Heat exchanger and reformer

The heat exchange device with intersecting honeycomb structures and a holding mat design addresses damage and misalignment issues, maintaining high efficiency and stability under high pressure, enhancing fuel reforming performance.

JP7564724B2Active Publication Date: 2024-10-09IBIDEN CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021016745
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-04
Publication Date
2024-10-09
Estimated Expiration
2041-02-04

AI Technical Summary

Technical Problem

Existing heat exchangers used in fuel reforming systems face issues with damage and misalignment due to high canning pressure and exhaust gas pressure, which affect their performance and stability.

Method used

A heat exchange device with a first and second honeycomb structure intersecting flow paths, a metal casing, and a holding mat with specific area ratios and materials to enhance mechanical strength and thermal capacity, preventing damage and misalignment.

Benefits of technology

The device maintains high heat exchange efficiency and reforming performance by stabilizing the heat exchanger under high pressure conditions, ensuring effective fuel reforming and improved fuel efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564724000002
    Figure 0007564724000002
  • Figure 0007564724000003
    Figure 0007564724000003
  • Figure 0007564724000004
    Figure 0007564724000004
Patent Text Reader

Abstract

To provide a heat exchange device in which breakage or positional deviation is hard to occur, and a reformer equipped with the heat exchange device.SOLUTION: A heat exchange device is composed of a heat exchanger in which a first circulation path and a second circulation path that are honeycomb structures are assembled so as to intersect each other, a metal casing that stores the heat exchanger, and a holding mat that is arranged between the heat exchanger and the metal casing. The heat exchanger has a substantially columnar shape in which the first circulation path opens on both end surfaces and the second circulation path opens on an outer peripheral surface. The holding mat is arranged along the outer peripheral surface of the heat exchanger so as not to cover a part of the second circulation path opening on the outer peripheral surface. A surface of the second honeycomb structure of the outer peripheral surface of the heat exchanger has an opening area where the second circulation path is not covered by the holding mat and opens on the outer peripheral surface of the heat exchanger, and sealing areas which are respectively provided on both end surface side of the head exchanger with respect to the opening area and where the second circulation path is covered by the holding mat.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat exchange device and a reformer. [Background technology]

[0002] Patent Document 1 discloses the following technology for improving fuel efficiency by reforming fuel for an internal combustion engine. That is, a part of exhaust gas from an exhaust passage of an internal combustion engine is recirculated to an intake passage as EGR (exhaust gas recirculation) gas, and a reforming fuel injection valve for injecting reforming fuel and a fuel reforming catalyst for reforming the reforming fuel are arranged in the middle of the EGR passage. Then, the reforming fuel injected by the reforming fuel injection valve and moisture (water vapor) in the EGR gas are reformed by the fuel reforming catalyst to generate hydrogen (H2) and carbon monoxide (CO), thereby reforming the reforming fuel to generate a highly combustible reformed gas, and the reformed gas is supplied to the intake passage of the internal combustion engine. In addition, the amount of injection of the reforming fuel is controlled so as to be within a control region set based on the temperature of the fuel reforming catalyst and the amount of reformed gas, thereby suppressing deterioration of the fuel reforming catalyst and improving the reforming performance.

[0003] The above-mentioned fuel reforming catalyst absorbs heat from the exhaust gas when water vapor and hydrocarbons react in the reformer. Therefore, the fuel reforming catalyst is configured to be able to exchange heat with the exhaust gas flowing through the exhaust pipe, supplying heat from the exhaust gas to promote the reforming reaction.

[0004] Patent Document 1 does not disclose the specific materials or configuration of the fuel reforming catalyst. However, in order to promote the reaction in the reformer, a temperature of 600°C or higher is required, and the material that constitutes the fuel reforming catalyst must be able to withstand temperatures of 600°C or higher and have a heat exchange function.

[0005] Patent Document 2 discloses a heat exchanger having a monolithic ceramic structure in which a first layer and a second layer having flow paths are stacked in a direction intersecting each other and fired. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-166591 A [Patent Document 2] Japanese Patent Application Publication No. 7-151478 Summary of the Invention [Problem to be solved by the invention]

[0007] In the reforming method described in Patent Document 1, the pressure from the exhaust gas environment is high, so the heat exchanger needs to be maintained at a high canning pressure. When the heat exchanger described in Patent Document 2 is used in the method described in Patent Document 1, a cylindrical heat exchanger is sometimes required instead of a prismatic one due to the installation location, piping arrangement, and the like. However, when the heat exchanger described in Patent Document 2 is deformed into a cylindrical shape and used in the method described in Patent Document 1, there is a problem that the heat exchanger is damaged by the high canning pressure, and when the canning pressure is set to a level that does not damage the heat exchanger, the position of the heat exchanger is displaced by the exhaust gas pressure.

[0008] The present invention has been made to solve the above problems, and has an object to provide a heat exchanger device that is less susceptible to damage and displacement, and a reformer including the heat exchanger device. [Means for solving the problem]

[0009] The heat exchanger of the present invention is a heat exchanger including a first honeycomb structure having a number of cells arranged in parallel in the longitudinal direction across partition walls to become first flow passages for a fluid, and a second honeycomb structure having a number of cells arranged in parallel in the longitudinal direction across partition walls to become second flow passages for a fluid, the first flow passages and the second flow passages being combined together such that the first flow passages and the second flow passages intersect, a metal casing that houses the heat exchanger, and a retaining mat that is disposed between the heat exchanger and the metal casing, the heat exchanger having a substantially cylindrical shape with the first flow passages opening on both end faces and the second flow passages opening on an outer peripheral surface, and the retaining mat is disposed along the outer peripheral surface of the heat exchanger, the first honeycomb structure is arranged so as not to cover a portion of the second flow passage opening to the peripheral surface, the entire surface of the first honeycomb structure of the outer peripheral surface of the heat exchanger is covered with a coating layer, the surface of the second honeycomb structure of the outer peripheral surface of the heat exchanger has an opening region where the second flow passage is not covered by the retaining mat and opens to the outer peripheral surface of the heat exchanger, and plugging regions which are provided on both end face sides of the heat exchanger with respect to the opening region and where the second flow passage is covered by the retaining mat, and the ratio of the area of ​​the opening region to the total area of ​​the opening region and the plugging region is 72 to 93%.

[0010] According to the heat exchange device of the present invention, the heat exchanger is combined so that the first flow passage and the second flow passage intersect, thereby improving heat exchange performance and enabling two types of fluids performing heat exchange to flow smoothly from different directions.

[0011] Furthermore, in the heat exchange device of the present invention, the entire surface of the first honeycomb structure on the outer peripheral surface of the heat exchanger is covered with a coating layer, and a portion of the surface of the second honeycomb structure is a plugged area in which the second flow passage is covered with a retaining mat. The portion covered with the coating layer has higher mechanical strength than the portion not covered with the coating layer. The portions covered with the coating layer, which has high mechanical strength, and the plugging regions provided on both ends of the second honeycomb structure are used as the portions to which the canning pressure is applied. Therefore, even if the canning pressure is increased, the heat exchanger is less likely to be damaged and can be prevented from shifting.

[0012] Furthermore, in the heat exchanger of the present invention, a portion of the second flow passage is covered with a support mat. In the second flow passage covered with the support mat, the flow of fluid is hindered, so that the temperature change caused by the flow of fluid becomes slow, and the second flow passage functions as a mass (heat capacity) that stores heat. Therefore, even if the temperature of the exhaust gas flowing into the second honeycomb structure drops, a high temperature can be maintained, and the reforming ability at the inlet can be improved.

[0013] In the heat exchanger of the present invention, the ratio of the area of ​​the open region to the total area of ​​the open region and the plugged region is 72 to 93%. Therefore, there is a good balance between the ratio of the second flow passages (open region) used for heat exchange with the first honeycomb structure under normal conditions and the ratio of the second flow passages (plugged region) functioning as a heat capacity when the exhaust gas temperature drops, and the reforming performance at the inlet when the exhaust gas temperature drops can be improved while ensuring sufficient heat exchange efficiency under normal conditions.

[0014] In the heat exchanger of the present invention, the support mat preferably has a thickness of 3 to 5 mm.

[0015] In the heat exchanger of the present invention, when the thickness of the support mat is 3 to 5 mm, the heat exchanger can be stably supported without significantly increasing the volume of the heat exchanger. If the thickness of the retaining mat is less than 3 mm, the mat may not be able to stably hold the heat exchanger and may be damaged, whereas if the thickness of the retaining mat is more than 5 mm, the volume of the heat exchanger may become too large.

