Toner manufacturing method

The toner with a core particle coated by inorganic oxide and organosilicon polymer addresses image graininess and ghosting by optimizing wax distribution and adhesion, ensuring high-quality images with stability.

JP7555746B2Active Publication Date: 2024-09-25CANON KK
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020124138
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-21
Publication Date
2024-09-25
Estimated Expiration
2040-07-21

AI Technical Summary

Technical Problem

Existing toners face issues with image graininess due to increased adhesion between toner particles and transfer members, especially in low humidity environments, leading to uneven image density and ghosting effects.

Method used

A toner formulation with a core particle containing a binder resin and wax, coated with inorganic oxide fine particles and an organosilicon polymer, where the wax is distributed such that 0.7≦Qi-Qh≦20.0, and the organosilicon polymer has a specific partial structure, ensuring high adhesion and low wettability, reducing particle adhesion and ghosting.

Benefits of technology

The toner achieves high fixing wrap resistance, charging stability, and reduced graininess, providing high-quality images over extended periods by minimizing adhesion to transfer members and suppressing ghosting effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555746000016
    Figure 0007555746000016
  • Figure 0007555746000017
    Figure 0007555746000017
  • Figure 0007555746000001
    Figure 0007555746000001
Patent Text Reader

Abstract

To provide a toner which includes a coating layer containing an organosilicon polymer that is highly adhesive even to a core particle having more wax content near a surface thereof, offers fixing wrapping resistance and development durability, allows for producing high quality images with less granular appearance for a prolonged period of time and suppressing external additive ghost images.SOLUTION: A toner provided herein comprises toner particles, each comprising a core particle containing a binder resin and wax, inorganic oxide fine particles provided on a surface of the core particle, and a coating layer containing an organosilicon polymer covering the core particle, and satisfies the following conditional expression: 0.7≤Qi-Qh≤20.0, where Qi (J / g) represents an endothermic peak heat absorption originating from the wax as obtained by differential scanning calorimetry (DSC), and Qh (J / g) represents an endothermic peak heat absorption originating from the wax as obtained by DSC after hexane treatment of the core particles. The organosilicon polymer has a partial structure represented by the following formula (T3): R-Si(O1 / 2)3 ...(T3), where, in the formula T3, R represents an alkyl group or phenyl group having 1 to 6 carbon atoms, inclusive. In a 29Si-NMR measurement of tetrahydrofuran insoluble content of the toner particles, a ratio [ST3] of peak area of the partial structure represented by the formula (T3) to total peak area of the organosilicon polymer satisfies a relationship expressed as: ST3≥0.05. The inorganic oxide fine articles are thermally fixed to a surface of each core particle.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner used in an electrophotographic system, an electrostatic recording system, an electrostatic printing system, and a toner jet system, and a method for producing the toner. [Background technology]

[0002] In recent years, full-color electrophotographic copiers have come into widespread use, and there is an increasing demand for energy-saving and high productivity. In addition, there is a demand for high-quality images approaching those of offset printing, and there is a demand for the development of high-quality toner technology to achieve these. In order to save energy, technology that melts toner quickly at low temperatures in the fixing process is being studied. In order to improve the low-temperature fixing ability of toner, there is a method of lowering the glass transition point or softening point of the binder resin of the toner and using a binder resin that has sharp melting properties. In recent years, many toners that contain crystalline polyester as a resin with even sharper melting properties have been proposed. For high productivity, various toners are being studied to shorten the time for various controls immediately after the power is turned on, during one job, and between jobs. For example, studies are being conducted to create toners whose charging properties do not decrease even when left in high-temperature and high-humidity environments, and toners that can be fixed at a wide range of temperatures and do not wrap around the fixing member even at high temperatures. As a toner that does not wrap around a fixing member even at high temperatures, for example, Patent Document 1 proposes a toner that contains two types of polyester resins and is characterized by controlling the degree of uneven distribution of wax in the depth direction of the toner from the toner surface toward the toner center. The toner of Patent Document 1 has a large amount of wax present near the toner particle surface, so the wax effectively seeps out during fixing, improving release properties and improving anti-wrapping properties. However, the inventor's research has revealed that when an image with a low printing ratio is output for a long period of time, the graininess of the image increases, making it difficult to obtain a high-quality image. It has become clear that the main cause of graininess in an image is an increase in the adhesion between toner particles and a transfer member, which reduces the uniformity of transfer, and techniques for reducing this are being studied. For example, as a proposal for reducing the adhesion to the member, studies have been conducted on covering toner particles with an external additive of inorganic fine particles at a high coverage rate, reducing the adhesion by the spacer effect of the fine particles, and covering core particles with a shell that has a lower adhesion than the core particles. For example, Patent Document 2 proposes a toner having toner particles with a coating layer containing an organosilicon polymer having a specific structure. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-83749 A [Patent Document 2] JP 2016-21041 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have been studying toners that have anti-fixing wrap-around properties, can reduce adhesion to a transfer member, and can obtain high-quality images with little graininess. As a result, it has been found that the adhesion between core particles in which a large amount of wax is present near the surface of the toner particles, as described in Patent Document 1, and the organosilicon polymer is low. The organosilicon polymer detached from the core particles migrates to the photoreceptor surface in the electrophotographic development process, and further, a part of it slips through the cleaning blade in the cleaning process. This tendency is more pronounced in low-humidity environments. As a result, a difference in latent image potential occurs in the next charging process between a portion where the organosilicon polymer has a large amount of slip-through and a portion where it has a small amount of slip-through, which may appear as a difference in image density (hereinafter also referred to as an external additive ghost). The object of the present invention is to provide a toner which has solved the above problems, specifically, a coating layer containing an organosilicon polymer which has high adhesion even to core particles which have a large amount of wax near the surface, which has excellent anti-wrapping properties and charge stability, and which can provide high quality images with little graininess over a long period of time, and which can suppress external additive ghosts. [Means for solving the problem]

[0005] The present invention relates to a toner having toner particles which have core particles containing a binder resin and a wax, and which have inorganic oxide fine particles on the surface of the core particles and a coating layer containing an organosilicon polymer which coats the core particles. Manufacturing method And, The core particles satisfy the following relationship when the endothermic heat of the endothermic peak derived from the wax measured by differential scanning calorimetry (DSC) is Qi (J / g) and the endothermic heat of the endothermic peak derived from the wax measured by DSC after the core particles are treated with hexane is Qh (J / g): 0.7≦Qi-Qh≦20.0 The organosilicon polymer has a partial structure represented by the following formula (T3): The tetrahydrofuran insoluble portion of the toner particles 29 In Si-NMR measurement, the ratio [ST3] of the peak area of ​​the partial structure represented by the following formula (T3) to the total peak area of ​​the organosilicon polymer satisfies the relationship ST3 ≧ 0.05, R-Si(O 1 / 2 )3(T3) (In formula (T3), R represents an alkyl group having 1 to 6 carbon atoms or a phenyl group.) The inorganic oxide fine particles are thermally fixed to the surface of the core particles. And, a step of adhering the inorganic oxide fine particles to the surface of the core particles containing the binder resin and the wax; and dispersing the core particles having the inorganic oxide fine particles attached thereto in an aqueous medium. coating the surfaces of the core particles to which the inorganic oxide fine particles are attached with the organosilicon polymer; The method includes a step of treating the core particles having the inorganic oxide fine particles attached thereto with hot air after the step of attaching the inorganic oxide fine particles to the surfaces of the core particles. A toner characterized in that Manufacturing method It is. Effect of the Invention

[0006] The toner of the present invention has a coating layer containing an organosilicon polymer which has high adhesion even to core particles which have a large amount of wax near the surface, and can provide a toner which has excellent fixing wrap-around resistance, excellent development durability, and which can produce high quality images with little graininess over a long period of time, while also suppressing external additive ghosts. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is an explanatory diagram of a surface treatment device suitable for thermally fixing inorganic oxide fine particles to the surface of a toner core particle. [Diagram 2] 2 is a measurement chart of 29Si-NMR of the toner particles of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the present invention, the expressions "xx or more and xx or less" and "xx to xx" expressing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified.

[0009] In the present invention, the term "monomer unit" refers to the reacted form of a monomer substance in a polymer.

[0010] The crystalline resin refers to a resin that shows a clear endothermic peak in a differential scanning calorimeter (DSC) measurement.

[0011] The toner of the present invention is a toner having core particles containing a binder resin and a wax, and having inorganic oxide fine particles on the surface of the core particles, and a coating layer containing an organosilicon polymer coating the core particles, The core particles satisfy the following relationship when the endothermic heat of the endothermic peak derived from the wax measured by differential scanning calorimetry (DSC) is Qi (J / g) and the endothermic heat of the endothermic peak derived from the wax measured by DSC after the core particles are treated with hexane is Qh (J / g): 0.7≦Qi-Qh≦20.0 The organosilicon polymer has a partial structure represented by the following formula (T3): The tetrahydrofuran insoluble portion of the toner particles 29 In Si-NMR measurement, the ratio [ST3] of the peak area of ​​the partial structure represented by the following formula (T3) to the total peak area of ​​the organosilicon polymer satisfies the relationship ST3 ≧ 0.05, R-Si(O 1 / 2 )3(T3) (In formula (T3), R represents an alkyl group having 1 to 6 carbon atoms or a phenyl group.) The toner is characterized in that the inorganic oxide fine particles are thermally fixed to the surface of the core particles.

[0012] The present inventors believe that the mechanism by which the effects of the present invention are realized is as follows. The surface of the core particles, which has a large amount of wax near the surface, is highly hydrophobic. On the other hand, the coating layer containing the organosilicon polymer of the present invention that coats the core particles is R-Si(O 1 / 2 )3(T3) In this structure, R is an alkyl group or a phenyl group having 1 to 6 carbon atoms, and is relatively hydrophobic, but since it also contains a large amount of hydrophilic Si-OH groups, the coating layer as a whole is hydrophilic. Therefore, it is believed that the core particle and the coating layer have low wettability and low adhesion because the polarity is significantly different.

[0013] The toner particles of the present invention are characterized in that inorganic oxide fine particles are thermally fixed to the surface of the core particles. Fixation of inorganic oxide fine particles by heat improves the adhesion of the inorganic oxide fine particles to the surface of the core particles, and can suppress the detachment of the inorganic oxide fine particles even after endurance testing. In addition, the inorganic oxide fine particles contain oxygen atoms with high electronegativity. Therefore, the oxygen atoms of the inorganic oxide fine particles fixed to the hydrophobic wax, which has a hydrophobic site in abundance near the surface of the core particles, and the hydrophilic hydroxyl groups of the silanol sites of the organosilicon polymer exhibit affinity through an interaction such as hydrogen bonding, which is believed to be the action of adhering the organosilicon polymer to the core particles in which a large amount of wax is present.

[0014] The core particle of the toner particle of the present invention is characterized in that, when the endothermic heat of the endothermic peak derived from the wax measured by differential scanning calorimetry (DSC) is Qi (J / g), and the endothermic heat of the endothermic peak derived from the wax measured by DSC after hexane treatment of the core particle is Qh (J / g), the core particle satisfies the following relationship: 0.7≦Qi-Qh≦20.0

[0015] Qi indicates the amount of heat absorption derived from the wax present throughout the core particle. On the other hand, Qh indicates the amount of heat absorption derived from the wax present inside the core particle after the wax present near the core particle surface is dissolved in hexane and removed by treating the core particle with hexane. Therefore, Qi-Qh is a parameter indicating the amount of heat absorption derived from the wax present near the core particle surface, and the larger the value of Qi-Qh, the more wax is present near the core particle surface, so that the wax can be melted quickly in the fixing process and a high release effect can be exhibited. When Qi-Qh is in the above range, high anti-fixing wrap-around properties and non-image graininess after durability can be achieved at the same time. When Qi-Qh exceeds 20.0, the non-image graininess after durability deteriorates. It is preferably 0.7 to 10.0, more preferably 1.0 to 7.0, and even more preferably 1.8 to 5.0.

[0016] The toner particles of the present invention are characterized in that, when the endothermic heat of the endothermic peak derived from the wax measured by differential scanning calorimetry (DSC) is Qit, and the endothermic heat of the endothermic peak derived from the wax measured by DSC after hexane treatment is Qht (J / g), the following relationship is satisfied. 0.8≦Qit-Qht≦21.0

[0017] When Qit-Qht is in the above range, it is possible to achieve both high resistance to wrapping around the toner when fixing and low graininess of the image after durability testing.

[0018] In addition, the core particles of the toner particles of the present invention preferably have a (Qi-Qh) / Qi value in the range of 0.05 to 0.90. (Qi-Qh) / Qi is a parameter indicating the proportion of wax present near the surface of the core particles, and a high value indicates that more wax is present near the surface than inside the core particles. When the (Qi-Qh) / Qi value is within the above range, high anti-wrapping properties and high levels of external additive ghost suppression effect and non-image graininess after durability testing can be achieved at the same time.

[0019] The toner particles of the present invention preferably have a value of (Qit-Qht) / Qit in the range of 0.06 to 0.95, more preferably 0.09 to 0.85, even more preferably 0.15 to 0.70, and even more preferably 0.21 to 0.42.

[0020] A preferred range of Qi is 3.0 to 40.0, more preferably 3.0 to 30.0, and even more preferably 5.0 to 15.0, from the viewpoint of easily controlling the ranges of Qi-Qh and (Qi-Qh) / Qi within the above ranges.

[0021] Qi can be controlled by the type of wax, the amount added, etc.

[0022] Qi-Qh can be controlled by the type and amount of wax, as well as the method of manufacturing the core particles. When forming toner particles in water, such as by the dissolution suspension method, emulsion aggregation method, or suspension polymerization method, hydrophilic materials tend to gather on the surface of the core particles, and hydrophobic wax tends to be unevenly distributed inside the toner particles. Therefore, it is preferable to form the core particles by a pulverization method after melt kneading. Furthermore, using the device shown in Figure 1 (details will be described later) and using core particles treated with hot air, the wax is unevenly distributed on the surface by the hot air treatment, and it is particularly preferable because it is easy to control Qi-Qh within the above range. Qi-Qh can be controlled by the temperature of the hot air, the flow rate of the hot air, the amount of core particles processed per hour, etc. In addition, when a wax dispersant is used, the moving speed of the wax by the hot air changes, so that the value of Qi-Qh can be changed.

[0023] The toner particles of the present invention have a coating layer containing an organosilicon polymer coating a core particle, the organosilicon polymer having a partial structure represented by the following formula (T3): The tetrahydrofuran (THF) insoluble portion of the toner particles 29 In Si-NMR measurement, the ratio [ST3] of the peak area of ​​the partial structure represented by the following formula (T3) to the total peak area of ​​the organosilicon polymer satisfies the relationship ST3 ≧ 0.05. R-Si(O 1 / 2 )3(T3) (In formula (T3), R represents an alkyl group or a phenyl group having 1 to 6 carbon atoms.)

[0024] The toner particles of the present invention are THF insoluble 29In the Si-NMR measurement, the ratio [ST3] of the peak area of ​​the partial structure represented by the above formula (T3) (hereinafter also referred to as T3 structure) to the total peak area of ​​the organosilicon polymer satisfies the relationship ST3≧0.05, so that the surface free energy of the toner particle surface can be lowered, and the adhesive force with the transfer member can be reduced, resulting in a good image with less graininess. If ST3 is less than 0.05, the graininess of the image deteriorates. A more preferable range for ST3 is 0.50 or more and 0.80 or less.

