Thermoplastic mixture

A tailored thermoplastic mixture with specific components balances flow, viscosity, and crystallization for improved processing and strength in molded parts and hollow bodies, addressing existing challenges in thermoplastic formulations.

JP2024541451AInactive Publication Date: 2024-11-08BASF SE
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024529956
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-22
Filing Date
2022-11-11
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure 2024541451000001
    Figure 2024541451000001
  • Figure 2024541451000002
    Figure 2024541451000002
  • Figure 2024541451000003
    Figure 2024541451000003
Patent Text Reader

Abstract

A) 30 to 100% by weight of a thermoplastic blend comprising: A-1) 65 to 75% by mass of polyester; A-2) 5 to 25% by mass of HD- or LD-polyethylene; A-3) 3 to 10% by mass of an ionomer, 3-1) 30 to 99% by mass ethylene 3-2) 0 to 60 mass% of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene, and 3-3) 0.01 to 50% by weight of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides and carboxylic esters, with the proviso that the proportion of carboxylic acids is 30 to 100% by weight, the proportion of carboxylic anhydrides and / or carboxylic esters is complementarily 0 to 70% by weight, and the hydrogen of the carboxyl group of the carboxylic acid is replaced by a metal selected from the group consisting of sodium, potassium and zinc in a proportion of at least 20% ("mol %) of the total number of carboxyl groups. wherein the sum of the proportions of components 3-1, 3-2 and 3-3 equals 100% by weight; The ionomer, A-4) 0.5 to 5% by weight of an epoxidized oil or oil mixture, wherein at least partially unsaturated fatty acids in the fatty acid esters on which the oil or oil mixture is based have 12 to 22 carbon atoms. wherein the sum of the proportions of components A-1, A-2, A-3 and A-4 is 100% by weight of component A); said thermoplastic blend, B) 0 to 70% by weight of further additives wherein the sum of the proportions of components A) and B) amounts to 100% by weight.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to A) 30 to 100% by weight of a thermoplastic blend comprising: A-1) 65 to 75% by mass of polyester; A-2) 5 to 25% by mass of HD- or LD-polyethylene; A-3) 3 to 10% by mass of an ionomer, 3-1) 30 to 99% by mass ethylene 3-2) 0 to 60 mass% of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene, and 3-3) 0.01 to 50% by weight of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides and carboxylic esters, with the proviso that the proportion of carboxylic acids is 30 to 100% by weight, the proportion of carboxylic anhydrides and / or carboxylic esters is complementarily 0 to 70% by weight, and the hydrogen of the carboxyl group of the carboxylic acid is replaced by a metal selected from the group consisting of sodium, potassium and zinc in a proportion of at least 20% ("mol %) of the total number of carboxyl groups. wherein the sum of the proportions of components 3-1, 3-2 and 3-3 equals 100% by weight; A-4) 0.5 to 5% by weight of an epoxidized oil or oil mixture, wherein at least partially unsaturated fatty acids in the fatty acid esters on which the oil or oil mixture is based have 12 to 22 carbon atoms. wherein the sum of the proportions of components A-1, A-2, A-3 and A-4 is 100% by weight of component A); said thermoplastic blend, B) 0 to 70% by weight of further additives wherein the sum of the proportions of components A) and B) amounts to 100% by weight.

[0002] The invention furthermore relates to molded parts and hollow bodies produced using said thermoplastic mixture, in particular to hollow bodies produced using said thermoplastic mixture by means of a blow molding process. [Background technology]

[0003] To produce hollow bodies and moldings from thermoplastics, mixtures containing thermoplastics, such as PET or PBT, are usually used. In order for these mixtures to meet the requirements of the respective molding process, they must have, among other things, specific rheological properties. Here, the balance between strength and viscosity on the one hand and sufficient flowability to fill the mold as well as possible on the other hand is important.

[0004] In the publications M.Joshi et al., Journal of Applied Polymer Science, Vol.43, 311-328, 1991 ("D1"), M.Joshi et al., Journal of Applied Polymer Science, Vol. 45, 1837-1847 1992 ("D2"), and M.Joshi et al., POLYMER Volume 35, Number 17, 3679-3685, 1994 ("D3"), blends from PBT and HDPE and the effect of ionomers on the miscibility of both plastics have been investigated. When PBT and HDPE alone form two-phase mixtures, the addition of ionomers (ethylene-methacrylic acid copolymers in which the acid hydrogens are partially replaced by sodium) results in an improved compatibility of the rather polar PBT with the non-polar HDPE, together with exotic properties of the ternary mixtures. As the degree of dispersion of HDPE in PBT increases, the crystallization rate of PBT increases with increasing proportion of ionomer, and as a whole the three phases of HDPE, PBT and ionomer can be seen as a homogeneous alloy phase.

[0005] In WO 1990 / 14391 A1 ("D4"), mixtures are claimed that consist of (i) a polyester, (ii-i) either a sodium or potassium salt of a carboxylic acid having 7 to 25 carbon atoms, or (ii-ii) a sodium or potassium salt of an ionic copolymer of an α-olefin containing 2 to 5 carbon atoms and an α,β-ethylenically unsaturated carboxylic acid containing 3 to 5 carbon atoms, and (iii) a polyolefin having a weight average molecular weight of 1,000 to 20,000. According to D4, these mixtures are characterized by increased impact resistance.

[0006] The older European Patent Application Publication No. 20190021.4 (20190021.4) ("D5") claims thermoplastic formulations containing polyesters, HD- or LD-polyethylenes, ionomers consisting of at least one copolymer of ethylene and a compound selected from the group of 1-octene, 1-butene and propylene with a functional monomer from the group of carboxylic acids, carboxylic anhydrides and carboxylic esters, and optionally further additives.

[0007] However, the incorporation of epoxidized oils or oil mixtures is not described in the aforementioned prior art. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 1990 / 14391 [Patent Document 2] European Patent Application Publication No. 20190021.4 [Non-patent literature]

[0009] [Non-Patent Document 1] M. Joshi et al., Journal of Applied Polymer Science, Vol.43, 311-328, 1991 [Non-Patent Document 2] M. Joshi et al., Journal of Applied Polymer Science, Vol. 45, 1837~1847 1992 [Non-Patent Document 3] M. Joshi et al., POLYMER Volume 35, Number 17, 3679~3685, 1994 Summary of the Invention [Problem to be solved by the invention]

[0010] The object of the present invention was to provide thermoplastic mixtures which are suitable for producing hollow bodies and moldings and whose composition allows the adjustment of a tailored balance for processing between flowability, viscosity and crystallization rate on the one hand, and on the other hand provides the required strength and impact resistance for the finished hollow bodies and moldings. [Means for solving the problem]

[0011] Accordingly, the thermoplastic mixture defined at the outset has been found. Preferred embodiments are set out in the dependent claims.

