High liquidus viscosity E-glass and its manufacturing method

The high liquidus viscosity E-glass composition addresses deformation and sagging issues in LTPS manufacturing by optimizing glass properties for stable production and handling, ensuring high mechanical strength and reduced sagging.

JP7551271B2Active Publication Date: 2024-09-17IRICO DISPLAY DEVICES CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023580923
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-29
Publication Date
2024-09-17
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Conventional glass substrates used in LTPS manufacturing suffer from deformation and sagging due to high processing temperatures, which affect production stability and glass handling, especially with increasing demand for larger displays and complex transportation requirements.

Method used

A high liquidus viscosity E-glass composition is developed, comprising specific ratios of SiO2, Al2O3, B2O3, SrO, BaO, CaO, and MgO, with controlled ranges to achieve a liquidus viscosity above 200,000 poise, strain point temperature between 670 to 739°C, and Young's modulus of 70 to 83 GPa, ensuring stable production and reduced sagging.

Benefits of technology

The E-glass composition prevents glass deformation during high-temperature processing, enhances mechanical strength, and facilitates stable production with reduced sagging, meeting the demands of large display manufacturing and complex transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551271000001
    Figure 0007551271000001
  • Figure 0007551271000002
    Figure 0007551271000002
  • Figure 0007551271000003
    Figure 0007551271000003
Patent Text Reader

Abstract

The present invention discloses high liquidus viscosity E-glass and its manufacturing method. The blending ratio of raw materials used in the E-glass is SiO2: 65.56-68.6%, Al2O3: 10.58-14%, B2O3: 7-11%, SrO: 0.27-3.26%, BaO: 7.20-10.12%, CaO: 0.22-1.22%, MgO: 0-1.05%, MgO+CaO+SrO+BaO<13%, and the liquidus viscosity of the E-glass exceeds 200,000 poise. The minimum value obtained by subtracting the temperature corresponding to 100,000 poise from the liquidus temperature of the E-glass is 22°C. The E-glass has a strain point temperature of 670-739°C, a Young's modulus of 70-83 GPa, and a density of 2.38-2.45 g / cm. 3 By ensuring that the liquidus viscosity is higher than 200,000 poise, it is advantageous for overflow downdraw molding and a small density value is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is in the field of optoelectronic displays, and more particularly, to high liquidus viscosity E-glass and methods for making same. [Background technology]

[0002] As display technology advances, there is a demand for higher resolution and quality screens, which in turn leads to demands for larger TFT sizes and faster response times. LTPS technology has high electron mobility (1,000 times higher than amorphous silicon technology) and allows electronic devices such as driver ICs to be manufactured on glass substrates, which has reduced device costs, simplified the subsequent modularization process, and improved yield rates, making it the currently mainstream TFT manufacturing technology.

[0003] In the LTPS process, laser annealing technology is commonly used to crystallize the amorphous silicon layer, and it is the most efficient polycrystalline silicon (p-Si) processing method, which operates at temperatures above 600 °C. Such a method can form a polycrystalline Si film with very high electron mobility (for high-speed conversion) and excellent uniformity for TFTs in a large area. The manufacturing method usually involves sequentially depositing thin films and forming patterns using a temperature-rise method in which the substrate is heated to a temperature of 500 °C or more. At such high temperatures, the glass substrate is prone to shrink and deform, which hinders pixel improvement, and a high strain point temperature is required for the glass substrate to prevent shrinkage and deformation during the subsequent hot processing process.

[0004] On the other hand, the market demand for large displays is increasing, and glass production is also advancing to higher generations, with the weight of glass increasing from generation to generation, and the automated transport equipment that transports the glass sequentially to each processing point (factory or process) becoming more complex. The elastic sagging (deflection) of Young's modulus adversely affects the ability to load, unload, and separate glass sheets into the boxes that transport them between processing points.

