Method for producing gold nanoparticle-supported powder
A plasma-based method efficiently produces gold nanoparticle-supported powder with a bright red color, addressing efficiency and safety concerns, suitable for cosmetics and medical applications.
Patent Information
- Application Number
- JP2020077857
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-25
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2040-04-25
AI Technical Summary
Existing methods for producing gold nanoparticles face challenges in efficiency, safety, and the need for impurity-free, additive-free production suitable for cosmetics and medical applications, particularly in controlling particle size and color development.
A method involving the use of a simple device that generates plasma between electrodes and the liquid surface of a mixed aqueous solution containing chloroauric acid and a polyhydric alcohol, using electrodes that do not contact the solution, and employing a mother powder to support gold nanoparticles, allowing for efficient production without additives.
The method produces gold nanoparticle-supported powder with a bright red color, free from impurities and additives, enhancing safety and reducing manufacturing costs and steps, suitable for cosmetics and medical applications.
Smart Images

Figure 0007551076000005 
Figure 0007551076000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing gold nanoparticle-supported powder using liquid surface plasma, and has applications in the fields of cosmetics and paints as a coloring material, and in medical diagnosis due to antibody reactivity. [Background technology]
[0002] Silver nanoparticles and silver ions used as antibacterial materials are subject to safety concerns for living organisms due to the penetration of nanoparticles into the skin, exposure to the lungs, and the elution of silver ions, and their use is often restricted in Europe, etc. Therefore, it is important to develop material forms that eliminate concerns about nanoparticles and materials that suppress elution due to ionization.
[0003] In view of these needs, it is important for the nanoparticles to have a material form in which they are fixed to submicron or micron-sized base powders or form agglomerates with other powders, etc., and to prevent dissolution due to ionization, it is possible to consider replacing them with metals that are less likely to ionize, such as platinum or gold.
[0004] Under these circumstances, nano-sized gold particles, which are difficult to ionize, exhibit chemical activity not seen in bulk gold, and are known to be used in fields such as catalysts and biosensors. In addition, it is known that the color produced by surface plasmon resonance of gold nanoparticles exhibits vivid colors from red to purple, and they are also used in the field of color materials. For this reason, it is important to establish a technology that produces good gold nanoparticles and fixes them to a mother powder in a safe manner.
[0005] Known methods for producing these gold nanoparticles include a technique in which gold ions are reduced using a reducing agent and a dispersing agent and the resulting gold particles are protected, and a method that uses plasma discharge in an aqueous solution containing gold ions.
[0006] One method for reducing gold ions is to use an alkali metal borohydride salt as a reducing agent (Non-Patent Document 1). However, in order to stably disperse gold nanoparticles, which are fine particles that tend to aggregate, it is necessary to use a protective agent such as thiol or polyvinylpyrrolidone, which have a strong interaction with gold and form a monolayer on the gold surface. There is also a method for reducing gold ions by heating in a mixed solvent of ethanol and water, but this reaction takes a long time (Non-Patent Document 2).
[0007] On the other hand, a method has been reported in which a pair of metal electrodes is placed in pure water and plasma discharge is performed to generate gold nanoparticles (Patent Document 1). However, this method also requires the use of a protective agent to stabilize the dispersion of the generated gold nanoparticles, and there are concerns that the electrodes are consumed, resulting in poor production efficiency.
[0008] In order to apply gold nanoparticles in a wide range of fields, it is necessary to efficiently generate fine gold nanoparticles. However, if reducing agents, dispersants, protective agents, etc. that are industrially hazardous to humans or that reduce the performance of gold nanoparticles are used, a process to remove the additives, such as a washing process, is required when finally extracting the gold nanoparticles. In addition, in consideration of application in the cosmetics field as a bright red coloring material using surface plasmon resonance coloring, it is necessary to avoid the use of additives such as dispersants that are irritating to human skin, to use a carrier that suppresses the scattering of nanoparticles, and to obtain good coloring by controlling the particle size.