[0012] As component A, the thermoplastic mixture according to the invention comprises A) 30 to 100% by weight of a thermoplastic blend comprising: A-1) 65 to 75% by mass of polyester; A-2) 5 to 25% by mass of HD- or LD-polyethylene; A-3) 3 to 10% by mass of an ionomer, 3-1) 30 to 99% by mass ethylene 3-2) 0 to 60 mass% of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene, and 3-3) 0.01 to 50% by weight of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides and carboxylic esters, with the proviso that the proportion of carboxylic acids is 30 to 100% by weight, the proportion of carboxylic anhydrides and / or carboxylic esters is complementarily 0 to 70% by weight, and the hydrogen of the carboxyl group of the carboxylic acid is replaced by a metal selected from the group consisting of sodium, potassium and zinc in a proportion of at least 20% ("mol %) of the total number of carboxyl groups. wherein the sum of the proportions of components 3-1, 3-2 and 3-3 equals 100% by weight; A-4) 0.5 to 5% by weight of an epoxidized oil or oil mixture, wherein at least partially unsaturated fatty acids in the fatty acid esters on which the oil or oil mixture is based have 12 to 22 carbon atoms. wherein the sum of the proportions of components A-1, A-2, A-3 and A-4 is 100% by weight of component A); It contains 30 to 100 mass % of a thermoplastic compound.

[0013] To total 100% by weight, the thermoplastic mixture contains still further additives as component B in a proportion of 0 to 70% by weight.

[0014] A preferred thermoplastic mixture contains 68 to 73% by weight of component A-1, 18 to 22% by weight of component A-2, 5 to 10% by weight of component A-3 and 2 to 5% by weight of component A-4.

[0015] It is noted here that typically, specific polyester, specific HD- or LD-polyethylene, or specific ionomer starting materials are used as components A-1, A-2, and A-3. However, mixtures of such polyester, HD- or LD-polyethylene, or ionomer starting materials, respectively, may also be used. It is further noted that the specific polyester, HD- or LD-polyethylene, or ionomer starting materials themselves are essentially mixtures of the respective polyester, HD- or LD-polyethylene, or ionomer starting materials, based on the molecular weight distribution resulting from their manufacture (but which is well known to those skilled in the art).

[0016] Generally, polyesters A-1 based on aromatic dicarboxylic acids and aliphatic or aromatic dihydroxy compounds are used.

[0017] Preferred dicarboxylic acids include 2,6-naphthalenedicarboxylic acid, terephthalic acid and isophthalic acid or mixtures thereof. Up to 60 mol %, advantageously up to 10 mol %, of the aromatic dicarboxylic acids may be replaced by aliphatic or cycloaliphatic dicarboxylic acids, such as adipic acid, azelaic acid, sebacic acid, dodecanedioic acid and cyclohexanedicarboxylic acid.

[0018] Among the aliphatic dihydroxy compounds, diols having 2 to 6 carbon atoms are preferred, in particular 1,2-ethanediol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,4-hexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol and neopentyl glycol or mixtures thereof.

[0019] A first group of preferred polyesters A-1 are polyalkylene terephthalates, especially those having 2 to 10 carbon atoms in the alcohol moiety.

[0020] Such polyalkylene terephthalates are known per se and described in the literature. They contain aromatic rings in the main chain which are derived from aromatic dicarboxylic acids. The aromatic rings may be substituted, for example, by halogens, such as chlorine and bromine, or by C1-C4-alkyl groups, such as methyl, ethyl, i-propyl or n-propyl, and n-butyl, i-butyl or t-butyl groups.

[0021] These polyalkylene terephthalates can be prepared in a manner known per se by reacting aromatic dicarboxylic acids, their esters or other ester-forming derivatives with aliphatic dihydroxy compounds.

[0022] Particularly preferred polyesters A-1 include polyalkylene terephthalates derived from alkanediols having 2 to 6 carbon atoms. Among these, in particular polyethylene terephthalate, polypropylene terephthalate and polybutylene terephthalate or mixtures thereof are preferred. Further preferred are PET and / or PBT containing up to 1% by weight, preferably up to 0.75% by weight, of 1,6-hexanediol and / or 2-methyl-1,5-pentanediol as further monomer units.

[0023] The viscosity number ("VZ") of polyester A-1 is generally in the range of 50 to 220, preferably at least 140 ml / g, in particular at least 145 ml / g (measured in a 0.5% by weight solution in a phenol / o-dichlorobenzene mixture (1:1 by weight at 25°C) according to ISO 1628).

[0024] Particularly preferred are polyesters having a carboxyl end group content of 0 to 100 mmol / kg, preferably 10 to 50 mmol / kg and in particular 15 to 40 mmol / kg per kg of polyester. Such polyesters can be prepared, for example, by the method of DE-A 44 01 055. The carboxyl end group content is usually determined by titration methods (for example potentiometric titration).

[0025] Particularly preferred thermoplastic mixtures contain as component A-1 a mixture of polyesters, at least one of which is PBT, for example the proportion of polyethylene terephthalate in the mixture is preferably up to 50% by weight, in particular from 10 to 35% by weight, based on 100% by weight of A).

[0026] Additionally, recycled PET material (also called scrap PET) may also be used, possibly mixed with polyalkylene terephthalates such as PBT.

[0027] By recycled materials, the following is generally understood: 1) So-called "recycled materials from industry": These are production waste from polycondensation or processing, for example sprues from injection moulding processes, starting waste from injection moulding processes or extrusion, or edge fragments of extruded plates or films.

[0028] 2) So-called "post-consumer recycled materials": These are plastic articles that have been collected and recycled after their final use. The most widespread articles in terms of quantity are blown-molded PET bottles for mineral water, soft drinks and juices.

