toner

The core-shell structured toner particles with specific resin compositions address charge-up issues during high-speed printing, ensuring stable charge distribution and print density by forming low resistance regions within the toner particles.

JP7555784B2Active Publication Date: 2024-09-25CANON KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020178369
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-23
Publication Date
2024-09-25
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Toner particles experience charge-up phenomena during high-speed printing, leading to decreased print density, especially in low-temperature, low-humidity environments, due to strong adhesion to the toner carrier and inadequate charge stability.

Method used

The toner particles are designed with a core-shell structure, where the core contains resin B with alkyl groups of 18 to 30 carbon atoms and the shell contains resin A with specific functional groups, forming low resistance regions to manage charge distribution and prevent surface charge-up.

Benefits of technology

The core-shell structure effectively suppresses charge-up, maintaining print density during high-speed and long-time printing by managing charge distribution and preventing local charge accumulation on the toner surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555784000018
    Figure 0007555784000018
  • Figure 0007555784000001
    Figure 0007555784000001
  • Figure 0007555784000002
    Figure 0007555784000002
Patent Text Reader

Abstract

To provide a toner capable of suppressing decrease in printing density due to charge-up even during high-speed and long-term printing.SOLUTION: A toner has toner core particles and toner particles having a shell on the surface of the toner core particles. The shell contains a resin A. The toner core particles contain a resin B. The resin A has a predetermined structure. The resin B is a resin containing an alkyl group having 18 to 30 carbon atoms.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to toners used in electrophotography and electrostatic recording. [Background technology]

[0002] In recent years, printers and copiers have been designed to last longer and operate at higher speeds, and as a result, toners are required to have higher charging stability and charge rise property. For example, Patent Document 1 proposes incorporating a resin having silanol groups on the surface of the toner base particles to reduce changes in chargeability that accompany changes in the adhesion state of external additives, thereby stabilizing the charge amount during durability testing. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2007-279712 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, after studying the toner described in Patent Document 1, it was found that a local charge-up phenomenon may occur on the toner surface during high-speed printing. It was also found that, particularly in low-temperature, low-humidity environments, the toner may adhere strongly to the toner carrier due to electrostatic attraction, preventing the formation of a toner layer on the developing roller and causing problems such as a decrease in print density. For the above reasons, there has been a demand for the development of a toner that can suppress the decrease in print density due to charge-up even during high-speed, long-term printing.

[0005] The present disclosure has been made in consideration of the above problems, and provides a toner that can suppress a decrease in print density due to charge-up even during high-speed, long-term printing. [Means for solving the problem]

[0006] The present disclosure for solving the above problems is as follows. Toner core particles and surfaces of the toner core particles exists on A toner having toner particles having a shell, The shell comprises resin A, The toner core particles contain a resin B, The resin A has a structure represented by the following formula (1): The resin B is It has a structure represented by the following formula (2): The content of the structure represented by the formula (2) in the resin B is 40% by mass or more and 80% by mass or less. A toner characterized by:

[0007] [ka]

[0008] In formula (1), R 1 ~R 3 each independently represents an alkoxy group having 1 to 3 carbon atoms or a hydroxy group. [ka] [In formula (2), R 4 represents a hydrogen atom or a methyl group, n represents an integer of 17 to 29, X is -COO-* or -OCO-*, and * is -(CH 2 ) n CH 3 ] Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a toner that can suppress a decrease in print density due to charge-up even during high-speed printing for long periods of time. [Brief description of the drawings]

[0010] [Figure 1] Schematic diagram of an example of a charge amount measuring device DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The embodiments are described in detail below, but the present disclosure is not limited to the following description. In the present disclosure, the expressions "XX or more and YY or less" and "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified.

[0012] The present inventors believe that the reason why the toner obtained according to the present disclosure exhibits these effects is as follows. The toner particles of the present disclosure have a toner core particle and a shell on the surface of the toner core particle. That is, the toner particles of the present disclosure have a core-shell structure. The shell contains a resin A, and the resin A has a structure represented by the following formula (1). Furthermore, the toner core particle contains a resin B, and the resin B is a resin containing an alkyl group having 18 to 30 carbon atoms.

[0013] [ka]

[0014] In formula (1), R 1 ~R 3 each independently represents an alkoxy group having 1 to 3 carbon atoms or a hydroxy group. The alkyl groups having 18 to 30 carbon atoms of the resin B present in the toner core particles gather together to form minute crystal domains, partially generating regions of low electrical resistance. The charge rapidly generated in the shell portion containing the resin A is temporarily stored in the benzene nucleus in formula (1), but the excess charge diffuses to the shell portion via the low resistance region present near the surface of the toner core particles described above. This is believed to suppress localized charge buildup on the toner surface, thereby exerting the effects of the present disclosure.

[0015] Resin A will be described in detail. The shell contains resin A, and resin A has a structure represented by the following formula (1).

[0016] [ka]

[0017] R in formula (1) 1 ~R 3 are each independently an alkoxy group or a hydroxy group having 1 to 3 carbon atoms. The number of carbon atoms in the alkoxy group is preferably 1 or 2, and more preferably 1.

[0018] R in formula (1) 1 ~R 3 In order to make one or more of R into a hydroxy group, 1 ~R 3 Resin A, in which one or more of the above groups are alkoxy groups, is hydrolyzed to convert the alkoxy groups into hydroxy groups. Good too. The hydrolysis may be carried out by any method, for example, the following method. R in the above formula (1) 1 ~R 3 Resin A, in which one or more of the above groups are alkoxy groups, is dissolved or suspended in a suitable solvent (which may be a polymerizable monomer), and the pH is adjusted to acidic using an acid or alkali, followed by mixing and hydrolysis. Further, hydrolysis may occur during the production of toner particles.