[0009] Among these, an electron beam irradiation reduction method has also been developed in which metal nanoparticles are obtained by irradiating an aqueous metal ion solution with an electron beam in the absence of additives such as reducing agents. However, the electron beam irradiation equipment is large-scale and requires a facility to block the electron beam, making the operation unsafe and impractical for production (Patent Document 2).
[0010] Therefore, a production method was developed to obtain powder carrying gold nanoparticles by using a simple device in which a base powder carrying gold nanoparticles is added to a mixed aqueous solution of chloroauric acid and ammonia, at least two electrodes are placed in the air above the liquid surface of the mixed aqueous solution, and a voltage is applied between the electrodes in an atmosphere of rare gas to generate plasma between the electrodes and the liquid surface. However, a more vivid red color was desired for use as a cosmetic raw material (Patent Document 3). [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Patent Publication No. 2016-27184 [Patent Document 2] Patent 4069193 [Patent Document 3] Patent application 2018-165869 [Non-patent literature]
[0012] [Non-Patent Document 1] M.Brust, M.Walker, D.Bethell, DJSchiffrin, R.Whyman, J.Chem.Soc.,Chem.Commun,p801~802(1994) [Non-Patent Document 2] N. Toshima, K. Kushihashi, T. Yonezawa, H. Hirai, Chem. Lett., 18(10), p1769-1772(1989) Summary of the Invention [Problem to be solved by the invention]
[0013] In light of the above background, the problem that the present invention aims to solve is to provide a method for efficiently producing gold nanoparticle-supported powder with a simple device that is free of impurities and has a vivid red color that can express a better, healthier complexion. [Means for solving the problem]
[0014] The present invention is a method for obtaining gold nanoparticle-supported powder by adding a base powder selected from a metal oxide or barium sulfate to a mixed aqueous solution in which a polyhydric alcohol or sugar alcohol has been added to a chloroauric acid aqueous solution (trivalent gold), placing at least two electrodes in the air above the liquid surface of the mixed aqueous solution, and applying a voltage between the electrodes in an air or rare gas atmosphere to generate plasma between the electrodes and the liquid surface. Figure 1 shows the basic configuration of the plasma processing apparatus of the present invention.
[0015] In the present invention, since the electrodes do not come into contact with the mixed aqueous solution containing the chloroauric acid solution as shown in Figure 1, there is little contamination from the electrodes due to deterioration of the electrodes caused by discharge. Furthermore, since plasma is generated between multiple electrodes and the liquid surface, more efficient plasma processing is possible compared to a plasma generation method in which one electrode is in the air and the other is in the aqueous solution, or a method in which plasma is generated between a pair of electrodes in the aqueous solution.
[0016] In the present invention, by increasing the number of power sources and pairs of electrodes as shown in Figure 2, and by increasing the number of batch processing devices as shown in Figures 1 and 2, it is possible to efficiently obtain powder carrying gold nanoparticles.
[0017] Therefore, the plasma processing apparatus of the present invention is cheaper and simpler than the electron beam irradiation method, and since there is no need to shield the electron beam, the operation can be performed safely. It is easy to improve the processing efficiency compared to the method of generating plasma in liquid.
[0018] The shape of the electrode used in the present invention is not particularly specified, but needle-shaped, hollow needle-shaped, wire-shaped, flat plate-shaped, etc. can be used, and among them, needle-shaped electrodes are preferred because they generate an uneven electric field, lowering the breakdown voltage and making it easier to generate plasma even at low voltages. The material of the electrode is also not particularly limited as long as it can maintain a stable discharge state. Metals and alloys such as platinum, tungsten, copper, copper tungsten, silver, titanium, stainless steel, molybdenum, aluminum, and iron, graphite, etc. can be used, and the surface of these electrodes may be covered with a different material in order to improve the performance of the electrode.
