Decorative sheet and method for producing the same, and substrate

A PET-based decorative sheet with a crystal nucleating agent and controlled cooling achieves enhanced water vapor barrier and adhesion, addressing the limitations of existing PET sheets by eliminating stretching and ensuring consistent dimensional stability.

JP2024167570AInactive Publication Date: 2024-12-04TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023083740
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Decorative sheets using paper or olefin resin as base materials have poor water vapor barrier properties, leading to issues like warping or cracking due to humidity, while PET-based sheets, though improved by stretching for crystallinity, suffer from inadequate adhesion and anisotropic dimensional changes.

Method used

A decorative sheet with a PET base material containing a crystal nucleating agent, such as sodium or lithium salts of saturated fatty acids, is produced by controlled cooling to achieve a cold crystallization heat of 3 J/g or less, eliminating the need for stretching and enhancing adhesion.

Benefits of technology

The solution provides a highly reliable decorative sheet with improved water vapor barrier properties and strong adhesion between layers, avoiding issues of anisotropy and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167570000001_ABST
    Figure 2024167570000001_ABST
Patent Text Reader

Abstract

To provide a decorative sheet with high reliability that offers superior water vapor barrier properties and ensures superior adhesion between a design layer and a substrate, and a method for producing the same.SOLUTION: A decorative sheet 10 has a design layer 2 laminated on a substrate 1. The substrate 1 is composed of polyethylene terephthalate, containing a crystal nucleating agent. The substrate 1 has a cold crystallization enthalpy of 3 J / g or less. The crystal nucleating agent is composed of one or more compounds selected from sodium or lithium salts of saturated fatty acids containing 18 to 28 carbon atoms per molecule.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a technique relating to a decorative sheet and a method for manufacturing a decorative sheet. The present invention is particularly suitable for a decorative sheet having excellent water vapor barrier properties and a method for manufacturing the same. [Background technology]

[0002] In a decorative sheet, for example, a design layer is formed on a substrate. Paper or olefin resin is generally used as the substrate for the decorative sheet. However, decorative sheets using these substrates have poor water vapor barrier properties. For this reason, there is concern that, depending on the application, the wood substrate to which the decorative sheet is attached may be affected by the humidity of the outside air, causing warping, cracking, or the like. In response to this, decorative sheets using polyethylene terephthalate resin (hereinafter also referred to as PET) as a substrate are known (see, for example, thermoplastic resin film 6 in Patent Document 1).

[0003] Resin substrates are manufactured, for example, by general cast film formation using a T-die. However, although PET is a crystalline resin, it has a slow crystallization rate. For this reason, a PET substrate manufactured using a T-die (hereinafter also referred to as a PET substrate) is in an amorphous state as is. Therefore, in order to bring it into a crystallized state that contributes to improving the water vapor barrier property, it is common to perform a stretching process on the PET substrate immediately after casting to crystallize the PET that constitutes the substrate.

[0004] Crystallization of PET by stretching improves various properties of the PET base material, such as mechanical strength and water vapor barrier properties. However, when the PET base material is used as the base material for a decorative sheet, there is a problem that the adhesion with the design layer printed on the base material is insufficient, which may cause problems with the reliability of the decorative sheet. In addition, the dimensional change due to heat shrinkage is anisotropic, which may have a negative effect on the manufacturing process of the decorative sheet. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-15739 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in light of the above-mentioned problems, and aims to provide a highly reliable decorative sheet that has good water vapor barrier properties and good adhesion between the design layer and the substrate, and a method for producing the same. [Means for solving the problem]

[0007] In order to solve the problems, one aspect of the present invention is a decorative sheet having a design layer laminated on a substrate, the substrate being made of polyethylene terephthalate containing a crystal nucleating agent and having a cold crystallization heat of 3 J / g or less, the crystal nucleating agent consisting of one or more compounds selected from sodium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule, and lithium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule.

