Transmission belt composition

A composition for power transmission belts using an ethylene/α-olefin/non-conjugated polyene copolymer with carbon black and short fibers addresses the heat and abrasion resistance issues of chloroprene rubber, enhancing belt durability and performance.

JP7566460B2Active Publication Date: 2024-10-15MITSUI CHEMICALS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019165716
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-09-11
Publication Date
2024-10-15
Estimated Expiration
2039-09-11

AI Technical Summary

Technical Problem

Existing power transmission belts made with chloroprene rubber lack sufficient heat resistance and abrasion resistance, failing to meet the demands for improved performance in automobiles, motorcycles, and industrial machinery.

Method used

A composition for power transmission belts comprising an ethylene/α-olefin/non-conjugated polyene copolymer, carbon black, short fibers, and a peroxide crosslinking agent, with specific molecular and viscoelastic properties to enhance heat resistance and abrasion resistance.

Benefits of technology

The composition results in power transmission belts with excellent heat resistance and abrasion resistance, improving durability and performance in demanding applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566460000017
    Figure 0007566460000017
  • Figure 0007566460000001
    Figure 0007566460000001
  • Figure 0007566460000002
    Figure 0007566460000002
Patent Text Reader

Abstract

To provide a composition for a transmission belt, capable of forming a transmission belt excellent in heat resistance and wear resistance.SOLUTION: The composition for a transmission belt contains: an ethylene / α-olefin / nonconjugated polyene copolymer (A) which has a structural unit derived from ethylene (a1), a structural unit derived from α-olefin (a2) having the carbon number from 3 to 20, and a structural unit derived from a nonconjugated polyene (a3) containing two or more specific partial structures in total in the molecule, and which satisfies specific requirements; carbon black (B); short fibers (C); a peroxide-based crosslinking agent (D); and a crosslinking aid (E) having two or more ethylenic double bonds.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for a power transmission belt. [Background technology]

[0002] Power transmission belts are widely used in automobiles, motorcycles, and general industrial machines. Power transmission belts are required to have high rubber elasticity and abrasion resistance. In order to manufacture power transmission belts that satisfy the above properties, chloroprene rubber is usually used, and in order to improve heat resistance and reduce weight, the use of ethylene-propylene-non-conjugated polyene copolymer rubber instead of chloroprene rubber has been considered (for example, see Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2001-310951 A [Patent Document 2] JP 2012-215212 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the studies of the present inventors, it has been found that when chloroprene rubber is used, the heat resistance and abrasion resistance of the obtained transmission belt are insufficient. An object of one aspect of the present invention is to provide a composition for a transmission belt capable of forming a transmission belt having excellent heat resistance and abrasion resistance. [Means for solving the problem]

[0005] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by a composition for a transmission belt having the following configuration, thereby completing the present invention. That is, the present invention relates to, for example, the following items [1] to [7].

[0006] [1] An ethylene-α-olefin-non-conjugated polyene copolymer (A) having a structural unit derived from ethylene (a1), a structural unit derived from an α-olefin (a2) having 3 to 20 carbon atoms, and a structural unit derived from a non-conjugated polyene (a3) ​​containing in the molecule a total of two or more partial structures selected from the group consisting of the following formulae (I) and (II), and satisfying the following requirements (i) to (vi): Carbon black (B); Short fibers (C); A peroxide-based crosslinking agent (D); A crosslinking coagent (E) having two or more ethylenic double bonds; A composition for a transmission belt comprising:

[0007] (i) the molar ratio of structural units derived from ethylene (a1) to structural units derived from an α-olefin (a2) having 3 to 20 carbon atoms [(a1) / (a2)] is 40 / 60 to 99.9 / 0.1; (ii) the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​is 0.07 mass% to 10 mass% in 100 mass% of the copolymer (A); (iii) the weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​(mass fraction (mass %) of (a3)), and the molecular weight of the non-conjugated polyene (a3) ​​(the molecular weight of (a3)) satisfy the following formula (1); 4.5≦Mw×(a3) mass fraction / 100 / (a3) molecular weight≦40 … (1)

[0008] (iv) Complex viscosity η at frequency ω = 0.1 rad / s obtained by linear viscoelastic measurement (190 °C) using a rheometer * ( ω =0.1) (Pa sec) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (Pa sec) * ( ω =0.1) / η * ( ω =100)), the intrinsic viscosity [η], and the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​(the mass fraction (mass%) of (a3)) satisfy the following formula (2); P / ([η] 2.9 ) ≦ (a3) ​​mass fraction × 6 … (2)

[0009] (v) the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (molecular weight distribution; Mw / Mn) measured by gel permeation chromatography (GPC) is in the range of 4 to 30; (vi) the number average molecular weight (Mn) is 30,000 or less;

[0010] [ka]

[0011] [2] The composition for a transmission belt according to [1], wherein the non-conjugated polyene (a3) ​​contains 5-vinyl-2-norbornene (VNB). [3] The composition for a transmission belt according to the above [1] or [2], wherein the α-olefin (a2) having 3 to 20 carbon atoms is propylene.

[0012] [4] The composition for a transmission belt according to any one of the above [1] to [3], wherein the short fibers (C) are aramid short fibers. [5] The composition for a transmission belt according to any one of [1] to [4], wherein the content of the carbon black (B) is 0.1 to 200 parts by mass and the content of the short fibers (C) is 0.1 to 100 parts by mass, relative to 100 parts by mass of the copolymer (A).

[0013] [6] A crosslinked molded article formed from the composition for a transmission belt according to any one of [1] to [5] above. [7] A power transmission belt having the cross-linked molded article according to [6] above. Effect of the Invention

[0014] According to the present invention, it is possible to provide a composition for a transmission belt capable of forming a transmission belt having excellent heat resistance and abrasion resistance. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic diagram of a continuous polymerization apparatus used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will now be described in detail. [Composition for transmission belts] One embodiment of the composition for a transmission belt of the present invention (hereinafter also referred to as "the composition of the present embodiment") contains an ethylene-α-olefin-non-conjugated polyene copolymer (A), carbon black (B), short fibers (C), a peroxide-based crosslinking agent (D), and a crosslinking aid having two or more ethylenic double bonds (E), which will be described below.

[0017] <Ethylene-α-olefin-non-conjugated polyene copolymer (A)> The ethylene-α-olefin-non-conjugated polyene copolymer (A) (hereinafter also referred to as "copolymer (A)") has structural units derived from ethylene (a1), an α-olefin (a2) having 3 to 20 carbon atoms, and a non-conjugated polyene (a3) ​​containing, in the molecule, two or more partial structures selected from the group consisting of the formulas (I) and (II) described below in total.

[0018] Examples of the α-olefin (a2) include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms, such as propylene, 1-butene, 1-hexene, and 1-octene, are preferred, and propylene is particularly preferred. Such α-olefins are preferred because the raw material cost is relatively low, the resulting copolymer (A) exhibits excellent mechanical properties, and a molded article having rubber elasticity can be obtained.

[0019] The α-olefin (a2) may be one or more of them. That is, the copolymer (A) contains structural units derived from at least one α-olefin (a2) having 3 to 20 carbon atoms, and may contain structural units derived from two or more α-olefins (a2) having 3 to 20 carbon atoms.

[0020] The non-conjugated polyene (a3) ​​is a compound having two or more non-conjugated unsaturated bonds, and is a compound containing, in the molecule, a total of two or more partial structures selected from the group consisting of the following formulas (I) and (II).

[0021] [ka]

[0022] Examples of the non-conjugated polyene (a3) ​​include 5-vinyl-2-norbornene (VNB), norbornadiene, 1,4-hexadiene, and dicyclopentadiene. Among these, it is preferable that the non-conjugated polyene (a3) ​​contains VNB, and it is more preferable that the non-conjugated polyene (a3) ​​is VNB, since VNB is highly available, has good reactivity with peroxide during crosslinking reaction after polymerization, and tends to improve the heat resistance of the composition.

[0023] The non-conjugated polyene (a3) ​​can be used alone or in combination. The copolymer (A) may have, in addition to the structural units derived from the above (a1), (a2) and (a3), a structural unit derived from a non-conjugated polyene (a4) containing only one partial structure selected from the group consisting of the above formulae (I) and (II) in the molecule.

[0024] Examples of the non-conjugated polyene (a4) include 5-ethylidene-2-norbornene (ENB), 5-methylene-2-norbornene, 5-(2-propenyl)-2-norbornene, 5-(3-butenyl)-2-norbornene, 5-(1-methyl-2-propenyl)-2-norbornene, 5-(4-pentenyl)-2-norbornene, 5-(1-methyl-3-butenyl)-2-norbornene, 5-(5-hexenyl)-2-norbornene, 5-(1-methyl-4-pentenyl)-2-norbornene, 5-(2,3-dimethyl-3-butenyl)-2-norbornene, 5-(2-ethyl-3-butenyl)-2-norbornene, 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(1,2-trimethyl-4-pentenyl)-2-norbornene, 5-(6-heptenyl)-2-norbornene, 5-(3-methyl-5-hexenyl)-2-norbornene, 5-(3,4-dimethyl-4-pentenyl)-2-norbornene, 5-(3-ethyl-4-pentenyl)-2-norbornene, 5-(7-octenyl)-2-norbornene, 5-(2-methyl-6-heptenyl)-2-norbornene, 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(5-ethyl-5-hexenyl)-2-norbornene, 5-(1,2,3-trimethyl-4-pentenyl)-2-norbornene. Among these, ENB is preferred because it is highly available, has high reactivity with the crosslinking agent during the crosslinking reaction after polymerization, is easy to control the crosslinking rate, and is easy to obtain good mechanical properties.

[0025] The non-conjugated polyene (a4) can be used alone or in combination. When the copolymer (A) contains a structural unit derived from a non-conjugated polyene (a4), its proportion is not particularly limited within the scope of the present invention, but is usually 0 to 20 mass%, preferably 0 to 8 mass%, more preferably 0.01 to 8 mass%, provided that the sum of the mass fractions of the above (a1), (a2), (a3), and (a4) is 100 mass%.

[0026] The composition of the present embodiment may contain one type of copolymer (A) or may contain two or more types of copolymers (A). The content of the copolymer (A) in the composition of the present embodiment is usually 20% by mass or more, and preferably 25 to 90% by mass.

[0027] The copolymer (A) satisfies the following requirements (i) to (vi) (hereinafter also referred to as requirements (i) to (vi) respectively). (i) The molar ratio of structural units derived from ethylene (a1) to structural units derived from an α-olefin (a2) having 3 to 20 carbon atoms [(a1) / (a2)] is 40 / 60 to 99.9 / 0.1. (ii) The mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​is 0.07 mass % to 10 mass % in 100 mass % of the copolymer (A).

[0028] (iii) The weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​(mass fraction (mass %) of (a3)), and the molecular weight of the non-conjugated polyene (a3) ​​(molecular weight of (a3)) satisfy the following formula (1): 4.5≦Mw×(a3) mass fraction / 100 / (a3) molecular weight≦40 … (1)

[0029] (iv) Complex viscosity η at frequency ω = 0.1 rad / s obtained by linear viscoelastic measurement (190 °C) using a rheometer * ( ω =0.1) (Pa sec) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (Pa sec) * ( ω =0.1) / η * ( ω =100) ), the intrinsic viscosity [η], and the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​(mass fraction (mass %) of (a3)) satisfy the following formula (2). P / ([η] 2.9 ) ≦ (a3) ​​mass fraction × 6 … (2)

[0030] (v) The ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (molecular weight distribution; Mw / Mn) measured by gel permeation chromatography (GPC) is in the range of 4 to 30. (vi) The number average molecular weight (Mn) is 30,000 or less.

[0031] ≪Requirement (i)≫ The requirement (i) specifies that the molar ratio of ethylene (a1) / α-olefin (a2) in the copolymer (A) satisfies 40 / 60 to 99.9 / 0.1, and this molar ratio is preferably 50 / 50 to 90 / 10, more preferably 55 / 45 to 85 / 15, and even more preferably 55 / 45 to 78 / 22.

[0032] By using the copolymer (A) that satisfies the requirement (i), it is possible to obtain a transmission belt that is excellent in heat resistance, cold resistance, and abrasion resistance. The amount of ethylene (a1) (the content of structural units derived from ethylene (a1)) and the amount of α-olefin (a2) (the content of structural units derived from α-olefin (a2)) in the copolymer (A) are 13 It can be determined by C-NMR.

[0033] Requirement (ii) Requirement (ii) specifies that the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​is in the range of 0.07% by mass to 10% by mass in 100% by mass of the copolymer (A) (i.e., in the total mass fraction of all the structural units, 100% by mass). The mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​is preferably 0.1% by mass to 8.0% by mass, more preferably 0.5% by mass to 5.0% by mass.