[0029] Both types of recycle material can be present as ground material or in the form of granules, in the latter case the crude recycle material is melted and granulated in an extruder after separation and washing, which often facilitates handling, flowability and dosing for further processing steps.

[0030] Both granulated and ground recycled materials can be used, where the maximum side length should be less than 10 mm, preferably less than 8 mm.

[0031] Due to the hydrolytic degradation of polyester during processing (due to traces of moisture), it is recommended to dry the recycled material beforehand. After drying, the residual moisture content should be less than 0.2%, in particular less than 0.05%.

[0032] A further group can include fully aromatic polyesters derived from aromatic dicarboxylic acids and aromatic dihydroxy compounds.

[0033] Suitable aromatic dicarboxylic acids are the compounds already described for the polyalkylene terephthalates. Preferably, mixtures of 5-100 mol % isophthalic acid and 0-100 mol % terephthalic acid, in particular mixtures of about 80 % terephthalic acid and 20 % isophthalic acid to mixtures of approximately equal amounts of these two acids, are used.

[0034] The aromatic dihydroxy compound advantageously has the general formula: [ka] [wherein Z represents an alkylene or cycloalkylene group having up to 8 carbon atoms, an arylene group having up to 12 carbon atoms, a carbonyl group, a sulfonyl group, an oxygen atom, a sulfur atom or a chemical bond, and m has a value from 0 to 2.] The compounds may also have C1-C6-alkyl or alkoxy groups and fluorine, chlorine or bromine as substituents on the phenylene group.

[0035] The parent structures of these compounds include, for example: Dihydroxydiphenyl, di-(hydroxyphenyl)alkanes, di-(hydroxyphenyl)cycloalkanes, di-(hydroxyphenyl)sulfide, di-(hydroxyphenyl) ether, Di-(hydroxyphenyl)ketone, di-(hydroxyphenyl)sulfoxide, α,α'-di-(hydroxyphenyl)-dialkylbenzenes, Di-(hydroxyphenyl)sulfone, di-(hydroxybenzoyl)benzene Resorcin, and Included are hydroquinones, as well as their nuclear alkylated or nuclear halogenated derivatives.

[0036] Among these, 4,4'-dihydroxydiphenyl, 2,4-di-(4'-hydroxyphenyl)-2-methylbutane, α,α'-di-(4-hydroxyphenyl)-p-diisopropylbenzene, 2,2-di-(3'-methyl-4'-hydroxyphenyl)propane, and 2,2-di-(3'-chloro-4'-hydroxyphenyl)propane, And in particular, 2,2-Di-(4'-hydroxyphenyl)propane 2,2-di-(3',5-dichlorodihydroxyphenyl)propane, 1,1-di-(4'-hydroxyphenyl)cyclohexane, 3,4'-dihydroxybenzophenone, 4,4'-dihydroxydiphenyl sulfone, and 2,2-di(3',5'-dimethyl-4'-hydroxyphenyl)propane, Or a mixture thereof is preferred.

[0037] Of course, mixtures of polyalkylene terephthalates and fully aromatic polyesters can also be used, which generally contain 20 to 98% by weight of polyalkylene terephthalate and 2 to 80% by weight of fully aromatic polyester.

[0038] Of course, polyester block copolymers, such as copolyetheresters, can also be used. Such products are known per se and are described in the literature, for example in US Pat. No. 3,651,014 (US-A 3,651,014). Corresponding products are also commercially available, for example Hytrel® (DuPont).

[0039] According to the invention, polyesters are also to be understood as halogen-free polycarbonates. Suitable halogen-free polycarbonates are, for example, those of the general formula [ka] [In the formula, Q is a single bond, a C1-C8 alkylene group, a C2-C3 alkylidene group, a C3-C6 cycloalkylidene group, a C6-C 12 -arylene group, -O-, -S- or -SO2-, and m is an integer of 0 to 2. It is based on diphenols.

[0040] The diphenols can carry substituents on the phenylene group, for example C1-C6-alkyl or C1-C6-alkoxy.

[0041] Preferred diphenols of the above formula are, for example, hydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, 2,2-bis-(4-hydroxyphenyl)-propane, 2,4-bis-(4-hydroxyphenyl)-2-methylbutane, 1,1-bis-(4-hydroxyphenyl)-cyclohexane. 2,2-bis-(4-hydroxyphenyl)-propane and 1,1-bis-(4-hydroxyphenyl)-cyclohexane, as well as 1,1-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, are particularly preferred.

[0042] Both homopolycarbonates and copolycarbonates are suitable as component A, and in addition to bisphenol A homopolymers, copolycarbonates of bisphenol A are preferred.

[0043] Suitable polycarbonates can be branched in a known manner, particularly advantageously by incorporating 0.05 to 2.0 mol %, relative to the sum of the diphenols used, of at least trifunctional compounds, for example those having three or more phenolic OH groups.

[0044] Relative viscosity η of 1.10 to 1.50, especially 1.25 to 1.40 rel It has been found that polycarbonates having an average molecular weight M w This corresponds to (weight average) 10 000 to 200 000 g / mol, advantageously 20 000 to 80 000 g / mol.

[0045] The diphenols of the above general formula are known per se or can be prepared by known methods.

[0046] The preparation of polycarbonates can be carried out, for example, by reacting diphenols with phosgene by the interfacial process or by reacting them with phosgene in a homogeneous phase (the so-called pyridine process), where the molecular weight to be adjusted in each case is achieved in a known manner by the corresponding amounts of known chain terminators (for polydiorganosiloxane-containing polycarbonates, see, for example, DE-OS 33 34 782).

[0047] Suitable chain terminators are, for example, phenol, pt-butylphenol, but also longer-chain alkylphenols, such as 4-(1,3-tetramethylbutyl)-phenol (according to DE-OS 28 42 005), or mono- or dialkylphenols having a total of 8 to 20 carbon atoms in the alkyl substituents (according to DE-A 35 06 472), such as p-nonylphenyl, 3,5-di-t-butylphenol, pt-octylphenol, p-dodecylphenol, 2-(3,5-dimethyl-heptyl)-phenol and 4-(3,5-dimethylheptyl)-phenol.