[0008] Another aspect of the present invention is a method for manufacturing a decorative sheet in which a design layer is laminated on a substrate, in which a mixture of polyethylene terephthalate resin and a crystal nucleating agent is used as a raw material, the resin is extruded in a molten state and in a sheet shape using a T-die extruder, and the extruded molten resin is solidified while controlling the cooling rate using a metal temperature-control roll to produce the substrate, and one or more compounds selected from sodium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule and lithium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule are used as the crystal nucleating agent. Effect of the Invention

[0009] According to an embodiment of the present invention, it is possible to provide a highly reliable decorative sheet that has good water vapor barrier properties and good adhesion between the design layer and the substrate. [Brief description of the drawings]

[0010] [Figure 1] 1 is a cross-sectional view illustrating an example of the configuration of a decorative sheet according to an embodiment of the present invention. [Diagram 2] 1 is a configuration diagram showing an example of a main part of a decorative sheet manufacturing apparatus according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Here, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of each thickness, etc. are different from the actual ones. In addition, the embodiments shown below are examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited to the materials, shapes, etc. of the components described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims.

[0012] (composition) The decorative sheet 10 of this embodiment is a laminate in which a design layer 2 is laminated directly on a substrate 1, as shown in FIG. The decorative sheet 10 shown in Fig. 1 is constructed by laminating a design layer 2, a transparent resin layer 3, and a surface protective layer 4 in this order on one surface (the upper surface in Fig. 1) of a substrate 1. Other layers may be laminated on the other surface (the lower surface in Fig. 1) of the substrate 1.

[0013] <Base material 1> The substrate 1 of this embodiment is made of PET. That is, the substrate 1 is mainly composed of polyethylene terephthalate resin. The main component means, for example, 90% by mass or more of the whole. The substrate 1 of the decorative sheet is flexible and in the form of a sheet. The substrate 1 contains a crystal nucleating agent as an additive. In this embodiment, one or more compounds selected from sodium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule and lithium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule are used as the crystal nucleating agent.

[0014] Examples of saturated fatty acids include stearic acid (carbon number 18), arachidic acid (carbon number 20), heneicosylic acid (carbon number 21), behenic acid (carbon number 22), lignoceric acid (carbon number 24), cerotic acid (carbon number 26), montanic acid (carbon number 28), and their chain isomers. In particular, stearic acid, behenic acid, and montanic acid, which are highly versatile, are preferred as saturated fatty acids. Furthermore, from the viewpoint of the appearance of the PET substrate 1, behenic acid (C21H43COOH) or montanic acid (C27H55COOH) are particularly preferred as saturated fatty acids.

[0015] The blending amount (addition amount) of the crystal nucleating agent varies depending on the manufacturing conditions of the PET substrate 1, but is, for example, 0.05 to 0.5 parts by mass relative to 100 parts by mass of the polyethylene terephthalate resin. If the blending amount is 0.05 parts or less, there is a risk of a decrease in the water vapor barrier property due to insufficient crystallinity of the PET substrate 1, and a deterioration in film formability in the manufacturing process described below. On the other hand, if the blending amount exceeds 0.5 parts by mass, the PET substrate 1 is prone to poor appearance such as cloudiness or bumps. When the PET substrate 1 is composed of a plurality of layers, the blending amount of the crystal nucleating agent is determined individually for each layer.

[0016] The PET substrate 1 may contain a pigment to impart hiding power and design properties. Examples of pigments that may be used include titanium oxide, iron oxide, and chromium oxide. The PET substrate 1 may contain known additives other than the crystal nucleating agent. When the PET substrate 1 is composed of a plurality of layers, the pigment is contained in at least the layer in contact with the design layer 2 .

[0017] The substrate 1 may be composed of multiple layers. In this case, each layer constituting the substrate 1 is made of PET. When the substrate 1 is composed of multiple layers, the above-mentioned crystal nucleating agent is added at least to the substrate 1 of the outermost layer away from the design layer 2 (the layer constituting the opposite surface). Furthermore, the PET substrate 1 of this embodiment has a cold crystallization heat quantity adjusted to 3 J / g or less. The amount of heat required for cold crystallization of the PET substrate 1 can be controlled, for example, by controlling the temperature of a temperature-regulating roll during the production of the PET substrate 1.