[0019] In the present invention, various types of power sources can be used for generating plasma, such as DC power sources, pulse power sources, low-frequency / high-frequency AC power sources, and microwave power sources, and a rectifier circuit may be combined depending on the power source. Among them, considering the production efficiency of gold nanoparticles, a wound neon transformer, a pulse power source combined with a rectifier circuit, and an inverter neon transformer combined with a rectifier circuit are good, and the wound neon transformer is the best because of its low cost and ease of use.
[0020] Furthermore, in consideration of the time it takes for the generated gold nanoparticles to be supported by the base powder, an intermittent method of turning the power on and off may be used. Gold nanoparticles are generated when the power is on, and when the power is off, the gold nanoparticles do not grow and are supported by the base powder. The intermittent time may be any time, but is preferably 0.01 to 1 second intervals in order to efficiently generate and support particles. In the case of a pulsed power source, the intermittent method can be used by turning the power on and off at a frequency lower than the pulse generation frequency.
[0021] In the plasma generation method of the present invention, the distance between the electrode placed in the air above the liquid surface and the liquid surface, the electrode-electrode distance of the electrodes placed in the air, and the applied voltage are not particularly limited as long as they are conditions that cause discharge between the electrodes and the liquid surface. The conditions are such that discharge does not occur between the electrodes in the air. The relationship between the electrode-electrode distance L that can cause discharge between the electrodes and the liquid surface and the electrode-liquid surface distance D is preferably L>3D (when the number of electrodes is three or more, the shortest distance between the electrodes of opposite polarity is L, and the longest electrode-liquid surface distance is D). The distance between the electrode placed in the air and the liquid surface is usually sufficient as long as the electrode is slightly separated from the liquid surface, and is performed at a distance greater than 0 mm and less than 50 mm. In particular, D=1 to 30 mm is preferable as a range in which a stable discharge state is maintained. In addition, it is preferable that the distance D of each electrode placed in the air and the liquid surface is equal to obtain a stable discharge. The voltage required for plasma generation is affected by the arrangement of electrodes, the material of the electrodes, etc., but is preferably 10 kV or less, taking into consideration the economy and safety of the power source, wear and tear of the electrodes, etc. Furthermore, 1 to 5 kV is most preferable from the viewpoint of ease of voltage application.
[0022] In the present invention, the atmosphere inside the vessel in which the plasma is generated is air or a rare gas. From an economical point of view, the atmosphere inside the reservoir is preferably air or argon, and the air atmosphere is the best in terms of the bright red color of the gold nanoparticle-supported powder produced and the economical aspect.
[0023] In the present invention, a mixed aqueous solution in which a polyhydric alcohol or sugar alcohol is added to an aqueous chloroauric acid solution is irradiated with plasma. The concentration of chloroauric acid (gold ion concentration) in the mixed aqueous solution is preferably 0.01 to 100 mM (M=mol / L), with 0.1 to 10 mM being even better in terms of yield efficiency based on the processing capacity of the power source and cost taking into account the price of gold, and 0.1 to 1.0 mM being best in terms of color tone.
[0024] In the present invention, a polyhydric alcohol or sugar alcohol is added to the mixed aqueous solution. In order to obtain a vivid red color tone, glycerin, diglycerin, propylene glycol, sorbitol, and erythritol are preferred, and from the viewpoint of economy, glycerin is the most preferred.
[0025] The concentration of the polyhydric alcohol or sugar alcohol in the mixed aqueous solution depends on the concentration of the charged chloroauric acid, but is preferably 0.1 to 2M, more preferably 0.1 to 1M.
[0026] Gold nanoparticles can be produced efficiently by mixing an aqueous solution of chloroauric acid with a polyhydric alcohol or sugar alcohol. If the concentration ratio of the chloroauric acid to the polyhydric alcohol or sugar alcohol is limited, the molar ratio of the chloroauric acid to the polyhydric alcohol or sugar alcohol should be in the range of 1:250 to 1:5000, and preferably 1:500 to 1:3500.