[0016] In the heat exchanger of the present invention, it is preferable that the second honeycomb structure is disposed on both sides of the first honeycomb structure.

[0017] In the heat exchange device of the present invention, when the second honeycomb structure is arranged on both sides of the first honeycomb structure, heat can be transmitted from the second honeycomb structures on both sides, and heat can be effectively supplied to the first honeycomb structure.

[0018] In the heat exchanger of the present invention, it is preferable that a catalyst is supported on the partition walls of the cells constituting the first honeycomb structure.

[0019] In the heat exchange device of the present invention, when a catalyst is supported on the partition walls of the cells constituting the first honeycomb structure, a reforming reaction can be carried out inside the first honeycomb structure, and the catalyst can fully function as a reforming catalyst by receiving heat from the exhaust gas flowing into the second honeycomb structure.

[0020] In the heat exchanger of the present invention, it is desirable that the ratio of the total opening area of ​​the second flow passages to the total opening area of ​​the first flow passages (total opening area of ​​the second flow passages / total opening area of ​​the first flow passages) be 1.25 to 2.

[0021] In the heat exchange device of the present invention, when the ratio of the total opening area of ​​the second flow passages to the total opening area of ​​the first flow passages (total opening area of ​​the second flow passages / total opening area of ​​the first flow passages) is 1.25 to 2, a good balance is achieved between the reforming reaction occurring inside the first honeycomb structure and the amount of heat transmitted from the second honeycomb structure to the first honeycomb structure. If the ratio is less than 1.25, the amount of heat transferred from the second honeycomb structure to the first honeycomb structure is relatively reduced, and the reforming reaction may not occur easily. On the other hand, if the ratio is more than 2, the opening area of ​​the second flow passage is large, and the plugging area is relatively small. As a result, the canning pressure cannot be sufficiently applied, and the heat exchanger may become misaligned during use.

[0022] In the heat exchanger of the present invention, it is desirable that both the first honeycomb structure and the second honeycomb structure are made of silicon carbide and silicon.

[0023] In the heat exchange device of the present invention, when the first honeycomb structure and the second honeycomb structure are both made of silicon carbide and silicon, they have excellent thermal conductivity and heat resistance, and therefore have a good heat exchange function and are less likely to be broken even when a large temperature difference occurs. Furthermore, they are less likely to be corroded by hydrogen contained in the reformed gas.

[0024] In the heat exchanger of the present invention, it is preferable that each of the first honeycomb structure and the second honeycomb structure is formed by bonding a plurality of ceramic honeycomb segments via an adhesive layer.

[0025] In the heat exchange device of the present invention, when the first honeycomb structure and the second honeycomb structure each have a structure in which a plurality of ceramic honeycomb segments are bonded together via an adhesive layer, the size of each honeycomb segment can be reduced, and the adhesive layer acts as a buffer material, so that even if a large temperature difference occurs throughout the heat exchanger, damage is less likely to occur.

[0026] In the heat exchanger of the present invention, it is preferable that the adhesive layer is made of silicon carbide and silicon.

[0027] In the heat exchanger of the present invention, when the adhesive layer is made of silicon carbide and silicon, the adhesive layer has excellent thermal conductivity, and the heat exchange performance between the first honeycomb structure and the second honeycomb structure can be further improved.

[0028] In the heat exchange device of the present invention, the volume of the heat exchanger is desirably 1.2 to 3.2 liters.

[0029] In the heat exchange device of the present invention, when the volume of the heat exchanger is 1.2 to 3.2 liters, the heat exchanger has an appropriate volume, making it easy to install in a vehicle, etc., and capable of fully exerting its effect as a heat exchange device. If the volume of the heat exchanger is less than 1.2 liters, the volume of the heat exchanger is too small, making it difficult to support a sufficient amount of catalyst, while if the volume of the heat exchanger exceeds 3.2 liters, the capacity of the heat exchanger device becomes too large, making it difficult to install it in a vehicle.

[0030] In the heat exchange device of the present invention, the heat exchanger is preferably configured such that the first honeycomb structure and the second honeycomb structure are alternately arranged, and includes three layers of the first honeycomb structure and four layers of the second honeycomb structure.

[0031] In the heat exchange device of the present invention, the heat exchanger is configured such that the first honeycomb structures and the second honeycomb structures are arranged alternately, and includes three layers of the first honeycomb structures and four layers of the second honeycomb structures, so that the contact area between the second honeycomb structures and the first honeycomb structures is large, enabling efficient heat exchange.

[0032] The reformer of the present invention is a reformer equipped with a heat exchanger of the above-mentioned configuration, characterized in that the second honeycomb structure is configured to allow exhaust gas discharged from an internal combustion engine and flowing through a main exhaust pipe to pass therethrough, and the first honeycomb structure has a reforming catalyst supported on its partition walls and is configured to allow exhaust gas that has flowed into an exhaust gas recirculation pipe branched off from the main exhaust pipe to pass therethrough.

[0033] When the reformer of the present invention is configured as described above, the heat of the exhaust gas can be effectively supplied from the second honeycomb structure to the first honeycomb structure, and the reformer can effectively perform the function of reforming the fuel for an internal combustion engine to improve fuel efficiency. Furthermore, in the reformer of the present invention, since a retaining mat is disposed between the heat exchanger and the metal casing, damage to the coating layer is unlikely to occur even if the heat exchanger becomes hot. [Brief description of the drawings]

[0034] [Figure 1] FIG. 1 is a perspective view that typically illustrates a heat exchanger that constitutes a heat exchanger device according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the heat exchanger shown in FIG. 1 taken along line II-II. [Diagram 3] FIG. 3 is a perspective view that typically shows a retaining mat that is used when the heat exchanger shown in FIG. 1 is housed in a metal casing. [Figure 4] FIG. 4 is an explanatory view that typically shows a method for winding the support mat shown in FIG. 3 around the heat exchanger shown in FIG. [Diagram 5] FIG. 5 is a perspective view that illustrates an example of a heat exchanger according to a first embodiment of the present invention. [Figure 6] FIG. 6 is a perspective view that diagrammatically shows one example of a honeycomb aggregate for manufacturing the heat exchanger shown in FIG. [Figure 7] FIG. 7 is a perspective view that illustrates a heat exchanger that constitutes a heat exchanger device according to a second embodiment of the present invention. [Figure 8] FIG. 8 is a cross-sectional view of the heat exchanger shown in FIG. 7 taken along line VIII-VIII. [Figure 9] FIG. 9 is an explanatory diagram that shows a schematic diagram of a fuel reformed gasoline engine system equipped with a reformer of the present invention.

[0035] Detailed Description of the Invention The heat exchange device of the present invention will now be described. The heat exchanger of the present invention is a heat exchanger including a first honeycomb structure having a number of cells arranged in parallel in the longitudinal direction across partition walls to become first flow passages for a fluid, and a second honeycomb structure having a number of cells arranged in parallel in the longitudinal direction across partition walls to become second flow passages for a fluid, the first flow passages and the second flow passages being combined together such that the first flow passages and the second flow passages intersect, a metal casing that houses the heat exchanger, and a retaining mat that is disposed between the heat exchanger and the metal casing, the heat exchanger having a substantially cylindrical shape with the first flow passages opening on both end faces and the second flow passages opening on an outer peripheral surface, and the retaining mat is disposed along the outer peripheral surface of the heat exchanger, the first honeycomb structure is arranged so as not to cover a portion of the second flow passage opening to the peripheral surface, the entire surface of the first honeycomb structure of the outer peripheral surface of the heat exchanger is covered with a coating layer, the surface of the second honeycomb structure of the outer peripheral surface of the heat exchanger has an opening region where the second flow passage is not covered by the retaining mat and opens to the outer peripheral surface of the heat exchanger, and plugging regions which are provided on both end face sides of the heat exchanger with respect to the opening region and where the second flow passage is covered by the retaining mat, and the ratio of the area of ​​the opening region to the total area of ​​the opening region and the plugging region is 72 to 93%.

