Vinyl resin particles and method for producing same

Vinyl resin particles with controlled thermal decomposition properties address the challenges of hazardous chemical use and high costs in porous polyimide film production, achieving smooth and mechanically strong thermosetting resin films.

JP7551709B2Active Publication Date: 2024-09-17SEKISUI PLASTICS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022145732
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-11
Filing Date
2022-09-14
Publication Date
2024-09-17
Estimated Expiration
2039-08-28

AI Technical Summary

Technical Problem

Existing methods for producing porous polyimide films face challenges such as the use of hazardous chemicals like hydrofluoric acid, high manufacturing costs, and poor coating properties due to solvent swelling, which affect the mechanical strength and surface smoothness of the films.

Method used

The development of vinyl resin particles with specific thermal decomposition behavior, characterized by a 10% mass loss between 230°C and 300°C, and a mass reduction rate of 85-100% at 350°C, which are used to create thermosetting resin films with improved surface smoothness and mechanical strength without the need for hydrofluoric acid.

Benefits of technology

The vinyl resin particles effectively smooth the surface of thermosetting resin films, enhancing mechanical strength and heat insulation properties while avoiding the use of hazardous chemicals and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551709000003
    Figure 0007551709000003
  • Figure 0007551709000001
    Figure 0007551709000001
  • Figure 0007551709000002
    Figure 0007551709000002
Patent Text Reader

Abstract

Provided are vinyl resin particles that, when used as a porosity-making material for thermosetting resins, can easily smooth the surface of a thermosetting resin film. [Solution] The present invention provides vinyl resin particles used to make thermosetting resins porous, which have a temperature of 230°C or higher but lower than 300°C at which they lose 10% of their mass when heated at a rate of 10°C / min in an air atmosphere, and a mass loss rate of 85% to 100% after heating at 350°C for 5 hours in an air atmosphere.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to vinyl resin particles and a method for producing the same. [Background technology]

[0002] Polyimide resins are used as heat-resistant materials and insulating materials for electronic components because of their excellent heat resistance, mechanical strength, electrical properties, chemical resistance, and moldability.

[0003] Polyimide resins used as insulating materials for electronic components are required to have improved electrical properties while maintaining heat resistance and mechanical strength. In particular, there is a demand for a lower dielectric constant in order to suppress attenuation of high-frequency current in electronic components.

[0004] As a low dielectric polyimide resin, for example, porous polyimide, in which the dielectric constant is reduced by increasing the porosity of the polyimide resin, is known.

[0005] The porosity can be easily increased by forming large pores in porous polyimide, but on the other hand, this reduces heat resistance and mechanical strength. Therefore, it is necessary to increase the porosity by dispersing as small pores as possible at a high density.

[0006] For example, Patent Document 1 describes a method for producing a porous polyimide film, which includes a step of applying a polyimide precursor slurry in which silica particles are uniformly dispersed to at least one surface of a substrate, a step of carrying out a dehydration cyclic polyimidization reaction to form a silica / polyimide film containing silica particles in a three-dimensional stereoregular arrangement to a thickness of 5 to 20 μm, and a step of removing the silica particles from the silica / polyimide film.

[0007] Patent Document 2 describes a porous polyimide film including a step of forming a coating film containing an aqueous polyimide precursor solution in which a polyimide precursor is dissolved in a water-soluble solvent and non-crosslinked resin particles that are not soluble in the solution, drying the coating film and heating it for imidization to form a polyimide film, and a step of dissolving and removing the non-crosslinked resin particles with an organic solvent to make the film porous.

[0008] Patent Document 3 describes a method for producing a porous polyimide film, which includes a firing step of firing an unsintered composite film containing polyamic acid or polyimide, resin fine particles, and a condensing agent at a temperature lower than the decomposition temperature of the resin fine particles to form a polyimide-resin fine particle composite film, and a fine particle removal step of removing the resin fine particles from the polyimide-resin fine particle composite film. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2013 / 084368 [Patent Document 2] Japanese Patent Publication No. 2016-183273 [Patent Document 3] International Publication No. 2014 / 196435 Summary of the Invention [Problem to be solved by the invention]

[0010] Patent Document 1 describes that the substrate on which the silica / polyimide film is formed is brought into contact with hydrofluoric acid (HF) in order to remove silica particles. However, hydrofluoric acid has problems such as being difficult to handle due to its toxicity, corrosiveness, risk of explosion during reaction, the need for special equipment to manage hydrofluoric acid, and the expense of waste liquid treatment, and therefore a method for producing a porous polyimide film without using hydrofluoric acid is desired.

[0011] In Patent Document 2, non-crosslinked resin particles are used as a substitute for silica particles, making it possible to remove the particles with an organic solvent without using hydrofluoric acid. However, since the process includes a step of removing the particles with a solvent, there is a problem that the manufacturing cost is higher than in a process in which the particles are removed in a baking step.

[0012] In the examples of Patent Document 3, it is described that by adding a condensing agent without using hydrofluoric acid, a porous polyimide film with good film strength was obtained even when heat-treated at a low temperature of 230° C. However, since N,N-dimethylacetamide is used as a solvent in the examples, there is a problem that, in the case of polymethyl methacrylate resin particles that are not crosslinked, the resin particles are swelled by the solvent, increasing the viscosity of the varnish, which leads to poor coatability of the varnish and insufficient surface smoothing of the polyimide film.

[0013] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide vinyl resin particles which can smooth the surface of a thermosetting resin film by a simple method, and a method for producing the same. [Means for solving the problem]

[0014] As a result of intensive research aimed at achieving the above object, the present inventors have succeeded in developing vinyl-based resin particles that exhibit specific thermal decomposition behavior in an air atmosphere, and have found that the above object can be achieved by using the vinyl-based resin particles. The present invention was completed by the present inventors through further research.

[0015] That is, the present invention provides the following aspects. Section 1. A vinyl resin particle used for making a thermosetting resin porous, The temperature at which the mass is reduced by 10% when the temperature is increased at 10°C / min in an air atmosphere is 230°C or higher and lower than 300°C, Vinyl resin particles, which have a mass reduction rate of 85 to 100% after heating in an air atmosphere at 350°C for 5 hours. Section 2. Item 2. The vinyl resin particles according to item 1, having a number average particle size in the range of 0.1 to 3 μm. Section 3. Item 3. The vinyl resin particles according to item 1 or 2, wherein the coefficient of variation of the number average particle size is 25% or less. Section 4. 2 to 10 times the median diameter (D50) based on number of pieces Grain Item 4. The vinyl resin particles according to any one of Items 1 to 3, wherein the number ratio of particles having a small diameter is in the range of 0 to 5%. Section 5. the vinyl-based resin particles are polymers having polymerizable vinyl-based monomer units composed of monofunctional monomer units and polyfunctional monomer units, Item 5. The vinyl resin particles according to any one of items 1 to 4, wherein the polymerizable vinyl monomer unit contains 8 to 150 parts by mass of the polyfunctional monomer unit relative to 100 parts by mass of the monofunctional monomer unit. Section 6. the monofunctional monomer unit is at least one of a monofunctional styrene-based monomer unit and a monofunctional (meth)acrylic monomer unit, Item 6. The vinyl resin particle according to item 5, wherein the polyfunctional monomer unit is at least one of a polyfunctional styrene monomer unit and a polyfunctional (meth)acrylic monomer unit. Section 7. Item 7. The vinyl resin particles according to item 6, wherein the monofunctional (meth)acrylic monomer unit is a (meth)acrylic acid alkyl ester monomer unit, and the alkyl group bonded to the ester has 1 to 10 carbon atoms. Section 8. Item 8. The vinyl resin particle according to any one of items 1 to 7, The vinyl resin particles have a pH of 3 to 9 when dispersed in water at a mass ratio of 1:10. Section 9. Item 9. The vinyl-based resin particles according to any one of items 1 to 8, wherein the Rsp value represented by the following formula (1) is 5 or more and 150 or less. Rsp = (Rav - Rb) / Rb (1) Rav: The reciprocal of the average value of the transverse relaxation time T2 (ms) obtained by measurement method 1 below Rb: the reciprocal of the transverse relaxation time T2 (ms) obtained by measurement method 2 below [Measurement method 1] For a polyimide precursor varnish obtained by mixing a vinyl resin particle dispersion liquid obtained by mixing the vinyl resin particles and a first organic solvent in a mass ratio of 1:3, a polyimide precursor solution having a solid content concentration of 18±1 mass%, and a second organic solvent in a mass ratio of 6:3.61:1.8, the transverse relaxation time T2 (ms) of protons derived from the varnish is measured three times by the CPMG method under measurement conditions of using hydrogen nuclei as the measurement nucleus, measuring temperature of 20°C, resonant frequency of 13 MHz, and 90° pulse width of 5.81 μs, and the average value is calculated. The reciprocal of the average value is defined as Rav. [Measurement method 2] For a blank solution obtained by mixing a first organic solvent, a polyimide precursor solution having a solids concentration of 18±1% by mass, and a second organic solvent in a mass ratio of 4.5:3.61:1.8, the transverse relaxation time T2 (ms) of protons derived from the blank solution was measured three times by the CPMG method under measurement conditions of a hydrogen nucleus as the measurement nucleus, a measurement temperature of 20°C, a resonance frequency of 13 MHz, and a 90° pulse width of 5.81 μs, and the average value was calculated. The reciprocal of the average value was designated as Rb. Section 10. A method for producing vinyl resin particles according to any one of items 1 to 9, a seed polymerization step of absorbing a first polymerizable vinyl monomer into seed particles and carrying out seed polymerization to obtain an aqueous dispersion containing polymer particles of the first polymerizable vinyl monomer and an aqueous medium; a spray drying step in which the aqueous dispersion obtained in the seed polymerization step is spray-dried under conditions of an inlet temperature of 80 to 220°C and an outlet temperature of 50 to 100°C to obtain an aggregate; and a crushing step for crushing the aggregates obtained in the spray drying step to obtain vinyl-based resin particles, A method for producing vinyl resin particles, wherein in the seed polymerization step, the first polymerizable vinyl monomer contains a monofunctional monomer and a polyfunctional monomer, and the first polymerizable vinyl monomer contains 8 to 150 parts by mass of the polyfunctional monomer per 100 parts by mass of the monofunctional monomer. Section 11. Item 11. The method for producing vinyl-based resin particles according to item 10, further comprising at least one of a first classification step of classifying the polymer particles obtained in the seed polymerization step and a second classification step of classifying the vinyl-based resin particles obtained in the crushing step. Section 12. A method for producing vinyl resin particles according to any one of items 1 to 9, an emulsion polymerization step of emulsion-polymerizing a second polymerizable vinyl monomer in an aqueous medium to obtain an aqueous dispersion containing polymer particles of the second polymerizable vinyl monomer and the aqueous medium; a spray drying step of spray-drying the aqueous dispersion obtained in the emulsion polymerization step under conditions of an inlet temperature of 80 to 220°C and an outlet temperature of 50 to 100°C to obtain an aggregate; and a crushing step for crushing the aggregates obtained in the spray drying step to obtain vinyl-based resin particles; A method for producing vinyl-based resin particles, comprising: Section 13. Item 13. The method for producing vinyl resin particles according to item 12, further comprising a pH adjustment step of adjusting the pH of the aqueous dispersion to 3 to 9 by adding a nitrogen-containing compound to the aqueous dispersion obtained in the emulsion polymerization step. Section 14. Item 14. The method for producing vinyl-based resin particles according to item 12 or 13, further comprising at least one of a first classification step of classifying the polymer particles obtained in the emulsion polymerization step and a second classification step of classifying the vinyl-based resin particles obtained in the crushing step. Effect of the Invention

[0016] When the vinyl resin particles of the present invention are used as a porosity-making material for thermosetting resin, the surface of the film of thermosetting resin can be easily smoothed.When the vinyl resin particles of the present invention are used, the surface of the film of thermosetting resin can be smoothed by a simple method without using hydrofluoric acid as in the conventional technology. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a scanning electron microscope (SEM) photograph of the vinyl resin particles obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Preferred embodiments of the present invention will now be described in detail.

[0019] In this specification, "(meth)acrylic" means "acrylic" or "methacrylic", and "(meth)acrylate" means "acrylate" or "methacrylate".

[0020] In this specification, the monofunctional styrene monomer unit refers to a repeating structural unit formed when a monofunctional styrene monomer is polymerized, but does not refer to the monomer itself.Similarly, the monofunctional (meth)acrylic monomer unit refers to a repeating structural unit formed when a monofunctional (meth)acrylic monomer is polymerized, but does not refer to the monomer itself.

[0021] In this specification, the term "polyfunctional styrene-based monomer unit" refers to a repeating structural unit formed when a polyfunctional styrene-based monomer is polymerized, but does not refer to the monomer itself. Similarly, the term "polyfunctional (meth)acrylic monomer unit" refers to a repeating structural unit formed when a polyfunctional (meth)acrylic monomer is polymerized, but does not refer to the monomer itself.

[0022] In this specification, the pH of vinyl resin particles means the pH measured by a pH meter at room temperature (20°C to 25°C) of a dispersion liquid (dispersion of vinyl resin particles) obtained by dispersing the vinyl resin particles in water at a mass ratio of vinyl resin particles to water of 1:10.

[0023] 1. Vinyl Resin Particles The vinyl resin particles of the present invention have the characteristics that the temperature at which they undergo a 10% mass loss when heated at 10°C / min in an air atmosphere is 230°C or higher and lower than 300°C, and that the mass loss rate after heating at 350°C for 5 hours in an air atmosphere is 85% to 100%.

[0024] The vinyl resin particles of the present invention have the above-mentioned properties and are therefore suitable for use in making thermosetting resins porous. Specifically, the vinyl resin particles of the present invention have the above-mentioned properties and therefore can easily smooth the surface of a thermosetting resin film when used as a porosity-making material for thermosetting resins.

[0025] <Thermal decomposition behavior> The vinyl resin particles of the present invention have a temperature at which they lose 10% of their mass (10% thermal decomposition temperature) when heated in an air atmosphere from 40°C to 500°C at a heating rate of 10°C / min using a thermogravimetry and differential thermal analyzer (hereinafter also referred to as a TGA apparatus), of 230°C or higher and lower than 300°C, and when heated in an air atmosphere from 40°C to 350°C at a heating rate of 10°C / min and then heated at 350°C for 5 hours, their mass loss is 85% to 100%.

[0026] In this specification, the 10% thermal decomposition temperature means the temperature at which the mass loss rate of a sample is 10% by mass when the sample is heated in an air atmosphere at a heating rate of 10°C / min using a TGA device. As the TGA device, for example, "TG / DTA6200" (manufactured by SII Nano Technology Co., Ltd.) can be used. The mass of the vinyl resin particles of the present invention as the sample is about 15 mg.

