Composite material and its manufacturing method

The composite material with a magnetic field enhancement layer and electromagnetic induction addresses temperature gradient issues, enabling efficient and cost-effective bonding of large composite parts with enhanced mechanical properties.

JP7565922B2Active Publication Date: 2024-10-11LEONARDO SPA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021535102
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-20
Filing Date
2019-12-20
Publication Date
2024-10-11
Estimated Expiration
2039-12-20

AI Technical Summary

Technical Problem

Current methods for consolidating and bonding composite materials, particularly those with thermoplastic matrices, face challenges such as excessive temperature gradients, material degradation, and difficulty in optimizing temperature distribution during in-situ bonding, limiting the thickness and mechanical properties of the bond.

Method used

A composite material design incorporating a magnetic field enhancement layer with electrically conductive fibers distributed in multiple directions, combined with electromagnetic induction, allows for localized heating to the melting point of the resin, ensuring uniform temperature distribution and efficient bonding without surface degradation.

Benefits of technology

Achieves high-temperature bonding with improved mechanical properties, enabling in-situ consolidation and bonding of large composite parts, reducing manufacturing costs and maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565922000003
    Figure 0007565922000003
  • Figure 0007565922000004
    Figure 0007565922000004
  • Figure 0007565922000005
    Figure 0007565922000005
Patent Text Reader

Abstract

A composite material, particularly for aeronautical applications, comprising a first pre-impregnated layer (2) having a resin-based matrix (3) reinforced with fibers (4) to impart predetermined mechanical properties to the first layer (2), and a second layer (6, 6') of magnetic field-enhancing material superimposed on a face (5) of the first layer (2) and bonded to the first layer (2) along the face (5), the second layer (6, 6') comprising conductive fibers (7), preferably carbon, having an equivalent electrical resistivity of less than 600 μΩm, preferably less than 200 μΩm, and even more preferably less than 100 μΩm, parallel to the face (5), dispersed in at least two directions with different orientations to facilitate localized heating by electromagnetic induction, the first and second layers (2; 6, 6') being bonded to each other to define a thin layer (L, L') of superweldable composite material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This patent application claims priority to Italian Patent Application No. 102018000020521, filed December 20, 2018, the entire disclosure of which is incorporated herein by reference.

[0002] The invention relates to composite materials in particular for aeronautical applications, to which the following description makes explicit reference, without loss of generality.

[0003] The present invention also relates to a method for producing the above composite material. [Background technology]

[0004] As is known, composite materials are used in various industrial sectors, including the aeronautical industry. In particular, fiber-reinforced composite materials, commonly called "pre-impregnated" or "prepreg", are known, which are generally constituted by a semi-finished product comprising a resin matrix and reinforcing fibers immersed in the matrix. The fibers can be arranged according to different configurations, for example in a single direction, in two or more mutually different directions, or so as to form a fabric. The matrix is ​​used to fix the fibers to each other and possibly to other components during manufacture.

[0005] Prepregs are generally prepared in the form of tapes and wound into rolls, and to achieve the desired mechanical properties the prepregs must undergo a consolidation process with heat and often under pressure.

[0006] Prepregs, which are primarily used in the aeronautical industry, can have a matrix of thermosetting or thermoplastic material.

[0007] In the first case (thermosetting materials), the matrix is ​​constituted by a polymer that, under appropriate temperature conditions and / or in the presence of certain substances, transforms into a rigid, insoluble and infusible material. This transformation occurs after a crosslinking reaction that occurs between the polymer chains with the formation of strong (covalent or ionic) bonds (a process known as curing, in which the polymer chains undergo reactions that generate bonds between different chains at the level of reactive functional groups).

[0008] Thermosetting materials prior to polymerization have adhesive properties. These materials can therefore be used to create layering by placing different layers one on top of the other in the appropriate order or orientation of the layers. The layering is then subjected to temperature and pressure cycles (using ovens, moulding presses etc. in vacuum bags and autoclaves) that polymerise the material, increase the molecular weight, induce the formation of bonds between macromolecules (crosslinking) and thus convert it into a material with structural and mechanical properties suitable for the intended application.