[0036] FIG. 1 is a perspective view showing a heat exchanger constituting a heat exchanger device according to a first embodiment of the present invention, and FIG. 2 is a cross-sectional view of the heat exchanger shown in FIG. 1 taken along line II-II. As shown in Figures 1 and 2, the heat exchanger 100 is a generally cylindrical heat exchanger which is formed by combining a first honeycomb structure 10 in which a number of first cells 13 which become first flow passages for fluid are arranged in the longitudinal direction separated by first partition walls 12, and a second honeycomb structure 20 in which a number of second cells 23 which become second flow passages for fluid are arranged in the longitudinal direction separated by second partition walls 22, such that the first flow passages (first cells 13) and second flow passages (second cells 23) intersect. In addition, when there is no particular distinction between the first honeycomb structure and the second honeycomb structure, they are also simply referred to as honeycomb structures. As with the honeycomb structure, when there is no particular distinction between the first cells and the second cells, and the first partition walls and the second partition walls, they are also simply referred to as cells and partition walls.

[0037] 1 and 2, the extension direction of the first cells 13 constituting the first honeycomb structure 10 is the vertical direction (the direction indicated by the arrow z in Figs. 1 and 2). The extension direction of the second cells 23 constituting the second honeycomb structure 20 is the horizontal direction (the direction indicated by the arrow y in Fig. 1). In the first honeycomb structure 10 and the second honeycomb structure 20, the flow passages intersect with each other, so that two types of fluids (particularly gases) can easily flow and heat exchange can be efficiently performed.

[0038] The heat exchanger 100 shown in Figs. 1 and 2 includes three layers of the first honeycomb structure 10 and four layers of the second honeycomb structure 20, in which the first honeycomb structure 10 and the second honeycomb structure 20 are alternately arranged with adhesive layers 19 interposed therebetween. In the heat exchanger 100 shown in Figs. 1 and 2, one first honeycomb segment 11 constitutes one layer of the first honeycomb structure 10, but two or more first honeycomb segments 11 may be bonded together with adhesive layers to constitute one layer of the first honeycomb structure 10. Therefore, in the present invention, an assembly of one or more first honeycomb segments 11 sandwiched between the second honeycomb structures 20 is counted as one layer of the first honeycomb structure 10. The first honeycomb segment is a member having the same structure as the first honeycomb structure.

[0039] In the heat exchange device of the present invention, the fluid to be subjected to heat exchange may be a liquid such as water, an organic solvent such as ethylene glycol, or a liquefied gas, or a gas, but a gas is preferable, and exhaust gas is more preferable. In addition, in this specification, when the term "heat exchange device of the present invention" is used, it is assumed that the term refers to the heat exchange device of the first embodiment described above, the heat exchange device of the second embodiment described below, and other components constituting the heat exchange devices of all embodiments of the present invention, and components related to the above heat exchange devices.

[0040] In the heat exchanger 100 shown in FIGS. 1 and 2, one layer of the second honeycomb structure 20 is formed by bonding two second honeycomb segments 21 together via an adhesive layer 18. The second honeycomb structures 20 are counted in the same way as the first honeycomb structures 10, and an assembly of one or two or more second honeycomb segments 21 sandwiched between the first honeycomb structures 10 is referred to as one layer of the second honeycomb structure 20. However, the second honeycomb structure 20 may be located on the outermost side, in which case the assembly of one or two or more second honeycomb segments 21 at the outermost side is also one layer of the second honeycomb structure 20. When there is no particular distinction between the first honeycomb segment and the second honeycomb segment, they are also simply referred to as honeycomb segments.

[0041] The first honeycomb structure and the second honeycomb structure constituting the heat exchange device of the present invention may each be composed of one ceramic honeycomb segment, or may be composed of multiple ceramic honeycomb segments bonded together via an adhesive layer.

[0042] The number of honeycomb segments constituting the first honeycomb structure and the second honeycomb structure may be the same or different from each other.

[0043] In the heat exchanger of the present invention, it is preferable that the second honeycomb structure is disposed on both sides of the first honeycomb structure. When the second honeycomb structures are arranged on both sides of the first honeycomb structure, heat can be transmitted from the second honeycomb structures on both sides, and heat can be efficiently supplied to the first honeycomb structure.

[0044] In a first embodiment of the heat exchange device of the present invention, the heat exchanger is composed of first honeycomb structures and second honeycomb structures arranged alternately, and desirably includes three layers of the first honeycomb structures and four layers of the second honeycomb structures. When a heat exchanger includes three layers of the first honeycomb structure and four layers of the second honeycomb structure, in which the first honeycomb structure and the second honeycomb structure are alternately arranged, the contact area between the second honeycomb structure and the first honeycomb structure is large, enabling efficient heat exchange.

[0045] In the heat exchanger 100 having an approximately cylindrical shape shown in Figures 1 and 2, first cells 13 which serve as first flow passages of the first honeycomb structure 10 open on both end faces, and second cells 23 which serve as second flow passages of the second honeycomb structure 20 open on the outer circumferential face. A part of the outer peripheral surface is covered with a coating layer 32. The coating layer 32 has a coating layer 32a that covers the entire surface of the first honeycomb structure 10 that constitutes the outer peripheral surface, and a coating layer 32b that covers a part of the surface of the second honeycomb structure 20 that constitutes the outer peripheral surface. The portion covered with the coating layer 32 has a higher mechanical strength than the portion not covered with the coating layer, and therefore the portion covered with the coating layer 32 can be used as a portion to which the canning pressure is applied.

[0046] In addition, since the entire surface of the first honeycomb structure 10 constituting the outer peripheral surface is covered with the coating layer 32a, it is possible to prevent the fluid flowing through the first cells 13 which form the first flow passages and the fluid flowing through the second cells 23 which form the second flow passages from mixing with each other. The surface of the second honeycomb structure 20 constituting the outer peripheral surface may be partially covered with the coating layer 32 or may not be covered.

[0047] Since the entire surface of the first honeycomb structure 10 constituting the outer peripheral surface is covered with the coating layer 32a, it is possible to prevent the fluid flowing through the first cells 13 which form the first flow passages and the fluid flowing through the second cells 23 which form the second flow passages from mixing with each other.

[0048] The thickness of the coating layer is not particularly limited, but is preferably 0.1 to 0.5 mm. If the thickness of the coating layer is less than 0.1 mm, the coating layer is too thin and may be damaged by the pressure during canning, whereas if the thickness of the coating layer is more than 0.5 mm, the coating layer is too thick and may be damaged by the temperature difference between the outermost surface of the coating layer and the part in contact with the honeycomb structure.

[0049] In the heat exchanger of the present invention, the material of the honeycomb structure or the honeycomb segments which are its constituent members is not particularly limited, and examples thereof include oxide-based ceramics such as cordierite, alumina, silica, mullite, etc., carbide-based ceramics such as silicon carbide, zirconium carbide, titanium carbide, tantalum carbide, tungsten carbide, etc., nitride-based ceramics such as aluminum nitride, silicon nitride, boron nitride, titanium nitride, etc., and composite materials of these ceramics and metals, etc. Among these, composite materials of silicon carbide are preferable, and composite materials of silicon and silicon carbide are particularly preferable.

[0050] Although the specific configuration of the composite material made of silicon and silicon carbide is not particularly limited, a composite material of silicon and silicon carbide in which silicon fills the gaps between silicon carbide particles and independent silicon carbide particles are bonded together by the silicon present around them is desirable. A composite material made of silicon and silicon carbide in this manner can be produced by bringing a degreased honeycomb formed body into contact with molten silicon, as described below. The porous sintered silicon carbide may have open pores filled with silicon.

[0051] When the molten silicon is brought into contact with silicon carbide, the degreased bodies of multiple honeycomb molded bodies are brought into contact with the molten silicon while being in close contact with each other via an adhesive layer containing silicon carbide, thereby forming an adhesive layer consisting of silicon carbide and silicon, and a heat exchanger can be created in which multiple honeycomb structures (or honeycomb segments) are bonded together with an adhesive layer consisting of silicon carbide and silicon.

[0052] The material of the adhesive layer that bonds the honeycomb structures (or honeycomb segments) together is not particularly limited, but it is desirable to use a composite material in which silicon fills the gaps between silicon carbide particles, similar to the honeycomb structures (or honeycomb segments). As described below, such a composite material can be produced by applying a raw material paste containing silicon carbide to the side walls in order to bond the honeycomb molded bodies together, drying the honeycomb molded bodies after bonding them together, and bringing them into contact with molten silicon.

[0053] The thickness of the adhesive layer that bonds the honeycomb structures (or honeycomb segments) together is not particularly limited, but is preferably 0.5 to 2.0 mm.

[0054] The material of the coating layer is not particularly limited, but is desirably a composite material in which silicon fills the gaps between silicon carbide particles, similar to the honeycomb structure (or honeycomb segment) and adhesive layer. As described below, such a composite material can be produced by applying a raw material paste containing silicon carbide to the portion of the outer surface of a cylindrical dried honeycomb body that will become the first honeycomb structure, drying it, and then contacting this with molten silicon.

