Fluff Pulp

Fluff pulp production achieves reduced resource and chemical use through oxygen delignification, addressing the cost and environmental issues of traditional bleaching methods, maintaining absorption properties.

JP7565343B2Active Publication Date: 2024-10-10STORA ENSO OYJ
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022514469
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-04
Filing Date
2020-09-03
Publication Date
2024-10-10
Estimated Expiration
2040-09-03

AI Technical Summary

Technical Problem

Existing fluff pulp production methods are costly and environmentally burdensome due to extensive bleaching processes, which are necessary to achieve desired brightness levels.

Method used

Production of fluff pulp with reduced resource and chemical use by employing oxygen delignification and avoiding bleaching steps, maintaining suitable properties through controlled oxygen delignification and pH adjustment, resulting in a kappa number of 5 to 18 and ISO brightness of 30 to 60%, with specific volume and absorption time optimized.

Benefits of technology

Fluff pulp with desirable absorption properties is achieved while significantly reducing resource consumption and environmental impact, maintaining comparable performance to traditionally bleached pulp.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565343000001
    Figure 0007565343000001
  • Figure 0007565343000002
    Figure 0007565343000002
  • Figure 0007565343000003
    Figure 0007565343000003
Patent Text Reader

Abstract

The present invention provides a fibrous sheet having a kappa number in the range of 5 to 18, an ISO brightness in the range of 30 to 60% when in the form of a dry sheet, and a densitometric value of at least 19 dm when dry and defibrated. 3 / kg and an absorption time in the range of 2 to 4 seconds.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention provides a fiber optic cable having a kappa number in the range of 5 to 18, an ISO brightness in the range of 30 to 60% when in the form of a dry sheet, and an optical density of at least 19 dm when dry and defibrated. 3 The present invention relates to a fluff pulp having a specific volume of 1000 g / kg and an absorption time in the range of 2 to 4 seconds. The present invention also relates to a process for producing such fluff pulp and to uses of the fluff pulp. [Background technology]

[0002] Fluff pulp is usually made from softwood pulp, which is derived from sulfate pulping. Depending on the pulping method, the characteristics of fluff pulp vary. The source of softwood pulp can be various softwood species such as Scandinavian pine, spruce, southern pine, loblolly pine, slash pine, radiata pine, Douglas fir, hemlock cedar, white spruce, lodgepole pine, alpine fir, or mixtures thereof.

[0003] Bleaching is a common method to remove lignin and color compounds remaining after pulp cooking, thereby increasing the brightness of pulps, including fluff pulp. The industry practice to improve the appearance of fluff pulp is to bleach the pulp until it reaches a desired brightness (according to the Technical Association of the Pulp & Paper Industry ("TAPPI") or the International Organization for Standardization ("ISO"). Bleached pulp has a final ISO brightness of 85-94%. However, bleaching is expensive, environmentally hazardous, and often causes manufacturing bottlenecks.

[0004] The pulp in turn is bleached or delignified, which requires the use of several bleaching steps and several bleaching chemicals to reach the desired brightness level. Examples of bleaching agents are oxygen, hydrogen peroxide, ozone, peracetic acid, and chlorine dioxide. Summary of the Invention [Problem to be solved by the invention]

[0005] Considering the manufacturing costs, resource requirements and environmental impacts of bleaching, it would be desirable to be able to achieve suitable fluff pulp properties, particularly good absorption, while using fewer resources. [Means for solving the problem]

[0006] The present invention provides a fiber optic cable having a kappa number in the range of 5 to 18, an ISO brightness in the range of 30 to 60% when in the form of a dry sheet, and an optical density of at least 19 dm when dry and defibrated. 3 / kg and an absorption time in the range of 2 to 4 seconds.

[0007] Surprisingly, it has been found that it is possible to produce fluff pulp with suitable properties while using significantly less resources, especially less chemical and energy.

[0008] The present invention also relates to a method for producing said fluff pulp.