[0025] The proportion of the T unit structure can be controlled by the type and amount of organosilicon compound used to form the organosilicon polymer, as well as the reaction temperature, reaction time, reaction solvent, and pH in producing the organosilicon polymer.

[0026] The toner particles of the present invention are characterized in that inorganic oxide fine particles are thermally fixed to the surface of the core particles. As described above, the inorganic oxide fine particles are essential for improving the adhesion between the core particles, which have a large amount of wax near the surface, and the organosilicon polymer that coats the core particles.

[0027] The inorganic oxide microparticles contain oxygen atoms with high electronegativity, and examples of such inorganic oxide microparticles include silica microparticles, aluminum oxide microparticles, titanium oxide microparticles, magnesium oxide microparticles, tin oxide microparticles, zinc oxide microparticles, cerium oxide microparticles, zirconium oxide microparticles, magnesium titanate microparticles, strontium titanate microparticles, calcium titanate microparticles, strontium zirconate microparticles, calcium zirconate microparticles, and composites of these compositions. Preferred inorganic oxide microparticles are silica microparticles, titanium oxide microparticles, and strontium titanate microparticles, and more preferably strontium titanate microparticles.

[0028] The inorganic oxide fine particles preferably have a number average particle size (D1) of primary particles of 7 nm to 300 nm, more preferably 7 nm to 55 nm, and even more preferably 30 nm to 50 nm. When D1 is within the above range, the inorganic oxide fine particles are not completely buried in the core particles by hot air treatment, and the adhesion with the organosilicon polymer is improved, the occurrence of ghosts is suppressed, and charging properties are improved, which is preferable.

[0029] The inorganic oxide fine particles preferably have a coverage of 1% to 50% of the surface of the core particles, more preferably 3% to 30%, and even more preferably 10% to 20%. With a coverage within the above range, the adhesion between the inorganic oxide fine particles and the organosilicon polymer is improved, the occurrence of ghosts is suppressed, and separability is improved. The coverage can be controlled by the amount and particle size of the inorganic oxide fine particles, external addition conditions, heat treatment conditions described below, etc.

[0030] In addition, it is preferable to use two types of inorganic oxide particles selected from the above-mentioned fine particles as the inorganic oxide particles to be thermally fixed to the core particle surface. By using two types of inorganic oxide particles selected from the above-mentioned fine particles, it is possible to improve not only the adhesion but also the fixing separation property and the charging stability.

[0031] The inorganic oxide fine particles are preferably thermally fixed in a form embedded in a part of the core particle surface, and can be thermally fixed by a heat treatment device described later. As a method for thermally fixing, a method in which the inorganic oxide fine particles are mixed with the toner particles at a low temperature and then surface-treated with hot air is preferred, since the inorganic oxide fine particles can be uniformly fixed. When the inorganic fine particles are thermally fixed, the coverage rate of the core particle surface described above refers to the coverage rate after thermal fixing.

[0032] The state in which inorganic oxide particles are embedded in the surface of a toner particle can be confirmed by observing the surface contour of a toner particle at 80,000 times magnification using a Hitachi ultra-high resolution field emission scanning electron microscope (FE-SEM; S-4800, Hitachi High-Technologies Corporation). FE stands for Field Emission.

[0033] <Organosilicon polymer> A representative example of the production method for the organosilicon polymer used in the present invention is the so-called sol-gel method.

[0034] The sol-gel method uses metal alkoxide M(OR)n (M: metal, O: oxygen, R: hydrocarbon, n: metal valence) as a starting material, hydrolyzes and condenses in a solvent to form a sol, then gels, and is used to synthesize glass, ceramics, organic-inorganic hybrids, and nanocomposites. Using this manufacturing method, functional materials in various shapes, such as surfaces, fibers, bulk bodies, and fine particles, can be produced from the liquid phase at low temperatures.

[0035] Specifically, the organosilicon polymer contained in the toner particles is preferably produced by hydrolysis and condensation polymerization of a silicon compound, typically an alkoxysilane.

[0036] In one preferred embodiment, the surface layer containing the organosilicon polymer is uniformly provided on the surface of the toner particles. By providing the surface layer containing the organosilicon polymer uniformly on the surface of the toner particles, the adhesive force with the transfer member can be reduced, and a toner can be obtained that produces good images with little graininess.

[0037] Furthermore, because the sol-gel process starts with a solution and forms the material by gelling the solution, a variety of microstructures and shapes can be created.

[0038] The above-mentioned fine structure and shape can be adjusted by the reaction temperature, reaction time, reaction solvent, pH, the type and amount of the organosilicon compound added, and the like.

[0039] The organosilicon polymer used in the present invention is preferably an organosilicon polymer obtained by polymerizing an organosilicon compound having a structure represented by the following formula (Z).

[0040] [ka]

[0041] R1 represents a hydrocarbon group having 1 to 6 carbon atoms or an aryl group. The hydrocarbon group in R1 is a hydrocarbon group other than an aryl group. When R1 is a hydrocarbon group or an aryl group, the hydrophobicity of the resulting organosilicon polymer can be improved, and a toner having excellent environmental stability can be obtained. When the hydrophobicity of R1 is high, the charge amount tends to fluctuate greatly in various environments, so in consideration of environmental stability, R1 preferably has 1 to 3 carbon atoms. Preferred examples of the hydrocarbon group having 1 to 3 carbon atoms include a methyl group, an ethyl group, and a propyl group, and preferred examples of the aryl group include a phenyl group. In this case, the chargeability and fogging suppression are good. More preferably, R1 is a methyl group from the viewpoint of environmental stability and storage stability.

[0042] R2 to R4 are each independently a halogen atom, a hydroxy group, an acetoxy group, or an alkoxy group (hereinafter also referred to as "reactive group"). These reactive groups undergo hydrolysis, addition polymerization, and condensation polymerization to form a crosslinked structure, thereby making it possible to obtain a toner having excellent resistance to component contamination and development durability. The hydrolysis is mild at room temperature, and from the viewpoint of deposition and coating properties on the surface of the toner particles, a methoxy group or an ethoxy group is preferred. The hydrolysis, addition polymerization, and condensation polymerization of R2 to R4 can be controlled by the reaction temperature, reaction time, reaction solvent, and pH.

[0043] The organosilicon polymer used in this invention can be obtained by using one or a combination of several organosilicon compounds having three reactive groups (R2, R3 and R4) in one molecule excluding R1 in the formula (Z) shown above (hereinafter referred to as "trifunctional silanes").

[0044] In the present invention, the content of the organosilicon polymer in the toner particles is preferably from 0.5 to 50% by weight, and more preferably from 0.75 to 40.0% by weight.

[0045] The above formula (Z) includes the following.

[0046] Trifunctional methylsilanes such as methyltrimethoxysilane, methyltriethoxysilane, methyldiethoxymethoxysilane, methylethoxydimethoxysilane, methyltrichlorosilane, methylmethoxydichlorosilane, methylethoxydichlorosilane, methyldimethoxychlorosilane, methylmethoxyethoxychlorosilane, methyldiethoxychlorosilane, methyltriacetoxysilane, methyldiacetoxymethoxysilane, methyldiacetoxyethoxysilane, methylacetoxydimethoxysilane, methylacetoxymethoxyethoxysilane, methylacetoxydiethoxysilane, methyltrihydroxysilane, methylmethoxydihydroxysilane, methylethoxydihydroxysilane, methyldimethoxyhydroxysilane, methylethoxymethoxyhydroxysilane, and methyldiethoxyhydroxysilane.

[0047] Trifunctional silanes such as ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrichlorosilane, ethyltriacetoxysilane, ethyltrihydroxysilane, propyltrimethoxysilane, propyltriethoxysilane, propyltrichlorosilane, propyltriacetoxysilane, propyltrihydroxysilane, butyltrimethoxysilane, butyltriethoxysilane, butyltrichlorosilane, butyltriacetoxysilane, butyltrihydroxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, hexyltrichlorosilane, hexyltriacetoxysilane, and hexyltrihydroxysilane.

[0048] Trifunctional phenylsilanes such as phenyltrimethoxysilane, phenyltriethoxysilane, phenyltrichlorosilane, phenyltriacetoxysilane, and phenyltrihydroxysilane.

[0049] Trifunctional vinyl silanes such as vinyl ethoxydimethoxysilane, vinyl trichlorosilane, vinyl methoxydichlorosilane, vinyl ethoxydichlorosilane, vinyl dimethoxychlorosilane, vinyl methoxyethoxychlorosilane, vinyl diethoxychlorosilane, vinyl triacetoxysilane, vinyl diacetoxymethoxysilane, vinyl diacetoxyethoxysilane, vinyl acetoxydimethoxysilane, vinyl acetoxymethoxyethoxysilane, vinyl acetoxydiethoxysilane, vinyl trihydroxysilane, vinyl methoxydihydroxysilane, vinyl ethoxydihydroxysilane, vinyl dimethoxyhydroxysilane, vinyl ethoxymethoxyhydroxysilane, and vinyl diethoxyhydroxysilane.

[0050] Trifunctional allylsilanes such as allyltrimethoxysilane, allyltriethoxysilane, allyltrichlorosilane, allyltriacetoxysilane, and allyltrihydroxysilane.

[0051] In the organosilicon polymer used in the present invention, the content of the organosilicon compound having the structure represented by formula (Z) in the organosilicon polymer is preferably 50 mol % or more, more preferably 60 mol % or more. By making the content of the organosilicon compound satisfying formula (Z) 50 mol % or more, the environmental stability of the toner can be further improved.

[0052] In addition, in the present invention, the organosilicon polymer obtained by using an organosilicon compound having a structure represented by formula (Z) and an organosilicon compound having four reactive groups in one molecule (tetrafunctional silane), an organosilicon compound having three reactive groups in one molecule (trifunctional silane), an organosilicon compound having two reactive groups in one molecule (bifunctional silane) or an organosilicon compound having one reactive group (monofunctional silane) may be used in combination to the extent that the effect of the present invention is not impaired.The organosilicon compound that may be used in combination includes the following.

[0053] Dimethyldiethoxysilane, tetraethoxysilane, hexamethyldisilazane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, Aminopropyltriethoxysilane, 3-phenylaminopropyltrimethoxysilane, 3-anilinopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, hexamethyldisiloxane, tetraisocyanate silane, methyltriisocyanate silane, vinyltriisocyanate silane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyldiethoxymethoxysilane.

[0054] In the toner of the present invention, when the surface layer (surface layer, outermost layer) of a toner particle is measured using X-ray photoelectron spectroscopy analysis (ESCA: Electron Spectroscopy for Chemical Analysis), the concentration of silicon atoms dSi (dSi / [dC+dO+dSi+dS]) relative to the sum (dC+dO+dSi+dS) of the concentration of carbon atoms dC, the concentration of oxygen atoms dO, the concentration of silicon atoms dSi, and the concentration of sulfur atoms dS in the surface layer of the toner particle is preferably 1.0 atomic % or more, more preferably 2.5 atomic % or more, even more preferably 5.0 atomic % or more, and particularly preferably 15.0 atomic % or more.

[0055] The ESCA is used to perform elemental analysis of the surface layer that is present at a thickness of several nm from the surface of the toner particle to the center of the toner particle (midpoint of the long axis). By making the concentration of silicon atoms (dSi / [dC+dO+dSi+dS]) in the surface layer of the toner particle 1.0 atomic % or more, the surface free energy of the surface layer can be reduced. As a result, contamination of the toner particle surface can be suppressed, and the charging stability can be further improved.

[0056] On the other hand, the concentration of silicon atoms in the surface layer of the toner particle (dSi / [dC+dO+dSi+dS]) is preferably 33.3 atomic % or less, and more preferably 28.6 atomic % or less, from the viewpoint of chargeability.

[0057] The concentration of silicon atoms in the surface layer of the toner particles can be controlled by the structure of Rf in the above formula (T3), the method of producing the toner particles when forming the organosilicon polymer, the reaction temperature, the reaction time, the reaction solvent, and the pH. It can also be controlled by the content of the organosilicon polymer. In the present invention, the surface layer of the toner particles means a layer that exists from the surface of the toner particles toward the center of the toner particles (the midpoint of the major axis) and has a thickness of 0.0 nm to 5.0 nm.

[0058] <Binding resin> The core particles in the present invention can use the following polymers as the binder resin. Homopolymers of styrene and its substitutes, such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-based copolymers, such as styrene-p-chlorostyrene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-acrylic acid ester copolymer, and styrene-methacrylic acid ester copolymer; polyvinyl chloride, phenolic resin, naturally modified phenolic resin, naturally resin modified maleic acid resin, acrylic resin, methacrylic resin, polyvinyl acetate, silicone resin, polyester resin, polyurethane, polyamide resin, furan resin, epoxy resin, xylene resin, polyethylene resin, and polypropylene resin. Among them, amorphous resins are preferred, and those containing amorphous polyester resin as the main component are more preferred from the viewpoint of low-temperature fixability. In addition, in order to fix inorganic oxide fine particles to the surface of the core particles, toners containing polyester resin as the binder resin are more preferred than toners containing styrene acrylic resin as the binder resin, because the fixation of the inorganic oxide fine particles is more likely to occur.

[0059] As the monomers used in the polyester unit of the polyester resin, polyhydric alcohols (divalent or trivalent or higher alcohols), polyvalent carboxylic acids (divalent or trivalent or higher carboxylic acids), their acid anhydrides or their lower alkyl esters are used. Here, in order to produce a branched polymer in order to express "strain hardening", it is effective to partially crosslink the amorphous resin molecule, and for this purpose, it is preferable to use a polyfunctional compound having a valence of three or more. Therefore, it is preferable to include a trivalent or higher carboxylic acid, its acid anhydride or its lower alkyl ester, and / or a trivalent or higher alcohol as the raw material monomer of the polyester unit.

[0060] As the polyhydric alcohol monomer used in the polyester unit of the polyester resin, the following polyhydric alcohol monomers can be used.

[0061] Examples of the dihydric alcohol component include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, hydrogenated bisphenol A, and bisphenol represented by formula (A) and its derivatives;

[0062] [ka] (In the formula, R is an ethylene or propylene group, x and y are each an integer of 0 or more, and the average value of x+y is 0 or more and 10 or less.)

[0063] Diols represented by formula (B);

[0064] [ka]

[0065] Examples of trihydric or higher alcohol components include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene. Among these, glycerol, trimethylolpropane, and pentaerythritol are preferably used. These dihydric alcohols and trihydric or higher alcohols can be used alone or in combination. As the polybasic carboxylic acid monomer used in the polyester unit of the polyester resin, the following polybasic carboxylic acid monomers can be used.

[0066] Examples of divalent carboxylic acid components include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, n-dodecenylsuccinic acid, isododecenylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid, n-octenylsuccinic acid, n-octylsuccinic acid, isooctylsuccinic acid, isooctylsuccinic acid, anhydrides of these acids, and lower alkyl esters thereof. Of these, maleic acid, fumaric acid, terephthalic acid, and n-dodecenylsuccinic acid are preferably used.

[0067] Examples of trivalent or higher carboxylic acids, their anhydrides or their lower alkyl esters include 1,2,4-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empol trimer acid, their anhydrides or their lower alkyl esters. Among these, 1,2,4-benzenetricarboxylic acid, i.e., trimellitic acid or its derivatives, is particularly preferred because it is inexpensive and easy to control the reaction. These divalent carboxylic acids and trivalent or higher carboxylic acids can be used alone or in combination.