[0027] In this specification, the mass loss rate after heating at 350° C. for 5 hours in an air atmosphere can be calculated from [(mass of sample before heating−mass of sample after heating) / mass of sample before heating]×100. The mass loss rate after heating at 350° C. for 5 hours can be measured using a TGA device.

[0028] If the 10% thermal decomposition temperature is 300° C. or higher, the viscosity of the thermosetting resin precursor solution in which the vinyl resin particles are dispersed may become high, and therefore, good coatability of the thermosetting resin precursor solution may not be obtained, so that when a thermosetting resin film is produced, it may be difficult to smooth the surface of the film.

[0029] If the 10% thermal decomposition temperature is lower than 230° C., the vinyl resin particles added may decompose before the thermosetting resin hardens, and therefore the vinyl resin particles may not remain in the thermosetting resin, which may result in the thermosetting resin film not being able to be made porous when produced.

[0030] Since the vinyl resin particles of the present invention can be suitably used by making thermosetting resins porous, it is preferred that the temperature at which a 10% mass loss occurs when heated from 40°C to 500°C at a heating rate of 10°C / min in an air atmosphere is 240 to 296°C, and that the mass loss rate when heated at a heating rate of 10°C / min in an air atmosphere and then heated at 350°C for 5 hours is 88% to 100%.

[0031] Since the vinyl resin particles of the present invention can be used more suitably due to the porosity of the thermosetting resin, it is preferred that the temperature at which a 10% mass loss occurs when heated from 40°C to 500°C at a heating rate of 10°C / min in an air atmosphere is 250 to 294°C, and that the mass loss rate when heated at a heating rate of 10°C / min in an air atmosphere and then heated at 350°C for 5 hours is 90% to 100%.

[0032] Since the vinyl resin particles of the present invention can be particularly suitably used for making thermosetting resins porous, it is preferable that the temperature at which a 10% mass loss occurs when heated from 40°C to 500°C at a heating rate of 10°C / min in an air atmosphere is 255 to 292°C, and that the mass loss rate when heated at a heating rate of 10°C / min in an air atmosphere and then heated at 350°C for 5 hours is 92% to 100%.

[0033] <Number average particle size> The vinyl resin particles of the present invention preferably have a number-average particle size of 0.15 to 1.5 μm. If the number-average particle size is within this range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the mechanical strength and heat insulation of the porous thermosetting resin film are improved.

[0034] The vinyl resin particles of the present invention more preferably have a number-average particle size of 0.2 to 1.2 μm. If the number-average particle size is within this range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the mechanical strength and heat insulation of the porous thermosetting resin film are further improved.

[0035] The vinyl resin particles of the present invention more preferably have a number-average particle size of 0.3 to 1.0 μm. If the number-average particle size is within this range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the mechanical strength and heat insulation of the porous thermosetting resin film are further improved.

[0036] <Coefficient of variation of number average particle size> The vinyl resin particles of the present invention preferably have a coefficient of variation of the number-average particle size of 25% or less. If the coefficient of variation is within this range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the mechanical strength of the porous thermosetting resin film is improved.

[0037] The vinyl resin particles of the present invention preferably have a coefficient of variation of the number-average particle size of 20% or less. If the coefficient of variation is within this range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the mechanical strength of the porous thermosetting resin film is further improved.

[0038] The vinyl resin particles of the present invention further preferably have a coefficient of variation of the number-average particle size of 15% or less. If the coefficient of variation is within this range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the mechanical strength of the porous thermosetting resin film is further improved.

[0039] <Ratio of coarse particles> In this specification, the ratio of coarse particles is 2 to 10 times the median diameter (D50) based on the number of the vinyl resin particles of the present invention relative to the total number of the particles. Grain This refers to the percentage of particles having the same diameter.

[0040] The vinyl resin particles of the present invention preferably have a coarse particle ratio of 0 to 5%. If the ratio is within the above range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the pore size of the pores formed in the porous thermosetting resin film is less likely to vary. Therefore, the mechanical strength of the porous thermosetting resin film is improved.

[0041] The vinyl resin particles of the present invention preferably have a coarse particle ratio of 0 to 3%. If the ratio is within the above range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the pore size of the pores formed in the porous thermosetting resin film is less likely to vary. Therefore, the mechanical strength of the porous thermosetting resin film is further improved.

[0042] The vinyl resin particles of the present invention more preferably have a coarse particle ratio of 0 to 1%. If the ratio is within the above range, when a porous thermosetting resin film is formed using the vinyl resin particles of the present invention, the pore size of the pores formed in the porous thermosetting resin film is further reduced. Therefore, the mechanical strength of the porous thermosetting resin film is further improved.

[0043] <Types of monofunctional and polyfunctional monomers> The vinyl-based resin particles of the present invention are preferably polymers having polymerizable vinyl-based monomer units consisting of monofunctional monomer units and polyfunctional monomer units. In particular, the polymerizable vinyl-based monomer units preferably contain 8 to 150 parts by mass of the polyfunctional monomer units per 100 parts by mass of the monofunctional monomer units.

[0044] In the present invention, from the viewpoint of improving the mechanical strength of the porous thermosetting resin film, the polymerizable vinyl monomer unit more preferably contains 12 to 100 parts by mass, and even more preferably contains 18 to 80 parts by mass, of the polyfunctional monomer unit per 100 parts by mass of the monofunctional monomer unit.

[0045] In the present invention, it is preferred that the monofunctional monomer unit is at least one of a monofunctional styrene-based monomer unit and a monofunctional (meth)acrylic monomer unit, and the polyfunctional monomer unit is at least one of a polyfunctional styrene-based monomer unit and a polyfunctional (meth)acrylic monomer unit.

[0046] Examples of monofunctional styrene monomers include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, and styrene sulfonates such as sodium styrene sulfonate and ammonium styrene sulfonate. Among these, styrene, α-methylstyrene, and sodium styrene sulfonate are preferred. These monofunctional styrene monomers may be used alone or in combination of two or more.

[0047] Examples of monofunctional (meth)acrylic monomers include methyl (meth)acrylate (methyl methacrylate, methyl acrylate), ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and (meth)acrylic acid. Examples of the acrylates include (meth)acrylic acid alkyl esters in which the alkyl group bonded to the ester has 1 to 20 carbon atoms, such as nonyl acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. Among these, preferred are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, and decyl (meth)acrylate, in which the number of carbon atoms in the alkyl group bonded to the ester is 1 to 10. One of these (meth)acrylic acid alkyl esters may be used alone, or two or more of them may be used in combination.

[0048] Examples of the polyfunctional styrene monomer include aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, and derivatives thereof. These polyfunctional styrene monomers may be used alone or in combination of two or more.

[0049] Examples of polyfunctional (meth)acrylic monomers include ethylene glycol di(meth)acrylate (ethylene glycol dimethacrylate), trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, decaethylene glycol di(meth)acrylate, pentadecaethylene glycol di(meth)acrylate, pentacontahexaethylene glycol di(meth)acrylate, 1,3-butylene di(meth)acrylate, allyl (meth)acrylate (allyl methacrylate, allyl acrylate), trimethylolpropane tri(meth)acrylate, pentaerythritol tetraacrylate, etc. Among these, ethylene glycol di(meth)acrylate (ethylene glycol dimethacrylate) and allyl (meth)acrylate (allyl methacrylate) are preferred. These polyfunctional (meth)acrylic monomers may be used alone or in combination of two or more.

[0050] <pH of vinyl resin particles> In the present invention, when the vinyl resin particles of the present invention and water are dispersed in water at a mass ratio of 1:10, the resulting dispersion (dispersion of the vinyl resin particles) preferably has a pH of 3 to 9, more preferably 4 to 8, even more preferably 4.5 to 7.5, and particularly preferably 5 to 7.

[0051] The water may be, for example, natural water, purified water, distilled water, ion-exchanged water, pure water, etc. Among these waters, ion-exchanged water is preferred. Furthermore, ion-exchanged water having a pH in the range of 5.5 to 7 is more preferred.

[0052] <Thermosetting resin> The vinyl resin particles of the present invention are used for the porosity of thermosetting resins. Examples of the thermosetting resin include polyphenylene ether resin, divinyl benzyl ether resin, polyarylate resin, diallyl phthalate resin, polyimide resin, benzoxazine resin, benzoxazole resin, bismaleimide resin, acrylate resin, and the like. Among these thermosetting resins, the vinyl resin particles of the present invention can be preferably used particularly as a porosity material for polyimide resins. When the vinyl resin particles of the present invention are used as a porosity material for polyimide resins, uniform pores can be formed in the polyimide resin film.

[0053] <Rsp value> In the present invention, the Rsp value of the vinyl resin particles is used as an index indicating the affinity between the vinyl resin particles and the thermosetting resin precursor solution.

[0054] The Rsp value is a numerical value defined by the "transverse relaxation time T2 (ms)" obtained by analyzing the physical properties of the thermosetting resin precursor solution in which the vinyl resin particles of the present invention are dispersed by pulse NMR.

[0055] The Rsp value is represented by the following formula. Also, the Rsp value can be measured by a pulse NMR particle interface property evaluation apparatus (for example, " Acorn Area", manufactured by Xigo nanotools). Rsp = (Rav - Rb) / Rb

[0056] Rav is the average relaxation time constant. The relaxation time constant is the reciprocal of the proton relaxation time of the thermosetting resin precursor solution that is in contact with or adsorbed on the surface of the vinyl resin particles when the vinyl resin particles are dispersed in the thermosetting resin precursor solution. The average relaxation time constant is the average value of the obtained relaxation time constants.

[0057] Rb is the proton relaxation time constant of the blank thermosetting resin precursor solution that does not contain vinyl resin particles.

[0058] A larger Rsp value indicates a stronger interaction between the particle surfaces of the vinyl resin particles and the thermosetting resin precursor solution.

[0059] The pulsed NMR method observes the spin (magnetic) state of an object, and measures the time (spin-spin relaxation time) from immediately after the application of energy (excited state) until it returns to a steady state. When the object is a solvent, the relaxation time of the solvent molecules (hydrogen nuclei) is measured, but in particle dispersions, the relaxation time changes depending on the state of the particles in the solvent. This is because the relaxation time is affected by the amount of solvent molecules in contact with the particles. Here, the amount of solvent molecules in contact with the particles is thought to change depending on the surface area of ​​the particles and the wettability between the solvent and the molecules. Therefore, by measuring the relaxation time of the solvent in a dispersion in which specific particles are dispersed using pulsed NMR, it is possible to capture the interface state between the solvent and the particles, and from this, it is possible to analyze minute changes in the state of the particle surface from the relaxation time of the solvent molecules.

[0060] In pulsed NMR, there are various evaluation methods that are suitable depending on the relaxation time, and the CPMG method is preferably used especially for samples with long relaxation times such as liquids.

[0061] In the vinyl resin particles of the present invention, the Rsp value represented by the following formula (1) is preferably 5 or more and 150 or less. Rsp = (Rav - Rb) / Rb (1) Rav: The reciprocal of the average value of the transverse relaxation time T2 (ms) obtained by measurement method 1 below Rb: the reciprocal of the transverse relaxation time T2 (ms) obtained by measurement method 2 below [Measurement method 1] For a polyimide precursor varnish obtained by mixing a vinyl resin particle dispersion liquid obtained by mixing the vinyl resin particles of the present invention and a first organic solvent in a mass ratio of 1:3, a polyimide precursor solution having a solid content concentration of 18±1 mass%, and a second organic solvent in a mass ratio of 6:3.61:1.8, the transverse relaxation time T2 (ms) of protons derived from the varnish is measured three times repeatedly by the CPMG method (Carr-Purcell Meiboom-Gill method) under measurement conditions of using hydrogen nuclei as the measurement nucleus, measuring temperature of 20°C, resonant frequency of 13 MHz, and 90° pulse width of 5.81 μs, and the average value is calculated. The reciprocal of the average value is defined as Rav. [Measurement method 2] For a blank solution obtained by mixing a first organic solvent, a polyimide precursor solution having a solids concentration of 18±1% by mass, and a second organic solvent in a mass ratio of 4.5:3.61:1.8, the transverse relaxation time T2 (ms) of protons derived from the blank solution was measured three times by the CPMG method under measurement conditions of a hydrogen nucleus as the measurement nucleus, a measurement temperature of 20°C, a resonance frequency of 13 MHz, and a 90° pulse width of 5.81 μs, and the average value was calculated. The reciprocal of the average value was designated as Rb.

[0062] When the Rsp value represented by the above formula (1) is 5 or more, the affinity between the vinyl resin particles and the thermosetting resin precursor solution is not too low, and an increase in the viscosity of the thermosetting resin precursor solution in which the vinyl resin particles are dispersed tends to be suppressed.

[0063] When the Rsp value represented by the above formula (1) is 150 or less, the affinity between the vinyl resin particles and the thermosetting resin precursor solution does not become too high, and a decrease in the viscosity of the thermosetting resin precursor solution in which the vinyl resin particles are dispersed tends to be suppressed.

[0064] The Rsp value represented by the above formula (1) is more preferably 8 or more and 100 or less, further preferably 10 or more and 80 or less, and particularly preferably 15 or more and 70 or less.

[0065] The first organic solvent and the second organic solvent are the same solvent in both the measurement method 1 and the measurement method 2. The first organic solvent and the second organic solvent in the measurement method 1 and the measurement method 2 are the same solvent.

[0066] Examples of the first organic solvent and the second organic solvent include phenol-based solvents such as phenol and m-cresol; amide-based solvents such as N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), and N,N-dimethylacetamide (DMAc); lactone-based solvents such as γ-butyrolactone (GBL), δ-valerolactone, ε-caprolactone, γ-crotonolactone, γ-hexanolactone, α-methyl-γ-butyrolactone, γ-valerolactone, α-acetyl-γ-butyrolactone, and δ-hexanolactone; sulfoxide-based solvents such as N,N-dimethylsulfoxide (DMSO); ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, and dimethyl carbonate. Among these, NMP, GBL, and DMAC are preferred from the viewpoint of the solubility of the polyimide precursor.