[0009] Some thermosetting polymers are crosslinked solely by heat or by a combination of pressure and heat, while others can be crosslinked by a chemical reaction at room temperature (cold crosslinking).

[0010] Lamination can be accomplished in an automated manner, offering great advantages in terms of cost, productivity, and repetition. For flat or moderately curved laminations, automated tape lamination (ATL) machines are used. Recently, a technology has become popular that allows lamination onto curved or closed (cylindrical) surfaces using prepreg tapes of rather small widths (known as slits); this technique is called fiber placement (FP).

[0011] In the second case (thermoplastic materials), the matrix resin has a high molecular weight so that, on the one hand, it does not have to undergo a polymerization cycle and, on the other hand, it does not have adhesive properties.

[0012] In a first approximation, the thermoplastic matrix prepreg can be considered as the manufactured product in the final state formed by a single lamina. To be able to form a laminate, it is necessary to heat the laminate so as to melt at least the contact surfaces of the constituent lamina or layers of the thermoplastic prepreg, compress it under pressure and then cool it. The temperature to be reached for melting is the glass transition temperature T of the amorphous thermoplastic resin. g and the melting point temperature T of the semicrystalline thermoplastic resin f It is.

[0013] Currently, the techniques of automated tape lamination (ATL) and fiber placement (FP) are only used for composite parts with a thermosetting matrix. These are also conceptually possible techniques for thermoplastic matrix prepregs, but have some additional technical requirements; indeed, in this case, the equipment for producing laminates based on thermoplastic prepregs must also provide heat to reach such a temperature (which, depending on the material, can be excessively high) that melts the resin and thus obtains adhesion between the various layers that make up the laminate; moreover, in the case of semi-crystalline thermoplastics, too fast cooling can cause amorphization of the part, with the result that the performance characteristics are reduced. If these problems were instead solved, the ATL and FP techniques would make it possible to achieve the finished part without further autoclave processes, significantly reducing the cost of manufacturing the part.

[0014] As mentioned above, the process of prepreg consolidation and bonding of the various prepreg layers to form the final part is usually carried out in an autoclave, oven or molding press. For very large parts, such as structural parts for the aeronautical, naval, etc. sectors, known consolidation and bonding processes can be excessively expensive and result in a number of undesirable limitations.

[0015] There is therefore a felt need to develop techniques that make it possible to achieve in situ consolidation and bonding of parts in composite materials, especially when the composite materials are very large.

[0016] One of the most promising techniques for composites with a thermoplastic matrix is ​​consolidation and bonding by electromagnetic induction, which, unlike other techniques such as adhesive bonding, does not use any filler material and only an overlap of two edges of the two parts to be joined (also known as adherends), at least one of which is electrically conductive, that remain in contact with each other.

[0017] According to this technique, an inductor, e.g. a coil, generates a variable electromagnetic field, which induces parasitic currents in the areas of the adherends to be joined, at least one of which is electrically conductive, and, by the Joule effect, these parasitic currents heat the matrix of the adherends, bringing them to a melting or softening point, and then, once the adherends are at a temperature considered ideal, a mechanical pressure, known as the consolidation pressure, can be applied, suitable to induce adhesion of the adherends.

[0018] In conventional inductive coupling systems, the heating effect due to parasitic currents, bearing in mind the dependence on the square of the distance from the inductor, tends to be concentrated on the surfaces directly exposed to the inductor, thus resulting in steep temperature gradients, which cause surface melting of the matrix rather than the adhesive areas of the adherend, which has a detrimental effect on the quality of the bond and the mechanical properties of the bond thus obtained.

[0019] Moreover, the direction of this temperature gradient results in a maximum temperature on the surface facing the inductor and a minimum temperature on the bonding surface in the thickness direction. Thus, to reach the ideal temperature on the adhesive surface of the adherend, the temperature of the outermost regions becomes excessive, which may lead to degradation of the matrix of the composite. As a result, the existence of this gradient quite significantly limits the possible thickness of the adherend.

[0020] Similarly, there are large current concentrations at the edges of the parts being joined, thus creating often unacceptable temperature gradients, which can also lead to material degradation.

[0021] In either case, the temperature reached at the bonding interface is too low (typically 60-70°C) compared to the temperature required to form a bond (approximately 350°C).