[0005] The amount of sagging (deflection) is a function of the geometry of the glass sheet, the density of the glass, and the Young's modulus, both of which may be expressed as a specific modulus. The geometry of the glass piece is determined by the specific technology used and is beyond the control of the glass manufacturer. For a given density, it is advantageous to increase the Young's modulus, as this reduces the amount of sagging that larger glass sheets exhibit during transportation, handling, and thermal processing. Similarly, an increase in density should be accompanied by a proportional increase in Young's modulus, or it will lead to increased sagging. Thus, to improve the pass rate of glass sheets and reduce the amount of sagging (deflection) of glass sheets, the Young's modulus of the glass matrix should be 70 Gp or more and the density should be 2.45 g / cm3 or more. 3 It should be controlled as follows:

[0006] However, in the prior art, although the strain point and Young's modulus of glass are increased, the liquidus viscosity of glass is small, and the difference between its corresponding temperature and the temperature corresponding to 100,000 poise during forming is small, resulting in a small margin in the forming process and causing the glass to crystallize during forming, which causes the glass plate to burst during downdrawing and affects production stability. Therefore, it is necessary to increase the liquidus viscosity of glass to at least 200,000 poise, and the minimum value obtained by subtracting the temperature corresponding to 100,000 poise from the liquidus temperature of glass is 22°C, i.e., △T≧22°C. Summary of the Invention [Problem to be solved by the invention]

[0007] In order to solve the above technical problems, the present invention provides a high liquidus viscosity E-glass and a method for producing the same.

[0008] In order to achieve the above objectives, the present invention provides the following technical solutions:

[0009] High liquidus viscosity E-glass, the raw materials used are, in mole percentage, SiO2: 65.56-68.6%, Al2O3: 10.58-14%, B2O3: 7-11%, SrO: 0.27-3.26%, BaO: 7.20-10.12%, CaO: 0.22-1.22%, MgO: 0-1.05%, MgO+CaO+SrO+BaO<13%, The liquidus viscosity is greater than 200,000 poise.

[0010] Preferably, the liquidus temperature of the E-glass minus the temperature corresponding to 100,000 poise is a minimum of 22°C.

[0011] Preferably, the strain point temperature Ts of the E-glass is in the range of 670 to 739°C.

[0012] Preferably, the Young's modulus of the E-glass is in the range of 70 to 83 GPa.

[0013] The density range of the E-glass is 2.38 to 2.45 g / cm 3 It is.

[0014] A method for producing high liquidus viscosity E-glass, comprising the steps of: Step 1: putting raw materials, in mole percentages of SiO2: 65.56-68.6%, Al2O3: 10.58-14%, B2O3: 7-11%, SrO: 0.27-3.26%, BaO: 7.20-10.12%, CaO: 0.22-1.22%, and MgO: 0-1.05%, into a mixer and mixing them uniformly to form a mix, where MgO+CaO+SrO+BaO<13%; Step 2: adding the mix from step 1 into the glass furnace and heating to melt the glass, and then the molten glass is fed into the platinum feed channel for fining to produce the glass melt; and step 3 forming the glass melt into a high liquidus viscosity E-glass with a liquidus viscosity >200,000 poise by a down-draw process.

[0015] Preferably, the liquidus temperature of the glass minus the temperature corresponding to 100,000 poise is a minimum of 22°C.

[0016] Preferably, the strain point temperature Ts of the E-glass is in the range of 670 to 739° C., the Young's modulus of the E-glass is in the range of 70 to 83 GPa, and the density of the E-glass is in the range of 2.38 to 2.45 g / cm. 3 It is.

[0017] Preferably, in step 2, the fining agent in the fining is SnO2, and the proportion of SnO2 in the raw material is 0.05%. Effect of the Invention

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention provides an optimized composition of high liquidus viscosity E-glass, which can obtain a glass substrate with high liquidus viscosity and meet the requirements of stable production. In the present invention, SiO2 is mainly used to improve the properties of viscosity, and by controlling the total mole percent of SiO2 to 65.56%-68.6%, the molding temperature of the glass substrate is not excessively high, which does not adversely affect the life of the overflow brick and glass defects, and reduces the production difficulty, while the total mole percent of SiO2 is kept above 65.56%, thus ensuring that the liquidus viscosity is greater than 200,000 poise, which is favorable for overflow downdraw molding, and also obtaining a small density value.