[0067] In the vinyl resin particles of the present invention, the Rsp value represented by the following formula (1) is more preferably 5 or more and 150 or less. Rsp = (Rav - Rb) / Rb (1) Rav: The reciprocal of the average value of the transverse relaxation time T2 (ms) obtained by measurement method 1 below Rb: the reciprocal of the transverse relaxation time T2 (ms) obtained by measurement method 2 below [Measurement method 1] The vinyl resin particle dispersion of the present invention and the first organic solvent NMP, GBL or DMAC are mixed in a mass ratio of 1:3, a polyimide precursor solution having a solid content concentration of 18±1 mass%, and a polyimide precursor varnish which is mixed in a mass ratio of 6:3.61:1.8 with NMP, GBL or DMAC as the second organic solvent. The measurement nucleus is hydrogen nucleus, and the measurement conditions are 20°C, 13MHz resonance frequency, and 5.81μs 90° pulse width. The transverse relaxation time T2 (ms) of the proton derived from the varnish is measured three times by the CPMG method (Carr-Purcell Meiboom-Gill method), and the average value is calculated. The reciprocal of the average value is Rav. However, the first organic solvent and the second organic solvent are the same solvent. [Measurement method 2] For a blank solution obtained by mixing the first organic solvent used in the above-mentioned Measurement Method 1, a polyimide precursor solution having a solids concentration of 18±1% by mass, and the second organic solvent used in the above-mentioned Measurement Method 1 in a mass ratio of 4.5:3.61:1.8, the transverse relaxation time T2 (ms) of protons derived from the blank solution was measured three times by the CPMG method under measurement conditions of using hydrogen nuclei as the measurement nuclei, a measurement temperature of 20°C, a resonance frequency of 13 MHz, and a 90° pulse width of 5.81 μs, and the average value was calculated. The reciprocal of the average value was designated as Rb.

[0068] 2. Method for producing vinyl resin particles The vinyl resin particle production method A and the production method B of the present invention will be described in detail below. However, the present invention is not limited to the production methods described below.

[0069] (Method A of Producing Vinyl Resin Particles) The production method A is a method for producing vinyl resin particles having (1) a seed polymerization step, (2) a spray drying step, and (3) a crushing step in this order. Furthermore, in the seed polymerization step of the production method A, the first polymerizable vinyl monomer contains a monofunctional monomer and a polyfunctional monomer, and the first polymerizable vinyl monomer contains 8 to 150 parts by mass of the polyfunctional monomer per 100 parts by mass of the monofunctional monomer.

[0070] The above steps (1) to (3) will now be described in detail.

[0071] <Seed polymerization process> In production method A, the seed polymerization process is a process of obtaining an aqueous dispersion containing polymer particles of the first polymerizable vinyl monomer and an aqueous medium by absorbing the first polymerizable vinyl monomer into seed particles and carrying out seed polymerization (a slurry containing polymer particles).

[0072] In the manufacturing method A, the seed polymerization is a process in which a seed particle is impregnated with and absorbs a first polymerizable vinyl monomer, and then a second polymerizable vinyl monomer is impregnated with and absorbs a second polymerizable vinyl monomer. 1 As the seed polymerization in Production Method A, for example, the method described in JP-A-2010-138365 can be applied.

[0073] The seed particles can be produced by applying a known method. For example, the seed particles can be produced by applying the method described in WO 2013 / 030977.

[0074] The seed particles can be obtained by emulsion polymerization, preferably soap-free polymerization, of a monomer for producing the seed particles in an aqueous medium.

[0075] The monomer for producing the seed particles is preferably a monofunctional monomer.

[0076] The monofunctional monomer is preferably at least one of a monofunctional styrene-based monomer and a monofunctional (meth)acrylic monomer.

[0077] Examples of monofunctional styrene monomers include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, and styrene sulfonates such as sodium styrene sulfonate and ammonium styrene sulfonate. Among these, styrene, α-methylstyrene, and sodium styrene sulfonate are preferred. These monofunctional styrene monomers may be used alone or in combination of two or more.

[0078] Examples of monofunctional (meth)acrylic monomers include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, ) isononyl acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and other (meth)acrylic acid alkyl esters in which the alkyl group bonded to the ester has 1 to 20 carbon atoms. Among these, preferred are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, and decyl (meth)acrylate, in which the number of carbon atoms in the alkyl group bonded to the ester is 1 to 10. One of these (meth)acrylic acid alkyl esters may be used alone, or two or more of them may be used in combination.

[0079] Examples of the aqueous medium for producing the seed particles include water and a mixed solvent of water and an organic solvent (e.g., a hydrophilic organic solvent such as a lower alcohol having 5 or less carbon atoms). The amount of the aqueous medium used is preferably 100 to 1000 parts by mass relative to 100 parts by mass of the monofunctional monomer in order to stabilize the vinyl resin particles.

[0080] In addition, in the seed polymerization step, in order to suppress the generation of emulsified particles in an aqueous medium, a known polymerization inhibitor commonly used in this field can be widely used. Examples of the polymerization inhibitor include nitrite compounds such as sodium nitrite. The polymerization inhibitor can be used in an amount of 0.1 to 10 parts by mass relative to 100 parts by mass of the monofunctional monomer.

[0081] Furthermore, in the seed polymerization step, in order to adjust the molecular weight, a known molecular weight regulator commonly used in this field can be widely used. The molecular weight regulator can be used in an amount of 0.1 to 10 parts by mass based on 100 parts by mass of the monofunctional monomer.

[0082] In the production of the seed particles, a water-soluble polymerization initiator is usually used. The water-soluble polymerization initiator may be any polymerization initiator that is soluble in an aqueous medium, and any known water-soluble polymerization initiator may be used. For example, peroxides such as potassium persulfate and ammonium persulfate, and azos such as 2,2-azobis-(2-methylpropionamidine)-dihydrochloride, 2,2-azobis-[2-(2-imidazolin-2-yl)propane])-dihydrochloride, and 4,4-azobis-(4-cyanovaleric acid) may be used.

[0083] The water-soluble polymerization initiator is usually used in an amount of 0.1 to 5 parts by mass based on 100 parts by mass of the monofunctional monomer. The polymerization for producing the seed particles can be carried out by heating at 50 to 80° C. for 2 to 20 hours.

[0084] The first polymerizable vinyl monomer includes a monofunctional monomer and a polyfunctional monomer, and the first polymerizable vinyl monomer contains 30 to 100 parts by mass of the polyfunctional monomer per 100 parts by mass of the monofunctional monomer.

[0085] In the seed polymerization step, if the content of the polyfunctional monomer is less than 30 parts by mass relative to 100 parts by mass of the monofunctional monomer, the solvent resistance of the vinyl resin particles may be reduced. Also, when preparing a thermosetting resin precursor, the vinyl resin particles tend to swell in a solvent, which may increase the viscosity of the precursor, which is undesirable from the viewpoint of handling.

[0086] In the seed polymerization step, if the content of the polyfunctional monomer is more than 100 parts by mass relative to 100 parts by mass of the monofunctional monomer, it becomes difficult to decompose the vinyl resin particles added when making the thermosetting resin porous, and therefore the vinyl resin particles remain in the thermosetting resin, and when a thermosetting resin film is produced, the thermosetting resin film may not be made porous.

[0087] In the seed polymerization step, in order to improve the solvent resistance of the vinyl resin particles, the first polymerizable vinyl monomer preferably contains 8 to 150 parts by mass, more preferably 12 to 100 parts by mass, and even more preferably 18 to 80 parts by mass of a polyfunctional monomer per 100 parts by mass of a monofunctional monomer.

[0088] In the seed polymerization step, the monofunctional monomer is preferably at least one of a monofunctional styrene-based monomer and a monofunctional (meth)acrylic monomer.

[0089] Examples of monofunctional styrene monomers include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, and styrene sulfonates such as sodium styrene sulfonate and ammonium styrene sulfonate. Among these, styrene, α-methylstyrene, and sodium styrene sulfonate are preferred. These monofunctional styrene monomers may be used alone or in combination of two or more.

[0090] Examples of monofunctional (meth)acrylic monomers include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, ) isononyl acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and other (meth)acrylic acid alkyl esters in which the alkyl group bonded to the ester has 1 to 20 carbon atoms. Among these, preferred are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, and decyl (meth)acrylate, in which the number of carbon atoms in the alkyl group bonded to the ester is 1 to 10. One of these (meth)acrylic acid alkyl esters may be used alone, or two or more of them may be used in combination.

[0091] In the seed polymerization step, the polyfunctional monomer is at least one of a polyfunctional styrene monomer and a polyfunctional (meth)acrylic monomer. By using the polyfunctional monomer, the solvent resistance of the vinyl resin particles obtained is improved, and the viscosity increase of the polyimide varnish caused by the swelling of the vinyl resin particles obtained can be suppressed.

[0092] Examples of the polyfunctional styrene monomer include aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, and derivatives thereof. These polyfunctional styrene monomers may be used alone or in combination of two or more.

[0093] Examples of the polyfunctional (meth)acrylic monomer include ethylene glycol di(meth)acrylate (ethylene glycol dimethacrylate), trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, decaethylene glycol di(meth)acrylate, pentadecaethylene glycol di(meth)acrylate, pentacontahexaethylene glycol di(meth)acrylate, 1,3-butylene di(meth)acrylate, allyl (meth)acrylate (allyl methacrylate), trimethylolpropane tri(meth)acrylate, and pentaerythritol tetraacrylate. Among these, ethylene glycol di(meth)acrylate (ethylene glycol dimethacrylate) and allyl (meth)acrylate (allyl methacrylate) are preferred. These polyfunctional (meth)acrylic monomers may be used alone or in combination of two or more.

[0094] In the seed polymerization step, an oil-soluble polymerization initiator is usually used. The oil-soluble initiator may be any polymerization initiator that is soluble in an aqueous medium, and any known oil-soluble polymerization initiator may be used. For example, peroxides such as benzoyl peroxide (BPO), lauroyl peroxide, bis-3,5,5-trimethylhexanoyl peroxide, t-butylperoxy-2-ethylhexanoate, di-t-butylperoxyhexahydroterephthalate, and t-butylperoxyisobutyrate, and azos such as azobisisobutyronitrile, azobisisovaleronitrile, 2,2-azobis-(2-methylpropionate), and 2,2-azobis-(2,4-dimethylvaleronitrile) (ADVN) may be mentioned. The amount of the oil-soluble polymerization initiator used is preferably 0.001 to 3 parts by mass, more preferably 0.003 to 1 part by mass, and even more preferably 0.004 to 0.5 parts by mass, based on 100 parts by mass of the total of the monofunctional monomer and the polyfunctional monomer.

[0095] In the seed polymerization step, in order to improve the polymerization stability during the preparation of the polymer particles of the first polymerizable vinyl monomer and to enhance the effect of suppressing the fusion of the polymer particles with each other, a suspension stabilizer can be used. Examples of the suspension stabilizer include water-soluble polymers such as polyvinyl alcohol and polyvinylpyrrolidone.

[0096] The amount of the suspension stabilizer used is usually 0.5 to 15 parts by mass per 100 parts by mass of the total of the monofunctional monomer and the polyfunctional monomer.

[0097] In the seed polymerization step, a surfactant can be used. By adding a surfactant, it is possible to suppress fusion between particles constituting the polymer particles obtained by seed polymerization. In addition, it is possible to promote absorption of the monomer mixture into seed particles in the seed polymerization described below by emulsifying the monomer mixture in an aqueous medium with a surfactant.

[0098] As the surfactant, any of anionic, cationic, nonionic and amphoteric surfactants can be used.

[0099] Examples of anionic surfactants include dialkyl sulfosuccinates such as sodium dioctyl sulfosuccinate; phosphates such as sodium polyoxyethylene alkyl phenyl ether phosphate (e.g., sodium polyoxyethylene nonyl phenyl ether phosphate) and sodium polyoxyalkylene aryl ether phosphate; fatty acid oils such as sodium oleate and potassium castor oil; alkyl sulfates such as sodium lauryl sulfate and ammonium lauryl sulfate; alkyl benzene sulfonates such as sodium dodecyl benzene sulfonate; alkyl naphthalene sulfonates; alkanesulfonates; alkyl phosphate ester salts; naphthalene sulfonate-formaldehyde condensates; polyoxyethylene alkyl phenyl ether sulfate ester salts; and polyoxyethylene alkyl sulfate ester salts.

[0100] Examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene tridecyl ether, polyoxyethylene alkylphenyl ethers, polyoxyethylene styrenated phenyl ethers, polyoxyalkylene alkyl ethers such as polyoxyalkylene tridecyl ethers in which the alkylene group has 3 or more carbon atoms, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene alkylamines, glycerin fatty acid esters, and oxyethylene-oxypropylene block copolymers.

[0101] Examples of cationic surfactants include alkylamine salts such as laurylamine acetate and stearylamine acetate, and quaternary ammonium salts such as lauryltrimethylammonium chloride.

[0102] Examples of zwitterionic surfactants include lauryl dimethylamine oxide, and phosphate or phosphite surfactants.

[0103] Among the above surfactants, it is preferable to use at least one of an anionic surfactant and a nonionic surfactant. Among the above surfactants, dioctyl sodium sulfosuccinate and sodium polyoxyethylene nonylphenyl ether phosphate are preferable as anionic surfactants, and polyoxyethylene alkylphenyl ether and polyoxyethylene styrenated phenyl ether are preferable as nonionic surfactants.

[0104] The amount of the surfactant used is preferably 0.001 to 5 parts by mass, more preferably 0.005 to 3 parts by mass, and even more preferably 0.01 to 1 part by mass, per 100 parts by mass of the total of the monofunctional monomer and the polyfunctional monomer.

[0105] In the seed polymerization step, an antioxidant can be used to improve the heat resistance of the vinyl resin particles.Examples of the antioxidant include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxymethyl]methane, tris[N-(3,5-di-t-butyl-4-hydroxybenzyl)]isocyanurate, butylidene-1,1-bis(2-methyl-4-hydroxy-5-t-butylphenyl), triethylene glycol bis[3-(3-t-butyl-4-hydroxyphenyl)propionyloxymethyl]methane, phenolic antioxidants such as 3,9-bis{2-[3(3-t-butyl-4-hydroxy-5-methylphenyl)propionate], 3,9-bis{2-[3(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane; dilauryl-3,3'-thio-dipropionate, dimyristyl-3,3'-thio-dipropionate, distearyl-3,3'-thio-dipropionate, pentaerythritol tetrakis(3-laurylthio-propionate), pentaerythritol tetrakis(3-laurylthio-propionate), bisthioglycolate (PETG), pentaerythritol thiopropionate, pentaerythritol tetrakis(4-butanate), pentaerythritol tetrakis(6-mercaptohexanate), trimethylolpropane tristhioglycolate, trimethylolpropane tristhiopropionate, trimethylolpropane tristhiobutanate, butanediol bisthioglycolate, ethylene glycol bisthioglycolate, hexanediol bisthioglycolate, butanediol bisthiopropionate, ethylene glycol Sulfur-based antioxidants such as coal bisthiopropionate, octyl thioglycolate, 1-octanethiol, 1-dodecanethiol, and thiosalicylic acid; and phosphorus-based antioxidants such as tris(nonylphenyl)phosphite, tris(2,4-di-t-butylphenyl)phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-t-butylphenyl)pentaerythritol phosphite, and 2,2-methylenebis(4,6-di-t-butylphenyl)-4,4'-biphenylene diphosphonite can be used.These antioxidants can be used alone or in combination of two or more kinds.

