Toner for developing electrostatic images

A toner formulation with a binder resin, colorant, and ester compound with a glycerin skeleton addresses the balance of low-temperature fixability, storage stability, and hot offset resistance, effectively suppressing UFPs, enhancing energy efficiency and printing speed in image forming devices.

JP7556356B2Active Publication Date: 2024-09-26ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021549003
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-24
Filing Date
2020-09-24
Publication Date
2024-09-26
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Existing toners fail to balance low-temperature fixability, storage stability, and hot offset resistance while effectively suppressing the generation of ultrafine particles (UFPs), which is crucial for reducing energy consumption and increasing printing speed in image forming devices.

Method used

A toner formulation containing a binder resin, colorant, aromatic vinyl thermoplastic elastomer with unsaturated bonds, and an ester compound with a glycerin skeleton as a mold release agent, optimized through specific polymerization methods to enhance low-temperature fixability, storage stability, and hot offset resistance, while minimizing UFP generation.

Benefits of technology

The toner achieves excellent low-temperature fixability, high storage stability, and effective hot offset resistance, with suppressed UFP generation, meeting energy efficiency and speed demands in image forming devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556356000003
    Figure 0007556356000003
  • Figure 0007556356000002
    Figure 0007556356000002
  • Figure 0007556356000001
    Figure 0007556356000001
Patent Text Reader

Abstract

Provided is an electrostatic image development toner that contains: coloring resin particles that include a binding resin, a colorant, an aromatic vinyl thermoplastic elastomer having an unsaturated bond that is capable of a polymerization reaction, and a mold-release agent; and an external additive, wherein the mold-release agent is an ester compound having a glycerin skeleton.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing electrostatic images, which is used for developing electrostatic latent images in electrophotography, electrostatic recording, electrostatic printing and the like. [Background technology]

[0002] 2. Description of the Related Art Image forming apparatuses such as electrophotographic apparatuses, electrostatic recording apparatuses, and electrostatic printing apparatuses widely employ a method of forming a desired image by developing an electrostatic latent image formed on a photoconductor with a toner for developing an electrostatic image, and this method is applied to copiers, printers, facsimiles, and multifunction machines thereof.

[0003] For example, in an electrophotographic device using electrophotography, the surface of a photoconductor made of a photoconductive material is generally uniformly charged by various means, an electrostatic latent image is then formed on the photoconductor, the electrostatic latent image is then developed using toner (developing process), and if necessary, the toner image is transferred to a recording material such as paper (transfer process), and the toner is then fixed to the recording material by heating or the like (fixing process) to obtain a printed matter.

[0004] Among the image forming processes, in the fixing process, it is usually necessary to heat the fixing roll to 150° C. or higher during fixing, and a large amount of electricity is consumed as an energy source. In response to this, in recent years, with the increasing demand for reducing energy consumption and increasing printing speed for the image forming apparatus, there is a demand for the design of a toner that can maintain a high fixing rate even at a low fixing temperature (a toner with excellent low-temperature fixing ability).

[0005] In response to the above demands, proposals have been made to lower the glass transition temperature (Tg) of the toner, to incorporate a low melting point resin and / or a low molecular weight resin into the toner, and to incorporate a low softening point substance (releasing agent) having releasability (peelability) such as wax into the toner.

[0006] However, while improving low-temperature fixability allows the temperature of the fixing roll to be set lower during fixing, when the toner is used at high temperatures or when the toner is left (stored) for a long period of time, fusion (blocking (aggregation)) between toner particles may occur more easily, and the storage stability of the toner may decrease. For this reason, when designing a toner, it is necessary to take into consideration storage stability, which is a property that is opposed to low-temperature fixability, and to develop a toner that can improve low-temperature fixability without impairing storage stability and reduce power consumption.

[0007] For example, Patent Document 1 discloses a toner for developing electrostatic images, which contains toner particles consisting of at least a binder resin, a colorant, a charge control agent, and a release agent, and the toner particles have a volume average particle size (Dv) of 3 to 10 μm, a ratio (Dv / Dp) of the volume average particle size to the number average particle size (Dp) of 1 to 1.3, and an average circularity of 0.93 to 0.995. The toner particles are embedded in a resin, a slice is cut out, and then a cross-sectional image of the toner particles is photographed with an electron microscope. In the cross-sectional image of the toner particles observed in the photograph, the island-like separated phase has a maximum diameter of 1 μm or more, and the outermost part of the island-like separated phase exists at a depth of 0.01 to 0.15 times the particle size of the toner particles from the surface of the toner particles, and the cross-sectional image of the toner particles is 25% or more by number. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2004-295065 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, although the technique of Patent Document 1 aims to improve storage stability and hot offset resistance by adopting the above-mentioned configuration, the low-temperature fixability is not sufficient. The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a toner for developing electrostatic images which is excellent in low-temperature fixing property, storage stability, and hot offset resistance, and which suppresses the generation of UFP (ultrafine particles). [Means for solving the problem]

[0010] The present inventors have conducted studies to achieve the above object, and have found that in a toner for developing electrostatic images containing colored resin particles including a binder resin, a colorant, and a release agent, and an external additive, by incorporating an aromatic vinyl thermoplastic elastomer having an unsaturated bond capable of polymerization reaction in the colored resin particles and using an ester compound having a glycerin skeleton as the release agent, it is possible to obtain a toner for developing electrostatic images which is excellent in low-temperature fixing property, storage stability, and hot offset resistance and which suppresses the generation of UFP (ultrafine particles), and have thus completed the present invention.

[0011] That is, according to the present invention, there is provided a toner for developing electrostatic images, comprising colored resin particles including a binder resin, a colorant, an aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond, and a release agent, and an external additive, The toner for developing electrostatic images is provided, wherein the release agent is an ester compound having a glycerin skeleton.

[0012] In the toner for developing electrostatic images of the present invention, the ester compound having a glycerin skeleton preferably contains an ester structure of glycerin and a monocarboxylic acid having 16 or more carbon atoms. In the electrostatic image developing toner of the present invention, the content of the aromatic vinyl thermoplastic elastomer is preferably 1 to 10 parts by mass with respect to 100 parts by mass of the binder resin. In the electrostatic image developing toner of the present invention, the content of the release agent is preferably 1 to 30 parts by mass with respect to 100 parts by mass of the binder resin. In the toner for developing electrostatic images of the present invention, the aromatic vinyl thermoplastic elastomer is preferably a block copolymer containing at least one aromatic vinyl polymer block and at least one conjugated diene polymer block. In the toner for developing electrostatic images of the present invention, the aromatic vinyl thermoplastic elastomer is preferably a composition containing an aromatic vinyl-conjugated diene block copolymer and an aromatic vinyl-conjugated diene-aromatic vinyl block copolymer. Effect of the Invention

[0013] According to the present invention, it is possible to provide a toner for developing electrostatic images which is excellent in low-temperature fixing property, storage stability and hot offset resistance, and which suppresses the generation of UFP (ultrafine particles). [Brief description of the drawings]

[0014] [Figure 1] FIG. 1A is a cross-sectional SEM photograph (secondary electron image) of a colored resin particle in Example 1, and FIG. 1B is a cross-sectional SEM photograph (secondary electron image) of a colored resin particle in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The toner for developing electrostatic images of the present invention (hereinafter, may be simply referred to as "toner") contains colored resin particles including a binder resin, a colorant, an aromatic vinyl thermoplastic elastomer having an unsaturated bond capable of polymerization reaction, and a release agent, and an external additive, and an ester compound having a glycerin skeleton is used as the release agent.

[0016] First, a method for producing the colored resin particles constituting the toner of the present invention will be described.

[0017] The manufacturing methods of the colored resin particles constituting the toner of the present invention are roughly divided into dry methods such as a pulverization method, and wet methods such as an emulsion polymerization aggregation method, a dispersion polymerization method, a suspension polymerization method, and a dissolution suspension method, and the wet method is preferred because it is easy to obtain a toner having excellent printing characteristics such as image reproducibility. Among the wet methods, the polymerization methods such as the emulsion polymerization aggregation method, the dispersion polymerization method, and the suspension polymerization method are preferred because it is easy to obtain a toner having a relatively small particle size distribution on the order of microns, and among these, the suspension polymerization method is more preferred.

[0018] The emulsion polymerization aggregation method is a method for producing colored resin particles by polymerizing an emulsified polymerizable monomer to obtain resin fine particles, and aggregating the resin fine particles with a colorant, etc. The dissolution suspension method is a method for producing colored resin particles by dropping a solution in which toner components such as a binder resin and a colorant are dissolved or dispersed in an organic solvent into an aqueous medium to form droplets, and then removing the organic solvent, and each of these methods can be known.

[0019] The colored resin particles constituting the toner of the present invention can be produced by either a wet method or a dry method, but when the colored resin particles are produced by adopting the (A) suspension polymerization method, which is preferable among the wet methods, or the (B) pulverization method, which is representative among the dry methods, the process is as follows. First, the (A) suspension polymerization method will be described.

[0020] (A) Suspension polymerization method (A-1) Preparation of polymerizable monomer composition In the suspension polymerization method, first, a polymerizable monomer, a colorant, an aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond, a release agent, and other additives such as a charge control agent, which are used as necessary, are mixed and dissolved to prepare a polymerizable monomer composition. Mixing in preparing the polymerizable monomer composition is carried out, for example, using a media type disperser.