[0048] Halogen-free polycarbonate means in the present invention that the polycarbonate is composed of halogen-free diphenols, halogen-free chain terminators and optionally halogen-free branching agents, where the incidental ppm content of saponifiable chlorine resulting from, for example, the preparation of polycarbonate by the interfacial process with phosgene is not to be considered as halogen-containing in the present invention.Such polycarbonates with ppm content of saponifiable chlorine are halogen-free polycarbonates in the present invention.

[0049] Further suitable components A) include amorphous polyester carbonates, in which phosgene is replaced by aromatic dicarboxylic acid units, such as isophthalic acid units and / or terephthalic acid units, during the preparation. Further details are taught in the corresponding places in EP A 365 916 A1.

[0050] Further suitable copolycarbonates which contain cycloalkyl groups as monomer units are described in EP A 365 916.

[0051] As component A-3, the thermoplastic mixture according to the invention comprises 10 to 25% by mass of an ionomer, 3-1) 30 to 99% by mass ethylene 3-2) 0 to 60 mass% of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene, and 3-3) 0.01 to 50% by weight of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides and carboxylic esters, with the proviso that the proportion of carboxylic acids is 30 to 100% by weight, the proportion of carboxylic anhydrides and / or carboxylic esters is complementarily 0 to 70% by weight, and the hydrogen of the carboxyl group of the carboxylic acid is replaced by a metal selected from the group consisting of sodium, potassium and zinc in a proportion of at least 20% ("mol %) of the total number of carboxyl groups. wherein the sum of the proportions of components 3-1, 3-2 and 3-3 equals 100% by weight; The ionomer is contained.

[0052] Preferred metal ions are sodium, potassium or zinc, especially sodium or potassium, or mixtures thereof. The use of sodium is particularly preferred. The percent neutralization is determined, for example, by flame atomic absorption spectrometry using commercially available equipment.

[0053] By ionomers is understood, for example according to Roempp Online Lexikon, Georg Thieme Verlag, August 2008, ionic polymers which contain a large proportion of hydrophobic monomers and often a small proportion of comonomers carrying ionic groups.

[0054] Examples of possible ionomers of component A-3 are also described in EP 0 419 274.

[0055] These ionomers can be obtained by direct copolymerization and converted to salts by subsequent reaction (eg with an alkali solution to produce an alkali-containing ionomer).

[0056] Preferred component 3-3 is selected from the group consisting of ethylenically unsaturated monocarboxylic acids, dicarboxylic acids and functional derivatives of these acids.

[0057] Such preferred components 3-3 are in particular selected from the group consisting of acrylic acid, methacrylic acid, maleic acid, fumaric acid, maleic anhydride, acrylic acid esters and methacrylic acid esters each having 1 to 18 carbon atoms in the alcohol moiety of the ester.

[0058] Essentially all C1-C primary, secondary and tertiary acrylic or methacrylic acids 18 -Alkyl esters are suitable, with esters having 1 to 12 carbon atoms, especially 2 to 10 carbon atoms, being preferred.

[0059] Examples of this are methyl-, ethyl-, propyl-, n-, i-butyl- and t-butyl-, 2-ethylhexyl-, octyl- and decyl acrylates and the corresponding esters of methacrylic acid, of which particular emphasis is placed on n-butyl acrylate and 2-ethylhexyl acrylate.

[0060] Instead of or in addition to the esters, potentially acid-functional monomers of ethylenically unsaturated mono- or dicarboxylic acids may be included in the olefin polymer. Examples of this include, as monomers of component 3-3, tertiary alkyl esters of acrylic acid, methacrylic acid, especially tert-butyl acrylate, tert-butyl methacrylate, or dicarboxylic acid derivatives, such as monoesters of maleic acid and fumaric acid, or derivatives of these acids.

[0061] Latently acid-functional monomers are to be understood as those compounds which form free acid groups under the polymerization conditions and / or when the olefin polymer is added to the molding composition.

[0062] Preferably, component A-3 is 3-1) 50-99% by mass ethylene 3-2) 0 to 50 mass% of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene, and 3-3) 0.05 to 50 mass% of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides, and carboxylic esters. Contains:

[0063] More preferably, component A-3 is 3-1) 50-90% by mass ethylene 3-2) 0 to 50 mass% of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene, and 3-3) 2 to 50 mass % of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides, and carboxylic esters. Contains:

[0064] The abovementioned ethylene copolymers can be prepared by methods known per se, preferably by random copolymerization under high pressure and elevated temperature.

[0065] The melt index of ethylene copolymers generally ranges from 1 to 80 g / 10 min (measured at 190° C. and a load of 2.16 kg).

[0066] The molecular weight of the ethylene-α-olefin copolymer is between 10,000 and 500,000 g / mol, preferably between 15,000 and 400,000 g / mol (Mn determined by GPC in 1,2,4-trichlorobenzene with polystyrene calibration).

[0067] In a particular embodiment, ethylene-α-olefin copolymers produced using so-called single-site catalysts are used. Further details can be obtained from US 5,272,236. In this case, the ethylene-α-olefin copolymer has a narrow molecular weight distribution of less than 4, preferably less than 3.5 for polyolefins.

[0068] As component A-4, the thermoplastic mixture according to the invention contains an epoxidized oil or oil mixture, in which the at least partially unsaturated fatty acid in the fatty acid ester on which said oil or oil mixture is based has 12 to 22 carbon atoms. Such oils as starting materials for epoxidation may be of petrochemical, vegetable or animal origin, may be present in pure form or mixed with one another and may be added accordingly to the thermoplastic mixture as pure epoxidized oil or as a mixture of such epoxidized oils.

[0069] US-Schrift 9,034,965 B2 describes in column 2, line 33 to column 3, line 12 various oils and mixtures thereof that can be subjected to epoxidation. Such epoxidized oils and oil mixtures can also be used according to the present invention.

[0070] Advantageously, epoxidized oils based on vegetable oils selected from the group consisting of soybean oil, linseed oil, rapeseed oil, castor oil, camelina oil, cottonseed oil, olive oil, peanut oil, sunflower oil, corn oil and hempseed oil are used.

[0071] In particular, epoxidized oils based on vegetable oils selected from the group consisting of soybean oil, linseed oil, rapeseed oil and castor oil come into consideration.

[0072] As component B, the molding materials according to the invention can contain from 0 to 70% by weight, in particular up to 50% by weight, of further additives and processing auxiliaries which are different from component A, based on 100% by weight of the sum of components A and B.