[0068] The method for producing the polyester unit of the present invention is not particularly limited, and a known method can be used. For example, the above-mentioned alcohol monomer and carboxylic acid monomer are simultaneously charged, and polymerized through an esterification reaction or an ester exchange reaction and a condensation reaction to produce a polyester resin. The polymerization temperature is not particularly limited, but is preferably in the range of 180°C to 290°C. For the polymerization of the polyester unit, for example, a polymerization catalyst such as a titanium-based catalyst, a tin-based catalyst, zinc acetate, antimony trioxide, or germanium dioxide can be used.

[0069] From the viewpoint of charging stability, it is preferable that the acid value of the polyester resin is 5 mgKOH / g or more and 30 mgKOH / g or less, and the hydroxyl value is 20 mgKOH / g or more and 70 mgKOH / g or less.

[0070] The binder resin may be a mixture of a low molecular weight resin and a high molecular weight resin. The content ratio of the high molecular weight resin to the low molecular weight resin is preferably 40 / 60 or more and 85 / 15 or less on a mass basis from the viewpoint of low temperature fixability and hot offset resistance.

[0071] Furthermore, it is preferable that the core particles contain a resin having crystallinity, since this further improves the low-temperature fixing property.

[0072] Examples of the resin having crystallinity include crystalline polyester, crystalline vinyl resin, crystalline polyurethane, and crystalline polyurea, with crystalline polyester and crystalline vinyl resin being preferred.

[0073] The crystalline polyester is obtained by polycondensation of a monomer composition containing an aliphatic diol and an aliphatic dicarboxylic acid as main components. The aliphatic diol and the aliphatic dicarboxylic acid preferably have 6 to 12 carbon atoms.

[0074] The aliphatic diol is not particularly limited, but is preferably a chain-like (more preferably a straight-chain) aliphatic diol, such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, 1,4-butanediol, 1,4-butadiene glycol, trimethylene glycol, tetramethylene glycol, pentamethylene glycol, hexamethylene glycol, octamethylene glycol, nonamethylene glycol, decamethylene glycol, neopentyl glycol. Among these, particularly preferred are straight-chain aliphatic α,ω-diols such as ethylene glycol, diethylene glycol, 1,4-butanediol, and 1,6-hexanediol. Of the above alcohol components, it is preferable that 50% by mass or more, more preferably 70% by mass or more, is an alcohol selected from aliphatic diols having 6 to 12 carbon atoms.

[0075] In addition, polyhydric alcohol monomers other than the above aliphatic diols can also be used. Among the polyhydric alcohol monomers, examples of dihydric alcohol monomers include aromatic alcohols such as polyoxyethylenated bisphenol A and polyoxypropylenated bisphenol A; 1,4-cyclohexanedimethanol, etc. Among the polyhydric alcohol monomers, examples of trihydric or higher polyhydric alcohol monomers include aromatic alcohols such as 1,3,5-trihydroxymethylbenzene; and aliphatic alcohols such as pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerin, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, and trimethylolpropane.

[0076] Furthermore, monohydric alcohols may be used to the extent that they do not impair the properties of the crystalline polyester. Examples of the monohydric alcohols include monofunctional alcohols such as n-butanol, isobutanol, sec-butanol, n-hexanol, n-octanol, lauryl alcohol, 2-ethylhexanol, decanol, cyclohexanol, benzyl alcohol, and dodecyl alcohol.

[0077] On the other hand, the aliphatic dicarboxylic acid is not particularly limited, but is preferably a chain (more preferably a straight-chain) aliphatic dicarboxylic acid.Specific examples include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, glutaconic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, maleic acid, fumaric acid, mesaconic acid, citraconic acid, and itaconic acid, and also includes those obtained by hydrolyzing the acid anhydrides or lower alkyl esters of these acids.

[0078] Of the carboxylic acid components, preferably 50% by mass or more, more preferably 70% by mass or more, is a carboxylic acid selected from aliphatic dicarboxylic acids having 6 to 12 carbon atoms.

[0079] Polycarboxylic acids other than aliphatic dicarboxylic acids can also be used. Among the other polycarboxylic acid monomers, examples of divalent carboxylic acids include aromatic carboxylic acids such as isophthalic acid and terephthalic acid; aliphatic carboxylic acids such as n-dodecyl succinic acid and n-dodecenyl succinic acid; and alicyclic carboxylic acids such as cyclohexane dicarboxylic acid, and also include their acid anhydrides or lower alkyl esters. Among the other carboxylic acid monomers, examples of trivalent or higher polycarboxylic acids include aromatic carboxylic acids such as 1,2,4-benzene tricarboxylic acid (trimellitic acid), 2,5,7-naphthalene tricarboxylic acid, 1,2,4-naphthalene tricarboxylic acid, and pyromellitic acid, and aliphatic carboxylic acids such as 1,2,4-butane tricarboxylic acid, 1,2,5-hexane tricarboxylic acid, and 1,3-dicarboxyl-2-methyl-2-methylene carboxypropane, and also include their acid anhydrides or lower alkyl esters.

[0080] Furthermore, the crystalline polyester may contain a monovalent carboxylic acid to the extent that the properties of the crystalline polyester are not impaired. Examples of the monovalent carboxylic acid include monocarboxylic acids such as benzoic acid, naphthalene carboxylic acid, salicylic acid, 4-methylbenzoic acid, 3-methylbenzoic acid, phenoxyacetic acid, biphenyl carboxylic acid, acetic acid, propionic acid, butyric acid, octanoic acid, decanoic acid, dodecanoic acid, and stearic acid.

[0081] The crystalline polyester of the present invention can be produced according to a conventional polyester synthesis method. For example, the above-mentioned carboxylic acid monomer and alcohol monomer are subjected to an esterification reaction or an ester exchange reaction, and then the desired crystalline polyester can be obtained by a conventional polycondensation reaction under reduced pressure or by introducing nitrogen gas.

[0082] The above esterification or transesterification reaction can be carried out, if necessary, using a common esterification catalyst or transesterification catalyst such as sulfuric acid, titanium butoxide, dibutyltin oxide, manganese acetate, magnesium acetate, etc.

[0083] The polycondensation reaction can be carried out using a conventional polymerization catalyst, such as titanium butoxide, dibutyltin oxide, tin acetate, zinc acetate, tin disulfide, antimony trioxide, germanium dioxide, etc. The polymerization temperature and the amount of catalyst are not particularly limited and may be appropriately determined.

[0084] In the esterification or transesterification reaction or polycondensation reaction, all the monomers may be charged at once in order to increase the strength of the resulting crystalline polyester. In addition, in order to reduce low molecular weight components, a method may be used in which a divalent monomer is reacted first, and then a trivalent or higher monomer is added and reacted.

[0085] An example of the crystalline vinyl resin is a resin containing a polymer having a unit derived from a polymerizable monomer that is a (meth)acrylic acid ester having an alkyl group having 18 or more and 36 or less carbon atoms.

[0086] Examples of (meth)acrylic acid esters having an alkyl group having 18 to 36 carbon atoms include (meth)acrylic acid esters having a straight-chain alkyl group having 18 to 36 carbon atoms [stearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, heneicosanyl (meth)acrylate, behenyl (meth)acrylate, lignoceryl (meth)acrylate, ceryl (meth)acrylate, octacosyl (meth)acrylate, myrisyl (meth)acrylate, dodriconta (meth)acrylate, etc.] and (meth)acrylic acid esters having a branched alkyl group having 18 to 36 carbon atoms [2-decyltetradecyl (meth)acrylate, etc.].

[0087] Among these, from the viewpoint of storage stability of the toner, preferred are (meth)acrylic acid esters having a linear alkyl group having 18 to 36 carbon atoms, more preferred are (meth)acrylic acid esters having a linear alkyl group having 18 to 30 carbon atoms, and even more preferred are linear stearyl (meth)acrylate and behenyl (meth)acrylate.

[0088] In addition, it is preferable that the ratio of units derived from a polymerizable monomer that is a (meth)acrylic acid ester having an alkyl group having 18 to 36 carbon atoms in the polymer is 10.0 mol % or more and 60.0 mol % or less relative to the total number of moles of all units in the polymer.

[0089] The content of these crystalline resins is preferably 0.5 parts by mass or more and 15 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0090] From the viewpoint of suppressing moisture adsorption, the acid value of the crystalline resin is preferably 2 mgKOH / g or more and 20 mgKOH / g or less.

[0091] In addition, for the purpose of controlling the state of wax present in the core particles, which will be described later, and controlling the state of wax present within the range of Qi-Qh of the present invention, it is preferable to contain a wax dispersant in the core particles.

[0092] As the wax dispersant, it is preferable to use a polymer in which a styrene-acrylic polymer is graft-modified to a polyolefin.

[0093] The polyolefin is not particularly limited, but examples thereof include low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and hydrocarbon wax such as Fischer-Tropsch wax.

[0094] The polyolefin preferably has a maximum endothermic peak temperature measured by a differential scanning calorimeter (DSC) of 70° C. to 100° C. From the viewpoint of wax dispersibility, the difference in peak temperature between the wax and the polyolefin, which are the maximum endothermic peaks measured by a differential scanning calorimeter (DSC), is preferably 0° C. to 20° C.

[0095] Examples of monomers constituting the monomer units of the styrene-acrylic polymer include styrenes such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-methoxystyrene, p-phenylstyrene, p-chlorostyrene, 3,4-dichlorostyrene, p-ethylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene; styrene-based monomers such as dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, and other amino group-containing α-methylene aliphatic monocarboxylic acid esters; vinyl-based monomers containing N atoms such as acrylic acid or methacrylic acid derivatives such as acrylonitrile, methacrylonitrile, and acrylamide; unsaturated dibasic acids such as maleic acid, citraconic acid, itaconic acid, alkenylsuccinic acid, fumaric acid, and mesaconic acid; maleic anhydride, citraconic anhydride, itaconic anhydride, and alkenylsuccinic acid-free unsaturated dibasic acid anhydrides such as water; unsaturated dibasic acid half esters such as methyl maleate half ester, ethyl maleate half ester, butyl maleate half ester, methyl citraconic acid half ester, ethyl citraconic acid half ester, butyl citraconic acid half ester, methyl itaconic acid half ester, methyl alkenyl succinate half ester, methyl fumaric acid half ester, methyl mesaconic acid half ester; unsaturated dibasic acid esters such as dimethyl maleate and dimethyl fumaric acid; acrylic acid α,β-unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, and cinnamic acid; α,β-unsaturated acid anhydrides such as crotonic acid anhydride and cinnamic acid anhydride, and anhydrides of the above α,β-unsaturated acids and lower fatty acids; vinyl monomers containing a carboxyl group such as alkenylmalonic acid, alkenylglutaric acid, alkenyladipic acid, acid anhydrides thereof, and monoesters thereof; acrylic acid or methacrylic acid esters such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate;Examples of the hydroxyl group-containing vinyl monomers include 4-(1-hydroxy-1-methylbutyl)styrene and 4-(1-hydroxy-1-methylhexyl)styrene; acrylic acid esters such as methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, propyl acrylate, n-octyl acrylate, dodecyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, 2-chloroethyl acrylate, and phenyl acrylate; and methacrylic acid esters such as α-methylene aliphatic monocarboxylic acid esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-octyl methacrylate, dodecyl methacrylate, 2-ethylhexyl methacrylate, stearyl methacrylate, phenyl methacrylate, dimethylaminoethyl methacrylate, and diethylaminoethyl methacrylate.

[0096] Furthermore, a vinyl monomer having a structural portion derived from a saturated alicyclic compound may be contained.

[0097] If the vinyl monomer having a structure portion derived from a saturated alicyclic compound is contained, it is preferable because it can further improve the charging stability.As the vinyl monomer having a structure portion derived from a saturated alicyclic compound, there can be mentioned cyclopropyl acrylate, cyclobutyl acrylate, cyclopentyl acrylate, cyclohexyl acrylate, cycloheptyl acrylate, cyclooctyl acrylate, cyclopropyl methacrylate, cyclobutyl methacrylate, cyclopentyl methacrylate, cyclohexyl methacrylate, cycloheptyl methacrylate, cyclooctyl methacrylate, dihydrocyclopentadiethyl acrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate and the like monomers and their combinations.

[0098] Among these, from the viewpoint of hydrophobicity, cyclohexyl acrylate, cycloheptyl acrylate, cyclooctyl acrylate, cyclohexyl methacrylate, cycloheptyl methacrylate, and cyclooctyl methacrylate are preferred.

[0099] In the present invention, the method for graft-modifying the polyolefin with the styrene-acrylic polymer is not particularly limited, and any conventionally known method can be used.

[0100] In the present invention, the weight average molecular weight (Mw) of the THF-soluble portion of the polymer, as determined by gel permeation chromatography (GPC), is preferably from 5,000 to 70,000, and more preferably from 10,000 to 50,000. When the weight average molecular weight (Mw) of the polymer is within the above range, the dispersibility of the wax in the toner particles is improved, and at the same time, the blocking resistance and hot offset resistance are improved.

[0101] The polymer is preferably contained in an amount of 1.0 part by mass or more and 10.0 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0102] <Wax> Examples of waxes that can be used in the core particles of the present invention include the following: hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof; waxes containing fatty acid esters as the main component such as carnauba wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax. Further examples include the following. Saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and valinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; esters of fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid with alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, hexamethylene Saturated fatty acid bisamides such as bisstearamide; unsaturated fatty acid amides such as ethylene bisoleamide, hexamethylene bisoleamide, N,N' dioleyl adipamide, and N,N' dioleyl sebacamide; aromatic bisamides such as m-xylene bisstearamide and N,N' distearyl isophthalamide; fatty metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.

[0103] Among these waxes, from the viewpoint of improving low-temperature fixability and fixation separation property, preferred are hydrocarbon waxes such as paraffin wax and Fischer-Tropsch wax, and fatty acid ester waxes such as carnauba wax. In the present invention, when a polyester resin is used as the binder resin for the core particles, the hydrocarbon wax is more preferred from the viewpoint of further improving fixation separation resistance.

[0104] In the present invention, the wax is preferably used in an amount of 2 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the binder resin.

[0105] In addition, in an endothermic curve during temperature rise measured by a differential scanning calorimetry (DSC) device, the peak temperature of the maximum endothermic peak of the wax is preferably 45° C. or more and 140° C. or less, more preferably 70° C. or more and 110° C. or less, and even more preferably 85° C. or more and 110° C. or less. If the peak temperature of the maximum endothermic peak of the wax is within the above range, it is preferable because it is easy to achieve both the storage stability and hot offset resistance of the toner.

[0106] <Coloring agent> The toner may contain a colorant. Examples of the colorant include the following.

[0107] Examples of black colorants include carbon black, and a mixture of a yellow colorant, a magenta colorant, and a cyan colorant toned to black. As the colorant, a pigment may be used alone, but it is more preferable to use a dye and a pigment in combination to improve the clarity of the colorant from the viewpoint of the image quality of a full-color image.

[0108] Magenta toner pigments include the following: CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.

[0109] Dyes for magenta toners include solvent dyes such as CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1; basic dyes such as CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28.

[0110] Pigments for cyan toners include the following: CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, 17; CI Vat Blue 6; CI Acid Blue 45; copper phthalocyanine pigments having 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton.