[0106] The amount of the antioxidant used is preferably 0.001 to 5 parts by mass, more preferably 0.005 to 3 parts by mass, and even more preferably 0.01 to 1 part by mass, per 100 parts by mass of the total of the monofunctional monomer and the polyfunctional monomer.

[0107] <Spray drying process> In the production method A, the spray drying step is a step of spray drying the aqueous dispersion (slurry containing polymer particles) obtained in the seed polymerization step under conditions of a slurry inlet temperature of 80°C to 220°C and a powder outlet temperature of 50°C to 100°C to obtain an aggregate.

[0108] In the spray drying step, spray drying is carried out in order to obtain an aggregate of vinyl resin particles from a slurry containing polymer particles.

[0109] The spray drying method generally involves spraying a slurry containing polymer particles using a spray dryer such as a spray drier to dry the particles. By appropriately adjusting the supply rate of the slurry containing polymer particles in the spray drying, the drying temperature, the atomizer rotation speed of the spray dryer, etc., it is possible to adjust the particle size, particle shape, etc. of the aggregate of vinyl resin particles.

[0110] The drying temperature is within the range of 80°C to 220°C for the inlet of the polymer particle-containing slurry, where the polymer particle-containing slurry is sprayed and introduced, and 50°C to 100°C for the powder outlet, where the vinyl resin particle aggregate is discharged. If the inlet temperature of the polymer particle-containing slurry is higher than 220°C, the vinyl resin particles are more likely to fuse together, forming an aggregate of vinyl resin particles in which the vinyl resin particles are linked to each other. If the inlet temperature of the polymer particle-containing slurry is lower than 80°C, the drying is more likely to be insufficient, and problems such as too low drying efficiency arise.

[0111] Furthermore, if the powder outlet temperature is lower than 50° C., drying may be insufficient, whereas if the powder outlet temperature is higher than 100° C., there arises a problem that the vinyl resin particles are more likely to fuse together.

[0112] The temperature of the slurry inlet containing the polymer particles is preferably 90°C to 200°C, and the temperature of the powder outlet from which the aggregates of vinyl resin particles are discharged is preferably 55°C to 95°C.

[0113] Furthermore, the temperature of the slurry inlet containing the polymer particles is preferably 30 to 120° C. higher than the aggregate outlet temperature (the powder outlet temperature from which the aggregates of vinyl resin particles are discharged) from the viewpoint of preventing mutual fusion of the vinyl resin particles.

[0114] <Crushing process> In the production method A, the crushing step is a step of obtaining vinyl resin particles by crushing the aggregates obtained in the spray drying step.

[0115] In the disintegration step, by using a fine pulverizer, the aggregates obtained in the spray drying step can be disintegrated with high disintegration efficiency to obtain vinyl resin particles.

[0116] As the above-mentioned fine pulverizer, a swirling jet mill such as a Current Jet Mill or a Super Jet Mill (manufactured by Nisshin Engineering Co., Ltd.) can be used.

[0117] <Classification process> It is preferable that the production method A includes at least one of a first classification step of classifying the polymer particles in the aqueous dispersion obtained in the seed polymerization step, and a second classification step of classifying the vinyl resin particles obtained in the disintegration step.

[0118] In the first classification process, coarse particles larger than the mesh size of the sieve can be removed by wet classification using a nylon mesh. For example, in the first classification process, coarse particles of 32 μm or more can be removed by using a 400 Mesh nylon net.

[0119] In the second classification step, classification can be performed using classifiers such as an elbow jet (manufactured by Nippon Steel Mining Co., Ltd.) with an inertial classification method, a turbo plex (manufactured by Hosokawa Micron Corporation) with a centrifugal classification method, a TSP separator (manufactured by Hosokawa Micron Corporation), and a faculty (manufactured by Hosokawa Micron Corporation), etc., to obtain vinyl resin particles having a desired particle size. For example, in the second classification step, by performing air classification, vinyl resin particles that can be used as products can be obtained.

[0120] <pH Adjustment Step> The production method A preferably includes a step of adjusting the pH of the aqueous dispersion to 3 to 9 by adding a nitrogen-containing compound to the aqueous dispersion (slurry containing polymer particles) obtained in the above seed polymerization step.

[0121] The nitrogen-containing compound is preferably at least one selected from the group consisting of ammonia, alkanolamine, and polyamine.

[0122] Examples of alkanolamine include monoethanolamine, diethanolamine, triethanolamine, isopropanolamine, etc.

[0123] Examples of polyamine include aliphatic amines such as ethylenediamine, propylenediamine, hexamethylenediamine, diethylenetriamine, and triethylenetetramine; aromatic polyamines such as phenylenediamine and tolylenediamine; and heterocyclic polyamines such as piperazine and aminoethylpiperazine.

[0124] (Production Method B of Vinyl Resin Particles) The production method B is a production method of vinyl resin particles having (1) an emulsion polymerization step, (2) a spray drying step, and (3) a crushing step in this order. Hereinafter, these steps will be specifically described.

[0125] <Emulsion Polymerization Step> In production method B, the emulsion polymerization step is a step of emulsion polymerizing a second polymerizable vinyl monomer in an aqueous medium to obtain an aqueous dispersion (a slurry containing polymer particles) containing polymer particles of the second polymerizable vinyl monomer and an aqueous medium.

[0126] Emulsion polymerization has the characteristic that the particle diameter of the particles constituting the obtained aggregate varies little. As the emulsion polymerization in Production Method B, for example, the method described in JP-A-2010-138365 can be applied.

[0127] In the production method B, among emulsion polymerizations, soap-free polymerization, which is emulsion polymerization that does not use a surfactant, is preferred.

[0128] In the emulsion polymerization step of the production method B, 2 The polymerizable vinyl monomer is preferably at least one of a monofunctional monomer and a polyfunctional monomer.

[0129] The monofunctional monomer is preferably at least one of a monofunctional styrene-based monomer and a monofunctional (meth)acrylic monomer.

[0130] Examples of monofunctional styrene monomers include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, and styrene sulfonates such as sodium styrene sulfonate and ammonium styrene sulfonate. Among these, styrene, α-methylstyrene, and sodium styrene sulfonate are preferred. These monofunctional styrene monomers may be used alone or in combination of two or more.

[0131] Examples of monofunctional (meth)acrylic monomers include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, ) isononyl acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and other (meth)acrylic acid alkyl esters in which the alkyl group bonded to the ester has 1 to 20 carbon atoms. Among these, preferred are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, and decyl (meth)acrylate, in which the number of carbon atoms in the alkyl group bonded to the ester is 1 to 10. One of these (meth)acrylic acid alkyl esters may be used alone, or two or more of them may be used in combination.

[0132] In the emulsion polymerization step, the second polymerizable vinyl monomer may be used in combination with other monomers such as a vinyl halide monomer, a vinyl cyanide monomer, etc. Examples of the vinyl halide monomer include vinyl chloride, vinylidene chloride, etc. Examples of the vinyl cyanide monomer include acrylonitrile, methacrylonitrile, etc.

[0133] In the emulsion polymerization step, the aqueous medium may be, for example, water or a mixed solvent of water and an organic solvent (for example, a hydrophilic organic solvent such as a lower alcohol having 5 or less carbon atoms). In order to stabilize the vinyl resin particles, the amount of the aqueous medium used is preferably 100 to 1000 parts by mass relative to 100 parts by mass of the second polymerizable vinyl monomer.

[0134] Furthermore, in the emulsion polymerization step, in order to adjust the molecular weight, a known molecular weight regulator commonly used in this field can be widely used. The molecular weight regulator can be used in an amount of 0.1 to 10 parts by mass per 100 parts by mass of the second polymerizable vinyl monomer.

[0135] In the emulsion polymerization step, a water-soluble polymerization initiator is usually used. The water-soluble polymerization initiator may be any polymerization initiator that is soluble in an aqueous medium, and known water-soluble polymerization initiators can be used. For example, peroxides such as potassium persulfate and ammonium persulfate (APS), and azos such as 2,2-azobis-(2-methylpropionamidine)-dihydrochloride, 2,2-azobis-[2-(2-imidazolin-2-yl)propane])-dihydrochloride, and 4,4-azobis-(4-cyanovaleric acid) can be mentioned. The water-soluble polymerization initiator is usually used in an amount of 0.1 to 5 parts by mass relative to 100 parts by mass of the second polymerizable vinyl monomer.

[0136] In the emulsion polymerization step, a wide variety of known surfactants commonly used in this field can be used. By adding a surfactant, it is possible to suppress fusion between particles constituting the polymer obtained by emulsion polymerization. In addition, when performing soap-free polymerization, it is not necessary to add a surfactant.

[0137] In the emulsion polymerization step, the average particle size can be adjusted by performing seed emulsion polymerization using seed particles. When a monomer mixture, a water-soluble initiator, and seed particles are added to an aqueous medium and emulsion polymerization is performed, the vinyl monomer is absorbed into the seed particles as oligosoap while polymerization proceeds, and polymer particles with a uniform particle size can be obtained.

[0138] The seed particles can be obtained by emulsion polymerization, preferably soap-free polymerization, of a monomer for producing the seed particles in an aqueous medium.

[0139] The second polymerizable vinyl monomer can be used as the monomer for producing the seed particles, and among the second polymerizable vinyl monomers, it is preferable to use at least one of the monofunctional styrene monomer and the monofunctional (meth)acrylic monomer. As the monofunctional styrene monomer, styrene, α-methylstyrene, and sodium styrenesulfonate are preferable. As the monofunctional (meth)acrylic monomer, methyl (meth)acrylate is preferable.

[0140] As the aqueous medium for producing the seed particles, the aqueous media described above can be used.

[0141] In the production of the seed particles, the above-mentioned water-soluble polymerization initiator can be used. The water-soluble polymerization initiator is usually used in an amount of 0.1 to 5 parts by mass based on 100 parts by mass of the monomer for producing the seed particles.

[0142] In the production of the seed particles, a molecular weight regulator commonly used in this field can be widely used to adjust the molecular weight. The molecular weight regulator is preferably used in the range of 0.1 to 10 parts by mass based on 100 parts by mass of the monomer for producing the seed particles.

[0143] The polymerization for producing the seed particles can be carried out by heating at 50 to 80° C. for 2 to 20 hours.

[0144] The second polymerizable vinyl monomer is absorbed into the seed particles as an oligosoap while polymerization proceeds, thereby obtaining polymer particles derived from the polymerizable vinyl monomer.

[0145] The polymerization temperature can be appropriately selected depending on the type of the second polymerizable vinyl monomer and the polymerization initiator. The polymerization temperature is preferably 25 to 110° C., more preferably 50 to 100° C. The polymerization time is preferably 1 to 12 hours.

[0146] <Spray drying process> In production method B, the spray drying step is a step of spray-drying the aqueous dispersion (slurry containing polymer particles) obtained in the above emulsion polymerization step under conditions of an inlet temperature of 80°C to 220°C and an outlet temperature of 50°C to 100°C to obtain an aggregate.

[0147] In the spray drying step, spray drying is carried out in order to obtain an aggregate of vinyl resin particles from a slurry containing polymer particles.

[0148] The spray drying method is generally a method of spraying a slurry containing polymer particles using a spray dryer such as a spray drier, and drying the particles. By appropriately adjusting the supply speed of the slurry containing polymer particles in the spray drying, the drying temperature, the atomizer rotation speed of the spray dryer, etc., it is possible to adjust the particle size, particle shape, etc. of the aggregate of vinyl resin particles.

[0149] The drying temperature is within a range of 80°C to 220°C for the temperature at the slurry inlet containing the polymer particles (hereinafter also referred to as the slurry inlet temperature) where the slurry containing the polymer particles is sprayed and introduced, and within a range of 50°C to 100°C for the powder outlet temperature where the aggregates of vinyl resin particles are discharged.

[0150] If the inlet temperature of the slurry containing polymer particles is higher than 220° C., the vinyl resin particles are more likely to fuse together, forming an aggregate of vinyl resin particles in which the vinyl resin particles are linked to each other.

[0151] When the slurry inlet temperature containing polymer particles is less than 80°C, drying tends to be insufficient, and problems such as too low drying efficiency occur.

[0152] Also, when the powder outlet temperature is lower than 50°C, there is a risk that drying will be insufficient. On the other hand, when the powder outlet temperature is higher than 100°C, the problem that fusion between vinyl resin particles easily occurs arises.

[0153] The temperature of the slurry inlet containing polymer particles is preferably 90°C to 200°C, and the powder outlet temperature at which the aggregate of vinyl resin particles is discharged is preferably 55 to 95°C.

[0154] Furthermore, from the viewpoint of preventing fusion between vinyl resin particles, the temperature of the slurry inlet containing polymer particles is preferably 30 to 120°C higher than the aggregate outlet temperature (the powder outlet temperature at which the aggregate of vinyl resin particles is discharged).

[0155] <Crushing step> In Production Method B, the crushing step is a step of obtaining vinyl resin particles by crushing the aggregate obtained in the spray drying step.

[0156] In the crushing step, by using a fine crusher, the aggregate obtained in the spray drying step can be crushed with high crushing efficiency to obtain vinyl resin particles.

[0157] As the above fine crusher, a swirling flow type jet mill such as a current jet mill or a super jet mill (manufactured by Nisshin Engineering Co., Ltd.) can be used.

[0158] <pH adjustment step> Production Method B preferably includes a pH adjustment step of adjusting the pH of the above aqueous dispersion (slurry containing polymer particles) obtained in the above emulsion polymerization step to 3 to 9 by adding a nitrogen-containing compound.

[0159] The production method B preferably includes a pH adjustment step between the emulsion polymerization step and the spray drying step.

[0160] When soap-free polymerization is carried out using a persulfate as a polymerization initiator in the emulsion polymerization step, anions such as persulfate ions are present on the surfaces of the polymer particles obtained by the above-mentioned Production Method B, and the particles are negatively charged. If a polyimide precursor varnish is prepared using negatively charged vinyl resin particles, electrostatic repulsion occurs between the polyamic acid, which is the polyimide precursor, and the negatively charged vinyl resin particles, which may lead to an increase in the viscosity of the polyimide precursor varnish.

