Combined flame retardant and synergist for use with thermoplastics - Patents.com

A combination of phosphorus-containing flame retardants and hypophosphite metal salts in thermoplastic compositions addresses the trade-off between flame retardancy and material performance, achieving enhanced stability and mechanical properties without nitrogen synergists.

JP2024541517APending Publication Date: 2024-11-08LANXESS CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024531358
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-26
Filing Date
2022-11-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing flame retardant compositions for thermoplastic polymers often compromise on processing stability and mechanical properties, necessitating a balance between flame retardancy and material performance.

Method used

A combination of phosphorus-containing flame retardants and hypophosphite metal salts, optionally with heat stabilizers and additional synergists, is formulated to enhance flame retardancy while maintaining processing stability and mechanical properties.

Benefits of technology

The solution provides thermoplastic compositions with superior flame retardancy, processing stability, and mechanical properties, eliminating the need for nitrogen-containing synergists and enhancing thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541517000001
    Figure 2024541517000001
  • Figure 2024541517000002
    Figure 2024541517000002
  • Figure 2024541517000003
    Figure 2024541517000003
Patent Text Reader

Abstract

The present disclosure provides novel flame retardant and synergist additive compositions comprising at least one phosphorus-containing flame retardant and at least one metal hypophosphite, as described herein. The additive combinations disclosed herein exhibit excellent flame retardant performance in thermoplastic polymers while also providing excellent processing stability and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to flame retardant and synergist additive compositions for thermoplastic polymers, and flame retardant thermoplastic compositions comprising the flame retardant and synergist. [Background technology]

[0002] WO 2020 / 132075 and WO 2021 / 076169 disclose certain phosphorus-containing flame retardants with high thermal stability for use in a variety of thermoplastic applications.

[0003] In accordance with the present disclosure, it has been found that certain phosphorus-containing flame retardants disclosed in WO 2020 / 132075 and WO 2021 / 076169 in combination with certain metal hypophosphites exhibit excellent flame retardant performance in thermoplastic polymers while also providing excellent processing stability and mechanical properties. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2020 / 132075 [Patent Document 2] International Publication No. 2021 / 076169 [Patent Document 3] U.S. Patent No. 9,745,449 Summary of the Invention [Means for solving the problem]

[0005] In one aspect, the present disclosure provides: (A) Empirical Formula (I)

[0006] [ka]

[0007] [wherein R is H, alkyl, aryl, alkylaryl, or arylalkyl group; M (+)y is a metal cation, where (+)y represents the charge formally assigned to the cation, M is a metal, y is 2 or 3, and a, b, and c represent the ratio of corresponding components to each other in the compound, satisfying the charge balance equation 2(a)+c=b(y), where c is not zero. and at least one phosphorus-containing flame retardant of (B) Chemical formula Me (+)n (H2PO2) n [wherein Me is a metal cation, (+)n represents the oxidation state of the metal cation, and n is 2 or 3] At least one metal hypophosphite salt of The present invention provides a flame retardant and synergist additive composition comprising:

[0008] Flame Retardant and Synergist The additive composition may further comprise (C) at least one heat stabilizer. The additive composition may additionally comprise (D) one or more additional synergists and / or one or more additional flame retardants.

[0009] In a further aspect, the present disclosure provides a method for producing a method for treating a cancer cell comprising: (i) at least one thermoplastic polymer; (ii) at least one phosphorus-containing flame retardant of empirical formula (I) above; (iii) at least one metal hypophosphite as described above; The flame retardant thermoplastic composition may further comprise one or more of the following: (iv) at least one inorganic filler (e.g., glass fiber), (v) at least one heat stabilizer, (vi) at least one additional synergist and / or additional flame retardant, and (vii) one or more further additives for enhancing the properties of the thermoplastic composition.

[0010] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention, as claimed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this application, unless otherwise specified, the words "a" or "an" mean "one or more than one."

[0012] The term "alkyl" in this application, unless the context indicates otherwise, includes "arylalkyl."

[0013] The term "aryl" in this application includes "alkylaryl", unless the context indicates otherwise.

[0014] The term "phosphonic acid," as used herein, unless the context indicates otherwise, refers to unsubstituted or alkyl- or aryl-substituted phosphonic acids.

[0015] The term "pyrophosphonic acid," as used herein, unless the context indicates otherwise, refers to unsubstituted or alkyl- or aryl-substituted pyrophosphonic acid.

[0016] At least one phosphorus-containing flame retardant (component (A)) of the present disclosure has the empirical formula:

[0017] [ka]

[0018] [wherein R is H, alkyl, aryl, alkylaryl, or arylalkyl group; M (+)yM is a metal such that (a) is a metal cation, where (+)y represents the charge formally assigned to the cation, y is 2 or 3, and a, b, and c represent the ratio of corresponding components to each other in the compound, satisfying the charge balance equation 2(a)+c=b(y), where c is not zero. Often, a is 0, 1, or 2 (e.g., 0 or 1), b is 1 to 4, e.g., 1 or 2, and c is 1 or 2, and the product is charged at equilibrium. Examples of suitable metals (M) include, but are not limited to, Al, Ga, Sb, Fe, Co, B, Bi, Mg, Ca, and Zn.

[0019] As is common in coordination compounds, formula (I) is empirical or idealized such that the compound may be a coordination polymer, a complex salt, a salt in which certain valences are shared, etc. In many embodiments, empirical formula (I) represents a monomer unit (i.e., a coordination entity) of a coordination polymer, whereby the extended coordination polymer structure forms the phosphorus-containing flame retardant of the present disclosure.

[0020] In certain embodiments, y in formula (I) is 2 (i.e., M (+)y is a dicationic metal), a is 0, b is 1, and c is 2. Often, the dicationic metal M is Mg, Ca, or Zn. In other embodiments, y in formula (I) is 3 (i.e., M (+)y is a tricationic metal), a is 1, b is 1, and c is 1. The tricationic metal M may be selected from, for example, Al, Ga, Sb, Fe, Co, B, and Bi. Often, the tricationic metal M is Al, Fe, Ga, Sb, or B.

[0021] Preferably, the phosphorus-containing flame retardant of empirical formula (I) has the following empirical formula:

[0022] [ka]

[0023] In formula (I), M is Al and y is 3, so that

[0024] As set forth herein, the absence of subscripts a, b, and c in the empirical formula indicates that each subscript is 1, meaning a 1:1:1 ratio of dianionic pyrophosphonate ligand, metal atom, and monoanionic pyrophosphonate ligand. In many embodiments, empirical formula (II) represents the repeating monomer unit (i.e., the coordination entity) of a coordination polymer, whereby the extended coordination polymer structure forms the phosphorus-containing flame retardant of the present disclosure.

[0025] In most cases, R is H, C 1~12 Alkyl, C 6~10 Aryl, C 7~18 Alkylaryl or C 7~18 and arylalkyl, wherein the alkyl, aryl, alkylaryl, or arylalkyl is unsubstituted or is selected from the group consisting of halogen, hydroxyl, amino, C 1~4 Alkylamino, DiC 1~4 Alkylamino, C 1~4 Alkoxy, carboxy, or C 2~5 In some embodiments, the alkyl, aryl, alkylaryl, or arylalkyl is an unsubstituted C 1~12 Alkyl, C6 aryl, C 7~10 Alkylaryl or C 7~10 Arylalkyl, e.g., C 1~6 Alkyl, phenyl, or C 7~9 In some embodiments, R is a substituted or unsubstituted C 1~6 Alkyl, C6 aryl, C 7~10 Alkylaryl or C 7~12 Arylalkyl, e.g., C 1~4 Alkyl, C6 aryl, C 7~9 Alkylaryl or C 7~10 In many embodiments, R is an unsubstituted C 1~12 Alkyl, e.g., C1~6 It is an alkyl.

[0026] R as alkyl may be a straight or branched chain alkyl group having the specified number of carbons, including, for example, unbranched alkyls such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, and branched alkyls such as isopropyl, isobutyl, sec-butyl, t-butyl, ethylhexyl, and t-octyl. For example, R as alkyl may be selected from methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, and t-butyl. In many embodiments, R is methyl, ethyl, propyl, or isopropyl, e.g., methyl or ethyl.

[0027] In most cases, when R is aryl, it is phenyl. Examples of R as alkylaryl include phenyl substituted with one or more alkyl groups, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, and t-butyl. Examples of R as arylalkyl include benzyl, phenethyl, styryl, cumyl, and phenpropyl.

[0028] In many embodiments, R is selected from methyl, ethyl, propyl, isopropyl, butyl, phenyl, and benzyl. In certain embodiments, R is methyl, ethyl, propyl, isopropyl, or butyl, and M is Al, Fe, Zn, or Ca.

[0029] The phosphorus-containing flame retardant of the present disclosure may be a mixture of compounds of empirical formula (I).

[0030] As described in WO2020 / 132075 and WO2021 / 076169, the phosphorus-containing flame retardant of the present disclosure has a high phosphorus content (i.e., a higher ratio of phosphorus atoms to metal atoms (P to M)) compared to phosphorus-containing flame retardants described in the art. For example, tricationic metals (e.g., aluminum) and dicationic metals (e.g., zinc) are known to form tri-substituted and di-substituted charge balance compounds, respectively. As seen in the art, tris-phosphonic acid aluminum salts having a phosphorus to aluminum ratio of 3:1 and diphosphonic acid zinc salts having a phosphorus to zinc ratio of 2:1 are known as flame retardants. However, according to the pyrophosphonic acid ligand formation of the phosphorus-containing flame retardant of the present disclosure, the phosphorus to metal ratio in the flame retardant product is greater. For example, as demonstrated in the examples disclosed in WO 2020 / 132075 and WO 2021 / 076169, the ratio of phosphorus to aluminum, or phosphorus to iron, was 4:1 in the resulting flame retardant product.

[0031] At least one metal hypophosphite (component (B)) has the chemical formula Me (+)n (H2PO2) n where Me is a metal cation and (+)n represents the oxidation state of the metal cation, where n is 2 or 3. Examples of suitable metal cations in the +2 oxidation state include calcium, zinc, magnesium, barium, manganese, iron(II), and copper(II). In many embodiments, the metal cation in the +2 oxidation state is a Group IIA metal (i.e., an alkaline earth metal), such as calcium, or the metal cation is zinc.

[0032] Examples of suitable metal cations in the +3 oxidation state include aluminum and iron(III).

[0033] Often, the metal hypophosphite is selected from calcium hypophosphite (Ca(HPO)) and aluminum hypophosphite (Al(HPO)). For example, in some embodiments, the metal hypophosphite is calcium hypophosphite. In some embodiments, the metal hypophosphite is aluminum hypophosphite.

[0034] The metal hypophosphites of the present disclosure are known in the art and / or may be produced by known methods. Many suitable metal hypophosphites are commercially available, such as from Italmatch Chemicals under the Phoslite® brand name.

[0035] The additive composition may additionally comprise one or more heat stabilizers (component (C)). Examples of suitable heat stabilizers include metal hydroxides, oxides, oxide hydrates, borates, molybdates, carbonates, sulfates, phosphates, silicates, siloxanes, stannates, mixed oxide-hydroxides, oxide-hydroxide-carbonates, hydroxide-silicates, hydroxide-borates, preferably where the metal is zinc, magnesium, calcium, or manganese, often zinc. For example, the one or more heat stabilizers may be selected from zinc borate, zinc stannate, zinc molybdate complexes (e.g., Kemgard® 911B), zinc molybdate / magnesium hydroxide complexes (e.g., Kemgard® MZM), zinc molybdate / magnesium silicate complexes (e.g., Kemgard® 911C), calcium zinc molybdate complexes (e.g., Kemgard® 911A), and zinc phosphate complexes (e.g., Kemgard® 981), montmorillonite, kaolinite, halloysite, and hydrotalcite.