[0111] Cyan toner dyes include CI Solvent Blue 70.

[0112] Yellow toner pigments include: CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185; CI Vat Yellow 1, 3, 20. Yellow toner dyes include CI Solvent Yellow 162.

[0113] The content of the colorant is preferably 0.1 parts by mass or more and 30 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0114] <Charge control agent> The toner may contain a charge control agent as necessary. Any known charge control agent may be used as the charge control agent contained in the toner, but a metal compound of an aromatic carboxylic acid is particularly preferred, as it is colorless, has a high charging speed, and can stably maintain a constant charge amount.

[0115] Examples of negative charge control agents include metal salicylate compounds, metal naphthoate compounds, metal dicarboxylate compounds, polymeric compounds having sulfonic acid or carboxylic acid on the side chain, polymeric compounds having sulfonate or sulfonate ester on the side chain, polymeric compounds having carboxylate or carboxylate ester on the side chain, boron compounds, urea compounds, silicon compounds, and calixarenes. The charge control agent may be added internally or externally to the toner particles.

[0116] The amount of the charge control agent added is preferably 0.2 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0117] <Inorganic fine particles> The toner particles of the present invention may contain inorganic fine particles as necessary, in addition to the inorganic oxide fine particles of the present invention fixed to the surface of the core particles. The inorganic fine particles may be added internally to the toner particles or may be mixed with the toner particles as an external additive. As the external additive, inorganic fine particles (inorganic fine powder) such as silica, titanium oxide, aluminum oxide, etc. are preferable. The inorganic fine particles are preferably hydrophobized with a hydrophobizing agent such as a silane compound, silicone oil, or a mixture thereof.

[0118] As an external additive to improve fluidity, 2 / g or more 400m 2 / g or less, and for stabilizing durability, inorganic fine particles with a specific surface area of ​​10 m 2 / g or more 50m 2 In order to simultaneously improve the flowability of the toner and stabilize its durability, inorganic fine particles having a specific surface area within the above range may be used in combination.

[0119] The external additive is preferably used in an amount of 0.1 parts by mass to 10.0 parts by mass based on 100 parts by mass of toner particles. The toner particles and the external additive can be mixed using a known mixer such as a Henschel mixer.

[0120] <Developer> The toner can be used as a one-component developer, but in order to further improve dot reproducibility, it is preferable to mix the toner with a magnetic carrier and use it as a two-component developer, in that stable images can be obtained over a long period of time. That is, it is preferable that the toner is the toner of the present invention, which is a two-component developer containing a toner and a magnetic carrier.

[0121] Examples of magnetic carriers that can be used include generally known magnetic carriers such as iron powder with an oxidized surface, unoxidized iron powder, metal particles such as iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, chromium, and rare earth elements, alloy particles thereof, oxide particles, magnetic materials such as ferrite, and magnetic material-dispersed resin carriers (so-called resin carriers) that contain a magnetic material and a binder resin that holds the magnetic material in a dispersed state.

[0122] When the toner is mixed with a magnetic carrier to be used as a two-component developer, good results are usually obtained when the carrier mixing ratio, in terms of the toner concentration in the two-component developer, is preferably 2% by mass or more and 15% by mass or less, and more preferably 4% by mass or more and 13% by mass or less.

[0123] [Method of manufacturing toner particles] <Production of core particles> As a method for producing the core particles of the toner particles of the present invention, a pulverization method is preferred because it is easy to make the wax exist near the surface of the core particles. When a production method for producing core particles in water, such as an emulsion aggregation method, a dissolution suspension method, or a suspension polymerization method, is used, the highly hydrophobic wax is unevenly distributed inside the core particles, and it is difficult to control the state of the wax within the Qi-Qh range of the present invention.

[0124] An example of a procedure for producing a toner by the pulverization method will be described below.

[0125] In the raw material mixing process, materials constituting the core particles, such as binder resin, wax, colorant, and other components such as charge control agent as necessary, are weighed out in predetermined amounts, blended, and mixed. Examples of mixing devices include double con mixers, V-type mixers, drum mixers, super mixers, Henschel mixers, Nauta mixers, and Mechano Hybrid (manufactured by Nippon Coke and Engineering Co., Ltd.).

[0126] Next, the mixed materials are melt-kneaded to disperse the wax in the binder resin. In the melt-kneading process, a batch kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used, and single-screw or twin-screw extruders are mainstream due to their advantage of continuous production. For example, a KTK twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a PCM kneader (manufactured by Ikegai Iron Works Co., Ltd.), a twin-screw extruder (manufactured by KCK Corporation), a Co-kneader (manufactured by Buss Co., Ltd.), and Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.) can be mentioned. Furthermore, the resin composition obtained by melt-kneading may be rolled with a two-roller or the like, and cooled with water or the like in a cooling process.

[0127] The cooled resin composition is then pulverized to a desired particle size in a pulverization process, which involves coarse pulverization using a pulverizer such as a crusher, hammer mill, or feather mill, followed by further pulverization using a pulverizer such as a Cryptron System (Kawasaki Heavy Industries), a Super Rotor (Nisshin Engineering), a Turbo Mill (Turbo Kogyo), or an air jet type pulverizer.

[0128] Thereafter, as necessary, the particles are classified using a classifier or sieve such as an inertial classification type Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), a centrifugal classification type Turboplex (manufactured by Hosokawa Micron Corporation), a TSP Separator (manufactured by Hosokawa Micron Corporation), or a Faculty (manufactured by Hosokawa Micron Corporation) to obtain classified products (core particles). Among these, the Faculty (manufactured by Hosokawa Micron Corporation) is preferred in terms of improving transfer efficiency because it can perform a spheroidizing process on the core particles simultaneously with classification.

[0129] <Inorganic oxide fine particle adhesion and thermal fixation process> A method for thermally fixing the inorganic oxide fine particles of the present invention to the surfaces of the core particles will be described below.

[0130] In the method of fixing inorganic oxide particles to the surface of the toner using hot air, inorganic oxide particles are first added to the surface of the core particles to attach the inorganic oxide particles to the core particles. Examples of the method of adding inorganic oxide particles include a method of mixing a predetermined amount of toner particles and inorganic oxide particles, and stirring and mixing them using a mixing device such as a double con mixer, V-type mixer, drum mixer, super mixer, Henschel mixer, Nauta mixer, Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.), or Nobilta (manufactured by Hosokawa Micron Corporation).

[0131] Next, the core particles with the inorganic oxide particles attached thereto are heat-treated in a heat treatment process using a heat treatment device as shown in Figure 1. This heat treatment further increases the wax near the surface, making it very easy to control the wax state within the range of Qi-Qh and (Qi-Qh) / Qi of the present invention. As a result, the anti-wrapping property is improved.

[0132] The mixture (core particles with inorganic oxide fine particles attached) supplied by the raw material supply means 1 is introduced into an introduction pipe 3 installed on a vertical line of the raw material supply means by compressed gas adjusted by a compressed gas adjustment means 2. The mixture passing through the introduction pipe is uniformly dispersed by a conical protruding member 4 installed in the center of the raw material supply means, and is introduced into eight supply pipes 5 that radiate outward, and then into a treatment chamber 6 where heat treatment is carried out.

[0133] In Fig. 1, the mixture supplied by the material supply means 1 is introduced into an introduction pipe 3 installed on the central axis of a treatment chamber 6 by compressed gas adjusted by a compressed gas adjustment means 2. The mixture passing through the introduction pipe is uniformly dispersed by a conical protruding member 4 installed in the center of the material supply means, and is introduced into eight supply pipes 5 that radiate out in eight directions, and is introduced into the treatment chamber 6 where heat treatment is carried out from a powder particle supply port 14.

[0134] At this time, the flow of the mixture supplied to the processing chamber 6 is regulated by a regulating means 9 for regulating the flow of the mixture, which is provided in the processing chamber 6. Therefore, the mixture supplied to the processing chamber 6 is heat-treated while swirling within the processing chamber 6, and then cooled.

[0135] Hot air for heat-treating the supplied mixture is supplied from hot air inlet 7 of hot air supplying means 7, and is introduced into treatment chamber 6 by spirally swirling it with swirling member 13 for swirling the hot air. In terms of configuration, swirling member 13 for swirling the hot air has multiple blades, and the swirling of the hot air can be controlled by the number and angle of the blades. At this time, the approximately conical distribution member 12 can reduce bias in the swirling hot air.

[0136] The hot air supplied into the processing chamber 6 preferably has a temperature of 100°C or more and 300°C or less at the hot air outlet 11 of the hot air supplying means 7. If the temperature at the hot air outlet 11 of the hot air supplying means 7 is within the above range, it is possible to move the wax to the vicinity of the surface of the core particles while preventing fusion or coalescence of the core particles due to excessive heating of the mixture, thereby improving the anti-wrapping property. More preferably, the temperature is 20°C or more higher than the peak temperature of the maximum endothermic peak of the wax.

[0137] Furthermore, the heat-treated core particles to which the inorganic oxide fine particles have been thermally fixed are cooled by cold air supplied from cold air supply means 8 (8-1, 8-2, 8-3). The temperature of the cold air supplied from the cold air supply means 8 is preferably -20°C or higher and 30°C or lower. If the temperature of the cold air is within the above range, the heat-treated core particles can be efficiently cooled, and fusion or coalescence of the heat-treated core particles can be prevented without impeding the uniform spheroidization of the mixture. The absolute moisture content of the cold air is 0.5 g / m 3 More than 15.0g / m 3 It is preferable that:

[0138] Next, the cooled heat-treated core particles are collected by the collection means 10 at the lower end of the treatment chamber 6. A blower (not shown) is provided ahead of the collection means 10, and the particles are transported by suction.

[0139] The powder particle supply port 14 is provided so that the swirling direction of the supplied mixture and the swirling direction of the hot air are the same, and the recovery means 10 is provided on the outer periphery of the processing chamber 6 so as to maintain the swirling direction of the swirled powder particles. Furthermore, the cold air supplied from the cold air supply means 8 is configured to be supplied from the outer periphery of the device to the inner periphery of the processing chamber 6 in a horizontal and tangential direction. The swirling direction of the toner supplied from the powder particle supply port 14, the swirling direction of the cold air supplied from the cold air supply means 8, and the swirling direction of the hot air supplied from the hot air supply means 7 are all the same. Therefore, no turbulence occurs in the processing chamber 6, the swirling flow in the device is strengthened, a strong centrifugal force is applied to the core particles, and the dispersibility of the core particles is further improved, so that core particles with a uniform shape and few coalesced particles can be obtained.

[0140] <Organosilicon polymer coating process> The resulting core particles are then coated with the organosilicon polymer of the present invention to obtain the toner particles of the present invention.

[0141] Specific embodiments in which an organosilicon polymer is incorporated into the surface layer of a core particle will be described below, but the present invention is not limited to these.

[0142] First, the obtained core particles are dispersed in an aqueous medium. The following can be used as a dispersion stabilizer for the core particles in the aqueous medium.

[0143] Examples of inorganic dispersion stabilizers include tricalcium phosphate, magnesium phosphate, zinc phosphate, aluminum phosphate, calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina.

[0144] Examples of the organic dispersion stabilizer include polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, and starch.

[0145] Furthermore, known nonionic, anionic and cationic surfactants can also be used.

[0146] Specific examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether and polyoxyethylene oleyl ether, polyoxyalkylene derivatives such as polyoxyethylene alkylene alkyl ethers, sorbitan fatty acid esters such as sorbitan monolaurate and sorbitan monostearate, glycerin fatty acid esters such as glycerol monostearate, and polyoxyethylene fatty acid esters such as polyethylene glycol monolaurate.

[0147] Specific examples of the anionic surfactant include alkyl sulfates such as sodium lauryl sulfate, polyoxyethylene alkyl ether sulfate salts such as sodium polyoxyethylene lauryl ether sulfate, sulfonates such as sodium dodecylbenzenesulfonate and sodium alkylnaphthalenesulfonate, and higher fatty acid salts such as sodium stearate and sodium laurate.

[0148] Specific examples of cationic surfactants include quaternary ammonium salts such as dodecyl ammonium bromide, dodecyl trimethyl ammonium bromide, dodecyl pyridinium chloride, dodecyl pyridinium bromide, hexadecyl trimethyl ammonium bromide, lauryl trimethyl ammonium chloride, and alkyl benzyl dimethyl ammonium chloride.

[0149] Among these dispersion stabilizers, nonionic ones are preferred because they are easier to disperse.

[0150] From the viewpoint of ease of removal of the dispersion stabilizer after formation of the organosilicon polymer, it is preferable to use an inorganic dispersion stabilizer, and it is even more preferable to use a poorly water-soluble inorganic dispersion stabilizer.

[0151] In the present invention, when a poorly water-soluble inorganic dispersion stabilizer is used to disperse core particles in an aqueous medium, the amount of the dispersion stabilizer added is preferably 0.2 parts by mass or more and 2.0 parts by mass or less per 100.0 parts by mass of core particles. Also, it is preferable to prepare a core particle dispersion medium using water in an amount of 300 parts by mass or more and 3,000 parts by mass or less per 100 parts by mass of core particles.

[0152] In the present invention, when preparing an aqueous medium in which the above-mentioned poorly water-soluble inorganic dispersant is dispersed, a commercially available dispersion stabilizer may be used as is. In addition, in order to obtain a dispersion stabilizer having a fine and uniform particle size, the poorly water-soluble inorganic dispersant may be generated in a liquid medium such as water under high-speed stirring. Specifically, when tricalcium phosphate is used as the dispersion stabilizer, a preferred dispersion stabilizer can be obtained by mixing an aqueous sodium phosphate solution and an aqueous calcium chloride solution under high-speed stirring to form fine particles of tricalcium phosphate. Furthermore, the use of a tricalcium phosphate dispersion stabilizer is preferable from the viewpoint of the shape stability and manufacturing stability of the coating layer of the organosilicon polymer. The reason for this is due to the crystal structure of tricalcium phosphate. Tricalcium phosphate forms a hexagonal crystal structure in which calcium ions are arranged around calcium ions. Therefore, calcium ions are easily oriented in the aqueous medium on the surface of the core particles, and the electrical attraction with the silanol groups, which are the hydrolyzed parts of the organosilicon compound in the aqueous medium, is increased, making it easier to form a coating layer of the organosilicon polymer.

[0153] The condensation step can be carried out under any pH condition, but the condensation of the organosilicon compound affects the pH of the aqueous medium, so the effects of the present invention can be further enhanced by controlling the pH of the aqueous medium.

[0154] Under acidic conditions, the hydrolysis of alkoxy groups proceeds electrophilically with protons as a catalyst, so the hydrolysis of alkoxy groups in the molecule proceeds sequentially. Therefore, silanol groups tend to remain in the condensation product of the organosilicon compound, and hydrophobization does not proceed easily. In addition, three-dimensional condensation reactions do not occur easily, and the molecular weight does not increase easily. On the other hand, under basic conditions, the hydrolysis of alkoxy groups proceeds nucleophilically with hydroxide ions as a catalyst, so the hydrolysis of alkoxy groups in the molecule proceeds simultaneously. Therefore, silanol groups tend to remain in the condensation product of the organosilicon compound, and hydrophobization tends to proceed easily. In addition, three-dimensional condensation reactions tend to occur easily, and the molecular weight tends to increase easily. As a result, large organosilicon polymer particles can be formed in an aqueous medium.