[0018] <Design layer 2> The design layer 2 is formed by various printing methods such as gravure printing and offset printing on one surface of the PET substrate 1. That is, the design layer 2 is a layer that imparts a picture pattern, such as a wood grain pattern or a stone grain pattern, printed for decorative purposes. The type of printing ink used to form the design layer 2 is not particularly limited, and any known printing ink used to form the decorative sheet 10 can be used. Specifically, the printing ink may be prepared by appropriately adding organic or inorganic dyes or pigments, and if necessary, fillers, tackifiers, dispersants, defoamers, stabilizers and other additives to binder resins such as polyvinyl chloride resins, vinyl chloride-vinyl acetate copolymer resins, butyral, acrylic, urethane, polyester, epoxy, alkyd, polyamide, etc., and adjusting the viscosity to a desired level with an appropriate diluting solvent. The printing ink may be a printing ink suitable for each printing method. The design layer 2 may be configured as a laminate of two or more layers.

[0019] <Transparent resin layer 3> The transparent resin layer 3 is formed of, for example, a transparent thermoplastic resin so that the design such as a picture of the design layer 2 can be seen through the transparent resin layer 3. The transparent resin layer 3 may be made of any resin other than polyvinyl chloride resin as long as it is transparent.

[0020] <Surface protection layer 4> The surface protective layer 4 is located on the outermost surface of the decorative sheet 10 and plays a role in protecting the design layer 2, etc. In other words, the surface protective layer 4 improves the surface properties of the decorative sheet 10, imparting scratch resistance, stain resistance, slipperiness, etc. to the surface of the decorative sheet 10, and influencing the gloss, tactile feel, etc. The surface protection layer 4 preferably contains an ionizing radiation curable resin such as an ultraviolet curable resin. Specifically, the material of the surface protection layer 4 is preferably a mixture (blend resin) of a thermosetting resin and an ultraviolet curable resin (UV curable resin), for example.

[0021] (Method of manufacturing decorative sheet 10) The decorative sheet 10 of this embodiment is produced by forming a design layer 2 on a substrate 1 by printing, and then laminating a transparent resin layer 3 and a surface protective layer 4 in this order on top of the design layer 2. The substrate 1 of this embodiment is produced using an apparatus as shown in FIG. That is, a raw material consisting of a mixture of PET and a crystal nucleating agent is fed into a T-die extruder 11, and melt-extruded by the T-die extruder 11, so that a molten resin 20 is molded into a sheet shape and extruded from the T-die 11A. The extruded molten resin 20 is guided and conveyed by a metal temperature control roll 12, and solidified while the cooling temperature is controlled in a direction to suppress the cooling rate. As described above, the crystal nucleating agent added to PET is one or more compounds selected from sodium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule and lithium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule. The amount of the crystal nucleating agent in the raw material is, for example, 0.05 to 0.5 parts by mass with respect to 100 parts by mass of PET resin.

[0022] When producing such a substrate 1, the line speed of the solidified resin 20 is controlled by the melt extrusion speed from the T-die extruder 11 and the rotation speed of the temperature-controlling roll 12, and the surface temperature of the temperature-controlling roll 12 is controlled by the temperature controller 13. Here, the crystallinity of the PET substrate 1 varies depending on the line speed and the surface temperature of the temperature-regulating roll 12 during solidification. The roll temperature (roll surface temperature) of the temperature-regulating roll 12 is usually adjusted to 140°C to 220°C. If the roll temperature is below 140°C, the cooling rate from the molten state becomes too high, resulting in insufficient crystallinity. As a result, the peelability from the temperature-regulating roll 12 becomes poor, and the substrate 1 is likely to deform when peeled. On the other hand, if the roll temperature is above 220°C, the temperature change after passing through the temperature-regulating roll 12 is large, and the substrate 1 is likely to deform.

[0023] From this viewpoint, the line speed and the surface temperature of the temperature-adjusting roll 12 are controlled so that the PET substrate 1 crystallizes. The cooling speed of the solidified PET substrate 1 is then suppressed to increase the crystallinity of the PET substrate 1. This makes it possible to keep the cold crystallization heat of the PET substrate 1 at 3 J / g or less without performing a stretching process.