[0022] Finally, the main drawback of the electromagnetic induction in situ composite consolidation and bonding technique is the difficulty in optimizing the temperature distribution through the thickness of the bond. WO 90 / 08027 discloses a composite material as defined in the preamble of claim 1. Summary of the Invention [Problem to be solved by the invention]

[0023] One object of the present invention is to produce a composite material making it possible to overcome the above-mentioned drawbacks. [Means for solving the problem]

[0024] According to the present invention there is provided a composite material, in particular for aeronautical applications, as claimed in claim 1 and its dependent claims.

[0025] The invention also relates to a method according to claims 10 and 11 for producing the aforementioned composite material. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a schematic perspective view of two layers of starting material that are joined to form a first embodiment of a lamina of composite material according to the invention; [Diagram 2] FIG. 2 is a highly enlarged schematic cross-sectional view taken along line II-II of FIG. 1. [Diagram 3] FIG. 3 is a schematic cross-sectional view similar to FIG. 2, showing a thin layer of composite material obtained by joining two layers of the starting material of FIGS. 1 and 2. [Figure 4] FIG. 4 is a perspective view of a layout showing a possible embodiment of the joining operation of two thin layers of composite material of the type shown in FIG. 3. [Diagram 5] FIG. 5 is a highly enlarged schematic cross-sectional view taken along line VV of FIG. 4. [Figure 6]6 is a photograph of a portion of two thin layers of the composite material bonded together shown in FIGS. 4 and 5, taken using a microscope. [Figure 7] FIG. 7 shows a highly enlarged detail of FIG. 6. [Figure 8] 8 shows the temperature-time diagram obtained at the bonding interface between two laminae of the composite material of FIGS. 4 to 7 during the bonding operation of FIG. [Figure 9] 1 shows a temperature-time diagram obtained at a bond interface between two thin layers of a composite material of known type. [Figure 10] 1 shows a histogram comparing the elastic modulus of a lamina of a composite material according to the present invention and a lamina of a different type of composite material. [Figure 11] 1 shows a histogram comparing calculated tensile strength for a composite lamina according to the invention and for laminas of different types of composites. [Figure 12] The same histogram as in Fig. 10 is shown, with one of the calculated elastic moduli for the different lamina of the composite set to unity. [Figure 13] The same histogram as in Figure 11 is shown, with one of the calculated tensile strengths for the different lamina of the composite set to unity. [Figure 14] 10 to 13 show histograms comparing the different lamina thicknesses for which the elastic modulus and tensile strength values ​​were calculated. [Figure 15] FIG. 3 is a view similar to FIG. 2, showing, on a greatly enlarged scale, a schematic cross-sectional view of two layers of starting material intended to be joined to form a second embodiment of a lamina of composite material according to the invention; [Figure 16] 16 is a schematic cross-sectional view similar to FIG. 3, showing a thin layer of composite material resulting from the joining of two layers of the starting material of FIG. 15; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The present invention will now be described in conjunction with the following.

[0028] 1 to 3 show diagrammatically a first embodiment of a lamina L of composite material manufactured according to the invention and designed in particular to be used in aeronautical applications.

[0029] The composite lamina L comprises a first pre-impregnated layer 2 having a resin-based matrix 3 reinforced with fibres 4 or fibrous material to give the layer 2 certain mechanical properties.

[0030] It should be noted that the term "system" or "base" means that the matrix 3 may contain, in addition to the resin, also commonly used additives such as, for example, fillers, stabilizers, etc.

[0031] The matrix 3 is preferably composed mainly of a semi-crystalline thermoplastic resin having a predetermined melting point Tf. f The semi-crystalline thermoplastic resin is, for example, polyetheretherketone, or PEEK, having a melting point temperature T of about 370° C. f The polymer may be a polyetherketoneketone, i.e., PEKK, having the formula:

[0032] The matrix 3 has a predetermined glass transition temperature T g The thermoplastic resin may also be based on an amorphous thermoplastic resin having a glass transition temperature of about 215° C., for example polyetherimide, or PEI.