[0027] In the present invention, before plasma is generated, mother powder for supporting gold nanoparticles is added to a mixed aqueous solution to which a polyhydric alcohol or sugar alcohol has been added. By adding the mother powder to this mixed aqueous solution before plasma treatment, the mother powder serves as a scaffold for the production of gold nanoparticles, promoting the production of gold nanoparticles and suppressing the aggregation of gold particles, allowing the gold nanoparticles to be supported by the mother powder.
[0028] In the present invention, the base powder for supporting gold nanoparticles can be made of metal oxides or barium sulfate. Among them, barium sulfate is most preferable due to its vivid reddish color. In addition, the shape of these powders is plate-like, which is more likely to support gold nanoparticles.
[0029] The concentration of the base powder on which the gold nanoparticles are supported is 0.5 to 20% by weight relative to the weight of the mixed aqueous solution of chloroauric acid and polyhydric alcohol or sugar alcohol. In order to support the gold nanoparticles in a well-dispersed state and obtain a vivid red color tone, the concentration is preferably 1 to 10% by weight, and most preferably 1 to 5% by weight.
[0030] Based on the above-mentioned concentrations of chloroauric acid and base powder, the coverage rate of gold nanoparticles in the final gold nanoparticle-supported powder is preferably 0.1 to 1.0% by weight, taking into account the vivid red color tone and the cost of producing gold nanoparticles.
[0031] Furthermore, the objective of the present invention is to obtain a gold nanoparticle-supported powder with a vivid red color tone. In order to obtain a gold nanoparticle-supported powder with a color tone that is highly red and slightly yellowish like hemoglobin bound to a large amount of oxygen (oxygenated hemoglobin), which can express the healthy complexion of a human being, it is most preferable to use glycerin as an additive to the mixed aqueous solution and barium sulfate as the base powder.
[0032] In order to suppress aggregation of the gold nanoparticles produced and to disperse the base powder in the mixed aqueous solution, it is preferable to use a mechanical stirring force in combination. For example, an ultrasonic disperser, a magnetic stirrer, a propeller stirrer, a disperser mixer, a homogenizer, etc. can be used. Effect of the Invention
[0033] The gold nanoparticle-supported powder produced by the present invention is free of impurities derived from devices such as electrodes, and the additives used are highly safe as cosmetic raw materials and are easy to remove. This can contribute to the development of safe, low-cost cosmetic raw materials and diagnostic materials. Furthermore, since the mother powder is added at the same time and gold nanoparticles are generated and supported on the mother powder by plasma treatment in one step, there are fewer steps, which is advantageous in terms of production costs, and the production method is also advantageous in terms of the simplicity of the production equipment and safety management. [Brief description of the drawings]
[0034] [Figure 1] FIG. 1 is a schematic diagram of a basic configuration of a plasma processing apparatus. [Diagram 2] FIG. 2 is a schematic diagram of the basic configuration of a plasma processing apparatus when the number of pairs of electrodes is increased to four. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] Next, the method for obtaining the gold nanoparticle-supported powder of the present invention and the gold nanoparticle-supported powder will be described in detail with reference to examples, but the present invention is not limited to these. EXAMPLES
[0036] In order to verify the effect of plasma treatment in a mixed aqueous solution using glycerin, gold nanoparticle-supported powder was prepared using a plasma treatment device with the basic configuration shown in Figure 2. Treatment was performed under the conditions shown in Table 1. Other treatment conditions included platinum wire (diameter 1.0 mm) for the electrodes, a constant temperature water bath outside the storage tank controlled by a constant temperature water circulator, a winding type neon transformer (60 Hz, manufactured by Resip LSP) for the power supply, a distance of approximately 5 mm between the electrodes and the liquid surface, a pair of electrodes for each power supply were placed in the air, approximately 5 cm apart on the diagonal of the water tank, and the applied voltage of each power supply was 2.0 kV. JPEG0007551076000001.jpg63170 EXAMPLES
[0037] In order to verify the effect of plasma treatment in a mixed aqueous solution using sorbitol, the same procedure as in Example 1 was carried out under the conditions shown in Table 1. EXAMPLES
[0038] In order to verify the effect of plasma treatment in a mixed aqueous solution using erythritol, the same procedure as in Example 1 was carried out under the conditions shown in Table 1. EXAMPLES
[0039] In order to verify the effect of plasma treatment in a mixed aqueous solution using propylene glycol, the same procedure as in Example 1 was carried out under the conditions shown in Table 1.