[0024] (Actions and others) PET is a resin that crystallizes slowly, and when extruded using a normal T-die, it solidifies from a molten state to an amorphous state. In this embodiment, a crystal nucleating agent is blended into the PET that constitutes the PET substrate 1. Then, a temperature-controlled roll 12 is used during T-die extrusion molding to suppress the cooling rate of the PET, thereby increasing the crystallinity of the PET substrate 1. One of the indicators of crystallinity is the heat of cold crystallization. Cold crystallization is a phenomenon in which solid amorphous PET crystallizes at temperatures below its melting point, and progresses when heated to 120°C to 140°C or higher. The amount of heat generated during cold crystallization is the heat of cold crystallization, and it can be measured using a differential scanning calorimeter (DSC).

[0025] In this embodiment, the cooling rate of the resin 20 is controlled so that the heat of cold crystallization of the PET substrate 1 is 3 J / g or less. If it exceeds 3 J / g, the crystallinity of the PET is insufficient, and the water vapor barrier property of the decorative sheet 10 is not fully expressed.

[0026] For the above reasons, in this embodiment, the adhesiveness with the design layer 2 required for the decorative sheet 10 is maintained while improving the water vapor barrier property of the substrate 1 . Here, the PET substrate 1 of this embodiment does not require stretching because the cooling rate is controlled to crystallize the PET. That is, since the PET substrate 1 of this embodiment does not require stretching, the anisotropy caused by dimensional changes is suppressed compared to conventional PET substrates that have been stretched, and the reliability of the decorative sheet is increased. In addition, the PET substrate 1 of this embodiment can improve the adhesion with the design layer 2 compared to PET substrates that have been stretched.

[0027] (others) The present disclosure may also have the following configuration. (1) A decorative sheet having a design layer laminated on a substrate, The substrate is made of polyethylene terephthalate containing a crystal nucleating agent and has a cold crystallization heat of 3 J / g or less; The crystal nucleating agent is composed of one or more compounds selected from the group consisting of sodium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule and lithium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule. Decorative sheet.

[0028] (2) At least one of the above compounds has a saturated fatty acid selected from the group consisting of behenic acid (C21H43COOH) and montanic acid (C27H55COOH). (3) The substrate is composed of two or more laminated layers, Among the multiple layers constituting the base material, the crystal nucleating agent is added to at least the outermost layer which is the layer farthest from the design layer. (4) The substrate further comprises a pigment.

[0029] (5) A substrate for a decorative sheet, The substrate is made of polyethylene terephthalate containing a crystal nucleating agent, and has a cold crystallization heat of 3 J / g or less; The crystal nucleating agent is composed of one or more compounds selected from the group consisting of sodium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule and lithium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule.

[0030] (6) A method for producing a decorative sheet having a design layer laminated on a substrate, comprising the steps of: A mixture of polyethylene terephthalate resin and a crystal nucleating agent is used as a raw material, and the resin is extruded in a molten state and in a sheet shape using a T-die extruder. The extruded molten resin is solidified while controlling the cooling rate using a metal temperature control roll, thereby producing the substrate. As the crystal nucleating agent, one or more compounds selected from sodium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule and lithium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule are used. (7) The cooling rate is adjusted so that the heat of cold crystallization of the base material is 3 J / g or less. EXAMPLES

[0031] Examples based on this embodiment will be described below, however, the present invention is not limited to the following examples. <Example 1> A mixture obtained by dry blending a pigment master batch (polyethylene terephthalate / titanium oxide=50 / 50 parts by mass) (40 parts by mass), PET resin pellets (60 parts by mass), and sodium montanate powder (chemical formula: C27H55COONa) (0.25 parts by mass) was used in Example 1. The mixture was extruded and formed into a film by a single-screw T-die extruder while controlling the temperature of the T-die to 280°C and the surface temperature of the temperature-regulating roll to 180°C, to produce a PET substrate (thickness 100 μm) of Example 1.

[0032] After corona treatment on both sides of the prepared PET substrate (after surface treatment), a wood grain pattern was gravure printed on the side that did not come into contact with the temperature control roll during the above extrusion film formation using a two-component urethane ink (V180; manufactured by Toyo Ink Co., Ltd.) to form a design layer. Hereinafter, this laminate of the PET substrate and the printing layer will be referred to as the printing substrate. Next, a polyolefin film (thickness 100 μm) was dry laminated onto the design layer side of the printed substrate as a transparent resin layer, and then a two-component cured polyurethane hard coat layer (thickness 8 μm) was applied and formed as a surface protective layer to produce the decorative sheet of Example 1.