[0034] The copolymer (A) satisfying the requirement (ii) has sufficient hardness and excellent mechanical properties, and when crosslinked using a peroxide, it exhibits a fast crosslinking rate. The amount of non-conjugated polyene (a3) ​​in the copolymer (A) (the content of structural units derived from non-conjugated polyene (a3)) is: 13 It can be determined by C-NMR.

[0035] ≪Requirement (iii)≫ Requirement (iii) specifies that in the copolymer (A), the weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​in the copolymer (A) (mass fraction (mass%) of (a3)), and the molecular weight of the non-conjugated polyene (a3) ​​(molecular weight of (a3)) satisfy the above formula (1). The above formula (1) in requirement (iii) is preferably the following formula (1'): 4.5≦Mw×(a3) mass fraction / 100 / (a3) molecular weight≦35 …(1')

[0036] When the copolymer (A) satisfies the requirement (iii), the content of the structural unit derived from the non-conjugated polyene (a3) ​​is appropriate, and a transmission belt can be produced that exhibits sufficient crosslinking performance, an excellent crosslinking rate, and excellent mechanical properties. The weight average molecular weight (Mw) of the copolymer (A) can be determined as a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0037] In the copolymer (A), when "Mw × mass fraction of (a3) / 100 / molecular weight of (a3)" satisfies the above formula (1) or (1'), the degree of crosslinking is appropriate, and a transmission belt having a good balance between mechanical properties and heat aging resistance can be produced. If the value of "Mw × mass fraction of (a3) / 100 / molecular weight of (a3)" is too low, the crosslinking may be insufficient, resulting in a slow crosslinking rate, whereas if the value is too high, excessive crosslinking may occur, resulting in deterioration of mechanical properties.

[0038] ≪Requirement (iv)≫ Requirement (iv) is the complex viscosity η of the copolymer (A) at a frequency ω = 0.1 rad / s obtained by linear viscoelasticity measurement (190 °C) using a rheometer. * ( ω =0.1) (Pa sec) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (Pa sec) * ( ω =0.1) / η * ( ω =100) ), the intrinsic viscosity [η], and the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​(mass fraction (mass%) of (a3)) satisfy the above formula (2). The above formula (2) in requirement (iv) is preferably the following formula (2'). P / ([η] 2.9 ) ≦ (a3) ​​mass fraction × 5.7 … (2')

[0039] Here, the complex viscosity η at frequency ω=0.1rad / s * ( ω =0.1) and the complex viscosity η at frequency ω=100rad / s * ( ω =100) Relative to P(η * ( ω =0.1) / η * ( ω =100) ) represents the frequency dependence of viscosity and is the left side of equation (2), P / ([η] 2.9 ) tends to show a high value when there are many long chain branches, although it is influenced by short chain branches, molecular weight, etc. In general, in an ethylene-α-olefin-non-conjugated polyene copolymer, the more structural units derived from non-conjugated polyenes it contains, the more long chain branches it tends to contain. However, since copolymer (A) has fewer long chain branches than conventionally known ethylene-α-olefin-non-conjugated polyene copolymers, it is considered that it can satisfy the above formula (2).

[0040] In the present invention, the P value is determined by performing measurements using a viscoelasticity measuring device Ares (manufactured by Rheometric Scientific) at 190° C., strain 1.0%, and various frequencies, and is calculated as the ratio (η * The intrinsic viscosity [η] is the value measured in decalin at 135°C.

[0041] ≪Requirement (v)≫ Requirement (v) specifies that the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (molecular weight distribution; Mw / Mn) of the copolymer (A) measured by gel permeation chromatography (GPC) is in the range of 4 to 30. This molecular weight distribution (Mw / Mn) is preferably in the range of 4 to 28, more preferably in the range of 4 to 26. In one embodiment, this molecular weight distribution (Mw / Mn) is in the range of 8 to 30, preferably in the range of 8 to 28, more preferably in the range of 8 to 26.

[0042] When the copolymer (A) satisfies the requirement (v), it contains an appropriate amount of low molecular weight components, and therefore the processability is good. The weight average molecular weight (Mw) and number average molecular weight (Mn) of the copolymer (A) can be determined as polystyrene-equivalent values ​​measured by gel permeation chromatography (GPC).

[0043] ≪Requirement (vi)≫ The requirement (vi) specifies that the number average molecular weight (Mn) of the copolymer (A) is not more than 30,000. The number average molecular weight (Mn) is preferably in the range of 3,000 to 26,000, more preferably 6,000 to 23,000.

[0044] When the copolymer (A) satisfies the requirement (vi), it contains an appropriate amount of low molecular weight components, and therefore the processability is good.

[0045] ≪Requirement (vii)≫ The chart obtained by GPC measurement of the copolymer (A) shows two or more peaks, and the area of ​​the peak appearing on the side of the smallest molecular weight is preferably 1 to 20% of the total peak area. The area of ​​the peak appearing on the side of the smallest molecular weight is more preferably 2 to 18%, and further preferably 3 to 16% of the total peak area.

[0046] When the copolymer (A) satisfies the requirement (vii), the molecular weight distribution of the copolymer (A) will be multimodal, such as bimodal, and will contain high molecular weight components and low molecular weight components in an appropriate ratio, resulting in good processability.

[0047] ≪Requirement (viii)≫ Copolymer (A) was determined by the number of long chain branches (LCB) per 1000 carbon atoms obtained using 3D-GPC. 1000C ) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)] preferably satisfy the following formula (3), and more preferably satisfy the following formula (3').

[0048] LCB 1000C ≦1-0.07×Ln(Mw) …(3) LCB 1000C ≦1-0.071×Ln(Mw) …(3') The upper limit of the long chain branch content per unit carbon number of the copolymer (A) is specified by the above formula (3) or (3').

[0049] Such a copolymer (A) contains a small proportion of long chain branches, and has excellent curing properties when crosslinked using a peroxide, and can provide a power transmission belt having excellent heat aging resistance.

[0050] Here, Mw and the number of long chain branches (LCB) per 1000 carbon atoms 1000C ) can be determined by a structural analysis method using 3D-GPC. In this specification, it was specifically determined as follows.

[0051] The absolute molecular weight distribution was measured using a 3D-high temperature GPC device PL-GPC220 (Polymer Laboratories), and the intrinsic viscosity was measured using a viscometer. The main measurement conditions were as follows: Detector: Differential refractometer / GPC device built-in 2-angle light scattering photometer PD2040 type (manufactured by Precison Detectors) Bridge type viscometer PL-BV400 (Polymer Laboratories) Column: TSKgel GMH HR -H(S)HT x 2 + TSKgel GMH HR -M(S)×1 piece (Each piece has an inner diameter of 7.8 mm and a length of 300 mm) Temperature: 140℃ Mobile phase: 1,2,4-trichlorobenzene (containing 0.025% BHT) Injection volume: 0.5mL Sample concentration: ca 1.5mg / mL Sample filtration: Filtration through a sintered filter with a pore size of 1.0 μm

[0052] In the above, the dn / dc value required to determine the absolute molecular weight was determined for each sample from the dn / dc value of standard polystyrene (molecular weight 190,000) of 0.053 and the response intensity of the differential refractometer per unit injected mass.

[0053] From the relationship between the intrinsic viscosity obtained from the viscometer and the absolute molecular weight obtained from the light scattering photometer, the long chain branching parameter g'i for each eluted component was calculated from the following formula (v-1).

[0054]

number

[0055] Here, [η] = KM v The relational equation v = 0.725 (K: constant determined by the type of polymer, etc., M: molecular weight) was applied. Further, the average values ​​of g' were calculated from the following formulas (v-2), (v-3), and (v-4). Note that a trendline assuming the presence of only short chain branches was determined for each sample.

[0056]

number

[0057] Furthermore, using g'w, the number of branching points per molecular chain, BrNo, and the number of long chain branches per 1000 carbon atoms, LCB, 1000CThe branching degree λ per unit molecular weight was calculated. BrNo was calculated using the following Zimm-Stockmayer formula (v-5). 1000C The following formulas (v-6) and (v-7) were used to calculate and λ. g is the long chain branching parameter calculated from the radius of gyration Rg, and the following simple correlation is made between g' calculated from the intrinsic viscosity.

[0058] g=g' (1 / ε) ε (structure factor) = 0.5 to 1.5 (usually 0.75) Various values ​​have been proposed for ε in the formula depending on the shape of the molecule. Here, the calculation was performed assuming ε = 1 (i.e. g' = g).

[0059]

number

[0060] λ=BrNo / M …(V-6) LCB 1000C =λ×14000 …(V-7) In formula (V-7), “14000” represents a molecular weight of 1000 methylene (CH2) units.

[0061] The intrinsic viscosity [η] of the copolymer (A) is preferably from 0.1 to 5.0 dL / g, more preferably from 0.5 to 5.0 dL / g, and further preferably from 0.9 to 4.0 dL / g. The weight average molecular weight (Mw) of the copolymer (A) is preferably from 10,000 to 600,000, more preferably from 30,000 to 500,000, and further preferably from 50,000 to 400,000.

[0062] It is preferable that the copolymer (A) satisfies both the above-mentioned intrinsic viscosity [η] and weight average molecular weight (Mw). In the copolymer (A), as described above, the non-conjugated polyene (a3) ​​preferably contains VNB, and more preferably is VNB. That is, in the above-mentioned formula (1), formula (2), and formula (4) described later, it is preferable that the "mass fraction of (a3)" is the "mass fraction of VNB" (mass%).

[0063] As described above, the copolymer (A) preferably contains, in addition to the structural units derived from the above (a1), (a2) and (a3), a structural unit derived from the non-conjugated polyene (a4) in a mass fraction of 0 to 20% (where the total mass fractions of the above (a1), (a2), (a3) ​​and (a4) is taken as 100% by mass). In this case, it is preferable that the following requirement (ix) is satisfied.

[0064] ≪Requirements (ix)≫ The weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​(mass fraction (mass %) of (a3)), the mass fraction of the structural unit derived from the non-conjugated polyene (a4) (mass fraction (mass %) of (a4)), the molecular weight of the non-conjugated polyene (a3) ​​(molecular weight of (a3)), and the molecular weight of the non-conjugated polyene (a4) (molecular weight of (a4)) satisfy the following formula (4): 4.5≦Mw×{(mass fraction of (a3) / 100 / molecular weight of (a3))+(mass fraction of (a4) / 100 / molecular weight of (a4))}≦45 …(4)

[0065] Formula (4) specifies the content of non-conjugated diene (the sum of (a3) ​​and (a4)) in one copolymer molecule.

[0066] When the copolymer (A) containing a structural unit derived from the non-conjugated polyene (a4) satisfies the formula (4), a power transmission belt excellent in mechanical properties and heat aging resistance can be obtained. If the requirement (ix) is not satisfied and the value of "Mw × {(mass fraction of (a3) / 100 / molecular weight of (a3)) + (mass fraction of (a4) / 100 / molecular weight of (a4))}" in formula (4) is too low, i.e., the content of non-conjugated diene is too low, sufficient crosslinking may not be achieved and appropriate mechanical properties may not be obtained. Conversely, if the value is too high, i.e., the content of non-conjugated diene is too high, excessive crosslinking may occur, resulting in deterioration of mechanical properties and further deterioration of heat aging resistance.

[0067] ≪Requirements (x)≫ The copolymer (A) is not particularly limited, but has a complex viscosity η at a frequency ω=0.01 rad / s obtained by linear viscoelasticity measurement (190° C.) using a rheometer. * ( ω =0.01) (Pa sec) and the complex viscosity η at frequency ω=10rad / s * ( ω =10) It is preferable that the apparent iodine value (Pa·sec) and the apparent iodine value derived from the non-conjugated polyene (a3) ​​satisfy the following formula (5). Log{η * ( ω =0.01)} / Log{η * ( ω =10)}≦0.0753×{apparent iodine value derived from non-conjugated polyene (a3)}+1.42 … (5)

[0068] Here, the complex viscosity η * ( ω =0.01) and the complex viscosity η * ( ω =10) is the complex viscosity η in requirement (iv) * ( ω =0.1) and the complex viscosity η * ( ω =100) The apparent iodine value derived from the non-conjugated polyene (a3) ​​can be calculated in the same manner as above, except for the measurement frequency.

[0069] Apparent iodine value derived from (a3) ​​= mass fraction of (a3) ​​× 253.81 / molecular weight of (a3) In the above formula (5), the left side represents the shear rate dependency which is an index of the amount of long chain branches, and the right side represents an index of the content of non-conjugated polyene (a3) ​​that is not consumed as long chain branches during polymerization. If the copolymer (A) satisfies the above formula (5), the degree of long chain branches is not too high, which is preferable. On the other hand, if the copolymer (A) does not satisfy the above formula (5), it is found that a large proportion of the copolymerized non-conjugated polyene (a3) ​​is consumed to form long chain branches.

