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0282] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0283] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 65.14° for the five experimental lenses in this example.
[0284] Example 22:
[0285] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the second formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 15.17%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP 61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount of the above as the denominator of weight %, and 10.17% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0286] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0287] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0288] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0289] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 54.09° for the five experimental lenses in this example.
[0290] Example 23:
[0291] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the third formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 16.11%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP 54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is calculated by using the total amount as the denominator of the weight percent, and 11.33% hexanol and 11.33% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0292] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0293] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0294] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0295] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 50.18° for the five experimental lenses in this example.
[0296] Example 24:
[0297] Step S100: provide a lens body. The lens body of this embodiment is used in the preparation of the fourth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% TPME separately, with the total amount above as the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex at this time is a dry lens (a lens that has not yet been hydrated).
[0298] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0299] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0300] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0301] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 44.98° for the five experimental lenses in this example.
[0302] Example 25:
[0303] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the fifth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, methacryloxypropyl terminated polydimethylsiloxane with polyethylene glycol modification 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% ethyl lactate separately to the total amount above as the weight percent denominator. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. The blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0304] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0305] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0306] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0307] As a result of observation or measurement and calculation, it was found that the average value of the contact angle of the contact lenses produced in this example was 40.17° for the five experimental lenses in this example.
[0308] Example 26:
[0309] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the sixth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification 0.58%, TEGDMA 1.26%, 819 0.60%, HMEPB 0.60%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 10.00% hexanol and 10.00% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0310] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0311] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0312] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0313] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 46.49° for the five experimental lenses in this example.
[0314] Example 27:
[0315] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the seventh formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 17.26%, MPDMS 16.15%, HEMA 16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above being 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 12.10% hexanol and 12.10% tAA are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0316] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0317] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0318] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0319] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 69.66° for the five experimental lenses in this example.
[0320] Example 28:
[0321] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the eighth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 17.25%, methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is the denominator of the total amount of the above in weight %, and 11.44% IPA and 11.44% hexanol are added separately. The mixed formulation is stirred for more than 4 hours while flowing nitrogen to ensure that the mixed formulation is completely and uniformly mixed. The mixed compound is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed compound exists in the space between the male mold and the female mold. This mixed mold complex is light-cured, with the ambient temperature maintained between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens mixed complex after the curing process, and the lens in the lens mixed complex is a dry lens (a lens that has not yet been hydrated).
[0322] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0323] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0324] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0325] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 81.07° for the five experimental lenses in this example.
[0326] Example 29:
[0327] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the ninth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 5.70%, 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 11.11%, MPDMS 12.00%, NVP 34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 11.33% butyl acetate and 11.33% hexanol are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0328] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0329] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0330] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0331] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 80.93° for the five experimental lenses in this example.
[0332] Example 30:
[0333] Step S100: provide a lens body. The lens body of this embodiment is used during the preparation of the tenth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 13.15%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP 32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.44% ethyl lactate and 12.44% hexanol separately, with the total amount above being the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0334] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 25 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0335] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0336] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0337] As a result of observation or measurement and calculation, it was found that the average value of the contact angle of the contact lenses produced in this example was 92.02° for the five experimental lenses in this example.
[0338] Example 31:
[0339] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the first formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 12.70%, MPDMS (molecular weight about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 819 0.58%, HMEPB 0.57%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount as the denominator of the weight %, and 9.53% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0340] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0341] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0342] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0343] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 50.21° for the five experimental lenses in this example.
[0344] Example 32:
[0345] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the second formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 15.17%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP 61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount of the above as the denominator of weight %, and 10.17% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0346] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0347] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0348] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0349] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 49.89° for the five experimental lenses in this example.
[0350] Example 33:
[0351] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the third formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 16.11%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP 54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is calculated by using the total amount as the denominator of the weight percent, and 11.33% hexanol and 11.33% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0352] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 0.5 wt% and 99.5 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, with the organic solvent accounting for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0353] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0354] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0355] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 20.02° for the five experimental lenses in this example.
[0356] Example 34:
[0357] Step S100: provide a lens body. The lens body of this embodiment is used in the preparation of the fourth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% TPME separately, with the total amount above as the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex at this time is a dry lens (a lens that has not yet been hydrated).