[0036] Flame Retardant and Synergist The additive composition may further comprise one or more additional synergists and / or one or more additional flame retardants (component (D)). Examples of additional flame retardant synergists include condensation products of melamine (e.g., melam, melem, melon), melamine cyanurate, reaction products of melamine with polyphosphoric acid (e.g., dimelamine pyrophosphate, melamine polyphosphate), reaction products of melamine condensation products with polyphosphoric acid (e.g., melem polyphosphate, melam polyphosphate, melon polyphosphate), melamine-poly(metal phosphate) (e.g., melamine-poly(zinc phosphate), triazine-based compounds such as the reaction product of trichlorotriazine, piperazine, and morpholine, e.g., poly[2,4-(piperazin-1,4-yl)-6-(morpholin-4-yl)-1,3,5-triazine] / piperazine (e.g., MCA® PPM Triazine HF), organic phosphinates such as aluminum dialkylphosphinates, for example aluminum diethylphosphinate (Exolit® OP), and aluminum hydrogen phosphite (Al2(HPO3)3).

[0037] In some embodiments, the additional synergist is a nitrogen-containing synergist. Suitable nitrogen-containing synergists may be selected from, for example, melamine derivatives such as melamine and its condensation products (melam, melem, melon, or similar compounds with higher condensation levels), melamine cyanurate, and phosphorus / nitrogen compounds such as dimelamine phosphate, dimelamine pyrophosphate, melamine phosphate, melamine pyrophosphate, melamine polyphosphate, melam polyphosphate, melon polyphosphate, and melem polyphosphate, and mixed polysalts thereof.

[0038] Examples of additional flame retardants suitable for the flame retardant and synergist additive composition of the present invention include halogenated flame retardants, alkyl or aryl phosphine oxide flame retardants, alkyl or aryl phosphate flame retardants, alkyl or aryl phosphonates, alkyl or aryl phosphinates, and salts of alkyl or aryl phosphinic acids. In many cases, the additional flame retardant is an alkyl or aryl phosphate (e.g., triphenyl phosphate, bisphenol-A bis(diphenyl phosphate), resorcinol bis(diphenyl phosphate), or resorcinol bis(dixylenyl phosphate).

[0039] As demonstrated herein, when using the combination of phosphorus-containing flame retardants and metal hypophosphites of the present disclosure, the use of nitrogen-containing synergists or nitrogen-containing flame retardants is not necessary to obtain excellent flame retardant performance and processing stability in thermoplastic polymer applications. Thus, in some embodiments, the flame retardant and synergist additive composition of the present disclosure does not include a nitrogen-containing synergist or nitrogen-containing flame retardant.

[0040] The flame retardant and synergist additive composition may further include other mixture components or additives (E), such as antioxidants, acid scavengers, phosphine inhibitors, UV stabilizers, processing agents, and other additives known in the art suitable for use in flame retardant compositions.

[0041] The flame retardant and synergist additive composition may consist essentially of or consist of components (A) and (B), and optionally any one or combination of components (C), (D), and (E).

[0042] The proportions of components (A) and (B), and optional components (C), (D), and (E) in the flame retardant and synergist additive composition may vary and generally depend, for example, on the intended application, processing conditions, etc. In many embodiments, the flame retardant and synergist additive composition comprises from 20 to 95 wt. %, such as from 30 to 90 wt. %, from 40 to 90 wt. %, from 50 to 80 wt. %, or from 60 to 70 wt. %, of at least one phosphorus-containing flame retardant (A), based on the total weight of the additive composition; from 5 to 80 wt. %, such as from 10 to 70 wt. %, from 10 to 60 wt. %, from 20 to 50 wt. %, or from 30 to 40 wt. %, of at least one phosphorus-containing flame retardant (B), based on the total weight of the additive composition; % of at least one metal hypophosphite (B), 0 to 20 wt %, such as 0 to 15 wt %, 1 to 15 wt %, or 1 to 10 wt %, of at least one heat stabilizer (C), and 0 to 20 wt %, such as 0 to 15 wt %, 2 to 12 wt %, or 5 to 10 wt %, of at least one additional synergist and / or additional flame retardant (D), based on the total weight of the additive composition. The optional additive (E) may be present in the flame retardant and synergist composition in an amount that is typically less than 30 weight percent, e.g., often less than 20 wt %, less than 15 wt %, less than 10 wt %, or less than 8 wt %, based on the total weight of the flame retardant and synergist additive composition. Typically, any one or combination of components (A) and (B), and optionally components (C), (D) and (E), as described herein, comprise 100% by weight of the flame retardant and synergist additive composition.

[0043] The present disclosure relates to (i) at least one thermoplastic polymer; (ii) at least one phosphorus-containing flame retardant of empirical formula (I) above; (iii) at least one metal hypophosphite as described above; The flame retardant thermoplastic composition may further comprise one or more of the following: (iv) at least one inorganic filler (e.g., glass fiber), (v) at least one heat stabilizer, (vi) at least one additional synergist and / or additional flame retardant, and (vii) one or more further additives for enhancing the properties of the thermoplastic composition.

[0044] The at least one thermoplastic polymer (i) is often present in the flame retardant thermoplastic composition in an amount of 30 to 95 wt%, such as 40 to 90 wt%, or 50 to 90 wt%, based on the total weight of the flame retardant thermoplastic composition. The at least one thermoplastic polymer may be a thermoplastic polyester, polyamide, polystyrene, including high impact polystyrene (HIPS), polyolefin, polycarbonate, polyurethane, polyphenylene ether, or other thermoplastic polymer. In many embodiments, the thermoplastic polymer comprises a polyester (e.g., polyalkylene terephthalate) or polyamide. In many embodiments, the thermoplastic polymer comprises a polyamide. More than one thermoplastic polymer (thermoplastic polymer blend) can be used, such as polyphenylene ether / styrene blends, polyvinyl chloride / acrylonitrile butadiene styrene (ABS), or methacrylonitrile and alpha-methylstyrene-containing ABS, as well as other impact-modifying polymers such as polyester / ABS or polycarbonate / ABS. The thermoplastic polymer may be unreinforced or reinforced, for example, with glass, such as glass-filled polyester (eg, glass-filled polyalkylene terephthalate) or glass-filled polyamide.

[0045] Examples of thermoplastic polyesters include homopolyesters and copolyesters obtained by polycondensation of an acid component and a diol component. For example, suitable polyesters may be selected from polybutylene terephthalate and polyethylene terephthalate.

[0046] The diol component may contain one or more of the following glycols: ethylene glycol, trimethylene glycol, 2-methyl-1,3-propane glycol, 1,4-butylene glycol, hexamethylene glycol, decamethylene glycol, cyclohexanedimethanol, or neopentylene glycol. The acid component may contain one or more of the following acids: terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, p-hydroxybenzoic acid, sebacic acid, adipic acid, and polyester-forming derivatives thereof.

[0047] In many embodiments, the thermoplastic polyester is selected from poly(ethylene terephthalate), poly(1,3-trimethylene terephthalate), poly(1,4-butylene terephthalate), and blends thereof. For example, the thermoplastic polyester blend can contain from about 1 to about 99 parts by weight of one polyester and from about 99 to about 1 part by weight of a different polyester, per 100 parts by weight of both components combined. Poly(1,4-butylene terephthalate) may be obtained by polymerization of a diol component consisting of at least 70 mol%, e.g., at least 80 mol%, 1,4-butylene glycol, and an acid component consisting of at least 70 mol%, e.g., at least 80 mol%, terephthalic acid and / or their polyester-forming derivatives.

[0048] Thermoplastic polyamides include polyamides derived from diamines and dicarboxylic acids, polyamides obtained from aminocarboxylic acids, including in combination with diamines and / or dicarboxylic acids, and polyamides derived from lactams, including in combination with diamines and / or dicarboxylic acids. Examples of suitable polyamides include aliphatic polyamides such as polyamide-4,6, polyamide-6, polyamide-6,6, polyamide-6,10, polyamide-6,12, polyamide-11, and polyamide-12; polyamides obtained from aromatic dicarboxylic acids such as terephthalic acid and / or isophthalic acid and aliphatic diamines such as hexamethylenediamine or nonamethylenediamine; polyamides obtained from aliphatic dicarboxylic acids such as adipic acid and / or azelaic acid and aromatic diamines such as meta-xylylenediamine; polyamides obtained from both aromatic and aliphatic dicarboxylic acids such as both terephthalic acid and adipic acid and aliphatic diamines such as hexamethylenediamine; polyamides obtained from adipic acid, azelaic acid, and 2,2-bis-(p-aminocyclohexyl)propane; and polyamides obtained from terephthalic acid and 4,4'-diaminodicyclohexylmethane. Mixtures and / or copolymers of two or more of the foregoing polyamides or prepolymers thereof, respectively, may also be used.

[0049] The polyamides may be prepared by any known method, such as by polymerization of monoamino monocarboxylic acids or lactams thereof having at least two carbon atoms between the amino group and the carboxylic acid group, by polymerization of substantially equimolar proportions of diamines containing at least two carbon atoms between the amino group and the dicarboxylic acid, or by polymerization of monoamino carboxylic acids or lactams thereof as defined above together with substantially equimolar proportions of diamines and dicarboxylic acids. The dicarboxylic acids may be used in the form of their functional derivatives, such as salts, esters, or acid chlorides.

[0050] Polyamides having a melting point of at least 280°C are widely used, for example, for the electrical and electronics industry to produce molding compositions that allow the production of molded articles with excellent dimensional stability at high temperatures. This type of molding composition is required, for example, in the electronics industry to produce components that are mounted on printed circuit boards according to the so-called surface mount technology SMT. In this application, these components must withstand temperatures of up to 270°C for a short period of time without dimensional changes.

[0051] Such high temperature polyamides include certain polyamides produced from alkyl diamines and diacids, such as polyamides 4, 6. Additionally, many high temperature polyamides are aromatic and semi-aromatic polyamides, i.e., homopolymers, copolymers, terpolymers, or higher order polymers derived from monomers containing aromatic groups. Aromatic or semi-aromatic polyamides may be used, or blends of aromatic and / or semi-aromatic polyamides may be used. Blends with aliphatic polyamides may also be used.

[0052] Examples of suitable high temperature aromatic or semi-aromatic polyamides include polyamide-4,T, poly(m-xylylene adipamide) (polyamide-MXD,6), poly(dodecamethylene terephthalamide) (polyamide-12,T), poly(decamethylene terephthalamide) (polyamide-10,T), poly(nonamethylene terephthalamide) (polyamide-9,T), hexamethylene adipamide / hexamethylene terephthalamide copolyamide (polyamide-6,T / 6,6), hexamethylene terephthalamide copolyamide (polyamide-7,T), hexamethylene terephthalamide copolyamide (polyamide-9,T), hexamethylene terephthalamide copolyamide (polyamide-8,T), hexamethylene terephthalamide copolyamide (polyamide-9,T), hexamethylene terephthalamide copolyamide (polyamide-10 ... hexamethylene adipamide / 2-methylpentamethylene terephthalamide copolyamide (polyamide-6,T / D,T); hexamethylene adipamide / hexamethylene terephthalamide / hexamethylene isophthalamide copolyamide (polyamide-6,6 / 6,T / 6,I); poly(caprolactam-hexamethylene terephthalamide) (polyamide-6 / 6,T); and hexamethylene terephthalamide / hexamethylene isophthalamide (polyamide-6,T / 6,I) copolymer.

[0053] Thus, certain embodiments of the invention are compositions that include polyamides that melt at high temperatures, for example, at or above 280° C., at or above 300° C., or at or above 320° C. In some embodiments, the polyamide has a melting temperature of from 280 to 340° C., such as the polyamides 4, 6 or aromatic and semi-aromatic polyamides described above.