[0070] Furthermore, it is preferable that the copolymer (A) contains a sufficient amount of structural units derived from the non-conjugated polyene (a3), and it is more preferable that the mass fraction of the structural units derived from the non-conjugated polyene (a3) ​​in the copolymer (mass fraction (mass%) of (a3)) and the weight average molecular weight (Mw) of the copolymer satisfy the following formula (6). 6-0.45×Ln(Mw)≦(a3) mass fraction≦10 …(6)

[0071] In addition, the copolymer (A) has a number of structural units (n a3 ) is preferably 6 or more, more preferably 6 or more and 40 or less, further preferably 7 or more and 39 or less, and particularly preferably 10 or more and 38 or less.

[0072] Such a copolymer (A) contains a sufficient amount of structural units derived from a non-conjugated polyene (a3) ​​such as VNB, has a low content of long chain branches, is excellent in curing characteristics when crosslinked using a peroxide, has good moldability, and is excellent in balance of physical properties such as mechanical properties, and is particularly excellent in heat aging resistance.

[0073] In addition, the copolymer (A) has a number of structural units (n a4 ) is preferably 29 or less, more preferably 10 or less, and even more preferably less than 1.

[0074] In such a copolymer (A), the content of structural units derived from a non-conjugated polyene (a4) such as ENB is controlled within a range that does not impair the object of the present invention, and it is less likely to undergo post-crosslinking and has sufficient heat aging resistance.

[0075] Here, the number of structural units derived from the non-conjugated polyene (a3) ​​per weight average molecular weight (Mw) of the copolymer (A) (n a3 ) or the number of structural units derived from the non-conjugated polyene (a4) (n a4 ) can be calculated from the molecular weight of the non-conjugated polyene (a3) ​​or (a4), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​or (a4) in the copolymer (the mass fraction (mass %) of (a3) ​​or (a4)), and the weight average molecular weight (Mw) of the copolymer (A) according to the following formula:

[0076] (n a3 )=(Mw)×{mass fraction of (a3) / 100} / molecular weight of non-conjugated polyene (a3) (n a4 )=(Mw)×{mass fraction of (a4) / 100} / molecular weight of non-conjugated polyene (a4) In the copolymer (A), the number of structural units derived from the non-conjugated polyenes (a3) ​​and (a4) per weight average molecular weight (Mw) (n a3 ) and (n a4 ) satisfy the above ranges, the copolymer (A) has a low content of long chain branches, is excellent in curing characteristics when crosslinking is performed using a peroxide, has good moldability, and is excellent in balance of physical properties such as mechanical properties, and is less likely to cause post-crosslinking, and is particularly excellent in heat aging resistance, which is preferable.

[0077] <Preparation of Copolymer (A)> The copolymer (A) is a copolymer obtained by copolymerizing monomers consisting of ethylene (a1), an α-olefin (a2) having 3 to 20 carbon atoms, a non-conjugated polyene (a3), and, as necessary, a non-conjugated polyene (a4).

[0078] The copolymer (A) may be prepared by any method as long as it satisfies the requirements (i) to (vi). However, the copolymer (A) is preferably prepared by copolymerizing monomers in the presence of a metallocene compound, more preferably by copolymerizing monomers in the presence of a catalyst system containing a metallocene compound, and even more preferably by a method including a step (1) of copolymerizing in the presence of a polymerization catalyst containing a specific metallocene compound, and a step (2) of deactivating the polymerization catalyst by adding an alcohol as a catalyst deactivator.

[0079] Metallocene compounds The copolymer (A) is preferably one obtained by copolymerizing monomers in the presence of a polymerization catalyst system containing at least one metallocene compound selected from the compounds represented by the following formula [A1]. When the copolymerization of monomers is carried out using a polymerization catalyst system containing such a metallocene compound, the long chain branching contained in the obtained copolymer is suppressed, and the copolymer (A) satisfying the above requirements can be easily prepared.

[0080] [ka]

[0081] In formula [A1], R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 each independently represents a hydrogen atom, a hydrocarbon group, a silicon-containing group, or a heteroatom-containing group other than a silicon-containing group; R 1 ~R 4 Among these, adjacent two groups may be bonded to each other to form a ring.

[0082] The hydrocarbon group is preferably a hydrocarbon group having 1 to 20 carbon atoms, and specific examples thereof include an alkyl group having 1 to 20 carbon atoms, an arylalkyl group having 7 to 20 carbon atoms, an aryl group or a substituted aryl group having 6 to 20 carbon atoms, etc. For example, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an allyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an amyl group, an n-pentyl group, a neopentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decanyl group, a 3-methylpentyl group, a 1,1-diethylpropyl group, a 1,1-dimethylbutyl group, a 1-methyl-1-propylbutyl group, a 1,1-propylbutyl group, a 1,1-dimethyl-2-methylpropyl group, a 1-methyl-1-isopropyl-2-methylpropyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, etc. Examples of the hydrocarbon group include oxygen-containing groups such as a methoxy group, an ethoxy group, and a phenoxy group; nitrogen-containing groups such as a nitro group, a cyano group, an N-methylamino group, an N,N-dimethylamino group, and an N-phenylamino group; boron-containing groups such as a boranetriyl group and a diboranyl group; and sulfur-containing groups such as a sulfonyl group and a sulfenyl group.

[0083] The above-mentioned hydrocarbon group may have a hydrogen atom substituted with a halogen atom, and examples thereof include a trifluoromethyl group, a trifluoromethylphenyl group, a pentafluorophenyl group, and a chlorophenyl group.

[0084] Examples of the silicon-containing group include a silyl group, a siloxy group, a hydrocarbon-substituted silyl group, a hydrocarbon-substituted siloxy group, etc. Examples include a methylsilyl group, a dimethylsilyl group, a trimethylsilyl group, an ethylsilyl group, a diethylsilyl group, a triethylsilyl group, a diphenylmethylsilyl group, a triphenylsilyl group, a dimethylphenylsilyl group, a dimethyl-t-butylsilyl group, and a dimethyl(pentafluorophenyl)silyl group.

[0085] R 6 and R 11 are the same atom or the same group selected from a hydrogen atom, a hydrocarbon group, a silicon-containing group, and a heteroatom-containing group other than a silicon-containing group, and R 7 and R 10 are the same atom or the same group selected from a hydrogen atom, a hydrocarbon group, a silicon-containing group, and a heteroatom-containing group other than a silicon-containing group, and R 6 and R 7 may be bonded to each other to form a ring, R 10 and R 11 may be bonded to each other to form a ring. 6 , R 7 , R 10 and R 11 are not all hydrogen atoms.

[0086] R 13 and R 14 each independently represents an aryl group. M 1 indicates a zirconium atom. Y 1 represents a carbon atom or a silicon atom.

[0087] Q represents a halogen atom, a hydrocarbon group, a halogenated hydrocarbon group, a neutral conjugated or non-conjugated diene having 4 to 20 carbon atoms, an anionic ligand, or a neutral ligand capable of coordinating with a lone electron pair, j represents an integer of 1 to 4, and when j is an integer of 2 or greater, multiple Qs may be the same or different.

[0088] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and preferably a chlorine atom. The hydrocarbon group is preferably a hydrocarbon group having 1 to 10 carbon atoms. Specific examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a 2-methylpropyl group, a 1,1-dimethylpropyl group, a 2,2-dimethylpropyl group, a 1,1-diethylpropyl group, a 1-ethyl-1-methylpropyl group, a 1,1,2,2-tetramethylpropyl group, a sec-butyl group, a t-butyl group, a 1,1-dimethylbutyl group, a 1,1,3-trimethylbutyl group, a neopentyl group, a cyclohexylmethyl group, a cyclohexyl group, a 1-methyl-1-cyclohexyl group, and a benzyl group. Of these, a methyl group, an ethyl group, and a benzyl group are preferred.

[0089] As the neutral conjugated or non-conjugated diene having 4 to 20 carbon atoms, a neutral conjugated or non-conjugated diene having 4 to 10 carbon atoms is preferable. Specific examples of the neutral conjugated or non-conjugated diene include s-cis- or s-trans-η 4 -1,3-butadiene, s-cis- or s-trans-η 4 -1,4-diphenyl-1,3-butadiene, s-cis- or s-trans-η 4 -3-Methyl-1,3-pentadiene, s-cis- or s-trans-η 4 -1,4-Dibenzyl-1,3-butadiene, s-cis- or s-trans-η 4 -2,4-Hexadiene, s-cis- or s-trans-η 4 -1,3-Pentadiene, s-cis- or s-trans-η 4 -1,4-Ditolyl-1,3-butadiene, s-cis- or s-trans-η 4 -1,4-bis(trimethylsilyl)-1,3-butadiene and the like.

[0090] Specific examples of the anionic ligand include alkoxy groups such as methoxy, t-butoxy, and phenoxy; carboxylate groups such as acetate and benzoate; and sulfonate groups such as mesylate and tosylate.

[0091] Specific examples of neutral ligands capable of coordinating with lone electron pairs include organic phosphorus compounds such as trimethylphosphine, triethylphosphine, triphenylphosphine, and diphenylmethylphosphine, and ethers such as tetrahydrofuran, diethyl ether, dioxane, and 1,2-dimethoxyethane.

[0092] The substituent R in the above formula [A1] 1 ~R 4 Cyclopentadienyl groups having the formula R 1 ~R 4 unsubstituted cyclopentadienyl group in which the first position is a hydrogen atom; 3-substituted cyclopentadienyl groups such as 3-t-butylcyclopentadienyl group, 3-methylcyclopentadienyl group, 3-trimethylsilylcyclopentadienyl group, 3-phenylcyclopentadienyl group, 3-adamantylcyclopentadienyl group, 3-amylcyclopentadienyl group, and 3-cyclohexylcyclopentadienyl group; Examples of 3,5-disubstituted cyclopentadienyl groups include, but are not limited to, 3-,5-disubstituted cyclopentadienyl groups such as 3-t-butyl-5-ethylcyclopentadienyl group, 3-phenyl-5-methylcyclopentadienyl group, 3,5-di-t-butylcyclopentadienyl group, 3,5-dimethylcyclopentadienyl group, 3-phenyl-5-methylcyclopentadienyl group, and 3-trimethylsilyl-5-methylcyclopentadienyl group. From the viewpoints of ease of synthesis of the metallocene compound, production costs, and copolymerization ability of the non-conjugated polyene, unsubstituted (R 1 ~R 4 A cyclopentadienyl group in which R is a hydrogen atom is preferred.

[0093] Substituent R in formula [A1] 5 ~R 12 As the fluorenyl group having the formula: R 5 ~R 12 an unsubstituted fluorenyl group, 2-1-substituted fluorenyl groups such as a 2-methylfluorenyl group, a 2-t-butylfluorenyl group, and a 2-phenylfluorenyl group; 4-1-substituted fluorenyl groups such as a 4-methylfluorenyl group, a 4-t-butylfluorenyl group, and a 4-phenylfluorenyl group; or a 2,7- or 3,6-disubstituted fluorenyl group such as a 2,7-di-t-butylfluorenyl group or a 3,6-di-t-butylfluorenyl group; 2,3,6,7-tetrasubstituted fluorenyl groups such as a 2,7-dimethyl-3,6-di-t-butylfluorenyl group and a 2,7-diphenyl-3,6-di-t-butylfluorenyl group; Or R represented by the following formulas [VI] and [V-II] 6 and R 7 are bonded to each other to form a ring, and R 10 and R 11 are bonded to each other to form a ring, and the like.

[0094] [ka]

[0095] In formulas [VI] and [V-II], R 5 , R 8 , R 9 , R 12 is the same as defined in the above formula [A1], and R a , R b , R c , R d , R e , R f , R g and R h are each independently a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and may be bonded to adjacent substituents to form a ring. Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an amyl group, and an n-pentyl group. In formula [VI], R x and R y are each independently a hydrocarbon group having 1 to 3 carbon atoms which may have an unsaturated bond, and R x R a or Rc may form a double bond together with the carbon to which R is bonded; y R e or R g may form a double bond together with the carbon to which R is bonded; x and R y and each are preferably a saturated or unsaturated hydrocarbon group having 1 or 2 carbon atoms.

[0096] Specific examples of the compound represented by the above formula [VI] or [V-II] include an octamethyloctahydrodibenzofluorenyl group represented by formula [V-III], a tetramethyldodecahydrodibenzofluorenyl group represented by formula [V-IV], an octamethyltetrahydrodicyclopentafluorenyl group represented by formula [VV], a hexamethyldihydrodicyclopentafluorenyl group represented by formula [V-VI], and a b,h-dibenzofluorenyl group represented by formula [V-VII].