[0033] According to a possible alternative, not shown and not part of the invention: The matrix of layer 2 can also be based on a thermosetting resin, for example an epoxy, a BMI (bismaleimide) or a phenolic resin.

[0034] The fibers 4 are preferably carbon fibers and are one or more unidirectional. In layers can be placed.

[0035] The carbon fiber 4 is preferably 100 to 300 g / m 2 The weight is between 1 and 2.

[0036] layer The fibres 4 of 2 are unidirectional, in particular the unidirectional fibres 4 are used to reinforce the stressed parts of the lamina L in one direction and to position them along the load path.

[0037] Alternatively, other types of fibres known in the aeronautical field can be used for layer 2, such as for example fibreglass or a combination of fibreglass and carbon fibres.

[0038] The fibres 4 are preferably continuous and may have a length comprised between 1 mm and 40 cm.

[0039] As can be seen in Figures 1 and 2, layer 2 is defined by respective opposing parallel surfaces 5, and a thickness S1 of layer 2 in a direction perpendicular to surfaces 5 is small relative to the size (length and width) of surfaces 5.

[0040] The thin layer L of composite material further comprises a second layer 6 of magnetic field enhancing material superimposed and bonded to one of the faces 5 of layer 2, and conductive fibers 7 having an equivalent electrical resistivity and less than 600 μΩm, preferably less than 200 μΩm, even more preferably less than 100 μΩm, are dispersed in layer 6 in at least two directions parallel to face 5 with different orientations to facilitate localized heating by electromagnetic induction.

[0041] Regarding the significance and calculation of the equivalent electrical resistivity (the inverse of the equivalent electrical conductivity) of a composite material, reference may be made, for example, to the following publications:

[0042] "Calculation of an equivalent electrical conductivity tensor for multidirectional carbon fiber reinforced materials", August 19, 2012, by N. Athanasopoulos and V. Kostopoulos.

[0043] In the illustrated example, layer 6 comprises a matrix 8 based on a semi-crystalline thermoplastic resin, which is identical to or compatible with the resin of matrix 3 of layer 2, in which fibers 7 are dispersed. More specifically, fibers 7 are carbon and are arranged in matrix 8 randomly in multiple directions, some of which run parallel to faces 5 and others transverse to faces 5.

[0044] The fibers 7 extending transversely to the face 5 have an equivalent electrical resistivity greater than 2,000 μΩm.

[0045] Carbon fiber 7 is 10 to 100 g / m 2 The weight is between 1 and 2.

[0046] The carbon fibers 7 are preferably obtained by oxidation and pyrolysis of polyacrylonitrile (PAN).

[0047] Alternatively, the carbon fibres 7 can be obtained by distillation of a carbon-based material, such as, for example, a viscoelastic material composed of plants, raw oil and carbon (PITCH), in this case aromatic hydrocarbons.

[0048] The fibers 7 can also be made of another electrically conductive material, for example a metallic material.

[0049] The fibres 7 are preferably continuous and may have a length comprised between 1 mm and 40 cm.

[0050] Advantageously, layer 6 is in the form of a veil or film and has, in the direction perpendicular to face 5, a thickness S2 comprised between 1 / 10 and 1 / 100 of the thickness S1 of layer 2.

[0051] The layers 2 and 6 are joined by compression molding, preferably by continuous compression molding. This joining can be done in a known manner in a hot press (known and not shown) or by passing the layers 2 and 6 to be joined between respective pairs of hot rollers (known and not shown) in a continuous lamination-like process. The temperature at which the joining process of layers 2 and 6 takes place depends on the type of thermoplastic matrix used and, in the case of a semi-crystalline thermoplastic matrix, is the melting point T f higher, but for an amorphous thermoplastic matrix, the glass transition temperature T g Higher.

[0052] FIG. 4 shows diagrammatically the practical means for carrying out the joining operation of two lamina L of composite material.

[0053] During this operation, an inductor 11 (known and shown only diagrammatically), e.g. an electric coil, is supplied with current to generate a variable electromagnetic field E (whose magnetic flux lines are shown diagrammatically in FIG. 4 by dashed lines).

[0054] At the same time, the new lamina L is gradually laid down on another already existing lamina L disposed on the support surface 12, or alternatively on an upper lamina L of a series of already joined or bonded lamina L disposed on the support surface 12.