[0009] The present invention also relates to the use of said fluff pulp. The fluff pulp is produced and delivered to the purchaser in rolls. The fluff pulp is first defibrated. The defibrated pulp is then used, for example, in the manufacture of absorbent cores for hygiene products and in airlaid nonwovens for various applications such as diapers, incontinence products, feminine hygiene products, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Detailed Description of the Invention As used herein, the term "fluff" means fluff pulp that has been defibrated, i.e., fiberized or shredded.

[0011] As used herein, the term "Kappa number" refers to the measurement of Kappa number according to the standard ISO 302:2015.

[0012] The kappa number of the fluff pulp according to the present invention is in the range of 5-18, preferably in the range of 5-15, for example in the range of 6-15, and more preferably in the range of 5-12 or 9-13.

[0013] As used herein, the term “ISO Brightness” refers to a measurement of brightness according to the standard ISO 2470.

[0014] The ISO brightness of the fluff pulp according to the present invention, when in the form of a dry sheet (i.e. before defibration), is in the range of 30 to 60%, preferably in the range of 35 to 55%, or 30 to 40%, more preferably in the range of 36 to 50% or 34 to 39%.

[0015] As used herein, the specific volume of fluff pulp in the dry state (specific volume of fluff pulp after defibration, i.e. in the defibrated state) refers to the specific volume measured according to the standard SCAN-C 33:80 and means the measurement of the volume of a test piece in the dry state per unit mass (weight) of fluff. A 3 g sample of fluff with a diameter of 50 mm is molded in a molding unit. The sample is placed in a sample holder and a load of 2.8 kPa is applied. The dry specific volume is measured after 30 seconds (measured as the average of 5 replicates).

[0016] The fluff according to the invention has a specific volume in the dry state (conditioned according to ISO 187) of at least 19 dm 3 / kg, preferably 19 to 23 dm 3 / kg range, e.g. 19~22dm3 / kg range.

[0017] As used herein, the term "absorption time" refers to the absorption properties of fluff pulp according to standard SCAN-C 33:80, which includes the measurement of the time it takes to completely saturate a standardized specimen with absorbed liquid. A 3 g fluff sample with a diameter of 50 mm is molded in a molding unit. The sample is placed in a sample holder and a load of 2.8 kPa is applied. Tap water (23°C) is applied to the bottom and the time required for the water to reach the top of the sample is recorded (measured as the average of five replicates).

[0018] As used herein, the term "absorbent capacity" refers to the property of the absorption capacity (volume) of fluff pulp according to standard SCAN-C 33:80. A 3 g fluff sample with a diameter of 50 mm is molded in a molding unit. The sample is placed in a sample holder and a load of 2.8 kPa is applied. Tap water (23°C) is applied to the bottom and the time required for the water to reach the top of the sample is recorded. After 30 seconds, the addition of water is stopped. After another 30 seconds, the absorbent capacity is recorded by weighing the specimen (measured as the average of 5 replicates).

[0019] As used herein, the "knot content" of fluff pulp refers to the knot content measured using an Alpine Air Jet with a screen DIN ISO 3310 1.4 mm. A sample of the fluff is agitated above a wire using a negative pressure of 4000 kPa for 10 minutes. The knots remaining on the wire are weighed and reported as a percentage of the total weight of the sample (measured as the average of two replicates).

[0020] The knot content of the fluff pulp according to the invention is preferably less than 13%.

[0021] The fluff pulp according to the present invention can be produced by the following steps: a) preparing a sulfate pulp; b) washing, screening and cleaning the pulp; c) subjecting the pulp to oxygen delignification; d) washing the pulp that has been subjected to oxygen delignification and optionally adjusting the pH of the pulp; e) drying the pulp to obtain a rolled fluff pulp having a moisture content of less than 10% by weight.