[0021] In the present invention, the polymerizable monomer refers to a compound that can be polymerized, and the polymerizable monomer becomes a binder resin by polymerization. As the polymerizable monomer, it is preferable to use a monovinyl monomer as a main component constituting the polymerizable monomer. Examples of the monovinyl monomer include styrene-based monomers such as styrene, vinyl toluene, α-methylstyrene, and ethylstyrene; (meth)acrylate-based monomers such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, dimethylaminoethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and dimethylaminoethyl methacrylate; acrylic acid and methacrylic acid; nitrile compounds such as acrylonitrile and methacrylonitrile; amide compounds such as acrylamide and methacrylamide; and olefins such as ethylene, propylene, and butylene. These monovinyl monomers can be used alone or in combination of two or more. Among these, styrene-based monomers and (meth)acrylate-based monomers are preferred, and styrene and butyl acrylate are more preferred. In addition, it is preferred to use at least a styrene-based monomer and a (meth)acrylate-based monomer as the monovinyl monomer, since the low-temperature fixing property of the resulting toner can be further improved.

[0022] The content of the styrene monomer unit in the binder resin used in the present invention is preferably 60% by mass or more, more preferably 65% ​​by mass or more, even more preferably 68% by mass or more, even more preferably 70% by mass or more, and particularly preferably 74% by mass or more, and the upper limit is preferably 85% by mass or less, more preferably 80% by mass or less, and even more preferably 77% by mass or less. The content of the (meth)acrylate monomer unit is preferably 20% by mass or more, more preferably 21% by mass or more, even more preferably 21.5% by mass or more, and particularly preferably 22% by mass or more, and the upper limit is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 28% by mass or less, and particularly preferably 26% by mass or less. By setting the content of the styrene monomer unit and the (meth)acrylate monomer unit in the above range, the toner obtained can be improved in low-temperature fixability while having excellent storage stability.

[0023] In the present invention, in order to improve hot offset and storage stability, it is preferable to use any crosslinkable polymerizable monomer together with the monovinyl monomer. The crosslinkable polymerizable monomer refers to a monomer having two or more polymerizable functional groups. Examples of the crosslinkable polymerizable monomer include aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, and derivatives thereof; ester compounds in which two or more carboxylic acids are ester-bonded to an alcohol having two or more hydroxyl groups, such as ethylene glycol dimethacrylate and diethylene glycol dimethacrylate; other divinyl compounds such as N,N-divinylaniline and divinyl ether; and compounds having three or more vinyl groups. These crosslinkable polymerizable monomers can be used alone or in combination of two or more. The amount of the crosslinkable polymerizable monomer used is preferably 0.1 to 5 parts by mass, more preferably 0.15 to 2 parts by mass, and even more preferably 0.2 to 0.7 parts by mass, relative to 100 parts by mass of the monovinyl monomer, and the content of the crosslinkable polymerizable monomer unit in the binder resin used in the present invention is preferably 0.1 to 5% by mass, more preferably 0.15 to 2% by mass, and even more preferably 0.2 to 0.7% by mass. By setting the amount and content of the crosslinkable polymerizable monomer within the above ranges, the storage stability and low-temperature fixability of the obtained toner can be further improved.

[0024] In addition, when a macromonomer is used as a part of the polymerizable monomer, the storage stability and low-temperature fixability of the obtained toner can be further improved, so it is preferable to use any macromonomer. A macromonomer is a reactive oligomer or polymer having a polymerizable carbon-carbon unsaturated bond at the end of the molecular chain, and usually has a number average molecular weight (Mn) of 1,000 to 30,000. It is preferable that the macromonomer gives a polymer having a higher Tg (glass transition temperature) than the Tg of a polymer obtained without polymerizing the macromonomer. The amount of the macromonomer used is preferably 0.03 to 5 parts by mass, more preferably 0.05 to 1 part by mass, based on 100 parts by mass of the monovinyl monomer.

[0025] In the present invention, a colorant is used, and when producing a color toner (usually, four types of toner are used: black toner, cyan toner, yellow toner, and magenta toner), a black colorant, a cyan colorant, a yellow colorant, and a magenta colorant can be used, respectively.

[0026] As the black colorant, for example, pigments and dyes such as carbon black, titanium black, and magnetic powders such as zinc iron oxide and nickel iron oxide can be used.

[0027] Examples of cyan colorants include copper phthalocyanine pigments, their derivatives, and anthraquinone pigments and dyes. Specific examples include CI Pigment Blue 2, 3, 6, 15, 15:1, 15:2, 15:3, 15:4, 16, 17:1, 60, etc.

[0028] Examples of the yellow colorant include azo pigments such as monoazo pigments and disazo pigments, condensed polycyclic pigments, dyes, and other compounds. Specific examples include CI Pigment Yellow 3, 12, 13, 14, 15, 17, 62, 65, 73, 74, 83, 93, 97, 120, 138, 151, 155, 180, 181, 185, 186, 214, 219, CI Solvent Yellow 98, 162, and the like.

[0029] Examples of magenta colorants include monoazo pigments, azo pigments such as disazo pigments, condensed polycyclic pigments, dyes, and other compounds. Specific examples include CI Pigment Red 31, 48, 57:1, 58, 60, 63, 64, 68, 81, 83, 87, 88, 89, 90, 112, 114, 122, 123, 144, 146, 149, 150, 163, 170, 184, 185, 187, 202, 206, 207, 209, 251, CI Solvent Violet 31, 47, 59, and CI Pigment Violet 19.

[0030] In the present invention, each colorant may be used alone or in combination of two or more kinds, and the amount of the colorant used is preferably 1 to 10 parts by mass based on 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin).

[0031] In the present invention, the colored resin particles contain an aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond. In addition, in the present invention, as described below, an ester compound having a glycerin skeleton is used as a release agent. That is, in the present invention, an aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond and an ester compound having a glycerin skeleton as a release agent are used in combination, thereby achieving the effects described below. That is, by containing an aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond, the polymerization-reactive unsaturated bond reacts with the binder resin, and the aromatic vinyl thermoplastic elastomer, while fixed to the binder resin, interacts with the ester compound having a glycerin skeleton as a release agent. By interacting in this manner, the ester compound having a glycerin skeleton as a release agent can be uniformly finely dispersed (uniformly dispersed in the form of fine particles) in the binder resin constituting the colored resin particles, and thus the effect of improving low-temperature fixability by adding the ester compound having a glycerin skeleton as a release agent can be sufficiently achieved while effectively suppressing blocking of the toner obtained, and as a result, the toner obtained can have excellent storage stability and low-temperature fixability. In addition, according to the present invention, by using an ester compound having a glycerin skeleton as a release agent, the action of the ester compound having a glycerin skeleton can make the toner obtained excellent in storage stability and low-temperature fixability, as well as excellent hot offset resistance, and the generation of UFP (ultrafine particles) can be effectively suppressed.

[0032] In the present invention, the term "aromatic vinyl thermoplastic elastomer" refers to a random, block, graft, or other copolymer of an aromatic vinyl monomer and another monomer that can be copolymerized with the aromatic vinyl monomer, and a hydrogenated product of such a copolymer. The term "polymerizable unsaturated bond" refers to an unsaturated bond having polymerization activity, and preferably includes an olefinic carbon-carbon double bond having polymerization activity. The method of introducing an olefinic carbon-carbon double bond having polymerization activity into an aromatic vinyl thermoplastic elastomer is not particularly limited, but may include, for example, a method of using a conjugated diene monomer as another monomer that can be copolymerized with an aromatic vinyl monomer.

[0033] The aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond used in the present invention is not particularly limited, but from the viewpoint of further improving the storage stability and low-temperature fixing property of the toner, a block copolymer containing at least one aromatic vinyl polymer block and at least one conjugated diene polymer block is preferred.

[0034] Hereinafter, a block copolymer containing at least one aromatic vinyl polymer block and at least one conjugated diene polymer block (hereinafter, sometimes simply referred to as "block copolymer"), which is a representative example of an aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond, will be described. The block copolymer used in the present invention contains at least one aromatic vinyl polymer block obtained by polymerizing an aromatic vinyl monomer and at least one conjugated diene polymer block obtained by polymerizing a conjugated diene monomer.

[0035] The aromatic vinyl monomer is not particularly limited as long as it is an aromatic vinyl compound, and examples thereof include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 4-bromostyrene, 2-methyl-4,6-dichlorostyrene, 2,4-dibromostyrene, and vinylnaphthalene. Among these, it is preferable to use styrene. These aromatic vinyl monomers can be used alone or in combination of two or more in each aromatic vinyl polymer block. In addition, when the block copolymer has a plurality of aromatic vinyl polymer blocks, each aromatic vinyl polymer block may be composed of the same aromatic vinyl monomer unit or may be composed of different aromatic vinyl monomer units.

[0036] The aromatic vinyl polymer block may contain other monomer units as long as the aromatic vinyl monomer unit is the main repeating unit. Examples of other monomers that can be used in the aromatic vinyl polymer block include conjugated diene monomers such as 1,3-butadiene and isoprene (2-methyl-1,3-butadiene), α,β-unsaturated nitrile monomers, unsaturated carboxylic acid or acid anhydride monomers, unsaturated carboxylic acid ester monomers, and non-conjugated diene monomers. The content of monomer units other than aromatic vinyl monomer units in the aromatic vinyl polymer block is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.