[0097] [ka]

[0098] All of these metallocene compounds containing a fluorenyl group and represented by the above formula [A1] have excellent copolymerization ability with non-conjugated polyenes. 1 When Y is a silicon atom, the transition metal compound having di-substituted fluorenyl groups at 2,7 positions, di-substituted fluorenyl groups at 3,6 positions, tetra-substituted fluorenyl groups at 2,3,6,7 positions, or tetra-substituted fluorenyl groups at 2,3,6,7 positions represented by the above formula [VI] is particularly excellent. 1 is a carbon atom, R 5 From R 12 Particularly preferred are metallocene compounds having an unsubstituted fluorenyl group in which R is a hydrogen atom, a 3- and 6-disubstituted fluorenyl group, a 2-, 3-, 6- and 7-tetrasubstituted fluorenyl group, and a 2-, 3-, 6- and 7-tetrasubstituted fluorenyl group represented by the above formula [VI].

[0099] In the present invention, in the metallocene compound represented by the above formula [A1], Y1 is a silicon atom, and R 5 From R 12 If all are hydrogen atoms, R 13 and R 14 is selected from groups other than a methyl group, a butyl group, a phenyl group, a silicon-substituted phenyl group, a cyclohexyl group, and a benzyl group; Y 1 is a silicon atom, and R 6 and R 11 and R are both t-butyl groups. 5 , R 7 , R 8 , R 9 , R 10 , R 12 If is not a t-butyl group, R 13 and R 14 is selected from groups other than a benzyl group and a silicon-substituted phenyl group; Y 1 is a carbon atom, and R 5 From R 12 If all are hydrogen atoms, R 13 , R 14 is selected from groups other than a methyl group, an isopropyl group, a t-butyl group, an isobutyl group, a phenyl group, a pt-butylphenyl group, a pn-butylphenyl group, a silicon-substituted phenyl group, a 4-biphenyl group, a p-tolyl group, a naphthyl group, a benzyl group, a cyclopentyl group, a cyclohexyl group, and a xylyl group; Y 1 is a carbon atom, and R 6 and R 11 is a common group selected from a t-butyl group, a methyl group, or a phenyl group, and R 5 , R 7 , R 8 , R 9 , R 10 and R 12 If it is a group or atom different from R 13 , R 14 is selected from groups other than a methyl group, a phenyl group, a pt-butylphenyl group, a pn-butylphenyl group, a silicon-substituted phenyl group, and a benzyl group; Y 1 is a carbon atom, and R 6 is a dimethylamino group, a methoxy group, or a methyl group, and R5 , R 7 , R 8 , R 9 , R 10 , R 11 and R 12 But R 6 If it is a group or atom different from R 13 , R 14 is selected from groups other than a methyl group and a phenyl group; Y 1 is a carbon atom, and R is a fluorenyl group. 5 ~R 12 When the moiety is b,h-dibenzofluorenyl or a,i-dibenzofluorenyl, R 13 , R 14 is selected from groups other than a methyl group and a phenyl group. It is preferable.

[0100] Specific examples of the metallocene compound represented by the above formula [A1] are shown below, but the scope of the present invention is not particularly limited thereto. Specific examples of the metallocene compound represented by the above formula [A1] include: Y 1 In the case where is a silicon atom, Diphenylsilylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Diphenylsilylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Diphenylsilylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Diphenylsilylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Diphenylsilylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Diphenylsilylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Diphenylsilylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Diphenylsilylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Diphenylsilylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(p-tolyl)silylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(m-tolyl)silylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride etc.

[0101] Y 1 If is a carbon atom, Diphenylmethylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Diphenylmethylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Diphenylmethylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Diphenylmethylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Diphenylmethylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Diphenylmethylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Diphenylmethylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Diphenylmethylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(p-tolyl)methylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(m-tolyl)methylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(pt-butylphenyl)methylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(pt-butylphenyl)methylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(pt-butylphenyl)methylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(pt-butylphenyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(pt-butylphenyl)methylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(pt-butylphenyl)methylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(pt-butylphenyl)methylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(pt-butylphenyl)methylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(4-biphenyl)methylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(p-chlorophenyl)methylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(m-chlorophenyl)methylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(m-trifluoromethylphenyl)methylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(2,7-di-t-butylfluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(3,6-di-t-butylfluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(2,7-dimethyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(2,7-diphenyl-3,6-di-t-butylfluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(tetramethyldodecahydrodibenzofluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(octamethyltetrahydrodicyclopentafluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(hexamethyldihydrodicyclopentafluorenyl)zirconium dichloride, Di(2-naphthyl)methylene(cyclopentadienyl)(b,h-dibenzofluorenyl)zirconium dichloride etc.

[0102] As examples of the structural formulas of these metallocene compounds, the structural formulas of di(p-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride ((A) below) and di(p-chlorophenyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride ((B) below) are shown below.

[0103] [ka]

[0104] The above metallocene compounds can be used alone or in combination of two or more. The metallocene compound represented by the above formula [A1], which can be suitably used for preparing the copolymer (A), can be produced by any method without any particular limitation.For example, it can be produced according to the methods described in J.Organomet.Chem.,63,509(1996), WO2005 / 100410, WO2006 / 123759, WO01 / 27124, JP-A-2004-168744, JP-A-2004-175759, JP-A-2000-212194, etc.

[0105] <Catalyst containing metallocene compound> The polymerization catalyst that can be suitably used for producing the copolymer (A) includes a metallocene compound represented by the above formula [A1] (metallocene compound (a)) and capable of copolymerizing monomers.

[0106] Preferably, The metallocene compound (a) represented by the above formula [A1], and at least one compound (b) selected from an organometallic compound (b-1), an organoaluminum oxy compound (b-2), and a compound (b-3) that reacts with the metallocene compound (a) to form an ion pair (hereinafter also referred to as the "ionizing ionic compound (b-3)"), and further, if necessary, a particulate carrier (c) include a polymerization catalyst composed of.

[0107] Hereinafter, each component will be specifically described. ≪Compound (b)≫ Compound (b) is at least one compound selected from an organometallic compound (b-1), an organoaluminum oxy compound (b-2), and an ionizing ionic compound (b-3), and preferably contains at least an organometallic compound (b-1).

[0108] Organometallic compound (b-1) As the organometallic compound (b-1), for example, organometallic compounds of Groups 1, 2, 12, and 13 of the periodic table represented by the following formulas [VII] to [IX] are used.

[0109] (b-1a) Formula: R a m Al(OR b ) n H p X q …[VII] (In formula [VII], R a and R b may be the same or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, X represents a halogen atom, m is a number where 0 < m ≦ 3, n is a number where 0 ≦ n < 3, p is a number where 0 ≦ p < 3, q is a number where 0 ≦ q < 3, and m + n + p + q = 3.) An organoaluminum compound represented by.

[0110] Examples of such compounds include trialkylaluminums such as trimethylaluminum, triethylaluminum, triisobutylaluminum, and tri-n-octylaluminum, tricycloalkylaluminums, isobutylaluminum dichloride, diethylaluminum chloride, ethylaluminum dichloride, ethylaluminum sesquichloride, methylaluminum dichloride, dimethylaluminum chloride, and diisobutylaluminum hydride.

[0111] (b-1b) Formula:M 2 AlR a 4. [VIII] (In formula [VIII], M 2 indicates Li, Na or K, and R a is a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms.

[0112] Such compounds include LiAl(C2H5)4, LiAl(C7H 15 ) 4 can be given as an example. (b-1c) Formula: R a R b M 3 …[IX] (In formula [IX], R a and R b may be the same or different and each represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; M 3 is Mg, Zn or Cd. Dialkyl compounds having a metal of Group 2 or 12 of the Periodic Table represented by the formula:

[0113] Among the organometallic compounds (b-1), organoaluminum compounds such as triethylaluminum, triisobutylaluminum, and tri-n-octylaluminum are preferred. The organometallic compound (b-1) can be used alone or in combination of two or more kinds.

[0114] Organoaluminum oxy compound (b-2) The organoaluminum oxy compound (b-2) may be a conventionally known aluminoxane, or may be a benzene-insoluble organoaluminum oxy compound such as those exemplified in JP-A-2-78687.

[0115] Conventionally known aluminoxanes can be produced, for example, by the following method, and are usually obtained as a solution in a hydrocarbon solvent. (1) A method in which an organoaluminum compound such as trialkylaluminum is added to a hydrocarbon medium suspension of a compound containing adsorbed water or a salt containing water of crystallization, such as magnesium chloride hydrate, copper sulfate hydrate, aluminum sulfate hydrate, nickel sulfate hydrate, or cerous chloride hydrate, to react the adsorbed water or the water of crystallization with the organoaluminum compound.

[0116] (2) A method in which water, ice or water vapor is allowed to act directly on an organoaluminum compound such as trialkylaluminum in a medium such as benzene, toluene, ethyl ether or tetrahydrofuran.

[0117] (3) A method in which an organoaluminum compound such as trialkylaluminum is reacted with an organotin oxide such as dimethyltin oxide or dibutyltin oxide in a medium such as decane, benzene, or toluene.

[0118] The aluminoxane may contain a small amount of an organometallic component. After the solvent or unreacted organoaluminum compound is removed by distillation from the recovered solution of the aluminoxane, the aluminoxane may be redissolved in a solvent or suspended in a poor solvent for the aluminoxane.

[0119] As the organoaluminum compound used in preparing the aluminoxane, there can be mentioned the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to (b-1a).

[0120] Of these, trialkylaluminum and tricycloalkylaluminum are preferred, and among these, trimethylaluminum and triisobutylaluminum are particularly preferred. The organoaluminum compounds can be used alone or in combination.

[0121] The benzene-insoluble organoaluminum oxy-compound, which is one embodiment of the organoaluminum oxy-compound (b-2), is preferably one in which the Al component soluble in benzene at 60°C is usually 10% by mass or less, preferably 5% by mass or less, and particularly preferably 2% by mass or less, calculated as Al atoms, relative to 100% by mass of benzene, i.e., one which is insoluble or poorly soluble in benzene.

[0122] The organoaluminum oxy compound (b-2) may also be an organoaluminum oxy compound containing boron represented by the following formula [X].

[0123] [ka]

[0124] In formula [X], R 1 represents a hydrocarbon group having 1 to 10 carbon atoms, R 2 ~R 5 may be the same or different and represent a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms. The boron-containing organoaluminum oxy compound represented by the formula [X] is Formula:R 1 -B(OH)2…[XI] (In formula [XI], R 1 is R in the above formula [X] 1 It shows the same group as and an alkylboronic acid represented by the formula: The compound can be produced by reacting the compound with an organoaluminum compound in an inert solvent under an inert gas atmosphere at a temperature of from −80° C. to room temperature for 1 minute to 24 hours.

[0125] Examples of the alkylboronic acid represented by the above formula [XI] include methylboronic acid, ethylboronic acid, isopropylboronic acid, n-propylboronic acid, n-butylboronic acid, isobutylboronic acid, n-hexylboronic acid, cyclohexylboronic acid, phenylboronic acid, 3,5-difluorophenylboronic acid, pentafluorophenylboronic acid, and 3,5-bis(trifluoromethyl)phenylboronic acid.

[0126] Of these, methylboronic acid, n-butylboronic acid, isobutylboronic acid, 3,5-difluorophenylboronic acid, and pentafluorophenylboronic acid are preferred. These can be used alone or in combination of two or more.

[0127] Examples of the organoaluminum compound to be reacted with such an alkylboronic acid include the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the above (b-1a). Among these, trialkylaluminum and tricycloalkylaluminum are preferred, and trimethylaluminum, triethylaluminum and triisobutylaluminum are particularly preferred.

[0128] The organoaluminum oxy-compound (b-2) can be used alone or in combination of two or more. Ionized ionic compounds (b-3) Examples of the ionized ionic compound (b-3) include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-A-1-501950, JP-A-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and USP 5321106. In addition, examples include heteropoly compounds and isopoly compounds.

[0129] The ionized ionic compound (b-3) can be used alone or in combination of two or more kinds. Specifically, Lewis acids include compounds represented by BR3 (R is fluorine or a phenyl group which may have a substituent such as fluorine, a methyl group, or a trifluoromethyl group), such as trifluoroboron, triphenylboron, tris(4-fluorophenyl)boron, tris(3,5-difluorophenyl)boron, tris(4-fluoromethylphenyl)boron, tris(pentafluorophenyl)boron, tris(p-tolyl)boron, tris(o-tolyl)boron, and tris(3,5-dimethylphenyl)boron.

[0130] An example of the ionic compound is a compound represented by the formula [XII].