[0055] In the heat exchanger of the present invention, the thickness of the partition walls of the first honeycomb structure and the second honeycomb structure is preferably uniform. Specifically, the thickness of the partition walls of the first honeycomb structure that supports the catalyst is preferably 0.08 to 0.30 mm, and more preferably 0.10 to 0.20 mm. Since the partition walls of the first honeycomb structure are thin, the surface area is increased, making it possible to support a larger amount of catalyst.

[0056] The thickness of the partition walls of the second honeycomb structure is preferably 0.10 to 0.40 mm, and more preferably 0.15 to 0.30 mm. Since the partition walls of the second honeycomb structure are thick, the heat capacity is increased and a large amount of heat can be supplied to the first honeycomb structure.

[0057] When the thickness of the partition walls of the first honeycomb structure and the second honeycomb structure are set as described above, a larger amount of catalyst can be supported, improving the reforming efficiency, and a larger amount of heat can be supplied from the second honeycomb structure to the first honeycomb structure, thereby increasing the activity of the catalyst.

[0058] In the heat exchanger of the present invention, the shape of the cells constituting the honeycomb structure is preferably, for example, a quadrangular prism with rectangular end faces as a whole, but may also be a triangular prism or hexagonal prism. The shapes of the cells may be different, but it is preferable that they are all the same. In other words, it is preferable that the size of the cells surrounded by the partition walls is the same in a cross section perpendicular to the longitudinal direction of the honeycomb structure. This is because it is easy to manufacture.

[0059] In the heat exchanger of the present invention, the cell density (first cell density) in a cross section perpendicular to the longitudinal direction of the cells of the first honeycomb structure is 46 to 124 cells / cm. 2 (300~800 pieces / inch 2 ) is preferable, and 62 to 93 pieces / cm 2 (400~600 pieces / inch 2) is more preferable. When the first cell density is within the above range, the surface area of ​​the first honeycomb structure becomes large, and a large amount of catalyst can be supported. The cell density (second cell density) in a cross section perpendicular to the longitudinal direction of the cells of the second honeycomb structure is 16 to 78 cells / cm 2 (100~500 pieces / inch 2 ) is preferable, and 31 to 62 pieces / cm 2 (200~400 pieces / inch 2 When the second cell density is within the above range, the heat capacity of the second honeycomb structure becomes large, and a large amount of heat can be supplied to the first honeycomb structure.

[0060] In the heat exchanger of the present invention, the ratio of the total opening area of ​​the second flow passages to the total opening area of ​​the first flow passages (total opening area of ​​the second flow passages / total opening area of ​​the first flow passages) is desirably 1.25 to 2. When the ratio of the total opening area of ​​the second flow passages to the total opening area of ​​the first flow passages (total opening area of ​​the second flow passages / total opening area of ​​the first flow passages) is 1.25 to 2, a good balance is achieved between the reforming reaction occurring inside the first honeycomb structure and the amount of heat transmitted from the second honeycomb structure to the first honeycomb structure. If the ratio is less than 1.25, the amount of heat transferred from the second honeycomb structure to the first honeycomb structure is relatively reduced, and the reforming reaction may not occur easily. On the other hand, if the ratio is more than 2, the opening area of ​​the second flow passage is large, and the plugging area is relatively small. As a result, the canning pressure cannot be sufficiently applied, and the heat exchanger may become misaligned during use.

[0061] In the heat exchanger of the present invention, it is preferable that the first cells constituting the first honeycomb structure support a catalyst, and it is more preferable that the first cells support a fuel reforming catalyst. The catalyst is preferably Co, Ni, Rh, Pt or Pd, and more preferably Rh. The catalyst may be supported on a carrier and supported in the first cell constituting the first honeycomb structure. The catalyst supported on the carrier is preferably Rh / ZrO2 or Rh / CoO2. The carrier may be other ceramics such as silica or alumina.

[0062] In the heat exchanger according to the first embodiment of the present invention, the volume of the heat exchanger is desirably 1.2 to 3.2 liters. When the volume of the heat exchanger is 1.2 to 3.2 liters, the heat exchanger has an appropriate volume, so that it can be easily mounted on a vehicle or the like and can fully exert its effect as a heat exchange device. If the volume of the heat exchanger is less than 1.2 liters, the volume of the heat exchanger is too small, making it difficult to support a sufficient amount of catalyst, while if the volume of the heat exchanger exceeds 3.2 liters, the capacity of the heat exchanger device becomes too large, making it difficult to install it in a vehicle.

[0063] Next, the metal casing constituting the heat exchanger of the present invention will be described. The metal casing is a metal container for housing the heat exchanger, and the shape thereof can be appropriately selected depending on the shape of the heat exchanger. The casing is made of a metal such as SUS.

[0064] The shape of the metal casing is not particularly limited, but it is desirable for the metal casing to have an opening so as not to cover the open area of ​​the outer circumferential surface of the heat exchanger.

[0065] Next, the support mat constituting the heat exchanger of the present invention will be described. The retaining mat is made of ceramic fibers and is disposed between the heat exchanger and the metal casing.

[0066] As the supporting mat, a needle mat obtained by needle punching, a mat obtained by a wet papermaking method, or the like can be used.

[0067] The ceramic fibers constituting the support mat preferably have an average fiber diameter of 3 to 50 μm, and more preferably have an average fiber length of 100 to 100,000 μm. The ceramic fibers constituting the support mat desirably contain at least one type selected from alumina fibers, silica fibers, alumina-silica fibers, mullite fibers, glass fibers, and biosoluble fibers. When the ceramic fibers constituting the support mat have the above-mentioned shape and material, the surface pressure of the support mat can be sufficiently improved, and the heat exchanger can be stably supported in the reformer.

[0068] The support mat may also contain an organic binder or an inorganic binder. Examples of the organic binder include rubber-based resins, styrene-based resins, silicone-based resins, acrylic-based resins, polyester-based resins, and polyurethane resins. Examples of the inorganic binder include alumina sol, silica sol, aerogel, fumed silica, and titanium particles.

[0069] The thickness of the retaining mat is preferably 3 to 5 mm. When the thickness of the support mat is 3 to 5 mm, the heat exchanger can be stably supported without significantly increasing the volume of the heat exchanger. If the thickness of the retaining mat is less than 3 mm, the mat cannot stably hold the heat exchanger and may be damaged, whereas if the thickness of the retaining mat is more than 5 mm, the volume of the heat exchanger may become too large.

[0070] Figure 3 is a schematic oblique view of a retaining mat used when storing the heat exchanger shown in Figure 1 in a metal casing, Figure 4 is a schematic explanatory diagram showing a winding method for winding the retaining mat shown in Figure 3 around the heat exchanger shown in Figure 1, and Figure 5 is a schematic oblique view of an example of a heat exchanger device related to the first embodiment of the present invention.

[0071] As shown in FIG. 3, the retaining mat 50 has convex portions 51a and concave portions 51b at both ends of the mat 51, and mat openings 51c, 51d, 51e, 51f, 51g, and 51h are formed so that the second cells 23, which are the fluid inlet and fluid outlet, are exposed when the mat 50 is wrapped around the heat exchanger 100. As shown in FIG. 4, when the support mat 50 is wrapped around the heat exchanger 100, the second cells 23, which are the fluid inlet and the fluid outlet, are exposed through the mat openings 51c, 51d, 51e, 51f, 51g, and 51h.

[0072] 4, the support mat 50 covers the entire surface of the first honeycomb structure 10 in the outer peripheral surface of the heat exchanger 100. On the other hand, the surface of the second honeycomb structure 20 constituting the outer peripheral surface of the heat exchanger 100 has an opening region A1 (a region shown by a dashed line in FIG. 4) where the second flow passages are not covered by the support mat 50 and open to the outer peripheral surface of the heat exchanger 100, and plugging regions A2 and A3 (a region shown by a dashed line in FIG. 4) which are provided on both end face sides of the heat exchanger 100 with respect to the opening region A1 and where the second flow passages are covered by the support mat 50. In addition, in Figure 4, the opening area A1 and the sealing areas A2, A3 are illustrated on the surface of the retaining mat 50, but this indicates the positions of the areas that will become the opening area A1, the sealing areas A2, A3 when the retaining mat 50 is wrapped around the heat exchanger 100, and the actual opening area A1 and the sealing areas A2, A3 are present on the outer peripheral surface of the heat exchanger 100.