[0073] A typical component B is, for example, an elastomeric polymer (often also called impact modifier, elastomer or rubber) in an amount of up to 40% by weight, preferably up to 15% by weight.

[0074] Examples of impact modifiers are rubbers that may have functional groups. Mixtures of two or more different impact modifying rubbers may also be used.

[0075] The rubber which increases the viscosity of the molding material generally contains an elastomeric portion having a glass transition temperature of less than -10°C, advantageously less than -30°C, which contains at least one functional group capable of reacting with the polyamide. Suitable functional groups are, for example, carboxylic acid groups, carboxylic anhydride groups, carboxylic ester groups, carboxylic amide groups, carboxylic imide groups, amino groups, hydroxy groups, epoxide groups, urethane groups or oxazoline groups, preferably carboxylic anhydride groups.

[0076] Preferred functionalized rubbers include functionalized polyolefin rubbers comprised of the following components: 1. 40 to 99% by weight of at least one α-olefin having 2 to 8 carbon atoms; 2. 0 to 50% by mass of a diene; 3. 0 to 45% by mass of C1 to C2 of acrylic acid or methacrylic acid 12- an alkyl ester, or a mixture of such esters, 4. 0 to 40% by mass of ethylenically unsaturated C2 to C 20 mono- or dicarboxylic acids or functional derivatives of such acids, 5. 0 to 40% by mass of an epoxy group-containing monomer, and 6. 0 to 5 mass % of other radical polymerizable monomers, Here, the total amount of components 3) to 5) is at least 1 to 45% by mass based on components 1) to 6).

[0077] Examples of suitable α-olefins include ethylene, propylene, 1-butylene, 1-pentylene, 1-hexylene, 1-heptylene, 1-octylene, 2-methylpropylene, 3-methyl-1-butylene and 3-ethyl-1-butylene, with ethylene and propylene being preferred.

[0078] Suitable diene monomers include, for example, conjugated dienes having 4 to 8 carbon atoms, such as isoprene and butadiene, non-conjugated dienes having 5 to 25 C atoms, such as penta-1,4-diene, hexa-1,4-diene, hexa-1,5-diene, 2,5-dimethylhexa-1,5-diene and octa-1,4-diene, cyclic dienes, such as cyclopentadiene, cyclohexadiene, cyclooctadiene and dicyclopentadiene, as well as alkenylnorbornenes, such as 5-ethylidene-2-norbornene, 5-butylidene-2-norbornene, 2-methallyl-5-norbornene, 2-isoprenyl-5-norbornene and tricyclodienes, such as 3-methyltricyclo(5.2.1.0.2.6)-3,8-decadiene or mixtures thereof. Hexa-1,5-diene, 5-ethylidene-norbornene and dicyclopentadiene are preferred.

[0079] The diene content is preferably 0.5 to 50, in particular 2 to 20, and particularly preferably 3 to 15% by weight, based on the total weight of the olefin polymer. Examples of suitable esters are methyl-, ethyl-, propyl-, n-butyl-, i-butyl- and 2-ethylhexyl-, octyl- and decyl acrylate or the corresponding esters of methacrylic acid. Of these, methyl-, ethyl-, propyl-, n-butyl- and 2-ethylhexyl acrylate or methacrylate are particularly preferred. Instead of or in addition to the esters, acid-functional and / or potentially acid-functional monomers of ethylenically unsaturated mono- or dicarboxylic acids may also be contained in the olefin polymer.

[0080] Examples of ethylenically unsaturated mono- or dicarboxylic acids are acrylic acid, methacrylic acid, the tertiary alkyl esters of these acids, in particular tert-butyl acrylate, and dicarboxylic acids, such as maleic acid and fumaric acid, or derivatives of these acids and their monoesters.

[0081] Potentially acid-functional monomers are to be understood as compounds which form free acid groups under the polymerization conditions or when the olefin polymer is added to the molding material. Examples of these include anhydrides of dicarboxylic acids having 2 to 20 carbon atoms, in particular maleic anhydride and the tertiary C1-C anhydrides of the aforementioned acids. 12 -alkyl esters, in particular tert-butyl acrylate and tert-butyl methacrylate.

[0082] Other monomers which come into consideration are, for example, vinyl esters and vinyl ethers.

[0083] Particularly preferred are olefin polymers from 50 to 98.9, in particular 60 to 94.85, % by weight of ethylene and 1 to 50, in particular 5 to 40, % by weight of esters of acrylic or methacrylic acid, 0.1 to 20.0, in particular 0.15 to 15, % by weight of glycidyl acrylate and / or glycidyl methacrylate, acrylic acid and / or methacrylic anhydride.

[0084] Particularly suitable functionalized rubbers are ethylene-methyl methacrylate-glycidyl methacrylate polymers, ethylene-methyl acrylate-glycidyl methacrylate polymers, ethylene-methyl acrylate-glycidyl acrylate polymers and ethylene-methyl methacrylate-glycidyl acrylate polymers.

[0085] The aforementioned polymers can be prepared by methods known per se, preferably by random copolymerization under high pressure and elevated temperature. The melt index of these copolymers is generally in the range of 1 to 80 g / 10 min (measured at 190° C. and a load of 2.16 kg).

[0086] A further group of suitable rubbers includes core-shell graft rubbers. These are graft rubbers made in emulsion, consisting of at least one hard component and at least one soft component. By hard component is usually understood a polymer having a glass transition temperature of at least 25 ° C, and by soft component is understood a polymer having a glass transition temperature of up to 0 ° C. These products have a structure consisting of one core and at least one shell, which structure is brought about by the order of addition of the monomers. The soft component is generally derived from butadiene, isoprene, alkyl acrylates, alkyl methacrylates or siloxanes, and optionally further comonomers. Suitable siloxane cores can be made, for example, starting from cyclic oligomeric octamethyltetrasiloxane or tetravinyltetramethyltetrasiloxane. These can be reacted, for example, in a ring-opening cationic polymerization, advantageously in the presence of sulfonic acid, with γ-mercaptopropylmethyldimethoxysilane to give soft siloxane cores. Siloxanes can also be crosslinked, for example, by carrying out a polymerization reaction in the presence of silanes having hydrolyzable groups, such as halogen or alkoxy groups, such as tetraethoxysilane, methyltrimethoxysilane or phenyltrimethoxysilane. Suitable comonomers include, for example, styrene, acrylonitrile, and crosslinking or grafting active monomers having more than one polymerizable double bond, such as diallyl phthalate, divinylbenzene, butanediol diacrylate or triallyl (iso)cyanurate. Hard components are generally derived from styrene, α-methylstyrene and their copolymers, where comonomers preferably include acrylonitrile, methacrylonitrile and methyl methacrylate.