[0020] Al2O3 can greatly improve the thermal stability of glass, reduce the crystallization tendency of glass, and increase the hardness and mechanical strength of glass, which is suitable for producing flat glass with high dimensional accuracy. However, if its total content is more than 14%, it will increase the crystallization temperature of glass, reduce the crystallization viscosity, and be unfavorable for overflow downdraw. Therefore, it is necessary to take into consideration the thermal stability, crystallization viscosity of glass, mechanical strength and hardness of glass, so the content of Al2O3 is 10.58%-14%.

[0021] B2O3 is a component that acts as a flux, and can reduce the viscosity to promote the melting of glass and reduce the temperature of the glass production process, but if its content is too high, it will rapidly reduce the temperature of the strain point of the glass and cause deterioration of thermal stability. Therefore, in one embodiment, the content of B2O3 is maintained at 7% to 11%. If the content of B2O3 is less than 7%, the effect as a flux is insufficient, and simply reducing the content of B2O3 will cause problems such as a decrease in melting ability and an increase in bubbles. On the other hand, if the content of B2O3 is high, it tends to reduce the acid resistance, and also reduces the strain point of the glass and reduces the thermal stability.

[0022] Alkaline earth metal oxides can reduce the viscosity of the entire molten glass and are favorable for reducing the temperature of the production process, but if their content is too high, the density will increase, the strain point temperature will decrease, the chemical durability will decrease, and the thermal expansion coefficient will increase, so the total content should not exceed 13%. Mixed oxides of alkaline earth metals can reduce the liquidus temperature and increase the liquidus viscosity, facilitating the production by overflow downdraw.

[0023] Furthermore, by setting the minimum value obtained by subtracting the temperature corresponding to 100,000 poise from the liquidus temperature of the glass to 22°C, crystallization during glass molding is avoided, and breakage of the glass after crystallization is prevented, allowing production to proceed reliably. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The present invention will now be described in more detail with reference to certain examples, which are intended to illustrate but not to limit the invention.

[0025] In the high liquidus viscosity E-glass of the present invention, according to the data in the table of the examples below, the raw materials used are, in mole percentages, SiO2: 65.56-68.6%, Al2O3: 10.58-14%, B2O3: 7-11%, SrO: 0.27-3.26%, BaO: 7.20-10.12%, CaO: 0.22-1.22%, MgO: 0-1.05%, MgO+CaO+SrO+BaO<13%, and the liquidus viscosity of this E-glass is greater than 200,000 poise.

[0026] The strain point temperature Ts of the E-glass of the present invention is in the range of 670 to 739°C, the Young's modulus is in the range of 70 to 83 GPa, and the density is in the range of 2.38 to 2.45 g / cm 3 It is.

[0027] The present invention provides an optimized composition of high liquidus viscosity E-glass, which can obtain a glass substrate with high liquidus viscosity and meet the requirements of stable production. In the present invention, SiO2 is mainly used to improve the properties of viscosity, and by controlling the total mole percent of SiO2 to 65.56%-68.6%, the molding temperature of the glass substrate is not excessively high, which does not adversely affect the life of the overflow brick and glass defects, and reduces the production difficulty, while the total mole percent of SiO2 is kept above 65.56%, thus ensuring that the liquidus viscosity is greater than 200,000 poise, which is favorable for overflow downdraw molding, and also obtaining a small density value.

[0028] Al2O3 can greatly improve the thermal stability of glass, reduce the crystallization tendency of glass, and increase the hardness and mechanical strength of glass, which is suitable for producing flat glass with high dimensional accuracy. However, if its total content is more than 14%, it will increase the crystallization temperature of glass, reduce the crystallization viscosity, and be unfavorable for overflow downdraw. Therefore, it is necessary to take into consideration the thermal stability, crystallization viscosity of glass, mechanical strength and hardness of glass, so the content of Al2O3 is 10.58%-14%.