[0055] The step of laying down the new lamina L is carried out by one or more rollers 13 (only one of which is shown in Figure 4) having an axis A parallel to the lamina L on which they act, rotating about the axis A and advancing parallel to the support surface 12.

[0056] The electromagnetic field E induces substantially parasitic currents in layer 6 of the new lamina L, which then bond to another lamina (e) L lying on the support surface 12 .

[0057] Since the fibers 7 of layer 6 are electrically conductive and are distributed in at least two different directions within the matrix 8, an actual "electrical circuit" is created, at least the inner layer 6 of the new lamina L, heating the matrix 8 of layer 6 and the adjacent lamina L by the Joule effect.

[0058] The localized heating is very efficient and locally, i.e. in the layer 6 and in the region of the matrix 3 adjacent to this layer, the melting point temperature T f or glass transition temperature T g This allows temperatures above 100° C.

[0059] Instead, in the regions of the matrix 3 furthest from the layer 6, the temperature is lower than the melting point temperature T f remains significantly lower than

[0060] The passage of the roller(s) 13 takes place after which parasitic currents are induced in the new lamina L which is bonded to other lamina (e) L disposed on the surface of the support surface 12 .

[0061] In this way, pressure is gradually applied to the areas of the thin layer L to be joined after electromagnetic induction and after the softening obtained at the interface between these areas during cooling thereof.

[0062] Preferably, the roller 13(s) is kept at a low temperature to gradually remove residual heat from the thin layer L during the bonding step.

[0063] At the end of the combining operation, the result is as diagrammed in FIG.

[0064] 6 and 7 show microscopic images of the bonded area of ​​thin layer L, each of which shows -200g / m 2 A layer 2 of PEKK having unidirectional carbon fiber 4 having a basis weight of -Matrix 8 in PEKK with 8g / m randomly distributed in all directions 2 and a VEIL layer 6 having carbon fiber 7 having a basis weight of 1000 g.

[0065] As can be seen, the fibers 7 have a substantially isotropic distribution in the matrix 8 of the layer 6, with some of the fibers 7 being oriented transversely to the face 5 of the layer 2. This makes it possible to achieve a high resistance / toughness of the bond material.

[0066] Figures 8 and 9 show two temperature / time diagrams comparing the behavior of the following during the coupling operation by electromagnetic induction: two thin layers L of a composite material according to the invention, - two thin layers of a composite material of a known type. In particular, the diagram of FIG. 8 refers to two lamina L, each of which is -200g / m 2 A layer 2 of PEKK having unidirectional carbon fiber having a basis weight of -Matrix 8 in PEKK with 8g / m randomly distributed in all directions 2 and a VEIL layer 6 having carbon fiber 7 having a basis weight of 1000 g.

[0067] The diagram in FIG. 9 shows instead the matrix in PEKK and 200 g / m 2 Reference is made to two thin layers of a composite material of a known type having unidirectional carbon fibres with a basis weight of

[0068] As can be observed, in the first case (FIG. 8), a temperature close to 400° C. is reached for a few tens of seconds (25-30 s).

[0069] In the second case (Figure 9), the maximum temperature reached is less than 60°C.

[0070] The Applicant has observed that by adopting a thickness of layer 6 comprised between 1 / 10 and 1 / 100 of the thickness of layer 2, it is possible, on the one hand, to achieve substantial preservation in thin layer L of the mechanical properties determined by layer 2 and, on the other hand, to achieve very easy in situ consolidation and bonding of the material by electromagnetic induction.

[0071] 10 to 14 show experimental results obtained by the Applicant with regard to mechanical properties and thickness, comparing the following types of thin layers: -Unidirectional PEKK / Carbon Laminate (APC(PEKK-FC)_AS 4(Wm%=34%, basis weight or grams / square meter=145g / m 2 ), hereinafter referred to as UD, which does not form part of the invention and corresponds to an example of a thin layer made up of only layer 2, - Front UD lamina (layer 2) 4g / m 2 A thin layer according to the present invention obtained by combining with a veil layer 6 (hereinafter referred to as UD / veil_4) having a basis weight of - Front UD lamina (layer 2) 8g / m 2 A thin layer according to the present invention obtained by combining with a veil layer 6 (hereinafter referred to as UD / veil_8) having a basis weight of - a thin layer not forming part of the present invention, the previous UD thin layer (layer 2) is 34 g / m 2 A thin layer obtained by combining with a veil layer 6 (hereinafter referred to as UD / veil_34) having a basis weight of - a lamina not forming part of the invention, the previous UD lamina (layer 2) being 145 g / m 2 It is a thin layer obtained by combining with a mat layer 6 having a basis weight of 145 mm (hereinafter referred to as UD / mat_145).