[0161] On the other hand, it is presumed that by adding a nitrogen-containing compound to a slurry containing polymer particles, amines derived from the nitrogen-containing compound become counter cations to persulfate ions and are unevenly distributed, thereby suppressing the electrostatic repulsion and preventing an increase in the viscosity of the polyimide precursor varnish.

[0162] The nitrogen-containing compound is preferably at least one selected from the group consisting of ammonia, alkanolamines and polyamines.

[0163] Examples of alkanolamines include monoethanolamine, diethanolamine, triethanolamine, and isopropanolamine.

[0164] Examples of polyamines include aliphatic amines such as ethylenediamine, propylenediamine, hexamethylenediamine, diethylenetriamine, and triethylenetetramine; aromatic polyamines such as phenylenediamine and tolylenediamine; and heterocyclic polyamines such as piperazine and aminoethylpiperazine.

[0165] The presence of amines on the surface of vinyl resin particles can be confirmed by various analytical methods, for example, by a change in pH.

[0166] Specifically, when soap-free polymerization is carried out using a persulfate as a polymerization initiator, the pH of the slurry is 1 to 2, which is in the strongly acidic range, but this can be confirmed by adding a nitrogen-containing compound so that the pH becomes 3 to 9, which is in the weakly acidic to weakly basic range.

[0167] In addition, the presence of amines on the surfaces of vinyl resin particles can also be confirmed by analysis using TOF-SIMS (time-of-flight secondary ion mass spectrometry).

[0168] <Classification process> It is preferable that the production method B includes at least one of a first classification step of classifying the polymer particles in the aqueous dispersion obtained in the above emulsion polymerization step, and a second classification step of classifying the vinyl resin particles obtained in the above disintegration step.

[0169] It is preferable that the production method B comprises the first classification step between the pH adjustment step and the spray drying step.

[0170] In the first classification process, coarse particles larger than the mesh size of the sieve can be removed by wet classification using a nylon mesh. For example, in the first classification process, coarse particles of 32 μm or more can be removed by using a 400 Mesh nylon net.

[0171] In the second classification step, vinyl resin particles having a desired particle size can be obtained by classification using a classifier such as Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.) of an inertial classification method, Turboplex (manufactured by Hosokawa Micron Corporation), TSP Separator (manufactured by Hosokawa Micron Corporation), Faculty (manufactured by Hosokawa Micron Corporation), etc. For example, in the second classification step, vinyl resin particles usable as products can be obtained by air classification.

[0172] 3. Method for producing porous membrane The method for producing the porous membrane will be described in detail below. Note that the method for producing the porous membrane is not limited to the following method.

[0173] The method for producing a porous film includes, in this order, (1) a step of preparing a coating liquid for forming a porous film containing vinyl-based resin particles and a thermosetting resin precursor, (2) a step of applying the coating liquid for forming a porous film onto a substrate to form an unsintered composite film containing the vinyl-based resin particles, and (3) a step of sintering the unsintered composite film to form a porous film.

[0174] The porous film produced by the above-mentioned production method can be used in any field where a porous film is used, for example, as a heat-resistant material, an insulating material for electronic components, etc.

[0175] The above steps (1) to (3) will now be described in detail.

[0176] <Process (1)> In the method for producing a porous membrane, step (1) is a step of preparing a coating liquid for forming a porous membrane, which contains the vinyl resin particles of the present invention and a thermosetting resin precursor.

[0177] Examples of the thermosetting resin precursor include precursors of polyphenylene ether resin, divinylbenzyl ether resin, polyarylate resin, diallyl phthalate resin, polyimide resin, benzoxazine resin, benzoxazole resin, bismaleimide resin, acrylate resin, and the like.

[0178] An example of a precursor of a polyimide resin is polyamic acid, which can be obtained by polymerizing an aromatic tetracarboxylic dianhydride with an aromatic diamine.

[0179] The mass ratio of the vinyl resin particles to the total mass of the vinyl resin particles and the thermosetting resin precursor is preferably 30 to 70 mass%, more preferably 40 to 60 mass%. Within this range, good coatability of the thermosetting resin precursor solution in which the vinyl resin particles are dispersed can be obtained, so that when a thermosetting resin film (porous film) is produced, the surface of the film can be smoothed.

[0180] The coating liquid for forming a porous film may contain an organic solvent as a diluent. Examples of the organic solvent include phenol-based solvents such as phenol and m-cresol; amide-based solvents such as N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), and N,N-dimethylacetamide (DMAc); lactone-based solvents such as γ-butyrolactone (GBL), δ-valerolactone, ε-caprolactone, γ-crotonolactone, γ-hexanolactone, α-methyl-γ-butyrolactone, γ-valerolactone, α-acetyl-γ-butyrolactone, and δ-hexanolactone; sulfoxide-based solvents such as N,N-dimethylsulfoxide (DMSO); ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, and dimethyl carbonate. Among these, NMP, GBL, and DMAC are preferred.

[0181] The mass ratio of the organic solvent to the total mass of the vinyl resin particles and the thermosetting resin precursor is preferably from 15 to 35% by mass, and more preferably from 20 to 30% by mass.

[0182] <Process (2)> In the method for producing a porous film, step (2) is a step of applying the porous film-forming coating liquid prepared in step (1) onto a substrate to form an unsintered composite film containing the vinyl resin particles of the present invention.

[0183] Examples of the substrate used in this step include substrates mainly made of triacetyl cellulose (TAC), polyethylene terephthalate (PET), polyethylene naphthalate, polybutylene terephthalate, polybutylene naphthalate, polyarylate, polytetramethylene terephthalate, etc. Here, the term "mainly made of" refers to the component that is contained at the highest ratio among the substrate constituents.

[0184] The thickness of the substrate is usually from 20 μm to 300 μm, and preferably from 30 μm to 200 μm.

[0185] The porous film-forming coating liquid is applied onto a substrate, and typically dried at normal pressure at 20 to 80°C for 30 minutes to 2 hours to remove the organic solvent, thereby forming an unsintered composite film containing vinyl resin particles.

[0186] <Process (3)> In the method for producing a porous membrane, step (3) is a step of firing the unfired composite membrane formed in step (2) to form a porous membrane.

[0187] When the green composite film is fired, it may be fired as it is while it is formed on the substrate, or it may be fired after being peeled off from the substrate in advance.

[0188] The firing conditions include, for example, increasing the temperature from 20°C to 320°C at a rate of 10°C / min, and then holding at 320°C for 5 hours, so that the vinyl resin particles are burned off and the desired porous film can be obtained. EXAMPLES

[0189] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples.

[0190] The ion-exchanged water used in the examples and comparative examples is water that has been deionized with an ion-exchange resin and has a conductivity of 1.0 μS / cm or less.

[0191] First, the evaluation methods, measurement methods and calculation methods in the examples and comparative examples will be described.

[0192] <Method for measuring pH of vinyl resin particles> 2 g of the obtained vinyl resin particles were added to 20 g of ion-exchanged water and dispersed using a test tube mixer (manufactured by AS ONE Corporation, "Test Tube Mixer TRIO HM-1N") and an ultrasonic homogenizer (manufactured by Emerson Japan, "BRANSON SONIFIER 450 Advanced") to obtain a dispersion for use.

[0193] The pH of the obtained dispersion was measured with a handy pH meter (D-51S; manufactured by Horiba, Ltd.) in an environment of room temperature (20° C. to 25° C.) The obtained pH value was regarded as the pH of the vinyl resin particles.

[0194] <Method for measuring the number-average particle size of seed particles> The number average particle size of the seed particles was measured using a laser diffraction scattering type particle size distribution analyzer (model number "LS230", manufactured by Beckman Coulter, Inc.). Specifically, 0.1 g of the seed particle dispersion (slurry A obtained in seed particle synthesis example 1 or slurry B obtained in seed particle synthesis example 2) and 20 ml of a 2 mass % anionic surfactant solution were placed in a test tube. Thereafter, the mixture was dispersed for 5 minutes using a test tube mixer (manufactured by AS ONE Corporation, "Test Tube Mixer TRIO HM-1N") and an ultrasonic cleaner (manufactured by AS ONE Corporation, "ULTRASONIC CLEANER VS-150") to obtain a dispersion. The number average particle size of the seed particles in the dispersion obtained was measured using a laser diffraction scattering type particle size distribution analyzer while irradiating the dispersion with ultrasonic waves.

[0195] The measurement conditions for the laser diffraction scattering type particle size distribution analyzer are as follows. <Measurement conditions for laser diffraction / scattering particle size distribution analyzer> medium = water Refractive index of medium = 1.333 Refractive index of solid = Refractive index of seed particles PIDS relative concentration: 40-55%

[0196] The optical model used during measurement was matched to the refractive index of the seed particles produced. When one type of monomer was used to produce the seed particles, the refractive index of the homopolymer of that monomer was used as the refractive index of the seed particles. When multiple types of monomers were used to produce the seed particles, the average value obtained by weighting the refractive indexes of the homopolymers of each monomer by the amount of each monomer used was used as the refractive index of the seed particles.

[0197] From the measurement results, a particle size distribution based on the number of seed particles was obtained. The arithmetic mean of the particle size distribution based on the number of seeds was defined as the number average particle size of the seed particles.

[0198] <Method for measuring number average particle size of vinyl resin particles> The number-average particle size of vinyl resin particles was measured using a Coulter Multisizer TM Measurements were performed using a Multisizer 4e (measurement device manufactured by Beckman Coulter, Inc.). TM 4e was performed with the aperture calibrated according to the user's manual.

[0199] The aperture used for the measurement was appropriately selected according to the size of the vinyl resin particles to be measured. For example, when measuring the particle size range of 0.2-6 μm, an aperture having a size of 10 μm was selected, and when measuring the particle size range of 0.4-16 μm, an aperture having a size of 20 μm was selected.

[0200] The measurement sample was prepared by adding 0.1 g of vinyl resin particles to 100 ml of a 2% by mass anionic surfactant aqueous solution and dispersing the particles using an ultrasonic homogenizer ("BRANSON SONIFIER 450 Advanced" manufactured by Emerson Japan Co., Ltd.) to prepare a dispersion. During the measurement, the mixture was gently stirred so as not to introduce air bubbles into the beaker, and the measurement was terminated when the measurement of 100,000 vinyl resin particles was completed.

[0201] From the measurement results, data on the particle size distribution based on the number of 100,000 vinyl resin particles was obtained. The arithmetic mean obtained from the particle size distribution data based on the number was taken as the number average particle size of the vinyl resin particles.

[0202] <Calculation method for coefficient of variation of number average particle size of vinyl resin particles> The coefficient of variation (CV value) of the number average particle size of the vinyl resin particles was calculated by the following formula. Coefficient of variation of number-average particle size of vinyl resin particles = [(standard deviation of number-based particle size distribution of vinyl resin particles) / (number-average particle size of vinyl resin particles)] x 100

[0203] <Method for measuring the number ratio of particles having a particle diameter 2 to 10 times the number-based median diameter (D50) of vinyl resin particles> The proportion of particles in the particle size range of 2 to 10 times the median diameter D50 of the number-average particle size relative to the total number of vinyl resin particles is measured using a Coulter Multisizer 4e (a measuring device manufactured by Beckman Coulter, Inc.) in the same manner as in the measurement of the number-average particle size.

[0204] "Number-average particle diameter median diameter D50" refers to the particle diameter at which the cumulative fraction in the number-based particle size distribution measured using a Coulter Multisizer 4e is 50%.

[0205] In particle size measurement, an aperture was appropriately selected so that a particle size range equivalent to 1 to 10 times the number-average particle size D50 could be measured. For example, when D50 was 0.5 μm, a 10 μm aperture with a measurable range of 0.2-6 μm was selected, and when D50 was 1.0 μm, a 20 μm aperture with a measurable range of 0.4-12 μm was selected.

[0206] <Method for evaluating the proportion of coarse particles> The proportion of coarse particles (proportion of the number of particles present in the particle diameter range of 2 to 10 times the number-based median diameter D50 to the total number of vinyl resin particles) was determined as follows.

[0207] Specifically, the proportion of coarse particles was determined by measuring the number ratio of particles having a particle diameter 2 to 10 times the number-based median diameter D50 relative to the total number of vinyl resin particles from the number-based particle size distribution data of 100,000 vinyl resin particles obtained by the above-mentioned method for measuring the number-average particle diameter of vinyl resin particles.

[0208] "The median diameter D50 based on the number of vinyl resin particles relative to the total number of particles" is the average diameter measured by Coulter Multisizer TMThis refers to the particle size at which the cumulative fraction in the number-based particle size distribution of 100,000 vinyl resin particles measured using 4e (a measuring device manufactured by Beckman Coulter, Inc.) is 50%.

[0209] The number-average particle size of vinyl resin particles is measured as 1 to 10 times the number-based median diameter D50. Grain The aperture was appropriately selected so that particles with a small diameter could be measured. For example, when D50 was 0.5 μm, a 10 μm aperture with a measurable range of 0.2-6 μm was selected, and when D50 was 1.0 μm, a 20 μm aperture with a measurable range of 0.4-12 μm was selected.

[0210] When the measured proportion of coarse particles was between 0 and 5%, the proportion of coarse particles was considered to be low.

[0211] <Method for measuring temperature at 10% mass loss> The temperature at which the mass decreased by 10% (also called the 10% thermal decomposition temperature) was measured using a thermogravimetric and differential thermal analyzer "TG / DTA6200" (manufactured by SII NanoTechnology Co., Ltd.). First, about 15 mg of vinyl resin particles as a sample was filled into an aluminum measurement container so that there was no gap at the bottom, and alumina was used as the reference substance under an air flow rate of 200 mL / min. Then, a mass loss curve (TG / DTA curve) was obtained when the temperature was raised from 40°C to 500°C at a rate of 10°C / min. From the obtained curve, the temperature at which the mass decreased by 10% was read using the analysis software attached to the TGA device, and was determined as the 10% thermal decomposition temperature.

[0212] <Method for measuring mass loss rate> The measurements were performed using the above-mentioned thermogravimetric and differential thermal simultaneous measurement device. First, about 15 mg of vinyl resin particles as a sample was filled into an aluminum measurement container so that there was no gap at the bottom, and alumina was used as a reference substance under an air flow rate of 200 mL / min. After that, the temperature was raised from 40°C to 350°C at a rate of 10°C / min, and the mass loss behavior was measured when the sample was heated at 350°C for 5 hours. The mass loss rate was calculated by reading the mass loss immediately after heating at 350°C for 5 hours from the mass loss curve obtained by this measurement.