[0022] The pulp is a sulfate pulp (kraft pulp). The fibres of the fluff pulp according to the invention are preferably derived from conifers (softwoods), such as spruce and / or pine. Preferably, the sulfate pulp is at least 90% derived from conifers, and less than 10% of hardwood has been used in the preparation of the sulfate pulp. Thus, the sulfate pulp is mainly derived from conifers, but may contain minor amounts of hardwood. The length-weighted average fibre length (measured with Metso Pulp Expert) is preferably in the range of 1.8-2.5 mm, for example in the range of 1.9-2.2 mm. The pulp is washed, sieved and cleaned before being subjected to the oxygen delignification step.

[0023] The oxygen delignification step is carried out using methods known in the art and can be carried out in one or more steps. The pulp is subjected to the oxygen delignification step in a wet state. Preferably, the oxygen delignification is carried out until the pulp subjected to the oxygen delignification reaches a kappa number in the range of 5 to 18.

[0024] The oxygen delignified pulp is washed. Washing is usually carried out using water and can be carried out in one or more steps and may involve filtration. As part of the washing or immediately after the washing step, the pH can be adjusted. Preferably, the pH of the washed pulp should be in the range of 5 to 8, for example in the range of 5 to 7. The washed pulp preferably contains less than 0.5% by weight (based on solids) of extractives, more preferably less than 0.2% by weight of extractives, even more preferably less than 0.1% by weight of extractives, most preferably less than 0.05% by weight of extractives. In this context, extractives are, for example, resins and fatty acids.

[0025] Optionally, hydrogen peroxide can be added to the washed pulp prior to the drying step.

[0026] The washed pulp is dried in a dryer using methods known in the art. The dried pulp is formed into rolls after drying. The dried material has a moisture content of less than 10% by weight (ISO 287), preferably less than 9% by weight, for example in the range of 6-9% by weight.

[0027] Preferably, the fluff pulp according to the invention has not been bleached. More preferably, the fluff pulp according to the invention has not been ECF (elemental chlorine free) or TCF (totally chlorine free) bleached.

[0028] Fluff pulp can be treated with aluminum sulfate solution to adjust the pH to 5.5-6.5 in the dryer stock preparation to reduce defibration energy and knot content. This treatment has a minor effect on the absorbent properties.

[0029] The fluff according to the present invention (i.e., the defibrated form of fluff pulp) can be used in articles and products where fluff is typically used. Thus, fluff can be used in absorbent cores of baby diapers, incontinence products, and feminine hygiene products. Fluff is also the main component of airlaid nonwovens.

[0030] Thus, after being defibrated, the fluff pulp according to the present invention can be used, for example, in absorbent cores and airlaid nonwovens. It can be used as or in liquid absorbing materials, for example, as absorbents in diapers, such as baby diapers and incontinence products. It can also be used, for example, in napkins and tissues. Such products can be produced using methods known in the art. The products typically include one or more additional components, such as superabsorbents, polymers, wetting agents, viscose / rayon / lyocell fibers, bicomponent fibers, cotton fibers, other fibers, standard latex binders, special latex binders, etc. EXAMPLES

[0031] Example 1 Kraft pulp samples were collected immediately after the production-scale pulp digester ("unbleached"), after the subsequent oxygen delignification step ("oxygen delignified"), and after the bleaching step ("bleached"). Thus, the "bleached" sample had been subjected to both oxygen delignification and bleaching.

[0032] Each pulp sample was rinsed thoroughly with water, centrifuged, granulated, and stored in a refrigerator prior to analysis.

[0033] Experimental sheets were formed from each type of pulp. The experimental sheets were defibrated using a laboratory hammer mill (Kamas H01).

[0034] Chemical and fluff properties were measured according to standard test methods. The results obtained are shown in Table 1. Kappa number was measured on the formed dry sheets. ISO brightness was measured on the formed dry sheets. Specific volume, absorption time and absorption capacity were measured on the fluffed material, i.e. after defibration. Sheet and pulp properties were evaluated in a conditioned climate according to ISO 187.