[0131] [ka]

[0132] In formula [XII], R 1+ As for H + , carbonium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptyltrienyl cation, ferrocenium cation having a transition metal, etc. 2 ~R 5 may be the same or different and are organic groups, preferably aryl groups or substituted aryl groups.

[0133] Specific examples of the carbonium cation include tri-substituted carbonium cations such as triphenylcarbonium cation, tri(methylphenyl)carbonium cation, and tri(dimethylphenyl)carbonium cation.

[0134] Specific examples of the ammonium cation include trialkylammonium cations such as trimethylammonium cation, triethylammonium cation, tripropylammonium cation, tributylammonium cation, and tri(n-butyl)ammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N,2,4,6-pentamethylanilinium cation; Examples of the cation include dialkylammonium cations such as di(isopropyl)ammonium cation and dicyclohexylammonium cation.

[0135] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tri(methylphenyl)phosphonium cation, and tri(dimethylphenyl)phosphonium cation.

[0136] R 1+ As the cation, a carbonium cation, an ammonium cation, etc. are preferred, and in particular, a triphenylcarbonium cation, an N,N-dimethylanilinium cation, and an N,N-diethylanilinium cation are preferred.

[0137] Further, examples of the ionic compound include trialkyl-substituted ammonium salts, N,N-dialkylanilinium salts, dialkylammonium salts, and triarylphosphonium salts.

[0138] Specific examples of trialkyl-substituted ammonium salts include triethylammonium tetra(phenyl)boron, tripropylammonium tetra(phenyl)boron, tri(n-butyl)ammonium tetra(phenyl)boron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o-tolyl)boron, tri(n-butyl)ammonium tetra(pentafluorophenyl)boron, tripropylammonium tetra(o,p-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(N,N-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(p-trifluoromethylphenyl)boron, tri(n-butyl)ammonium tetra(3,5-ditrifluoromethylphenyl)boron, and tri(n-butyl)ammonium tetra(o-tolyl)boron.

[0139] Specific examples of N,N-dialkylanilinium salts include N,N-dimethylanilinium tetra(phenyl)boron, N,N-diethylanilinium tetra(phenyl)boron, and N,N,2,4,6-pentamethylanilinium tetra(phenyl)boron.

[0140] Specific examples of dialkylammonium salts include di(1-propyl)ammonium tetra(pentafluorophenyl)boron and dicyclohexylammonium tetra(phenyl)boron.

[0141] Further examples of the ionic compound include triphenylcarbenium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, ferrocenium tetra(pentafluorophenyl)borate, triphenylcarbenium pentaphenylcyclopentadienyl complex, N,N-diethylanilinium pentaphenylcyclopentadienyl complex, and boron compounds represented by the following formula [XIII] or [XIV]. In the following formula, Et represents an ethyl group.

[0142] [ka]

[0143] Specific examples of the borane compound include Decaborane; Salts of anions such as bis[tri(n-butyl)ammonium]nonaborate, bis[tri(n-butyl)ammonium]decaborate, bis[tri(n-butyl)ammonium]undecaborate, bis[tri(n-butyl)ammonium]dodecaborate, bis[tri(n-butyl)ammonium]decachlorodecaborate, and bis[tri(n-butyl)ammonium]dodecachlorododecaborate; Salts of metal borane anions, such as tri(n-butyl)ammonium bis(dodecahydridedodecaborate)cobaltate(III) and bis[tri(n-butyl)ammonium]bis(dodecahydridedodecaborate)nickelate(III); Examples include:

[0144] Specific examples of the carborane compound include: 4-Carbanonaborane, 1,3-Dicarbanonaborane, 6,9-Dicarbadecaborane, Dodecahydride-1-phenyl-1,3-dicarbanonaborane, Dodecahydride-1-methyl-1,3-dicarbanonaborane, Undecahydride-1,3-dimethyl-1,3-dicarbanonaborane, 7,8-Dicarbaundecaborane, 2,7-Dicarbaundecaborane, Undecahydride-7,8-dimethyl-7,8-dicarbaundecaborane, Dodeca Hydride-11-methyl-2,7-dicarboxundecaborane, tri(n-butyl)ammonium 1-carbadecaborate, tri(n-butyl)ammonium-1-carbaundecaborate, tri(n-butyl)ammonium-1-carbadodecaborate, tri(n-butyl)ammonium-1-trimethylsilyl-1-carbadecaborate, tri(n-butyl)ammonium bromo-1-carbadodecaborate, tri(n-butyl)ammonium-6-carbadecaborate Rubadecaborate, tri(n-butyl)ammonium-7-carboundecaborate, tri(n-butyl)ammonium-7,8-dicarboxaundecaborate, tri(n-butyl)ammonium-2,9-dicarboxaundecaborate, tri(n-butyl)ammonium dodecahydride-8-methyl-7,9-dicarboxaundecaborate, tri(n-butyl)ammonium undecahydride-8-ethyl-7,9-dicarboxaundecaborate, tri(n -butyl)ammonium undecahydride-8-butyl-7,9-dicarboxaundecaborate, tri(n-butyl)ammonium undecahydride-8-allyl-7,9-dicarboxaundecaborate, tri(n-butyl)ammonium undecahydride-9-trimethylsilyl-7,8-dicarboxaundecaborate, tri(n-butyl)ammonium undecahydride-4,6-dibromo-7-carbaundecaborate, and other salts of anions; Tri(n-butyl)ammonium bis(nonahydride-1,3-dicarbanonaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)ferrate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)nickelate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cuprate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)aurate(III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarbandecaborate) salts of metal carborane anions such as tri(n-butyl)ammonium bis(undecahydride-7-carboondecaborate)ferrate(III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarboxaborate)chromate(III), tri(n-butyl)ammonium bis(tribromooctahydride-7,8-dicarboxaborate)cobaltate(III), tris[tri(n-butyl)ammonium]bis(undecahydride-7-carboondecaborate)chromate(III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carboondecaborate)manganate(IV), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carboondecaborate)cobaltate(III), and bis[tri(n-butyl)ammonium]bis(undecahydride-7-carboondecaborate)nickelate(IV); Examples include:

[0145] The heteropoly compound is composed of an atom selected from silicon, phosphorus, titanium, germanium, arsenic and tin, and one or more atoms selected from vanadium, niobium, molybdenum and tungsten. Specifically, usable are phosphovanadic acid, germanovanadic acid, arsenic vanadic acid, phosphoniobic acid, germanoniobic acid, siliconomolybdic acid, phosphomolybdic acid, titanomolybdic acid, germanomolybdic acid, arsenic molybdic acid, tinmolybdic acid, phosphotungstic acid, germanotungstic acid, tintungstic acid, phosphomolybdovanadic acid, phosphotungstovanadic acid, germanotungstovanadic acid, phosphomolybdotungstovanadic acid, germanomolybdotungstovanadic acid, phosphomolybdotungstic acid, phosphomolybdoniobic acid, and salts of these acids, for example, salts with metals of Group 1 or 2 of the periodic table, specifically, lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc., and organic salts such as triphenylethyl salts. However, the present invention is not limited to these.

[0146] Among the ionizing ionic compounds (b-3), the above-mentioned ionic compounds are preferred, and among them, triphenylcarbenium tetrakis(pentafluorophenyl)borate and N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate are more preferred.

[0147] In the present invention, when a metallocene catalyst containing a metallocene compound (a) represented by the above formula [A1], an organometallic compound (b-1) such as triisobutylaluminum, an organoaluminum oxy compound (b-2) such as methylaluminoxane, and an ionizing ionic compound (b-3) such as triphenylcarbenium tetrakis(pentafluorophenyl)borate is used as a polymerization catalyst, extremely high polymerization activity can be exhibited in the production of the copolymer (A).

[0148] Particulate carrier (c) In the present invention, the particulate carrier (c) used as necessary is an inorganic or organic compound, and is a granular or fine particle solid.

[0149] The inorganic compound is preferably a porous oxide, an inorganic halide, a clay, a clay mineral, or an ion-exchangeable layered compound, specific examples of which are described in WO2015 / 122495.

[0150] The clay, clay mineral, and ion-exchangeable layered compound may be used as is, or after treatment such as ball milling or sieving. They may also be used after adding and adsorbing new water or after heat dehydration treatment. Furthermore, these may be used alone or in combination.

[0151] Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, hectorite, taeniolite and synthetic mica are particularly preferred. The organic compound may be a granular or fine particle solid having a particle size in the range of 10 to 300 μm.Specific examples include (co)polymers mainly made of α-olefins having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, or (co)polymers mainly made of vinylcyclohexane and styrene, and their modifications.

[0152] Organic compound component (d) The metallocene catalyst comprises a metallocene compound (a), at least one compound (b) selected from an organometallic compound (b-1), an organoaluminum oxy compound (b-2) and an ionizing ionic compound (b-3), and a carrier (c) used as needed, and may further contain a specific organic compound component (d) as needed.

[0153] In the present invention, the organic compound component (d) is used as necessary for the purpose of improving the polymerization performance and the physical properties of the resulting polymer. Examples of such organic compounds include, but are not limited to, alcohols, phenolic compounds, carboxylic acids, phosphorus compounds, and sulfonates.

[0154] <Production method and conditions of copolymer (A)> The copolymer (A) can be produced by copolymerizing monomers consisting of ethylene (a1), an α-olefin (a2) having 3 to 20 carbon atoms, a non-conjugated polyene (a3), and, as necessary, a non-conjugated polyene (a4).

[0155] When copolymerizing such monomers, the method of use and the order of addition of each component constituting the above-mentioned polymerization catalyst may be selected arbitrarily, and examples thereof include the following methods (1) to (5). (1) A method in which the metallocene compound (a) is added alone to a polymerization reactor. (2) A metallocene compound (a) and a compound (b), A method of adding ingredients to a polymerization reactor in any order. (3) A catalyst component in which a metallocene compound (a) is supported on a carrier (c), and a compound (b) is A method of adding ingredients to a polymerization reactor in any order. (4) A catalyst component in which the compound (b) is supported on a carrier (c), the metallocene compound (a), A method of adding ingredients to a polymerization reactor in any order. (5) A catalyst component in which the metallocene compound (a) and the compound (b) are supported on a carrier (c), Addition to the polymerization vessel.

[0156] In each of the above methods (2) to (5), at least two of the metallocene compound (a), the compound (b) and the support (c) may be contacted in advance. In the above methods (4) and (5) in which the compound (b) is supported, the unsupported compound (b) may be added in any order, if necessary. In this case, the compound (b) may be the same as or different from the compound (b) supported on the support (c).

[0157] In addition, the solid catalyst component in which the metallocene compound (a) is supported on the carrier (c) and the solid catalyst component in which the metallocene compound (a) and the compound (b) are supported on the carrier (c) may be a solid catalyst component in which an olefin is prepolymerized, or a catalyst component may be further supported on the prepolymerized solid catalyst component.

[0158] The copolymer (A) can be suitably obtained by copolymerizing monomers in the presence of the above-mentioned polymerization catalyst. When olefin polymerization is carried out using the above polymerization catalyst, the metallocene compound (a) is usually used in an amount of 10 -12 ~10 -2 Molar, preferably 10 -10 ~10 -8 It is used in molar amounts.

[0159] The compound (b-1) is used in an amount such that the molar ratio [(b-1) / M] of the compound (b-1) to the total transition metal atoms (M) in the metallocene compound (a) is usually 0.01-50000, preferably 0.05-10000. The compound (b-2) is used in an amount such that the molar ratio [(b-2) / M] of the aluminum atoms in the compound (b-2) to the total transition metals (M) in the metallocene compound (a) is usually 10-50000, preferably 20-10000. The compound (b-3) is used in an amount such that the molar ratio [(b-3) / M] of the compound (b-3) to the transition metal atoms (M) in the metallocene compound (a) is usually 1-20, preferably 1-15.

[0160] In the present invention, the method for producing the copolymer (A) can be carried out by any of liquid phase polymerization methods such as solution (dissolution) polymerization and suspension polymerization, or gas phase polymerization methods, and is not particularly limited. However, it is preferable that the method includes a step of obtaining the following polymerization reaction liquid.

[0161] The step of obtaining a polymerization reaction liquid is a step of carrying out a polymerization reaction using an aliphatic hydrocarbon as a polymerization solvent, 1 R bonded to 13 , R 14is a phenyl group or a phenyl group substituted with an alkyl group or a halogen group, and R 7 , R 10 The process comprises copolymerizing monomers consisting of ethylene (a1), an α-olefin (a2) having 3 to 20 carbon atoms, a non-conjugated polyene (a3) ​​and, if necessary, a non-conjugated polyene (a4) in the presence of a polymerization catalyst containing a transition metal compound having an alkyl substituent, to obtain a polymerization reaction liquid of copolymer (A).