[0040] <Comparative Examples 1 to 3> In order to compare the difference in plasma treatment effect between a mixed aqueous solution using a polyhydric alcohol or sugar alcohol and a mixed aqueous solution of ammonia or other alcohol, experiments of comparative examples were carried out in the same manner as in Example 1 under the conditions shown in Table 1. Comparative Example 1 is an example of a mixed aqueous solution using ammonia, Comparative Example 2 is an example of a mixed aqueous solution using ethanol, and Comparative Example 3 is an example of a mixed aqueous solution using 2-propanol.
[0041] <Evaluation of gold nanoparticle loading rate> The aqueous solution containing the gold nanoparticle-supported powder prepared by plasma treatment was filtered using a syringe filter (pore size 0.2 μm), and the filtrate was diluted with 1 M dilute hydrochloric acid and subjected to ICP measurement (inductively coupled plasma atomic emission spectroscopy) to measure the gold concentration [Au] in the solution. T The loading rate was determined by the initial gold concentration [Au] before adding the base powder. O was calculated using the following formula: Au loading rate (%) = 100 × (1-[Au] T / [Au] O )
[0042] <Color evaluation of gold nanoparticle-supported powder> The aqueous solution containing the gold nanoparticle-supported powder prepared by plasma treatment was filtered through a membrane filter, washed with water, and then dried to obtain the gold nanoparticle-supported powder. The gold nanoparticle-supported powder was then pressed into an inner plate for eye color cosmetics, and the surface color was measured with a spectrophotometer SE7700 (manufactured by Nippon Denshoku).
[0043] In the case of small, monodisperse gold nanoparticles of about 20 nm, the surface plasmon resonance phenomenon causes light in the blue to green range to be absorbed and red to be reflected, resulting in a slightly yellowish red color. As the particle size increases, the wavelength of the surface plasmon resonance related to absorption shifts to the red side of longer wavelengths, so red is absorbed and blue is reflected, gradually increasing the blueness and approaching purple.
[0044] Furthermore, in order to be able to express a healthy complexion as a coloring material for cosmetic ingredients, the present invention aimed to produce a gold nanoparticle-supported powder that is bright red with a high redness and slight yellowness, like oxygenated hemoglobin, which has a high amount of oxygen bound, rather than the dark red color of hemoglobin with little oxygen bound (deoxygenated hemoglobin).
[0045] For this reason, in the present invention, in the evaluation of the color tone of the gold nanoparticle-supported powder, the L * a * b * Color space a * and b * The evaluation was carried out by focusing on a * The more positive the value, the more reddish the color becomes, and the more negative the value, the more greenish the color becomes. * Since the more positive the value, the more yellow the color becomes, and the more negative the value, the more blue the color becomes, the evaluation criteria were set with the aim of achieving a color tone that reflects the characteristics of gold nanoparticles and the complexion of human skin.
[0046] That is, 1)a * is positive and the higher the number the better. 2)b * Considering that the blueness increases and the color becomes dark red, a negative value is not desirable. 3) Judging the color tone from visual judgment, the absolute value of the numerical value fluctuates greatly, and the redness index is a * We place importance on: The evaluation criteria were set as follows.