[0033] <Example 2> A decorative sheet of Example 2 was produced in the same manner as in Example 1, except that the surface temperature of the temperature-regulating roll 12 of the T-die extruder of Example 1 was set to 170°C. <Example 3> A decorative sheet of Example 3 was produced in the same manner as in Example 1, except that the sodium montanate of Example 1 was replaced with lithium montanate (chemical formula: C27H55COOLi).

[0034] <Example 4> A decorative sheet of Example 4 was produced in the same manner as in Example 1, except that the sodium montanate of Example 1 was replaced with sodium behenate (chemical formula: C22H45COONa). <Example 5> A decorative sheet of Example 5 was produced in the same manner as in Example 1, except that the sodium montanate of Example 1 was replaced with sodium stearate (chemical formula: C17H35COONa).

[0035] <Example 6> A decorative sheet of Example 6 was produced in the same manner as in Example 1, except that the PET substrate of Example 1 was made into a two-layer structure by multilayer extrusion. The two-layer structure of the PET substrate in Example 6 is as follows. First layer (design layer on the side in contact with temperature control roll 12 and non-contact layer) The layer was made using the same mixture as in Example 1 and had a thickness of 90 μm. Second layer (layer in contact with the design layer on the non-contact side of the temperature control roll 12) The layer was made using only PET resin pellets and had a thickness of 10 μm. In addition, neither of the layers was subjected to a stretching process.

[0036] <Comparative Example 1> A decorative sheet of Comparative Example 1 was produced in the same manner as in Example 1, except that the sodium montanate in Example 1 was replaced with sodium palmitate (chemical formula: C15H31COONa). <Comparative Example 2> A decorative sheet of Comparative Example 2 was produced in the same manner as in Example 1, except that the surface temperature of the temperature-regulating roll 12 of the T-die extruder in Example 1 was set to 160°C.

[0037] <Comparative Example 3> A decorative sheet of Comparative Example 3 was produced in the same manner as in Example 1, except that the sodium montanate of Example 1 was replaced with zinc montanate (chemical formula: (C27H55COO)2Zn). <Comparative Example 4> A decorative sheet of Comparative Example 4 was produced in the same manner as in Example 1, except that the sodium montanate of Example 1 was replaced with sodium benzoate (chemical formula: (C6H5COONa).

[0038] <Comparative Example 5> A decorative sheet of Comparative Example 5 was produced in the same manner as in Example 1, except that the PET substrate of Example 1 was replaced with biaxially stretched white PET (Lumirror #100E20, thickness 100 μm, manufactured by Toray Industries, Inc.).

[0039] (evaluation) Table 1 shows the configuration conditions of each of the examples and comparative examples, and the evaluation results of the following evaluations. [Table 1]

[0040] <Cold crystallization heat> For each of the PET substrates 1 in each of the Examples and Comparative Examples, the heat of cold crystallization was measured by a differential scanning calorimeter (DSC) in accordance with JIS K7121 (measurement method for heat of transition of plastics). <Appearance of substrate> The appearance of each PET substrate in each of the Examples and Comparative Examples was evaluated visually. The criteria for judgment were as follows:

[0041] ○ (Pass): No wrinkles, cracks, particulate foreign matter, or other abnormalities were found. △(Pass): Slight wrinkles are observed, but no cracks or particulate foreign matter are observed. × (Fail): Any of wrinkles, cracks, or particulate foreign matter is found.

[0042] <Ink adhesion> For each of the printed substrates in each of the Examples and Comparative Examples, a grid-cut cell (1 mm square, 25 pieces) was peeled off with Cellophane Tape (registered trademark) in accordance with JIS K5600 (general coating test method). The appearance after peeling was visually confirmed and judged according to the following criteria. As mentioned above, the printed substrate refers to a laminate in which only a printed layer is formed on a PET substrate. The criteria for judgment were as follows: ○ (Pass): The edges of the cut are completely smooth and there is no peeling on any of the grid holes. △ (Pass): Small peeling is observed in some (5% or less) of the intersections of the cuts. × (Fail): Peeling occurs in one or more places inside the cut cell.