[0213] <Evaluation of viscosity of polyimide precursor varnish> 5 mL of polyimide precursor varnish containing vinyl resin particles was collected as a measurement sample, and the viscosity was measured using a cone-plate viscometer (manufactured by Brookfield, model number: DV2TCP) at a spindle speed of 10 rpm and 25°C for 20 seconds, and the value displayed was stabilized. The spindle used for measurement was a CPA-42Z spindle, and for varnishes in which torque over was confirmed, a CPA-51Z spindle was used. As a pre-measurement condition, a polyimide precursor varnish that had been stirred and degassed for 3 minutes with a degassing mixer (manufactured by Kurabo, product name: Mazerustar KK, model number: 250S) was used. Note that the CPA-42Z spindle was used in the following Test Examples 1 to 9, and the CPA-51Z spindle was used in Test Examples 10 to 13.

[0214] <Evaluation method of polyimide porous film> The polyimide porous film was observed at a magnification of 10,000 times using a scanning electron microscope (SEM) to determine whether or not pores (pores in the polyimide porous film) formed by burning off vinyl resin particles were formed. 100 pores in the polyimide porous film were randomly selected and measured using a side length tool of the SEM to measure the long and short diameters of the pores in the polyimide porous film. Then, (long diameter of the pores in the polyimide porous film + short diameter of the pores in the polyimide porous film) / 2=average pore diameter of the pores in the polyimide porous film (hereinafter also referred to simply as "average pore diameter"). Furthermore, the manufactured polyimide porous film was confirmed with a magnifying microscope, and the maximum and minimum thicknesses of the film surface of the polyimide porous film were measured with a length measuring tool of the magnifying microscope.

[0215] Next, a synthesis example of the seed particles used in the examples and comparative examples will be described.

[0216] (Seed particle synthesis example 1) In a polymerization vessel equipped with a stirrer and a thermometer, 20 g of methyl methacrylate (MMA) as a monofunctional (meth)acrylic monomer (first polymerizable vinyl monomer) and 0.4 g of n-octyl mercaptan as a molecular weight regulator were mixed to prepare an oil phase (hereinafter referred to as oil phase 1). Meanwhile, in a different polymerization vessel equipped with a stirrer and a thermometer, 80 g of ion-exchanged water as an aqueous medium, 0.072 g of sodium styrenesulfonate as a monofunctional styrene monomer (first polymerizable vinyl monomer), and 0.1 g of potassium persulfate as a polymerization initiator were prepared. Then, oil phase 1 was added to the different polymerization vessel, and the temperature was raised to 70°C while stirring. Then, stirring was continued and soap-free polymerization was performed for 12 hours at an internal temperature of 70°C to obtain slurry A. The number average particle diameter of the seed particles (polymethyl methacrylate particles) in the obtained slurry A was 0.28 μm.

[0217] (Seed particle synthesis example 2) In a polymerization vessel equipped with a stirrer and a thermometer, 30 g of methyl methacrylate (MMA) as a monofunctional (meth)acrylic monomer (first polymerizable vinyl monomer) and 0.6 g of n-octyl mercaptan as a molecular weight regulator were mixed to prepare an oil phase (hereinafter referred to as oil phase 2). Meanwhile, in a different polymerization vessel equipped with a stirrer and a thermometer, 70 g of ion-exchanged water as an aqueous medium, 0.21 g of sodium styrenesulfonate as a monofunctional styrene monomer (first polymerizable vinyl monomer), and 0.15 g of potassium persulfate as a polymerization initiator were prepared. Then, oil phase 2 was added to the different polymerization vessel, and the temperature was raised to 80°C while stirring. Then, stirring was continued and soap-free polymerization was performed for 4 hours at an internal temperature of 80°C, and then the temperature was raised to 100°C. Then, stirring was continued and polymerization was performed for 1 hour at an internal temperature of 100°C, to obtain a slurry B. The number average particle diameter of the seed particles (polymethyl methacrylate particles) in the obtained slurry B was 0.195 μm.

[0218] Example 1 <Production Example of Vinyl Resin Particles A> In a polymerization vessel equipped with a stirrer and a thermometer, 20.9 g of isobutyl methacrylate as a monofunctional (meth)acrylic monomer (first polymerizable vinyl monomer), 8.9 g of ethylene glycol dimethacrylate as a polyfunctional (meth)acrylic monomer (first polymerizable vinyl monomer), and 0.15 g of 2,2-azobis-(2,4-dimethylvaleronitrile) as a polymerization initiator were mixed to obtain a monomer mixture.

[0219] To the obtained monomer mixture, 63.3 g of ion-exchanged water as an aqueous medium, 0.15 g of sodium dioctyl sulfosuccinate as an anionic surfactant, 0.3 g of sodium polyoxyethylene nonylphenyl ether phosphate as an anionic surfactant, 0.3 g of polyoxyethylene styrenated phenyl ether as a nonionic surfactant, and 0.01 g of sodium nitrite as a polymerization inhibitor were added. Then, the mixture was stirred at 8000 rpm for 10 minutes with a TK homomixer (manufactured by Primix Corporation) to obtain a monomer mixture.

[0220] To this monomer mixture, 6.9 g of the slurry A obtained in Seed Particle Synthesis Example 1 was added while stirring, and the mixture was stirred at 30° C. for 3 hours to allow the seed particles to absorb the monomer. Thereafter, the internal temperature of the polymerization vessel was raised to 55° C. while stirring, and seed polymerization was carried out over 3 hours by maintaining the temperature at 55° C. for 3 hours. Thereafter, the internal temperature of the polymerization vessel was raised to 80° C., and seed polymerization was further carried out over 3 hours by maintaining the temperature at 80° C. for 3 hours to obtain a slurry containing polymer particles (aqueous dispersion containing polymer particles of the first polymerizable vinyl monomer and the above-mentioned aqueous medium).

[0221] The slurry containing the polymer particles was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0222] The slurry containing the classified polymer particles was spray-dried under the following equipment conditions using a spray dryer (manufactured by Sakamoto Giken Co., Ltd., machine name: spray dryer, type: atomizer take-up type, model number: TRS-3WK) to obtain an aggregate of vinyl resin particles. <Equipment conditions> Slurry feed rate containing polymer particles: 25mL / min Atomizer rotation speed: 12000 rpm Air volume: 2m 3 / min Inlet temperature (temperature of the polymer particle-containing slurry inlet provided in the spray dryer where the polymer particle-containing slurry is sprayed and introduced): 150°C Outlet temperature (the temperature of the powder outlet from which the vinyl resin particle aggregates are discharged from the spray dryer): 70°C

[0223] The obtained vinyl-based resin particle aggregate was subjected to a crushing process using a current jet mill (manufactured by Nisshin Engineering, product name: CJ-10, crushing air pressure: 0.5 MPa) to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles A).

[0224] An SEM photograph of vinyl-based resin particles A obtained by crushing aggregates of vinyl-based resin particles is shown in Figure 1. As shown in Figure 1, it was found that vinyl-based resin particles A were spherical and had a uniform particle size distribution.

[0225] The number-average particle diameter of the vinyl resin particles A was 0.83 μm, and the coefficient of variation of the number-average particle diameter was 13.9%. Grain The proportion of vinyl resin particles A having a small diameter was 0%.

[0226] The aqueous dispersion of the vinyl resin particles A had a pH of 5.4 when measured with a handy pH meter (D-51S, manufactured by Horiba, Ltd.).

[0227] When vinyl resin particles A were heated to 500°C at a heating rate of 10°C / min in an air atmosphere, the 10% thermal decomposition temperature was 257°C. When vinyl resin particles A were heated in an air atmosphere at a heating rate of 10°C / min and then heated at 350°C for 5 hours, the mass reduction rate was 97%.

[0228] Example 2 <Production Example of Vinyl Resin Particles B> As shown in Table 1, seed polymerization was carried out under the same conditions as in Example 1, except that 20.3 g of n-butyl acrylate, 0.3 g of 2-ethylhexyl acrylate, and 0.3 g of methyl acrylate were used as monofunctional (meth)acrylic monomers (first polymerizable vinyl monomers), 8.6 g of ethylene glycol dimethacrylate was used as a polyfunctional (meth)acrylic monomer (first polymerizable vinyl monomer), and 0.3 g of pentaerythritol tetrakisthioglycolate (PETG) was used as an antioxidant, to obtain a slurry containing polymer particles.

[0229] The slurry containing the polymer particles was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0230] Thereafter, the slurry containing the classified polymer particles was subjected to classification, spray drying, and crushing under the same conditions as in Example 1 to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles B).

[0231] The number-average particle diameter of the vinyl resin particles B was 0.82 μm, and the coefficient of variation of the number-average particle diameter was 13.1%. Grain The proportion of vinyl resin particles B having a small diameter was 1%.

[0232] When the aqueous dispersion of vinyl resin particles B was measured with the above-mentioned handy pH meter, the pH was 5.6.

[0233] When vinyl resin particles B were heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere, the 10% thermal decomposition temperature was 291° C. When vinyl resin particles B were heated to 350° C. for 5 hours in an air atmosphere at a heating rate of 10° C. / min, the mass reduction rate was 95%.

[0234] Example 3 <Production Example of Vinyl Resin Particles C> As shown in Table 1, seed polymerization was carried out under the same conditions as in Example 1, except that 16.4 g of methyl methacrylate was used as the monofunctional (meth)acrylic monomer (first polymerizable vinyl monomer), 0.3 g of styrene was used as the monofunctional styrene monomer (first polymerizable vinyl monomer), and 8.6 g of ethylene glycol dimethacrylate was used as the polyfunctional (meth)acrylic monomer (first polymerizable vinyl monomer), to obtain a slurry containing polymer particles.

[0235] The slurry containing the polymer particles was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0236] Thereafter, the slurry containing the classified polymer particles was subjected to classification, spray drying, and crushing under the same conditions as in Example 1 to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles C).

[0237] The number-average particle diameter of the vinyl resin particles C was 0.83 μm, and the coefficient of variation of the number-average particle diameter was 13.4%. Grain The proportion of vinyl resin particles C having a small diameter was 0%.

[0238] When the aqueous dispersion of vinyl resin particles C was measured with the above-mentioned handy pH meter, the pH was 4.7.

[0239] When vinyl resin particles C were heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere, the 10% thermal decomposition temperature was 288° C. When vinyl resin particles C were heated to 350° C. for 5 hours in an air atmosphere at a heating rate of 10° C. / min, the mass reduction rate was 92%.

[0240] Example 4 <Production Example of Vinyl Resin Particles D> As shown in Table 1, seed polymerization was carried out under the same conditions as in Example 1, except that 12.9 g of methyl methacrylate was used as the monofunctional (meth)acrylic monomer (first polymerizable vinyl monomer), 5.5 g of ethylene glycol dimethacrylate and 0.09 g of 2,2-azobis-(2,4-dimethylvaleronitrile) were used as the polyfunctional (meth)acrylic monomer (first polymerizable vinyl monomer), 73.5 g of ion-exchanged water, and 8.1 g of the slurry B obtained in Seed Particle Synthesis Example 2 were used, to obtain a slurry containing polymer particles.

[0241] The slurry containing the polymer particles was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0242] Thereafter, the slurry containing the classified polymer particles was subjected to classification, spray drying, and crushing under the same conditions as in Example 1 to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles D).

[0243] The number-average particle diameter of the vinyl resin particles D was 0.38 μm, and the coefficient of variation of the number-average particle diameter was 14%. Grain The proportion of vinyl resin particles D having a small diameter was 0%.

[0244] When the aqueous dispersion of vinyl resin particles D was measured with the above-mentioned handy pH meter, the pH was 6.2.

[0245] When vinyl resin particles D were heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere, the 10% thermal decomposition temperature was 283° C. When vinyl resin particles D were heated to 350° C. for 5 hours in an air atmosphere at a heating rate of 10° C. / min, the mass reduction rate was 96%.

[0246] Example 5 <Production Example of Vinyl Resin Particles E> As shown in Table 1, seed polymerization was carried out under the same conditions as in Example 1, except that 14.9 g of isobutyl methacrylate was used as the monofunctional (meth)acrylic monomer (first polymerizable vinyl monomer) and 14.9 g of ethylene glycol dimethacrylate was used as the polyfunctional (meth)acrylic monomer (first polymerizable vinyl monomer), to obtain a slurry containing polymer particles.

[0247] The slurry containing the polymer particles was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0248] Thereafter, the slurry containing the classified polymer particles was subjected to classification, spray drying, and crushing under the same conditions as in Example 1 to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles E).

[0249] The number-average particle diameter of the vinyl resin particles E was 0.82 μm, and the coefficient of variation of the number-average particle diameter was 13.8%. Grain The proportion of vinyl resin particles E having a small diameter was 0%.

[0250] When the aqueous dispersion of the vinyl resin particles E was measured with the above-mentioned handy pH meter, the pH was 5.2.

[0251] When vinyl resin particles E were heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere, the 10% thermal decomposition temperature was 249° C. In addition, when vinyl resin particles E were heated at a heating rate of 10° C. / min in an air atmosphere and then heated at 350° C. for 5 hours, the mass reduction rate was 98%.

[0252] Example 6 <Production Example of Vinyl Resin Particles F> In a polymerization vessel equipped with a stirrer, a thermometer, and a nitrogen gas inlet tube, 80 g of ion-exchanged water as an aqueous medium and 0.1 g of ammonium persulfate as a polymerization initiator were mixed to obtain a mixed liquid. In the polymerization vessel, 14 g of methyl methacrylate as a monofunctional (meth)acrylic monomer (second polymerizable vinyl monomer) and 6 g of allyl methacrylate as a polyfunctional (meth)acrylic monomer (second polymerizable vinyl monomer) were added to the mixed liquid, and the temperature was raised to 70°C while bubbling nitrogen gas from the nitrogen gas inlet tube under stirring. Thereafter, stirring was continued and soap-free emulsion polymerization was performed at an internal temperature of 70°C for 12 hours to obtain a slurry containing polymer particles (aqueous dispersion containing polymer particles of the second polymerizable vinyl monomer and the above aqueous medium). The pH of the obtained slurry containing polymer particles was measured with a handy meter (D-51S: manufactured by Horiba, Ltd.) to find that the pH was 2.

[0253] Thereafter, 0.1 g of a 28% by mass aqueous ammonia solution was added to 100 g of the slurry containing the polymer particles, and the mixture was stirred for 10 minutes at 20° C. The pH of the slurry after stirring was measured to be 7.9.