[0073] As shown in FIG. 4, the support mat 50 is wrapped around the heat exchanger 100 and housed in a metal casing 60, thereby obtaining a heat exchange device 70 shown in FIG. The heat exchange device 70 shown in FIG. 5 comprises a heat exchanger 100, a metal casing 60 that houses the heat exchanger 100, and a retaining mat 50 disposed between the heat exchanger 100 and the metal casing 60. The surface of the metal casing 60 has openings 60c, 60d, 60e, 60f, 60g, and 60h formed thereon corresponding to the openings 51c, 51d, 51e, 51f, 51g, and 51h of the retaining mat 50 (however, openings 60d and 60e are not shown). Therefore, in the heat exchange device 70, the opening area A1 is exposed and not covered by the metal casing 60. Therefore, the areas of the opening area A1 and the sealed areas A2 and A3 described in FIG.

[0074] In the heat exchanger of the present invention, the ratio of the area of ​​the open area A1 to the total area of ​​the open area A1 and the sealed areas A2 and A3 is 72 to 93%, and preferably 72 to 83%. When the above ratio is 72 to 93%, a good balance is achieved between the ratio of the second flow passages (open area) used for heat exchange with the first honeycomb structure under normal conditions and the ratio of the second flow passages (sealed area) functioning as a heat capacity when the exhaust gas temperature drops, and the reforming ability at the inlet portion when the exhaust gas temperature drops can be improved while sufficiently ensuring heat exchange efficiency under normal conditions. When the above ratio is 72 to 83%, the balance between the ratio of the second flow passages (open area) used for heat exchange with the first honeycomb structure under normal conditions and the ratio of the second flow passages (sealed area) functioning as a heat capacity when the exhaust gas temperature drops is particularly good, and the reforming ability at the inlet portion when the exhaust gas temperature drops can be further improved while further ensuring the heat exchange efficiency under normal conditions.

[0075] If the ratio is less than 72%, the ratio of the second flow passages (open area) used for heat exchange with the first honeycomb structure under normal conditions is too small, resulting in a decrease in the heat exchange efficiency under normal conditions. On the other hand, if the ratio exceeds 93%, the ratio of the second flow passages (closed area) that function as a heat capacity when the exhaust gas temperature drops is too small, resulting in a decrease in the reforming ability at the inlet when the exhaust gas temperature drops. Furthermore, the area for holding the second honeycomb structure during canning is too small, which may damage the heat exchanger. The sealing regions are regions provided on both end face sides of the heat exchanger with respect to the opening region. Therefore, in the heat exchanger 100 shown in Fig. 1, the region where the coating layer 32b is formed is covered with the retaining mat 50 as shown in Fig. 4, but since it is not located on both end face sides of the heat exchanger with respect to the opening region, the region is not included in the area of ​​the sealing region.

[0076] The ratio of the area of ​​the opening region to the total area of ​​the opening region and the area of ​​the sealing region is determined by the shape of the retaining mat disposed between the heat exchanger and the metal casing, and therefore the ratio can be adjusted by adjusting the shape of the retaining mat (particularly the shape and position of the opening).

[0077] [Heat exchanger manufacturing method] Next, a method for producing the heat exchanger of the present invention will be described. In manufacturing the heat exchanger of the present invention, first, a heat exchanger including a first honeycomb structure and a second honeycomb structure is manufactured through the steps described below. Then, a support mat is wrapped around the manufactured heat exchanger, and the manufactured heat exchanger is housed in a metal casing to complete the heat exchanger. In the following, a case where silicon carbide and silicon are used as materials constituting the honeycomb structure will be described, but the materials constituting the honeycomb structure are not limited to the above materials.

[0078] The heat exchanger includes a forming step of forming a honeycomb formed body having a plurality of cells arranged in parallel in the longitudinal direction with a partition wall therebetween by forming a raw material paste containing, for example, silicon carbide powder, an organic binder, etc., a drying step of drying the honeycomb formed body formed by the forming step, a honeycomb aggregate fabricating step of bonding the honeycomb formed body to be a first honeycomb structure and the honeycomb formed body to be a second honeycomb structure, both of which have been dried by the drying step, via an adhesive layer paste to form an adhesive layer, to fabricate an aggregate of honeycomb formed bodies (honeycomb aggregate), and The heat exchanger can be manufactured by carrying out a columnar body fabrication process in which a honeycomb aggregate is processed into an approximately cylindrical shape, a coating layer paste application process in which a coating layer paste is applied to part of the outer periphery of the columnar body processed into an approximately cylindrical shape to form a coating layer paste layer, and a degreasing, impregnation, and bonding process in which the columnar body to which the coating layer paste has been applied is degreased, heated to a high temperature, and impregnated with molten silicon to manufacture a heat exchanger consisting of a honeycomb structure made of a composite material of silicon carbide and silicon, an adhesive layer, and a coating layer.

[0079] (molding process) In the molding process, first, silicon carbide powder, an organic binder, and the like are mixed to prepare a raw material paste. The raw material paste may further contain a pore-forming agent, a forming aid, a dispersion medium such as water, and the like.

[0080] The organic binder is not particularly limited, but examples thereof include methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, polyethylene glycol, phenol resin, epoxy resin, and the like, and two or more of these may be used in combination.

[0081] The pore-forming agent is not particularly limited, and examples thereof include acrylic resin, coke, starch, etc. The pore-forming agent refers to a material used for introducing pores into the inside of a honeycomb structure (or a honeycomb segment) when manufacturing the honeycomb structure (or a honeycomb segment).

[0082] The molding aid is not particularly limited, but examples thereof include ethylene glycol, dextrin, fatty acid, fatty acid soap, polyalcohol, etc., and two or more of these may be used in combination.

[0083] The dispersion medium is not particularly limited, but examples thereof include water, organic solvents such as benzene, and alcohols such as methanol, and two or more of these may be used in combination.

[0084] When preparing the raw material paste, it is desirable to mix and knead the ingredients. The ingredients may be mixed using a mixer, an attritor, or the like, or kneaded using a kneader, or the like.

[0085] In the molding step, the raw material paste is extrusion molded to obtain a honeycomb molded body in which a plurality of cells are arranged in parallel in the longitudinal direction with partition walls between them. The shape of the honeycomb formed body is not particularly limited, but a prismatic shape is preferable, and a quadrangular prismatic shape is more preferable. In addition, since it is preferable that the honeycomb formed body to become the first honeycomb structure (or the first honeycomb segment) and the honeycomb formed body to become the second honeycomb structure (or the second honeycomb segment) have different partition wall thicknesses and cell densities, it is necessary to prepare honeycomb formed bodies having shapes that match these.

[0086] When the end face of the honeycomb formed body is rectangular, it is desirable that the length of the longer side is 20 to 120 mm.

[0087] (drying process) Next, a drying step is carried out to dry the honeycomb formed body to obtain a dried honeycomb body. In the drying step, the honeycomb molded body is dried using a dryer such as a microwave dryer, a hot air dryer, a dielectric dryer, a reduced pressure dryer, a vacuum dryer, or a freeze dryer to produce a dried honeycomb body. By this step, a dried honeycomb body for the first honeycomb structure (or the first honeycomb segment) and a dried honeycomb body for the second honeycomb structure (or the second honeycomb segment) are produced.

[0088] (Honeycomb assembly manufacturing process) In this step, an adhesive layer paste having substantially the same composition as the raw material paste is used, and the dried honeycomb bodies are bonded via the adhesive layer paste to produce an assembly of the dried honeycomb bodies (honeycomb assembly). In this case, by undergoing the degreasing, impregnation and bonding processes, the two types of honeycomb dried bodies having different shapes as described above, i.e., a honeycomb dried body for a first honeycomb structure (or a first honeycomb segment) and a honeycomb dried body for a second honeycomb structure (or a second honeycomb segment), are combined and bonded together to form the heat exchanger configuration described above.

[0089] FIG. 6 is a perspective view that diagrammatically shows one example of a honeycomb aggregate for manufacturing the heat exchanger shown in FIG. The honeycomb dried body assembly 90 shown in FIG. 6 is a rectangular columnar honeycomb assembly 90 in which first honeycomb structures 10 and second honeycomb structures 20 are alternately stacked and bonded via adhesive layers 19. The honeycomb assembly 90 has three layers of first honeycomb structures 10 and four layers of second honeycomb structures 20. One layer of the first honeycomb structure 10 is made of one first honeycomb segment 11. One layer of the second honeycomb structure 20 is made of two second honeycomb segments 21 bonded via adhesive layers 18.