[0019] As a method for introducing the structure represented by formula (1) into resin A, for example, there is a method of polymerizing a vinyl monomer or a resin containing an ethylenically unsaturated bond with a styryl-based silane coupling agent. Examples of styryl-based silane coupling agents include p-styryltrimethoxysilane, p-styryltriethoxysilane, and p-styryltripoxysilane. In addition, two or more types of silane coupling agents may be used in combination.

[0020] The content of the resin A in the toner particles is preferably 0.1% by mass to 20.0% by mass. If it is 0.1% by mass or more, it is easy to obtain an appropriate charge amount, and if it is 20.0% by mass or less, it is easy to suppress charge-up. More preferably, it is 1.0% by mass to 10.0% by mass. The content of resin A in the toner particles can be controlled by, for example, changing the amount of resin A or the polymerizable monomer capable of forming resin A added in the process of forming a shell on the surface of the toner core particles. The content of the structure represented by formula (1) in resin A is preferably 0.5% by mass to 5.0% by mass, and more preferably 1.0% by mass to 2.5% by mass. Furthermore, the content of resin A in the shell is preferably from 50% by mass to 100% by mass, and more preferably from 80% by mass to 100% by mass. The shell may completely cover the surface of the toner core particle, or the surface of the toner core particle may be partially exposed.

[0021] Resin B will now be described in detail. The toner core particles contain a resin B, and the resin B is a resin containing an alkyl group having a carbon number of 18 to 30. The alkyl group may be a linear alkyl group or a branched alkyl group, but is preferably a linear alkyl group. As described above, the alkyl group having 18 to 30 carbon atoms serves as a path for transferring charges, and having 18 to 30 carbon atoms provides an appropriate length for transferring charges between the toner core particle and the shell. If the carbon number is less than 18, it becomes difficult to form a crystalline domain by the alkyl group, and it becomes difficult to obtain a low resistance region of the toner core particle, so that the effect of the present disclosure cannot be obtained. Also, if the carbon number exceeds 30, the formation of the crystalline domain is easily hindered due to entanglement with other polymer chains, and the effect of the present disclosure cannot be obtained. In order to enhance the above effect, the carbon number is preferably 20 or more and 25 or less.

[0022] Resin B preferably has a structure represented by the following formula (2).

[0023] [ka]

[0024] In formula (2), R 4represents a hydrogen atom or a methyl group, n represents an integer from 17 to 29, X is -COO-* or -OCO-*, and * is -(CH2) n It represents a bond to CH3. n is preferably an integer of 19 to 24. When Resin B has the structure represented by the above formula (2), an alkyl group having 18 to 30 carbon atoms is present in the side chain of Resin B, increasing the degree of freedom of the alkyl group, making it easier to form appropriately small crystal domains during triboelectric charging, and making it easier to suppress charge-up.

[0025] X in formula (2) is -COO-* (* is -(CH2) n It is more preferable that X is represented by -COO-*, where X is an alkyl group having 18 to 30 carbon atoms and is directly bonded to an oxygen atom, so that the degree of freedom of the alkyl group is further increased and the alkyl group rotates appropriately, so that the crystalline domain is easily formed and the charge-up is further suppressed.

[0026] The content of the structure represented by the above formula (2) in the resin B is preferably 5% by mass or more and 80% by mass or less. If it is 5% by mass or more, the charge transfer becomes smoother and the charge-up suppression effect is more easily obtained, and if it is 80% by mass or less, an appropriate charge amount is easily obtained. More preferably, it is 40% by mass or more and 65% by mass or less. As a method for introducing the structure represented by formula (2) into resin B, for example, there is a method of polymerizing a vinyl monomer or a resin containing an ethylenically unsaturated bond with a monomer such as the following. Examples of monomers for introducing the structure represented by formula (2) into Resin B include stearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, heneicosanyl (meth)acrylate, behenyl (meth)acrylate, lignoceryl (meth)acrylate, ceryl (meth)acrylate, octacosyl (meth)acrylate, myrisyl (meth)acrylate, dotriacontyl (meth)acrylate, and 1,18-octadecanedioic acid. The content of the structure shown in the above formula (2) in resin B can be controlled by, for example, changing the proportion of the monomer for introducing the structure shown in the above formula (2) into resin B, in the polymerizable monomer capable of forming resin B.

[0027] It is preferable that resin B further has a structure represented by the following formula (3). When resin B further has a structure represented by formula (3), an interaction between aromatic rings works between the toner core particle and the shell, and adhesion is enhanced, so that charge-up can be more easily suppressed. The content of the structure represented by formula (3) in resin B is preferably 5% by mass to 65% by mass, and more preferably 5% by mass to 10% by mass.

[0028] [ka]

[0029] As a method for introducing the structure represented by formula (3) into resin B, there is a method of polymerizing a vinyl monomer or a resin containing an ethylenically unsaturated bond with styrene. The content of the structure represented by the above formula (3) in Resin B can be controlled by changing the proportion of styrene in the polymerizable monomer capable of forming Resin B, or the like.

[0030] The weight average molecular weight MwB of resin B is preferably 15,000 or more and 250,000 or less. When MwB is in this range, alkyl groups having 18 to 30 carbon atoms present in resin B tend to gather together, and low resistance regions tend to be formed, which makes it easier to transfer charges. It is easier to suppress charge-up. A more preferable range of MwB is from 20,000 to 80,000. MwB can be controlled by changing the reaction temperature, reaction time, monomer charging ratio, initiator amount, etc. when producing the resin.