[0358] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0359] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0360] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0361] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 18.12° for the five experimental lenses in this example.
[0362] Example 35:
[0363] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the fifth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, methacryloxypropyl terminated polydimethylsiloxane with polyethylene glycol modification 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% ethyl lactate separately to the total amount above as the weight percent denominator. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. The blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0364] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0365] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0366] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0367] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 16.89° for the five experimental lenses in this example.
[0368] Example 36:
[0369] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the sixth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification 0.58%, TEGDMA 1.26%, 819 0.60%, HMEPB 0.60%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 10.00% hexanol and 10.00% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0370] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0371] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0372] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0373] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 25.37° for the five experimental lenses in this example.
[0374] Example 37:
[0375] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the seventh formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 17.26%, MPDMS 16.15%, HEMA 16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above being 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 12.10% hexanol and 12.10% tAA are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0376] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0377] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0378] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0379] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 13.79° for the five experimental lenses in this example.
[0380] Example 38:
[0381] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the eighth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 17.25%, methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is the denominator of the total amount of the above in weight %, and 11.44% IPA and 11.44% hexanol are added separately. The mixed formulation is stirred for more than 4 hours while flowing nitrogen to ensure that the mixed formulation is completely and uniformly mixed. The mixed compound is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed compound exists in the space between the male mold and the female mold. This mixed mold complex is light-cured, with the ambient temperature maintained between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens mixed complex after the curing process, and the lens in the lens mixed complex is a dry lens (a lens that has not yet been hydrated).
[0382] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0383] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0384] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0385] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 38.04° for the five experimental lenses in this example.
[0386] Example 39:
[0387] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the ninth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 5.70%, 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 11.11%, MPDMS 12.00%, NVP 34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 11.33% butyl acetate and 11.33% hexanol are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0388] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0389] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0390] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0391] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 80.47° for the five experimental lenses in this example.
[0392] Example 40:
[0393] Step S100: provide a lens body. The lens body of this embodiment is used during the preparation of the tenth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 13.15%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP 32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.44% ethyl lactate and 12.44% hexanol separately, with the total amount above being the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0394] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 100 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0395] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0396] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0397] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 32.03° for the five experimental lenses in this example.
[0398] Example 41:
[0399] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the first formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 12.70%, MPDMS (molecular weight about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 819 0.58%, HMEPB 0.57%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount as the denominator of the weight %, and 9.53% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0400] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0401] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0402] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0403] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 51.47° for the five experimental lenses in this example.
[0404] Example 42:
[0405] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the second formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 15.17%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP 61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount of the above as the denominator of weight %, and 10.17% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0406] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0407] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0408] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0409] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 46.38° for the five experimental lenses in this example.
[0410] Example 43:
[0411] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the third formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 16.11%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP 54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is calculated by using the total amount as the denominator of the weight percent, and 11.33% hexanol and 11.33% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0412] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0413] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0414] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0415] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 13.98° for the five experimental lenses in this example.
[0416] Example 44:
[0417] Step S100: provide a lens body. The lens body of this embodiment is used in the preparation of the fourth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% TPME separately, with the total amount above as the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex at this time is a dry lens (a lens that has not yet been hydrated).
[0418] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0419] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0420] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0421] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 8.09° for the five experimental lenses in this example.
[0422] Example 45:
[0423] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the fifth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, methacryloxypropyl terminated polydimethylsiloxane with polyethylene glycol modification 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% ethyl lactate separately to the total amount above as the weight percent denominator. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. The blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0424] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0425] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0426] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0427] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 7.46° for the five experimental lenses in this example.
[0428] Example 46:
[0429] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the sixth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification 0.58%, TEGDMA 1.26%, 819 0.60%, HMEPB 0.60%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 10.00% hexanol and 10.00% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0430] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 1 wt% and 99 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0431] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0432] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0433] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 13.55° for the five experimental lenses in this example.
[0434] Example 47:
[0435] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the seventh formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 17.26%, MPDMS 16.15%, HEMA 16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above being 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 12.10% hexanol and 12.10% tAA are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0436] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and dipropylene glycol n-butyl ether or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared.