[0090] (Cylinder manufacturing process) In this step, the above-mentioned honeycomb aggregate having a rectangular column shape is cut using a cutting tool such as a diamond cutter to process it into a cylindrical shape in which the second flow passages of the second honeycomb structure are opened on the outer circumferential surface.

[0091] (Coating layer paste application process) The paste for the coating layer is applied to the entire surface of the first honeycomb structure constituting the outer peripheral surface of the pillar-shaped body, and then dried and solidified to form a layer that serves as the coating layer. The coating layer paste may have substantially the same composition as the raw material paste. After the degreasing, impregnation and adhesion steps described below, a coating layer paste application step may be carried out, and the coating layer paste may be dried and heated to solidify, thereby forming a coating layer.

[0092] (Degreasing, impregnation, and adhesion processes) In this process, the honeycomb aggregate, which has been processed into a cylindrical shape and on which a layer that will become a coating layer has been formed, is subjected to a degreasing process, and then to an impregnation and adhesion process. Therefore, in this process, silicon (metallic silicon) is placed on the bottom of a ceramic container with an open top, and a honeycomb aggregate is placed inside the container via a support made of porous ceramic. After the degreasing process, the impregnation and bonding process is carried out.

[0093] In the degreasing process, the aggregate of the dried honeycomb bodies dried in the drying process is heated at a temperature of 400 to 1400° C. to burn off the organic matter contained in the dried honeycomb bodies. The degreasing temperature is more preferably 400 to 600° C. The atmosphere is preferably an oxygen-containing atmosphere.

[0094] Subsequently, the impregnation and adhesion process is carried out. That is, the degreased body after the degreasing process is heated at a temperature of 1420 to 2000°C to produce a composite material of silicon carbide and silicon. The heating temperature is more preferably 1420 to 1600°C. The atmosphere is preferably an inert gas atmosphere. By heating at the above temperature, the molten silicon (silicon metal) penetrates by capillary action through the porous support into the gaps between the silicon carbide particles that make up the partitions of the degreased body, and the silicon is impregnated into the gaps.

[0095] The molten silicon also penetrates between the degreased body of the adhesive layer paste and the degreased body of the coating layer paste, forming a composite material with the silicon carbide contained in the degreased body. The degreased body of the adhesive layer paste becomes an adhesive layer that firmly bonds the honeycomb structures (or honeycomb segments) together. The degreased body of the coating layer paste becomes a coating layer that covers the outer periphery.

[0096] When the temperature of the impregnation and adhesion process is within the above temperature range, the heat exchanger obtained is an unsintered honeycomb structure in which most of the silicon carbide, which is a constituent of the heat exchanger, is not sintered and silicon carbide particles and silicon exist independently. In other words, the partition walls that make up the honeycomb structure (or honeycomb segment) are composed of a composite material of silicon and silicon carbide in which independent silicon carbide particles are bonded by silicon existing around them. This unsintered honeycomb structure has a high Young's modulus and is difficult to deform, making it useful as a heat exchanger.

[0097] Furthermore, by undergoing the above-mentioned steps, it is possible to produce a heat exchanger in which a first honeycomb structure in which a large number of cells that become first flow passages for fluid are arranged in parallel in the longitudinal direction separated by partition walls, and a second honeycomb structure in which a large number of cells that become second flow passages for fluid are arranged in parallel in the longitudinal direction separated by partition walls, are combined such that the first flow passages and the second flow passages intersect.

[0098] In the manufacturing method for the heat exchanger of the present invention, a degreasing process is performed to degrease each of the dried honeycomb bodies, and then a normal firing process is performed to produce a honeycomb fired body made of a porous silicon carbide sintered body. Then, a bonding process is performed to bond the honeycomb fired bodies together, a processing process is performed to process the honeycomb fired bodies into a circumferential shape, an impregnation / bonding process is performed to impregnate the honeycomb fired bodies with silicon, a process is performed to form a coating layer, a process is performed to form a plugging region, and the like may be performed.

[0099] (Catalyst Supporting Process) The heat exchanger of the present invention can be used as a fuel reforming catalyst by supporting a catalyst such as a fuel reforming catalyst on the heat exchanger. As a method for supporting a catalyst such as a fuel reforming catalyst made of a precious metal such as rhodium on the above-mentioned heat exchanger, for example, a method in which a honeycomb structure is immersed in a solution containing precious metal particles or complexes, then pulled out and heated can be mentioned.

[0100] The resulting heat exchanger is then wrapped with a support mat and housed in a metal casing. In this case, the shape of the retaining mat is selected so that the surface of the second honeycomb structure on the outer peripheral surface of the heat exchanger has an opening region where the second flow passage is not covered by the retaining mat and opens to the outer peripheral surface of the heat exchanger, and plugged regions are provided on both end faces of the heat exchanger relative to the opening region and where the second flow passage is covered by the retaining mat, and the proportion of the opening region to the total area of ​​the opening region and the plugged region is 72 to 93%. When wrapping the retaining mat around the heat exchanger, a wound body is produced by aligning the position where the second flow passage of the heat exchanger opens on the outer peripheral surface of the heat exchanger with the position of the mat opening of the retaining mat, and the wound body is then pushed into and fixed in a metal casing to obtain a reformer.

[0101] An example of a heat exchanger constituting a heat exchanger device according to a second embodiment of the present invention will be described with reference to FIGS. FIG. 7 is a perspective view showing a schematic diagram of a heat exchanger constituting a heat exchanger device according to a second embodiment of the present invention, and FIG. 8 is a cross-sectional view of the heat exchanger shown in FIG. 7 taken along line VIII-VIII.

[0102] As shown in Figures 7 and 8, a heat exchanger 200 constituting a heat exchanger device according to the second embodiment of the present invention is a cylindrical heat exchanger 200 formed by combining a first ceramic honeycomb structure 110 in which a number of first cells 113 serving as first flow passages for fluid are arranged in parallel in the longitudinal direction separated by a first partition wall 112, and a second ceramic honeycomb structure 120 in which a number of second cells 123 serving as second flow passages for fluid are arranged in parallel in the longitudinal direction separated by a second partition wall 122, such that the first flow passages (first cells 113) and second flow passages (second cells 123) intersect.

[0103] 7 and 8, the extension direction of the first cells 113 constituting the first honeycomb structure 110 is the vertical direction (the direction indicated by the arrow z in Figs. 7 and 8). The extension direction of the second cells 123 constituting the second honeycomb structure 120 is the horizontal direction (the direction indicated by the arrow y in Fig. 7). In the first honeycomb structure 110 and the second honeycomb structure 120, the flow passages intersect with each other, so that two types of fluids (particularly gases) can easily flow and heat exchange can be efficiently performed.

[0104] In a heat exchanger 200 constituting a heat exchanger device according to a second embodiment of the present invention, a second honeycomb structure 120 is disposed on both sides of a first honeycomb structure 110 with adhesive layers 119 interposed therebetween. As in the case of the heat exchanger constituting the heat exchange device according to the second embodiment of the present invention, the single layer first honeycomb structure 110 and the single layer second honeycomb structure 120 may each be constructed by bonding two or more honeycomb segments together via an adhesive layer.

[0105] In the heat exchanger 200 shown in Figures 7 and 8, first cells 113 that serve as first flow passages of the first honeycomb structure 110 open on both end faces, and second cells 123 that serve as second flow passages of the second honeycomb structure 120 open on the outer circumferential face. The outer peripheral surface is covered with a coating layer 132. The coating layer 132 has a coating layer 132a that covers the entire surface of the first honeycomb structure 10 that constitutes the outer peripheral surface. The portion covered with the coating layer 132 has a higher mechanical strength than the portion not covered with the coating layer, and therefore the portion covered with the coating layer 132 can be used as a portion to which the canning pressure is applied.

[0106] In addition, since the entire surface of the first honeycomb structure 110 constituting the outer peripheral surface is covered with the coating layer 132, it is possible to prevent the fluid flowing through the first cells 113 which form the first flow passages and the fluid flowing through the second cells 123 which form the second flow passages from mixing with each other.

[0107] The volume of the heat exchanger constituting the heat exchanger according to the second embodiment of the present invention is desirably 1.2 to 3.2 liters. When the volume of the heat exchanger constituting the heat exchanger according to the second embodiment of the present invention is 1.2 to 3.2 liters, the heat exchanger has an appropriate volume, making it easy to install in a vehicle, etc., and capable of fully exerting its effect as a heat exchanger. If the volume of the heat exchanger constituting the heat exchanger device of the second embodiment of the present invention is less than 1.2 liters, the volume of the heat exchanger will be too small, making it difficult to support a sufficient amount of catalyst, while if the volume of the heat exchanger constituting the heat exchanger device of the second embodiment of the present invention exceeds 3.2 liters, the capacity of the heat exchanger device will be too large, making it difficult to install it in a vehicle.