[0029] B2O3 is a component that acts as a flux, and can reduce the viscosity to promote the melting of glass and reduce the temperature of the glass production process, but if its content is too high, it will rapidly reduce the temperature of the strain point of the glass and cause deterioration of thermal stability. Therefore, in one embodiment, the content of B2O3 is maintained at 7% to 11%. If the content of B2O3 is less than 7%, the effect as a flux is insufficient, and simply reducing the content of B2O3 will cause problems such as a decrease in melting ability and an increase in bubbles. On the other hand, if the content of B2O3 is high, it tends to reduce the acid resistance, and also reduces the strain point of the glass and reduces the thermal stability.

[0030] Alkaline earth metal oxides can reduce the viscosity of the entire molten glass and are favorable for reducing the temperature of the production process, but if their content is too high, the density will increase, the strain point temperature will decrease, the chemical durability will decrease, and the thermal expansion coefficient will increase, so the total content should not exceed 13%. Mixed oxides of alkaline earth metals can reduce the liquidus temperature and increase the liquidus viscosity, facilitating the production by overflow downdraw.

[0031] The minimum value obtained by subtracting the temperature corresponding to 100,000 poise from the liquidus temperature of E-glass was 22° C. By setting the minimum value obtained by subtracting the temperature corresponding to 100,000 poise from the liquidus temperature of glass to 22° C., crystallization during glass molding is avoided, glass breakage after crystallization is avoided, and production can be reliably carried out.

[0032] The method for making high liquidus viscosity E-glass of the present invention includes the following steps. Step 1, put the raw materials of SiO2:65.56~68.6%, Al2O3:10.58~14%, B2O3:7~11%, SrO:0.27~3.26%, BaO:7.20~10.12%, CaO:0.22~1.22%, MgO:0~1.05% into the mixer, mix evenly, and make the mixture of MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is put into the platinum feed channel for fining to produce the glass melt. Step 3, using a down-draw process to form the glass melt into high liquidus viscosity E-glass with a liquidus viscosity >200,000 poise. Example 1

[0033] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 66.00%, Al2O3: 13.00%, B2O3: 10.01%, SrO: 1.27%, BaO: 8.86%, CaO: 0.73%, and MgO: 0.07%, in mole percentage, into a mixer and mix evenly to make a mixture, where the ratio is MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 267719.7 poise. In Example 1, the E-glass has a strain point temperature Ts of 723° C., a Young's modulus of 82 GPa, and a density of 2.39 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 25°C. Example 2

[0034] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 68.60%, Al2O3: 14.00%, B2O3: 7.32%, SrO: 0.27%, BaO: 8.95%, CaO: 0.74%, and MgO: 0.07%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 218351.3 poise. In Example 2, the E-glass has a strain point temperature Ts of 739° C., a Young's modulus of 83 GPa, and a density of 2.38 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 30°C. Example 3

[0035] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 67.00%, Al2O3: 10.87%, B2O3: 9.82%, SrO: 3.23%, BaO: 8.24%, CaO: 0.71%, and MgO: 0.08%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 206347.1 poise. In Example 3, the E-glass has a strain point temperature Ts of 687° C., a Young's modulus of 75 GPa, and a density of 2.42 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 28°C. Example 4

[0036] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 66.56%, Al2O3: 10.87%, B2O3: 9.82%, SrO: 2.24%, BaO: 9.67%, CaO: 0.71%, MgO: 0.07% into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 317280.6 poise. In Example 4, the E-glass has a strain point temperature Ts of 680° C., a Young's modulus of 76 GPa, and a density of 2.45 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 38°C. Example 5

[0037] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 66.23%, Al2O3: 10.82%, B2O3: 11.00%, SrO: 1.22%, BaO: 10.12%, CaO: 0.49%, and MgO: 0.07%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 290999.8 poise. In Example 5, the E-glass has a strain point temperature Ts of 673° C., a Young's modulus of 70 GPa, and a density of 2.43 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 26°C. Example 6