[0437] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0438] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0439] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 16.01° for the five experimental lenses in this example.
[0440] Example 48:
[0441] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the eighth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 17.25%, methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is the denominator of the total amount of the above in weight %, and 11.44% IPA and 11.44% hexanol are added separately. The mixed formulation is stirred for more than 4 hours while flowing nitrogen to ensure that the mixed formulation is completely and uniformly mixed. The mixed compound is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed compound exists in the space between the male mold and the female mold. This mixed mold complex is light-cured, with the ambient temperature maintained between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens mixed complex after the curing process, and the lens in the lens mixed complex is a dry lens (a lens that has not yet been hydrated).
[0442] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0443] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0444] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0445] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 42.96° for the five experimental lenses in this example.
[0446] Example 49:
[0447] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the ninth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 5.70%, 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 11.11%, MPDMS 12.00%, NVP 34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 11.33% butyl acetate and 11.33% hexanol are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0448] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0449] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0450] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0451] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 69.77° for the five experimental lenses in this example.
[0452] Example 50:
[0453] Step S100: provide a lens body. The lens body of this embodiment is used during the preparation of the tenth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 13.15%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP 32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.44% ethyl lactate and 12.44% hexanol separately, with the total amount above being the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0454] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 200 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0455] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0456] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0457] As a result of observation or measurement and calculation, it was found that the average value of the contact angle of the contact lenses produced in this example was 41.48° for the five experimental lenses in this example.
[0458] Example 51:
[0459] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the first formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 12.70%, MPDMS (molecular weight about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 819 0.58%, HMEPB 0.57%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount as the denominator of the weight %, and 9.53% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0460] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0461] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0462] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0463] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 48.15° for the five experimental lenses in this example.
[0464] Example 52:
[0465] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the second formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 15.17%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP 61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount of the above as the denominator of weight %, and 10.17% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0466] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0467] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0468] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0469] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 47.09° for the five experimental lenses in this example.
[0470] Example 53:
[0471] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the third formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 16.11%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP 54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is calculated by using the total amount as the denominator of the weight percent, and 11.33% hexanol and 11.33% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0472] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0473] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0474] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0475] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 15.72° for the five experimental lenses in this example.
[0476] Example 54:
[0477] Step S100: provide a lens body. The lens body of this embodiment is used in the preparation of the fourth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% TPME separately, with the total amount above as the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex at this time is a dry lens (a lens that has not yet been hydrated).
[0478] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0479] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0480] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0481] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 7.98° for the five experimental lenses in this example.
[0482] Example 55:
[0483] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the fifth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, methacryloxypropyl terminated polydimethylsiloxane with polyethylene glycol modification 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% ethyl lactate separately to the total amount above as the weight percent denominator. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. The blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0484] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0485] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0486] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0487] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 6.5° for the five experimental lenses in this example.
[0488] Example 56:
[0489] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the sixth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification 0.58%, TEGDMA 1.26%, 819 0.60%, HMEPB 0.60%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 10.00% hexanol and 10.00% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0490] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0491] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0492] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0493] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 8.19° for the five experimental lenses in this example.
[0494] Example 57:
[0495] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the seventh formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 17.26%, MPDMS 16.15%, HEMA 16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above being 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 12.10% hexanol and 12.10% tAA are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0496] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0497] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0498] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0499] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 20.14° for the five experimental lenses in this example.
[0500] Example 58:
[0501] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the eighth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 17.25%, methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is the denominator of the total amount of the above in weight %, and 11.44% IPA and 11.44% hexanol are added separately. The mixed formulation is stirred for more than 4 hours while flowing nitrogen to ensure that the mixed formulation is completely and uniformly mixed. The mixed compound is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed compound exists in the space between the male mold and the female mold. This mixed mold complex is light-cured, with the ambient temperature maintained between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens mixed complex after the curing process, and the lens in the lens mixed complex is a dry lens (a lens that has not yet been hydrated).
[0502] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0503] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0504] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0505] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was found to be 49.87° for the five experimental lenses in this example.