[0254] After the pH measurement, the slurry was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0255] The slurry containing the classified polymer particles was spray-dried under the following conditions using a spray dryer (manufactured by Sakamoto Giken Co., Ltd., machine name: spray dryer, type: atomizer take-up type, model number: TRS-3WK) to obtain an aggregate of vinyl resin particles. <Equipment conditions> Slurry feed rate containing polymer particles: 25mL / min Atomizer rotation speed: 9000 rpm Air volume: 2m 3 / min Inlet temperature (temperature of the polymer particle-containing slurry inlet provided in the spray dryer where the polymer particle-containing slurry is sprayed and introduced): 130°C Outlet temperature (the temperature of the powder outlet from which the vinyl resin particles are discharged from the spray dryer): 60°C

[0256] The obtained vinyl-based resin particle aggregate was subjected to a crushing process using a current jet mill (manufactured by Nisshin Engineering, product name: CJ-10, crushing air pressure: 0.5 MPa) to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles F).

[0257] The number-average particle diameter of the vinyl resin particles F was 0.32 μm, and the coefficient of variation of the number-average particle diameter was 13.2%. Grain The percentage of particles having a small diameter was 0%.

[0258] When the aqueous dispersion of vinyl resin particles F was measured with a handy pH meter, the pH was 7.1.

[0259] When vinyl resin particles F were heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere, the 10% thermal decomposition temperature was 287° C. In addition, when vinyl resin particles F were heated at a heating rate of 10° C. / min in an air atmosphere and then heated at 350° C. for 5 hours, the mass reduction rate was 95%.

[0260] Comparative Example 1 <Production Example of Vinyl Resin Particles G> As shown in Table 1, seed polymerization was carried out under the same conditions as in Example 1, except that 29.6 g of styrene was used as the monofunctional styrene-based monomer (first polymerizable vinyl-based monomer) and 0.2 g of ethylene glycol dimethacrylate was used as the polyfunctional (meth)acrylic monomer (first polymerizable vinyl-based monomer), to obtain a slurry containing polymer particles.

[0261] The slurry containing the polymer particles was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0262] Thereafter, the slurry containing the classified polymer particles was subjected to classification, spray drying, and crushing under the same conditions as in Example 1 to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles G).

[0263] The number-average particle diameter of the vinyl resin particles G was 0.82 μm, and the coefficient of variation of the number-average particle diameter was 13.6%. Grain The proportion of vinyl resin particles G having a small diameter was 0%.

[0264] When the aqueous dispersion of the vinyl resin particles G was measured with the above-mentioned handy pH meter, the pH was 4.2.

[0265] When vinyl resin particles G were heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere, the 10% thermal decomposition temperature was 313° C. In addition, when vinyl resin particles G were heated at a heating rate of 10° C. / min in an air atmosphere and then heated at 350° C. for 5 hours, the mass reduction rate was 75%.

[0266] Comparative Example 2 <Production Example of Vinyl Resin Particles H> As shown in Table 1, seed polymerization was carried out under the same conditions as in Example 1, except that 29.6 g of methyl methacrylate was used as the monofunctional (meth)acrylic monomer (first polymerizable vinyl monomer) and 0.2 g of ethylene glycol dimethacrylate was used as the polyfunctional (meth)acrylic monomer (first polymerizable vinyl monomer), to obtain a slurry containing polymer particles.

[0267] The slurry containing the polymer particles was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0268] Thereafter, the slurry containing the classified polymer particles was subjected to classification, spray drying, and crushing under the same conditions as in Example 1 to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles H).

[0269] The number-average particle diameter of the vinyl resin particles H was 0.81 μm, and the coefficient of variation of the number-average particle diameter was 14.2%. Grain The proportion of vinyl resin particles H having a small diameter was 0%.

[0270] When the aqueous dispersion of the vinyl resin particles H was measured with the above-mentioned handy pH meter, the pH was 5.8.

[0271] When vinyl resin particles H were heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere, the 10% thermal decomposition temperature was 319° C. In addition, when vinyl resin particles H were heated at a heating rate of 10° C. / min in an air atmosphere and then heated at 350° C. for 5 hours, the mass reduction rate was 86%.

[0272] Comparative Example 3 <Production Example of Vinyl Resin Particles I> As shown in Table 1, seed polymerization was carried out under the same conditions as in Example 6, except that 19.8 g of methyl methacrylate was used as the monofunctional (meth)acrylic monomer (second polymerizable vinyl monomer) and 0.2 g of allyl methacrylate was used as the polyfunctional (meth)acrylic monomer (second polymerizable vinyl monomer), to obtain a slurry containing polymer particles.

[0273] The slurry containing the polymer particles was passed through a 400 Mesh nylon net to classify the polymer particles, thereby obtaining a slurry containing classified polymer particles.

[0274] Thereafter, the slurry containing the classified polymer particles was subjected to classification, spray drying, and crushing under the same conditions as in Example 6 to obtain vinyl-based resin particles (hereinafter referred to as vinyl-based resin particles I).

[0275] The number-average particle diameter of the vinyl resin particles I was 0.30 μm, and the coefficient of variation of the number-average particle diameter was 14.1%. Grain The proportion of vinyl resin particles I having the small diameter was 0%.

[0276] When the aqueous dispersion of vinyl resin particles I was measured with the above-mentioned handy pH meter, the pH was 7.1.

[0277] When vinyl resin particles I were heated to 500° C. at a heating rate of 10° C. / min in an air atmosphere, the 10% thermal decomposition temperature was 308° C. In addition, when vinyl resin particles I were heated at a heating rate of 10° C. / min in an air atmosphere and then heated at 350° C. for 5 hours, the mass reduction rate was 84%.

[0278] (Test Example 1) <Preparation of polyimide precursor varnish with vinyl resin particles A dispersed therein> In a beaker, 8 g of vinyl resin particles A obtained in Example 1 and 24 g of N-methyl-2-pyrrolidone (NMP) as the first organic solvent were mixed to prepare a dispersion of vinyl resin particles A. In a different beaker, 3.61 g of an NMP solution (solid content concentration 18 ± 1 mass%, manufactured by Ube Industries, Ltd., U-Varnish A) as a polyimide precursor solution and 1.8 g of NMP as the second organic solvent were mixed, and 6 g of the prepared dispersion of vinyl resin particles A was added. Then, it was stirred and defoamed for 15 minutes with a defoaming stirrer (manufactured by Kurabo Industries Ltd., product name: Mazelstar KK, model number: 250S) to obtain a varnish of a polyimide precursor in which vinyl resin particles A were dispersed (hereinafter referred to as varnish A of the polyimide precursor).

[0279] Regarding the varnish A of the polyimide precursor, when the viscosity value was measured under the above conditions using a cone and plate viscometer (manufactured by Brookfield, model number: DV2TCP), it was 239 (mPa·s).

[0280] <Preparation of Blank Solution A> In a beaker, 4.5 g of NMP as the first organic solvent, 3.61 g of an NMP solution (solid content concentration 18 ± 1 mass%, manufactured by Ube Industries, Ltd., U-Varnish A) as a polyimide precursor solution, and 1.8 g of NMP as the second organic solvent were mixed, and it was stirred and defoamed for 15 minutes with a defoaming stirrer to obtain Blank Solution A.

[0281] <Calculation of Rsp Value> The varnish A of the polyimide precursor and Blank Solution A were sampled into different NMR tubes. Then, regarding the varnish A of the polyimide precursor, a pulsed NMR particle interface property evaluation apparatus (「 AcornThe transverse relaxation time T2 (ms) of protons derived from varnish A, a polyimide precursor, was measured three times by the CPMG method (Carr-Purcell Meiboom-Gill method) under the measurement conditions of a hydrogen nucleus as the measurement nucleus, a measurement temperature of 20°C, a resonance frequency of 13 MHz, and a 90° pulse width of 5.81 μs, and the average value was calculated. The average value was 60.5 (ms), so the reciprocal of the average value was taken as the Rav value. In other words, the Rav value was 1 / [60.5 (ms)].

[0282] In addition, for blank solution A, the transverse relaxation time T2 (ms) of protons derived from the blank solution was measured three times in the same manner as above, and the average value was calculated. Since the average value was 1095.2 (ms), the reciprocal of the average value was taken as the Rb value. In other words, the Rb value was 1 / [1095.2 (ms)].

[0283] The Rsp value was calculated based on the following formula (1) and was found to be 17.1. Rsp = (Rav - Rb) / Rb (1)

[0284] <Evaluation of polyimide porous film> The polyimide precursor varnish A was applied as a coating liquid for forming a porous film to a silicone-coated polyethylene terephthalate (PET) film using a coater (IMC-70F0-C type; manufactured by Imoto Manufacturing Co., Ltd.) and an applicator (Baker Applicator YBA type; manufactured by Yoshimitsu Seiki Co., Ltd.). The film was then dried at 60°C for 1 hour to remove the first and second organic solvents, thereby obtaining an unbaked composite film (film thickness: about 32 μm) containing vinyl resin particles.

[0285] The unsintered composite membrane peeled off from the PET film was heated in an air atmosphere from 20°C to 320°C at a heating rate of 10°C / min using a microwave muffle furnace (Phoenix; CEM). Polyimide was then generated by heating at 320°C for 5 hours, resulting in a polyimide porous membrane.

[0286] The major and minor diameters of the pores in the resulting polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.79 μm.

[0287] Furthermore, the maximum and minimum film thicknesses of the film surface of the obtained polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum film thickness was 38 μm and the minimum film thickness was 26 μm, so it was confirmed that a polyimide porous film with a uniform film thickness was obtained.From these results, the vinyl resin particles of the present invention can be used to smooth the surface of the polyimide porous film.

[0288] (Test Example 2) A polyimide precursor varnish having vinyl resin particles A dispersed therein (hereinafter referred to as polyimide precursor varnish B) and a blank solution (hereinafter referred to as blank solution B) were prepared under the same conditions as in Test Example 1, except that γ-butyrolactone (GBL) was used as the first and second organic solvents.

[0289] The viscosity of polyimide precursor varnish B was measured under the above conditions using a cone-plate viscometer and found to be 294 (mPa·s).

[0290] The Rav value of the polyimide precursor varnish B and the Rb value of the blank solution B were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [66.3 (ms)] and the Rb value was 1 / [1218.9 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 17.4.

[0291] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that varnish B, a polyimide precursor, was used.

[0292] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.77 μm.

[0293] The maximum and minimum thicknesses of the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum thickness was 38 μm and the minimum thickness was 28 μm, so it was confirmed that a polyimide porous film with a uniform thickness was obtained.By using the vinyl resin particles of the present invention, the surface of the polyimide porous film could be smoothed.

[0294] (Test Example 3) A polyimide precursor varnish in which vinyl resin particles B were dispersed (hereinafter referred to as polyimide precursor varnish C) and a blank solution (hereinafter referred to as blank solution C) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles B were used.

[0295] The viscosity of polyimide precursor varnish C was measured under the above conditions using a cone-plate viscometer and found to be 187 (mPa·s).

[0296] The Rav value of the polyimide precursor varnish C and the Rb value of the blank solution C were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [38.4 (ms)] and the Rb value was 1 / [1095.2 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 27.5.

[0297] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that varnish C, a polyimide precursor, was used.

[0298] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.69 μm.

[0299] The maximum and minimum thicknesses of the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum thickness was 39 μm and the minimum thickness was 26 μm, so it was confirmed that a polyimide porous film with a uniform thickness was obtained.By using the vinyl resin particles of the present invention, the surface of the polyimide porous film could be smoothed.

[0300] (Test Example 4) A polyimide precursor varnish in which vinyl resin particles B were dispersed (hereinafter referred to as polyimide precursor varnish D) and a blank solution (hereinafter referred to as blank solution D) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles B were used and N,N-dimethylacetamide (DMAc) was used as the first and second organic solvents.

[0301] The viscosity of polyimide precursor varnish D was measured under the above conditions using a cone-plate viscometer and found to be 149 (mPa·s).

[0302] The Rav value of the polyimide precursor varnish D and the Rb value of the blank solution D were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [22.1 (ms)] and the Rb value was 1 / [1359 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 60.5.

[0303] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish D, a polyimide precursor, was used.

[0304] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.71 μm.

[0305] The maximum and minimum film thicknesses of the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum film thickness was 36 μm and the minimum film thickness was 27 μm, so it was confirmed that a polyimide porous film with a uniform film thickness was obtained.By using the vinyl resin particles of the present invention, the surface of the polyimide porous film could be smoothed.

[0306] (Test Example 5) A polyimide precursor varnish in which vinyl resin particles C were dispersed (hereinafter referred to as polyimide precursor varnish E) and a blank solution (hereinafter referred to as blank solution E) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles C were used.

[0307] The viscosity of polyimide precursor varnish E was measured under the above conditions using a cone-plate viscometer and found to be 211 (mPa·s).

[0308] The Rav value of the polyimide precursor varnish E and the Rb value of the blank solution E were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [94.5 (ms)] and the Rb value was 1 / [1095.2 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 10.6.

[0309] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish E, a polyimide precursor, was used.

[0310] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.78 μm.

[0311] The maximum and minimum film thicknesses of the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum film thickness was 35 μm and the minimum film thickness was 26 μm, so it was confirmed that a polyimide porous film with a uniform film thickness was obtained.By using the vinyl resin particles of the present invention, the surface of the polyimide porous film could be smoothed.

[0312] (Test Example 6) A polyimide precursor varnish in which vinyl resin particles D were dispersed (hereinafter referred to as polyimide precursor varnish F) and a blank solution (hereinafter referred to as blank solution F) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles D were used.

[0313] The viscosity of polyimide precursor varnish F was measured under the above conditions using a cone-plate viscometer and found to be 179 (mPa·s).

[0314] The Rav value of the polyimide precursor varnish F and the Rb value of the blank solution F were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [37.5 (ms)] and the Rb value was 1 / [1095.2 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 28.2.

[0315] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish F, a polyimide precursor, was used.

[0316] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.31 μm.

[0317] The maximum and minimum thicknesses of the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum thickness was 35 μm and the minimum thickness was 27 μm, so it was confirmed that a polyimide porous film with a uniform thickness was obtained.By using the vinyl resin particles of the present invention, the surface of the polyimide porous film could be smoothed.

[0318] (Test Example 7) A polyimide precursor varnish in which vinyl resin particles D were dispersed (hereinafter referred to as polyimide precursor varnish G) and a blank solution (hereinafter referred to as blank solution G) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles D were used and N,N-dimethylacetamide (DMAc) was used as the first and second organic solvents.

[0319] The viscosity of polyimide precursor varnish G was measured under the above conditions using a cone-plate viscometer and found to be 158 (mPa·s).

[0320] The Rav value of the polyimide precursor varnish G and the Rb value of the blank solution G were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [22.2 (ms)] and the Rb value was 1 / [1359 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 60.2.