[0162] Examples of the polymerization solvent include aliphatic hydrocarbons and aromatic hydrocarbons. Specifically, examples include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; and halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane. One or more of these can be used. Olefin itself can also be used as the solvent. Among these, hexane is preferred from the viewpoint of separation and purification from the resulting copolymer (A).

[0163] The polymerization temperature is usually in the range of -50 to +200°C, preferably in the range of 0 to +150°C, and more preferably in the range of +70 to +110°C. Although it depends on the attained molecular weight and polymerization activity of the metallocene catalyst system used, a higher temperature (+70°C or higher) is desirable from the viewpoints of catalytic activity, copolymerizability, and productivity.

[0164] The polymerization pressure is usually normal pressure to 10 MPa gauge pressure, preferably 1.1 to 5.0 MPa gauge pressure, more preferably 1.2 to 2.0 MPa gauge pressure, and the polymerization reaction can be carried out by any of batch, semi-continuous, and continuous methods. Furthermore, the polymerization can be carried out in two or more stages with different reaction conditions. Among these, in the present invention, it is preferable to adopt a method in which the monomers are continuously fed into a reactor to carry out copolymerization.

[0165] The reaction time (average residence time when copolymerization is carried out by a continuous method) varies depending on conditions such as catalyst concentration and polymerization temperature, but is usually 0.5 minutes to 5 hours, preferably 5 minutes to 3 hours, and more preferably 10 minutes to 2 hours.

[0166] The molecular weight of the resulting copolymer (A) can be adjusted by making hydrogen exist in the polymerization system or by changing the polymerization temperature. Furthermore, it can also be adjusted by the amount of compound (b) used. Specific examples include triisobutylaluminum, methylaluminoxane, and diethylzinc. When hydrogen is added, the amount is suitably about 0.001 to 100 NL per kg of olefin.

[0167] The molar ratio of ethylene (a1) to α-olefin (a2) (ethylene (a1) / α-olefin (a2)) is preferably 40 / 60 to 99.9 / 0.1, more preferably 50 / 50 to 90 / 10, further preferably 55 / 45 to 85 / 15, and most preferably 55 / 45 to 78 / 22.

[0168] The amount of the non-conjugated polyene (a3) ​​charged is usually 0.07 to 10 mass%, preferably 0.1 to 8.0 mass%, and more preferably 0.5 to 5.0 mass%, relative to 100 mass% of the total of ethylene (a1), α-olefin (a2), and non-conjugated polyene (a3) ​​(total monomer charging amount).

[0169] In the present invention, it is preferable to include a step (2) of deactivating the polymerization catalyst by adding a catalyst deactivator after the step (1) of carrying out copolymerization in the presence of the polymerization catalyst. As the catalyst deactivator, alcohols can be used, with methanol or ethanol being preferred, and ethanol being particularly preferred.

[0170] In step (2), the catalyst deactivator is preferably added in an amount of 0.05 to 3.0 mol times, more preferably 0.06 to 2.5 mol times, and even more preferably 0.08 to 2.0 mol times relative to the organometallic compound (b-1), so that a small amount of catalyst degraded by the catalyst deactivator such as ethanol is generated and the low molecular weight components are moderately polymerized, resulting in a copolymer (A) with a moderately wide molecular weight distribution. On the other hand, if the amount of catalyst deactivator added is too large, almost no modified catalyst is generated and almost no polymerization of low molecular weight components is performed, so the molecular weight distribution of the resulting copolymer (A) tends to be narrow. In addition, if the catalyst deactivator is not added or the amount added is too small, a large amount of modified catalyst is generated and a large amount of low molecular weight components are polymerized, so the content of low molecular weight components in the resulting copolymer (A) tends to be too high.

[0171] <Carbon black (B)> The composition of the present embodiment contains carbon black (B). Carbon black (B) is a component that contributes to improving, for example, the mechanical strength, modulus, and abrasion resistance of the resulting crosslinked molded article.

[0172] Examples of carbon black (B) include SRF, GPF, FEF, MAF, HAF, ISAF, SAF, FT, and MT. The surface of the carbon black may be treated with a silane coupling agent. Examples of commercially available carbon black include "Asahi #55G", "Asahi #50HG", "Asahi #60G", "Asahi #60UG", and "Asahi #70" (trade names, manufactured by Asahi Carbon Co., Ltd.), "Seest V", and "Seest SO" (trade names, manufactured by Tokai Carbon Co., Ltd.).

[0173] The composition of the present embodiment may contain one type of carbon black (B) or may contain two or more types of carbon black (B). The content of carbon black (B) in the composition of this embodiment is preferably 0.1 to 200 parts by mass, more preferably 10 to 200 parts by mass, and further preferably 20 to 100 parts by mass, based on 100 parts by mass of copolymer (A). Such an embodiment is preferable from the viewpoints of the mechanical strength of the obtained crosslinked molded article and the processability of the composition of this embodiment.

[0174] <Short Fiber (C)> The composition of the present embodiment contains short fibers (C). By using the short fibers (C), the modulus and mechanical strength of the crosslinked molded article formed from the composition can be improved. Since the copolymer (A) has excellent kneadability with the short fibers (C), the composition of the present embodiment tends to have excellent moldability even if it contains the short fibers (C).

[0175] Examples of the short fibers (C) include fibers made of synthetic resins such as polyamide, polyimide, polyester, polyvinyl alcohol, rayon, polyolefin, polyarylate, polyphenylene sulfide, polyether ether ketone, polyparaphenylene benzobisoxazole, and fluorine-based polymers; and natural fibers such as cotton and wood cellulose fibers. Among these, short fibers made of synthetic resins are preferred, and short fibers made of polyamide are more preferred. The short fibers (C) are usually not short fibers formed from the copolymer (A).

[0176] Examples of polyamides include aliphatic polyamides such as polycapramide, poly-ω-aminoheptanoic acid, poly-ω-aminononanoic acid, polyundecaneamide, polyethylenediamineadipamide, polytetramethyleneadipamide, polyhexamethyleneadipamide, polyhexamethylenesebacamide, polyhexamethylenedodecamamide, polyoctamethyleneadipamide, and polydecamethyleneadipamide; Examples of the polyamides include aromatic polyamides (aramids) such as polyparaphenylene terephthalamide (trade name "Kevlar", manufactured by DuPont-Toray Co., Ltd.), polymetaphenylene isophthalamide, copolyparaphenylene-3,4'-oxydiphenylene terephthalamide, polymetaxylylene adipamide, polymetaxylylene pimelamide, polymetaxylylene azelamide, polyparaxylylene azelamide, and polyparaxylylene decanamide.

[0177] As the short fibers (C), from the viewpoint of further improving the tensile stress and tear strength of the resulting crosslinked molded article, short fibers made of aromatic polyamide, i.e., aramid short fibers, are preferred, and polyparaphenylene terephthalamide short fibers, polymetaphenylene isophthalamide short fibers, and copolyparaphenylene-3,4'-oxydiphenylene terephthalamide short fibers are more preferred.

[0178] The short fibers (C) have an average fiber length of usually 0.1 to 50 mm, preferably 0.5 to 10 mm, and more preferably 0.5 to 6 mm. The short fibers (C) have a fiber diameter of usually 0.1 to 100 μm, preferably 0.1 to 25 μm, and more preferably 1 to 20 μm.

[0179] The average fiber length of the staple fibers (C) can be determined, for example, by photographing the staple fibers with an optical microscope, measuring the lengths of 100 staple fibers randomly selected from the photograph, and calculating the arithmetic average.

[0180] The staple fibers (C) may be chopped fiber (cut fiber)-like staple fibers or pulp-like staple fibers having fibrils. The composition of the present embodiment may contain one type of short fiber (C) or may contain two or more types of short fibers (C).

[0181] The content of the short fibers (C) in the composition of the present embodiment is preferably 0.1 to 100 parts by mass, more preferably 0.1 to 30 parts by mass, and further preferably 3 to 20 parts by mass, based on 100 parts by mass of the copolymer (A). Such an embodiment is preferable from the viewpoints of the modulus and mechanical strength of the obtained crosslinked molded article.

[0182] <Peroxide-based crosslinking agent (D)> The composition of the present embodiment contains a peroxide-based crosslinking agent (D). It is believed that the use of the peroxide-based crosslinking agent (D) can satisfactorily crosslink the copolymer (A) and improve the heat aging resistance of the resulting crosslinked molded article.

[0183] The peroxide-based crosslinking agent (D) is preferably an organic peroxide. Examples of the organic peroxide include dicumyl peroxide, di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, tert-butylperoxyisopropylcarbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.

[0184] The composition of the present embodiment may contain one type of peroxide-based crosslinking agent (D), or may contain two or more types of peroxide-based crosslinking agents (D). In the composition of the present embodiment, the content of the peroxide-based crosslinking agent (D) is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the total of the copolymer (A) and other polymers (rubbers, etc.) that require crosslinking and are blended as necessary. In such an embodiment, crosslinking proceeds well, and is preferable from the viewpoint of the heat resistance and abrasion resistance of the obtained crosslinked molded article.

[0185] <Crosslinking coagent (E) having two or more ethylenic double bonds> The composition of the present embodiment contains a crosslinking aid (E) having two or more ethylenic double bonds. The number of ethylenic double bonds in the crosslinking aid (E) is preferably 2 to 6, more preferably 2 to 4. It is believed that the use of the crosslinking aid (E) allows a good network to be formed between the copolymer (A) and the short fibers (C).

[0186] Examples of the crosslinking aid (E) include (meth)acrylic crosslinking aids such as ethylene glycol di(meth)acrylate and trimethylolpropane tri(meth)acrylate, allyl crosslinking aids such as diallyl phthalate and triallyl isocyanurate, and vinyl crosslinking aids such as divinylbenzene. Among these, (meth)acrylic crosslinking aids are preferred, and ethylene glycol dimethacrylate is more preferred.

[0187] The composition of the present embodiment may contain one type of crosslinking auxiliary (E), or may contain two or more types of crosslinking auxiliary (E). In the composition of the present embodiment, the content of the crosslinking auxiliary (E) is preferably 0.01 to 22 mol, more preferably 0.1 to 11 mol, and further preferably 0.1 to 8 mol, relative to 1 mol of the peroxide-based crosslinking agent (D). In such an embodiment, crosslinking proceeds well, and is preferable from the viewpoint of the heat resistance and abrasion resistance of the obtained crosslinked molded article.

[0188] <Other ingredients> The composition of the present embodiment may further contain at least one selected from a crosslinking agent other than the peroxide-based crosslinking agent (D), a crosslinking assistant other than the crosslinking assistant (E), a softener, an inorganic filler, a reinforcing agent, an antiaging agent, a processing assistant, an activator, a moisture absorbent, an antistatic agent, a colorant, a lubricant, and a thickener. The composition of the present embodiment may further contain other polymers other than the copolymer (A), such as elastomers and / or rubbers. Each of the components described below may be used alone or in combination.

[0189] {Crosslinking agents other than peroxide-based crosslinking agents (D), crosslinking assistants other than crosslinking assistant agents (E)} A crosslinking agent other than the crosslinking agent (D) may be used in combination with the peroxide crosslinking agent (D). Examples of the crosslinking agent other than the crosslinking agent (D) include crosslinking agents that are generally used when crosslinking rubber, such as sulfur-based compounds, phenolic resins, hydrosilicone-based compounds, amino resins, quinones or derivatives thereof, amine-based compounds, azo-based compounds, epoxy-based compounds, and isocyanate-based compounds.

[0190] Examples of sulfur-based compounds include sulfur, sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dithiocarbamate.

[0191] In the composition of the present embodiment, when a sulfur-based compound is also used as a crosslinking agent, the content of the sulfur-based compound is preferably 0.3 to 10 parts by mass, more preferably 0.5 to 7.0 parts by mass, and even more preferably 0.7 to 5.0 parts by mass, relative to 100 parts by mass in total of the copolymer (A) and other polymers (rubbers, etc.) that require crosslinking and are blended as necessary.

[0192] When a sulfur-based compound is used as a crosslinking agent, it is preferable to use a vulcanization accelerator in combination. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole, 2-(4-morpholinodithio)benzothiazole, 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-diethyl-4-morpholinothio)benzothiazole, and dibenzothiazyl disulfide; guanidine-based vulcanization accelerators such as diphenylguanidine, triphenylguanidine, and diorthotolylguanidine; aldehyde amine-based vulcanization accelerators such as acetaldehyde-aniline condensation product and butylaldehyde-aniline condensation product; 2-mercaptoimidazoline; imidazoline-based vulcanization accelerators such as diethylthiourea and dibutylthiourea; thiuram-based vulcanization accelerators such as tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, and dipentamethylenethiuram tetrasulfide; dithioacid salt-based vulcanization accelerators such as zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, and tellurium diethyldithiocarbamate; thiourea-based vulcanization accelerators such as ethylenethiourea (for example, Suncerer 22C (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), N,N'-diethylthiourea, and N,N'-dibutylthiourea; xanthate-based vulcanization accelerators such as zinc dibutylxatogenate; and others such as zinc oxide.