[0035] [Table 1]

[0036] The results reported in Table 1 show that the absorption and fluff properties (specific volume) of the bleached fluff pulp are almost identical compared to the oxygen delignified fluff pulp.

[0037] Example 2 Kraft pulp samples were collected immediately after the production-scale subsequent oxygen delignification step ("oxygen delignified") and after the bleaching step ("bleached"). Thus, the "bleached" sample had been subjected to both oxygen delignification and bleaching.

[0038] The pulp was then centrifuged, granulated and stored in dark plastic bags in the refrigerator at 25-30% dry content. One sheet of pulp was soaked, moistened and disintegrated. The pH of the pulp suspension was adjusted to 5.8, stirred for 10 min and then dewatered in a sheet former. A portion of the sample was treated with Al2(S04)3 solution, after which the pH was adjusted to 5.8 with NaOH.

[0039] The wet sheets were pressed and dried until the moisture content was less than 7%.

[0040] The chemical and fluff properties were measured according to standard test methods. The results obtained are shown in Table 1. The kappa number was measured on the formed dry sheets. The ISO brightness was measured on the formed dry sheets. The specific volume, absorption time and absorption capacity were measured on the fluffed material, i.e. after defibration. The sheet and pulp properties were evaluated in conditioned climatic conditions according to ISO 187.

[0041] [Table 2]

[0042] From the results reported in Table 2, it can be seen that the absorption and fluff properties (specific volume) of the bleached fluff pulp are almost identical compared to the oxygen delignified fluff pulp. The effect of treatment with aluminum sulfate solution on the absorption properties is slight.

[0043] Example 3 Production tests were carried out on a sulfate pulp fibre line equipped with a dryer for fluff pulp. The sulfate pulp was oxygen delignified and bleached or unbleached. The kappa number of the pulp measured online after oxygen delignification was between 8 and 11. Bleached reference fluff pulp was produced on the same fibre line, but this pulp was bleached to a kappa number of 1 in the bleach plant.

[0044] In the dryer, the pulps from test points 2 and 3 were treated with Al2(SO4)3 and the pH was adjusted with NaOH.

[0045] The fluff properties were tested according to standard test methods. The results obtained are shown in Table 1. ISO brightness was measured on the fluff pulp. Knot content, specific volume, absorption time and absorption capacity were measured on the fluffed material, i.e. after defibration. Sheet and pulp properties were evaluated under controlled climatic conditions according to ISO 187.

[0046] [Table 3]

[0047] The results reported in Table 3 show that the bleached fluff pulp has nearly identical absorption and fluff properties (specific volume) compared to the oxygen delignified fluff pulp.

[0048] In view of the above detailed description of the invention, other modifications and variations will be apparent to those skilled in the art. It should be apparent, however, that such other modifications and variations can be made without departing from the spirit and scope of the invention. Various aspects or embodiments that can be included in the present invention are summarized as follows. [1]. It has a kappa number in the range of 5 to 18, an ISO brightness in the range of 30 to 60% when in dry sheet form, and a densification coefficient of at least 19 dm 3 Fluff pulp having a specific volume of 1000 g / kg and an absorption time in the range of 2 to 4 seconds measured according to the SCAN-C 33:80 standard. [2]. The fluff pulp described in item 1 above, wherein the ISO brightness is in the range of 30 to 40%. [3]. The fluff pulp described in item 1 above, wherein the ISO brightness is in the range of 35 to 50%. [4]. The specific volume in a dry, defibrated state is 19 to 23 dm 3 The fluff pulp according to any one of items 1 to 3, wherein the fluff pulp has a molecular weight in the range of 1 / kg. [5]. 5. The fluff pulp according to any one of items 1 to 4, wherein the kappa number is in the range of 5 to 12. [6]. 5. The fluff pulp according to any one of items 1 to 4, wherein the ISO brightness is in the range of 36 to 50%. [7]. The fluff pulp according to any one of items 1 to 6, which is in the form of a roll. [8]. 1. A process for preparing fluff pulp, comprising: a) preparing a sulfate pulp; b) washing, sieving and cleaning the pulp; c) subjecting the pulp to an oxygen delignification treatment; d) washing the pulp that has been subjected to oxygen delignification treatment and optionally adjusting the pH of the pulp; e) drying the pulp to obtain fluff pulp in the form of rolls having a moisture content of less than 10% by weight. [9]. 9. The process according to claim 8, wherein the sulfate pulp is prepared from at least 90% softwood.