[0031] The content of the resin B in the toner core particles is preferably 50.0% by mass to 95.0% by mass, and more preferably 70.0% by mass to 90.0% by mass. Within this range, the effects of the present disclosure are easily obtained. The content of the resin B in the toner core particles can be controlled by changing the amount of the resin B or the polymerizable monomer capable of forming the resin B added in the step of forming the toner core particles.

[0032] Resin B is not particularly limited as long as it is a resin containing an alkyl group having 18 to 30 carbon atoms, and known resins such as vinyl resins, maleic acid copolymers, polyester resins, and epoxy resins can be used. Among these, resin B is preferably a vinyl resin. Examples of vinyl resins include polymers of monomers containing ethylenic unsaturated bonds.

[0033] More preferred embodiments of the toner particles will be described in detail below. The intensity ratio of silicon ions to the total ion count at mass numbers of 0.5 to 1850, obtained when the toner particles are measured using time-of-flight secondary ion mass spectrometry (TOF-SIMS), is preferably 0.00100 or more and 0.00500 or less, and more preferably 0.00150 to 0.00300. When the intensity ratio is 0.00100 or more, an appropriate charge amount is easily obtained, and when it is 0.00500 or less, charge transfer is facilitated, so that the charge-up suppression effect is easily obtained. The intensity ratio can be controlled by changing the composition and amount of resin A added, as well as by changing the manufacturing method of the toner particles for introducing the above-mentioned resin A.

[0034] The SP value of resin A is SPA (J / cm 3 ) 1 / 2 The SP value of resin B is SPB (J / cm 3 ) 1 / 2 When │SPA-SPB│≦1.00(J / cm 3 ) 1 / 2 │SPA-SPB│≦1.00(J / cm 3) 1 / 2 When the toner core particle and the shell are in close contact with each other, charge-up can be more easily suppressed. More preferably, |SPA-SPB|≦0.80 (J / cm 3 ) 1 / 2 The lower limit of |SPA-SPB| ​​is not particularly limited, but is, for example, 0.00 or more. In addition, the SPA is 15.0 (J / cm 3 ) 1 / 2 ~25.0(J / cm 3 ) 1 / 2 It is preferable that the saturation temperature is 17.0 (J / cm 3 ) 1 / 2 ~22.0(J / cm 3 ) 1 / 2 It is more preferable that: Furthermore, the SPB is 14.0 (J / cm 3 ) 1 / 2 ~24.0(J / cm 3 ) 1 / 2 It is preferable that the saturation temperature is 16.0 (J / cm 3 ) 1 / 2 ~21.0(J / cm 3 ) 1 / 2 It is more preferable that: SPA and SPB can be controlled by changing the compositions of resins A and B.

[0035] The SP value, also known as the solubility parameter, is a number used as an index of solubility and affinity, showing how much a substance dissolves in another substance. Materials with similar SP values ​​have high solubility and affinity, while materials with different SP values ​​have low solubility and affinity. The SP value of a monomer can be calculated using solubility parameter calculation software (Hansen Solubility Parameters in Practice 4th Edition 4.1.03). The SP value is calculated based on the Hansen solubility parameter theory. In the Hansen solubility parameter theory, the energy of evaporation of a molecule is divided into three parts: energy due to dispersion forces (dispersion term D), energy due to dipole interactions (polarization term P), and energy due to hydrogen bonds (hydrogen bond term H), and these are treated as three-dimensional vectors. . The SP value is calculated by first calculating the dispersion term D, the polarization term P, and the hydrogen bond term H using solubility parameter calculation software, and then taking the square root of the sum of the squared values ​​of each term to obtain the scalar quantity of the three-dimensional vector.

[0036] The toner particles may contain a release agent. Examples of the release agent include aliphatic hydrocarbon waxes, oxides of aliphatic hydrocarbon waxes, block copolymers of aliphatic hydrocarbon waxes, waxes mainly composed of fatty acid esters, and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax, partial esterification products of fatty acids and polyhydric alcohols, methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats, and Fischer-Tropsch wax. The content of the release agent in the toner particles is preferably 1.50% by mass or more and 20.0% by mass or less.

[0037] A method for producing the toner particles will now be described. Toner particles can be produced by a known method. For example, a suspension polymerization method is used in which a polymerizable monomer composition containing a polymerizable monomer for obtaining resin B, resin A, and optionally a release agent is suspended and granulated in an aqueous medium, and the polymerizable monomer in the polymerizable monomer composition is polymerized; a kneading and grinding method is used in which various toner constituent materials such as resin B, resin A, and optionally a release agent are kneaded, ground, and classified; an emulsion aggregation method is used in which a dispersion obtained by emulsifying and dispersing resin B and resin A is mixed with a dispersion liquid containing a release agent and the like as required, and the mixture is aggregated and heat-fused to obtain toner particles; an emulsion polymerization aggregation method is used in which a dispersion liquid obtained by emulsion-polymerizing a polymerizable monomer constituting resin B is mixed with a dispersion liquid obtained by emulsifying and dispersing resin A and a dispersion liquid containing a release agent and the like as required, and the mixture is aggregated and heat-fused to obtain toner particles; a dissolution suspension method is used in which an organic solvent dispersion liquid containing resin B, resin A, and optionally a release agent is suspended in an aqueous medium, and the mixture is granulated; and the like.