[0108] The material of the honeycomb structure constituting the heat exchanger constituting the heat exchanger according to the second embodiment of the present invention, the type of catalyst supported, and other configurations of the above heat exchanger are the same as those of the honeycomb structure constituting the heat exchanger constituting the heat exchanger according to the first embodiment. In addition, the manufacturing method of the heat exchanger according to the second embodiment of the present invention is also the same as that of the heat exchanger according to the first embodiment of the present invention, so the description thereof will be omitted.

[0109] In the heat exchanger constituting the heat exchanger device according to the first embodiment of the present invention, three layers of the first honeycomb structure and four layers of the second honeycomb structure are arranged alternately, and in the heat exchanger constituting the heat exchanger device according to the second embodiment of the present invention, the second honeycomb structure is arranged on both sides of the first honeycomb structure. However, the heat exchanger constituting the heat exchanger device of the present invention is not limited to these embodiments. As long as a first honeycomb structure having a large number of cells that become a first flow passage for fluid arranged in parallel in the longitudinal direction separated by partition walls and a second honeycomb structure having a large number of cells that become a second flow passage for fluid arranged in parallel in the longitudinal direction separated by partition walls are combined such that the extension direction of the first flow passage and the extension direction of the second flow passage intersect, the number of combinations is not limited, but it is preferable that the first honeycomb structure and the second honeycomb structure are arranged alternately.

[0110] The reformer of the present invention is a reformer equipped with the heat exchange device of the present invention, characterized in that the second honeycomb structure is configured to allow exhaust gas discharged from an internal combustion engine and flowing through a main exhaust pipe to pass therethrough, and the first honeycomb structure has a reforming catalyst supported on its partition walls and is configured to allow exhaust gas that has flowed into an exhaust gas recirculation pipe branched off from the main exhaust pipe to pass therethrough.

[0111] When the reformer of the present invention is configured as described above, the heat of the exhaust gas can be effectively supplied from the second honeycomb structure to the first honeycomb structure, and the reformer can effectively perform the function of reforming the fuel for an internal combustion engine to improve fuel efficiency.

[0112] FIG. 9 is an explanatory diagram that shows a schematic diagram of a fuel reformed gasoline engine system equipped with a reformer of the present invention. In this fuel reforming gasoline engine system 300, an exhaust pipe 42 through which exhaust gas discharged from a gasoline engine 41 passes is branched into a main exhaust pipe 43 and an exhaust gas recirculation pipe 44 (hereinafter referred to as an EGR pipe), and a reformer 80 containing a heat exchanger 70 functioning as a fuel reforming catalyst is disposed in the EGR pipe 44. As shown in FIG. 9, the main exhaust pipe 43 is also connected to the reformer 80, and the gas flowing through the main exhaust pipe 43 is introduced into and discharged from the cells of the second honeycomb structure through the mat openings 51c, 51d, 51e, 51f, 51g, and 51h of the retaining mat 50 and the mat openings which are the fluid inlet and fluid outlet of the heat exchanger 100, while the gas flowing through the EGR pipe 44 passes through the cells of the first honeycomb structure constituting the heat exchanger 100 and undergoes heat exchange. In the figure, 45 is an automatic valve that opens and closes as appropriate depending on the situation.

[0113] A reforming fuel injection device 46 is disposed at the inlet of the reformer 80 in the EGR pipe 44, and reforming fuel is injected from this reforming fuel injection device 46. Meanwhile, a port type fuel injection device 48 is disposed in an intake pipe 49 of the gasoline engine 41, and fuel for the engine is injected at the time of intake.

[0114] In the reformer 80, the fuel injected from the reforming fuel injection device 46 reacts with the water vapor in the exhaust gas and the hydrocarbons that are the main components of gasoline fuel, activated by the fuel reforming catalyst supported on the heat exchanger 100, and is converted into hydrogen, carbon monoxide, and methane. The hydrogen-containing gas with this composition mixes with the intake air of the engine and also with the fuel injected from the port type fuel injection device 48, forming an air-fuel mixture that enters the gasoline engine 41 and is combusted inside the gasoline engine 41. The hydrogen mixed into the air-fuel mixture can increase the combustion speed, thereby improving the combustion efficiency of the gasoline engine 41.

[0115] In the first honeycomb structure in the reformer 80, heat is absorbed by an endothermic reaction in the presence of the above-mentioned fuel reforming catalyst, but in the heat exchange device of the present invention, the heat of the exhaust gas can be effectively supplied from the second honeycomb structure to the first honeycomb structure, the temperature drop is suppressed, and the performance as a reforming catalyst that reforms the fuel of an internal combustion engine (gasoline engine) to improve fuel efficiency can be effectively exhibited. Furthermore, when the heat exchanger is made of silicon carbide and silicon, it is not easily corroded by the hydrogen contained in the reformed gas.

[0116] (Example) EXAMPLES Hereinafter, examples will be given that more specifically disclose the embodiments of the present invention, however, the present invention is not limited to these examples.

[0117] Example 1 56.3% by weight of coarse silicon carbide powder having an average particle size of 22 μm and 24.1% by weight of fine silicon carbide powder having an average particle size of 0.5 μm were mixed, and 4.4% by weight of an organic binder (methyl cellulose), 0.8% by weight of a lubricant (UNILUBE manufactured by NOF Corp.), 0.8% by weight of glycerin, 2.2% by weight of oleic acid, and 11.4% by weight of water were added to the resulting mixture and kneaded to obtain a raw material paste.

[0118] After that, the raw material paste was extrusion molded using a mold for manufacturing honeycomb segments that constitute the first honeycomb structure, and a mold for manufacturing a honeycomb molded body that constitutes the second honeycomb structure, to produce a honeycomb molded body.

[0119] The honeycomb formed body for the honeycomb segment constituting the first honeycomb structure produced by the above process had a rectangular end face shape of 14.6 mm × 105.4 mm, a length of 140 mm, and a cell density of 47 cells / cm. 2 (300 pieces / inch 2) and the thickness of the partition wall was 0.25 mm. The honeycomb formed body for the honeycomb segment constituting the second honeycomb structure produced by the above process had a rectangular end face shape of 14.6 × 70 mm, a length of 105 mm, and a cell density of 47 cells / cm. 3 (300 pieces / inch 3 ), and the thickness of the partition was 0.25 mm.

[0120] Next, the green honeycomb formed body was dried using a microwave dryer to prepare a dried honeycomb formed body.

[0121] The obtained dried honeycomb bodies for the honeycomb segments constituting the first honeycomb structure and the dried honeycomb bodies for the honeycomb segments constituting the second honeycomb structure were used, and the raw material paste was used as an adhesive to combine the dried honeycomb bodies so that the assembly of the dried honeycomb bodies after the manufacturing process (honeycomb assembly) had the configuration shown in Fig. 6. The thickness of each adhesive layer was set to 1 mm. The first honeycomb structure was composed of one first honeycomb segment, and the second honeycomb structure was composed of two second honeycomb segments. The dimensions of the dried honeycomb body were such that the surface of the second honeycomb structure where the second flow passages were exposed was a substantially rectangular parallelepiped shape with a width of 108.2 mm, a length of 140 mm, and a depth of 105 mm.

[0122] The obtained honeycomb dried body aggregate was machined into a cylindrical shape with a diameter of 105 mm and a length of 140 mm so that both end faces of the honeycomb dried body became the end faces of the first honeycomb structure. Furthermore, a coating layer paste was applied to the entire surface of the first honeycomb structure constituting the outer peripheral surface of the cylindrical honeycomb aggregate and a part of the surface of the second honeycomb structure, and then dried and solidified.

[0123] The honeycomb dried body assembly with the coating layer formed thereon was placed, via a support, in a ceramic container with metal silicon placed on the bottom surface, and then carried into a heating furnace. After a degreasing process in which the honeycomb dried body was degreased at 400°C in an air atmosphere, the atmosphere inside the heating furnace was replaced with argon gas, and an impregnation and bonding process was carried out under heating conditions of 1450°C for 1 hour, to obtain a heat exchanger with the configuration shown in Figure 1.