[0037] The conjugated diene monomer is not particularly limited as long as it is a conjugated diene compound, and examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. Among these, it is preferable to use 1,3-butadiene and / or isoprene, and it is particularly preferable to use isoprene, from the viewpoint of high effect of improving storage stability and low-temperature fixability by introducing unsaturated bonds capable of polymerization reaction. These conjugated diene monomers can be used alone or in combination of two or more in each conjugated diene polymer block. In addition, when the block copolymer has a plurality of conjugated diene polymer blocks, each conjugated diene polymer block may be composed of the same conjugated diene monomer unit or may be composed of different conjugated diene monomer units. Furthermore, a hydrogenation reaction may be performed on a part of the unsaturated bonds of each conjugated diene polymer block.

[0038] The conjugated diene polymer block may contain other monomer units as long as the conjugated diene monomer unit is the main repeating unit. Examples of other monomers that can be used in the conjugated diene polymer block include aromatic vinyl monomers such as styrene and α-methylstyrene, α,β-unsaturated nitrile monomers, unsaturated carboxylic acid monomers, unsaturated carboxylic anhydride monomers, unsaturated carboxylic ester monomers, and non-conjugated diene monomers. The content of monomer units other than the conjugated diene monomer units in the conjugated diene polymer block is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.

[0039] The vinyl bond content of the conjugated diene polymer block (the ratio of 1,2-vinyl bond units and 3,4-vinyl bond units to all conjugated diene monomer units in the conjugated diene polymer block) is not particularly limited, but is preferably 1 to 20 mol%, more preferably 2 to 15 mol%, and particularly preferably 3 to 10 mol%.

[0040] The block copolymer is not particularly limited in the number of each polymer block and the bonding form thereof, so long as it contains at least one aromatic vinyl polymer block and at least one conjugated diene polymer block. Specific examples of the block copolymer used in the present invention include the following. In the following specific examples, Ar represents an aromatic vinyl polymer block, D represents a conjugated diene polymer block, X represents a residue of a coupling agent, and n represents an integer of 2 or more. (a) Aromatic vinyl-conjugated diene block copolymer represented as Ar-D (b) Aromatic vinyl-conjugated diene-aromatic vinyl block copolymers represented as Ar-D-Ar and / or (Ar-D)nX (c) conjugated diene-vinyl aromatic-conjugated diene block copolymers represented as D-Ar-D and / or (D-Ar)nX (d) Aromatic vinyl-conjugated diene-aromatic vinyl-conjugated diene block copolymer represented as Ar-D-Ar-D (e) A block copolymer composition comprising any combination of two or more of the above (a) to (d).

[0041] In the present invention, it is preferable to use, as the block copolymer, one containing at least the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D, and it is more preferable to use one containing at least the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D and the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by (b) Ar-D-Ar and / or (Ar-D)X.

[0042] In the aromatic vinyl-conjugated diene block copolymer represented by Ar-D, the weight average molecular weight (Mw(Ar)) of the aromatic vinyl polymer block Ar is not particularly limited, but is preferably 10,000 to 50,000, more preferably 15,000 to 30,000, and the weight average molecular weight (Mw(D)) of the conjugated diene polymer block D is not particularly limited, but is preferably 50,000 to 200,000, more preferably 60,000 to 150,000.

[0043] In the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by Ar-D-Ar and / or (Ar-D)nX, the weight average molecular weight (Mw(Ar)) of the aromatic vinyl polymer block Ar is not particularly limited, but is preferably 15,000 to 70,000, more preferably 16,000 to 50,000, and the weight average molecular weight (Mw(D)) of the conjugated diene polymer block D is not particularly limited, but is preferably 100,000 to 300,000, more preferably 120,000 to 250,000. The weight average molecular weights are all values ​​calculated as polystyrene equivalents measured by gel permeation chromatography (GPC) using tetrahydrofuran.

[0044] In the block copolymer used in the present invention, the content ratio of aromatic vinyl monomer units to all monomer units is preferably 10 to 30% by mass, more preferably 12 to 25% by mass, and even more preferably 15% by mass or more and less than 25% by mass. By setting the content ratio of aromatic vinyl monomer units within the above range, it is possible to highly balance the affinity of the block copolymer to the release agent and the affinity of the block copolymer to the binder resin, and thus the obtained toner can have excellent storage stability and low-temperature fixability.

[0045] In the case where all polymer components constituting the block copolymer are composed only of aromatic vinyl monomer units and conjugated diene monomer units, the content of aromatic vinyl monomer units in the block copolymer can be easily measured by subjecting the block copolymer to ozonolysis and then reduction with lithium aluminum hydride according to the method described in Rubber Chem. Technol., 45, 1295 (1972), whereby the conjugated diene monomer unit portion is decomposed and only the aromatic vinyl monomer unit portion can be isolated, so that the total aromatic vinyl monomer unit content can be easily measured.

[0046] The weight average molecular weight (Mw) of the aromatic vinyl monomer unit in the block copolymer is not particularly limited, but is preferably 10,000 to 50,000, more preferably 15,000 to 40,000, in terms of polystyrene measured by gel permeation chromatography (GPC) using tetrahydrofuran. The weight average molecular weight (Mw) of the conjugated diene monomer unit in the block copolymer is not particularly limited, but is preferably 50,000 to 200,000, more preferably 60,000 to 180,000.

[0047] The melt index (MI) of the block copolymer is not particularly limited, but is selected, for example, from the range of 1 to 1000 g / 10 min, and preferably from 5 to 30 g / 10 min, as a value measured in accordance with ASTM D-1238 (G condition, 200° C., 5 kg).

[0048] The block copolymer used in the present invention can be produced by a conventional method. For example, a method of producing such a block copolymer includes a method of sequentially polymerizing an aromatic vinyl monomer and a conjugated diene monomer by an anionic living polymerization method to form a polymer block, and then reacting a coupling agent to perform coupling, if necessary.

[0049] In addition, when the block copolymer used in the present invention contains at least the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D and the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by (b) Ar-D-Ar and / or (Ar-D)X, the following method can be adopted.

[0050] That is, first, an aromatic vinyl monomer is polymerized by an anionic living polymerization method, and then a conjugated diene monomer is added and polymerized to obtain a diblock copolymer having an active end. Next, a coupling agent less than 1 molar equivalent is added to the active end of the diblock copolymer having an active end, and a part of the diblock copolymer having an active end is subjected to a coupling reaction to obtain an aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented as (Ar-D)nX, and then a polymerization terminator is added to inactivate the remaining diblock copolymer having an active end to obtain a diblock copolymer represented as Ar-D. In this case, a bifunctional coupling agent such as dichlorosilane, monomethyldichlorosilane, dimethyldichlorosilane, diphenyldimethoxysilane, diphenyldiethoxysilane, dichloroethane, dibromoethane, methylene chloride, and dibromomethane can be used as the coupling agent to obtain an aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented as Ar-D-Ar (D includes a residue of the coupling agent).

[0051] In the present invention, the content ratio of the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D and the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by (b) Ar-D-Ar and / or (Ar-D)nX is not particularly limited, but the content ratio of the aromatic vinyl-conjugated diene block copolymer represented by (a) Ar-D is preferably 10 to 90 mass%, more preferably 20 to 80 mass%. Also, the content ratio of the aromatic vinyl-conjugated diene-aromatic vinyl block copolymer represented by (b) Ar-D-Ar and / or (Ar-D)nX is preferably 10 to 90 mass%, more preferably 20 to 80 mass%.

[0052] The weight average molecular weight (Mw) of the aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond used in the present invention is not particularly limited, but is preferably 60,000 to 350,000, more preferably 80,000 to 250,000, in terms of polystyrene measured by gel permeation chromatography (GPC) using tetrahydrofuran. By setting the weight average molecular weight (Mw) within the above range, the storage stability and low-temperature fixability of the obtained toner can be further improved.

[0053] The content of the aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond is preferably 1 to 10 parts by mass, more preferably 1.5 to 8 parts by mass, and even more preferably 2 to 5 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin). By setting the content of the aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond within the above range, the effect of adding the elastomer, i.e., the effect of improving the storage stability and low-temperature fixability of the toner obtained, can be further enhanced.

[0054] In the present invention, the toner contains an ester compound having a glycerin skeleton as a release agent. By using an ester compound having a glycerin skeleton as a release agent, the toner can have excellent storage stability and low-temperature fixing property due to the interaction with the aromatic vinyl thermoplastic elastomer described above, and in addition, the hot offset resistance can be improved, and the generation of UFP (ultrafine particles) can be effectively suppressed. In particular, in the present invention, the toner contains an ester compound having a glycerin skeleton as a release agent, and the ester compound having a glycerin skeleton as a release agent can be uniformly finely dispersed (uniformly dispersed in the form of extremely fine particles) in the binder resin constituting the colored resin particles due to the interaction with the aromatic vinyl thermoplastic elastomer described above. As a result, the toner obtained can have excellent storage stability and low-temperature fixing property, as well as excellent hot offset resistance, and the generation of UFP (ultrafine particles) can be effectively suppressed.

[0055] The ester compound having a glycerin skeleton used in the present invention is not particularly limited as long as it has a glycerin skeleton, and is sufficient as long as it has at least one ester structure composed of glycerin and a carboxylic acid. Any of a monoester of glycerin, a diester of glycerin, and a triester of glycerin may be used, but a triester of glycerin is preferred from the viewpoint of being able to further enhance the effect of adding the compound.