[0038] It is preferable that resin A is formed uniformly and densely on the surface of the toner core particles containing resin B, but this is not necessarily the case as long as the surface of the toner core particles is coated with resin A. There is no limitation on the method of forming the shell containing the resin A. For example, when the shell is provided after the formation of the toner core particles, the toner core particles and the resin fine particles forming the shell are dispersed in an aqueous medium, and then the resin fine particles are aggregated and adsorbed on the surface of the toner core particles. In addition, after the formation of the toner core particles, a polymerizable monomer constituting the shell is added to perform seed polymerization, so that the surface of the toner core particles is uniformly covered.

[0039] The toner particles may be used as a toner as it is, but an external additive may be added to the toner particles to improve the image quality of the toner. As the external additive, inorganic fine particles such as silica fine particles, titanium oxide fine particles, or aluminum oxide fine particles are preferably used. These inorganic fine particles are preferably hydrophobic inorganic fine particles that have been hydrophobized with a hydrophobizing agent such as a silane coupling agent, silicone oil, or a mixture thereof. Furthermore, if necessary, an external additive other than the inorganic fine particles or hydrophobic inorganic fine particles may be added to the toner particles. The amount of the external additive added is preferably 0.5 parts by mass or more and 5.0 parts by mass or less with respect to 100 parts by mass of the toner particles.

[0040] The toner particles may contain a colorant. The colorant is not particularly limited, and the following known colorants can be used. Examples of yellow pigments include condensed azo compounds such as yellow iron oxide, navel yellow, naphthol yellow S, Hansa yellow G, Hansa yellow 10G, benzidine yellow G, benzidine yellow GR, quinoline yellow lake, permanent yellow NCG, and tartrazine lake, isoindolinone compounds, anthraquinone compounds, and azo metal complexes. Compounds such as aryl amide compounds, methine compounds, and aryl amide compounds are used. CI Pigment Yellow 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 109, 110, 111, 128, 129, 147, 155, 168, 180. Examples of magenta pigments include condensed azo compounds such as red iron oxide, permanent red 4R, lithol red, pyrazolone red, watching red calcium salt, lake red C, lake red D, brilliant carmine 6B, brilliant carmine 3B, eosine lake, rhodamine lake B, and alizarin lake, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include the following. CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 254. Examples of cyan pigments include alkali blue lake, Victoria blue lake, phthalocyanine blue, metal-free phthalocyanine blue, phthalocyanine blue partial chloride, fast sky blue, copper phthalocyanine compounds such as indanthrene blue BG and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include the following. CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, 66. Examples of black pigments include carbon black, aniline black, non-magnetic ferrite, magnetite, and pigments toned to black using the above-mentioned yellow, magenta and cyan colorants. These colorants can be used alone or in combination, or in the form of a solid solution. The content of the colorant in the toner particles is preferably 3.0% by mass to 15.0% by mass.

[0041] The methods for measuring the various physical properties of the toner will be described below. <Separation of toner and additives> First, in the case where the surface of the toner particles has been treated with an external additive or the like, the external additive is removed by the following method to obtain the toner particles. Add 160 g of sucrose (Kishida Chemical) to 100 mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Add 31 g of the concentrated sucrose solution and 6 mL of Contaminon N (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of nonionic surfactants, anionic surfactants, and organic builders, manufactured by Wako Pure Chemical Industries, Ltd.) to a centrifuge tube (50 mL capacity) to prepare a dispersion. Add 1.0 g of toner to this dispersion and break up the toner clumps with a spatula or similar. The centrifuge tube is shaken in a shaker at 350 strokes per minute (spm) for 20 minutes. After shaking, the solution is transferred to a glass tube for a swing rotor (capacity 50 mL) and separated in a centrifuge (H-9R, manufactured by Kokusan Co., Ltd.) at 3500 rpm for 30 minutes. This operation separates the toner particles from the removed external additives. Visually check that the toner and the aqueous solution are sufficiently separated, and collect the toner that has separated to the top layer with a spatula. The collected toner is filtered through a vacuum filter, and then dried in a dryer for at least one hour to obtain toner particles. This operation is repeated several times to ensure the required amount.

[0042] <Method of extracting Resin A and Resin B from toner particles> Resin A in the toner particles was extracted by dissolving the extract using tetrahydrofuran (THF). The preparation method is as follows: Weigh out 10.0 g of toner particles, place them in a cylindrical filter paper (Toyo Roshi No. 84) and place them in a Soxhlet extractor. Extract for 20 hours using 200 mL of THF as the solvent, and the solid obtained by removing the solvent from the extract is the THF-soluble fraction. The THF-soluble fraction contains resin A or resin B. Repeat this process multiple times to obtain the required amount of THF-soluble fraction. For the solvent gradient elution method, gradient preparative HPLC (Shimadzu LC-20AP high pressure gradient preparative system, Waters SunFire preparative column 50mm φ250mm) is used. The column temperature is 30°C, the flow rate is 50mL / min, and the mobile phase uses acetonitrile as a poor solvent and THF as a good solvent. 0.02g of the THF soluble fraction obtained by extraction is dissolved in 1.5mL of THF to prepare the sample for separation. The mobile phase starts with a composition of 100% acetonitrile, and 5 minutes after the sample injection, the ratio of THF is increased by 4% per minute until the mobile phase composition becomes 100% THF over 25 minutes. The components can be separated by drying the obtained fraction. This allows resin A or resin B to be obtained. It is possible to determine which fraction components are resin A and which are resin B. 13 It can be distinguished by C-NMR measurement.

[0043] <Measurement of Resin A and Resin B Content in Toner Particles> By identifying and extracting resin A from each fraction obtained by the method of extracting resin A and resin B from toner particles, the content of resin A in the toner particles subjected to the Soxhlet extractor can be calculated. Furthermore, the content of resin B in the toner core particles can be calculated from the mass of the toner particles used to extract resin B minus the mass of resin A and the mass of the resulting resin B.