[0506] Example 59:
[0507] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the ninth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 5.70%, 3-[tris(trimethylsiloxy)silyl]propylvinylcarbamate 11.11%, MPDMS 12.00%, NVP 34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100% including monomers, initiators, and crosslinkers. The lens formulation is based on the total amount of the above as the denominator of weight percent, and 11.33% butyl acetate and 11.33% hexanol are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0508] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0509] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0510] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0511] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 72.06° for the five experimental lenses in this example.
[0512] Example 60:
[0513] Step S100: provide a lens body. The lens body of this embodiment is used during the preparation of the tenth formulation among the ten different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 13.15%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP 32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.44% ethyl lactate and 12.44% hexanol separately, with the total amount above being the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0514] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 450 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0515] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0516] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0517] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 36.74° for the five experimental lenses in this example.
[0518] Example 61:
[0519] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the first formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 12.70%, MPDMS (molecular weight about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 819 0.58%, HMEPB 0.57%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount as the denominator of the weight %, and 9.53% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0520] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 1250 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0521] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0522] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0523] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 50.27° for the five experimental lenses in this example.
[0524] Example 62:
[0525] Step S100: Provide a lens body. The lens body of this embodiment is used in the preparation of the second formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: TRIS 15.17%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP 61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is made by using the total amount of the above as the denominator of weight %, and 10.17% hexanol and 9.53% ethyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0526] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 1250 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0527] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0528] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0529] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 52.07° for the five experimental lenses in this example.
[0530] Example 63:
[0531] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the third formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: SIGMA 16.11%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP 54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100% including monomer, initiator, and crosslinker. The lens formulation is calculated by using the total amount as the denominator of the weight percent, and 11.33% hexanol and 11.33% propyl acetate are added separately. The mixed blend is stirred for more than 4 hours under nitrogen flow to ensure that the mixed blend is completely and uniformly mixed. The mixed blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a mixed mold complex is formed, and the liquid mixed blend is present in the space between the male mold and the female mold. This mixed mold complex is light-cured by maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The mixed mold complex becomes a lens blend complex after the curing process, and the lens in the lens blend complex is a dry lens (a lens that has not yet been hydrated).
[0532] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 1250 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0533] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0534] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0535] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 18.64° for the five experimental lenses in this example.
[0536] Example 64:
[0537] Step S100: provide a lens body. The lens body of this embodiment is used in the preparation of the fourth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% TPME separately, with the total amount above as the denominator in weight percent. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. This blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex at this time is a dry lens (a lens that has not yet been hydrated).
[0538] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 1250 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0539] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0540] Step S400: The lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is immersed in the four water tanks in sequence for one hour for a total of four hours. During immersion, stirring may be performed occasionally. In this process, the immersion time may be increased or decreased, and the number of times the water tanks are replaced may be increased or decreased. The more times the water tanks are replaced, the more the total immersion time can be shortened. For example, the process is changed to immersing in five water tanks in sequence for 30 minutes each. The immersion temperature is room temperature. In another embodiment, the lens body is immersed in water or an aqueous solution for at least 60 minutes to form a contact lens. In this case, the lens body is immersed in four water tanks in sequence, and is immersed in each water tank for 15 minutes for a total of 60 minutes.
[0541] As a result of observation or measurement and calculation, the average value of the contact angle of the contact lenses produced in this example was obtained to be 13.28° for the five experimental lenses in this example.
[0542] Example 65:
[0543] Step S100: Provide a lens body. The lens body of this embodiment is used during the preparation of the fifth formulation among the 10 different formulations used in the embodiment. The different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, the type of silicon-containing units, and the type of non-silicon-containing units. In this embodiment, the lens formulation is prepared with the following ratio: 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, methacryloxypropyl terminated polydimethylsiloxane with polyethylene glycol modification 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomer, initiator, and crosslinker. The lens blend is made by adding 10.00% ethyl acetate and 10.00% ethyl lactate separately to the total amount above as the weight percent denominator. The blend is stirred for more than 4 hours while flowing nitrogen to ensure that the blend is completely and uniformly mixed. The blend is injected into a female mold made by injection molding, and a male mold made by injection molding is pressed against this female mold. In this way, a blended mold complex is formed, and the liquid blend is present in the space between the male mold and the female mold. The blended mold complex is photocured by maintaining the atmospheric temperature between 33°C and 38°C, and the irradiation time is 60 minutes. The blended mold complex becomes a lens blended complex after a curing process, and the lens in the lens blended complex is a dry lens (a lens that has not yet been hydrated).