[0054] Preferred polyamides are polyphthalamides such as polyamide-6, polyamide-6,6, polyamide-11, polyamide-12, polyamide-4,T, polyamide-6,T / 6,6, and polyamide-6,6 / 6,T / 6,I copolymers, glass-filled polyamides thereof, and blends thereof. For example, a thermoplastic polyamide blend may contain from about 1 to 99 parts by weight of one polyamide and from about 99 to about 1 part by weight of a different polyamide, per 100 parts by weight of both components combined.

[0055] In some embodiments, the polymer is a thermoplastic elastomer (e.g., a thermoplastic polyolefin or a thermoplastic polyurethane). In some embodiments, the thermoplastic elastomer is a thermoplastic polyurethane.

[0056] The at least one phosphorus-containing flame retardant (ii) is as described above and is present in the flame retardant thermoplastic composition in a flame retardant effective amount. Often, the phosphorus-containing flame retardants disclosed herein are present in an amount of 5 to 30 wt%, such as 8 to 30 wt%, 10 to 30 wt%, 12 to 30 wt%, or 15 to 30 wt%, based on the total weight of the flame retardant thermoplastic composition.

[0057] The at least one metal hypophosphite (iii) in the flame retardant thermoplastic composition is as described above and is often present in the flame retardant thermoplastic composition in an amount of from 0.1 to 20 wt%, such as from 1 to 20 wt%, from 2 to 15 wt%, from 2 wt% or 5 wt% to 15 wt%, or from 2 wt% or 5 wt% to 10 wt%, based on the total weight of the composition.

[0058] At least one inorganic filler (iv) may be present in the flame retardant thermoplastic composition. As known in the art, inorganic fillers can reduce the molding shrinkage coefficient and linear expansion coefficient of the resulting molded article and improve high and low thermal shock properties. Various fillers in fibrous or non-fibrous (e.g., powder, plate) form may be used depending on the desired article. Some examples of fibrous fillers, which are types of inorganic fillers, include glass fibers, glass fibers with non-circular cross sections such as flat fibers, carbon fibers, silica fibers, silica alumina fibers, zirconia fibers, boron nitride fibers, silicon nitride fibers, boron fibers, potassium titanate fibers, and even metal fibrous materials such as stainless steel, aluminum, titanium, copper, and brass. Typical fibrous fillers are glass fibers or carbon fibers. Alternatively, the inorganic filler may be a powdered filler such as carbon black, graphite, silica, quartz powder, glass beads, glass powder, silicates such as calcium silicate, kaolin, talc, clay, diatomaceous earth, wollastonite, metal oxides such as iron oxide, titanium oxide, zinc oxide, and alumina, metal hydroxides, metal carbonates such as calcium carbonate and magnesium carbonate, metal sulfates such as calcium sulfate and barium sulfate, silicon carbide, silicon nitride, boron nitride, and various metal powders. Another example of an inorganic filler is a plate-like filler such as mica, glass flakes, and various metal foils. These inorganic fillers can be used alone or in combination of two or more kinds. When used, the inorganic filler is desirably pretreated with a sizing agent or surface treatment agent as necessary.

[0059] When present, the amount of the at least one inorganic filler in the flame retardant thermoplastic composition is often from 1 to 50 wt %, for example, from 5 to 50 wt %, from 10 to 40 wt %, or from 15 to 30 wt %, based on the total weight of the flame retardant thermoplastic composition.

[0060] The flame retardant thermoplastic composition may further comprise at least one heat stabilizer (v). Exemplary heat stabilizers are described above. The amount of the at least one heat stabilizer, if present, is often from 0.1 to 5 wt %, based on the total weight of the flame retardant thermoplastic composition.

[0061] The flame retardant thermoplastic composition may further comprise at least one additional synergist and / or additional flame retardant (vi). Exemplary additional flame retardant synergists and additional flame retardants are described above. The amount of the at least one additional flame retardant synergist and / or additional flame retardant (vi), if present, is often from 0.1 to 10 wt%, such as from 0.5 to 10 wt%, based on the total weight of the flame retardant thermoplastic composition.

[0062] As described herein, when using the combination of phosphorus-containing flame retardants and metal hypophosphites of the present disclosure, the use of nitrogen-containing synergists or nitrogen-containing flame retardants is not necessary to obtain superior flame retardant performance in thermoplastic polymer applications. Thus, in some embodiments, the flame retardant thermoplastic composition does not include a nitrogen-containing synergist or nitrogen-containing flame retardant.

[0063] Other mixture components or additives (vii) may be present in the flame retardant thermoplastic composition and are typically used in amounts less than 10 weight percent of the flame retardant thermoplastic composition, for example, often less than 5 weight percent, such as 3 wt % or less. Non-limiting examples include antioxidants, UV stabilizers, lubricants, impact modifiers, plasticizers, acid scavengers (e.g., carbodiimides or epoxides), phosphine inhibitors, pigments, dyes, optical brighteners, antistatic agents, anti-drip agents, e.g., PTFE, and other additives used to enhance the properties of the resin.

[0064] In many embodiments, the flame retardant thermoplastic composition comprises at least one thermoplastic polymer (i) in an amount of 30 to 95 wt%, at least one phosphorus-containing flame retardant (ii) in an amount of 5 to 30 wt%, at least one metal hypophosphite (iii) in an amount of 0.1 to 20 wt%, at least one inorganic filler (iv) in an amount of 0 to 50 wt%, and at least one heat stabilizer (v) in an amount of 0 to 5 wt%, all based on the total weight of the flame retardant thermoplastic composition. In many embodiments, the flame retardant thermoplastic composition comprises at least one thermoplastic polymer (i) in an amount of 30 to 95 wt%, such as 40 to 90 wt%, at least one phosphorus-containing flame retardant (ii) in an amount of 5 to 30 wt%, such as 8 to 30 wt%, 10 to 30 wt%, or 15 to 30 wt%, at least one inorganic filler (iv) in an amount of 1 to 20 wt%, 2 to 15 wt%, 2 to 20 wt%, 3 to 40 wt%, 4 to 50 wt%, 5 to 60 wt%, 6 to 80 wt%, 7 to 90 wt%, 8 to 10 wt%, 10 to 10 wt%, 15 to 10 wt%, 2 to 20 wt%, 3 to 40 wt%, 4 to 50 wt%, 5 to 60 wt%, 6 to 80 wt%, 7 to 90 wt%, 8 to 100 wt%, 10 ... At least one metal hypophosphite (iii) in an amount of 0.1 to 20 wt%, such as t% or 5 wt% to 15 wt%, or 2 wt% or 5 wt% to 10 wt%, at least one inorganic filler (iv) in an amount of 0 to 50 wt%, such as 10 to 40 wt%, or 15 to 30 wt%, and at least one heat stabilizer (v) in an amount of 0 to 5 wt%, such as 0.01 to 5 wt%. The composition may further comprise at least one additional synergist and / or additional flame retardant (vi) as described herein. The composition may also comprise one or more other mixture components or additives (vii) as described herein.

[0065] In certain embodiments, the thermoplastic polymer (i) is a thermoplastic polyamide, such as one selected from aliphatic polyamides and / or aromatic and semi-aromatic high temperature polyamides, and the metal hypophosphite (iii) has the chemical formula Me (+)n (H2PO2) nwhere Me is a metal cation, (+)n represents the oxidation state of the metal cation, n is 2, and preferably the metal hypophosphite is calcium hypophosphite. Preferably the polyamide is polyamide-4,6, polyamide-6, polyamide-6,6, polyamide-6,10, polyamide-6,12, polyamide-11, polyamide-12, polyamide-4,T, poly(m-xylylene adipamide) (polyamide-MXD,6), poly(dodecamethylene terephthalamide) (polyamide-12,T), poly(decamethylene terephthalamide) (polyamide-10,T), poly(nonamethylene terephthalamide) (polyamide-9,T), hexamethylene adipamide / hexamethylene terephthalamide copolyamide. Polyamides are selected from polyamide-6,T / 6,6, hexamethylene terephthalamide / 2-methylpentamethylene terephthalamide copolyamide (polyamide-6,T / D,T); hexamethylene adipamide / hexamethylene terephthalamide / hexamethylene isophthalamide copolyamide (polyamide-6,6 / 6,T / 6,I); poly(caprolactam-hexamethylene terephthalamide) (polyamide-6 / 6,T); hexamethylene terephthalamide / hexamethylene isophthalamide (polyamide-6,T / 6,I) copolymers. More preferably, the polyamides are polyamide-6 and polyamide-6,6. The proportions and amounts of the components in the thermoplastic polymer composition may be as described herein for each component part.

[0066] In certain embodiments, the thermoplastic polymer (i) is a thermoplastic polyester, preferably a polyalkylene terephthalate, such as polybutylene terephthalate and / or polyethylene terephthalate, and the metal hypophosphite (iii) has the formula Me (+)n (H2PO2) n where Me is a metal cation, (+)n represents the oxidation state of the metal cation, n is 3, and preferably the metal hypophosphite is aluminum hypophosphite. The proportions and amounts of the components in the thermoplastic polymer composition may be as described herein for each component part.

[0067] In certain embodiments, the thermoplastic polymer (i) is a thermoplastic polyamide, such as an aliphatic polyamide and / or an aromatic and semi-aromatic high temperature polyamide, preferably selected from aliphatic polyamides such as polyamide 6 and polyamide 6,6, and the metal hypophosphite (iii) is represented by the chemical formula Me (+)n (H2PO2) n where Me is a metal cation, (+)n represents the oxidation state of the metal cation, n is 3, and preferably the metal hypophosphite is aluminum hypophosphite. The proportions and amounts of the components in the thermoplastic polymer composition may be as described herein for each component part.

[0068] The phosphorus-containing flame retardants of the present disclosure may be prepared according to the procedures disclosed in WO2020 / 132075 and WO2021 / 076169. One suitable method is referred to herein as the solvent method. Another suitable method is referred to herein as the molten state method.

[0069] Preparation of phosphorus-containing flame retardants by solvent method A suitable method for preparing the phosphorus-containing flame retardant of the present disclosure comprises reacting a metal or suitable metal compound with an unsubstituted or alkyl- or aryl-substituted phosphonic acid. The process comprises (i) preparing a reaction mixture containing (a) an unsubstituted or alkyl- or aryl-substituted phosphonic acid, (b) a solvent for the phosphonic acid, and (c) a metal or suitable metal compound, and (ii) heating or reacting the reaction mixture at a reaction temperature of 105° C. or greater for a sufficient time to produce the phosphorus-containing flame retardant. In the reaction, the metal is oxidized to form a phosphonic acid of formula M (+)y where M is a metal, (+)y represents the charge of the metal cation, and y is 2 or 3. Suitable metal compounds are represented by the formula M p (+)y X qwhere M is a metal, (+)y represents the charge of the metal cation, y is 2 or 3, X is an anion, and the values ​​of p and q provide a charge balanced metal compound.

[0070] In another embodiment, the phosphorus-containing flame retardant may be prepared by reacting a metal or suitable metal compound with an unsubstituted or alkyl- or aryl-substituted pyrophosphonic acid. The process includes (i) preparing a reaction mixture containing (a) an unsubstituted or alkyl- or aryl-substituted pyrophosphonic acid, (b) a solvent for the pyrophosphonic acid, and (c) the metal or suitable metal compound described above, and (ii) heating or reacting the reaction mixture at a reaction temperature of 20° C. or greater for a sufficient time to produce the phosphorus-containing flame retardant.

[0071] The reaction product typically forms as a slurry when the phosphorus-containing flame retardant product precipitates from the reaction mixture. The phosphonic acid, pyrophosphonic acid, and / or solvent remaining after the reaction, along with any by-products that may result, can be removed by filtration and / or washing, for example, with water. In many embodiments, a substantially pure flame retardant material is produced, for example a flame retardant that contains essentially a single compound having flame retardant activity, or essentially a mixture of active compounds. Conversion based on the metal or metal compound is typically high, and the product can be easily separated and, if desired, further purified.