[0044] <How to confirm the structure of Resin A and Resin B> R in formula (1) for resin A 1 ~R 3 The structures of the site and resin B represented by formula (2) and formula (3) can be confirmed by 13 C-NMR analysis, 29 This is carried out using Si-NMR. The measurement sample is either resin A or resin B itself, or resin A or resin B extracted from toner particles by the above-mentioned extraction method. R in formula (1) 1 ~R 3 The alkoxy group or hydroxy group in 29The valence of the alkoxy group or hydroxy group relative to the silicon atom can be determined by the method shown in "Si-NMR (solid) measurement conditions."

[0045] ( 29 Si-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample size: 150mg Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 97.38MHz ( 29 Si) Reference material: DSS (external standard: 1.534ppm) Sample rotation speed: 10kHz Contact time: 10ms Delay time: 2s Number of times: 2000 to 8000 From the above measurement, the abundance ratio of multiple silane components according to the number of oxygen atoms bonded to Si can be calculated by peak separation and integration using curve fitting. In this way, R in formula (1) 1 ~R 3 The valence of the alkoxy group or hydroxy group relative to the silicon atom can be confirmed. R in formula (1) 1 ~R 3 The structures shown in formula (2) and formula (3) are 13 C-NMR(Solid The measurement conditions are as follows:

[0046] ( 13 C-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample size: 150mg Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 123.25MHz ( 13 C) Reference substance: Adamantane (external standard: 29.5ppm) Sample rotation speed: 20kHz Contact time: 2ms Delay time: 2s Number of times accumulated: 1024 Formula (1), R in formula (1) 1 ~R 3 The monomer units in resin B represented by formulas (2) and (3) are separated into various peaks according to their types, and each peak is identified to obtain R 1 ~R 3 The structures of formula (2) and formula (3) are determined. The content of the structure represented by formula (2) in resin B is determined from the integral value of the obtained peak.

[0047] <Method of measuring weight average molecular weight (Mw)> The weight average molecular weight (Mw) of a polymer, resin or toner particle is measured by gel permeation chromatography (GPC) as follows. First, the sample is dissolved in tetrahydrofuran (THF) at room temperature for 24 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is prepared so that the concentration of components soluble in THF is approximately 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: HLC8120 GPC (detector: RI) (Tosoh Corporation) Column: Shodex KF-801, 802, 803, 804, 805, 806, 807 (Showa Denko) Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Oven temperature: 40.0℃ Sample injection volume: 0.10 mL When calculating the molecular weight of the sample, a molecular weight calibration curve prepared using a standard polystyrene resin (trade names "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.

[0048] <Method for Measuring the Intensity Ratio of Silicon Ions to Total Ion Count at Mass Numbers from 0.5 to 1850 in TOF-SIMS Measurement> The toner particles are measured using a time-of-flight secondary ion mass spectrometer (TOF-SIMS), and the intensity ratio of silicon ions to the total ion count at mass numbers from 0.5 to 1850 is confirmed. The apparatus used and the measurement conditions are shown below. Measuring apparatus: TOFSIMS TRIFT IV (manufactured by ULVAC-PHI, Inc.) Primary ion species: Gold ions (Au + ) Primary ion acceleration voltage: 30 keV Primary ion current value: 2 pA Analysis area: 300 × 300 μm 2 Number of pixels: 256 × 256 pixel Analysis time: 3 min Repetition frequency: 8.2 kHz Charge neutralization: on Secondary ion polarity: Positive Secondary ion mass range (m / z): 0.5 to 1850 Analysis is performed using the ULVAC-PHI, Inc. standard software (Win Cadense). The intensity ratio of silicon ions is calculated as the intensity ratio of the ion count derived from silicon with a mass number of 28 to the total ion count at mass numbers from 0.5 to 1850.

[0049] <Method for Measuring the Weight Average Particle Diameter (D4) of Toner Particles and Toner> The toner particles and the weight average particle size (D4) of the toner are measured using a precision particle size distribution measuring device "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.). The measurement is performed under the following conditions. Effective number of measurement channels: 25,000 Total number of control motors: 50,000 Aperture: 100μm Current: 1600μA Gain; 2 The Kd value is measured using a "Standard particle size of 10.0 μm" (Beckman Coulter, Inc.). The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume %, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4). EXAMPLES

[0050] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these examples. Unless otherwise specified, the "parts" of each material in the examples and comparative examples are all based on mass.

[0051] <Production of Resin V1> Resin V1 was prepared according to the following procedure. 100.0 parts of propylene glycol monomethyl ether was heated while replacing with nitrogen, and refluxed at a liquid temperature of 120°C or higher. A mixture of 100 parts of styrene as a polymerizable monomer and 0.50 parts of tert-butyl peroxybenzoate [manufactured by NOF Corp., trade name: Perbutyl Z] as a polymerization initiator was added dropwise over 3 hours. After the dropwise addition was completed, the solution was stirred for 3 hours, and then distilled at normal pressure while raising the liquid temperature to 170°C. After the liquid temperature reached 170°C, the pressure was reduced to 1 hPa, and the solvent was removed by distillation for 1 hour to obtain a resin solid. The resin solid was dissolved in tetrahydrofuran, reprecipitated with n-hexane, and the precipitated solid was filtered to obtain resin V1. The weight average molecular weight (Mw) of the obtained resin V1 was 24500.

[0052] <Production of Resin V2> As shown in Table 1, Resin V2 was produced in the same manner as Resin V1, except that the polymerizable monomer was changed.