[0544] Step S200: Prepare the hydration liquid. The hydration liquid (hydration liquid 1) in this embodiment is a complete mixture of 3 wt% and 97 wt% organic aqueous solutions of PAA with a molecular weight of 1250 KDa, and the organic solvent accounts for 30 wt% of the weight of the hydration liquid, and IPA or the like is used as the organic solvent. In this embodiment, the hydration liquids in the first tank and the second tank are prepared in advance.
[0545] Step S300: Immerse the lens body in the hydration liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and immersed in the hydration liquid of the first tank for 1 hour, then in the hydration liquid of the second tank for 1 hour, for a total of 2 hours to process the first portion. The lens body can also be immersed in the same tank for a sufficient time without changing the tank. The immersion temperature is room temperature.
[0546] Step S400: The lens body is immers...
Claims
1. A contact lens comprising at least one silicone-containing monomer and wherein the surface of the contact lens comprises polyacrylic acid and / or sodium polyacrylate having a molecular weight greater than 100 kDa.
2. The contact lens of claim 1 , wherein the polyacrylic acid and / or the sodium polyacrylate has a molecular weight of greater than 200 kDa.
3. The contact lens of claim 1 , wherein the polyacrylic acid and / or the sodium polyacrylate has a molecular weight of greater than 450 kDa.
4. 2. The contact lens of claim 1, wherein the at least one silicone-containing monomer comprises at least one of 3-[tris(trimethylsiloxy)silyl]propyl methacrylate, (3-methacryloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methylsilane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propyl carbamate, 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate.
5. 5. The contact lens of claim 4, wherein the at least one silicone-containing monomer further comprises at least one of monomethacryloyloxypropyl terminated polydimethylsiloxane, monomethacryloxypropyl terminated carbamate polydimethylsiloxane, mono-(3-methacryloxy-2-hydroxypropyloxy)propyl terminated mono-butyl terminated polydimethylsiloxane.
6. The contact lens of claim 1 comprising N-vinylpyrrolidone or N-methyl-N-vinylacetamide.
7. 7. The contact lens of claim 6, further comprising a filler, the content of said N-vinylpyrrolidone or said N-methyl-N-vinylacetamide being 30 to 65% of the weight excluding said filler.
8. 7. The contact lens of claim 6, further comprising a filler, the content of said N-vinylpyrrolidone or said N-methyl-N-vinylacetamide being 35 to 55% of the weight excluding said filler.
9. The contact lens of claim 6 comprising 2-hydroxyethyl methacrylate.
10. The contact lens of claim 5 further comprising at least one silicon-containing crosslinker.
11. 11. The contact lens of claim 10, wherein the at least one silicon-containing crosslinker comprises at least one of methacryloxypropyl-terminated polydimethylsiloxane, methacryloxypropyl-terminated carbamate polydimethylsiloxane, methacryloxypropyl-terminated polydimethylsiloxane with polyethylene glycol modification, 1,3-bis[4-(vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, bis-3-methacryloxy-2-hydroxypropyloxypropylpolydimethylsiloxane.
12. The contact lens of claim 10, wherein the molecular weight of the at least one silicon-containing crosslinker is in the range of 500 to 3000.
13. The contact lens of claim 1 further comprising at least one non-silicon containing crosslinker.
14. 14. The contact lens of claim 13, wherein the at least one non-silicon containing crosslinker comprises at least one of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane trimethacrylate.
15. 2. The contact lens of claim 1, wherein the contact lens has a contact angle of 60 degrees or less and a water break time (WBUT) of 20 seconds or more.