[10] . 10. The process according to item 8 or 9, wherein the oxygen delignification is carried out until the pulp subjected to oxygen delignification has a kappa number in the range of 5 to 18.

[11] . 11. The process according to any one of items 8 to 10 above, which does not include a bleaching step.

[12] . Fluff pulp obtained by the process described in any one of items 8 to 11 above.

[13] . A product comprising or prepared from defibrated fluff pulp, which, before being defibrated, is the fluff pulp described in any one of items 1 to 7 or item 12 above.

[14] . An airlaid nonwoven fabric comprising or prepared from defibrated fluff pulp, which, before being defibrated, is the fluff pulp described in any one of items 1 to 7 or item 12 above.

[15] . An absorbent core containing or prepared from defibrated fluff pulp, which, before being defibrated, is the fluff pulp described in any one of items 1 to 7 or item 12 above.

[16] . 16. A hygiene product comprising an absorbent core according to item 15.

Claims

1. A sheet of paper having a moisture content of less than 10% by weight, a kappa number in the range of 5 to 18, an ISO brightness in the range of 30 to 60% when in the form of a dry sheet, and a brightness of at least 19 dm 3 / kg and has an absorption time in the range of 2 to 4 seconds measured according to the SCAN-C 33:80 standard.

2. The fluff pulp of claim 1, wherein the ISO brightness is in the range of 30 to 40%.

3. The fluff pulp of claim 1, wherein the ISO brightness is in the range of 35 to 50%.

4. The specific volume in a dry defibrated state is 19 to 23 dm 3 The fluff pulp according to any one of claims 1 to 3, wherein the fluff pulp has a molecular weight in the range of 1 / kg.

5. The fluff pulp according to any one of claims 1 to 4, wherein the kappa number is in the range of 5 to 12.

6. The fluff pulp according to any one of claims 1 to 4, wherein the ISO brightness is in the range of 36 to 50%.

7. The fluff pulp according to any one of claims 1 to 6, which is in the form of a roll.

8. 1. A process for preparing fluff pulp, comprising: This process does not include a bleaching step. a) preparing a sulfate pulp; b) washing, sieving and cleaning the pulp; c) subjecting the pulp to an oxygen delignification treatment; d) washing the pulp that has been subjected to oxygen delignification treatment and optionally adjusting the pH of the pulp; e) drying the pulp to obtain fluff pulp in the form of a roll having a moisture content of less than 10% by weight, having a kappa number in the range of 5 to 18, an ISO brightness in the range of 30 to 60% when in the form of a dry sheet, a specific volume of at least 19 dm 3 / kg in a dry defibrated state, and an absorption time in the range of 2 to 4 seconds measured according to the SCAN-C 33:80 standard.

9. 9. The process of claim 8, wherein the sulfate pulp is prepared from at least 90% softwood.

10. 10. The process of claim 8 or 9, wherein the oxygen delignification is carried out until the pulp subjected to oxygen delignification has a Kappa number in the range of 5 to 18.

11. A product comprising or prepared from the fluff pulp described in any one of claims 1 to 7.

12. An airlaid nonwoven fabric comprising or prepared from the fluff pulp described in any one of claims 1 to 7.

13. An absorbent core comprising or prepared from fluff pulp described in any one of claims 1 to 7.

14. A sanitary product comprising an absorbent core as described in claim 13.

Citation Information

Patent Citations

  • Fluffed pulp

    JP2015151655A

  • Feed for ruminants

    JP2015198653A