[0053] [Table 1] BA: n-butyl acrylate

[0054] <Production Example of Resin A1> Resin A1 was prepared according to the following procedure. 98.4 parts of resin V1 were dissolved in 400.00 parts of N,N-dimethylacetamide, and 1.6 parts of p-styryltrimethoxysilane as a silane compound, 3.0 parts of triethylamine, and 3.20 parts of DMT-MM [4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride] as a condensing agent were added, and the mixture was stirred at room temperature for 5 hours. After the reaction was completed, the solution was dropped into methanol, reprecipitated, and filtered to obtain resin A1. The weight average molecular weight Mw of resin A1 was 20,000. The physical properties of the obtained resin A1 are shown in Table 3.

[0055] <Production Example of Resin A2> Resin A2 was obtained in the same manner as in Production Example for Resin A1, except that the base resin was changed to Resin V2. The structure and physical properties of the obtained Resin A2 are shown in Table 3.

[0056] [Table 2]

[0057] [Table 3]

[0058] <Production Example of Toner Particle 1> 98.4 parts of styrene and 1.6 parts of p-styryltrimethoxysilane were mixed using a stirrer until a homogeneous phase was obtained, to obtain a monomer solution 1. Next, 50 parts of ion-exchanged water was measured out, and 50 parts of the monomer solution 1 was added to adjust the solid concentration to 50 mass%, and then a dispersion treatment was performed using an ultrasonic homogenizer (manufactured by SONICS & MATERIAL) at a strength of 97% at 25°C for 1 minute, to obtain a monomer suspension 1.

[0059] Next, 390.0 parts of ion-exchanged water and 14.0 parts of sodium phosphate (12-hydrate) (manufactured by Rasa Kogyo Co., Ltd.) were added to the reaction vessel, and the mixture was kept warm at 65°C for 1.0 hours while purging with nitrogen. Next, an aqueous calcium chloride solution in which 9.2 parts of calcium chloride (dihydrate) was dissolved in 10.0 parts of ion-exchanged water was added all at once using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) while stirring at 12,000 rpm, to prepare an aqueous medium containing a dispersion stabilizer. Furthermore, hydrochloric acid was added to the aqueous medium to adjust the pH to 6.0, and aqueous medium 1 was obtained.

[0060] Next, the following materials were mixed: Behenyl acrylate 54.0 parts Acrylonitrile 27.0 parts Styrene 9.0 parts Wax (Fischer-Tropsch wax, melting point: 78°C) 4.0 parts CI Pigment Blue 15:3 4.00 parts The mixture was kept at 65° C. and uniformly dissolved and dispersed using a TK homomixer at 500 rpm to prepare a polymerizable monomer composition 1.

[0061] While maintaining the temperature of the aqueous medium 1 at 70° C. and the rotation speed of the stirring device at 12,000 rpm, the polymerizable monomer composition 1 was charged into the aqueous medium 1, and 9.0 parts of t-butyl peroxypivalate was added as a polymerization initiator. Granulation was continued for 10 minutes while maintaining the stirring speed at 12,000 rpm. The stirring device was changed to a stirrer equipped with a propeller stirring blade, and polymerization was carried out for 5.0 hours while stirring at 150 rpm and maintaining the temperature at 70°C. The temperature was then further increased to 85°C and maintained at that temperature for 2.0 hours. Thereafter, the mixture was cooled to room temperature, and ion-exchanged water was added, followed by decantation and filtration to adjust the solids concentration to 20.0% by mass, thereby obtaining toner core particle dispersion 1.

[0062] 98.0 parts of the obtained toner core particle dispersion 1 was placed in a reaction vessel equipped with a stirrer, heated to 70° C. with stirring, and purged with nitrogen for 1 hour. 2.0 parts of monomer suspension 1 and 0.1 parts of potassium persulfate (KPS) were added to a reaction vessel and reacted at 70°C for 3 hours to form resin A3 on the surface of the toner core particles. After cooling to room temperature, hydrochloric acid was added to adjust the pH to 1.4 or less, and stirring was performed for 1 hour. The dispersion stabilizer was dissolved, and the mixture was filtered, washed, and dried to obtain toner particles 1. Table 5 shows the physical properties of resin B1 of toner particles 1. Table 6 shows the physical properties of toner particles 1.

[0063] <Production Examples of Toner Particles 2, 5 to 28, and Comparative Toner Particles 1, 3, and 4> Toner particles 2, 5 to 28 and comparative toner particles 1, 3 and 4 were produced in the same manner as in the production example of toner particle 1, except that the composition of the resin polymerizable monomer composition was changed as shown in Table 3-1 and the composition and number of parts of the monomer solution were changed as shown in Table 3-2. The physical properties of resins B1 and 3 to 18 of the obtained toner particles 2, 5 to 28 and comparative toner particles 1, 3 and 4 are shown in Table 5. The physical properties of the obtained toner particles 2, 5 to 28 and comparative toner particles 1, 3 and 4 are shown in Table 6.

[0064] [Table 4-1] BHA: Behenyl acrylate AN: Acrylonitrile BA: n-butyl acrylate

[0065] [Table 4-2] BA: n-butyl acrylate

[0066] <Production Example of Comparative Toner Particles 2> Comparative toner particles 2 were obtained in the same manner as in the production example of toner particles 1, except that the production process of monomer suspension 1 was omitted and the parts of wax and pigment were changed. The physical properties of the obtained comparative toner particles 2 are shown in Table 6.