[0072] Typically, the molar ratio of phosphonic acid or pyrophosphonic acid to metal or suitable metal compound in the reaction mixture is higher than 2:1, such as about 3:1 or more, about 4:1 or more, about 5:1 or more, about 6:1 or more, about 7:1 or more, or about 8:1 or more. Often, a larger molar excess of phosphonic acid or pyrophosphonic acid to metal or suitable metal compound is used in the reaction mixture, such as about 10:1 or more, about 15:1 or more, about 20:1 or more, about 25:1 or more, about 30:1 or more, or any range therebetween. A larger molar excess of phosphonic acid or pyrophosphonic acid to metal or suitable metal compound may also be used. For example, the molar ratio may be up to about 50:1, up to about 100:1, up to about 300:1, up to about 500:1, or any range therebetween. However, as will be appreciated, process efficiency may be compromised at certain large molar excesses, for example, product precipitation from the reaction mixture may be hindered. In many embodiments, the molar ratio ranges from about 4:1, from about 5:1, from about 6:1, from about 8:1, or from about 10:1 to about 100:1, or to about 50:1, such as from about 8:1, from about 12:1, from about 16:1, or from about 20:1 to about 50:1, or to about 40:1.

[0073] The reaction mixture is heated at a reaction temperature for a sufficient time to produce a flame retardant product. As used herein, the step of "heating the reaction mixture at a reaction temperature for a sufficient time to produce a phosphorus-containing flame retardant" and the like includes, but is not limited to, embodiments in which all or substantially all of the solvent for component (b) of the reaction mixture, i.e., the phosphonic acid or pyrophosphonic acid, is boiled off from the reaction mixture during the process of heating the reaction mixture to or at the reaction temperature. Thus, it is understood that even when all or substantially all of the solvent component (b) is boiled off during the process of heating the reaction mixture to or at the reaction temperature, the "reaction mixture" described herein is still said to be heated at a reaction temperature.

[0074] The reaction temperature for producing the phosphorus-containing flame retardant of the present disclosure according to the solvent method should be selected to promote the formation of pyrophosphonic acid ligands in the reaction product. For phosphonic acid, a reaction temperature of 105°C or higher is used. Without being bound to a particular theory, the reaction temperature is selected to produce pyrophosphonic acid ligands by dehydration reaction. In many embodiments, the metal or suitable metal compound and phosphonic acid are reacted at a temperature higher than 105°C, such as about 115°C or higher, about 120°C or higher, about 130°C or higher, about 140°C or higher, about 150°C or higher, about 160°C or higher, about 170°C or higher, about 180°C or higher, about 200°C or higher, about 220°C or higher, about 240°C or higher, about 260°C or higher, about 280°C or higher, or any range therebetween. The reaction temperature may be higher than those mentioned above, such as up to about 350° C., up to about 400° C., or higher, but typically does not reach or exceed the boiling point of the phosphonic acid. In many embodiments, the reaction temperature ranges from about 110° C. to about 350° C., about 115° C. to about 300° C., about 125° C. to about 280° C., or about 140° C. to about 260° C. The dehydration reaction forms water, which can potentially lead to an undesirable reverse (hydrolysis) reaction. Thus, in some embodiments, the reaction system is designed to facilitate removal, such as continuous removal, of water from the reaction mixture. For example, the reaction temperature may be selected above the boiling point of water to an extent necessary to boil off at least a portion or a desired amount (e.g., most, substantially all, or all) of the water from the reaction. Additional means, such as gas purging, vacuum, and / or other known means, may be used to facilitate removal of water from the reaction system.

[0075] For pyrophosphonic acid, a reaction temperature of 20° C. or higher is used. Because dehydration is not required for pyrophosphonic acid, the reaction temperature can be lower than that described above for phosphonic acid. In many embodiments, the metal or suitable metal compound and pyrophosphonic acid are reacted at a temperature higher than 20° C., such as about 40° C. or higher, about 60° C. or higher, about 80° C. or higher, about 100° C. or higher, about 140° C. or higher, about 180° C. or higher, about 200° C. or higher, or any range therebetween. The reaction temperature may be higher than those described above, such as up to about 300° C., up to about 400° C., or higher, but typically does not reach or exceed the boiling point of pyrophosphonic acid. In many embodiments, the reaction temperature ranges from about 25° C. to about 350° C., about 25° C. to about 280° C., about 30° C. to about 260° C., about 40° C. to about 260° C., or about 60° C. to about 240° C. For example, depending on the metal compound used to react with the pyrophosphonic acid, water may be produced from the reaction. As discussed above, in some embodiments, the reaction system is designed to facilitate removal, such as continuous removal, of water from the reaction. For example, the reaction temperature may be selected above the boiling point of water to an extent necessary to boil off at least a portion or a desired amount (e.g., most, substantially all, or all) of the water from the reaction. Additional means, such as gas purging, vacuum, and / or other known means, may be used to facilitate removal of water from the reaction system.

[0076] The reaction may be carried out under reduced pressure or vacuum, but this is not necessary.

[0077] In some embodiments of the solvent method, the solvent is a protic solvent (e.g., water) and the reaction system is designed to facilitate removal, such as continuous removal, of the protic solvent during heating of the reaction mixture. For example, the reaction temperature may be selected at or above the boiling point of the protic solvent to the extent necessary to boil off at least a portion or a desired amount (e.g., most, substantially all, or all) of the protic solvent during heating of the reaction mixture. In certain embodiments, the solvent is water and the reaction temperature is about 110° C. or higher, about 115° C. or higher, about 120° C. or higher, about 130° C. or higher, about 140° C. or higher, about 150° C. or higher, or about 160° C. or higher, such as the exemplary ranges described above. The reaction temperature may also be selected at or above the melting temperature of the phosphonic acid or pyrophosphonic acid, such as those further described herein.

[0078] Typically, the flame retardant product will precipitate from the reaction mixture such that the reaction is carried out for a sufficient time to achieve such precipitation. Generally, the time required to achieve at least substantial conversion to the flame retardant product based on the metal or suitable metal compound in the reaction mixture will depend on the reaction temperature, with higher temperatures generally resulting in shorter reaction times. In many cases, the heating or reaction is carried out at the reaction temperature for about 0.2 to about 36 hours, about 0.5 to about 30 hours, about 1 hour to about 24 hours, for example, about 1 hour to about 12 hours, about 1 hour to about 8 hours, or about 1 hour to about 5 hours, for about 0.1 to about 48 hours, such as, for example, about 1 hour to about 12 hours, about 1 hour to about 8 hours, or about 1 hour to about 5 hours, although other durations may be used.

[0079] The reaction mixture can be prepared in any manner suitable for combining or mixing (a) unsubstituted or alkyl or aryl substituted phosphonic or pyrophosphonic acid, (b) a solvent for the phosphonic or pyrophosphonic acid, and (c) a metal or suitable metal compound. For example, the components may be combined at the same time or at different times. In some embodiments, the metal or suitable metal compound (c) is added to a mixture, such as a solution, of the phosphonic or pyrophosphonic acid (a) and the solvent (b). The metal or suitable metal compound (c) can be added to the reaction mixture in one batch or in portions. Similarly, the phosphonic or pyrophosphonic acid (a), the solvent (b), or a mixture, such as a solution, of the phosphonic or pyrophosphonic acid (a) and the solvent (b) can be added to the reaction mixture in one batch or in portions.

[0080] In preparing the reaction mixture, the phosphonic or pyrophosphonic acid (a), the solvent (b), and the metal or suitable metal compound (c) may be combined at a preparation temperature below the reaction temperature. The reaction mixture is then heated to the reaction temperature. The preparation temperature may be selected, for example, to facilitate dissolution of the phosphonic or pyrophosphonic acid (a) in the solvent (b) or to otherwise form a homogeneous liquid or solution of the phosphonic or pyrophosphonic acid (a) and the solvent (b). At the preparation temperature and depending on the metal compound (c), the reaction mixture may form a solution, suspension, or slurry, such as a homogeneous or substantially homogeneous suspension or slurry. In some embodiments, such as at higher preparation temperatures, the reaction mixture may form a solution. In many cases, near or at the reaction temperature, the reaction mixture exists as a solution. In many embodiments, the preparation temperature is about 0° C. or higher, but often below 150° C., such as below 125° C., below 115° C., below 100° C., below 85° C., or below 65° C. For example, the preparation temperature may range from about 0° C. to about 65° C., or from about 15° C. to about 40° C. In some embodiments, the reaction mixture is prepared at room temperature (e.g., from about 15° C. to about 25° C.). In some embodiments, the solvent (b) is preheated to the preparation temperature and combined with the phosphonic acid or pyrophosphonic acid (a) and the metal or suitable metal compound (c). In some embodiments, the mixture of the solvent (b) and the phosphonic acid or pyrophosphonic acid (a) is preheated to the preparation temperature and combined with the metal or suitable metal compound (c).

[0081] The reaction mixture may alternatively be prepared at the reaction temperature. In other words, the reaction mixture is prepared by combining (a) phosphonic acid or pyrophosphonic acid, (b) a solvent for phosphonic acid or pyrophosphonic acid, and (c) a metal or suitable metal compound at the reaction temperature. For example, in some embodiments, preparing the reaction mixture includes preheating a mixture of solvent (b) and phosphonic acid or pyrophosphonic acid (a) to the reaction temperature and combining with metal or suitable metal compound (c).

[0082] In some embodiments where the reaction temperature is above the melting temperature of the phosphonic acid or pyrophosphonic acid and the desired conversion to the flame retardant product, e.g., complete or substantially complete conversion, is achieved, and residual phosphonic acid or pyrophosphonic acid is present in the product reaction mixture, the product reaction mixture is cooled to a temperature above or equal to the melting temperature of the residual phosphonic acid or pyrophosphonic acid to ensure that the phosphonic acid or pyrophosphonic acid remains in liquid form. This may be particularly useful in embodiments where a large amount of the solvent for the phosphonic acid or pyrophosphonic acid (i.e., component (b)) is boiled off as a result of heating, such that the remaining excess phosphonic acid or pyrophosphonic acid may have a greater tendency to come out of solution. The excess phosphonic acid or pyrophosphonic acid and solvent, if present in the product reaction mixture, may be removed by filtration / washing and optionally recovered. The recovered excess phosphonic acid or pyrophosphonic acid and / or solvent may be recycled, for example, by returning to the reactor where the metal or suitable metal compound (c) reacts with the phosphonic acid or pyrophosphonic acid (a). After conversion to the reaction product, a solvent for the phosphonic acid or pyrophosphonic acid, which may be but need not be the same as the solvent component (b), may be optionally added to dissolve or otherwise aid in the removal of excess phosphonic acid or pyrophosphonic acid. The phosphorus-containing flame retardant product is often separated by filtration, optionally followed by additional workup (e.g., washing, drying, sieving, etc.). The resulting phosphorus-containing flame retardant product is generally in the form of a powder or small particles and is easily processable, i.e., it does not require or require crushing, grinding, or other such physical processing before use. It should be appreciated that producing the phosphorus-containing flame retardant product "directly" as a powder or small particles allows for work-up of the reaction product, which may include processing the reaction product, such as isolating the flame retardant product (e.g., separating the flame retardant product from remaining solvent), for example, by filtering, sieving, washing, drying, and the like.