[0072] The veils and mats described above have a semi-crystalline thermoplastic resin-based matrix identical to the resin in the matrix of the UD lamina.

[0073] The add-on level of the veil and mat is 34% by weight.

[0074] The fibers used in the veils and mats shown above are carbon and are randomly arranged in their respective matrices in all directions.

[0075] The mechanical properties of the above different types of lamina have been determined in terms of elastic modulus E and tensile strength σ, both quantities being calculated in the direction parallel to the unidirectional fibres in layer 2 or the UD lamina.

[0076] The thicknesses of the different lamina considered, calculated in the direction perpendicular to the lamina, are listed in the table below.

[0077] [Table 1]

[0078] Instead, the following table lists the values ​​of elastic modulus E and tensile strength σ calculated for the lamina defined above.

[0079] [Table 2]

[0080] The results of this table are summarized in the histograms in Figures 10 and 11, and in normalized form in Figures 12 and 13.

[0081] In particular, as can be observed both from the previous table and from Figures 10 and 11, the degradation of the mechanical properties starts to become noticeable already at a thickness of layer 6 equal to 23% of the thickness of layer 2, becoming very pronounced when the two layers 2, 6 have the same thickness.

[0082] The histograms in Figures 12 and 13 refer to the same results shown in Figures 10 and 11, but the elastic modulus E and tensile strength σ of the UD lamina are used as the denominators of the ratios to the values ​​of the corresponding quantities calculated for the other types of lamina.

[0083] FIG. 14 shows the ratio of the thickness of the different types of lamina to the thickness of the reference UD lamina.

[0084] Figures 15 and 16 show a lamina of composite material, generally designated L', manufactured according to different embodiments of the invention, which will be described hereinafter only with respect to how lamina L' differs from lamina L, where possible indicating with the same reference numbers parts which are identical, corresponding or equivalent to parts already described.

[0085] In particular, the composite lamina L' differs from the lamina L essentially in that it comprises a magnetic field-enhancing layer 6' without a resin matrix.

[0086] More specifically, layer 6' may be a carbon veil extending in at least two directions in which the fibers 7 have different orientations, preferably in at least three directions that are transverse to the face 5 of layer 2, where the fibers 7 are held together to form the veil by an adhesive or binder, such as PVA (polyvinyl alcohol) or other substance that is chemically compatible with the matrix 3 of layer 2.

[0087] Alternatively, layer 6' may be a fabric in which the fibres 7 extend in at least two directions with different orientations.

[0088] According to a further alternative, the layer 6' may be a nonwoven fabric, for example of the Optiveil® type.

[0089] From a consideration of the properties of composite materials produced in accordance with the principles of the present invention, the advantages which may be achieved thereby are apparent.

[0090] In particular, as mentioned above, the fibers 7 of the layers 6, 6' are electrically conductive and are arranged in at least two directions with different orientations, so that it is possible to generate real "electrical circuits" by electromagnetic induction at least inside the layers 6, 6', the formation of these circuits making it possible to achieve an effective heating by Joule effect of the layers 6, 6' and the adjacent resin matrix 3, so that the melting point temperature T of the resin is precisely at the bonding interface of the two different thin layers L, L'. f reaches.

[0091] In reality, the melting point temperature T f 11 , without creating higher temperatures in the regions of the resin closest to inductor 11 , where the composite matrix may degrade.

[0092] As shown in the diagrams in Figures 8 and 9, the temperature reached at the bonding interface between two thin layers L, L' according to the invention during the operation of in situ consolidation and bonding by electromagnetic induction is at least 7 times higher than the temperatures reached in the case of known types of composite materials.