[0067] <Production Example of Toner Particle 3> (Production of Resin B2) Behenyl acrylate 54.0 parts Acrylonitrile 27.0 parts Styrene 9.0 parts Toluene 100.0 parts The above materials were mixed and heated to 70°C, and then 1.0 part of t-butyl peroxypivalate was added as a polymerization initiator while stirring. The temperature was then maintained at 70°C and polymerization was carried out for 5.0 hours, and the temperature was then raised to 85°C and held for 2.0 hours. After cooling, the mixture was re-immersed in methanol. Resin B2 was obtained by precipitation, filtration and drying. The physical properties of the obtained resin B2 are shown in Table 4.

[0068] (Production of dispersion of resin B2 fine particles) 60 parts of resin B2 were added to 200 parts of toluene (manufactured by Wako Pure Chemical Industries), heated to 90°C, and then stirred for 3 hours to dissolve. 180 parts of ion-exchanged water in which 6 parts of anionic surfactant (manufactured by Daiichi Kogyo Seiyaku: Neogen RK) and 3 parts of anionic surfactant (manufactured by Nippon Oil & Fats: Nonsar LN1) were dissolved were added to the toluene solution in which resin B2 was dissolved. Then, the mixture was thoroughly stirred at 4000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Co., Ltd.). After that, the mixture was dispersed for about 1 hour using a high-pressure impact type dispersing machine Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.), and then the toluene was removed using an evaporator to obtain a dispersion of resin B2 fine particles. The physical properties of the obtained resin B2 are shown in Table 5.

[0069] (Preparation of Dispersion of Resin A1) A dispersion of Resin A1 was obtained in the same manner as in the production of the dispersion of Resin B2 fine particles, except that Resin B2 was changed to Resin A1.

[0070] (Production of dispersion of release agent particles) Release agent (Fischer-Tropsch wax, melting point: 78°C) 4.0 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 1.0 part 79.0 parts of ion-exchanged water The above formulation was placed in a mixing vessel equipped with a stirrer, heated to 90°C, and circulated through a Clearmix W Motion (manufactured by M Technique) while being stirred at a shear stirring section with a rotor outer diameter of 3 cm and a clearance of 0.3 mm under conditions of a rotor rotation speed of 19,000 r / min and a screen rotation speed of 19,000 r / min. After dispersing for 60 minutes, the mixture was cooled to 40°C under cooling treatment conditions of a rotor rotation speed of 1,000 r / min, a screen rotation speed of 0 r / min, and a cooling rate of 10°C / min, to obtain a dispersion of release agent fine particles.

[0071] (Production of pigment dispersion) CI Pigment Blue 15:3 4.0 parts 78.0 parts of ion-exchanged water Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 2.0 parts The above materials were mixed and then dispersed for 1 hour using a high-pressure impact disperser Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.) to prepare a pigment dispersion liquid.

[0072] Resin B2 fine particle dispersion (solid content 28%) 360.0 parts Pigment dispersion (solid content 7%) 40.0 parts Dispersion of release agent particles (solid content 6%) 20.0 parts Dispersion of Resin A1 (28% solids) 8.0 parts First, the above materials except for the dispersion of resin A1 were put into a round stainless steel flask and mixed. An aqueous solution of 8 parts of magnesium sulfate dissolved in 98 parts of ion-exchanged water was added to the flask, and the mixture was dispersed for 5 minutes at 5000 r / min using a homogenizer (IKA: Ultra Turrax T50). Next, the dispersion of resin A1 was added, and the mixture was dispersed for 5 minutes at 5000 r / min using a homogenizer (IKA: Ultra Turrax T50). The mixture was then heated to 50°C in a heating water bath using a stirring blade while appropriately adjusting the rotation speed so that the mixture was stirred. After holding at 50°C for 1 hour, the weight average particle size of the formed aggregated particles was measured. As a result, it was confirmed that aggregated particles with a weight average particle size of about 6.0 μm were formed.

[0073] The obtained dispersion of aggregated particles was mixed with 360 parts of ion-exchanged water and ethylenediaminetetraacetic acid. An aqueous solution in which 40 parts of sodium hydroxide had been dissolved was added, and then 2,800 parts of ion-exchanged water was added. The mixture was heated to 80°C while continuing to stir, and held in a sealed state for 2 hours to obtain fully fused particles. After that, the mixture was filtered and separated into solid and liquid, and the filtered cake was thoroughly washed with ion-exchanged water and dried using a vacuum dryer to obtain toner particles 3 having a weight average particle size of 6.2 μm. The physical properties of the obtained toner particles 3 are shown in Table 6.

[0074] <Production Example of Toner Particle 4> Toner particles 4 were obtained in the same manner as in the production of toner particles 3, except that resin A2 was used instead of resin A1. The physical properties of toner particles 4 obtained are shown in Table 6.

[0075] [Table 5]

[0076] [Table 6] *: The intensity ratio of silicon ions to the total ion count in the mass numbers 0.5 to 1850 obtained by measuring using time-of-flight secondary ion mass spectrometry.

[0077] <Production Examples of Toners 1 to 28 and Comparative Toners 1 to 4> For 100.0 parts of each of the obtained toner particles 1 to 28 and the comparative toner particles 1 to 4, the BET value was 200 m 2 / g, and the number average particle size of the primary particles is 8 nm. 0.6 parts of the fine particles were mixed in a Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.). After the above-mentioned mixing treatment, the mixture was sieved through a mesh having an opening of 150 μm to obtain toners 1 to 28 and comparative toners 1 to 4.

[0078] <Examples 1 to 28> In Examples 1 to 28, evaluations were carried out using Toners 1 to 28, respectively. The evaluation methods and results are shown below. In the following, Examples 9, 10, 12 and 13 will be referred to as Reference Examples 9, 10, 12 and 13, respectively.