[0056] In addition, the carboxylic acid for forming an ester bond with glycerin to form an ester structure is not particularly limited, and examples thereof include monocarboxylic acids, polycarboxylic acids such as dicarboxylic acids, and monoesters of polycarboxylic acids such as dicarboxylic acid monoesters. Monocarboxylic acids having 16 or more carbon atoms are preferred, and monocarboxylic acids having 16 to 30 carbon atoms are more preferred.

[0057] The monocarboxylic acid having 16 or more carbon atoms is not particularly limited, but is preferably a saturated fatty acid and / or an unsaturated fatty acid having 16 or more carbon atoms.

[0058] Examples of saturated fatty acids having 16 or more carbon atoms include palmitic acid (16 carbon atoms), margaric acid (17 carbon atoms), stearic acid (18 carbon atoms), arachidic acid (20 carbon atoms), behenic acid (22 carbon atoms), lignoceric acid (24 carbon atoms), cerotic acid (26 carbon atoms), montanic acid (28 carbon atoms), melissic acid (30 carbon atoms), etc. Among these saturated fatty acids, palmitic acid (16 carbon atoms), stearic acid (18 carbon atoms), and behenic acid (22 carbon atoms) are preferred, and stearic acid (18 carbon atoms) is more preferred.

[0059] Specific examples of unsaturated fatty acids having 16 or more carbon atoms include, but are not limited to, the following compounds: Palmitoleic acid (CH3(CH2)5CH=CH(CH2)7COOH) Oleic acid (CH3(CH2)7CH=CH(CH2)7COOH) Vaccenic acid (CH3(CH2)5CH=CH(CH2)9COOH) Linoleic acid (CH3(CH2)3(CH2CH=CH)2(CH2)7COOH) (9,12,15)-Linolenic acid (CH3(CH2CH=CH)3(CH2)7COOH) (6,9,12)-Linolenic acid (CH3(CH2)3(CH2CH=CH)3(CH2)4COOH) Eleostearic acid (CH3(CH2)3(CH=CH)3(CH2)7COOH) Arachidonic acid (CH3(CH2)3(CH2CH=CH)4(CH2)3COOH)

[0060] The ester compound having a glycerin skeleton used in the present invention can be produced according to a conventional method. For example, a method of producing an ester compound having a glycerin skeleton includes a method of carrying out an ester reaction using glycerin and a carboxylic acid. In this case, two or more carboxylic acids may be used in combination as the carboxylic acid, thereby forming a compound in which two or more carboxylic acids are ester-bonded to glycerin.

[0061] Specific examples of ester compounds having a glycerin skeleton include palmitic acid triglyceride, margaric acid triglyceride, stearic acid triglyceride, arachidic acid triglyceride, behenic acid triglyceride, lignoceric acid triglyceride, cerotic acid triglyceride, montanic acid triglyceride, melissic acid triglyceride, palmitoleic acid triglyceride, oleic acid triglyceride, vaccenic acid triglyceride, linoleic acid triglyceride, (9,12,15)-linolenic acid triglyceride, (6,9,12)-linolenic acid triglyceride, eleostearic acid triglyceride, and arachidonic acid triglyceride. The ester compounds having a glycerin skeleton may be used alone or in combination of two or more. Among these, palmitic acid triglyceride, stearic acid triglyceride, and behenic acid triglyceride are preferred, and behenic acid triglyceride is more preferred.

[0062] From the viewpoint of further improving the low-temperature fixing property of the toner obtained, the ester compound having a glycerin skeleton used in the present invention preferably has a number average molecular weight (Mn) of 500 to 1500, more preferably 550 to 1200, and even more preferably 550 to 1100. The number average molecular weight (Mn) of the ester compound having a glycerin skeleton can be measured, for example, in terms of polystyrene, by gel permeation chromatography (GPC) using tetrahydrofuran.

[0063] The content of the ester compound having a glycerin skeleton as a releasing agent is preferably 1 to 30 parts by mass, more preferably 8 to 28 parts by mass, further preferably 12 to 25 parts by mass, and particularly preferably 17 to 23 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin). By setting the content of the ester compound having a glycerin skeleton as a releasing agent within the above range, it is possible to further improve low-temperature fixability while making the particle size distribution of the obtained toner relatively uniform.

[0064] In the present invention, a release agent other than an ester compound having a glycerin skeleton may be used together with the above-mentioned ester compound having a glycerin skeleton as the release agent, and examples of such release agents include low molecular weight polyolefin waxes and modified waxes thereof, natural plant waxes such as jojoba, petroleum waxes such as paraffin, mineral waxes such as ozokerite, synthetic waxes such as Fischer-Tropsch wax, polyhydric alcohol esters such as dipentaerythritol esters, etc. These may be used alone or in combination of two or more.

[0065] In the present invention, an acrylic resin can be used as another additive in order to further suppress bleeding out of the release agent. The acrylic resin is a copolymer (acrylate copolymer) mainly composed of at least one of an acrylic acid ester and a methacrylic acid ester and at least one of an acrylic acid and a methacrylic acid. The acid monomer is preferably acrylic acid.

[0066] Examples of the acrylic resin include copolymers of an acrylic acid ester and acrylic acid, copolymers of an acrylic acid ester and methacrylic acid, copolymers of a methacrylic acid ester and acrylic acid, copolymers of a methacrylic acid ester and methacrylic acid, copolymers of an acrylic acid ester, a methacrylic acid ester and acrylic acid, copolymers of an acrylic acid ester, a methacrylic acid ester and methacrylic acid, and copolymers of an acrylic acid ester, a methacrylic acid ester, an acrylic acid and a methacrylic acid. Of these, it is preferable to use a copolymer of an acrylic acid ester, a methacrylic acid ester and acrylic acid.

[0067] The acid value of the acrylic resin is usually 0.5 to 7 mgKOH / g, preferably 1 to 6 mgKOH / g, and more preferably 1.5 to 4 mgKOH / g. By setting the acid value of the acrylic resin within the above range, it is possible to satisfactorily prepare desired colored resin particles, while improving heat-resistant storage stability, low-temperature fixability, and print durability under temperature and humidity environments ranging from low-temperature and low-humidity environments to high-temperature and high-humidity environments. The acid value of the acrylic resin is a value measured in accordance with JIS K 0070, a standard method for analyzing fats and oils established by the Japanese Industrial Standards Committee (JICS).

[0068] The weight average molecular weight (Mw) of the acrylic resin is usually from 6,000 to 50,000, preferably from 8,000 to 25,000, and more preferably from 10,000 to 20,000. When the weight average molecular weight (Mw) of the acrylic resin is within the above range, the heat-resistant storage stability, durability, and low-temperature fixability can be improved.

[0069] The glass transition temperature Tg of the acrylic resin is usually 60 to 85° C., preferably 65 to 80° C., and more preferably 70 to 77° C. When the glass transition temperature is in the above range, the heat-resistant storage stability and low-temperature fixability can be improved. The glass transition temperature Tg of the acrylic resin can be determined, for example, in accordance with ASTM D3418-82.

[0070] The ratio of the acrylic acid ester monomer units, the methacrylic acid ester monomer units, the acrylic acid monomer units, and the methacrylic acid monomer units in the acrylic resin is not particularly limited as long as the above-mentioned acid value, weight average molecular weight Mw, and glass transition temperature are satisfied.

[0071] The ratio of the above four types of monomer units can be adjusted by the mass ratio of the amounts of acrylic acid ester, methacrylic acid ester, acrylic acid, and methacrylic acid added during copolymer synthesis. The mass ratio of the amounts added may be, for example, (acrylic acid ester and / or methacrylic acid ester):(acrylic acid and / or methacrylic acid)=(99-99.95):(0.05-1), preferably (acrylic acid ester and / or methacrylic acid ester):(acrylic acid and / or methacrylic acid)=(99.4-99.9):(0.1-0.6), and more preferably (acrylic acid ester and / or methacrylic acid ester):(acrylic acid and / or methacrylic acid)=(99.5-99.7):(0.3-0.5). Among these polymerizable monomers, the acrylic acid esters and / or methacrylic acid esters may be substituted with other monomers such as styrene derivatives, nitrile compounds, and amide compounds exemplified as the monovinyl monomers constituting the binder resin described above, within the scope that does not impair the effects of the present invention. The proportion of such monomers is 10% by mass or less, preferably 2% by mass or less, of the total amount of the acrylic acid esters and / or methacrylic acid esters added, and it is preferable that they are not substituted.

[0072] Examples of acrylic esters used in the acrylic resin include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-pentyl acrylate, sec-pentyl acrylate, isopentyl acrylate, neopentyl acrylate, n-hexyl acrylate, isohexyl acrylate, neohexyl acrylate, sec-hexyl acrylate, and tert-hexyl acrylate, and among these, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, and n-butyl acrylate are preferred, and n-butyl acrylate is more preferred.

[0073] Examples of methacrylic acid esters used in acrylic resins include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, n-pentyl methacrylate, sec-pentyl methacrylate, isopentyl methacrylate, neopentyl methacrylate, n-hexyl methacrylate, isohexyl methacrylate, neohexyl methacrylate, sec-hexyl methacrylate, and tert-hexyl methacrylate, and among these, methyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, and n-butyl methacrylate are preferred, and methyl methacrylate is more preferred.

[0074] The amount of the acrylic resin added is preferably 0.3 to 4 parts by mass, more preferably 0.5 to 3.0 parts by mass, and even more preferably 0.7 to 2.0 parts by mass, per 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin). By setting the amount of the acrylic resin added within the above range, it is possible to ensure a sufficient effect of the addition while ensuring good environmental stability.