[0087] Preferred core-shell graft rubbers contain a soft core and a hard shell, or a hard core, a first soft shell and at least one further hard shell. The incorporation of functional groups, such as carbonyl, carboxylic, anhydride, amide, imide, carboxylic ester, amino, hydroxyl, epoxy, oxazoline, urethane, urea, lactam or halogen benzyl groups, is advantageously carried out here by adding suitable functionalizing monomers during the polymerization of the last shell. Suitable functionalizing monomers are, for example, maleic acid, maleic anhydride, mono- or diesters of maleic acid, tertiary butyl-(meth)acrylate, acrylic acid, glycidyl (meth)acrylate and vinyloxazoline. The proportion of monomers with functional groups is generally 0.1 to 25% by weight, preferably 0.25 to 15% by weight, based on the total weight of the core-shell graft rubber. The mass ratio of the soft component to the hard component is generally 1:9 to 9:1, preferably 3:7 to 8:2.

[0088] Such rubbers are known per se and are described, for example, in EP 0 208 187. The incorporation of oxazine groups for functionalization can be carried out, for example, according to EP 0 791 606.

[0089] A further group of suitable impact modifiers are thermoplastic polyester elastomers.By polyester elastomers, we mean segmented copolyetheresters, which usually contain long-chain segments derived from poly(alkylene) ether glycols and short-chain segments derived from low molecular weight diols and dicarboxylic acids.Such products are known per se and are described in the literature, for example in US 3,651,014.Corresponding products are also commercially available under the names Hytrel (Du Pont), Arnitel (Akzo) and Pelprene (Toyobo Co. Ltd.).

[0090] Of course, mixtures of different rubbers may also be used.

[0091] Fibrous or particulate fillers, such as glass fibres, glass spheres, amorphous silica, calcium silicate, calcium metasilicate, magnesium carbonate, kaolin, chalk, powdered quartz, mica, barium sulfate and feldspar, can be added as additives to component B. Based on the overall mixture of the thermoplastic mixture, fibrous fillers B are used in amounts of up to 60% by weight, in particular up to 35% by weight, and particulate fillers are used in amounts of up to 30% by weight, in particular up to 10% by weight.

[0092] Preferred fibrous fillers include aramid and potassium titanate fibers, with glass fibers as E-glass being particularly preferred. These may be used in commercially available forms as rovings or chopped glass.

[0093] Further possible fillers are laser-absorbing materials, such as carbon fibers, carbon black, graphite, graphene or carbon nanotubes, which are preferably used in amounts of less than 1% by weight, particularly preferably less than 0.05% by weight, in certain cases.

[0094] To make the fibrous filler more compatible with the thermoplastic resin, it can be surface pretreated with a silane compound. Suitable silane compounds are of the general formula: (X-(CH2) n ) k -Si-(OC m H 2m+1 ) 4-k In the above formula, the substituents have the following meanings: X is [ka] and n is an integer from 2 to 10, preferably from 3 to 4; m is an integer from 1 to 5, preferably from 1 to 2; k is an integer of 1 to 3, preferably 1.

[0095] Preferred silane compounds are aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane, aminobutyltriethoxysilane and the corresponding silanes which contain a glycidyl group as the substituent X.

[0096] The silane compounds are generally used for the surface coating in amounts of 0.05 to 5% by weight, preferably 0.1 to 1.5% by weight and in particular 0.2 to 0.5% by weight (based on component B).

[0097] Acicular mineral fillers are also suitable.

[0098] By acicular mineral filler, in the sense of the present invention, is understood a mineral filler that has a very pronounced acicular character.An example is acicular wollastonite.Advantageously, the mineral has an L / D (length to diameter) ratio of 8:1 to 35:1, preferably 8:1 to 11:1.The mineral filler can be optionally pretreated with the above-mentioned silane compound, but pretreatment is not necessary.

[0099] The thermoplastic mixtures according to the invention may contain, as component B, customary processing aids, such as stabilizers, oxidation retardants, thermal decomposition inhibitors, UV decomposition inhibitors, lubricants and release agents, nucleating agents, such as sodium phenylphosphinate, aluminum oxide, silicon dioxide, nylon 22, and colorants, such as dyes and pigments or plasticizers.

[0100] As a preferred nucleating agent B, the thermoplastic mixture according to the invention contains 0 to 5% by weight of talc, which, if used, is preferably used in an amount of 0.001 to 4, in particular 0.01 to 1% by weight.

[0101] Talc is a hydrolyzed magnesium silicate in which additional trace elements such as Mn, Ti, Cr, Ni, Na, and K may be present and the OH groups may be replaced with fluoride.

[0102] It is particularly preferred to use talc in which the particle size of up to 100% is less than 20 μm. The particle size distribution is usually determined by sedimentation analysis and is advantageously <20 μm: 100% by weight, <10 μm: 99% by weight, <5 μm: 85% by weight, <3 μm: 60% by weight, <2 μm: 43% by weight. Such products are commercially available as Micro-Talc ITextra.

[0103] Examples of oxidation retarders and heat stabilizers include sterically hindered phenols and / or phosphites, hydroquinones, aromatic secondary amines such as diphenylamine, various substituted alternatives of the aforementioned groups and mixtures thereof, in concentrations of up to 1% by weight, based on the weight of the thermoplastic molding material.

[0104] UV stabilizers, which are generally used in amounts of up to 2% by weight based on the molding material, include various substituted resorcinols, salicylates, benzotriazoles and benzophenones.

[0105] Inorganic and organic pigments, as well as dyes, such as nigrosine and anthraquinone, can be added as colorants. Particularly suitable colorants are listed, for example, in EP1722984 B1, EP1353986 B1 or DE10054859 A1.