[0047] For this reason, the evaluation was performed using a spectrophotometer. * Value and b * The evaluation was performed by focusing on the a value. * Value and b * The values were shown.
[0048] In the study of the present invention, the color tone of Comparative Example 1 using ammonia, which is the technology of the prior patent document 3, was set as the judgment standard. * The value is 5.04, which is reddish, but b *The value was -1.05, a negative value, and the color tone was closer to a dark purple with a bluish tint.
[0049] In contrast, in Example 1 using glycerin, * The redness index increased by 1.7 times to 8.75, and * The value was a positive 1.59, indicating a bright red color with no dark spots.
[0050] Similarly, Example 2 using sorbitol, Example 3 using erythritol, and Example 4 using propylene glycol all showed a nearly two-fold increase in redness and a vivid red color without any blue tinge.
[0051] On the other hand, in Comparative Example 2 using ethanol and Comparative Example 3 using 2-propanol, the redness was greater than in Comparative Example 1, but * The value was negative, the blue tinge was not eliminated, and the color was a dark red. Therefore, it was found that even if the compound has a hydroxyl group, the monohydric alcohol has a dark bluish color, and it is difficult to obtain a color similar to that of healthy oxygenated hemoglobin. EXAMPLES
[0052] Next, the type of base powder was changed and the study was carried out. In Example 5, the base powder used in Example 1, which was carried out using glycerin, was changed from tabular alumina to tabular barium sulfate. EXAMPLES
[0053] Similarly, Example 6 was carried out using sorbitol, but the base powder was changed from plate-shaped alumina to plate-shaped barium sulfate in Example 2. Table 2 shows the plasma treatment conditions and the color tone results. JPEG0007551076000002.jpg168170
[0054] In Examples 5 and 6, the base powder was replaced with plate-like barium sulfate to prepare gold nanoparticle-supported powders, but the a was greater in both the glycerin mixed aqueous solution system and the sorbitol mixed aqueous solution system than in the case of plate-like alumina.* The value increased, the redness increased, and the a value of Comparative Example 1, which was used as the standard, * The value was more than twice the value of the original value, and the color was a vivid red. * It was confirmed by visual observation that the value also increased in the positive direction and approached the bright red color of oxygenated hemoglobin with a yellowish tint. Therefore, it was confirmed that plate-shaped barium sulfate is preferable as the base powder, and a * From the values, it can be seen that when plate-shaped barium sulfate is used as the base powder, glycerin shows a higher value than sorbitol and is therefore preferable. EXAMPLES
[0055] In Example 7, taking into consideration the manufacturing cost, the experiment was carried out under an air atmosphere instead of the argon atmosphere used in Example 5. EXAMPLES
[0056] In Example 8, the method of generating plasma continuously in Example 7 was changed to an intermittent discharge of 0.1 seconds, and the dependency of the power supply was examined in Example 8. Table 3 shows the plasma treatment conditions and results of Examples 7 and 8. The color tone is a change in redness. * We focused on the amount of change in the values. JPEG0007551076000003.jpg173170
[0057] In the plasma treatment in an air atmosphere in Example 7, * The value was nearly three times higher than the value obtained in Example 1, showing a vivid color tone with an extremely high reddish hue. Similarly, Example 8, which used intermittent discharge in an air atmosphere, was found to show a reddish hue that was 2.7 times higher. Therefore, in consideration of cost, discharge in an air atmosphere or intermittent discharge is preferable as a method for increasing the reddish hue. EXAMPLES
[0058] In Example 9, in order to increase the amount of gold nanoparticle-supported powder that could be prepared, the concentrations of both chloroauric acid and the plate-like barium sulfate base powder were doubled from the conditions in Example 5, and an experiment was conducted. EXAMPLES
[0059] In Example 10, in order to increase the amount of gold nanoparticle-supported powder that could be prepared, the concentrations of both the chloroauric acid and the base powder of plate-like barium sulfate were increased four-fold from the conditions in Example 5. EXAMPLES
[0060] Example 11 was prepared by doubling the amount of plate-like barium sulfate in the base powder from Example 5, and the change in color tone was confirmed.