[0155] And, when the hydrophobicity of the organosilicon polymer is high, the stability in the aqueous medium is low, and it is easy to migrate to the core particle. As a result, the surface of the obtained toner particle can be uneven, so it is preferable to carry out the condensation process under basic conditions. In addition, when the condensation process is carried out under basic conditions, the molecular weight of the organosilicon polymer tends to be high, so it is possible to reduce the amount of organosilicon compound dissolved in the aqueous medium. Therefore, it is possible to reduce the organosilicon compound in the wastewater, which is also preferable from the viewpoint of reducing the load on the wastewater treatment.

[0156] Specifically, the pH of the aqueous medium in the condensation step is preferably from 7.5 to 12.0, more preferably from 8.0 to 11.0 The pH in the condensation step can be controlled with a known acid or base.

[0157] Examples of acids for adjusting the pH include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, boric acid, hydrofluoric acid, hydrobromic acid, permanganic acid, thiocyanic acid, phosphonic acid, phosphoric acid, diphosphoric acid, hexafluorophosphoric acid, tetrafluoroboric acid, and tripolyphosphoric acid; inorganic acids such as aspartic acid, hydrochloric acid, sulfuric acid, nitric acid, boric acid, hydrofluoric acid, hydrobromic acid, permanganic acid, thiocyanic acid, phosphonic acid, phosphoric acid, diphosphoric acid, hexafluorophosphoric acid, tetrafluoroboric acid, and tripolyphosphoric acid; and organic acids such as aspartic acid, o-aminobenzoic acid, p-aminobenzoic acid, isonicotinic acid, oxaloacetic acid, citric acid, 2-glyceric acid, glutamic acid, cyanoacetic acid, oxalic acid, trichloroacetic acid, o-nitrobenzoic acid, nitroacetic acid, picric acid, picolinic acid, pyruvic acid, fumaric acid, fluoroacetic acid, bromoacetic acid, o-bromobenzoic acid, maleic acid, and malonic acid. These acids can be used without any particular limitation. These acids may be used alone or in combination of two or more.

[0158] Examples of bases for adjusting pH include alkali metals such as lithium, sodium, and potassium, and their aqueous solutions, alkali metal salts and their aqueous solutions, alkaline earth metals such as calcium and magnesium, and their aqueous solutions, alkaline earth metal salts, ammonia, and amines including urea. More specifically, examples include an aqueous solution of lithium hydroxide, an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, an aqueous solution of calcium hydroxide, an aqueous solution of magnesium hydroxide, an aqueous solution of lithium carbonate, an aqueous solution of sodium carbonate, an aqueous solution of potassium carbonate, an aqueous solution of ammonia, and urea. These bases can be used without any particular restrictions. In addition, these bases may be used alone or in combination of two or more.

[0159] Furthermore, if necessary, external additives such as inorganic fine particles are added to the surface of the toner particles for external addition treatment. Examples of the external addition treatment method include a method in which toner particles and various known external additives are mixed in predetermined amounts and stirred and mixed using a mixing device such as a double con mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, a Mechano Hybrid (manufactured by Nippon Coke and Engineering Co., Ltd.), or a Nobilta (manufactured by Hosokawa Micron Corporation).

[0160] The methods for measuring various physical properties of the toner and raw materials are described below.

[0161] <Method for measuring Qi and Qh in core particles> Qi and Qh in the core particles are measured using a DSC Q1000 (manufactured by TA Instruments) under the following conditions. Heating rate: 10℃ / min Measurement start temperature: 20℃ End of measurement temperature: 180℃ The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction.

[0162] Specifically, about 5 mg of a sample is weighed out and placed in an aluminum pan, and differential scanning calorimetry is performed using an empty aluminum pan as a reference. The endothermic heat Qi can be calculated from the integral value (J / g) of the endothermic peak derived from the wax obtained by the measurement.

[0163] When the endothermic peak derived from the wax does not overlap with the endothermic peak of other raw materials (e.g., crystalline resin), the endothermic amount of the obtained endothermic peak is treated as the endothermic amount of the maximum endothermic peak derived from the wax. When the endothermic peak of the wax overlaps with the endothermic peak of other raw materials (e.g., crystalline resin), it is necessary to subtract the endothermic amount of the other raw materials from the endothermic amount of the obtained endothermic peak.

[0164] The endothermic heat amount derived from other raw materials can be obtained as follows. The core particles are subjected to Soxhlet extraction with a hexane solvent to dissolve the wax in the core particles in hexane. The remaining toner particles after the hexane extraction are subjected to DSC measurement in the same manner to measure the endothermic heat amount of the endothermic peak.

[0165] Qh is determined by treating the core particles with hexane and then performing DSC measurement. 100 mg of core particles are weighed out and 30 mL of hexane is added. After shaking for 5 seconds, the mixture is filtered by suction. The hexane-treated particles on the filter are dried under reduced pressure for 2 hours, then collected and similarly subjected to DSC measurement. The endothermic amount of the endothermic peak derived from the wax obtained in this manner is designated as Qh (J / g).

[0166] In the case of core particles of the present invention, which have been subjected to hot air treatment and have a large amount of wax near the surface, the surface is highly hydrophobic and the core particles are easily dispersed in hexane when hexane is added. On the other hand, core particles formed by polymerization or aggregation in an aqueous medium, or core particles formed by a pulverization method that have not been subjected to hot air treatment or are insufficient, have extremely low wettability with hexane, so that the core particles may not disperse in hexane and may aggregate. In such cases, the aggregated core particles are collected by suction filtration and then Qh is measured by DSC measurement.

[0167] From the Qi and Qh thus obtained, Qi-Qh and (Qi-Qh) / Qi are calculated. For toner particles, Qi-Qh and (Qi-Qh) / Qi can be calculated in the same manner as above.

[0168] <Method of confirming the partial structure represented by formula (T3)> The partial structure represented by formula (T3) in the organosilicon polymer contained in the toner particles is confirmed by the following method.

[0169] The presence or absence of an alkyl group, a phenyl group, or an alkylamino group represented by R in formula (T3) is as follows: 13 The detailed structure of formula (T3) was confirmed by C-NMR.1 H-NMR, 13 C-NMR and 29 The measurement was confirmed by Si-NMR. The equipment and measurement conditions used are as follows:

[0170] (Measurement conditions) Equipment: BRUKER AVANCE III 500 Probe: 4mm MAS BB / 1H Measurement temperature: room temperature Sample rotation speed: 6kHz Sample: 150 mg of the measurement sample (THF insoluble portion of toner particles for NMR measurement) was placed in a 4 mm diameter container. was placed in a sample tube.

[0171] Using this method, the presence or absence of an alkyl group, a phenyl group, or an alkylamino group represented by R in formula (T3) was confirmed. If a signal was confirmed, the structure of formula (T3) was deemed to be "present."

[0172] ( 13 C-NMR (solid state) measurement conditions Measurement nuclear frequency: 125.77MHz Reference substance: Glycine (external standard: 176.03ppm) Observation width: 37.88kHz Measurement method: CP / MAS Contact time: 1.75ms Repeat time: 4s Number of times accumulated: 2048 LB value: 50Hz

[0173] ( 29 Si-NMR (solid state) measurement method (Measurement conditions) Equipment: BRUKER AVANCE III 500 Probe: 4mm MAS BB / 1H Measurement temperature: room temperature Sample rotation speed: 6kHz Sample: 150 mg of the measurement sample (THF insoluble portion of toner particles for NMR measurement) was placed in a 4 mm diameter container. Place in a sample tube. Measured nuclear frequency: 99.36 MHz Reference substance: DSS (external standard: 1.534 ppm) Observation width: 29.76 kHz Measurement method: DD / MAS, CP / MAS 29Si 90° pulse width: 4.00 μs @ -1 dB Contact time: 1.75 ms to 10 ms Repetition time: 30 s (DD / MAS), 10 s (CP / MAS) Number of integrations: 2048 times LB value: 50 Hz

[0174] <In the organosilicon polymer contained in the toner particles, the partial structure (T3 structure) represented by the formula (T3) and the O bonded to silicon 1 / 2 >Calculation method of the ratio of the structure (SX2 structure) in which the number of is 2.0 <Confirmation and quantification methods of T3 structure, X1 structure, X2 structure, X3 structure, X4 structure> The partial structures of T3, X1, X2, X3 and X4 are 1 H-NMR, 13 C-NMR and 29 Si-NMR can be confirmed by

[0175] Of the THF-insoluble matter of the toner particles 29 After Si-NMR measurement of the toner particles, a plurality of silane components with different substituents and bonding groups in the toner particles are curve-fitted, and the O bonded to silicon represented by the following general formula (X4) 1 / 2 The X4 structure in which the number of is 4.0, the O bonded to silicon represented by the following general formula (X3) 1 / 2 The X3 structure in which the number of is 3.0, the O bonded to silicon represented by the following formula (X2) 1 / 2 The X2 structure in which the number of is 2.0, the O bonded to silicon represented by the following formula (X1) 1 / 2 The X1 structure in which the number of is 1.0, and the T unit structure represented by the formula (T3) are peak-separated, and the mol% of each component is calculated from the area ratio of each peak

[0176]

Chemical formula

[0177] [ka] (Rg and Rh in formula (X2) are silicon-bonded organic groups, halogen atoms, hydroxyl groups, or alkoxy groups.)

[0178] [ka] (Rf in formula (X3) is a silicon-bonded organic group, a halogen atom, a hydroxyl group, or an alkoxy group).

[0179] [ka]

[0180] For curve fitting, EXcalibur for Windows (product name) version 4.2 (EX series), software for JNM-EX400 manufactured by JEOL Ltd., is used. Click "1D Pro" from the menu icon to load the measurement data. Next, select "Curve fitting function" from "Command" on the menu bar to perform curve fitting. An example is shown in Figure 2. Peak division is performed so that the peak of the composite peak difference (a), which is the difference between the composite peak (b) and the measurement result (d), is the smallest.

[0181] Calculate the areas of the X1 structure, X2 structure, X3 structure, and X4 structure, and then calculate SX1, SX2, SX3, and SX4 using the following formulas.

[0182] In the present invention, the silane monomer is identified by its chemical shift value, and the toner particles are 29In the Si-NMR measurement, the total peak area of ​​the organosilicon polymer was determined as the sum of the areas of the X1 structure, the X2 structure, the X3 structure and the X4 structure, which are the total peak areas excluding the monomer components. SX1+SX2+SX3+SX4=1.00 SX1 = {Area of ​​X1 structure / (Area of ​​X1 structure + Area of ​​X2 structure + Area of ​​X3 structure + Area of ​​X4 structure)} SX2 = {area of ​​X2 structure / (area of ​​X1 structure + area of ​​X2 structure + area of ​​X3 structure + area of ​​X4 structure)} SX3 = {Area of ​​X3 structure / (Area of ​​X1 structure + Area of ​​X2 structure + Area of ​​X3 structure + Area of ​​X4 structure)} SX4 = {Area of ​​X4 structure / (Area of ​​X1 structure + Area of ​​X2 structure + Area of ​​X3 structure + Area of ​​X4 structure)} ST3 = {area of ​​T3 structure / (area of ​​X1 structure + area of ​​X2 structure + area of ​​X3 structure + area of ​​X4 structure)}

[0183] The chemical shift values ​​of silicon in the X1, X2, X3 and X4 structures are shown below. An example of X1 structure (Ri=Rj=-OC2H5, Rk=-CH3): -47ppm An example of X2 structure (Rg = -OC2H5, Rh = -CH3): -56 ppm An example of X3 structure (Rf=-CH3): -65ppm

[0184] The chemical shift values ​​of silicon in the presence of the X4 structure are shown below. X4 structure: -108ppm

[0185] <Method for separating organosilicon polymer contained in toner particles> To obtain the THF-insoluble organosilicon polymer from the toner particles, the toner particles are first eluted with a strong acid, and the remaining organosilicon polymer is dried and solidified. Then, THF is added to obtain the THF-insoluble fraction.

[0186] <Method for measuring the concentration of silicon element present on the toner particle surface> In the present invention, the silicon element concentration (atomic %) relative to the total concentration (dC+dO+dSi) of the carbon element concentration dC, oxygen element concentration dO, and silicon element concentration dSi present on the toner particle surface was calculated by performing a surface composition analysis by ESCA (X-ray photoelectron spectroscopy analysis).

[0187] In the present invention, the ESCA apparatus and measurement conditions are as follows. Equipment used: ULVAC-PHI Quantum2000 X-ray photoelectron spectrometer measurement conditions: X-ray source Al Kα X-ray: 100μm 25W 15kV Raster: 300μm x 200μm PassEnergy:58.70eV StepSize:0.125eV Neutralization electron gun: 20μA, 1V Ar ion gun: 7mA, 10V Sweep number: Si 15 times, C 10 times, O 5 times

[0188] In the present invention, the surface atomic concentration (atomic %) was calculated from the measured peak intensity of each element using a relative sensitivity factor provided by PHI.

[0189] <Method for measuring the number-average diameter of primary particles of inorganic fine powder> The number-average diameter of the primary particles of the inorganic fine particles is measured using a Hitachi ultra-high resolution field emission scanning electron microscope (FE-SEM) S-4800 (Hitachi High-Technologies Corporation).

[0190] The measurement is carried out on the toner after the inorganic fine particles are mixed therein.

[0191] The photograph is taken at a magnification of 50,000 times, and the photograph is then enlarged by 2 times. From the obtained FE-SEM photograph, the maximum diameter (long axis diameter) a and the minimum diameter (short axis diameter) b of the inorganic microparticles are measured, and (a+b) / 2 is defined as the particle diameter of the particle. The particle diameters of 100 randomly selected inorganic microparticles are measured and the arithmetic average is calculated, which is defined as the number-average diameter of the primary particles of the inorganic micropowder.

[0192] <Method for measuring coverage of inorganic oxide fine particles> The coverage rate of inorganic oxide microparticles is calculated by analyzing surface images of toner particles taken with a Hitachi ultra-high resolution field emission scanning electron microscope (FE-SEM; S-4800, Hitachi High-Technologies Corporation) using image analysis software (Image-Pro Plus ver.5.0, Nippon Roper Co., Ltd.).

[0193] The inorganic oxide fine particles present on the surface of the toner core particles are observed by the above SEM device.

[0194] When making an observation, it is advisable to select a location where the surface of the core particle is as flat as possible.

[0195] The image of only the inorganic oxide microparticles on the core particle surface is binarized, and the ratio of the area of ​​the inorganic oxide microparticles to the area of ​​the core particle surface is calculated. The same operation is performed for 10 core particles, and the arithmetic mean value is calculated.

[0196] <Molecular weight measurement of THF-soluble resin> The weight average molecular weight (Mw) of the THF-soluble portion of the resin is measured by gel permeation chromatography (GPC) as follows.

[0197] First, the sample is dissolved in tetrahydrofuran (THF) at room temperature for 24 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of components soluble in THF is approximately 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: HLC8120 GPC (detector: RI) (Tosoh Corporation) Column: Shodex KF-801, 802, 803, 804, 805, 806, 807 (Showa Denko) Eluent: tetrahydrofuran (THF) Flow rate: 1.0ml / min Oven temperature: 40.0℃ Sample injection volume: 0.10 ml

[0198] In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using standard polystyrene resins (e.g., trade names "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500" manufactured by Tosoh Corporation) is used.