[0093] Precisely for the reasons stated above, the Applicant has also measured a bonding rate between two thin layers L, L' according to the invention which is ten times higher than the bonding rate of conventional prepregs.

[0094] Since the thickness S2 of the layers 6, 6' is comprised between 1 / 10 and 1 / 100 of the thickness S1 of the layer 2, easy in situ consolidation and bonding of the material according to the invention is indeed achieved without impairing the mechanical properties imparted to the thin layers L, L' by the orientation and arrangement of the carbon fibers of the layer 2. Finally, it is evident that modifications and variations can be made in the composite material described herein, as well as in the method for producing said composite material, without departing from the scope defined in the claims.

Claims

1. 1. A composite material comprising: a first layer (2) which is a pre-impregnated layer, the first layer (2) having a thermoplastic resin matrix (3) reinforced with unidirectional fibers (4); a second layer (6,6') of magnetic field enhancing material overlaid on a face (5) of said first layer (2) and bonded to said first layer (2) along said face (5); said second layer (6, 6') comprising electrically conductive fibres (7) of carbon dispersed therein so as to extend in at least two directions with different orientations in order to facilitate localised heating by electromagnetic induction, said first and second layers (2; 6, 6') being joined together to define a thin layer (L, L') of composite material to be heated, In a direction perpendicular to the face (5), the second layer (6, 6') has a thickness (S2) comprised between 1 / 10 and 1 / 100 of the thickness (S1) of the first layer (2). A composite material comprising:

2. the conductive fibers (7) of the second layer (6, 6') have an equivalent electrical resistivity parallel to the face (5) of less than 600 μΩm; 2. The composite material of claim 1.

3. The conductive fibers (7) have an equivalent electrical resistivity of less than 200 μΩm.

3. The composite material of claim 2.

4. The conductive fibers (7) have an equivalent electrical resistivity of less than 100 μΩm.

4. The composite material of claim 3.

5. one of the directions in which the conductive fibers (7) are distributed in the second layer (6, 6') is transverse to the face (5); A composite material according to any one of claims 1 to 4.

6. the conductive fibers (7) are distributed in the second layer (6, 6') so as to extend in at least three directions with mutually different orientations, at least one of the at least three directions being transverse to the face (5); A composite material according to any one of claims 1 to 5.

7. The conductive fibers (7) of the second layer (6, 6') - held together by a resin-based matrix (8) identical to the resin of the matrix (5) of the first layer (2), or - held together to form a film by an adhesive or binder; A composite material according to any one of claims 1 to 6.

8. The conductive fibers (7) of the second layer (6, 6') form a fabric, 8. The composite material of claim 7.

9. The fabric is a nonwoven fabric.

9. The composite material of claim 8.

10. one said first layer and one said second layer (2; 6, 6') are joined together to form one said layer (L, L') of weldable composite material by hot compression molding by passing said first and second layers (2; 6, 6') between at least one pair of hot rollers, A method for producing a composite material according to any one of claims 1 to 9.

11. The hot compression molding is continuous compression molding. A method for producing the composite material according to claim 10.

12. - gradually spreading a first one of said thin layers (L, L') onto a second one of said thin layers (L, L') lying on a support (12); - inducing a parasitic current in at least the second layer (6, 6') of the first thin layer (L, L') by means of an inductor (11) so as to result in localized heating of a region of the first and second thin layers (L, L') adjacent to the second layer (6, 6') of the first thin layer (L, L'); applying a pressure to the first thin layer (L, L') after the induction step, so as to bond the first thin layer to the second thin layer (L, L') during cooling of the thin layer (L, L'); bonding at least two of said lamina (L, L') of composite material to each other by 12. The method according to claim 10 or 11.

Citation Information

Patent Citations

  • Method for joining composite material

    JP1992504386A

  • Metal mold and method for manufacturing thermoplastic resin-based fiber-reinforced composite material molding

    JP2013154625A

  • Connection device and connection method of component

    JP2014019076A

  • Intermediate substrate for press molding, preform, and method for manufacturing a molding

    JP2014028510A

  • Induction bondable high-pressure laminate

    US20040091694A1