[0083] The solvent for the phosphonic acid or pyrophosphonic acid may be any solvent capable of dissolving the phosphonic acid or pyrophosphonic acid component, should be inert or substantially inert to the reaction of the phosphonic acid or pyrophosphonic acid with the metal or suitable metal compound, and may further be selected taking into consideration other reaction parameters, such as the preparation temperature and / or reaction temperature, or the type of metal or suitable metal compound, such as to prepare a homogeneous or substantially homogeneous reaction mixture. In some embodiments, the solvent may be a combination of solvents for the phosphonic acid or pyrophosphonic acid. In many cases, the phosphonic acid or pyrophosphonic acid is substantially or completely dissolved in the solvent. For example, the phosphonic acid or pyrophosphonic acid and the solvent may form a solution. In some embodiments, the phosphonic acid or pyrophosphonic acid may be partially dissolved, partially suspended or dispersed in the solvent. The type of solvent, the amount of solvent relative to the phosphonic acid or pyrophosphonic acid, and the mixing conditions can be selected to achieve a desired level of dissolution of the phosphonic acid, such as to obtain a high concentration of the phosphonic acid or pyrophosphonic acid in the mixture while maintaining the phosphonic acid or pyrophosphonic acid in solution. Often, the ratio of acid to solvent ranges from about 10:1 to 1:10, about 5:1 to 1:5, or about 3:1 to 1:3 by weight. In some embodiments where the acid is partially dissolved and partially suspended or dispersed in the solvent, the preparation or reaction temperature may be selected above the melting temperature of the acid to liquefy the acid suspended or dispersed in the solvent.

[0084] As mentioned above, depending on the reaction temperature and the boiling point of the solvent for the phosphonic acid or pyrophosphonic acid, at least a portion of the solvent may be boiled off from the reaction mixture during heating to or at the reaction temperature. In some embodiments, all, substantially all, or at least most of the solvent is boiled off from the reaction mixture during heating. The solvent may be high boiling (e.g., sulfolane or dimethylsulfoxide (DMSO)) or low boiling (e.g., chloroform or tetrahydrofuran (THF)). For example, in some embodiments, the solvent boils at a temperature below the reaction temperature, such that at least a portion of the solvent is boiled off during heating of the reaction mixture, e.g., all, substantially all, or most of the solvent is boiled off. The reaction temperature may be selected above the melting temperature of the phosphonic acid or pyrophosphonic acid to ensure that the phosphonic acid or pyrophosphonic acid remains in liquid form when the solvent is being boiled off. In this manner, the use of a larger excess of phosphonic acid or pyrophosphonic acid in the reaction mixture may allow the phosphonic acid or pyrophosphonic acid to serve as both a reactant and a solvent for the reaction.

[0085] In yet other embodiments, the solvent has a boiling point higher than the reaction temperature to ensure that it remains in the product reaction mixture from which the flame retardant product of the reaction can be separated as described herein, hi some embodiments, the reaction temperature is selected below the melting temperature of the phosphonic acid or pyrophosphonic acid.

[0086] Suitable solvents may be organic or inorganic. Examples of suitable solvents for phosphonic or pyrophosphonic acids include, but are not limited to, water, sulfones, sulfoxides, halogenated (e.g., chlorinated) hydrocarbons, aromatic hydrocarbons, and ethers. For example, in some embodiments, the solvent may be selected from water, sulfolane, dimethylsulfone, tetrahydrofuran (THF), dimethoxyethane (DME), 1,4-dioxane, dimethylsulfoxide (DMSO), 1,2-dichlorobenzene, chloroform, carbon tetrachloride, xylene, and mesitylene. In some embodiments, the solvent comprises water. In some embodiments, the solvent comprises an aqueous solution. In some embodiments, the reaction mixture is an aqueous reaction mixture.

[0087] The solvent may be protic or aprotic, hi many embodiments, the solvent for the pyrophosphonic acid is an aprotic solvent.

[0088] In some embodiments, the solvent (b) comprises a sulfone of formula R1R2SO2, where R1 and R2 are independently selected from the group consisting of C 1~6 Hydrocarbon groups, e.g., C 1~3 R1 and R2 taken together with S are selected from hydrocarbon groups or form a ring having 2, 3, 4, or 5 carbon atoms, the ring being unsubstituted or C 1~3 In some embodiments, R1 and R2 taken together with S form a di-, tri-, tetra-, or penta-methylene ring. In some embodiments, R1 and R2 are independently selected from the group consisting of C 1~6 In some embodiments, R1 or R2 is selected from C 1~6 alkyl and the other is C 1~3 In some embodiments, R and R are independently C 1~3The alkyl group may be branched or linear. In some embodiments, R1 and R2 are both methyl, both ethyl, or both propyl. In other embodiments, R1 or R2 is methyl and the other is ethyl or propyl. In other embodiments, R1 or R2 is ethyl and the other is propyl. In some embodiments, the sulfone is sulfolane.

[0089] Phosphonic acids have the formula

[0090] [ka]

[0091] In many embodiments, R is H, alkyl, aryl, alkylaryl, or arylalkyl. 1~12 Alkyl, C 6~10 Aryl, C 7~18 Alkylaryl or C 7~18 and arylalkyl, wherein the alkyl, aryl, alkylaryl, or arylalkyl is unsubstituted or is selected from the group consisting of halogen, hydroxyl, amino, C 1~4 Alkylamino, DiC 1~4 Alkylamino, C 1~4 Alkoxy, carboxy, or C 2~5 In some embodiments, the alkyl, aryl, alkylaryl, or arylalkyl is an unsubstituted C 1~12 Alkyl, C6 aryl, C 7~10 Alkylaryl or C 7~10 Arylalkyl, e.g., C 1~6 Alkyl, phenyl, or C 7~9 In some embodiments, R is a substituted or unsubstituted C 1~6 Alkyl, C6 aryl, C 7~10 Alkylaryl or C 7~12 Arylalkyl, e.g., C1~4 Alkyl, C6 aryl, C 7~9 Alkylaryl or C 7~10 In many embodiments, R is an unsubstituted C 1~12 Alkyl, e.g., C 1~6 In many embodiments, lower alkyl phosphonic acids are used, such as methyl-, ethyl-, propyl-, isopropyl-, butyl-, and t-butyl-.

[0092] Pyrophosphonic acid has the formula

[0093] [ka]

[0094] wherein R is as defined above.

[0095] The process for preparing the phosphorus-containing flame retardant may use more than one phosphonic acid, more than one pyrophosphonic acid, or a combination of phosphonic acid and pyrophosphonic acid. In some embodiments, the phosphonic acid or pyrophosphonic acid is generated in situ. For example, preparing the reaction mixture may include preparing the phosphonic acid or pyrophosphonic acid, such as by hydrolysis of a higher oligomeric phosphonic acid and / or cyclic phosphonic anhydride starting material.

[0096] As used herein, a "suitable metal compound" or the like is a compound of the formula M p (+)y X qwhere M is a metal that forms a 2+ or 3+ cation, and X is any anion that provides a compound in equilibrium with the metal M. Suitable examples for X include, but are not limited to, anions that form oxides, halides, alkoxides, hydroxides, carbonates, carboxylates, and phosphonates with the metal M. The values ​​of p and q provide a charge-balanced metal compound, e.g., alumina Al2O3. In some embodiments, unsubstituted metal M is used as described herein. Examples of suitable metals (M) include, but are not limited to, Al, Ga, Sb, Fe, Co, B, Bi, Mg, Ca, and Zn. In some embodiments, M is selected from Al, Fe, Mg, Zn, and Ca.

[0097] Suitable metal compounds include compounds having a metal-oxygen bond, a metal-nitrogen bond, a metal-halogen bond, a metal-hydrogen bond, a metal-phosphorus bond, a metal-sulfur bond, a metal-boron bond, and the like, such as oxides, halides, alkoxides, hydroxides, carboxylates, carbonates, phosphonates, phosphinates, phosphonites, phosphates, phosphites, nitrates, nitrites, borates, hydrides, sulfonates, sulfates, sulfides, and the like, such as oxides, hydroxides, halides, or alkoxides of Al, Ga, Sb, Fe, Co, B, Bi, Mg, Ca, and Zn.

[0098] In some embodiments, the metal M of the metal or suitable metal compound is aluminum or iron. In some embodiments, suitable metal compounds are selected from aluminum halides, oxides, hydroxides, alkoxides, carbonates, carboxylic acids, and phosphonates. In some embodiments, suitable metal compounds are selected from aluminum halides, oxides, hydroxides, and alkoxides. In some embodiments, suitable metal compounds are selected from alumina, aluminum trichloride, aluminum trihydroxide, aluminum isopropoxide, aluminum carbonate, and aluminum acetate. In other embodiments, suitable metal compounds are selected from iron halides, oxides, alkoxides, carbonates, and acetates. In some embodiments, suitable metal compounds are selected from iron(III) oxide, iron(III) chloride, iron(III) isopropoxide, and iron(III) acetate.

[0099] In some embodiments, the suitable metal compound is a metal phosphonate salt. The metal in the metal phosphonate salt may be a metal M, as described herein. In some embodiments, the metal phosphonate salt is prepared from the reaction of an initial metal compound and a phosphonic acid with a solvent for the phosphonic acid (e.g., water). The initial metal compound may be a compound according to the suitable metal compounds described herein. In some embodiments, the initial metal compound and the phosphonic acid are reacted at a temperature at or about room temperature, or at a temperature ranging from about 0 to about 20° C. The resulting metal phosphonate salt may then be used as a suitable metal compound. For example, a phosphonic acid, such as one or more alkyl phosphonic acids described above, and a solvent (e.g., water) may be stirred to form a homogeneous solution. The solution may be cooled, for example, to about 0 to about 20° C., and an initial metal compound, such as a metal oxide, halide, alkoxide, or hydroxide, is added to react with the phosphonic acid. The metal phosphonate salt is formed and then used as a suitable metal compound for preparing a phosphorus-containing flame retardant.

[0100] Although the preparation process may result in a mixture of phosphorus-containing flame retardant compounds, in many embodiments the process produces the phosphorus-containing flame retardant product as one, or primarily one, compound at high conversions, such as at least 70%, 80%, 85%, 90%, 95%, 98%, or higher, or any range therebetween, based on the metal or metal compound, in contrast to the mixtures of compounds obtained by prior art processes involving heat treatment of metal phosphonate salts, such as those disclosed in U.S. Pat. No. 9,745,449.

[0101] Reactions following the solvent method are generally shown

[0102] [ka]

[0103] [In the formula, M (+)y is a metal cation, where (+)y represents the charge of the cation, M is a metal, y is 2 or 3; X is an anionic ligand or ligands attached to the metal, and the stoichiometry of M and X (i.e., p and q) provides a metal compound with a charge in equilibrium; R is H, alkyl, aryl, alkylaryl, or arylalkyl (as described herein); a, b, and c represent the ratio of the corresponding components to each other in the reaction product, satisfying the charge balance equation 2(a)+c=b(y), where c is not zero. In many cases, a is 0, 1, or 2 (e.g., 0 or 1), b is 1 to 4, e.g., 1 or 2, and c is 1 or 2, and the compound is charged in equilibrium. In certain embodiments, R as described herein is methyl, ethyl, propyl, isopropyl, or butyl, and M is Al, Fe, Zn, or Ca. In further embodiments, X is oxygen, hydroxy, alkoxy, or halogen.

[0104] The general reaction scheme using pyrophosphonic acid is:

[0105] [ka]

[0106] [In the formula, R, M, X, p, q, y, a, b, and c are as defined above].

[0107] As discussed above, and as is typical for inorganic coordination compounds, the formulas for the reaction products are empirical or idealized such that the products may be coordination polymers, complex salts, salts in which certain valences are shared, etc. In many embodiments, the reaction products described above represent the monomer units (i.e., coordination entities) of a coordination polymer, whereby the extended coordination polymer structure forms the phosphorus-containing flame retardants of the present disclosure.

[0108] In certain embodiments, y is 2 (i.e., M (+)y is a dicationic metal), a is 0, b is 1, and c is 2. In certain embodiments, the dicationic metal M is Mg, Ca, or Zn. In other embodiments, y is 3 (i.e., M (+)y is a tricationic metal), a is 1, b is 1, and c is 1. In certain embodiments, the tricationic metal M is selected from Al, Ga, Sb, Fe, Co, B, and Bi. In certain embodiments, the tricationic metal M is Al, Fe, Ga, Sb, or B. In certain embodiments, M is aluminum (i.e., the reaction product is produced using aluminum or one or more aluminum compounds such as those described herein), or iron (i.e., the reaction product is produced using iron or one or more iron compounds such as those described herein).