[0199] <Method for measuring the softening point Tm of binder resin> The softening point of the binder resin is measured using a constant load extrusion type capillary rheometer "Flow characteristic evaluation device Flow Tester CFT-500D" (manufactured by Shimadzu Corporation) according to the manual that comes with the device. With this device, a constant load is applied from above the measurement sample by a piston while the measurement sample filled in a cylinder is heated and melted, and the molten measurement sample is extruded from a die at the bottom of the cylinder, and a flow curve showing the relationship between the piston descent amount and temperature can be obtained.

[0200] The "melting temperature in the 1 / 2 method" described in the manual attached to the "Flow characteristic evaluation device Flow Tester CFT-500D" is taken as the softening point. The melting temperature in the 1 / 2 method is calculated as follows. First, half the difference between the amount of piston descent Smax at the time when the outflow ends and the amount of piston descent Smin at the time when the outflow starts is calculated (this is taken as X; X=(Smax-Smin) / 2). The temperature of the flow curve when the amount of piston descent on the flow curve is X is the melting temperature in the 1 / 2 method.

[0201] The measurement sample is prepared by compressing approximately 1.0 g of resin at approximately 10 MPa for approximately 60 seconds using a tablet molding machine (e.g., NT-100H, manufactured by NPA Systems) in an environment of 25°C to form a cylindrical shape with a diameter of approximately 8 mm.

[0202] The measurement conditions for the CFT-500D are as follows. Test mode: Temperature rise method Starting temperature: 50℃ Achieved temperature: 200℃ Measurement interval: 1.0℃ Heating rate: 4.0℃ / min Piston cross-sectional area: 1.000cm 2 Test load (piston load): 10.0kgf (0.9807MPa) Preheat time: 300 seconds Die hole diameter: 1.0mm Die length: 1.0mm

[0203] <Acid value measurement method> The acid value is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of a sample. The acid value of the polyester resin in the present invention is measured in accordance with JIS K 0070-1992, and specifically, is measured according to the following procedure.

[0204] (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 mL of ethyl alcohol (95% by volume), and add ion-exchanged water to make 100 mL to obtain a phenolphthalein solution.

[0205] Dissolve 7 g of special grade potassium hydroxide in 5 mL of water, and add ethyl alcohol (95% by volume) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave for 3 days, then filter to obtain a potassium hydroxide solution. Store the obtained potassium hydroxide solution in an alkali-resistant container. The factor of the potassium hydroxide solution is calculated by placing 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding several drops of the phenolphthalein solution, and titrating with the potassium hydroxide solution, from the amount of the potassium hydroxide solution required for neutralization. The 0.1 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998.

[0206] (2) Operation (A) Main Test 2.0 g of the crushed polyester resin sample is accurately weighed into a 200 mL Erlenmeyer flask, and 100 mL of a toluene / ethanol (2:1) mixed solution is added and dissolved over 5 hours. Next, several drops of the phenolphthalein solution are added as an indicator, and titration is performed using the potassium hydroxide solution. The end point of the titration is when the light red color of the indicator continues for about 30 seconds. (B) Blank test The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene / ethanol (2:1) mixed solution is used).

[0207] (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CB) × f × 5.61] / S Here, A is the acid value (mgKOH / g), B is the amount of potassium hydroxide solution added for the blank test (mL), C is the amount of potassium hydroxide solution added for the main test (mL), f is the factor of the potassium hydroxide solution, and S is the mass of the sample (g).

[0208] <Measurement of BET specific surface area of ​​inorganic oxide particles and external additives (inorganic fine particles)> The BET specific surface area of ​​inorganic fine particles is measured in accordance with JIS Z8830 (2001). The specific measurement method is as follows.

[0209] The measurement device used is the "Automatic Surface Area / Porosity Distribution Measurement Device TriStar3000 (manufactured by Shimadzu Corporation)" which employs the gas adsorption method based on the constant volume method. The measurement conditions are set and the measurement data is analyzed using the dedicated software "TriStar3000 Version 4.00" that comes with this device. A vacuum pump, nitrogen gas piping, and helium gas piping are connected to this device. The value calculated by the BET multipoint method using nitrogen gas as the adsorption gas is regarded as the BET specific surface area of ​​the inorganic microparticles in this invention.

[0210] The BET specific surface area is calculated as follows.

[0211] First, nitrogen gas is adsorbed onto the inorganic fine particles, and the equilibrium pressure P (Pa) in the sample cell and the nitrogen adsorption amount Va (mol / g) of the external additive are measured. Then, an adsorption isotherm is obtained with the relative pressure Pr, which is the equilibrium pressure P (Pa) in the sample cell divided by the saturated vapor pressure Po (Pa) of nitrogen, on the horizontal axis and the nitrogen adsorption amount Va (mol / g) on ​​the vertical axis. Next, the monolayer adsorption amount Vm (mol / g), which is the adsorption amount required to form a monolayer on the surface of the external additive, is calculated using the following BET formula. Pr / Va(1-Pr)=1 / (Vm×C)+(C-1)×Pr / (Vm×C)

[0212] Here, C is a BET parameter, which is a variable that varies depending on the type of measurement sample, the type of adsorption gas, and the adsorption temperature.

[0213] The BET formula can be interpreted as a line with a slope of (C-1) / (Vm×C) and an intercept of 1 / (Vm×C) when the X-axis is Pr and the Y-axis is Pr / Va(1-Pr). This line is called a BET plot. Slope of the line = (C-1) / (Vm×C) Line intercept = 1 / (Vm×C)

[0214] If you plot the measured values ​​of Pr and Pr / Va(1-Pr) on a graph and draw a line using the least squares method, you can calculate the slope and intercept of the line. By substituting these values ​​into the above formula and solving the resulting simultaneous equations, you can calculate Vm and C.

[0215] Furthermore, the calculated Vm and the molecular occupancy cross section of the nitrogen molecule (0.162 nm 2 ) and the BET specific surface area S (m 2 / g) is calculated. S = Vm × N × 0.162 × 10 -18

[0216] where N is Avogadro's number (mol -1 ).

[0217] Measurements using this device should be performed in accordance with the "TriStar3000 Instruction Manual V4.0" that comes with the device, and specifically, the measurements should be performed in the following order.

[0218] Accurately weigh the mass of a tared glass sample cell (stem diameter 3 / 8 inch, volume approximately 5 ml) that has been thoroughly washed and dried. Then, use a funnel to place approximately 0.1 g of the additive into the sample cell.

[0219] The sample cell containing the inorganic fine particles is set in a pretreatment device VacuPrep 061 (Shimadzu Corporation) connected to a vacuum pump and nitrogen gas piping, and vacuum degassing is continued for about 10 hours at 23°C. During vacuum degassing, the valve is adjusted to gradually degas the inorganic fine particles so that they are not sucked into the vacuum pump. The pressure in the sample cell gradually decreases with degassing, and finally reaches about 0.4 Pa (about 3 mTorr). After completion of vacuum degassing, nitrogen gas is gradually injected into the sample cell to return the sample cell to atmospheric pressure, and the sample cell is removed from the pretreatment device. The mass of this sample cell is then precisely weighed, and the exact mass of the external additive is calculated from the difference with the tare mass. During this time, the sample cell is covered with a rubber stopper during weighing to prevent the external additive in the sample cell from being contaminated by moisture in the air.

[0220] Next, a special "isothermal jacket" is attached to the stem of the sample cell containing the inorganic fine particles. A special filler rod is then inserted into the sample cell, and the sample cell is set in the analysis port of the device. The isothermal jacket is a cylindrical member with a porous inner surface and an impermeable outer surface that can suck up liquid nitrogen to a certain level by capillary action.

[0221] Next, the free space of the sample cell including the connecting device is measured. The free space is calculated by measuring the volume of the sample cell at 23°C using helium gas, then measuring the volume of the sample cell after cooling it with liquid nitrogen, again using helium gas, and converting it from the difference between these volumes. The saturated vapor pressure Po (Pa) of nitrogen is also measured automatically using the Po tube built into this device.

[0222] Next, the sample cell is evacuated and then cooled with liquid nitrogen while continuing the vacuum evacuation. Nitrogen gas is then gradually introduced into the sample cell to adsorb nitrogen molecules to the inorganic fine particles. At this time, the equilibrium pressure P (Pa) is measured at any time to obtain the adsorption isotherm, which is then converted into a BET plot. The relative pressure Pr points at which data is collected are set to 0.05, 0.10, 0.15, 0.20, 0.25, and 0.30, for a total of six points. A straight line is drawn for the obtained measurement data by the least squares method, and Vm is calculated from the slope and intercept of the straight line. Furthermore, the BET specific surface area of ​​the inorganic fine particles is calculated using this Vm value as described above.

[0223] <Measurement of weight average particle size (D4) of toner particles> The weight-average particle diameter (D4) of the toner particles is measured with an effective measurement channel count of 25,000 channels using a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube, and the accompanying dedicated software for setting measurement conditions and analyzing measurement data, "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.), and the measurement data is analyzed and calculated.

[0224] The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in deionized water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).

[0225] Before carrying out the measurements and analyses, the dedicated software is set up as follows.

[0226] In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement.

[0227] In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.

[0228] The specific measurement methods are as follows (1) to (7). (1) Pour about 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) Approximately 30 ml of the aqueous electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and approximately 0.3 ml of a solution prepared by diluting "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) three times by mass with deionized water is added as a dispersant. (3) A specified amount of deionized water is placed in the water tank of an ultrasonic disperser "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and approximately 2 ml of the Conaminon N is added to this water tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) In the round-bottom beaker (1) placed in the sample stand, the electrolytic solution (5) in which the toner is dispersed is dropped using a pipette to adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the weight-average particle size (D4). EXAMPLES

[0229] The present invention will be described in more detail with reference to the following examples. However, these examples are not intended to limit the present invention. In the following formulations, "parts" are all by weight unless otherwise specified.

[0230] <Production Example 1 of Strontium Titanate Microparticles> Metatitanic acid obtained by the sulfuric acid method was deironized and bleached, then sodium hydroxide solution was added to adjust the pH to 9.0, desulfurized, neutralized to pH 5.8 with hydrochloric acid, filtered and washed with water. Water was added to the washed cake to make a slurry of 1.5 mol / L in terms of TiO2, and hydrochloric acid was added to adjust the pH to 1.5, followed by peptization.

[0231] The desulfurized and peptized metatitanic acid was collected as TiO2 and put into a 3L reaction vessel. A strontium chloride aqueous solution was added to the peptized metatitanic acid slurry so that the SrO / TiO2 molar ratio was 1.15, and then the TiO2 concentration was adjusted to 0.8 mol / L. Next, the mixture was heated to 90°C while stirring and mixing, and 444mL of a 10 mol / L sodium hydroxide aqueous solution was added over 45 minutes while microbubbling nitrogen gas at 600ml / min, and then the mixture was stirred at 95°C for 1 hour while microbubbling nitrogen gas at 400ml / min.

[0232] The reaction slurry was then stirred while flowing 10°C cooling water through the jacket of the reaction vessel to rapidly cool it to 15°C, and hydrochloric acid was added until the pH reached 2.0, and stirring was continued for 1 hour. The resulting precipitate was washed by decantation, and then 5.0 mass% of sodium stearate based on the solid content was dissolved in water to form an aqueous solution, which was added and stirred for 2 hours, after which hydrochloric acid was added to adjust the pH to 6.5, and stirring was continued for 1 hour to precipitate stearic acid on the surface of strontium titanate.

[0233] Next, after filtering and washing, the resulting cake was left in the air at 120°C for 10 hours, and then crushed in a jet mill until no agglomerates remained, yielding strontium titanate microparticles (inorganic microparticles 1). In powder X-ray diffraction measurement, inorganic microparticles 1 showed a diffraction peak of strontium titanate.

[0234] <Production Examples 2 to 6 of Strontium Titanate Microparticles> Strontium titanate microparticles (inorganic microparticles 2 to 6) were obtained by carrying out the same production as in Production Example 1 of strontium titanate microparticles, except that the dropwise addition time of the 10 mol / L sodium hydroxide aqueous solution was changed.

[0235] <Manufacturing example of silica fine particles> A double-tube hydrocarbon-oxygen mixed burner capable of forming an inner flame and an outer flame was used as the combustion furnace. A two-fluid nozzle for injecting slurry was installed in the center of the burner, and the silicon compound raw material was introduced. Combustible hydrocarbon-oxygen gas was injected from around the two-fluid nozzle to form the inner and outer flames, which were reducing atmospheres.

[0236] The atmosphere, temperature, flame length, etc. were adjusted by controlling the amount and flow rate of the combustible gas and oxygen. Silica fine particles were formed from the silicon compound in the flame, and were further fused until the desired particle size was reached. After cooling, the silica fine particles were collected using a bag filter or the like to obtain silica fine particles. 100 parts of the obtained silica fine particles were surface-treated with 4 parts of hexamethyldisilazane to obtain silica fine particles (inorganic fine particles 7 to 10). The physical properties are shown in Table 1.

[0237] <Production example of titanium oxide fine particles> The titanium oxide hydrous slurry obtained by thermal hydrolysis of an aqueous solution of titanyl sulfate was neutralized to pH 7 with aqueous ammonia, filtered, and washed to obtain a cake. The titanium oxide in the cake was peptized with hydrochloric acid to obtain an anatase-type titania sol. The average primary particle size of this sol was 7 nm.

[0238] In addition, ilmenite ore containing 50% by mass of TiO2 equivalent was used as the starting material, and this raw material was dried at 150°C for 2 hours, and then sulfuric acid was added to dissolve it, to obtain a TiOSO4 aqueous solution. This was concentrated, and 4.0 parts of the anatase-type titania sol was added as a seed to 100 parts of TiO2 equivalent, and hydrolysis was performed at 120°C to obtain a slurry of TiO(OH)2 containing impurities.

[0239] This slurry was repeatedly washed with water at pH 5-6 to thoroughly remove sulfuric acid, FeSO4, and impurities, and a high-purity metatitanic acid [TiO(OH)2] slurry was obtained.

[0240] The metatitanic acid was heat-treated at 270°C for 6 hours, and then thoroughly crushed to obtain a powder with a BET specific surface area of ​​50 m 2Titanium oxide fine particles having an anatase type crystallinity and a number-average particle size of 50 nm were obtained.

[0241] Next, 5.0% by mass of n-octyltriethoxysilane was dissolved in water and added to the anatase type titanium oxide fine particles, and the mixture was stirred for 2 hours. Then, hydrochloric acid was added to adjust the pH to 6.5, and the mixture was stirred for 1 hour.

[0242] Next, after filtration and washing, the resulting cake was dried in air at 120° C. for 10 hours and then crushed using a jet mill until no agglomerates of titanium fine particles remained, yielding titanium oxide fine particles (inorganic fine particles 11). The physical properties are shown in Table 1.

[0243] [Table 1]

[0244] <Examples of binder resin production> (Polyester Resin Production Example 1) Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane: 59.0 parts (0.15 moles; 80.0 mol% based on the total number of moles of polyhydric alcohol) Polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: 13.6 parts (0.04 moles; 20.0 mol% based on the total number of moles of polyhydric alcohol) Terephthalic acid: 20.8 parts (0.13 moles; 80.0 mol% based on the total number of moles of polycarboxylic acids) Trimellitic anhydride: 6.6 parts (0.03 moles; 20.0 mol% based on the total number of moles of polycarboxylic acids) The above materials were put into a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Then, 1.5 parts of tin 2-ethylhexanoate (esterification catalyst) was added as a catalyst for 100 parts of total monomer. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised while stirring, and the reaction was carried out for 3 hours at a temperature of 200°C while stirring.