16. 1. A silicone hydrogel contact lens comprising a first silicone-containing monomer, a second silicone-containing monomer, a first hydrophilic monomer, a second hydrophilic monomer, and a silicon-containing crosslinker, The first silicone-containing monomer has the following structure: 【Chemistry 1】 Among these, A has the following structure: 【Chemistry 2】 or the following structure: 【Chemistry 3】 R 1 is H or CH 3 Or OSi(CH 3 ) 3 and R 2 is H or CH 3 Or OSi(CH 3 ) 3 And L 1 is the following structure or a combination thereof: 【Chemistry 4】 n1 is 1 to 5, m1 is 1 to 4, m2 is 0 to 1, m3 is 1 to 4, m4 is 0 to 1, m5 is 1 to 4, and m6 is 1 to 4. The second silicone-containing monomer comprises a first structure or a second structure. The first structure: 【Chemistry 5】 a is 0 to 20. 3 is H or CH 3 Or C 2 H 5 and R 4 is H or CH 3 Or OSi(CH 3 ) 3 and R 5 is H or CH 3 Or OSi(CH 3 ) 3 And L 2 is the following structure or a combination thereof: 【Chemistry 6】 n6 is 1 to 5, n7 is 1 to 5, m7 is 1 to 4, m8 is 0 to 1, m9 is 1 to 4, m10 is 0 to 1, m11 is 1 to 4, m12 is 1 to 4, m13 is 0 to 1, m14 is 1 to 4, and m15 is 1 to 4. The second structure: 【Chemistry 7】 c is 0 to 20. 10 is H or CH 3 Or C 2 H 5 and R 11 is H or CH 3 Or OSi(CH 3 ) 3 and R 12 is H or CH 3 Or OSi(CH 3 ) 3 And L 5 is the following structure or a combination thereof: O or NH; L 6 is the following structure or a combination thereof: 【Chemistry 8】 n20 is 1 to 5, m34 is 1 to 4, m35 is 0 to 1, m36 is 1 to 4, m37 is 0 to 1, m38 is 1 to 4, and m39 is 1 to 4. The first hydrophilic monomer includes an N-vinyl group. The second hydrophilic monomer is different from the first hydrophilic monomer. The surface of the silicone hydrogel contact lens comprises polyacrylic acid and / or sodium polyacrylate having a molecular weight greater than 100 kDa.
17. 17. The silicone hydrogel contact lens of claim 16, wherein the first silicone-containing monomer comprises at least one of 3-[tris(trimethylsiloxy)silyl]propyl methacrylate, (3-methacryloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methylsilane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propyl carbamate, and 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate.
18. 17. The silicone hydrogel contact lens of claim 16, wherein the second silicone-containing monomer comprises at least one of monomethacryloyloxypropyl terminated polydimethylsiloxane, monomethacryloxypropyl terminated carbamate polydimethylsiloxane, mono-(3-methacryloxy-2-hydroxypropyloxy)propyl terminated mono-butyl terminated polydimethylsiloxane.
19. The silicone hydrogel contact lens of claim 18, wherein the second silicone-containing monomer has a molecular weight of 350 to 2500.
20. The silicone hydrogel contact lens of claim 18, wherein the second silicone-containing monomer has a molecular weight of 500 to 1500.
21. 17. The silicone hydrogel contact lens of claim 16, further comprising a filler, wherein the combined content of the first silicone-containing monomer and the second silicone-containing monomer accounts for 15-60% of the weight of the silicone hydrogel contact lens after removal of the filler.
22. 17. The silicone hydrogel contact lens of claim 16, further comprising a filler, wherein the combined content of the first silicone-containing monomer and the second silicone-containing monomer accounts for 25-45% of the weight of the silicone hydrogel contact lens after removal of the filler.
23. The silicone hydrogel contact lens of claim 16, wherein the first hydrophilic monomer is N-vinylpyrrolidone or N-methyl-N-vinylacetamide.
24. The silicone hydrogel contact lens of claim 23, further comprising a filler, and wherein the content of the first hydrophilic monomer is 30-65% of the weight of the silicone hydrogel contact lens after removal of the filler.
25. The silicone hydrogel contact lens of claim 23, further comprising a filler, and wherein the content of the first hydrophilic monomer is 35-55% of the weight of the silicone hydrogel contact lens after removal of the filler.