[0193] When the composition of the present embodiment contains a vulcanization accelerator, the content of the vulcanization accelerator is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass, relative to 100 parts by mass in total of the copolymer (A) and other polymers (rubbers, etc.) that require crosslinking and are blended as necessary.

[0194] The vulcanization aid can be preferably used when a sulfur-based compound is also used as a crosslinking agent, and examples thereof include zinc oxide (e.g., ZnO#1 / zinc oxide type 2, manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name; manufactured by Inoue Lime Industry Co., Ltd.)).

[0195] When the composition of the present embodiment contains a vulcanization aid, the content of the vulcanization aid is preferably 1 to 20 parts by mass per 100 parts by mass of the total of the copolymer (A) and other polymers (rubbers, etc.) that require crosslinking and are blended as necessary.

[0196] In addition, a crosslinking assistant other than the crosslinking assistant (E) may be used in combination with the crosslinking assistant (E). Examples of the crosslinking assistant include sulfur; quinone dioxime-based crosslinking assistants such as p-quinone dioxime; and metal oxides such as zinc oxide (e.g., ZnO#1-zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name; manufactured by Inoue Seki Kogyo Co., Ltd.)).

[0197] When the composition of the present embodiment contains a crosslinking aid other than the crosslinking aid (E), the content of the crosslinking aid other than the crosslinking aid (E) is preferably 0.5 to 10 mol, more preferably 0.5 to 7 mol, and even more preferably 1 to 5 mol, relative to 1 mol of the peroxide-based crosslinking agent (D).

[0198] Softener Examples of softeners include petroleum-based softeners such as process oil, lubricating oil, paraffin oil, liquid paraffin, petroleum asphalt, and Vaseline; coal tar-based softeners such as coal tar; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, soybean oil, and coconut oil; waxes such as beeswax and carnauba wax; fatty acids or salts thereof such as ricinoleic acid, palmitic acid, stearic acid, barium stearate, and calcium stearate; naphthenic acid, pine oil, rosin, and derivatives thereof; synthetic polymeric substances such as terpene resins, petroleum resins, and coumarone-indene resins; ester-based softeners such as dioctyl phthalate and dioctyl adipate; and other microcrystalline waxes, liquid polybutadiene, modified liquid polybutadiene, hydrocarbon-based synthetic lubricating oils, tall oil, and sub(factice). Petroleum-based softeners are preferred, and process oils are more preferred.

[0199] When the composition of the present embodiment contains a softener, the content of the softener is preferably 2 to 100 parts by mass, more preferably 5 to 100 parts by mass, per 100 parts by mass of the total of the copolymer (A) and other polymers (elastomers, rubbers, etc.) blended as necessary.

[0200] <Inorganic fillers> Examples of inorganic fillers include light calcium carbonate, heavy calcium carbonate, talc, and clay. Of these, heavy calcium carbonate is preferred.

[0201] When the composition of the present embodiment contains an inorganic filler, the content of the inorganic filler is preferably 2 to 50 parts by mass, more preferably 5 to 50 parts by mass, per 100 parts by mass in total of the copolymer (A) and other polymers (elastomers, rubbers, etc.) blended as necessary.

[0202] Reinforcement Examples of the reinforcing agent include silica, calcium carbonate, activated calcium carbonate, fine talc, and differential silicic acid, except for the above-mentioned carbon black (B).

[0203] When the composition of the present embodiment contains a reinforcing agent, the content of the reinforcing agent is preferably 0.1 to 100 parts by mass, more preferably 5 to 30 parts by mass, per 100 parts by mass in total of the copolymer (A) and other polymers (elastomers, rubbers, etc.) blended as necessary.

[0204] {Anti-aging agent (stabilizer)} The composition of the present embodiment contains an antioxidant (stabilizer), which can extend the life of the crosslinked molded article formed from the composition. Examples of the antioxidant include amine-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants.

[0205] Examples of the amine-based antiaging agents include aromatic secondary amine-based antiaging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine. Examples of the phenol-based antiaging agents include dibutylhydroxytoluene and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]. Examples of the sulfur-based antiaging agents include thioether-based antiaging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based antiaging agents such as nickel dibutyldithiocarbamate; 2-mercaptobenzoylimidazole, 2-mercaptobenzimidazole, zinc salt of 2-mercaptobenzimidazole, dilaurylthiodipropionate, and distearylthiodipropionate.

[0206] When the composition of the present embodiment contains an antioxidant, the content of the antioxidant is preferably 0.3 to 10 parts by mass, more preferably 0.5 to 7.0 parts by mass, per 100 parts by mass in total of the copolymer (A) and other polymers (elastomers, rubbers, etc.) blended as necessary.

[0207] Processing aids As the processing aid, a wide variety of processing aids that are generally compounded with rubber can be used. Examples of processing aids include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, and esters. Among these, stearic acid is preferred.

[0208] When the composition of the present embodiment contains a processing aid, the content of the processing aid is preferably 10 parts by mass or less, more preferably 8.0 parts by mass or less, per 100 parts by mass of the total of the copolymer (A) and other polymers (elastomers, rubbers, etc.) that are blended as necessary.

[0209] Activator Examples of the activator include amines such as di-n-butylamine, dicyclohexylamine, and monoethanolamine; activators such as diethylene glycol, polyethylene glycol, lecithin, triaryl methylate, and zinc compounds of aliphatic or aromatic carboxylic acids; zinc peroxide preparations; octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds.

[0210] When the composition of the present embodiment contains an activator, the content of the activator is preferably 0.2 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, per 100 parts by mass of the total of the copolymer (A) and other polymers (elastomers, rubbers, etc.) blended as necessary.

[0211] Moisture absorbent Examples of moisture absorbents include calcium oxide, silica gel, sodium sulfate, molecular sieves, zeolite, and white carbon.

[0212] When the composition of the present embodiment contains a moisture absorbent, the content of the moisture absorbent is preferably 0.5 to 15 parts by mass, more preferably 1.0 to 12 parts by mass, per 100 parts by mass in total of the copolymer (A) and other polymers (elastomers, rubbers, etc.) blended as necessary.

[0213] Other Polymers The composition of the present embodiment may further contain other polymers other than the copolymer (A). Examples of other polymers that require crosslinking include ethylene-α-olefin-non-conjugated polyene copolymers other than the copolymer (A), natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, chloroprene rubber, nitrile rubber, butyl rubber, acrylic rubber, silicone rubber, fluororubber, urethane rubber, and other rubbers. Examples of other polymers that do not require crosslinking include elastomers such as styrene-butadiene block copolymers (SBS), polystyrene-poly(ethylene-butylene)-polystyrene (SEBS), polystyrene-poly(ethylene-propylene)-polystyrene (SEPS), and other styrene-based thermoplastic elastomers (TPS), olefin-based thermoplastic elastomers (TPO), vinyl chloride-based elastomers (TPVC), ester-based thermoplastic elastomers (TPC), amide-based thermoplastic elastomers (TPA), urethane-based thermoplastic elastomers (TPU), and other thermoplastic elastomers (TPZ).

[0214] When the composition of the present embodiment contains another polymer, the content of the other polymer is preferably 100 parts by mass or less, more preferably 90 parts by mass or less, based on 100 parts by mass of the copolymer (A).

[0215] <Preparation of Composition> The composition of the present embodiment can be prepared by kneading the above-mentioned components at a desired temperature using a kneading machine such as a mixer, a kneader, or a roll.

[0216] The composition of this embodiment is prepared, for example, as follows. The copolymer (A), carbon black (B), short fiber (C), and other predetermined components are put into a kneader and kneaded and homogenized under predetermined heating conditions (for example, at 80 to 200°C for 3 to 30 minutes) (kneading A). In kneading A, a crosslinking agent or the like that crosslinks the copolymer (A) when heated to the heating temperature of kneading A is not added. The temperature of the mixture kneaded in kneading A is then lowered to below the crosslinking temperature of the peroxide-based crosslinking agent (D) (for example, 130°C or less), and the peroxide-based crosslinking agent (D) and crosslinking assistant agent (E) that were not added in kneading A are then added to the mixture, and further kneaded and homogenized under predetermined heating conditions (for example, at a roll temperature of 30 to 80°C for 1 to 30 minutes) (kneading B), to obtain the composition of this embodiment.

[0217] The composition of the present embodiment has a Mooney viscosity ML at 100° C. in the composition (mixture A) before the crosslinking agent is mixed. (1+4) However, it is usually from 10 to 250, preferably from 10 to 100, and more preferably from 10 to 70. A composition having a Mooney viscosity within the above range exhibits good post-treatment quality and has excellent rubber properties.

[0218] [Cross-linked molded products, power transmission belts] A crosslinked molded article can be obtained from the composition of this embodiment. The composition of this embodiment can be molded by a thermoforming method such as extrusion molding, injection molding, press molding, calendar molding, transfer molding, and foam molding. In this embodiment, the crosslinking temperature of the composition is usually 140° C. or higher, preferably 150 to 220° C., and more preferably 160 to 200° C. In addition, this crosslinking reaction can be carried out in air.

[0219] In this embodiment, the crosslinked molded article can be suitably used as a component of a power transmission belt. For example, the composition of this embodiment has high adhesive strength suitable for molding processability, and is excellent in belt processability. In addition, by using the composition of this embodiment, a component of a power transmission belt excellent in high rubber elasticity, abrasion resistance, heat resistance, cold resistance, and light weight can be manufactured.

[0220] One embodiment of the power transmission belt of the present invention (hereinafter also referred to as "the power transmission belt of this embodiment") has a crosslinked molded article formed from the composition of this embodiment. Examples of the transmission belt of the present embodiment include friction transmission belts such as V-belts and V-ribbed belts, and meshing transmission belts such as timing belts. Examples of the transmission belt include automobile transmission belts, motorcycle transmission belts, and general industrial machine transmission belts. Examples of the V-belt include wrapped belts and raw edge belts.

[0221] One embodiment of the transmission belt may have, for example, an adhesive rubber part in which a core wire is embedded, and may further have a bottom rubber part formed on the lower surface of the adhesive rubber part. The transmission belt may have an upper canvas formed on the adhesive rubber part and / or a lower canvas formed under the bottom rubber part, as necessary. The composition of this embodiment is preferably used to form, for example, the adhesive rubber part and / or the bottom rubber part. Specifically, a cross-linked molded part formed from the composition of this embodiment is preferably used as the adhesive rubber part and / or the bottom rubber part.

[0222] The core wire, which is a tensile member of the power transmission belt, extends in the longitudinal direction of the belt in the bonded rubber section. An example of the core wire is a polyester cord. The bonded rubber section surrounds the core wire and is bonded to the core wire. In one embodiment, for example, the composition of the present embodiment is disposed around the core wire and crosslinked to form the bonded rubber section bonded to the core wire. Examples of the canvas include canvas made of cotton, a blend of cotton and polyester, and a blend of cotton and polyamide. EXAMPLES

[0223] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" refers to "parts by mass".

[0224] <Composition of ethylene-α-olefin-non-conjugated polyene copolymer> The mass fraction (mass%) of each structural unit of the ethylene-α-olefin-non-conjugated polyene copolymer is: 13 The measured values ​​were obtained by C-NMR. The measured values ​​were obtained by using an ECX400P nuclear magnetic resonance apparatus (manufactured by JEOL Ltd.) at a measurement temperature of 120°C, a measurement solvent of orthodichlorobenzene / deuterated benzene = 4 / 1, and an accumulation number of 8000 times. 13 The C-NMR spectrum was obtained.

[0225] <Iodine value> The iodine value of ethylene-α-olefin-non-conjugated polyene copolymer was determined by titration as follows.

[0226] 0.5g of ethylene-α-olefin-non-conjugated polyene copolymer was dissolved in 60ml of carbon tetrachloride, a small amount of Wiss's reagent and 20% potassium iodide solution were added, and the solution was titrated with 0.1mol / L sodium thiosulfate solution. Near the end point, starch indicator was added and the solution was titrated while stirring well until the light purple color disappeared, and the amount of halogen consumed per 100g of sample was calculated as the number of grams of iodine.

[0227] <Intrinsic viscosity> The intrinsic viscosity [η] was measured using a fully automatic intrinsic viscometer manufactured by Rigo Co., Ltd. at a temperature of 135° C. and in decalin as a measurement solvent.

[0228] <Weight average molecular weight (Mw), number average molecular weight (Mn), molecular weight distribution (Mw / Mn)> The weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) are values ​​calculated in terms of polystyrene measured by gel permeation chromatography (GPC). The measuring device and conditions are as follows. The molecular weight was calculated based on a calibration curve prepared using commercially available monodisperse polystyrene and a conversion method.