[0245] Furthermore, the pressure in the reaction tank was reduced to 8.3 kPa and maintained for 1 hour, after which it was cooled to 180°C and reacted as is. After confirming that the softening point measured according to ASTM D36-86 reached 90°C, the temperature was reduced to stop the reaction, thereby obtaining polyester resin L. The resulting polyester resin L had a softening point (Tm) of 97°C and an acid value of 7 mgKOH / g.

[0246] <Production Example 2 of Amorphous Polyester> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane: 73.4 parts (0.19 moles; 100.0 mol% based on the total number of moles of polyhydric alcohol) Terephthalic acid: 11.6 parts (0.07 moles; 82.0 mol% based on the total number of moles of polycarboxylic acids) Adipic acid: 6.8 parts (0.05 moles; 14.0 mol% based on the total number of moles of polycarboxylic acids) Tin di(2-ethylhexyl)ate: 0.8 parts The above materials were weighed and put into a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 3 hours at a temperature of 200°C with stirring.

[0247] Furthermore, the pressure inside the reaction vessel was reduced to 8.3 kPa and maintained for 1 hour, after which it was cooled to 180° C. and returned to atmospheric pressure (first reaction step). Trimellitic anhydride: 8.2 parts (0.04 moles; 6.0 mol% based on the total number of moles of polycarboxylic acids) tert-Butylcatechol (polymerization inhibitor): 0.1 parts Thereafter, the above materials were added, the pressure in the reaction vessel was reduced to 8.3 kPa, and the reaction was carried out for 12 hours while maintaining the temperature at 145° C., and the reaction was stopped by reducing the temperature (second reaction step), thereby obtaining amorphous polyester resin H. The obtained amorphous polyester resin H had a softening point of 150° C. and an acid value of 10 mg / KOH.

[0248] (Example of synthesis of vinyl amorphous resin) 50 parts of xylene was charged into an autoclave, and after replacing with nitrogen, the temperature was raised to 185°C in a sealed state with stirring. A mixed solution of 97 parts of styrene, 3 parts of n-butyl acrylate, 3 parts of di-t-butyl peroxide, and 20 parts of xylene was continuously dropped for 4 hours while controlling the temperature inside the autoclave at 170°C, and polymerization was carried out. The same temperature was maintained for another 1 hour to complete the polymerization, and the solvent was removed to obtain a vinyl-based amorphous resin. The weight average molecular weight (Mw) of the obtained resin was 5000, and the softening point (Tm) was 108°C.

[0249] <Production example of wax dispersant> ·Low molecular weight polypropylene (melting point 80℃): 15.0 parts (0.03 moles; 3.0 mol% based on the total moles of constituent monomers) Xylene: 25.0 parts The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised to 175° C. while stirring. ·styrene: 64.5 parts (0.62 moles; 76.0 mol% based on the total moles of constituent monomers) Cyclohexyl methacrylate: 9.6 parts (0.06 moles; 7.0 mol% based on the total moles of constituent monomers) Butyl acrylate: 11.5 parts (0.09 moles; 11.0 mol% based on the total moles of constituent monomers) Methyl methacrylate: 2.4 parts (0.02 moles; 3.0 mol% based on the total moles of constituent monomers) Xylene: 10.0 parts Di-t-butylperoxyhexahydroterephthalate: 0.5 parts The above material was then added dropwise over 2.5 hours and stirred for another 40 minutes. The solvent was then distilled off to obtain a vinyl resin in which a styrene-acrylic polymer was grafted onto polypropylene. The vinyl resin thus obtained had a peak molecular weight Mp of 7000 and a softening point of 120°C.

[0250] <Production example of crystalline polyester> 1,6-Hexanediol: 34.5 parts (0.29 moles; 100.0 mol% based on the total number of moles of polyhydric alcohol) Dodecanedioic acid: 65.5 parts (0.28 moles; 100.0 mol% based on the total number of moles of polycarboxylic acids) ·Tin 2-ethylhexanoate: 0.5 parts The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. After replacing the atmosphere in the flask with nitrogen gas, the temperature was gradually raised with stirring, and the reaction was carried out for 2.5 hours at 140°C with stirring.

[0251] Next, the pressure inside the reaction vessel was reduced to 8.3 kPa, and the reaction was carried out for 4 hours while maintaining the temperature at 200°C.

[0252] Thereafter, the pressure in the reaction vessel was reduced to 5 kPa or less, and the mixture was reacted at 200° C. for 3 hours to obtain a crystalline polyester having a melting point of 70° C.

[0253] <Production Example 1 of Core Particles> Polyester resin L 75 parts Polyester resin H 25 parts Crystalline polyester 3 parts Wax Dispersant 3 parts Hydrocarbon wax 7 parts (Fischer-Tropsch wax; maximum endothermic peak temperature 90℃) CI Pigment Blue 15:3 5 parts The above materials were mixed in a Henschel mixer (FM-75, manufactured by Nippon Coke and Engineering Co., Ltd.) at a rotation speed of 20 s -1After mixing for 5 min, the mixture was kneaded at a discharge temperature of 120°C in a twin-screw kneader (PCM-30, Ikegai Corporation) set at a temperature of 110°C. The kneaded mixture was cooled and coarsely crushed to 1 mm or less in a hammer mill to obtain a coarsely crushed product. The coarsely crushed product was finely crushed in a mechanical crusher (T-250, Freund Turbo Corporation). A Faculty F-300 (Hosokawa Micron Corporation) was further used, and the operating conditions were a classifying rotor rotation speed of 130 s -1 , Dispersion rotor speed 120s -1 The mixture was classified to obtain core particles 1.

[0254] <Core particle manufacturing example 2> Core particles 2 were obtained by carrying out the same production process as in Core Particle Production Example 1, except that polyester resin L and polyester resin H were not used and were replaced with 100 parts of an amorphous vinyl resin.

[0255] <Production Example 3 of Core Particles> Core particles 3 were obtained by carrying out production in the same manner as in Core Particle Production Example 1, except that the hydrocarbon wax in Core Particle Production Example 1 was replaced with 5 parts of ester wax (carnauba wax; peak temperature of maximum endothermic peak: 85°C).

[0256] <Core particle production examples 4 to 11> Core particles 4 to 11 were obtained by carrying out the same production process as in Core Particle Production Example 1, except that the parts of the hydrocarbon wax and / or the parts of the wax dispersant were replaced with those shown in Table 2. The physical properties are shown in Table 2.

[0257] [Table 2]

[0258] <Production Example 1 of Core Particles Having Inorganic Oxide Fine Particles Adhered to Their Surfaces Before Heat Treatment> The obtained core particles 1 and inorganic oxide fine particles were mixed in a predetermined amount and mixed in a Henschel mixer FM-10C type (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 30 s. -1The mixture was mixed at 100 parts by weight for a rotation time of 10 minutes to obtain pre-heat-treatment core particles 1. At this time, inorganic oxide fine particles were blended with 100 parts by weight of the core particles. The number of parts of the inorganic oxide fine particles added is shown in Table 3.

[0259] <Production Examples 2 to 32 of Core Particles Having Inorganic Oxide Fine Particles Adhered to Their Surfaces Before Heat Treatment> Pre-heat-treated core particles 2 to 32 were obtained in the same manner as in Pre-heat-treated core particles having inorganic oxide fine particles attached to their surfaces, except that the types and parts of inorganic oxide fine particles used in Pre-heat-treated core particles having inorganic oxide fine particles attached to their surfaces were replaced with those shown in Table 3. Their physical properties are shown in Table 3.

[0260] [Table 3]

[0261] <Production Example 1 of Heat-Treated Core Particles Having Inorganic Oxide Fine Particles Thermally Adhered to Their Surfaces> Next, the pre-heat-treated core particles 1 were heat-treated using the surface treatment device shown in Fig. 1 to obtain heat-treated core particles 1 having inorganic oxide fine particles thermally fixed to the surface. The operating conditions were feed rate = 2 kg / hr, hot air temperature = 160°C, hot air flow rate = 6 m 3 / min., cold air temperature = -5℃, cold air flow rate = 4m 3 / min., Blower air volume = 20m 3 / min., Injection air flow rate = 1m 3 / min.

[0262] <Production Examples 2 to 38 of Heat-Treated Core Particles Having Inorganic Oxide Fine Particles Thermally Adhered to the Surface> Heat-treated core particles 2 to 38 having inorganic oxide fine particles thermally adhered to their surfaces were produced in the same manner as in Production Example 1 of core particles having inorganic oxide fine particles thermally adhered thereto, except that the core particles before heat treatment and the hot air temperature were changed to those shown in Table 4.

[0263] [Table 4]

[0264] <Production Example of Dispersion Stabilizer Aqueous Solution 1> ·Na3PO4 aqueous solution (0.1 mol / L) 100.0 parts 70.0 parts of ion-exchanged water HCl aqueous solution (1.0 mol / L) 2.4 parts The above materials were charged into a reaction vessel equipped with a reflux condenser and a thermometer. Next, the inside of the reaction vessel was kept at 60° C. while stirring at 12,000 rpm using a high-speed stirring device TK-Homomixer. CaCl2 aqueous solution (1.0 mol / L) 85.0 parts The above materials were gradually added thereto to obtain an aqueous dispersion stabilizer solution 1 containing fine poorly water-soluble dispersion stabilizer Ca3(PO4)2.

[0265] <Production Example of Silane Compound Hydrolyzed Solution 1> Methyltriethoxysilane 50.0 parts 50.0 parts ion-exchanged water The above materials were placed in a reaction vessel equipped with a stirrer, the pH was adjusted to 3.0 with 10% by mass hydrochloric acid, and hydrolysis was carried out with stirring to obtain a silane compound hydrolyzed liquid 1. Completion of hydrolysis was confirmed when the liquid, which was initially separated into two phases, became a single phase.

[0266] <Production Examples of Silane Compound Hydrolyzed Solutions 2 to 5> Silane compound hydrolyzed solutions 2 to 5 were obtained by carrying out the reaction in the same manner as in the production example of silane compound hydrolyzed solution 1, except that the silane compounds were changed to those shown in Table 5.

[0267] [Table 5]

[0268] <Production example of surfactant aqueous solution 1> Polyoxyethylene styrenated phenyl ether 10.0 parts Ion-exchanged water 90.0 parts The above materials were placed in a reaction vessel equipped with a stirrer and dissolved under stirring to obtain an aqueous surfactant solution 1.

[0269] <Toner Production Example 1> (Dispersion process in aqueous medium) Heat-treated core particles 1 15.0 parts Dispersion stabilizer aqueous solution 1 100.0 parts The above materials were placed in a reaction vessel equipped with a thermometer. The reaction vessel was kept at 25° C., and the materials were dispersed for 6 minutes at 5000 rpm with a homogenizer (Ultra Turrax T50, manufactured by IKA Japan Co., Ltd.) to obtain heat-treated core particle dispersion liquid 1.

[0270] (condensation process) Heat-treated core particle dispersion 1 100.0 parts Silane compound hydrolysis solution 1 1.8 parts The above materials were put into a reaction vessel equipped with a stirrer and a thermometer. The temperature in the reaction vessel was raised to 70°C while stirring at 200 rpm. The pH was adjusted to 9.0 with 1 mol / L NaOH aqueous solution, and the mixture was stirred for 240 minutes to carry out a condensation reaction. The pH was then adjusted to 1.5 with dilute hydrochloric acid to remove the dispersion stabilizer. After that, the mixture was filtered using Kiriyama filter paper (No. 5C: pore size 1 μm) to separate the particles from the filtrate. The obtained particles were further washed with ion-exchanged water and vacuum-dried at 30°C for 24 hours to obtain toner particles 1 coated with an organosilicon polymer.

[0271] Further, the obtained toner particles 1 (99.5 parts) coated with the organosilicon polymer were subjected to a surface treatment with 5% by mass of polydimethylsiloxane to obtain a toner having a BET specific surface area of ​​100 m 2 0.5 parts of hydrophobic silica particles / g were added, and the mixture was mixed in a Henschel mixer (FM-75, manufactured by Nippon Coke and Engineering Co., Ltd.) at a rotation speed of 30 s -1 The mixture was mixed for 10 minutes at a rotation time to obtain Toner 1 containing Toner Particles 1. The physical properties are shown in Table 6.

[0272] <Toner Production Examples 2 to 43> Toners 2 to 43 were obtained by performing the same production procedure as in Toner Production Example 1, except that the heat-treated core particles, inorganic oxide fine particles, and silane compound hydrolyzate were changed to those shown in Table 6.

[0273] [Table 6]

[0274] <Production Example of Magnetic Core Particle 1> Step 1 (weighing and mixing): Fe2O362.7 parts MnCO329.5 parts Mg(OH)26.8 parts SrCO31.0 parts The ferrite raw materials were weighed so as to obtain the above composition ratio, and then pulverized and mixed for 5 hours in a dry vibration mill using stainless steel beads with a diameter of 1 / 8 inch.

[0275] Step 2 (Pre-firing): The obtained pulverized material was made into pellets of about 1 mm square using a roller compactor. The pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then through a vibrating sieve with 0.5 mm openings to remove fine powder. The pellets were then fired in a burner-type firing furnace at 1000°C for 4 hours in a nitrogen atmosphere (oxygen concentration 0.01% by volume) to produce calcined ferrite. The composition of the calcined ferrite obtained was as follows: (MnO)a(MgO)b(SrO)c(Fe2O3)d In the above formula, a = 0.257, b = 0.117, c = 0.007, d = 0.393

[0276] Step 3 (Crushing): After crushing to about 0.3 mm in a crusher, 30 parts of water were added to 100 parts of calcined ferrite and crushed in a wet ball mill using zirconia beads with a diameter of 1 / 8 inch for 1 hour. The slurry was crushed in a wet ball mill using alumina beads with a diameter of 1 / 16 inch for 4 hours to obtain a ferrite slurry (finely crushed calcined ferrite).

[0277] ·Process 4 (granulation process): To the ferrite slurry, 1.0 part of ammonium polycarboxylate as a dispersant and 2.0 parts of polyvinyl alcohol as a binder were added per 100 parts of calcined ferrite, and the mixture was granulated into spherical particles using a spray dryer (manufacturer: Okawara Kakoki). After adjusting the particle size of the resulting particles, the mixture was heated at 650°C for 2 hours in a rotary kiln to remove the organic components of the dispersant and binder.

[0278] Step 5 (firing): In order to control the firing atmosphere, the material was heated from room temperature to 1300°C in a nitrogen atmosphere (oxygen concentration 1.00% by volume) in an electric furnace over a period of 2 hours, and then fired at 1150°C for 4 hours. The material was then cooled to 60°C over a period of 4 hours, returned from the nitrogen atmosphere to the air, and removed at a temperature of 40°C or less.

[0279] Step 6 (sorting step): After crushing the agglomerated particles, low magnetic particles were removed by magnetic separation, and coarse particles were removed by sieving through a sieve with 250 μm openings to obtain magnetic core particles 1 having a volume distribution standard 50% particle size (D50) of 37.0 μm.