[0075] Although commercially available acrylic resins can be used, the acrylic resins can be produced by known methods such as solution polymerization, aqueous solution polymerization, ionic polymerization, high-temperature high-pressure polymerization, and suspension polymerization.

[0076] In the present invention, a positively or negatively chargeable charge control agent can be used as another additive in order to improve the chargeability of the toner. The charge control agent is not particularly limited as long as it is one that is generally used as a charge control agent for toners. Among the charge control agents, positively or negatively charged charge control resins are preferred from the viewpoint of having high compatibility with polymerizable monomers and being able to impart stable chargeability (charge stability) to toner particles, thereby improving the dispersibility of the colorant. Furthermore, from the viewpoint of obtaining a negatively charged toner, negatively charged charge control resins are more preferably used.

[0077] Positively charged charge control agents include nigrosine dyes, quaternary ammonium salts, triaminotriphenylmethane compounds, and imidazole compounds, as well as polyamine resins, quaternary ammonium group-containing copolymers, and quaternary ammonium base-containing copolymers, which are preferably used as charge control resins.

[0078] Examples of negatively chargeable charge control agents include azo dyes containing metals such as Cr, Co, Al, and Fe, metal salicylate compounds, and metal alkylsalicylate compounds, as well as sulfonic acid group-containing copolymers, sulfonate salt group-containing copolymers, carboxylate group-containing copolymers, and carboxylate salt group-containing copolymers, which are preferably used as charge control resins.

[0079] The weight average molecular weight (Mw) of the charge control resin is in the range of 5,000 to 30,000, preferably in the range of 8,000 to 25,000, and more preferably in the range of 10,000 to 20,000, in terms of polystyrene, measured by gel permeation chromatography (GPC) using tetrahydrofuran.

[0080] Furthermore, the copolymerization ratio of the monomer having a functional group such as a quaternary ammonium group or a sulfonate group in the charge control resin is preferably within the range of 0.5 to 12 mass%, more preferably within the range of 1.0 to 6 mass%, and even more preferably within the range of 1.5 to 3 mass%.

[0081] The content of the charge control agent is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 8 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin). By setting the amount of the charge control agent added within the above range, it is possible to effectively suppress the occurrence of fog and print stains while appropriately increasing the dispersibility of the colorant.

[0082] Furthermore, a molecular weight regulator may be used as another additive. The molecular weight regulator is not particularly limited as long as it is generally used as a molecular weight regulator for toners, and examples thereof include mercaptans such as t-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, and 2,2,4,6,6-pentamethylheptane-4-thiol; and thiuram disulfides such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, N,N'-dimethyl-N,N'-diphenylthiuram disulfide, and N,N'-dioctadecyl-N,N'-diisopropylthiuram disulfide. These molecular weight regulators may be used alone or in combination of two or more kinds. The amount of the molecular weight regulator used is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin).

[0083] (A-2) Suspension step for obtaining a suspension (droplet formation step) Next, the polymerizable monomer composition obtained by the above (A-1) preparation step of the polymerizable monomer composition, which includes the polymerizable monomer, the colorant, the aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond, and the ester compound having a glycerin skeleton as a mold release agent, is dispersed in an aqueous dispersion medium, a polymerization initiator is added, and then droplets of the polymerizable monomer composition are formed. Here, the suspension means that droplets of the polymerizable monomer composition are formed in an aqueous dispersion medium. The dispersion process for forming droplets can be performed using a device capable of strong stirring, such as an in-line type emulsifying and dispersing machine (manufactured by Pacific Machinery Works, product name: Milder) or a high-speed emulsifying and dispersing machine (manufactured by Primix Corporation, product name: TK Homomixer MARK II type).

[0084] Examples of the polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; azo compounds such as 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide), 2,2'-azobis(2-amidinopropane)dihydrochloride, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobisisobutyronitrile; and organic peroxides such as di-t-butyl peroxide, benzoyl peroxide, t-butylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylbutanoate, diisopropylperoxydicarbonate, di-t-butylperoxyisophthalate, and t-butylperoxyisobutyrate. These can be used alone or in combination of two or more. Among these, organic peroxides are preferred because they can reduce the amount of residual polymerizable monomers and have excellent print durability. Among organic peroxides, peroxyesters are preferred because they have good initiator efficiency and can reduce the amount of residual polymerizable monomers, and non-aromatic peroxyesters, i.e., peroxyesters without an aromatic ring, are more preferred.

[0085] As described above, the polymerization initiator may be added after the polymerizable monomer composition is dispersed in an aqueous medium and before droplets are formed, or may be added to the polymerizable monomer composition before it is dispersed in an aqueous medium (a medium mainly composed of water).

[0086] The amount of the polymerization initiator used for polymerization of the polymerizable monomer composition is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, and particularly preferably 1 to 10 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin).

[0087] In the present invention, it is preferable to add a dispersion stabilizer to the aqueous medium. Examples of the dispersion stabilizer include inorganic compounds such as sulfates such as barium sulfate and calcium sulfate; carbonates such as barium carbonate, calcium carbonate, and magnesium carbonate; phosphates such as calcium phosphate; metal oxides such as aluminum oxide and titanium oxide; metal hydroxides such as aluminum hydroxide, magnesium hydroxide, and ferric hydroxide; and organic compounds such as water-soluble polymers such as polyvinyl alcohol, methyl cellulose, and gelatin; anionic surfactants; nonionic surfactants; and amphoteric surfactants. The dispersion stabilizers can be used alone or in combination of two or more. The amount of the dispersion stabilizer added is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 10 parts by mass, relative to 100 parts by mass of the binder resin (100 parts by mass of the polymerizable monomer for obtaining the binder resin).

[0088] Among the above dispersion stabilizers, inorganic compounds, particularly colloids of poorly water-soluble metal hydroxides, are preferred. By using an inorganic compound, particularly colloids of poorly water-soluble metal hydroxides, the particle size distribution of the colored resin particles can be narrowed and the amount of the dispersion stabilizer remaining after washing can be reduced, so that the environmental stability is not deteriorated and the reproduction of images by the obtained toner can be made clearer.

[0089] (A-3) Polymerization process The desired suspension (aqueous dispersion medium containing droplets of the polymerizable monomer composition) obtained in the above (A-2) step of obtaining a suspension (droplet forming step) is heated to initiate polymerization, thereby obtaining an aqueous dispersion of colored resin particles containing a binder resin, a colorant, an aromatic vinyl thermoplastic elastomer having an unsaturated bond capable of polymerization, and an ester compound having a glycerin skeleton as a release agent.

[0090] The polymerization temperature in the present invention is preferably 50° C. or higher, and more preferably from 60 to 95° C. The polymerization time in the present invention is preferably from 1 to 20 hours, and more preferably from 2 to 15 hours.

[0091] From the viewpoint of carrying out polymerization in a state in which droplets of the polymerizable monomer composition are stably dispersed, in the polymerization step, following the step of obtaining the suspension (A-2) (droplet formation step), the polymerization reaction may be allowed to proceed while carrying out a dispersion treatment by stirring.

[0092] In the present invention, the thus obtained colored resin particles may be used as a toner by adding an external additive as it is, but the colored resin particles obtained by the polymerization process may be used as a core layer, and a shell layer different from the core layer may be formed on the outside of the core layer to obtain so-called core-shell type (also called "capsule type") colored resin particles. The core-shell type colored resin particles can further improve the storage stability and low-temperature fixability of the obtained toner by covering the core layer made of a material with a low softening point with a material with a higher softening point.

[0093] The method for producing the core-shell type colored resin particles is not particularly limited and may be any conventionally known method, but in situ polymerization method or phase separation method is preferred from the viewpoint of production efficiency.

[0094] A method for producing core-shell type colored resin particles by in situ polymerization will be described below. In the in situ polymerization method, a polymerizable monomer for forming a shell layer (polymerizable monomer for shell) and a polymerization initiator for the shell are added to an aqueous dispersion medium in which colored resin particles are dispersed, and polymerization is carried out to obtain core-shell type colored resin particles.

[0095] As the polymerizable monomer for the shell, the same polymerizable monomers as those mentioned above can be used. Among them, it is preferable to use a monomer that can give a polymer with a Tg of more than 80° C., such as styrene or methyl methacrylate, either alone or in combination of two or more kinds.

[0096] Examples of the polymerization initiator for the shell used in the polymerization of the polymerizable monomer for the shell include metal persulfates such as potassium persulfate and ammonium persulfate; and water-soluble azo compounds such as 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide) and 2,2'-azobis-(2-methyl-N-(1,1-bis(hydroxymethyl)2-hydroxyethyl)propionamide). The amount of the polymerization initiator for the shell used is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the polymerizable monomer for the shell.

[0097] The polymerization temperature for the shell layer is preferably 50° C. or higher, more preferably 60 to 95° C. The polymerization time for the shell layer is preferably 1 to 20 hours, more preferably 2 to 15 hours.

[0098] (A-4) Washing, filtering, dehydrating, and drying steps After the polymerization is completed, the aqueous dispersion of colored resin particles obtained in the above polymerization step (A-3) is preferably subjected to a series of operations of washing, filtering, dehydrating, and drying in a conventional manner, and if necessary, repeated several times.