[0106] As additives of component B ("lubricants, glidants and release agents"), the thermoplastic mixtures according to the invention can contain esters or amides of saturated or unsaturated aliphatic carboxylic acids having 10 to 40, preferably 16 to 22, carbon atoms and of aliphatic saturated alcohols or amines having 2 to 40, advantageously 2 to 6, carbon atoms.

[0107] The carboxylic acids may be mono- or difunctional. Examples include pelargonic acid, palmitic acid, lauric acid, margaric acid, dodecanedioic acid, behenic acid and, particularly preferably, stearic acid, capric acid and montanic acid (a mixture of fatty acids having 30 to 40 carbon atoms).

[0108] The fatty alcohols may be monohydric to tetrahydric. Examples for the alcohols are n-butanol, n-octanol, stearyl alcohol, ethylene glycol, propylene glycol, neopentyl glycol, pentaerythritol, where glycerin and pentaerythritol are preferred.

[0109] The fatty amines may be mono- to trifunctional. Examples thereof are stearylamine, ethylenediamine, propylenediamine, hexamethylenediamine, di(6-aminohexyl)amine, with ethylenediamine and hexamethylenediamine being particularly preferred. Preferred esters or amides are the corresponding glycerol distearate, glycerol tristearate, ethylenediamine distearate, glycerol monopalmitate, glycerol trilaurate, glycerol monobehenate and pentaerythritol tetrastearate.

[0110] It is also possible to use mixtures of different esters or amides, or combinations of esters and amides, in any ratio.

[0111] Further suitable are polyether or polyester polyols which are esterified or etherified with mono- or polycarboxylic acids, preferably fatty acids. Suitable products are commercially available, for example, as Loxiol® EP 728 from Henkel KGaA.

[0112] Preferred ethers derived from alcohols and ethylene oxide have the general formula RO(CH2CH2O) n H [wherein R is an alkyl group having 6 to 40 carbon atoms, and n is an integer of 1 or more]. Particularly preferred for R is a saturated C 16 ~C 18 - a fatty alcohol, commercially available as Lutensol® AT 50 from BASF.

[0113] Further examples of such additives ("lubricants, glidants and release agents") are long chain fatty acids (e.g. stearic acid or behenic acid), their salts (e.g. Ca or Zn stearate), or montan wax (a mixture of linear saturated carboxylic acids with a chain length of 28 to 32 carbon atoms), as well as Ca or Na montanate, and low molecular weight polyethylene or polypropylene waxes.

[0114] The aforementioned additives of component B ("lubricants, glidants and release agents") are usually used in amounts of up to 1% by weight, based on the total mixture.

[0115] Examples of plasticizers as additives of component B include dioctyl phthalate, dibenzyl phthalate, butyl benzyl phthalate, hydrocarbon oils, and N-(n-butyl)benzenesulfonamide.

[0116] The molding materials according to the invention may also contain 0 to 2% by weight of fluorine-containing ethylene polymers, which are polymers of ethylene having a fluorine content of 55 to 76% by weight, preferably 70 to 76% by weight.

[0117] Examples of this are polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymers or tetrafluoroethylene copolymers with relatively small proportions (usually up to 50% by weight) of copolymerizable ethylenically unsaturated monomers, as described, for example, by Schildknecht in "Vinyl and Related Polymers", Wiley-Verlag, 1952, pages 484-494, and by Wall in "Fluorpolymers" (Wiley Interscience, 1972).

[0118] These fluorine-containing ethylene polymers are present in the molding material in a homogeneous distribution and preferably have a particle size d in the range from 0.05 to 10 μm, in particular from 0.1 to 5 μm. 50 (number average). These small particle sizes are particularly preferably achieved by using aqueous dispersions of the fluorine-containing ethylene polymers and incorporating them into the polyester melt.

[0119] The thermoplastic mixtures according to the invention can be prepared in a manner known per se by mixing the starting components A-1, A-2, A-3 and B in a conventional mixing apparatus, for example a (twin-screw) extruder, a Brabender mill or a Banbury mill, followed by extrusion. After extrusion, the extrudate can be cooled and crushed. It is also possible for the individual starting components to be premixed and then the remaining starting components to be added individually and / or mixed. The mixing temperature is usually 230-320° C. In particular, the individual components, for example A-3 and / or B, can also be added via “hot feed” or directly at the inlet of the extruder.

[0120] In the scope of the present application, furthermore, moldings and hollow bodies are claimed which are produced using the thermoplastic mixture according to the invention, in particular hollow bodies which are produced using the thermoplastic mixture according to the invention by blow molding methods, for example extrusion blow molding and stretch blow molding. EXAMPLES

[0121] I. Starting Materials: Ingredient A-1: Polybutylene terephthalate (BASF Ultradur® B 6550) Features: Carboxyl end group content: 34mmol / kg Viscosity: 160 ml / g (VZ measured at 25°C in a 0.5% by weight solution of a 1:1 mixture of phenol / o-dichlorobenzene according to ISO 1628) Melt volume rate: 9.5cm 3 / 10 min (measured at 250 °C and 2.16 kg in accordance with ISO 1133).

[0122] Component A-2: HDPE HTA 108 (ExxonMobil®) Features: Density: 0.961g / cm 3 (Complies with ASTM D1505) Melt index (190℃ / 2.16kg): 0.70g / 10min (based on ASTM D1238) Melt Mass Flow Rate (MFR): 46g / 10min (According to ASTM D1238)

[0123] Component A-3: SURLYN® 1707 (Dow Chemical Company) Features: An ionomer of ethylene-acrylic acid copolymer neutralized to 80% with sodium ions. The acrylic acid content is 15%.

[0124] Component A-4: Epoxidized linseed oil (TRANSFORMACIONES QUIMICO-INDUSTRIALES, SL -TRAQUISA) Characteristics by percentage of fatty acids (% by weight): Stearic acid: 3~5 Palmitic acid: 5~7 Oleic acid (monounsaturated): 18-26 Linoleic acid (diunsaturated): 14-20 Linolenic acid (triunsaturated): 51-56 (Hereinafter, epoxidized linseed oil will be abbreviated as ELO (Epoxidized Linseed Oil)).