[0038] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 67.91%, Al2O3: 13.20%, B2O3: 7.00%, SrO: 2.31%, BaO: 7.85%, CaO: 0.73%, and MgO: 0.95%, in mole percentage, into a mixer and mix evenly to make a mixture, where the ratio is MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 412501.0 poise. In Example 6, the E-glass has a strain point temperature Ts of 723° C., a Young's modulus of 82 GPa, and a density of 2.43 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 46°C. Example 7

[0039] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 68.08%, Al2O3: 11.04%, B2O3: 9.24%, SrO: 2.22%, BaO: 8.83%, CaO: 0.49%, and MgO: 0.02%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 223978.5 poise. In Example 7, the E-glass has a strain point temperature Ts of 704° C., a Young's modulus of 81 GPa, and a density of 2.44 g / cm 3and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 31°C. Example 8

[0040] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 67.56%, Al2O3: 11.04%, B2O3: 9.96%, SrO: 2.27%, BaO: 8.82%, CaO: 0.22%, MgO: 0.07% into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 260487.4 poise. In Example 8, the E-glass has a strain point temperature Ts of 694° C., a Young's modulus of 81 GPa, and a density of 2.38 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 36°C. Example 9

[0041] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 66.89%, Al2O3: 10.93%, B2O3: 9.86%, SrO: 2.25%, BaO: 8.73%, CaO: 1.22%, MgO: 0.07% into a mixer and mix evenly to make a mixture with MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 395876.8 poise. In Example 9, the E-glass has a strain point temperature Ts of 679° C., a Young's modulus of 74 GPa, and a density of 2.42 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 52°C. Example 10

[0042] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 67.28%, Al2O3: 10.99%, B2O3: 9.92%, SrO: 2.21%, BaO: 7.78%, CaO: 0.72%, MgO: 1.05% into a mixer and mix evenly to make a mixture with the following content: MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 363697.3 poise. In Example 10, the E-glass has a strain point temperature Ts of 688° C., a Young's modulus of 76 GPa, and a density of 2.43 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 42°C. Example 11

[0043] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 67.09%, Al2O3: 10.96%, B2O3: 9.89%, SrO: 2.26%, BaO: 8.75%, CaO: 0.72%, MgO: 0.27% into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 359805.6 poise. In Example 11, the E-glass has a strain point temperature Ts of 691° C., a Young's modulus of 75 GPa, and a density of 2.4 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 44°C. Example 12

[0044] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 67.23%, Al2O3: 12.98%, B2O3: 8.42%, SrO: 2.26%, BaO: 8.27%, CaO: 0.72%, and MgO: 0.07%, in mole percentage, into a mixer and mix evenly to make a mixture, where the ratio is MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 258442.4 poise. In Example 12, the E-glass has a strain point temperature Ts of 715° C., a Young's modulus of 75 GPa, and a density of 2.41 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 34°C. Example 13

[0045] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 67.23%, Al2O3: 11.98%, B2O3: 8.41%, SrO: 2.26%, BaO: 9.27%, CaO: 0.72%, and MgO: 0.07%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 276728.3 poise. In Example 13, the E-glass has a strain point temperature Ts of 715° C., a Young's modulus of 79 GPa, and a density of 2.4 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 37°C. Example 14

[0046] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 67.08%, Al2O3: 10.99%, B2O3: 10.12%, SrO: 2.26%, BaO: 8.78%, and CaO: 0.72%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 229892.2 poise. In Example 14, the E-glass has a strain point temperature Ts of 690° C., a Young's modulus of 72 GPa, and a density of 2.39 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 31°C. Example 15

[0047] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 66.89%, Al2O3: 10.93%, B2O3: 9.86%, SrO: 2.25%, BaO: 8.73%, CaO: 0.72%, and MgO: 0.57%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 200550.0 poise. In Example 15, the E-glass has a strain point temperature Ts of 686° C., a Young's modulus of 76 GPa, and a density of 2.4 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 23°C. Example 16