[0099] First, in order to remove the dispersion stabilizer remaining in the aqueous dispersion of the colored resin particles, it is preferable to add an acid or an alkali to the aqueous dispersion of the colored resin particles and wash it. When the dispersion stabilizer used is an inorganic compound soluble in acid, it is preferable to add an acid to the aqueous dispersion of the colored resin particles and wash it, while when the dispersion stabilizer used is an inorganic compound soluble in alkali, it is preferable to add an alkali to the aqueous dispersion of the colored resin particles and wash it.

[0100] Furthermore, when an acid-soluble inorganic compound is used as the dispersion stabilizer, it is preferable to add an acid to the aqueous dispersion of the colored resin particles to adjust the pH to preferably 6.5 or less, more preferably 6 or less. The acid to be added may be an inorganic acid such as sulfuric acid, hydrochloric acid, or nitric acid, or an organic acid such as formic acid or acetic acid, but sulfuric acid is particularly preferable because it has a high efficiency of removing the dispersion stabilizer and places a small burden on the production equipment.

[0101] The dehydration and filtration methods can be any of various known methods, and are not particularly limited. For example, centrifugal filtration, vacuum filtration, pressure filtration, etc. The drying method is also not particularly limited, and various methods can be used.

[0102] (B) Crushing method When the colored resin particles are produced by the pulverization method, the process is as follows. First, the binder resin, the colorant, the aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond, the ester compound having a glycerin skeleton as a release agent, and other additives such as a charge control agent added as necessary are mixed using a mixer such as a ball mill, a V-type mixer, a Henschel mixer (trade name), a high-speed dissolver, an internal mixer, a Forberg, etc. Next, the mixture obtained above is kneaded while heating using a pressure kneader, a twin-screw extrusion kneader, a roller, etc. The kneaded product obtained is coarsely pulverized using a pulverizer such as a hammer mill, a cutter mill, a roller mill, etc. Furthermore, after finely pulverizing using a pulverizer such as a jet mill or a high-speed rotary pulverizer, the particles are classified into the desired particle size using a classifier such as an air classifier or an airflow classifier, and colored resin particles can be obtained by a pulverization method.

[0103] The binder resin, colorant, aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond, and ester compound having a glycerin skeleton as a release agent used in the pulverization method, as well as other additives such as a charge control agent added as needed, may be the same as those listed in the (A) suspension polymerization method. The colored resin particles obtained by the pulverization method may also be made into core-shell type colored resin particles by a method such as in situ polymerization, like the colored resin particles obtained by the (A) suspension polymerization method.

[0104] In addition to the above-mentioned binder resins, resins that have been widely used in toners can be used as the binder resin. Specific examples of the binder resin used in the pulverization method include polystyrene, styrene-butyl acrylate copolymer, polyester resin, and epoxy resin.

[0105] (Colored resin particles) The colored resin particles can be obtained by the above-mentioned (A) suspension polymerization method or (B) pulverization method. The colored resin particles constituting the toner will be described below. The colored resin particles described below include both core-shell type and non-core-shell type particles.

[0106] From the viewpoint of image reproducibility, the volume average particle diameter Dv of the colored resin particles is preferably 3 to 15 μm, more preferably 4 to 12 μm, and further preferably 5 to 8 μm. If the volume average particle diameter Dv of the colored resin particles is less than the above range, the toner fluidity may decrease, and deterioration of image quality due to fogging or the like may easily occur. On the other hand, if the volume average particle diameter Dv of the colored resin particles exceeds the above range, the resolution of the obtained image may decrease.

[0107] In addition, the particle size distribution (Dv / Dn), which is the ratio of the volume average particle size (Dv) to the number average particle size (Dn) of the colored resin particles, is preferably 1.00 to 1.30, more preferably 1.00 to 1.20, from the viewpoint of image reproducibility. If the particle size distribution (Dv / Dn) of the colored resin particles exceeds the above range, the fluidity of the toner may decrease, and image quality may be easily deteriorated due to fogging or the like. The volume average particle size Dv and number average particle size Dn of the colored resin particles can be measured, for example, using a particle size analyzer (manufactured by Beckman Coulter, product name: Multisizer) or the like.

[0108] Moreover, the average circularity of the above-mentioned colored resin particles is preferably from 0.960 to 1.000, more preferably from 0.970 to 1.000, and even more preferably from 0.980 to 1.000, from the viewpoint of image reproducibility.

[0109] In addition, from the viewpoint of improving hot offset resistance and low-temperature fixability, the gel content (amount insoluble in tetrahydrofuran) of the above-mentioned colored resin particles is preferably 1 to 50% by weight, more preferably 5 to 47% by weight, even more preferably 10 to 45% by weight, and particularly preferably 15 to 40% by weight.

[0110] The weight average molecular weight (Mw) of the above-mentioned colored resin particles is preferably 20,000 to 200,000, more preferably 30,000 to 180,000, further preferably 35,000 to 150,000, and particularly preferably 40,000 to 90,000.

[0111] The above-mentioned colored resin particles may be used as a toner as is or by mixing the colored resin particles with carrier particles (ferrite, iron powder, etc.). In order to adjust the chargeability, fluidity, storage stability, etc. of the toner, an external additive may be added and mixed into the colored resin particles using a high-speed mixer (for example, FM Mixer (product name, manufactured by Nippon Coke & Engineering Co., Ltd.)) to form a one-component toner, or the colored resin particles, an external additive, and carrier particles may be mixed to form a two-component toner.

[0112] The agitator used for the external addition treatment is not particularly limited as long as it is a stirring device that can adhere an external additive to the surface of the colored resin particles, and the external addition treatment can be performed using an agitator capable of mixing and stirring, such as FM Mixer (product name, manufactured by Nippon Coke and Engineering Co., Ltd.), Super Mixer (product name, manufactured by Kawada Manufacturing Co., Ltd.), Q Mixer (product name, manufactured by Nippon Coke and Engineering Co., Ltd.), Mechanofusion System (product name, manufactured by Hosokawa Micron Corporation), or Mechano Mill (product name, manufactured by Okada Seiko Co., Ltd.).

[0113] Examples of the external additive include inorganic fine particles made of silica, titanium oxide, aluminum oxide, zinc oxide, tin oxide, calcium carbonate, calcium phosphate, and cerium oxide; and organic fine particles made of polymethyl methacrylate resin, silicone resin, and melamine resin. Among these, inorganic fine particles are preferred, silica and titanium oxide are more preferred, and silica is particularly preferred. In addition, it is preferred to use two or more types of fine particles in combination as the external additive. Although each of these external additives can be used alone, it is preferred to use two or more types in combination.

[0114] The external additive is preferably used in an amount of 0.3 to 6 parts by mass, and more preferably 1.2 to 3 parts by mass, based on 100 parts by mass of the colored resin particles.

[0115] The toner of the present invention uses colored resin particles that further contain an aromatic vinyl thermoplastic elastomer having an unsaturated bond capable of polymerization reaction in addition to a binder resin, a colorant, and a release agent, and further contains external additives. The toner of the present invention has excellent storage stability, low-temperature fixing property, and hot offset resistance, and further effectively suppresses the generation of UFP (ultrafine particles). Therefore, it can fully meet the recent demands for reducing energy consumption and increasing printing speed. EXAMPLES

[0116] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Note that "parts" and "%" are by weight unless otherwise specified. The test methods used in the present examples and comparative examples are as follows.

[0117] (1) Weight average molecular weight of each block copolymer in the aromatic vinyl thermoplastic elastomer The molecular weight was calculated as polystyrene equivalent molecular weight by high performance liquid chromatography using tetrahydrofuran as a carrier at a flow rate of 0.35 ml / min. The apparatus used was a Tosoh HLC8220, the column used was a combination of three Showa Denko Shodex (registered trademark) KF-404HQ columns (column temperature 40°C), and the detectors used were a differential refractometer and an ultraviolet detector. The molecular weight was calibrated at 12 points using standard polystyrene (5 to 3 million) from Polymer Laboratory.

[0118] (2) Content of each block copolymer in aromatic vinyl thermoplastic elastomer The ratio was determined from the area ratio of the peaks corresponding to each block copolymer in the chart obtained by the above-mentioned high performance liquid chromatography.

[0119] (3) Weight average molecular weight of the styrene polymer block of the block copolymer constituting the aromatic vinyl thermoplastic elastomer According to the method described in Rubber Chem. Technol., 45, 1295 (1972), the block copolymer was reacted with ozone and reduced with lithium aluminum hydride to decompose the isoprene polymer block of the block copolymer. Specifically, the following procedure was followed. That is, 300 mg of the sample was dissolved in a reaction vessel containing 100 ml of dichloromethane treated with molecular sieves. After placing this reaction vessel in a cooling bath and lowering the temperature to -25°C, ozone generated by an ozone generator was introduced into the reaction vessel while oxygen was flowing at a flow rate of 170 ml / min. After 30 minutes had passed since the start of the reaction, the completion of the reaction was confirmed by introducing the gas flowing out of the reaction vessel into the potassium iodide aqueous solution. Next, 50 ml of diethyl ether and 470 mg of lithium aluminum hydride were charged into another reaction vessel substituted with nitrogen, and the solution reacted with ozone was slowly dropped into the reaction vessel while cooling the reaction vessel with ice water. The reaction vessel was then placed in a water bath, gradually heated, and refluxed at 40°C for 30 minutes. After that, while stirring the solution, dilute hydrochloric acid was dripped into the reaction vessel in small amounts until hydrogen generation was almost no longer observed. After this reaction, the solid product generated in the solution was filtered, and the solid product was extracted with 100 ml of diethyl ether for 10 minutes. This extract was combined with the filtrate obtained by filtration, and the solvent was distilled off to obtain a solid sample. The weight average molecular weight of the sample thus obtained was measured according to the above-mentioned method for measuring weight average molecular weight, and the value was taken as the weight average molecular weight of the styrene polymer block.