[0125] II. Sample preparation: A mixture of Ultradur® B6550 (component A-1), HDPE HTA108 (component A-2) and Surlyn® 1707 (component A-3) was mixed in granular form in the proportions (% by weight) shown in Table 1 below and dried overnight at 80° C. This mixture was fed into a twin-screw extruder (model number CTW100, Thermo Fischer Polylab QC) equipped by the manufacturer with screws for intensive mixing. ELO (component A-4) was metered in as a liquid to the mixture of components A-1, A-2 and A-3. The extruder was rotated at a speed of 140 min -1 The extruded strands were cooled in a water bath and granulated. The resulting granules were submitted for Rheotens analysis.

[0126] III. Measurements taken: The melt volume fraction of samples C1, C2 and E1-E6 was measured according to ISO 1133 at 250°C and 2.16 kg.

[0127] IV. Measurement results: According to the above mentioned standard ISO 1133, values ​​of Melt Volume-Flow Rate (MVR) were determined for various thermoplastic mixtures. The compositions of comparative examples C1 and C2 show the results for a thermoplastic mixture of components A-1, A-2 and A-3 without component A-4 (see the prior art D5 mentioned at the beginning) and for a thermoplastic mixture from components A-1 and A-4 only. In contrast, examples E1 to E6 contain thermoplastic mixtures according to the invention.

[0128] [Table 1]

[0129] The MVR values ​​for comparative examples C1 and C2 are 30 cm 3 / 10 min and therefore exhibit the behavior of a relatively thin liquid, whereas the thermoplastic mixtures E1 to E6 according to the invention are without exception above 5 cm 3 / 10 minutes. Since the measurement (point III) is especially directed to the flow behavior of the thermoplastic mixture, it is believed that the properties of the thermoplastic mixture according to the invention are also reflected in the processing by molding, for example blow molding. In the case of the thermoplastic mixture according to the invention, the undesirable rapid break-off of the molten strand during processing ("flow / drip of the thermoplastic mixture") is effectively reduced.

Claims

1. A) 30 to 100% by weight of a thermoplastic blend comprising: A-1) 65 to 75% by mass of polyester; A-2) 5 to 25% by mass of HD- or LD-polyethylene; A-3) 3 to 10% by mass of an ionomer, 3-1) 30 to 99% by mass of ethylene 3-2) 0 to 60% by mass of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene; and 3-3) 0.01 to 50% by weight of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides and carboxylic esters, with the proviso that the proportion of carboxylic acids is 30 to 100% by weight, and the proportion of carboxylic anhydrides and / or carboxylic esters is complementary 0 to 70% by weight, and the hydrogen of the carboxyl group of the carboxylic acid is replaced by a metal selected from the group consisting of sodium, potassium and zinc in a proportion of at least 20% ("mol %) of the total number of carboxyl groups. wherein the sum of the proportions of components 3-1, 3-2 and 3-3 equals 100% by weight; A-4) 0.5 to 5% by weight of an epoxidized oil or oil mixture, wherein at least a partially unsaturated fatty acid in the fatty acid ester on which the oil or oil mixture is based has 12 to 22 carbon atoms. wherein the sum of the proportions of components A-1, A-2, A-3 and A-4 equals 100% by weight of component A); said thermoplastic blend, B) 0 to 70% by weight of further additives wherein the sum of the proportions of components A) and B) amounts to 100% by weight.

2. The thermoplastic mixture of claim 1, wherein in component 3-3 of A-3, the hydrogens of the carboxyl groups of the carboxylic acid are replaced by metals selected from the group consisting of sodium, potassium and zinc in a proportion of at least 50% ("mol %) of the total number of carboxyl groups.

3. 3. The thermoplastic mixture of claim 1 or 2, wherein the metal in component 3-3 of A-3 corresponds to sodium, potassium, or a mixture of both in any ratio.

4. 4. The thermoplastic mixture according to claim 1, wherein the proportion of component A-1 is 68 to 73% by weight, the proportion of component A-2 is 18 to 22% by weight, the proportion of component A-3 is 5 to 10% by weight, and the proportion of component A-4 is 2 to 5% by weight.

5. 5. The thermoplastic mixture according to claim 1, wherein component A has a carboxyl end group content of 10 to 50 mmol per kg of polyester.

6. The thermoplastic mixture according to any one of claims 1 to 5, wherein the functional monomer of component 3-3 of A-3 is selected from the group consisting of ethylenically unsaturated monocarboxylic acids, dicarboxylic acids, and functional derivatives of these acids.

7. 7. The thermoplastic mixture according to claim 1, wherein the functional monomer of component 3-3 of A-3 is selected from the group consisting of acrylic acid, methacrylic acid, maleic acid, fumaric acid, maleic anhydride, acrylic acid esters and methacrylic acid esters each having 1 to 18 carbon atoms in the alcohol portion of the ester.

8. Component A-3 is 3-1) 50 to 99% by mass of ethylene 3-2) 0 to 50% by mass of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene; and 3-3) 0.05 to 50% by weight of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides, and carboxylic esters.

8. The thermoplastic mixture according to claim 1 , which consists of

9. Component A-3 is 3-1) 50 to 90% by mass of ethylene 3-2) 0 to 50% by mass of one or more compounds selected from the group consisting of 1-octene, 1-butene, and propylene; and 3-3) 2 to 50% by weight of one or more functional monomers selected from the group consisting of carboxylic acids, carboxylic anhydrides, and carboxylic esters.

8. The thermoplastic mixture according to claim 1 , which consists of

10. 10. The thermoplastic mixture of any one of claims 1 to 9, wherein the epoxidized oil or oil mixture of component A-4 is derived from one or more vegetable oils selected from the group consisting of soybean oil, linseed oil, rapeseed oil, camelina oil, castor oil, cottonseed oil, olive oil, peanut oil, sunflower oil, corn oil and hempseed oil.

11. The thermoplastic mixture of claim 10, wherein the epoxidized oil or oil mixture of component A-4 is derived from one or more vegetable oils selected from the group consisting of soybean oil, linseed oil, rapeseed oil and castor oil.

12. 12. The thermoplastic mixture according to claim 1, wherein the proportion of component A-4 is from 1 to 3% by weight.

13. 13. A molded part produced using a thermoplastic mixture according to any one of claims 1 to 12.

14. 13. A hollow body produced using a thermoplastic mixture according to any one of claims 1 to 12.

15. 13. A hollow body produced by means of a blow moulding process using a thermoplastic mixture according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • EP20190021.4

  • Reinforced polyester molding compositions

    WO1990014391A1