[0109] In one example, the empirical formula:

[0110] [ka]

[0111] A phosphorus-containing flame retardant compound having the formula:

[0112] As shown herein, the absence of subscripts a, b, and c in the empirical formula indicates that the subscripts are each 1, signifying a 1:1:1 ratio of dianionic pyrophosphonate ligand, metal atom, and monoanionic pyrophosphonate ligand.

[0113] Often, in many embodiments, the phosphorus-containing flame retardant compound that is an extended coordination polymer as described herein constitutes all, substantially all, or at least a majority of the phosphorus-containing flame retardant product, such as at least 75%, 85%, 90%, 95%, 98%, or more, or any range therebetween, by weight of the flame retardant product.

[0114] The product reaction mixture formed from the reaction, often present as a slurry, may be combined with an additional solvent, which may be the same or different solvent as that used in the reaction mixture. The additional solvent may be selected, for example, from those described herein with respect to the solvent components for phosphonic acid or pyrophosphonic acid. The additional solvent / slurry mixture may be agitated as desired to break up any agglomerates that may have formed. The solid product may be separated by filtration, optionally washed, and dried to obtain the product in the form of a powder or small particles. In some cases, the product may be sieved to refine the particle size.

[0115] The reaction may optionally be accelerated with a seeding material. For example, the use of a seeding material may reduce the time to achieve conversion to the phosphorus-containing flame retardant product and may increase the consistency in the physical properties of the product. Thus, in some embodiments, the reaction mixture further comprises a seeding material. Often, the seeding material is added to the reaction mixture upon or after heating to the reaction temperature. In many embodiments, the seeding material is added before conversion to the flame retardant product and / or precipitation of the flame retardant product occurs. In some embodiments, the seeding material comprises a phosphorus-containing flame retardant produced according to the methods described herein. The seeding material may be selected or refined to have a desired particle size.

[0116] In some embodiments of the solvent process, the preferred metal compound is alumina, and the phosphorus-containing flame retardant product is:

[0117] [ka]

[0118] It is produced as follows.

[0119] In one example, C1 to C 12A reaction mixture containing a phosphonic acid, such as an alkyl phosphonic acid (e.g., methyl, ethyl, propyl, iso-propyl, butyl, or t-butyl phosphonic acid), a solvent for the phosphonic acid, such as water, and an oxide, hydroxide, halide, alkoxide, carbonate, or carboxylate of Al, such as alumina, aluminum trichloride, aluminum trihydroxide, aluminum isopropoxide, aluminum carbonate, or aluminum acetate, is heated to a reaction temperature as described herein, such as about 115°C or higher, about 125°C or higher, about 150°C or higher, or about 165°C or higher. Typically, a slurry forms as the reaction proceeds, and the solid phosphorus-containing flame retardant product may be separated by filtration to obtain the product in the form of a powder or small particles. Additional workup of the product reaction mixture, such as cooling the product reaction mixture above or above the melting point of the excess phosphonic acid and combining with an additional solvent, such as water, as described herein, may be performed prior to isolating the solid product. The additional solvent / slurry mixture may optionally be agitated as described above. The solid phosphorus-containing flame retardant product may be isolated by filtration, optionally washed with additional solvent, and dried to obtain a product in the form of a powder or small particles. The flame retardant product may be represented by the following empirical formula:

[0120] [ka]

[0121] In a further example, the example described immediately above is carried out using iron or a suitable iron compound such as an iron halide, oxide, alkoxide, carbonate, or acetate, for example, iron(III) oxide, iron(III) chloride, iron(III) isopropoxide, or iron(III) acetate. The flame retardant product may be represented by the following empirical formula:

[0122] [ka]

[0123] It contains phosphorus and iron in a ratio of 4:1 according to the

[0124] In many cases, the compound of the empirical formula above (which in many embodiments is an extended coordination polymer as described herein) constitutes all, substantially all, or at least a majority of the phosphorus-containing flame retardant product, such as at least 75%, 85%, 90%, 95%, 98%, or more, or any range therebetween, by weight of the flame retardant product.

[0125] In a further embodiment, suitable metal compounds have the formula

[0126] [ka]

[0127] [In the formula, R and M are as defined above, and M (+)y is a metal cation, where (+)y represents the charge formally assigned to the cation, and p is 2 or 3 and y is 2 or 3, such that the metal phosphonate salt is charge balanced (i.e., p=y). The metal phosphonate salts may be prepared according to methods known in the art.

[0128] In one example, a phosphonic acid, such as an alkyl phosphonic acid (e.g., methyl, ethyl, propyl, iso-propyl, butyl, or t-butyl phosphonic acid), is combined with water (e.g., about 1:1 by mass), stirred, and cooled below room temperature (e.g., cooled to 10° C. or less, such as about 0° C.). An initial metal compound is added to the phosphonic acid and water mixture to form a metal phosphonate salt. The metal phosphonate salt is then used as a suitable metal compound to produce a phosphorus-containing flame retardant product in the form of a powder or small particles. In an embodiment that includes an aluminum phosphonate salt as a suitable metal compound, the flame retardant product may be represented by the following empirical formula:

[0129] [ka]

[0130] It contains phosphorus and aluminum in a phosphorus to aluminum ratio of 4:1 according to: The compound of empirical formula (which in many embodiments is an extended coordination polymer as described herein) typically constitutes all, substantially all, or at least a majority of the flame retardant product, such as at least 75%, 85%, 90%, 95%, 98%, or more, or any range therebetween, by weight of the flame retardant product.

[0131] Preparation of phosphorus-containing flame retardants by the melt-state method Another suitable method for preparing the phosphorus-containing flame retardant of the present disclosure comprises reacting a metal or suitable metal compound with a stoichiometric excess of unsubstituted or alkyl- or aryl-substituted phosphonic acid. The reaction temperature is 105° C. or higher, the phosphonic acid is in a molten state at the reaction temperature, and the molar ratio of phosphonic acid to metal or suitable metal compound in the reaction mixture is greater than 4:1. In the reaction, the metal is oxidized to form a phosphonic acid of formula M (+)y where M is a metal, (+)y represents the charge of the metal cation, and y is 2 or 3. Suitable metal compounds are represented by the formula M p (+)y X q where M is a metal, (+)y represents the charge of the metal cation, y is 2 or 3, X is an anion, and the values ​​of p and q provide a charge balanced metal compound.

[0132] In another embodiment, the phosphorus-containing flame retardant of empirical formula (I) may be prepared by reacting a metal or suitable metal compound with a stoichiometric excess of unsubstituted or alkyl- or aryl-substituted pyrophosphonic acid, the pyrophosphonic acid being in a molten state at the reaction temperature, and the molar ratio of pyrophosphonic acid to the metal or suitable metal compound in the reaction mixture being greater than 2:1.

[0133] As used herein, a "stoichiometric excess" of an unsubstituted or alkyl- or aryl-substituted phosphonic acid or pyrophosphonic acid relative to a metal or suitable metal compound refers to an amount of phosphonic acid or pyrophosphonic acid that exceeds the amount stoichiometrically required for the reaction of the metal or suitable metal compound with the phosphonic acid or pyrophosphonic acid. The stoichiometric excess is typically expressed in terms of the molar ratio of phosphonic acid or pyrophosphonic acid to the metal or suitable metal compound in the reaction mixture, as described herein.

[0134] The unsubstituted or alkyl or aryl substituted phosphonic or pyrophosphonic acid, used in stoichiometric excess as described herein, acts as a reagent and solvent for the reaction. The reaction product typically forms as a slurry when the resulting phosphorus-containing flame retardant product precipitates from the reaction mixture. The excess phosphonic or pyrophosphonic acid remaining after the reaction can be removed by filtration and / or washing, for example, with water, along with any by-products that may result. In many embodiments, a substantially pure flame retardant material is produced, for example a flame retardant that contains essentially a single compound having flame retardant activity, or essentially a mixture of active compounds. The conversion rate based on the metal or metal compound is typically high, and the product can be easily separated and, if desired, optionally further purified.

[0135] Typically, the molar ratio of phosphonic acid to metal or suitable metal compound in the reaction mixture is 5:1 or more, such as about 6:1 or more, about 8:1 or more, or about 10:1 or more. A larger molar excess of phosphonic acid to metal or suitable metal compound may be used in the reaction mixture, such as about 12:1 or more, about 15:1 or more, about 20:1 or more, about 25:1 or more, about 30:1 or more, or any range therebetween. A larger molar excess of phosphonic acid to metal or suitable metal compound may be used. For example, the molar ratio may be up to about 50:1, up to about 100:1, up to about 300:1, up to about 500:1, or any range therebetween. However, as will be appreciated, process efficiency may be compromised at certain large molar excesses, for example, product precipitation from the reaction mixture may be hindered. In many embodiments, the molar ratio ranges from about 8:1, from about 10:1, from about 12:1, or from about 16:1 to about 100:1, or to about 50:1, such as from about 10:1, from about 15:1, or from about 20:1 to about 50:1, or to about 40:1.

[0136] Typically, for pyrophosphonic acid, the molar ratio of pyrophosphonic acid to metal or suitable metal compound in the reaction mixture is 3:1 or more, such as about 4:1 or more, about 6:1 or more, or about 8:1 or more. Often, a larger molar excess of pyrophosphonic acid to metal or suitable metal compound is used in the reaction mixture, such as about 10:1 or more, about 12:1 or more, about 15:1 or more, about 18:1 or more, about 20:1 or more, or any range therebetween. A larger molar excess of pyrophosphonic acid to metal or suitable metal compound may also be used. For example, the molar ratio may be up to about 30:1, up to about 50:1, up to about 100:1, up to about 250:1, or any range therebetween. However, as will be appreciated, process efficiency may be compromised at certain large molar excesses, for example, product precipitation from the reaction mixture may be hindered. In many embodiments, the molar ratio ranges from about 4:1, about 5:1, about 6:1, or about 8:1 to about 50:1, or to about 25:1, such as from about 5:1, about 8:1, or about 10:1 to about 25:1, or to about 20:1.

[0137] The reaction temperature for producing phosphorus-containing flame retardants according to the molten state method should be selected so that phosphonic acid or pyrophosphonic acid is in a molten state at the reaction temperature.For example, phosphonic acid and pyrophosphonic acid (e.g., alkyl-substituted phosphonic acid or pyrophosphonic acid) are often solid at room temperature (e.g., methylphosphonic acid melts at about 105°C, and ethylphosphonic acid melts at about 62°C), and therefore, heating phosphonic acid or pyrophosphonic acid to obtain a liquefied physical state (i.e., a molten state) is generally suitable for forming a consistent reaction mixture.As will be recognized by those skilled in the art, the desired reaction temperature at which phosphonic acid or pyrophosphonic acid is in a molten state may vary depending on the reagents and thermodynamic conditions selected.

[0138] The reaction temperature should also be selected to promote the formation of pyrophosphonic acid ligands in the reaction product. For phosphonic acids, a reaction temperature of 105° C. or higher is used. Without being bound to a particular theory, the reaction temperature is selected to produce pyrophosphonic acid ligands by a dehydration reaction. In many embodiments, the metal or suitable metal compound and phosphonic acid are reacted at a temperature higher than 105° C., such as about 115° C. or higher, about 120° C. or higher, about 130° C. or higher, about 140° C. or higher, about 150° C. or higher, about 160° C. or higher, about 170° C. or higher, about 180° C. or higher, about 200° C. or higher, about 220° C. or higher, about 240° C. or higher, about 260° C. or higher, about 280° C. or higher, or any range therebetween. The reaction temperature may be higher than those mentioned above, such as up to about 350° C., up to about 400° C., or higher, but typically does not reach or exceed the boiling point of the phosphonic acid. For example, the reaction temperature may range from about 150° C. to about 300° C., such as from about 150° C. to about 280° C., from about 160° C. to about 260° C., or from about 160° C. to about 240° C. In many embodiments, the reaction temperature ranges from about 110° C. to about 350° C., from about 115° C. to about 300° C., from about 125° C. to about 280° C., or from about 140° C. to about 260° C. The dehydration reaction forms water, which can potentially lead to an undesirable reverse (hydrolysis) reaction. Thus, in some embodiments, the reaction system is designed to facilitate removal, such as continuous removal, of water from the reaction. For example, the reaction temperature may be selected above the boiling point of water to an extent necessary to boil off at least a portion or a desired amount (e.g., most, substantially all, or all) of the water from the reaction. Additional means, such as gas purging, vacuum, and / or other known means, may be used to facilitate removal of water from the reaction system.