[0048] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 65.56%, Al2O3: 13.87%, B2O3: 7.82%, SrO: 2.24%, BaO: 8.68%, CaO: 1.70%, MgO: 0.07% into a mixer and mix evenly to make a mixture with MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 229342.6 poise. In Example 16, the E-glass has a strain point temperature Ts of 722° C., a Young's modulus of 83 GPa, and a density of 2.42 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 28°C. Example 17

[0049] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 66.55%, Al2O3: 11.87%, B2O3: 9.82%, SrO: 2.24%, BaO: 8.68%, CaO: 0.71%, MgO: 0.07% into a mixer and mix evenly to make a mixture with MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 229342.6 poise. In Example 17, the E-glass has a strain point temperature Ts of 696° C., a Young's modulus of 78 GPa, and a density of 2.41 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 37°C. Example 18

[0050] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 67.73%, Al2O3: 10.98%, B2O3: 9.41%, SrO: 2.26%, BaO: 8.77%, CaO: 0.72%, MgO: 0.07% into a mixer and mix evenly to make a mixture with MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 269925.4 poise. In Example 18, the E-glass has a strain point temperature Ts of 695° C., a Young's modulus of 74 GPa, and a density of 2.41 g / cm 3and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 39°C. Example 19

[0051] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 68.30%, Al2O3: 10.88%, B2O3: 10.50%, SrO: 2.20%, BaO: 7.20%, CaO: 0.80%, and MgO: 0.07%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 348081.8 poise. In Example 19, the E-glass has a strain point temperature Ts of 683° C., a Young's modulus of 72 GPa, and a density of 2.4 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 49°C. Example 20

[0052] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 67.53%, Al2O3: 11.68%, B2O3: 8.98%, SrO: 2.76%, BaO: 8.28%, and CaO: 0.72%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 210081.0 poise. In Example 20, the E-glass has a strain point temperature Ts of 689° C., a Young's modulus of 74 GPa, and a density of 2.4 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 22°C. Example 21

[0053] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 67.64%, Al2O3: 10.58%, B2O3: 9.98%, SrO: 3.26%, BaO: 7.77%, and CaO: 0.72%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 415818.6 poise. In Example 21, the E-glass has a strain point temperature Ts of 686° C., a Young's modulus of 71 GPa, and a density of 2.39 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 46°C. Example 22

[0054] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 67.93%, Al2O3: 12.78%, B2O3: 7.42%, SrO: 2.26%, BaO: 8.77%, CaO: 0.72%, MgO: 0.07% into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 273255.6 poise. In Example 22, the E-glass has a strain point temperature Ts of 729° C., a Young's modulus of 81 GPa, and a density of 2.39 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 36°C. Example 23

[0055] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials, which are SiO2: 66.73%, Al2O3: 11.00%, B2O3: 10.40%, SrO: 2.26%, BaO: 8.77%, CaO: 0.72%, and MgO: 0.07%, in mole percentage, into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 408819.2 poise. In Example 23, the E-glass has a strain point temperature Ts of 687° C., a Young's modulus of 72 GPa, and a density of 2.4 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 55°C. Example 24

[0056] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 67.23%, Al2O3: 10.98%, B2O3: 10.42%, SrO: 2.16%, BaO: 8.40%, CaO: 0.69%, MgO: 0.07% into a mixer and mix evenly to make a mixture, where MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 338660.9 poise. In Example 24, the E-glass has a strain point temperature Ts of 670° C., a Young's modulus of 70 GPa, and a density of 2.39 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 40°C. Example 25

[0057] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 67.57%, Al2O3: 11.04%, B2O3: 9.96%, SrO: 2.17%, BaO: 8.44%, CaO: 0.69%, MgO: 0.07% into a mixer and mix evenly to make a mix with MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 491490.0 poise. In Example 25, the E-glass has a strain point temperature Ts of 693° C., a Young's modulus of 76 GPa, and a density of 2.4 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 49°C. Example 26