[0229] Equipment: Gel permeation chromatograph Alliance GP2000 (Waters), Analysis equipment: Empower2 (Waters), Column: TSKgel GMH6-HT x 2 + TSKgel GMH6-HTL x 2 (7.5 mm I.D. x 30 cm, Tosoh Corporation), Column temperature: 140°C, Mobile phase: o-dichlorobenzene (containing 0.025% BHT), Detector: Differential refractometer (RI), Flow rate: 1.0mL / min, Injection volume: 400μL, Sampling time interval: 1s, Column calibration: monodisperse polystyrene (Tosoh Corporation), Molecular weight conversion: Old EPR conversion / calibration method that takes viscosity into account.

[0230] <Peak area> When the chart obtained by the above GPC measurement showed two or more peaks, the ratio (%) of the area of ​​the peak appearing on the side with the smallest molecular weight to the total peak area was calculated.

[0231] <Complex viscosity η * > The rheometer used was the Ares viscoelasticity measuring device (manufactured by Rheometric Scientific), and the complex viscosity η at a frequency of ω = 0.01 rad / s was measured under the conditions of 190°C and 1.0% strain. * ( ω =0.01) , complex viscosity η at frequency ω=0.1rad / s * ( ω =0.1) , complex viscosity η at frequency ω=10rad / s * ( ω =10) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (All units are Pa sec) were measured. * ( ω =0.1) and η * ( ω =100) The ratio of complex viscosity to *The P-value (η * ( ω =0.1) / η * ( ω =100) ) was calculated.

[0232] < Number of long chain branches (LCB) per 1000 carbon atoms 1000c )> The measurement was performed by the method described above. <Production of ethylene-α-olefin-non-conjugated polyene copolymer (A)> An example of the production of the ethylene-α-olefin-non-conjugated polyene copolymer (A) is shown below.

[0233] [Production Example 1] Using the continuous polymerization apparatus shown in Figure 1, ethylene-propylene-5-vinyl-2-norbornene (VNB) copolymer (A-1) was produced as follows.

[0234] A dehydrated and purified hexane solvent was continuously fed from tube 6 at 58.3 L / hr, triisobutylaluminum (TiBA) at 4.5 mmol / hr, (C6H5)3CB(C6F5)4 at 0.150 mmol / hr, and di(p-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride at 0.030 mmol / hr from tube 7 into a 300-liter polymerization reactor C. At the same time, ethylene was continuously fed from tubes 2, 3, 4, and 5 at 6.6 kg / hr, propylene at 9.3 kg / hr, hydrogen at 18 L / hr, and VNB at 340 g / hr, respectively, into the polymerization reactor C, and copolymerization was carried out under the conditions of a polymerization temperature of 87°C, a total pressure of 1.6 MPaG, and a residence time of 1.0 hour.

[0235] The ethylene-propylene-VNB copolymer solution produced in the polymerization reactor C was continuously discharged through the pipe 8 at a flow rate of 88.0 L / hr, heated to 170°C (pressure increased to 4.1 MPaG), and supplied to the phase separator D. At this time, ethanol, a polymerization inhibitor, was continuously introduced into the pipe 8 in an amount of 0.1 mol times the amount of TiBA in the liquid component extracted from the polymerization reactor C.

[0236] In phase separator D, the ethylene-propylene-vinyl alcohol copolymer solution was separated into a dense phase (lower phase) containing most of the ethylene-propylene-vinyl alcohol copolymer and a dilute phase (upper phase) containing a small amount of the polymer.

[0237] The separated thick phase was led to heat exchanger K via pipe 11 at a rate of 85.4 L / hr, and then led to hopper E, where the solvent was evaporated and separated, yielding ethylene-propylene-VNB copolymer at a rate of 7.8 kg / hr.

[0238] The physical properties of the obtained ethylene-propylene-VNB copolymer (A-1) were evaluated as described above. The results are shown in Table 1. The molecular weight distribution of the obtained copolymer (A-1) was bimodal, and the chart obtained by GPC measurement showed two or more peaks, and the area of ​​the peak appearing on the side of the smallest molecular weight was 5% of the total peak area.

[0239] [Production Example 2] An ethylene-propylene-VNB copolymer (A-2) was produced in the same manner as in Production Example 1, except that the molecular weight of the resulting copolymer was controlled by the amount of hydrogen fed. The results are shown in Table 1.

[0240] [Table 1]

[0241] [Example 1] Using a MIXTRON BB MIXER (manufactured by Kobe Steel, Ltd., BB-2 type, volume 1.7L, rotor 2WH), 57.5 parts of copolymer (A-1) and 50 parts of copolymer (A-2) were mixed with 5 parts of ZnO#1 as a crosslinking aid, 1 part of stearic acid as a processing aid, 1 part of Irganox 1010 as an antioxidant, 2 parts of Sandant MB as an antioxidant, 50 parts of Asahi#70 as carbon black, 7.5 parts of PW-380 as a softener, and 5 parts of Kevlar Dip Cut Fiber 3.5mm as short fibers in a blending amount, and then kneaded to obtain Blend 1.

[0242] The mixing conditions for compound 1 were: rotor speed 40 rpm, floating weight pressure 3 kg / cm 2 The kneading time was 5 minutes, and the kneading discharge temperature was 144°C. Mooney Viscosity ML of Formulation 1 (1+4) The viscosity was measured at 100°C using a Mooney viscometer (Shimadzu Corporation, Model SMV202) in accordance with JIS K6300 (1994).

[0243] Next, after confirming that the temperature of Compound 1 had reached 40°C, 6.3 parts of DCP-40C (dicumyl peroxide 40% by mass) as a crosslinking agent and 2 parts of SunEster EG were added to Compound 1 and kneaded using a 6-inch roll to obtain Compound 2.

[0244] The kneading conditions for preparing compound 2 were as follows: roll temperature: front roll / rear roll = 50°C / 50°C, roll peripheral speed: front roll / rear roll = 18 rpm / 15 rpm, roll gap: 3 mm, and kneading time: 8 minutes to obtain compound 2.

[0245] Compound 2 was pressed at 170° C. for 15 minutes using a press molding machine to produce a crosslinked sheet having a thickness of 2 mm or 1 mm. The crosslinked sheets thus obtained were subjected to the hardness test, tensile test, heat aging resistance test, and DIN friction test described below.

[0246] [Comparative Example 1] A compound and a crosslinked sheet were obtained in the same manner as in Example 1, except that a commercially available chloroprene rubber (DCR-40) was used instead of the ethylene-propylene-VNB copolymers (A-1) and (A-2) used in Example 1, and the types and amounts of each compounding ingredient were as shown in Table 3.

[0247] The materials used in the examples and comparative examples are shown in Table 2 below.

[0248] [Table 2]

[0249] [specific gravity] A test piece was prepared by cutting 1 g of Compound 1 (Mix A). The test piece was attached to an automatic specific gravity meter (Toyo Seiki Seisakusho: M-1 type) in an atmosphere of 25°C, and the specific gravity was measured from the difference in mass in air and in pure water.

[0250] [Hardness test (Duro-A)] The flat portions of the above crosslinked sheets having a thickness of 2 mm were overlapped to form a sheet having a thickness of 12 mm, and the hardness (Duro-A) was measured according to JIS K6253.

[0251] [Tensile test: modulus, tensile stress at break, tensile elongation at break] A 2 mm thick dumbbell test piece of type 3 described in JIS K6251 (1993) was prepared by punching out the above crosslinked sheet. Using this test piece, a tensile test was carried out according to the method specified in JIS K6251, section 3, at a measurement temperature of 25°C and a tensile speed of 500 mm / min, and the tensile stress at an elongation rate of 25% (25% modulus (M25)), tensile stress at break (TB), and tensile elongation at break (EB) were measured.

[0252] [Heat resistance test (heat aging resistance test)] The crosslinked sheet having a thickness of 2 mm was subjected to a heat aging test in which the sheet was held at 180° C. for 70 hours according to JIS K6257. The hardness, TB and EB of the sheet after the heat aging test were measured in the same manner as in the hardness test and tensile test.

[0253] AH (Duro-A) was calculated from the difference in hardness before and after the heat aging test, and the rate of change after the test from the value before the heat aging test was calculated as Ac(TB) and Ac(EB), respectively, from the TB and EB before and after the heat aging test.

[0254] [DIN friction test (DIN wear amount)] A disk-shaped test piece with a diameter of 16.0±0.2 mm and a thickness of 6 mm or more was prepared from the above crosslinked sheet with a thickness of 2 mm in accordance with JIS-K6264-2:2005. The test piece was subjected to a DIN abrasion test by rotating a drum with a diameter of 150.0±0.2 mm and a length of 500 mm at 40 revolutions per minute under a load of 1 kgf over an abrasion distance of 40.0±0.2 m, and the amount of abrasion (DIN abrasion amount: unit mm 3 ) was measured.

[0255] [Viscoelasticity measurement] A 1 cm wide test piece was cut from the above crosslinked sheet with a thickness of 1 mm using a punching blade, and tan δ was measured at room temperature, a frequency of 10 Hz, and a strain of 2% using an RSA viscoelasticity measuring system (manufactured by TA Instruments).

[0256] A low value of tan δ means less energy loss, which is thought to lead to an increase in the power transmission rate in the power transmission belt.

[0257] [Table 3] [Explanation of symbols]

[0258] 2~13 tubes C Polymerization reactor D phase separator E Hopper F Pump G Heat exchanger H heat exchanger I Heat exchanger J heat exchanger K heat exchanger

Claims

1. An ethylene / α-olefin / non-conjugated polyene copolymer (A) having a structural unit derived from ethylene (a1), a structural unit derived from an α-olefin (a2) having 3 to 20 carbon atoms, and a structural unit derived from a non-conjugated polyene (a3) ​​containing, in the molecule, two or more partial structures selected from the group consisting of the following formulae (I) and (II), in total, the non-conjugated polyene (a3) ​​containing 5-vinyl-2-norbornene (VNB) and satisfying the following requirements (i) to (vi): Carbon black (B); Short fibers (C); A peroxide-based crosslinking agent (D); A crosslinking coagent (E) having two or more ethylenic double bonds; Contains The short fibers (C) are composed only of aramid short fibers, The content of the aramid short fibers is 0.1 to 20 parts by mass based on 100 parts by mass of the copolymer (A), The composition for a transmission belt, wherein the crosslinking assistant (E) is a (meth)acrylic crosslinking assistant. (i) the molar ratio of the structural units derived from ethylene (a1) to the structural units derived from an α-olefin (a2) having 3 to 20 carbon atoms [(a1) / (a2)] is 55 / 45 to 78 / 22; (ii) the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​is 0.07% by mass to 10% by mass in 100% by mass of the copolymer (A); (iii) the weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​(mass fraction (mass %) of (a3)), and the molecular weight of the non-conjugated polyene (a3) ​​(molecular weight of (a3)) satisfy the following formula (1); 4.5≦Mw×mass fraction of (a3) / 100 / molecular weight of (a3)≦40 … (1) (iv) Complex viscosity η at frequency ω=0.1 rad / s obtained by linear viscoelastic measurements (190° C.) using a rheometer * (ω=0.1) (Pa sec) and the complex viscosity η at a frequency ω = 100 rad / s * (ω=100) (Pa sec) P(η * (ω=0.1) / * (ω=100) ), the intrinsic viscosity [η], and the mass fraction of the structural unit derived from the non-conjugated polyene (a3) ​​(mass fraction (mass%) of (a3)) satisfy the following formula (2): P / ([η] 2.9 ) ≦ mass fraction of (a3) ​​× 6 ... (2) (v) the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (molecular weight distribution; Mw / Mn) measured by gel permeation chromatography (GPC) is in the range of 4 to 30; (vi) the number average molecular weight (Mn) is 30,000 or less; 【Chemistry 1】

2. 2. The composition for a transmission belt according to claim 1, wherein the α-olefin (a2) having 3 to 20 carbon atoms is propylene.

3. Relative to 100 parts by mass of the copolymer (A), The content of the carbon black (B) is 0.1 to 200 parts by mass. The composition for a transmission belt according to claim 1 or 2.

4. A crosslinked molded article formed from the composition for a transmission belt according to any one of claims 1 to 3.

5. A power transmission belt comprising the crosslinked molded article according to claim 4.

Citation Information

Patent Citations

  • Short fiber reinforced elastomer composition for transmission belt and transmission belt

    JP2001310951A

  • Transmission belt

    JP2007009966A

  • Friction transmission belt

    JP2012215212A

  • Rubber composition for transmission belt

    JP2016044198A

  • Rubber composition for power transmission belt

    JP2017165926A