[0124] The obtained heat exchanger having the configuration shown in FIG. 1 had an outer diameter of 105 mm and a length of 140 mm, and the cell density of the honeycomb segments constituting the first and second honeycomb structures was 47 cells / cm. 2 (300 pieces / inch 2 ) and the thickness of the partition wall is 0.25 mm in both cases. The first honeycomb structure was composed of one first honeycomb segment, and the second honeycomb structure was composed of two second honeycomb segments bonded together via their end faces with an adhesive layer. In addition, the flow paths (cells that become the first flow paths) of the first honeycomb segment constituting the first honeycomb structure and the flow paths (cells that become the second flow paths) of the second honeycomb segment constituting the second honeycomb structure were arranged to intersect with each other.

[0125] The mat was cut into a shape having recesses, protrusions and openings as shown in FIG. 3 to prepare a support mat. The obtained support mat was wrapped around a heat exchanger having the configuration shown in Fig. 1 and housed in a cylindrical metal casing having an opening similar to that of the support mat and an inner diameter slightly larger than the diameter of the heat exchanger, to obtain a heat exchanger according to Example 1. The thickness of the mat after housing was 4 mm. In the heat exchanger according to Example 1, the ratio of the opening area to the total area of ​​the opening area and the sealing area was 90%.

[0126] (Example 2, Comparative Examples 1-2) The heat exchange devices of Example 2 and Comparative Examples 1 and 2 were manufactured using the same procedures as Example 1, except that the shape of the opening formed in the retaining mat was changed to change the ratio of the area of ​​the opening area to the total area of ​​the opening area and the sealing area to the values ​​shown in Table 1.

[0127] (evaluation) [Evaluation of canning properties] When the heat exchanger was wrapped with the retaining mat and housed in the metal casing, the heat exchanger was checked for damage and evaluated according to the following criteria. The results are shown in Table 1. However, the thickness and basis weight of the support mats were all the same. [evaluation] ◯: No damage such as cracks occurred in the heat exchanger after canning. ×: Damage such as cracks occurred in the heat exchanger after canning.

[0128] [Heat exchange test and retention stability measurement] A gas at 800°C was passed through the cells constituting the second honeycomb structure at a flow rate of 50 g / sec, and a gas at 500°C was passed through the cells constituting the first honeycomb structure at a flow rate of 15 g / sec for 10 minutes. After 10 minutes, the temperature of the gas flowing out of the first honeycomb structure was measured and evaluated according to the following criteria. The results are shown in Table 1. Also, it was confirmed whether the retaining mat and / or the heat exchanger were displaced before and after this operation. The results are shown in Table 1. [Evaluation of heat exchange efficiency] ◯: The temperature of the gas flowing out from the first honeycomb structure is 600° C. or higher. ×: The temperature of the gas flowing out from the first honeycomb structure is less than 600°C. [Evaluation of storage stability] ◯: No misalignment of the retaining mat and heat exchanger is observed. ×: Misalignment of the retaining mat and / or heat exchanger is observed.

[0129] [Table 1]

[0130] As shown in Table 1, in the heat exchange devices of Examples 1 and 2, even when the temperature of the gas flowing into the cells constituting the second honeycomb structure decreased, the temperature of the gas flowing out of the first honeycomb structure was able to be maintained at 600°C or higher. The heat exchanger according to Comparative Example 1 was damaged during canning. This is believed to be because the area (plugging area) where the second honeycomb structure contacts the support mat is narrower than in Examples 1 and 2, and excessive pressure was applied to the plugging area, leading to the damage. It was found that when the basis weight of the support mat was adjusted so that the heat exchanger according to Comparative Example 1 would not be damaged during canning, the heat exchanger was displaced in the heat exchange test, and the support stability was insufficient. In the heat exchange device according to Comparative Example 2, the temperature of the gas flowing out of the first honeycomb structure during normal heat exchange was less than 600° C. This is believed to be because the ratio of the plugged regions was too high, which reduced the heat exchange efficiency during normal heat exchange. [Explanation of symbols]

[0131] 10, 110 First honeycomb structure 11, 111 First honeycomb segment 12, 112 First bulkhead 13, 113 first cell (first flow passage) 18, 19, 119 Adhesive layer 20, 120 Second honeycomb structure 21, 121 Second honeycomb segment 22, 122 Second bulkhead 23, 123 Second cell (second flow passage) 32, 32a, 32b, 132, 132a, 132b Coating layer 41 Gasoline engine 42 Exhaust pipe 43 Main exhaust pipe 44 Exhaust gas recirculation pipe (EGR pipe) 45 Automatic valve 46 Fuel injection device for reforming 48 Port fuel injection system 49 Suction piping 50 Retaining Mat 51 Matt 51a Convex part 51b Recess 51c, 51d, 51e, 51f, 51g, 51h opening 60 Metal Casing 60c, 60d, 60e, 60f, 60g, 60h opening 70 Heat exchange equipment 80 Reformer 90 Assembly of dried honeycomb bodies 100, 200 heat exchanger 300 Gasoline Engine System A1 opening area A2, A3 sealing area

Claims

1. a heat exchanger including a first honeycomb structure in which a number of cells serving as first fluid flow paths are arranged in parallel in the longitudinal direction with partition walls therebetween, and a second honeycomb structure in which a number of cells serving as second fluid flow paths are arranged in parallel in the longitudinal direction with partition walls therebetween, the first flow paths and the second flow paths being combined together such that the first flow paths and the second flow paths intersect; a metal casing that houses the heat exchanger; A heat exchanger comprising: a retaining mat disposed between the heat exchanger and the metal casing; the heat exchanger has a generally cylindrical shape with the first flow passage opening at both end surfaces and the second flow passage opening at an outer circumferential surface thereof, the retaining mat is disposed along the outer circumferential surface of the heat exchanger so as not to cover a portion of the second flow passage that opens to the outer circumferential surface, The entire surface of the first honeycomb structure of the outer peripheral surface of the heat exchanger is covered with a coating layer, Among the outer peripheral surface of the heat exchanger, a surface of the second honeycomb structure has an opening region in which the second flow passage is not covered by the retaining mat and opens to the outer peripheral surface of the heat exchanger, and a plugging region provided on each of the end face sides of the heat exchanger with respect to the opening region, the second flow passage being covered by the retaining mat, A heat exchange device, characterized in that a ratio of an area of ​​the open region to a total area of ​​the open region and the sealed region is 72 to 93%.

2. The heat exchange device according to claim 1, wherein the retaining mat has a thickness of 3 to 5 mm.

3. 3. The heat exchange device according to claim 1, wherein the second honeycomb structure is disposed on both sides of the first honeycomb structure.

4. 4. The heat exchange device according to claim 1, wherein a catalyst is supported on partition walls of cells constituting the first honeycomb structure.

5. The heat exchange device according to any one of claims 1 to 4, wherein a ratio of a total opening area of ​​the second flow passages to a total opening area of ​​the first flow passages (total opening area of ​​the second flow passages / total opening area of ​​the first flow passages) is 1.25 to 2.

6. 6. The heat exchange device according to claim 1, wherein the first honeycomb structure and the second honeycomb structure are both made of silicon carbide and silicon.

7. The heat exchange device according to any one of claims 1 to 6, wherein the first honeycomb structure and the second honeycomb structure are each formed by bonding a plurality of ceramic honeycomb segments together via an adhesive layer.

8. The heat exchange device of claim 7 , wherein the adhesive layer comprises silicon carbide and silicon.

9. 9. The heat exchange device according to claim 1, wherein the volume of the heat exchanger is 1.2 to 3.2 liters.

10. The heat exchanger is configured such that the first honeycomb structures and the second honeycomb structures are alternately arranged, and includes three layers of the first honeycomb structures and four layers of the second honeycomb structures. The heat exchanger according to any one of claims 1 to 9,

11. A reformer comprising the heat exchange device according to any one of claims 1 to 10, A reformer characterized in that the second honeycomb structure is configured to allow exhaust gas emitted from an internal combustion engine and flowing through a main exhaust pipe to pass therethrough, and the first honeycomb structure has a reforming catalyst supported on its partition walls and is configured to allow exhaust gas that flows into an exhaust gas recirculation piping branched off from the main exhaust pipe to pass therethrough.

Citation Information

Patent Citations

  • Crosscurrent heat exchanger and production thereof

    JP1995151478A

  • Fuel reforming device for internal combustion engine

    JP2015166591A

  • Exhaust emission control device and holding seal material

    JP2016138554A

  • Honeycomb filter

    JP2017170384A

  • Method for manufacturing heat exchanger

    JP2019174013A