[0043] <Water vapor barrier properties> For each of the decorative sheets in each of the Examples and Comparative Examples, the moisture permeability was measured in accordance with JIS Z0208 (Test method for moisture permeability of moisture-proof packaging materials (cup method)). The criteria for judgment were as follows. The unit of moisture permeability is [g / m 2 / day]. ○(Pass): Less than 5 △ (Pass): 5 or more but less than 7 × (Fail): 7 or more

[0044] (Evaluation Results) As shown in Table 1, even if a crystal nucleating agent was blended into the PET substrate, as in Comparative Example 1 and Comparative Example 4, when the crystal nucleating agent was not a compound selected from among sodium salts or lithium salts of saturated fatty acids having 18 to 28 carbon atoms per molecule, the PET substrate 1 was not subjected to a stretching process, and therefore was not in a state that could be evaluated or had poor water vapor barrier properties. Furthermore, as in Comparative Examples 2 and 3, even if the crystal nucleating agent in the PET substrate 1 satisfied the conditions of the present invention, when the cold crystallization heat of the PET substrate exceeded 3 J / g, the water vapor barrier property deteriorated.

[0045] On the other hand, the decorative sheets of the examples formed based on the present invention were excellent in terms of substrate appearance, ink adhesion, and water vapor barrier properties. These examples also had better ink adhesion than the PET substrate of Comparative Example 5. In Example 6, the PET substrate has a two-layer structure. The first layer contains a crystal nucleating agent based on the present invention and has a cold crystallization heat of 3 J / g or less, thereby ensuring the water vapor barrier properties of the PET substrate. Furthermore, the second layer has a cold crystallization heat of 3 J / g or less, thereby ensuring the ink adhesion between the PET substrate and the design layer. In addition, although not described in the above example, it was confirmed that the substrate appearance, ink adhesion, and water vapor barrier properties were all good even for decorative sheets produced under the same conditions as in Example 1, except that the cooling rate of the resin was controlled to set the cold crystallization heat of the PET substrate to 3 J / g. [Explanation of symbols]

[0046] 1 PET base material 2 Design Layer 3 Transparent resin layer 4 Surface protective layer 10 Decorative Sheet 11 T-die extruder 11A T-die 12 Temperature control roll 13 Temperature controller 20 Resin in sheet form

Claims

1. A decorative sheet having a design layer laminated on a substrate, The substrate is made of polyethylene terephthalate containing a crystal nucleating agent and has a cold crystallization heat of 3 J / g or less; The crystal nucleating agent is composed of one or more compounds selected from a sodium salt of a saturated fatty acid having 18 to 28 carbon atoms per molecule and a lithium salt of a saturated fatty acid having 18 to 28 carbon atoms per molecule. Decorative sheet.

2. At least one of the above compounds is characterized in that the saturated fatty acid is behenic acid (C21H43COOH) or montanic acid (C27H55COOH). The decorative sheet according to claim 1.

3. The substrate is composed of two or more laminated layers, Among the layers constituting the base material, the crystal nucleating agent is added to at least the outermost layer which is the layer farthest from the design layer. A decorative sheet according to claim 1 or 2.

4. The substrate further comprises a pigment. The decorative sheet according to claim 1.

5. A substrate for a decorative sheet, The substrate is made of polyethylene terephthalate containing a crystal nucleating agent, and has a cold crystallization heat of 3 J / g or less; The crystal nucleating agent is composed of one or more compounds selected from a sodium salt of a saturated fatty acid having 18 to 28 carbon atoms per molecule and a lithium salt of a saturated fatty acid having 18 to 28 carbon atoms per molecule. Base material.

6. A method for producing a decorative sheet having a design layer laminated on a substrate, comprising the steps of: A mixture of polyethylene terephthalate resin and a crystal nucleating agent is used as a raw material, and the resin is extruded in a molten state and in a sheet shape using a T-die extruder. The extruded molten resin is solidified while controlling the cooling rate using a metal temperature control roll, thereby producing the substrate. As the crystal nucleating agent, one or more compounds selected from a sodium salt of a saturated fatty acid having 18 to 28 carbon atoms per molecule and a lithium salt of a saturated fatty acid having 18 to 28 carbon atoms per molecule are used. A method for producing a decorative sheet.

7. The cooling rate is adjusted so that the cold crystallization heat of the base material is 3 J / g or less. A method for producing the decorative sheet according to claim 6.