[0139] Since dehydration is not required for pyrophosphonic acid, the reaction temperature for pyrophosphonic acid may be lower than that described above for phosphonic acid. In general, the limiting criterion for choosing a suitable reaction temperature when using pyrophosphonic acid is the requirement that the pyrophosphonic acid be in a molten state at the reaction temperature. In many cases, the metal or a suitable metal compound and the pyrophosphonic acid are reacted at a temperature of 20° C. or higher. In many embodiments, the metal or a suitable metal compound and the pyrophosphonic acid are reacted at a temperature higher than 20° C., such as about 40° C. or higher, about 60° C. or higher, about 80° C. or higher, about 100° C. or higher, about 140° C. or higher, about 180° C. or higher, about 200° C. or higher, or any range therebetween. The reaction temperature may be higher than those described above, such as up to about 300° C., up to about 400° C., or higher, but typically does not reach or exceed the boiling point of the pyrophosphonic acid. In many embodiments, the reaction temperature ranges from about 25° C. to about 350° C., about 25° C. to about 280° C., about 30° C. to about 260° C., about 40° C. to about 260° C., about 60° C. to about 260° C., about 80° C. to about 240° C., about 100° C. to about 240° C., about 110° C. to about 240° C., or about 120° C. to about 240° C. For example, depending on the metal compound used to react with the pyrophosphonic acid, water may be produced from the reaction. As mentioned above, in some embodiments, the reaction system is designed to facilitate the removal, such as the continuous removal, of water from the reaction. For example, the reaction temperature may be selected above the boiling point of water to an extent necessary to boil off at least a portion or a desired amount (e.g., most, substantially all, or all) of the water from the reaction. Additional means, such as gas purging, vacuum, and / or other known means, may be used to facilitate the removal of water from the reaction system.

[0140] The reaction may be carried out under reduced pressure or vacuum, but this is not necessary.

[0141] Typically, as the reaction proceeds, the product forms as a slurry when the phosphorus-containing flame retardant product precipitates from the product reaction mixture. Thus, the reaction is typically carried out for a time sufficient to achieve such precipitation. In general, the time required to achieve at least substantial conversion to a flame retardant product based on the metal or suitable metal compound will depend on the reaction temperature, with higher temperatures generally resulting in shorter reaction times. In many embodiments, the metal or suitable metal compound and the phosphonic acid or pyrophosphonic acid are heated at the reaction temperature for about 0.2 to about 36 hours, about 0.5 to about 30 hours, about 1 hour to about 24 hours, for example, about 0.1 to about 48 hours, such as about 1 hour to about 12 hours, about 1 hour to about 8 hours, or about 2 hours to about 5 hours, although other durations may be used.

[0142] The metal or suitable metal compound and the molar excess of phosphonic acid or pyrophosphonic acid can be combined in any manner suitable for forming a reaction mixture. For example, the phosphonic acid or pyrophosphonic acid and the metal or metal compound may be mixed (e.g., stirred) together to form a homogeneous reaction mixture, etc. In some embodiments, the metal or suitable metal compound is added to the phosphonic acid or pyrophosphonic acid that has been preheated to the reaction temperature. In some embodiments, the phosphonic acid or pyrophosphonic acid is preheated, such as under nitrogen atmosphere or reduced pressure / vacuum, and stirred upon melting. In further embodiments, the metal or metal compound is added as quickly as possible without causing a large change in reaction temperature due to the exothermic nature of the reaction. In some embodiments, the phosphonic acid or pyrophosphonic acid and the metal or suitable metal compound are combined without preheating the phosphonic acid or without sufficient heating to liquefy the phosphonic acid or pyrophosphonic acid, and the components are subsequently heated to the reaction temperature. The entire amount of the metal or suitable metal compound or the phosphonic acid or pyrophosphonic acid can be added to the reaction in one lump or in portions. Since the phosphonic acid or pyrophosphonic acid used in molar excess acts as both a reagent and a solvent, no additional solvent is required, although additional solvent may be used if desired. In some embodiments, additional solvent is used when using a molar ratio of phosphonic acid or pyrophosphonic acid to metal or suitable metal compound at or near the lower bound of the molar ratios disclosed herein.

[0143] In some embodiments, after the desired conversion to the flame retardant product, e.g., complete or substantially complete conversion, is achieved, the product reaction mixture is cooled to a temperature above or equal to the melting temperature of the excess phosphonic acid or pyrophosphonic acid, so that the excess phosphonic acid or pyrophosphonic acid is kept in a liquefied state. The excess phosphonic acid or pyrophosphonic acid can be removed by filtration / washing and optionally recovered. The recovered excess phosphonic acid or pyrophosphonic acid may be recycled, for example, by returning it to the reactor where the metal or suitable metal compound reacts with the phosphonic acid or pyrophosphonic acid. After conversion to the reaction product, a solvent, e.g., water, alcohol, and / or another suitable (e.g., polar) liquid, may be optionally added to dissolve or otherwise aid in the removal of the excess phosphonic acid or pyrophosphonic acid. The phosphorus-containing flame retardant product is often separated by filtration, optionally followed by additional workup (e.g., washing, drying, sieving, etc.). The resulting phosphorus-containing flame retardant product, which is generally in the form of a powder or small particles, is easily processable, i.e., no crushing, grinding, or other such physical processing is required or required prior to use. It should be appreciated that producing the flame retardant material "directly" as a powder or small particles allows for work-up of the reaction product, which may include processing the reaction product by, for example, filtering, sieving, washing, and drying, such as separating the flame retardant product (e.g., separating the flame retardant product from excess phosphonic acid or pyrophosphonic acid or remaining solvent). After the reaction, the resulting product reaction mixture, often a slurry, may be cooled to or slightly above the melting temperature of the excess phosphonic acid, and the slurry may be combined with water. The water / slurry mixture may be agitated as necessary to break up any large agglomerates that may have formed. The solid product may be separated by filtration, optionally washed with water, and dried to obtain the product in the form of a powder or small particles. In some cases, the product may be sieved to refine the particle size.

[0144] The phosphonic acid or pyrophosphonic acid used to prepare the phosphorus-containing flame retardant may be a phosphonic acid or pyrophosphonic acid as described above. The process may use more than one phosphonic acid, more than one pyrophosphonic acid, or a combination of phosphonic acid and pyrophosphonic acid. In some embodiments, the phosphonic acid or pyrophosphonic acid is generated in situ. For example, preparing the reaction mixture may include preparing the phosphonic acid or pyrophosphonic acid, such as by hydrolysis of a higher oligomeric phosphonic acid and / or cyclic phosphonic anhydride starting material.

[0145] Suitable metals and metal compounds for the reaction are described above.

[0146] Although the preparation process may result in a mixture of phosphorus-containing flame retardant compounds, in many embodiments the process produces the phosphorus-containing flame retardant product as one, or primarily one, compound at high conversions, such as at least 70%, 80%, 85%, 90%, 95%, 98%, or higher, or any range therebetween, based on the metal or metal compound, in contrast to the mixtures of compounds obtained by prior art processes involving heat treatment of metal phosphonate salts, such as those disclosed in U.S. Pat. No. 9,745,449.

[0147] The reaction according to the molten state method is generally shown

[0148] [ka]

[0149] [In the formula, M (+)yis a metal cation, where (+)y represents the charge of the cation, M is a metal, y is 2 or 3; X is an anionic ligand or ligands attached to the metal, and the stoichiometry of M and X (i.e., p and q) provides a metal compound with a charge in equilibrium; R is H, alkyl, aryl, alkylaryl, or arylalkyl (as described herein); a, b, and c represent the ratio of the corresponding components to each other in the reaction product, satisfying the charge balance equation 2(a)+c=b(y), where c is not zero. In many cases, a is 0, 1, or 2 (e.g., 0 or 1), b is 1 to 4, e.g., 1 or 2, and c is 1 or 2, and the compound is charged in equilibrium. In certain embodiments, R as described herein is methyl, ethyl, propyl, isopropyl, or butyl, and M is Al, Fe, Zn, or Ca. In further embodiments, X is oxygen, hydroxy, alkoxy, or halogen.

[0150] The general reaction scheme using pyrophosphonic acid is:

[0151] [ka]

[0152] [In the formula, R, M, X, p, q, y, a, b, and c are as defined above].

[0153] As discussed above, and as is typical for inorganic coordination compounds, the formulas for the reaction products are empirical or idealized such that the products may be coordination polymers, complex salts, salts in which certain valences are shared, etc. In many embodiments, the reaction products described above represent the monomer units (i.e., coordination entities) of a coordination polymer, whereby the extended coordination polymer structure forms the phosphorus-containing flame retardants of the present disclosure.

[0154] In certain embodiments, y is 2 (i.e., M (+)yis a dicationic metal), a is 0, b is 1, and c is 2. In certain embodiments, the dicationic metal M is Mg, Ca, or Zn. In other embodiments, y is 3 (i.e., M (+)y is a tricationic metal), a is 1, b is 1, and c is 1. In certain embodiments, the tricationic metal M is selected from Al, Ga, Sb, Fe, Co, B, and Bi. In certain embodiments, the tricationic metal M is Al, Fe, Ga, Sb, or B. In certain embodiments, M is aluminum (i.e., the reaction product is produced using aluminum or one or more aluminum compounds such as those described herein), or iron (i.e., the reaction product is produced using iron or one or more iron compounds such as those described herein).

[0155] In one example, the empirical formula:

[0156] [ka]

[0157] A phosphorus-containing flame retardant compound having the formula:

[0158] As noted above, the absence of subscripts a, b, and c in the empirical formula indicates that each subscript is 1, signifying a 1:1:1 ratio of dianionic pyrophosphonate ligand, metal atom, and monoanionic pyrophosphonate ligand.

[0159] Often, in many embodiments, the phosphorus-containing flame retardant compound that is an extended coordination polymer as described herein constitutes all, substantially all, or at least a majority of the phosphorus-containing flame retardant product, such as at least 75%, 85%, 90%, 95%, 98%, or more, or any range therebetween, by weight of the flame retardant product.

[0160] The product reaction mixture formed from the reaction, often present as a slurry, may be combined with a liquid (e.g., water) and agitated as desired to break up any agglomerates that may have formed. The solid product may be separated by filtration, optionally washed, and dried to obtain the product in the form of a powder or small particles. In some cases, the product may be sieved to refine particle size.

[0161] The reaction may optionally be accelerated with a seeding material. For example, the use of a seeding material may reduce the time to achieve conversion to the phosphorus-containing flame retardant product and may increase the consistency in the physical properties of the product. Thus, in some embodiments, the reaction mixture further comprises a seeding material. Often, the seeding material is added to the reaction mixture upon or after heating to the reaction temperature. In some embodiments, the seeding material comprises a phosphorus-containing flame retardant produced according to the methods described herein. The seeding material may be selected or refined to have a desired particle size.

[0162] In some embodiments of the molten state process, the preferred metal compound is alumina and the flame retardant material is

[0163] [ka]

[0164] It is produced as follows.