[0079] <Comparative Examples 1 to 4> In Comparative Examples 1 to 4, evaluation was carried out using Comparative Toners 1 to 4, respectively. The evaluation was carried out in the same manner as in Examples 1 to 28.

[0080] <Toner Evaluation Method> <Evaluation of developability> A modified LBP712Ci (Canon) color laser printer was used to evaluate durability in a low temperature and low humidity environment (15°C / 10%). The modifications were as follows: The process speed was set to 350 mm / sec by changing the gear and software of the evaluation machine body. The cartridge used for the evaluation was a cyan cartridge. That is, the product toner was removed from a commercially available cyan cartridge, the inside was cleaned with an air blower, and then 100 g of Toner 1 was filled in. Note that the magenta, yellow, and black cartridges were inserted into each station from which the product toner had been removed and whose remaining toner amount detection mechanisms had been disabled. Under the above conditions, the media (XEROX4200 paper (XEROX 75g / m 2 ) was used to continuously output images with a print rate of 1%. A solid image was output on the 50th sheet. After that, a total of 10,000 images with a print rate of 1% were printed. After printing the 10,000th sheet, a solid image was output again. The rate of decrease in density of the 10,000th solid image compared to the 50th sheet was used to evaluate durability. The image density was measured using a color reflection densitometer (X-Rite 404A, manufactured by X-Rite Co., Ltd.). The evaluation results are shown in Table 7. [Evaluation Criteria] A: Concentration reduction rate is less than 5.0% B: Concentration reduction rate is 5.0% or more and less than 7.0% C: Concentration reduction rate is 7.0% or more and less than 10.0% D: Concentration reduction rate is 10.0% or more

[0081] <Evaluation of Charge Amount> The charge amount was evaluated in a high temperature and high humidity environment (30°C / 80% RH). The charge amount of the toner is measured by mixing 1.0 g of toner with 19.0 g of magnetic carrier (Standard Carrier for q / m Measurement N-01, manufactured by Nippon Imaging Co., Ltd.), leaving it for 24 hours in a 30°C, 80% humidity environment, shaking it at 150 rpm for 1 minute using a YAYOI YS-8D model, and then measuring it as follows. Figure 1 shows an example of a charge amount measuring device. First, about 0.4 g of the mixture of pigment and carrier for which the charge amount is to be measured is placed in a metal measurement container 2 with a 500 mesh screen 3 at the bottom, and then the metal lid 4 is placed on the container. The total weight of the measurement container 2 at this point is weighed, and this value is taken as W1 (g). Next, the aspirator 1 (at least the part in contact with the measurement container 102 is an insulator) sucks air from the suction port, and the air flow control valve 6 is adjusted to set the pressure on the vacuum gauge 5 to 250 mmAq. is sufficient, preferably suction is performed for one minute to remove the toner. The potential of the electrometer 9 at this time is V (volts). Here, 8 is a capacitor with a capacity of C (μF). Next, the total weight of the measurement container after suction is weighed and designated as W2 (g). The charge amount (mC / kg) of this toner is calculated using the values ​​measured above according to the following formula: Toner charge (mC / kg) = -(C x V) / (W1-W2) The evaluation criteria are as follows: A: Electrostatic charge of -50mC / kg or less B: Electrostatic charge of -40mC / kg or less -50mC / kg or more C: Electrostatic charge of -30mC / kg or less -40mC / kg or more D: Electrostatic charge of -20mC / kg or less -30mC / kg or more E: Charge amount is over -20mC / kg

[0082] [Table 7]

Claims

1. A toner having toner particles having a toner core particle and a shell present on a surface of the toner core particle, The shell comprises resin A, The toner core particles contain a resin B, The resin A has a structure represented by the following formula (1): The resin B has a structure represented by the following formula (2): The toner, wherein the content of the structure represented by the formula (2) in the resin B is 40% by mass or more and 80% by mass or less. 【Chemistry 1】 [In formula (1), R 1 ~R 3 each independently represents an alkoxy group or a hydroxy group having 1 to 3 carbon atoms. 【Chemistry 2】 [In formula (2), R 4 represents a hydrogen atom or a methyl group, n represents an integer of 17 to 29, X is -COO-* or -OCO-*, and * represents a bond to -(CH 2 ) n CH 3 .]

2. 2. The toner according to claim 1, wherein the X is represented by --COO--*.

3. The toner according to claim 1 or 2, wherein the resin B further has a structure represented by the following formula (3): 【Chemistry 3】

4. The toner according to any one of claims 1 to 3, wherein the weight average molecular weight MwB of the resin B is 15,000 or more and 250,000 or less.

5. The toner according to any one of claims 1 to 4, wherein the content of the resin A in the toner particles is 0.1% by mass to 20.0% by mass.

6. 6. The toner according to claim 1, wherein the content of the resin B in the toner core particles is 50.0% by mass to 95.0% by mass.

7. The toner according to any one of claims 1 to 6, wherein an intensity ratio of silicon ions to a total ion count at a mass number of 0.5 to 1850, obtained when the toner particles are measured using a time-of-flight secondary ion mass spectrometry, is 0.00100 or more and 0.00500 or less.

8. The SP value of the resin A is SPA (J / cm 3 ) 1/2 The SP value of the resin B is SPB (J / cm 3 ) 1/2 When |SPA-SPB|≦1.00 (J / cm 3 ) 1/2 The toner according to any one of claims 1 to 7, wherein

Citation Information

Patent Citations

  • Non-magnetic toner, image forming apparatus and process cartridge

    JP2007279712A

  • toner

    JP2013011884A

  • toner

    JP2014130242A

  • Toner

    JP2015075662A

  • Toner and manufacturing method of toner

    JP2016212387A