[0120] (4) Weight average molecular weight of the isoprene polymer block of the block copolymer constituting the aromatic vinyl thermoplastic elastomer The weight average molecular weight of the corresponding styrene polymer block was subtracted from the weight average molecular weight of the block copolymer thus determined, and the weight average molecular weight of the isoprene polymer block was calculated based on the calculated value.

[0121] (5) Styrene unit content of block copolymer constituting aromatic vinyl thermoplastic elastomer The value was determined based on the ratio of the detection intensities of the differential refractometer and the ultraviolet detector in the measurement by high performance liquid chromatography. Note that copolymers having different styrene unit contents were prepared in advance, and a calibration curve was prepared using them.

[0122] (6) Vinyl bond content of the isoprene polymer block of the block copolymer constituting the aromatic vinyl thermoplastic elastomer It was determined based on proton NMR measurement.

[0123] (7) Styrene unit content of aromatic vinyl thermoplastic elastomer It was determined based on proton NMR measurement.

[0124] (8) Melt index of aromatic vinyl thermoplastic elastomer Measurements were performed in accordance with ASTM D1238 (G condition, 200°C, 5 kg load).

[0125] (9) Volume average particle size (Dv) of colored resin particles Approximately 0.1 g of colored resin particles were weighed out and placed in a beaker, and 0.1 mL of a surfactant solution (manufactured by Fujifilm, product name: Drywell) was added as a dispersant. 10 to 30 mL of Isoton II was further added to the beaker, and the particles were dispersed for 3 minutes using a 20 W ultrasonic disperser. The volume average particle size (Dv) of the colored resin particles was then measured using a particle size measuring device (manufactured by Beckman Coulter, product name: Multisizer) under the following conditions: aperture diameter: 100 μm, medium: Isoton II, number of particles measured: 100,000.

[0126] (10) Evaluation of toner storage stability 10 g of toner was placed in a 100 mL polyethylene container and sealed, and then the container was submerged in a thermostatic water bath set at a predetermined temperature, and after 8 hours, it was taken out. The toner was transferred from the container onto a 42 mesh sieve with as little vibration as possible, and set in a powder measuring instrument (manufactured by Hosokawa Micron Corporation, product name: Powder Tester PT-R). The sieve amplitude was set to 1.0 mm, and the sieve was vibrated for 30 seconds, after which the mass of the toner remaining on the sieve was measured, and this was taken as the mass of the aggregated toner. The maximum temperature (°C) at which the mass of the aggregated toner became 0.5 g or less was taken as the storage stability temperature, and was used as an index of storage stability.

[0127] (11) Minimum fixing temperature of toner A fixing test was conducted using a commercially available non-magnetic single-component development printer (printing speed 20 ppm) modified to change the temperature of the fixing roll. The fixing test was conducted by printing a solid black image (100% print density) and changing the temperature of the fixing roll of the modified printer by 5°C increments, measuring the toner fixing rate at each temperature, and determining the relationship between temperature and fixing rate. The fixing rate was calculated from the ratio of image density before and after tape peeling by peeling off tape in the printed area of ​​the solid black image (100% print density). In other words, if the image density before tape peeling is ID (before) and the image density after tape peeling is ID (after), the fixing rate can be calculated by the following formula. Retention rate (%) = (ID (later) / ID (previous)) x 100 Here, the tape peeling operation refers to a series of operations in which an adhesive tape (manufactured by Sumitomo 3M, product name: Scotch Mending Tape 810-3-18) is applied to the measurement portion of the test paper, pressed with a constant pressure to adhere, and then the adhesive tape is peeled off in the direction along the paper at a constant speed. The image density was measured using a reflection type image densitometer (manufactured by Macbeth, product name: RD914). In this fixing test, the lowest fixing roll temperature at which the fixing rate exceeded 80% was determined as the minimum fixing temperature of the toner.

[0128] (12) Toner hot offset occurrence temperature A hot offset test was conducted using a commercially available non-magnetic single-component development printer (printing speed 20 ppm) modified to change the temperature of the fixing roll. The hot offset test was conducted by changing the temperature of the fixing roll from 150°C to 220°C in 5°C increments, printing a 5cm square solid image on paper (Xerox, product name: Vitarity), and visually observing whether the toner had melted onto the fixing roll or whether the hot offset phenomenon had occurred. In this hot offset test, the lowest set temperature at which the toner started to melt and adhere to the fixing roll was taken as the hot offset occurrence temperature.

[0129] (13) UFP (ultrafine particle) generation temperature A predetermined amount of toner was heated on a heater installed in a chamber. The ultrafine particles discharged into the chamber were continuously measured using a particle counter (TSI, model: CPC3007). Next, the heater temperature was raised from 160°C, and the total count number of ultrafine particles with particle sizes in the range of 10 to 1,000 nm observed during the measurement was read in 5°C increments. The temperature at which the total count number exceeded 10,000 was taken as the emission start temperature of the toner (UFP (ultrafine particle) generation temperature).

[0130] [Production Example 1] In a pressure-resistant reactor, 23.2 kg of cyclohexane, 1.5 mmol of N,N,N',N'-tetramethylethylenediamine (hereinafter referred to as TMEDA), and 1.70 kg of styrene were added, and while stirring at 40°C, 99.1 mmol of n-butyllithium was added, and polymerization was carried out for 1 hour while raising the temperature to 50°C. The polymerization conversion rate of styrene was 100% by mass. Subsequently, 6.03 kg of isoprene was continuously added to the reactor over 1 hour while controlling the temperature to maintain 50-60°C. After the addition of isoprene was completed, polymerization was carried out for another 1 hour to form a styrene-isoprene diblock copolymer B (copolymer B represented by Ar-D). The polymerization conversion rate of isoprene was 100%. Next, 15.0 mmol of dimethyldichlorosilane was added as a coupling agent to carry out a coupling reaction for 2 hours, and a styrene-isoprene-styrene triblock copolymer (copolymer A represented by Ar-D-Ar) was formed. After that, 198 mmol of methanol was added as a polymerization terminator and mixed thoroughly to stop the reaction, thereby obtaining a reaction liquid containing a block copolymer composition (α1). A part of the obtained reaction liquid was taken out, and the weight average molecular weight, content ratio, and vinyl bond content of each block copolymer and the entire block copolymer composition were determined. The obtained results are shown in Table 1. Then, 0.3 parts of 2,6-di-tert-butyl-p-cresol was added as an antioxidant to 100 parts of the reaction liquid obtained in this way (containing 30 parts of polymer component) and mixed, and the mixed solution was dropped into hot water heated to 85 to 95 ° C. in small amounts to volatilize the solvent and obtain a precipitate, which was crushed and dried with hot air at 85 ° C. to recover the block copolymer composition (α1). The melt index of the obtained block copolymer composition (α1) was measured, and the obtained results are shown in Table 1.

[0131] [Production Example 2, Production Example of Acrylic Resin] 200 parts of toluene were put into the reaction vessel, and the inside of the reaction vessel was thoroughly replaced with nitrogen while stirring the toluene, and then the temperature was raised to 90°C, and then a mixed solution of 95 parts of methyl methacrylate, 4.6 parts of n-butyl acrylate, 0.4 parts of acrylic acid, and 2.8 parts of t-butylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, trade name: Perbutyl O) was dropped into the reaction vessel over 2 hours. Furthermore, the polymerization was completed by holding the mixture under toluene reflux for 10 hours, and then the solvent was distilled off under reduced pressure. In this way, an acrylic resin (Tg 70°C, acid value 2.5, weight average molecular weight (Mw) 11000) was obtained.

[0132] [Table 1]

[0133] [Example 1] 75.5 parts of styrene and 24.5 parts of n-butyl acrylate as monovinyl monomers, 7 parts of carbon black (manufactured by Mitsubishi Chemical Corporation, product name: #25B) as a colorant, 0.6 parts of divinylbenzene as a crosslinkable polymerizable monomer, 1.2 parts of t-dodecyl mercaptan as a molecular weight regulator, and 1 part of the acrylic resin obtained in Production Example 2 were wet-ground using a media-type wet grinder, and then 1 part of a charge control resin (styrene / acrylic resin containing a quaternary ammonium salt as a functional group, copolymerization ratio of a monomer containing a functional group of a quaternary ammonium salt: 2%) as a charge control agent, 20 parts of stearic acid triglyceride (number average molecular weight (Mn): 890, ester compound having a glycerin skeleton) as a mold release agent, and 2 parts of the block copolymer composition (α1) obtained in Production Example 1 as an aromatic vinyl thermoplastic elastomer were added and mixed to obtain a polymerizable monomer composition.

[0134] Separately, in a stirring tank at room temperature, an aqueous solution of 4.1 parts of sodium hydroxide (alkali metal hydroxide) in 50 parts of ion-exchanged water was gradually added to an aqueous solution of 7.4 parts of magnesium chloride (water-soluble polyvalent metal salt) in 250 parts of ion-exchanged water while stirring, to prepare a magnesium hydroxide colloid (poorly water-soluble metal hydroxide colloid) dispersion.