26. The silicone hydrogel contact lens of claim 16, wherein the second hydrophilic monomer comprises 2-hydroxyethyl methacrylate.
27. 17. The silicone hydrogel contact lens of claim 16, wherein the silicon-containing crosslinker comprises the following structure: 【Chemistry 9】 b is 0 to 20. 6 is H or CH 3 Or C 2 H 5 and R 7 is H or CH 3 Or OSi(CH 3 ) 3 And L 3 is the following structure or a combination thereof: 【Chemistry 10】 n12 is 1 to 5, n13 is 1 to 5, m16 is 1 to 4, m17 is 0 to 1, m18 is 1 to 4, m19 is 0 to 1, m20 is 1 to 4, m21 is 1 to 4, m22 is 0 to 1, m23 is 1 to 4, and m24 is 1 to 4. R 8 is the following structure or a combination thereof: 【Chemistry 11】 R 9 is H or CH 3 Or C 2 H 5 And L 4 is the following structure or a combination thereof: 【Chemistry 12】 n18 is 1 to 5, n19 is 1 to 5, m25 is 1 to 4, m26 is 0 to 1, m27 is 1 to 4, m28 is 0 to 1, m29 is 1 to 4, m30 is 1 to 4, m31 is 0 to 1, m32 is 1 to 4, and m33 is 1 to 4.
28. 17. The silicone hydrogel contact lens of claim 16, wherein the silicon-containing crosslinker comprises the following structure: 【Chemistry 13】 d is 0 to 20. 13 is H or CH 3 Or C 2 H 5 and R 14 is H or CH 3 Or C 2 H 5 And L 7 is the following structures or combinations thereof: O or NH; L 8 is the following structure or a combination thereof: 【Chemistry 14】 n25 is 1 to 5, m40 is 1 to 4, m41 is 0 to 1, m42 is 1 to 4, m43 is 0 to 1, m44 is 1 to 4, and m45 is 1 to 4. R 15 is the following structure or a combination thereof: 【Chemistry 15】 R 16 is H or CH 3 Or C 2 H 5 And L 9 is the following structure or a combination thereof: 【Chemistry 16】 n31 is 1 to 5, m46 is 1 to 4, m47 is 0 to 1, m48 is 1 to 4, m49 is 0 to 1, m50 is 1 to 4, and m51 is 1 to 4.
29. 17. The silicone hydrogel contact lens of claim 16, wherein the silicon-containing crosslinker comprises at least one of methacryloxypropyl-terminated polydimethylsiloxane, methacryloxypropyl-terminated carbamate polydimethylsiloxane, methacryloxypropyl-terminated polydimethylsiloxane containing polyethylene glycol modification, 1,3-bis[4-(vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, and bis-3-methacryloxy-2-hydroxypropyloxypropylpolydimethylsiloxane.
30. 30. The silicone hydrogel contact lens of claim 29, wherein the molecular weight of the silicon-containing crosslinker is in the range of 500 to 3000.
31. 17. The silicone hydrogel contact lens of claim 16, further comprising at least one non-silicon containing crosslinker.
32. 32. The silicone hydrogel contact lens of claim 31, wherein the at least one non-silicon containing crosslinker comprises at least one of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane trimethacrylate.
33. The silicone hydrogel contact lens of claim 16, wherein the polyacrylic acid and / or the sodium polyacrylate has a molecular weight of greater than 200 kDa.
34. The silicone hydrogel contact lens of claim 16, wherein the polyacrylic acid and / or the sodium polyacrylate has a molecular weight of greater than 450 kDa.
Citation Information
Patent Citations
Contact lenses and methods of coating contact lenses
JP2003511734A
Wet hydrogels containing acyclic polyamides
JP2007526946A
Method for producing silicone-containing copolymer molded article having hydrophilic surface, and silicone hydrogel contact lens having hydrophilic surface
JP2015011314A
Ophthalmic devices derived from grafted polymer networks and processes for preparing and using them - Patents.com
JP2021512374A
Silicone hydrogel lenses with cross-linked hydrophilic coatings - Patent Application 20070122999
JP2022031756A