[0280] <Preparation of Coating Resin 1> Cyclohexyl methacrylate monomer 26.8% by mass Methyl methacrylate monomer 0.2% by mass Methyl methacrylate macromonomer 8.4% by mass (A macromonomer with a weight-average molecular weight of 5000 and a methacryloyl group at one end) Toluene 31.3% by mass Methyl ethyl ketone 31.3% by mass Azobisisobutyronitrile 2.0% by mass Of the above materials, cyclohexyl methacrylate, methyl methacrylate, methyl methacrylate macromonomer, toluene, and methyl ethyl ketone were added to a four-necked separable flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer, and nitrogen gas was introduced to create a sufficient nitrogen atmosphere, and then the mixture was heated to 80°C, azobisisobutyronitrile was added, and the mixture was refluxed for 5 hours to polymerize. Hexane was poured into the resulting reaction product to precipitate a copolymer, and the precipitate was filtered and then vacuum dried to obtain coating resin 1. 30 parts of the resulting coating resin 1 were dissolved in 40 parts of toluene and 30 parts of methyl ethyl ketone to obtain polymer solution 1 (solid content 30% by mass).

[0281] <Preparation of coating resin solution 1> Polymer solution 1 (resin solids concentration 30%) 33.3% by mass Toluene 66.4% by mass Carbon black (Regal 330; manufactured by Cabot Corporation) 0.3% by mass (Primary particle size 25 nm, nitrogen adsorption specific surface area 94 m 2 / g, DBP oil absorption 75ml / 100g) These were dispersed for 1 hour using a paint shaker with zirconia beads having a diameter of 0.5 mm. The resulting dispersion was filtered through a 5.0 μm membrane filter to obtain a coating resin solution 1.

[0282] <Magnetic Carrier 1 Manufacturing Example> (Resin coating process): The coating resin solution 1 was added to a vacuum degassing kneader maintained at room temperature so that the resin component was 2.5 parts per 100 parts of the filled core particles 1. After addition, the mixture was stirred at a rotation speed of 30 rpm for 15 minutes, and after a certain amount of the solvent (80 mass%) had evaporated, the mixture was heated to 80°C while mixing under reduced pressure, and the toluene was distilled off over 2 hours, after which it was cooled. The magnetic carrier obtained was separated into low magnetic products by magnetic separation, passed through a sieve with an opening of 70 μm, and then classified with a wind classifier to obtain magnetic carrier 1 having a 50% particle size (D50) of 38.2 μm based on volume distribution.

[0283] <Production Example 1 of Two-Component Developer> Toner 1 (8.0 parts) was added to magnetic carrier 1 (92.0 parts), and mixed in a V-type mixer (V-20, manufactured by Seishin Enterprises) to obtain two-component developer 1.

[0284] <Production Examples of Two-Component Developers 2 to 43> Two-component developers 2 to 43 were obtained by carrying out production in the same manner as in the production example of two-component developer 1, except that the toner was changed as shown in Table 7.

[0285] [Table 7]

[0286] Example 1 [evaluation] [1. Low temperature fixability evaluation] The image forming apparatus was a modified Yanon full-color copier imageRUNNER ADVANCE C5560, and the above-mentioned two-component developer 1 was placed in the cyan developer and / or magenta developer of the image forming apparatus, and the evaluation described below was performed. The modifications were made so that the fixing temperature, process speed, DC voltage VDC of the developer carrier, charging voltage VD of the electrostatic latent image carrier, and laser power could be freely set.

[0287] The image was printed in a normal temperature and humidity (NN) environment (temperature 23°C, relative humidity 50% to 60%) with a toner load of 1.0 mg / cm on the paper. 2 The unfixed image was created so that it had a horizontal band with an image printing ratio of 25% on the trailing edge of the paper feed direction. The evaluation paper was copy paper GF-C300 (A4, basis weight 300.0 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0288] Then, in a low temperature and low humidity (LL) environment (temperature 15°C, relative humidity 15% or less), the process speed was set to 450 mm / sec, and the fixing temperature was increased in increments of 5°C from 120°C, and the lowest temperature at which no offset occurred was defined as the low-temperature fixing temperature. The evaluation results are shown in Table 8.

[0289] (Evaluation Criteria for Low Fixing Temperature) A: Less than 150℃ (Good) B: 150℃ or higher but lower than 160℃ (good). C: 160° C. or higher and lower than 170° C. (This is the level at which the effects of the present invention are obtained). D: 170° C. or higher (a level at which the effects of the present invention are not fully obtained).

[0290] [2. Evaluation of anti-wrapping property] Using the evaluation machine used in the low-temperature fixing property evaluation, the two-component developer 1 was tested in the fixing temperature range. The image was printed in monochrome mode under normal temperature and humidity (NN) environment (temperature 23°C, relative humidity 50% to 60%) with a toner loading amount of 1.0 mg / cm on paper. 2 The paper was adjusted so that the print ratio was 25%, and an unfixed image was created with a margin of 2 mm from the leading edge in the paper feed direction. The evaluation paper was copy paper CS-680 (A4, basis weight 68.0 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0291] Then, in a high temperature and high humidity (HH) environment (temperature 30°C, relative humidity 80%), the process speed was set to 300 mm / sec, and the fixing temperature was increased in increments of 5°C from 140°C. The upper limit temperature at which the fixing paper did not wrap around was determined as the anti-wrapping temperature.

[0292] The anti-wrapping property was ranked according to the following criteria. The evaluation results are shown in Table 8.

[0293] (Evaluation Criteria for Anti-Wrapping Property) A: 175℃ or higher (very good) B: 165℃ or higher but lower than 175℃ (good). C: 155°C or higher and lower than 165°C (this is the level at which the effects of the present invention are obtained). D: Less than 155°C (a level at which the effects of the present invention are not fully achieved)

[0294] [3.Charge stability evaluation] The image forming apparatus was a modified Yanon full-color copier imageRUNNER ADVANCE C5560, the above-mentioned two-component developer 1 was placed in the cyan developer of the image forming apparatus, the cyan toner bottle was filled with toner 1, and the evaluation described below was performed. The modification was to remove the mechanism for discharging the excess magnetic carrier from the developer.

[0295] The amount of toner on the paper in a FFh image (solid image) is 0.45 mg / cm 2 FFh is the hexadecimal value of 256 gradations, with 00h being the 1st gradation (white background) of the 256 gradations, and FF being the 256th gradation (solid area) of the 256 gradations.

[0296] In the durability image output test, a durability image output test of 10,000 sheets was performed with an image ratio of 5%. The test environment was a high temperature and high humidity (HH) environment (temperature 30°C, relative humidity 80%). During the continuous printing of 10,000 sheets, the sheets were printed under the same development and transfer conditions (without calibration) as the first sheet.

[0297] The evaluation paper was copy paper GF-C081 (A4, basis weight 81.4 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0298] The image output evaluation items and evaluation criteria for the initial (first sheet) and 10,000 continuous sheets are shown below. The evaluation results are shown in Table 8.

[0299] (Image Density Measurement) Using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite), the image densities of the FFh image area and solid area at the initial (first sheet) and 10,000th sheets were measured, and the difference Δ between the two image densities was used to rank them according to the following criteria. The evaluation results are shown in Table 8. A: Less than 0.04 (very good). B: 0.04 or more and less than 0.09 (good). C: 0.09 or more and less than 0.15 (this is the level at which the effects of the present invention are obtained). D: 0.15 or more (a level at which the effects of the present invention are not fully achieved)

[0300] [4. Evaluation of external additive ghosting] The image forming apparatus was a modified Yanon full-color copier imageRUNNER ADVANCE C5560, the above-mentioned two-component developer 1 was placed in the cyan developer of the image forming apparatus, the cyan toner bottle was filled with toner 1, and the evaluation described below was performed. The modification was to remove the mechanism for discharging the excess magnetic carrier from the developer.

[0301] The amount of toner on the paper in a FFh image (solid image) is 0.45 mg / cm 2 FFh is the hexadecimal value of 256 gradations, with 00h being the 1st gradation (white background) of the 256 gradations, and FF being the 256th gradation (solid area) of the 256 gradations.

[0302] The test was performed in a normal temperature and low humidity (NL) environment (temperature 23°C, relative humidity 5%).

[0303] The evaluation paper was copy paper GF-C081 (A4, basis weight 81.4 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0304] First, 100 sheets of an image with vertical bands parallel to the paper feed direction and white areas other than the vertical bands were printed at an image ratio of 10%. The vertical bands were FFh images (solid images). During the continuous paper feed, the same development and transfer conditions (without calibration) as for the first sheet were used.

[0305] After passing 100 sheets, a full-surface halftone image (80h) was output and used to evaluate the initial ghost property of external additives.

[0306] After that, 10,000 more images with vertical bands parallel to the paper feed direction and white areas other than the vertical bands were printed at an image ratio of 10%. During the continuous paper feed, the paper was fed under the same development and transfer conditions (without calibration) as the first sheet.

[0307] After passing 10,000 sheets, a full-surface halftone image (80h) was output and used to evaluate the ghost properties of external additives after durability.

[0308] Using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite), the image density of the part where the vertical band was printed and the part where the white background was printed in the halftone image (80h) 8 at the beginning (after 100 sheets) and after durability (after 10,000 sheets) was measured, and the ghost property of the external additive was evaluated from the difference Δ between the two image densities and ranked according to the following criteria. The evaluation results are shown in Table 8. A: Less than 0.03 (very good). B: 0.03 or more and less than 0.06 (good). C: 0.06 or more and less than 0.11 (this is the level at which the effects of the present invention are obtained). D: 0.11 or more (a level at which the effects of the present invention are not fully obtained)

[0309] [5. Evaluation of transfer uniformity] The image forming apparatus was a modified Yanon full-color copier imageRUNNER ADVANCE C5560, the above-mentioned two-component developer 1 was placed in the cyan developer of the image forming apparatus, the cyan toner bottle was filled with toner 1, and the evaluation described below was performed. The modification was to remove the mechanism for discharging the excess magnetic carrier from the developer.

[0310] The amount of toner on the paper in a FFh image (solid image) is 0.45 mg / cm 2 FFh is the hexadecimal value of 256 gradations, with 00h being the 1st gradation (white background) of the 256 gradations, and FF being the 256th gradation (solid area) of the 256 gradations.

[0311] In the durability image output test, a durability image output test of 10,000 sheets was conducted with an image ratio of 0.6%. The test was conducted in a normal temperature and low humidity (NL) environment (temperature 23°C, relative humidity 5%). During the continuous passing of 10,000 sheets, the sheets were passed under the same development and transfer conditions (without calibration) as the first sheet. The evaluation paper was recycled copy paper GF-R100W (A4, basis weight 67.0 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0312] The image output evaluation items and evaluation criteria for the initial (first sheet) and 10,000 continuous sheets are shown below. The evaluation results are shown in Table 8.

[0313] (Image uniformity evaluation) After the durability test of 10,000 sheets, a solid image was printed, a 2 cm square image was captured with a digital microscope, and the captured image was converted to 8-bit grayscale using Image-J. The density histogram was then measured and its standard deviation was calculated. The standard deviation was ranked according to the following evaluation criteria. A: Standard deviation less than 2.0 (very good, no unevenness visible to the naked eye) B: Standard deviation 2.0 or more and less than 4.0 (very good) C: Standard deviation of 4.0 or more and less than 6.0 (the effect of the present invention is obtained) D: Standard deviation of 6.0 or more (the effect of the present invention is not obtained, non-uniformity is felt from a distance)

[0314] [Examples 2 to 39, Comparative Examples 1 to 4] The evaluation was carried out in the same manner as in Example 1, except that the two-component developer 1 was changed to two-component developers 2 to 43. The evaluation results are shown in Table 8.

[0315] [Table 8] [Explanation of symbols]

[0316] 1. Means for quantitatively supplying raw material, 2. Means for adjusting the flow rate of compressed gas, 3. Inlet pipe, 4. Projecting member, 5. Supply pipe, 6. Treatment chamber, 7. Means for supplying hot air, 8 (8-1, 8-2, 8-3). Means for supplying cold air, 9. Regulating means, 10. Recovery means, 11. Outlet for the means for supplying hot air, 12. Distribution member, 13. Swirling member, 14. Powder particle supply port

Claims

1. 1. A method for producing a toner having toner particles having core particles containing a binder resin and a wax, and inorganic oxide fine particles on the surface of the core particles, and a coating layer containing an organosilicon polymer coating the core particles, comprising the steps of: The core particles satisfy the following relationship, where the endothermic heat of the endothermic peak derived from the wax measured by differential scanning calorimetry (DSC) is Qi (J / g) and the endothermic heat of the endothermic peak derived from the wax measured by DSC after the core particles are treated with hexane is Qh (J / g): 0.7≦Qi−Qh≦20.0 The organosilicon polymer has a partial structure represented by the following formula (T3): The tetrahydrofuran insoluble portion of the toner particles 29 In Si-NMR analysis, the ratio [ST3] of the peak area of ​​the partial structure represented by the following formula (T3) to the total peak area of ​​the organosilicon polymer satisfies the relationship ST3 ≧ 0.05, R-Si(O 1 / 2 ) 3 (T3) (In formula (T3), R represents an alkyl group having 1 to 6 carbon atoms or a phenyl group.) the inorganic oxide fine particles are thermally fixed to the surface of the core particles, a step of adhering the inorganic oxide fine particles to the surface of the core particles containing the binder resin and the wax; and dispersing the core particles having the inorganic oxide fine particles attached thereto in an aqueous medium. coating the surfaces of the core particles to which the inorganic oxide fine particles are attached with the organosilicon polymer; a step of treating the core particles having the inorganic oxide fine particles adhered thereto with hot air after the step of adhering the inorganic oxide fine particles to the surfaces of the core particles;

2. 2. The method for producing a toner according to claim 1, wherein the value of Qi-Qh is 1.0 or more and 7.0 or less.

3. The organosilicon polymer has, when measured using X-ray photoelectron spectroscopy, The sum of the concentration of silicon atoms dSi, the concentration of oxygen atoms dO, and the concentration of carbon atoms dC in the surface layer of the core particle 3. The method for producing a toner according to claim 1, wherein the concentration of silicon atoms relative to (dSi+dO+dC), (dSi / [dSi+dO+dC]), is 2.5 atom % or more.

4. 4. The method for producing a toner according to claim 1, wherein the core particles satisfy the relationship: 0.15≦(Qi−Qh) / Qi≦0.

90.

5. 5. The method for producing a toner according to claim 1, wherein the coverage of the inorganic oxide fine particles with respect to the surface of the core particles is 3% or more and 30% or less.

6. 6. The method for producing a toner according to claim 1, wherein the inorganic oxide fine particles have a number average particle size of primary particles of 7 nm or more and 55 nm or less.

7. 7. The method for producing a toner according to claim 1, wherein the inorganic oxide fine particles are strontium titanate fine particles.

8. The method for producing a toner according to any one of claims 1 to 7, wherein the binder resin contains a polyester resin.

9. 9. The method for producing a toner according to claim 1, wherein the wax is a hydrocarbon wax.

Citation Information

Patent Citations

  • Toner, two-component developer, developing device, and image forming apparatus

    JP2010160451A

  • Toner

    JP2012083749A

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2014038177A

  • Toner for electrostatic latent image development

    JP2015034976A

  • Electrostatic latent image development toner

    JP2015132654A