[0135] On the other hand, 2 parts of methyl methacrylate as a polymerizable monomer for the shell and 65 parts of ion-exchanged water were subjected to a fine dispersion treatment by an ultrasonic emulsifier to obtain an aqueous dispersion of the polymerizable monomer for the shell.

[0136] The polymerizable monomer composition was added to the magnesium hydroxide colloidal dispersion obtained above and stirred until the droplets became stable. 6 parts of t-butyl peroxyisobutyrate (manufactured by NOF Corp., product name: Perbutyl IB) was added as a polymerization initiator. Then, using an in-line emulsifying disperser (manufactured by Pacific Machinery Works, product name: Milder), the mixture was stirred with high shear at a rotation speed of 15,000 rpm, and dispersed while circulating, to form droplets of the polymerizable monomer composition.

[0137] Next, 1 part of sodium tetraborate decahydrate was added to the aqueous dispersion of the polymerizable monomer composition that had formed droplets, and the mixture was placed in a reactor equipped with an agitator and heated to 85°C to carry out a polymerization reaction. After the polymerization conversion rate reached nearly 100%, the aqueous dispersion of the shell polymerizable monomer prepared above and 0.3 parts of 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)-propionamide) (manufactured by Wako Pure Chemical Industries, Ltd., trade name: VA-086, water-soluble) as a polymerization initiator for the shell were added to the reactor. After further continuing the polymerization for 4 hours, the reaction was stopped by cooling with water to obtain an aqueous dispersion of colored resin particles having a core-shell structure.

[0138] The aqueous dispersion of the colored resin particles was washed with dilute sulfuric acid (25°C, 10 minutes) to adjust the pH to 4.5 or less. Next, the water was separated by filtration, and 200 parts of ion-exchanged water was added to reslurry the mixture. The water washing treatment (washing, filtration, dehydration) was repeated several times at room temperature (25°C), and the obtained solid content was separated by filtration and then vacuum dried to obtain dried colored resin particles.

[0139] To 100 parts of the colored resin particles obtained above, 0.5 parts of silica fine particles with a number average primary particle diameter of 7 nm that have been hydrophobized with cyclic silazane and 1 part of silica fine particles with a number average primary particle diameter of 35 nm that have been hydrophobized with amino-modified silicone oil were added as external additives, and the mixture was mixed and stirred using a high-speed mixer (manufactured by Nippon Coke & Engineering Co., Ltd., product name: FM Mixer) to perform external addition treatment, thereby preparing the toner for developing electrostatic images of Example 1, which was then subjected to testing. The results are shown in Table 2.

[0140] [Example 2] A toner for developing electrostatic images of Example 2 was prepared and tested in the same manner as in Example 1, except that 20 parts of behenic acid triglyceride (an ester compound having a number average molecular weight (Mn): 1060 and a glycerin skeleton) was used instead of 20 parts of stearic acid triglyceride. The results are shown in Table 2.

[0141] [Example 3] The toner for developing electrostatic images of Example 2 was prepared and tested in the same manner as in Example 1, except that 20 parts of palmitic acid triglyceride (number average molecular weight (Mn): 806, ester compound having a glycerin skeleton) was used instead of 20 parts of stearic acid triglyceride. The results are shown in Table 2.

[0142] [Example 4] The toner for developing electrostatic images of Example 4 was prepared and tested in the same manner as in Example 2, except that the amount of behenic acid triglyceride was changed from 20 parts to 12 parts. The results are shown in Table 2.

[0143] [Example 5] The toner for developing electrostatic images of Example 5 was prepared and tested in the same manner as in Example 2, except that the amount of behenic acid triglyceride was changed from 20 parts to 25 parts. The results are shown in Table 2.

[0144] [Example 6] The toner for developing electrostatic images of Example 6 was prepared and tested in the same manner as in Example 2, except that the blending amount of the block copolymer composition (α1) obtained in Production Example 1 was changed from 2 parts to 5 parts. The results are shown in Table 2.

[0145] [Example 7] The toner for developing electrostatic images of Example 7 was prepared and tested in the same manner as in Example 2, except that the blending amount of the block copolymer composition (α1) obtained in Production Example 1 was changed from 2 parts to 8 parts. The results are shown in Table 2.

[0146] [Comparative Example 1] A toner for developing electrostatic images of Comparative Example 1 was prepared and tested in the same manner as in Example 1, except that the block copolymer composition (α1) obtained in Production Example 1 was not used. The results are shown in Table 2.

[0147] [Comparative Example 2] A toner for developing electrostatic images of Comparative Example 2 was prepared and tested in the same manner as in Example 2, except that the block copolymer composition (α1) obtained in Production Example 1 was not used. The results are shown in Table 2.

[0148] [Comparative Example 3] An electrostatic image developing toner of Comparative Example 3 was prepared and tested in the same manner as in Example 1, except that 20 parts of pentaerythritol tetrapalmitate (an ester compound having a pentaerythritol skeleton, number average molecular weight (Mn): 1090) was used instead of 20 parts of stearic acid triglyceride, and the block copolymer composition (α1) obtained in Production Example 1 was not used. The results are shown in Table 2.

[0149] [Comparative Example 4] A toner for developing electrostatic images of Comparative Example 4 was prepared and tested in the same manner as in Example 1, except that 20 parts of pentaerythritol tetrapalmitate (an ester compound having a pentaerythritol skeleton, number average molecular weight (Mn): 1090) was used instead of 20 parts of stearic acid triglyceride. The results are shown in Table 2.

[0150] [Comparative Example 5] A toner for developing electrostatic images of Comparative Example 5 was prepared and tested in the same manner as in Example 1, except that 20 parts of behenyl stearate (number average molecular weight (Mn): 592, ester compound having a monoalcohol skeleton) was used instead of 20 parts of stearic acid triglyceride. The results are shown in Table 2.

[0151] [Table 2]

[0152] As shown in Table 2, the toners of Examples 1 to 7 obtained by using the colored resin particles containing, in addition to the binder resin, colorant, and release agent, an aromatic vinyl thermoplastic elastomer having an unsaturated bond capable of polymerization reaction, and the release agent containing an ester compound having a glycerin skeleton, had high storage temperature, excellent storage stability, low minimum fixing temperature, excellent low-temperature fixing property, high hot offset occurrence temperature, excellent hot offset resistance, and high UFP (ultrafine particle) occurrence temperature, and the occurrence of UFP (ultrafine particle) was effectively suppressed. In addition, the state of the ester compound having a glycerin skeleton as a release agent in the colored resin particles constituting the toners of Examples 1 to 7 was confirmed by cross-sectional SEM and TEM, and it was confirmed that the ester compound having a glycerin skeleton as a release agent was uniformly finely dispersed. FIG. 1(A) shows a cross-sectional SEM photograph (secondary electron image) of the colored resin particles of Example 1.

[0153] On the other hand, the toners of Comparative Examples 1 and 2, which contain an ester compound having a glycerin skeleton as a release agent but do not contain an aromatic vinyl thermoplastic elastomer having an unsaturated bond capable of polymerization reaction, had a high minimum fixing temperature and were poor in low-temperature fixing property. In addition, the toners of Comparative Examples 3 and 4, which contain an ester compound having a pentaerythritol skeleton instead of an ester compound having a glycerin skeleton as a release agent, have a low storage temperature and poor storage stability, and further have a low hot offset occurrence temperature and poor hot offset resistance. Furthermore, the toner of Comparative Example 5, which contains an ester compound having a monoalcohol skeleton instead of an ester compound having a glycerin skeleton as a release agent, had a low UFP (ultra-fine particle) generation temperature and was prone to UFP (ultra-fine particle) generation. In addition, when the state of the release agent in the colored resin particles constituting the toners of Comparative Examples 1 to 5 was confirmed by cross-sectional SEM and TEM, it was confirmed that the release agent was localized near the center of the toner particle and formed a large domain structure. Figure 1 (B) shows a cross-sectional SEM photograph (secondary electron image) of the colored resin particles of Comparative Example 1.

Claims

1. A toner for developing electrostatic images, comprising colored resin particles including a binder resin, a colorant, an aromatic vinyl thermoplastic elastomer having a polymerization-reactive unsaturated bond, and a release agent, and an external additive, The toner for developing electrostatic images, wherein the release agent is a triester of glycerin and a monocarboxylic acid having 16 or more carbon atoms.

2. 2. The toner for developing electrostatic images according to claim 1, wherein the content of the aromatic vinyl thermoplastic elastomer is 1 to 10 parts by mass based on 100 parts by mass of the binder resin.

3. 3. The toner for developing electrostatic images according to claim 1, wherein the content of the release agent is 1 to 30 parts by mass based on 100 parts by mass of the binder resin.

4. 4. The toner for developing electrostatic images according to claim 1, wherein the aromatic vinyl thermoplastic elastomer is a block copolymer containing at least one aromatic vinyl polymer block and at least one conjugated diene polymer block.

5. 5. The toner for developing electrostatic images according to claim 4, wherein the aromatic vinyl thermoplastic elastomer is a composition containing an aromatic vinyl-conjugated diene block copolymer and an aromatic vinyl-conjugated diene-aromatic vinyl block copolymer.

Citation Information

Patent Citations

  • Resin composition for toner and toner

    JP1992184357A

  • Electrostatic charge image developing toner and method for manufacturing same

    JP2004295065A

  • Electrostatic charge image developing toner

    JP2010085841A

  • Toner for developing electrostatic images

    WO2019065868A1