[0165] In one example, C1 to C 12A phosphonic acid, such as an alkyl phosphonic acid (e.g., methyl, ethyl, propyl, iso-propyl, butyl, or t-butyl phosphonic acid), upon melting, is heated with stirring (e.g., under nitrogen) to or above its melting point of 105° C., such as 115° C., 125° C., 140° C., 150° C., 160° C., 180° C., 200° C., 220° C., or 240° C. or higher. An oxide, hydroxide, halide, alkoxide, carbonate, or carboxylate of Al, such as alumina, aluminum trichloride, aluminum trihydroxide, aluminum isopropoxide, aluminum carbonate, or aluminum acetate, is added with stirring in a stoichiometric excess of phosphonic acid, such as in a molar ratio of phosphonic acid to metal compound as described herein, e.g., 5:1 or more, 10:1 or more, or 15:1 or more. Typically, as the reaction proceeds, a slurry forms and the solid flame retardant product may be isolated, such as by filtration, washing, etc., to obtain the product in the form of a powder or small particles. Additional work-up on the product reaction mixture, such as cooling the product reaction mixture above or above the melting point of the excess phosphonic acid and combining with a liquid, such as water, and optionally agitating as described above, may be performed prior to isolating the solid product. The solid flame retardant product may be isolated by filtration and, optionally, washed with additional solvent and dried to obtain the product in the form of a powder or small particles. The flame retardant product may be represented by the empirical formula:

[0166] [ka]

[0167] In a further example, the example described immediately above is carried out using iron or a suitable iron compound such as an iron halide, oxide, alkoxide, carbonate, or acetate, for example, iron(III) oxide, iron(III) chloride, iron(III) isopropoxide, or iron(III) acetate. The flame retardant product may be represented by the following empirical formula:

[0168] [ka]

[0169] It contains phosphorus and iron in a ratio of 4:1 according to the

[0170] In many cases, the compound of the empirical formula above (which in many embodiments is an extended coordination polymer as described herein) constitutes all, substantially all, or at least a majority of the phosphorus-containing flame retardant product, such as at least 75%, 85%, 90%, 95%, 98%, or more, or any range therebetween, by weight of the flame retardant product.

[0171] In a further example where the suitable metal compound is a metal phosphonate salt, the metal phosphonate salt is prepared by mixing a phosphonic acid, such as an alkyl phosphonic acid, e.g., methyl, ethyl, propyl, iso-propyl, butyl, or t-butyl phosphonic acid, and a solvent (e.g., water) to form a homogeneous solution. For example, any convenient ratio of water to phosphonic acid may be used, e.g., 10:1 to 1:10 by weight, such as 5:1 to 1:5 by weight, or 2:1 to 1:2 by weight. The solution may be cooled, e.g., to a range of about 0 to about 20° C., and an initial metal compound, such as a metal oxide, halide, alkoxide, or hydroxide, is added to react with the phosphonic acid. The metal phosphonate salt is formed and then used as the suitable metal compound. For example, a molar excess of phosphonic acid as described herein (such as in a 5:1 molar ratio of phosphonic acid to metal phosphonate salt) is preheated to a molten state and reacted with the metal phosphonate salt to form a phosphorus-containing flame retardant product. In embodiments that include an aluminum phosphonate salt as a suitable metal compound, the flame retardant product has the empirical formula:

[0172] [ka]

[0173] It contains phosphorus and aluminum in a phosphorus to aluminum ratio of 4:1 according to: The compound of empirical formula (which in many embodiments is an extended coordination polymer as described herein) typically constitutes all, substantially all, or at least a majority of the flame retardant product, such as at least 75%, 85%, 90%, 95%, 98%, or more, or any range therebetween, by weight of the flame retardant product.

[0174] Preparation of Flame Retardant and Synergist Additive Composition The present invention is not limited by any particular method of mixing the components (A), (B), (C), (D) and (E) of the flame retardant and synergist additive composition disclosed herein. For example, at least one phosphorus-containing flame retardant (A) and at least one metal hypophosphite (B) may be mixed / blended, optionally with any one or combination of at least one heat stabilizer (C), at least one additional synergist, and / or additional flame retardant (D), and at least one additional additive (E), by conventional mixing techniques such as tumbling mixing, convection mixing, fluidized bed mixing, high shear mixing, etc. Conventional processing agents, such as dispersants, antistatic agents, binders, coupling agents, etc., may be used.

[0175] Preparation of flame retardant thermoplastic compositions The present invention is not limited by any particular method of blending the components of the flame retardant thermoplastic composition disclosed herein. Suitable compounding and blending techniques known in the art may be used. For example, one method includes blending the thermoplastic polymer and additives in powder or granular form and melt-mixing the blend (e.g., using a twin-screw extruder). The thermoplastic polymer, flame retardant, synergist, and other additives are typically pre-dried before melt-mixing. The extruded blend may be comminuted into granular pellets or other suitable shapes by standard techniques. Other melt-mixing process equipment, such as a kneader mixer or bowl mixer, may be used to compound the flame retardant additive and any additional mixture components with the thermoplastic polymer. In either case, generally suitable equipment temperatures may range from about 200°C to 330°C, depending on the particular type of thermoplastic material selected.

[0176] The flame retardant thermoplastic composition can be molded in any equipment suitable for such purposes, for example, in an injection molding machine. After pelletization, the granular pellets are typically re-dried before being molded in an injection molding machine suitable for such purposes. In most cases, the process temperature ranges from about 200°C to 280°C, depending on the molding characteristics of the specific thermoplastic polymer, the loading level of additives and / or reinforcing fillers, and other factors such as the thickness of the cavity and gate size of the mold. Those skilled in the art can make suitable adjustments in the molding process to accommodate differences in composition or equipment.

[0177] Further non-limiting disclosure is provided in the Examples below. EXAMPLES

[0178] The combination of flame retardants and metal hypophosphite synergists disclosed herein was evaluated in a polyamide-6,6 thermoplastic composition (Formulation 1), as well as two comparative formulations using nitrogen-containing synergists (Formulations 2C and 3C). The composition of each sample is listed below and shown in Table 1, including the ratios of the blended components. Thermoplastic polymers: Polyamide-6,6 Inorganic fillers: Glass fiber Phosphorus-containing flame retardants (Phos-FR): Prepared according to Example 1 of WO 2020 / 132075, empirical formula:

[0179] [ka]

[0180] Phosphorus-containing flame retardant materials. Synergists: Formulation 1: Calcium hypophosphite (Phoslite® B85CX) Compound 2C: Melem Blend 3C: Melon

[0181] A twin screw extruder is used to compound the formulations shown in Table 1 at 265° C. An injection molding machine is used to prepare 0.8 mm (thickness) samples at 260-280° C. and at a mold temperature of 80° C. The formulations were evaluated for flame retardant activity under UL-94 test and processing stability.

[0182] [Table 1]

[0183] As shown in Table 1, the combination of Phos-FR and Phoslite B85CX in glass-filled polyamide 66 (Formulation 1) achieved UL-94 V-0 at 0.8 mm thickness. Additionally, a weak flame and brown charred residue were observed after UL-94 vertical burn testing, indicating that the combination formed a strong physical barrier to protect against combustion. The combination also showed excellent processing stability.

[0184] In comparison, Formulation 2C with melem as a synergist and Formulation 3C with melon as a synergist resulted in a less stable injection molding process. Additionally, Formulation 2C did not achieve UL-94 V-0 at a thickness of 0.8 mm.

[0185] While particular embodiments of the invention have been illustrated and described, it will be apparent to those skilled in the art from consideration of the specification and practice of the disclosure that various modifications and changes can be made without departing from the scope of the invention as claimed. It is therefore intended that the specification and examples be considered as exemplary only, with the true scope of the invention being indicated by the following claims and their equivalents.

Claims

1. (A) Empirical formula (I) 【Chemistry 1】 [wherein R is H, alkyl, aryl, alkylaryl, or arylalkyl group; M (+)y is a metal cation, where (+)y represents the charge formally assigned to said cation, M is a metal, y is 2 or 3, and a, b, and c represent the ratio of corresponding components to each other in the compound, satisfying the charge balance equation 2(a)+c=b(y), where c is not zero. and at least one phosphorus-containing flame retardant of (B) Chemical formula Me (+)n (H 2 PO 2 ) n [wherein Me is a metal cation, (+)n represents the oxidation state of the metal cation, and n is 2 or 3] At least one metal hypophosphite salt of 1. A flame retardant and synergist additive composition comprising:

2. 2. The flame retardant and synergist additive composition of claim 1, wherein in empirical formula (I), a is 0, 1, or 2, b is 1 to 4, and c is 1 or 2.

3. 2. The flame retardant and synergist additive composition of claim 1, wherein y is 3, a is 1, b is 1, and c is 1.

4. 4. The flame retardant and synergist additive composition of claim 3, wherein M is selected from Al, Ga, Sb, Fe, Co, B, and Bi.

5. 5. The flame retardant and synergist additive composition of claim 4, wherein M is Al or Fe.

6. In the empirical formula (I), R is H, C 1~12 Alkyl, C 6~10 Aryl, C 7~18 Alkylaryl or C 7~18 and arylalkyl, wherein the alkyl, aryl, alkylaryl, or arylalkyl is unsubstituted or is selected from the group consisting of halogen, hydroxyl, amino, C 1~4 Alkylamino, DiC 1~4 Alkylamino, C 1~4 Alkoxy, carboxy, or C 2~5 6. The flame retardant and synergist additive composition of any one of claims 1 to 5, which is substituted by alkoxycarbonyl.

7. R is unsubstituted C 1~12 Alkyl, C 6 Aryl, C 7~10 Alkylaryl or C 7~10 7. The flame retardant and synergist additive composition of claim 6, wherein the compound is arylalkyl.

8. R is unsubstituted C 1~6 7. The flame retardant and synergist additive composition of claim 6, wherein the alkyl group is aryl.

9. 9. The flame retardant and synergist additive composition of claim 8, wherein R is selected from methyl, ethyl, propyl, isopropyl, butyl, and t-butyl.

10. 10. The flame retardant and synergist additive composition of any one of claims 1 to 9, wherein M is Al, y is 3, a is 1, b is 1, and c is 1.

11. 11. The flame retardant and synergist additive composition of claim 1, wherein n in the formula is 2 for the metal hypophosphite.

12. 12. The flame retardant and synergist additive composition of claim 11, wherein the metal hypophosphite is calcium hypophosphite.

13. 11. The flame retardant and synergist additive composition of claim 1, wherein n in the formula is 3 for the metal hypophosphite.

14. 14. The flame retardant and synergist additive composition of claim 13, wherein the metal hypophosphite is aluminum hypophosphite.

15. 16. A flame retardant thermoplastic composition comprising at least one thermoplastic polymer and the flame retardant and synergist additive composition according to any one of claims 1 to 15.

16. 16. The flame retardant thermoplastic composition of claim 15, wherein the at least one thermoplastic polymer is a thermoplastic polyester or a thermoplastic polyamide.

17. 17. The flame retardant thermoplastic composition of claim 16, wherein the at least one thermoplastic polymer is a thermoplastic polyamide selected from polyamide-4,6, polyamide-6, polyamide-6,6, polyamide-6,10, polyamide-6,12, polyamide-11, polyamide-12, polyamide-4,T, polyamide-MXD,6, polyamide-12,T, polyamide-10,T, polyamide-9,T, polyamide-6,T / 6,6, polyamide-6,T / D,T, polyamide-6,6 / 6,T / 6,I, polyamide-6 / 6,T, polyamide-6,T / 6,I, and mixtures thereof.

18. 17. The flame retardant thermoplastic composition of claim 16, wherein the at least one thermoplastic polymer is a thermoplastic polyester selected from polyalkylene terephthalates.

Citation Information

Patent Citations

  • Flame retardant composition and flame-retardant thermoplastic resin composition containing said flame retardant composition

    WO2019093066A1

  • Method of preparing phosphorus-containing flame retardants and their use in polymer compositions

    WO2020132075A2

  • Method of preparing phosphorus-containing flame retardants and their use in polymer compositions

    WO2021076169A1

  • Phosphorus containing flame retardants

    US9745449B2