[0061] In Example 12, the concentration of chloroauric acid was doubled from that in Example 7, and a change in color tone was confirmed. Table 4 shows the plasma treatment conditions and results for Examples 9 to 12. The color tone is a change in redness. * We focused on the amount of change in the values. JPEG0007551076000004.jpg104170
[0062] From the results of Examples 9 and 10, * The value of a in Comparative Example 1 * The redness was more than twice as much as the value of the a value, and the color tone was good. * The value of the chlorauric acid was slightly decreased, and it was preferable to keep the concentration of the chloroauric acid at an appropriate level. The results of the tested examples suggested that a concentration of 0.1 to 1.0 mM was most preferable.
[0063] In Example 11, * The value of a in Comparative Example 1 * The redness was about twice as much as the original value, and the color tone was good, but the amount of parent powder increased, and a tendency for the redness to decrease was observed.
[0064] In Example 12, the concentration of chloroauric acid was increased from that in Example 7, * The increase in the value of a * The a value of Comparative Example 1 was used as the standard. * The gold nanoparticle-loaded powder obtained was extremely reddish, more than three times the original value.
[0065] Therefore, based on the results of Examples 11 and 12, it was determined that by adjusting the concentration of chloroauric acid and the concentration of the base powder to make the gold nanoparticle coverage rate of the final gold nanoparticle-supported powder 0.1 to 1.0 wt %, a desirable color tone and cost could be obtained. [Industrial Applicability]
[0066] By using the present invention, it is possible to efficiently produce gold nanoparticle-supported powder with a brighter reddish color tone without impurities using a simple device. In addition, since the generation of gold nanoparticles and their support on the base powder are carried out in a single step, the number of manufacturing steps is reduced, which is also advantageous in terms of cost. In addition to supporting gold nanoparticles on powders such as metal oxides and barium sulfate, the technology of the present invention is expected to be used in a wide range of fields, including the support of metal nanoparticles on ceramic molded products to impart catalytic properties and as indicators for antibody reactions, and can be used not only in cosmetics but also in a wide range of fields. [Explanation of symbols]
[0067] 1. Storage tank for the liquid to be treated 2 Liquid to be treated 3 Power supply 4. Electrode placed in air above the liquid surface 5. Insulating tube 6. Plasma 7 Air or rare gases 8 Constant temperature water 9. Aquarium 10 Mixer
Claims
1. A method for producing a powder carrying gold nanoparticles, comprising the steps of: adding a base powder selected from a metal oxide or barium sulfate to a mixed aqueous solution in which a polyhydric alcohol or sugar alcohol has been added to an aqueous chloroauric acid solution (trivalent gold); placing at least two electrodes in the air above the liquid surface of the mixed aqueous solution; and applying a voltage between the electrodes in an air or rare gas atmosphere to generate plasma between the electrodes and the liquid surface.
2. 2. The method for producing gold nanoparticle-supported powder according to claim 1, wherein the polyhydric alcohol or sugar alcohol is glycerin.
3. 3. The method for producing gold nanoparticle-supported powder according to claim 1, wherein the base powder is barium sulfate.
4. The method according to any one of claims 1 to 3, wherein the atmosphere inside the storage tank is air.
Citation Information
Patent Citations
Preparation method of liquid gold nanoparticle by barometric pressure low-temperature plasma plume
CN108115148A
Solution plasma reaction apparatus, and manufacturing method for nanomaterial using the solution plasma reaction apparatus
JP2008071656A
Cosmetic including aqueous dispersion of particulates
JP2014009228A
Method for producing noble metal carrying photocatalyst particle
JP2014097476A
Method for producing metal nanoparticle
JP2014152391A