[0058] The process for making high liquidus viscosity E-glass includes the following steps: Step 1: Put the raw materials with the molar percentage of SiO2: 66.73%, Al2O3: 12.56%, B2O3: 7.91%, SrO: 2.59%, BaO: 8.40%, CaO: 0.69%, MgO: 0.07% into a mixer and mix evenly to make a mix with MgO+CaO+SrO+BaO<13%. Step 2, the mix from step 1 is added to the glass furnace, heated to melt the glass, and the molten glass is fed into the platinum feed channel, and clarified by adding SnO2 0.05% to produce the glass melt. Step 3, using a down-draw process, the glass melt is formed into a high liquidus viscosity E-glass with a liquidus viscosity of 263689.7 poise. In Example 26, the E-glass has a strain point temperature Ts of 717° C., a Young's modulus of 82 GPa, and a density of 2.42 g / cm 3 and the liquidus temperature of E-glass minus the temperature corresponding to 100,000 poise is 24°C.

[0059] Table showing data on the mixing ratio of components in the above examples JPEG0007551271000001.jpg10091 JPEG0007551271000002.jpg10390JPEG0007551271000003.jpg10389JPEG0007551271 000004.jpg10391JPEG0007551271000005.jpg10389JPEG0007551271000006.jpg8690

Claims

1. 1. A high liquidus viscosity E-glass, The raw materials used are, in mole percentage, SiO 2 :65.56~68.6%, Al 2 O 3 :10.58~14%, B 2 O 3 : 7-11%, SrO: 0.27-3.26%, BaO: 7.20-10.12%, CaO: 0.22-1.22%, MgO: 0-1.05%, MgO + CaO + SrO + BaO < 13%, A high liquidus viscosity E-glass characterized by a liquidus viscosity greater than 200,000 poise.

2. 2. The high liquidus viscosity E-glass of claim 1, wherein the liquidus temperature of said E-glass minus the temperature corresponding to 100,000 poise is a minimum of 22°C.

3. 2. The high liquidus viscosity E-glass of claim 1, wherein the E-glass has a strain point temperature Ts in the range of 670 to 739°C.

4. 2. The high liquidus viscosity E-glass of claim 1, wherein the E-glass has a Young's modulus in the range of 70 to 83 GPa.

5. The density range of the E-glass is 2.38 to 2.45 g / cm 3 2. The high liquidus viscosity E-glass of claim 1,

6. 1. A method for producing high liquidus viscosity E-glass, comprising the steps of: As a raw material, in mole percentage, SiO 2 :65.56~68.6%, Al 2 O 3 :10.58~14%, B 2 O 3 Step 1 of feeding 7-11%, SrO, 0.27-3.26%, BaO, 7.20-10.12%, CaO, 0.22-1.22%, and MgO, 0-1.05%, into a mixer and mixing them uniformly to obtain a mix, where MgO+CaO+SrO+BaO<13%; Step 2: adding the mix from step 1 to a glass furnace and heating to melt the glass, and then fining the molten glass into a platinum feed channel to produce a glass melt; and step 3. forming the glass melt into a high liquidus viscosity E-glass with a liquidus viscosity >200,000 poise by a downdraw process.

7. 7. The method of claim 6, wherein the minimum liquidus temperature of the glass minus the temperature corresponding to 100,000 poise is 22°C.

8. The strain point temperature Ts of the E-glass is in the range of 670 to 739° C., the Young's modulus of the E-glass is in the range of 70 to 83 GPa, and the density of the E-glass is in the range of 2.38 to 2.45 g / cm 3 7. The method for producing high liquidus viscosity E-glass according to claim 6,

9. In step 2, the fining agent in the fining step is SnO 2 The content of SnO in the raw material 2 7. The method for producing high liquidus viscosity E-glass according to claim 6, wherein the proportion of is 0.05%.

Citation Information

Patent Citations

  • Method for manufacturing glass substrate for flat panel display

    JP2013212943A

  • Low-boron, barium-free, alkaline earth aluminosilicate glass and its applications

    US20180319700A1

  • Method for producing alkali-free glass substrate, and alkali-free glass substrate

    WO2019093129A1

  • Glass substrate and method for manufacturing same

    WO2019146379A1