[0321] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish G, a polyimide precursor, was used.

[0322] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.33 μm.

[0323] The maximum and minimum thicknesses of the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum thickness was 40 μm and the minimum thickness was 28 μm, so it was confirmed that a polyimide porous film with a uniform thickness was obtained.By using the vinyl resin particles of the present invention, the surface of the polyimide porous film could be smoothed.

[0324] (Test Example 8) A polyimide precursor varnish in which vinyl resin particles E were dispersed (hereinafter referred to as polyimide precursor varnish H) and a blank solution (hereinafter referred to as blank solution H) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles E were used.

[0325] The viscosity of polyimide precursor varnish H was measured under the above conditions using a cone-plate viscometer and found to be 238 (mPa·s).

[0326] The Rav value of the polyimide precursor varnish H and the Rb value of the blank solution H were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [60 (ms)] and the Rb value was 1 / [1095.2 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 17.3.

[0327] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish H, a polyimide precursor, was used.

[0328] The major and minor diameters of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.76 μm.

[0329] The maximum and minimum film thicknesses of the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum film thickness was 39 μm and the minimum film thickness was 27 μm, so it was confirmed that a polyimide porous film with a uniform film thickness was obtained.By using the vinyl resin particles of the present invention, the surface of the polyimide porous film could be smoothed.

[0330] (Test Example 9) A polyimide precursor varnish in which vinyl resin particles F were dispersed (hereinafter referred to as polyimide precursor varnish I) and a blank solution (hereinafter referred to as blank solution I) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles F were used.

[0331] The viscosity of polyimide precursor varnish I was measured under the above conditions using a cone-plate viscometer and found to be 289 (mPa·s).

[0332] The Rav value of the polyimide precursor varnish I and the Rb value of the blank solution I were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [50 (ms)] and the Rb value was 1 / [1095.2 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 20.9.

[0333] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish I, a polyimide precursor, was used.

[0334] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.29 μm.

[0335] The maximum and minimum thicknesses of the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, and the maximum thickness was 40 μm and the minimum thickness was 27 μm, so it was confirmed that a polyimide porous film with a uniform thickness was obtained.By using the vinyl resin particles of the present invention, the surface of the polyimide porous film could be smoothed.

[0336] (Test Example 10) A polyimide precursor varnish in which vinyl resin particles G were dispersed (hereinafter referred to as polyimide precursor varnish J) and a blank solution (hereinafter referred to as blank solution J) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles G were used.

[0337] The viscosity of polyimide precursor varnish J was measured under the above conditions using a cone-plate viscometer, and was found to be 1010 (mPa·s).

[0338] Rav value of varnish J of polyimide precursor and blank solution J When the Rb value was calculated under the same conditions as in Test Example 1, the Rav value was 1 / [439 (ms)] and the Rb value was 1 / [1095.2 (ms)]. When the Rsp value was calculated from these values ​​based on the above formula (1), the Rsp value was 1.49.

[0339] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish J, a polyimide precursor, was used.

[0340] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 1.08 μm.

[0341] When the maximum and minimum film thicknesses of the film surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, the maximum film thickness was 89 μm and the minimum film thickness was 25 μm, confirming that a polyimide porous film of uniform thickness had not been obtained.

[0342] (Test Example 11) A polyimide precursor varnish in which vinyl resin particles G were dispersed (hereinafter referred to as polyimide precursor varnish K) and a blank solution (hereinafter referred to as blank solution K) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles G were used and γ-butyrolactone (GBL) was used as the first and second organic solvents.

[0343] The viscosity of polyimide precursor varnish K was measured under the above conditions using a cone-plate viscometer and found to be 1045 (mPa·s).

[0344] The Rav value of the polyimide precursor varnish K and the Rb value of the blank solution K were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [434 (ms)] and the Rb value was 1 / [1218.9 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 1.81.

[0345] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish K, a polyimide precursor, was used.

[0346] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 1.09 μm.

[0347] When the maximum and minimum film thicknesses of the film surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, the maximum film thickness was 92 μm and the minimum film thickness was 26 μm, confirming that a polyimide porous film with a uniform film thickness had not been obtained.

[0348] (Test Example 12) A polyimide precursor varnish in which vinyl resin particles G were dispersed (hereinafter referred to as polyimide precursor varnish L) and a blank solution (hereinafter referred to as blank solution L) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles H were used.

[0349] The viscosity of polyimide precursor varnish L was measured under the above conditions using a cone-plate viscometer and found to be 1060 (mPa·s).

[0350] The Rav value of the polyimide precursor varnish L and the Rb value of the blank solution L were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [350 (ms)] and the Rb value was 1 / [1095.2 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 2.13.

[0351] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish L, a polyimide precursor, was used.

[0352] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 1.07 μm.

[0353] When the maximum and minimum film thicknesses of the film surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, the maximum film thickness was 92 μm and the minimum film thickness was 28 μm, confirming that a polyimide porous film of uniform thickness had not been obtained.

[0354] (Test Example 13) A polyimide precursor varnish in which vinyl resin particles I were dispersed (hereinafter referred to as polyimide precursor varnish M) and a blank solution (hereinafter referred to as blank solution M) were prepared under the same conditions as in Test Example 1, except that vinyl resin particles I were used.

[0355] The viscosity of polyimide precursor varnish M was measured under the above conditions using a cone-plate viscometer and found to be 1097 (mPa·s).

[0356] The Rav value of the polyimide precursor varnish M and the Rb value of the blank solution M were calculated under the same conditions as in Test Example 1, and the Rav value was 1 / [340 (ms)] and the Rb value was 1 / [1095.2 (ms)]. The Rsp value was calculated from these values ​​based on the above formula (1), and was 2.22.

[0357] Moreover, a polyimide porous film was produced under the same conditions as in Test Example 1, except that Varnish M, a polyimide precursor, was used.

[0358] The major and minor axes of the pores in the polyimide porous film were measured using a length measuring tool of an SEM, and the average pore diameter was found to be 0.39 μm.

[0359] When the maximum and minimum film thicknesses on the surface of the polyimide porous film were measured using a length measuring tool of a magnifying microscope, the maximum film thickness was 111 μm and the minimum film thickness was 27 μm, confirming that a polyimide porous film with a uniform film thickness had not been obtained.

[0360] (Evaluation Results) The evaluation results of each Example, Comparative Example, and Test Example are shown in Tables 1 and 2. In Tables 1 and 2, Particles A to I respectively mean vinyl resin particles A to I. In Table 1, the proportion (%) of coarse particles means the proportion (%) of the number of particles present in the particle diameter range of 2 to 10 times the number-based median diameter D50 to the total number of vinyl resin particles.

[0361] [Table 1]

[0362] [Table 2]

Claims

1. A vinyl-based resin particle for making a polyimide resin porous, comprising: The temperature at which the mass is reduced by 10% when the temperature is increased at 10° C. / min in an air atmosphere is 230° C. or higher and lower than 300° C.; The mass loss rate after heating at 350° C. for 5 hours in an air atmosphere is 85 to 100%; the vinyl-based resin particles are polymers having first polymerizable vinyl-based monomer units composed of monofunctional monomer units and polyfunctional monomer units, The first polymerizable vinyl monomer unit contains 12 to 150 parts by mass of the polyfunctional monomer unit relative to 100 parts by mass of the monofunctional monomer unit, the monofunctional monomer unit is at least one of a monofunctional styrene-based monomer unit and a monofunctional (meth)acrylic monomer unit, The polyfunctional monomer unit is at least one of a polyfunctional styrene-based monomer unit and a polyfunctional (meth)acrylic monomer unit (excluding diethylene glycol dimethacrylate and allyl methacrylate as the polyfunctional (meth)acrylic monomer).

2. 2. The vinyl resin particles according to claim 1, having a number average particle size in the range of 0.1 to 3 μm.

3. The vinyl resin particles according to claim 2 , wherein the coefficient of variation of the number average particle size is 25% or less.

4. The vinyl resin particles according to any one of claims 1 to 3, wherein the number ratio of particles having a particle diameter 2 to 10 times the number-based median diameter (D50) is in the range of 0 to 5%.

5. The vinyl resin particle according to any one of claims 1 to 4, wherein the monofunctional (meth)acrylic monomer unit is a (meth)acrylic acid alkyl ester monomer unit, and the alkyl group bonded to the ester has 1 to 10 carbon atoms.

6. The vinyl resin particles according to any one of claims 1 to 5, The vinyl resin particles have a pH of 3 to 9 when dispersed in water at a mass ratio of 1:

10.

7. The vinyl-based resin particles according to any one of claims 1 to 6, wherein the Rsp value represented by the following formula (1) is 5 or more and 150 or less. Rsp=(Rav-Rb) / Rb...(1) Rav: Transverse relaxation time T obtained by the following measurement method 1 2 Reciprocal of the average value of (ms) Rb: Transverse relaxation time T obtained by the following measurement method 2 2 Reciprocal of (ms) [Measurement method 1] The vinyl resin particles and the first organic solvent were mixed in a mass ratio of 1:3 to form a polyimide precursor varnish, which was prepared by mixing a polyimide precursor solution having a solid content concentration of 18±1% by mass and a second organic solvent in a mass ratio of 6:3.61:1.

8. The transverse relaxation time T of protons derived from the varnish was measured by a CPMG method under the following measurement conditions: a measurement nucleus was a hydrogen nucleus, a measurement temperature was 20° C., a resonance frequency was 13 MHz, and a 90° pulse width was 5.81 μs. 2 (ms) is measured three times, the average value is calculated, and the reciprocal of the average value is defined as Rav. Here, the first organic solvent and the second organic solvent are the same organic solvent. [Measurement method 2] A blank solution obtained by mixing the first organic solvent, a polyimide precursor solution having a solid content concentration of 18±1% by mass, and the second organic solvent in a mass ratio of 4.5:3.61:1.8 was measured by a CPMG method under the following measurement conditions: a measurement nucleus was a hydrogen nucleus, a measurement temperature was 20° C., a resonance frequency was 13 MHz, and a 90° pulse width was 5.81 μs. 2 (ms) is measured three times, the average value is calculated, and the reciprocal of the average value is designated as Rb. Here, the first organic solvent and the second organic solvent are the same organic solvent.

8. A method for producing porosity-making vinyl resin particles of polyimide resin (excluding porosity-making vinyl resin particles made of polyoxyethylene di(meth)acrylate, methyl methacrylate, and isobutyl methacrylate), comprising the steps of: a seed polymerization step of absorbing a first polymerizable vinyl monomer into seed particles and carrying out seed polymerization to obtain an aqueous dispersion containing polymer particles of the first polymerizable vinyl monomer and an aqueous medium; a spray drying step in which the aqueous dispersion obtained in the seed polymerization step is spray-dried under conditions of an inlet temperature of 80 to 220° C. and an outlet temperature of 50 to 100° C. to obtain an aggregate; and a crushing step of crushing the aggregates obtained in the spray drying step to obtain vinyl-based resin particles, In the seed polymerization step, the first polymerizable vinyl monomer comprises a monofunctional monomer and a polyfunctional monomer, and the first polymerizable vinyl monomer contains 12 to 150 parts by mass of the polyfunctional monomer relative to 100 parts by mass of the monofunctional monomer; The vinyl resin particles are The temperature at which the mass is reduced by 10% when the temperature is increased at 10° C. / min in an air atmosphere is 230° C. or higher and lower than 300° C.; The mass loss rate after heating at 350° C. for 5 hours in an air atmosphere is 85 to 100%; the vinyl-based resin particles are polymers having first polymerizable vinyl-based monomer units composed of monofunctional monomer units and polyfunctional monomer units, The first polymerizable vinyl monomer unit contains 12 to 150 parts by mass of the polyfunctional monomer unit relative to 100 parts by mass of the monofunctional monomer unit, the monofunctional monomer unit is at least one of a monofunctional styrene-based monomer unit and a monofunctional (meth)acrylic monomer unit, The polyfunctional monomer unit is at least one of a polyfunctional styrene-based monomer unit and a polyfunctional (meth)acrylic monomer unit (provided that diethylene glycol dimethacrylate and allyl methacrylate are excluded as the polyfunctional (meth)acrylic monomer). A method for producing vinyl resin particles for making polyimide resin porous.

9. 9. The method for producing vinyl-based resin particles according to claim 8, comprising at least one of a first classification step of classifying the polymer particles obtained in the seed polymerization step and a second classification step of classifying the vinyl-based resin particles obtained in the crushing step.

10. A method for producing vinyl-based resin particles for making a polyimide resin porous, comprising the steps of: an emulsion polymerization step of emulsion-polymerizing a second polymerizable vinyl monomer in an aqueous medium to obtain an aqueous dispersion containing polymer particles of the second polymerizable vinyl monomer and the aqueous medium; a spray drying step of spray-drying the aqueous dispersion obtained in the emulsion polymerization step under conditions of an inlet temperature of 80 to 220° C. and an outlet temperature of 50 to 100° C. to obtain an aggregate; and a crushing step for crushing the aggregates obtained in the spray drying step to obtain vinyl-based resin particles; Including, The vinyl resin particles are The temperature at which the mass is reduced by 10% when the temperature is increased at 10° C. / min in an air atmosphere is 230° C. or higher and lower than 300° C.; The mass loss rate after heating at 350° C. for 5 hours in an air atmosphere is 85 to 100%; the vinyl-based resin particles are polymers having second polymerizable vinyl-based monomer units composed of monofunctional monomer units and polyfunctional monomer units, the monofunctional monomer unit is at least one of a monofunctional styrene-based monomer unit and a monofunctional (meth)acrylic monomer unit, The polyfunctional monomer unit is at least one of a polyfunctional styrene-based monomer unit and a polyfunctional (meth)acrylic monomer unit. A method for producing vinyl resin particles for making polyimide resin porous.

11. The method for producing vinyl resin particles according to claim 10, further comprising a pH adjustment step of adjusting the pH of the aqueous dispersion obtained in the emulsion polymerization step to 3 to 9 by adding a nitrogen-containing compound to the aqueous dispersion.

12. 12. The method for producing vinyl-based resin particles according to claim 10, further comprising at least one of a first classification step of classifying the polymer particles obtained in the emulsion polymerization step and a second classification step of classifying the vinyl-based resin particles obtained in the crushing step.

Citation Information

Patent Citations

  • Production of porous film

    JP1998316795A

  • Porous material

    JP2001210142A

  • Porous substance

    JP2002037912A

  • Porous material and method for producing the same

    JP2006077245A

  • Method for producing porous resin film, porous resin film, and cell separator

    JP2010024385A