Spiroacridan compound, hole transport material containing said compound, and organic electronic device containing said compound in hole transport layer

Novel spiroacridan compounds address charge imbalance and stability issues in organic EL devices by enhancing charge recombination and energy transfer, resulting in high-efficiency, long-lasting, low-voltage operation.

JP7566504B2Active Publication Date: 2024-10-15KANTO CHEM CO INC
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
JP2020110333
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-27
Filing Date
2020-06-26
Publication Date
2024-10-15
Estimated Expiration
2040-06-26

AI Technical Summary

Technical Problem

Existing organic electroluminescent (EL) devices face challenges in achieving high luminous efficiency and extended lifetime due to imbalances in charge injection and transport, poor material stability, and inefficient energy transfer within the light-emitting layer.

Method used

Development of novel spiroacridan compounds with a rigid structure, represented by general formulas (1-1) to (1-3), which act as hole transport materials, enhancing charge recombination efficiency and stability by suppressing molecular stacking and energy transfer, thereby improving device performance.

Benefits of technology

The spiroacridan compounds exhibit high excitation energy, leading to improved photostability, electrical stability, and thermal stability, resulting in organic EL devices with higher efficiency and longer lifespan, capable of low-voltage operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566504000048
    Figure 0007566504000048
  • Figure 0007566504000001
    Figure 0007566504000001
  • Figure 0007566504000002
    Figure 0007566504000002
Patent Text Reader

Abstract

To provide a compound usable as a hole transport material excellent in hole injection and transport performance, electron blocking performance, optical stability, electrical stability, and thermal stability, to provide a hole transport material comprising the compound, and to provide an organic electronic device including an organic EL element or an organic photoelectric conversion element of which hole transport layer comprises the compound, in particular an organic electronic device including an organic EL element with long life and high light emission efficiency.SOLUTION: Provided is a compound represented by general formulae (1-1) to (1-3). (n, L, R and Ar1 to Ar5 are as defined in the specification.)SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to providing a novel compound, use of the compound as a hole transport material or a material for an organic electronic device, and providing an organic electronic device using the compound. [Background technology]

[0002] 2. Description of the Related Art Known organic electronic devices that convert electrical energy into light energy and vice versa include those that include an organic electroluminescence element (organic EL element) or an organic photoelectric conversion element.

[0003] Among these, organic EL elements have a structure in which a light-emitting material that emits light in response to an electric field is sandwiched between a cathode and an anode. In organic EL elements, holes and electrons injected from the electrodes are recombined in the light-emitting layer, causing the light-emitting material to emit light.

[0004] Organic EL elements are self-luminous, have a wide viewing angle, and are excellent in visibility. For this reason, organic EL elements are used as display elements for displays and the like. In addition, organic EL elements are thin solid-state elements that can be made lightweight and have excellent strength. For this reason, displays using organic EL elements are useful not only for stationary displays such as televisions, but also for mobile applications. Furthermore, display elements using organic EL elements can be easily resized and emit light over the entire surface, making them useful for lighting applications.

[0005] The challenges facing organic EL devices include improving their luminous efficiency (external quantum efficiency) and extending their lifespan. To address these challenges, various efforts have been made. For example, in addition to the electrodes and the light-emitting layer, organic EL elements often have a hole injection layer, a hole transport layer, an electron transport layer, and an electron injection layer. Usually, these layers are stacked in the order of an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a cathode. By providing these layers in addition to the electrodes and the light-emitting layer, the probability of holes and electrons recombining in the light-emitting layer can be increased, and the light-emitting efficiency of the organic EL element can be improved.

[0006] The light-emitting layer of an organic EL element is generally made by doping a fluorescent compound or a phosphorescent compound called a guest material into a charge-transporting compound called a host material. Holes and electrons injected from an electrode recombine in the light-emitting layer formed of the host material and the guest material, and the energy of the excited host material is transferred to the guest material, which is excited by the energy and released as light energy, resulting in efficient light emission.

[0007] In order to improve the recombination probability of holes and electrons, it is important to efficiently transfer both charges to the light-emitting layer, and therefore it is necessary to adjust the transport balance between holes and electrons. In order to adjust the balance between hole and electron transport, it is necessary to take into consideration many factors, such as the hole mobility of the hole injection material and the hole transport material, the electron mobility of the electron injection material and the electron transport material, the charge injection barrier at the layer interface, and the thickness of each film. However, the transportability of holes and electrons in the material itself differs depending on the material, and a charge injection barrier occurs at the interface between layers formed of different materials, so it is not easy to recombine holes and electrons in a well-balanced manner in the light-emitting layer. Examples of poor balance in charge injection and transport include a case where there are few holes or electrons, or a case where there are too many of either and they pass through without recombining. When the charge flows out to the opposite electrode, there is a method of providing a layer that blocks the charge to confine the charge in the light-emitting layer and increase the recombination efficiency. Furthermore, high light-emitting efficiency can be obtained by confining the excitation energy generated in the light-emitting layer. Usually, the role of confining the outflowing charge and excitation energy in the light-emitting layer is often played by the hole transport layer or electron transport layer, so the role of the hole transport material is very important.

[0008] The properties required for a hole transport material used to increase the recombination efficiency of an organic EL element are high hole transportability and low electron transportability, and it is important that the band gap, ionization potential (IP), and electron affinity (Ea) have appropriate values. The ionization potential of the hole transport material is preferably a value between the work function of the anode or the ionization potential of the hole injection material and the ionization potential of the light-emitting material, which can reduce the hole injection barrier to the light-emitting layer. The electron affinity of the hole transport material is preferably larger than the electron affinity of the light-emitting material, which can provide an electron blocking effect. Note that the HOMO level is sometimes used as a nearly synonymous term for the ionization potential (IP), which is one of the indices of charge injection characteristics, and the LUMO level is sometimes used as a nearly synonymous term for the electron affinity (Ea).

[0009] Regarding the life of an organic EL element, the light stability and electrical stability of the material are important (see, for example, Non-Patent Document 1 and Non-Patent Document 2). In the case of a material with low light stability, the material is deteriorated by the excitation energy in the light-emitting layer. In addition, if the excitation energy of the hole transport layer is smaller than that of the light-emitting layer, the excitation energy generated in the light-emitting layer moves to the hole transport layer, promoting the deterioration of the hole transport material and also leading to a decrease in the efficiency of the element, so it is desirable that the excitation energy of the hole transport layer is higher than that of the light-emitting layer. On the other hand, in the case of a material with low electrical stability, the material is deteriorated by the holes and electrons flowing through the element, causing a decrease in efficiency and a short life.

[0010] Heat resistance and amorphousness are also important for extending the life of elements. Materials with low heat resistance undergo thermal decomposition due to the heat generated when the element is in operation, causing the material to deteriorate. Materials with low amorphousness are prone to crystallization, accelerating the deterioration of the element. For this reason, materials used in elements are required to have high heat resistance and good amorphousness. The glass transition temperature (Tg) is used as a measure of amorphousness, and if the Tg of a material is low, it will crystallize and turn into a non-uniform film over a long period of time even at room temperature, so the higher the Tg of an organic EL material, the better. Considering the operating environment of the device, it is preferable for the Tg to be at least 135°C or higher.

[0011] A similar problem may arise in an organic photoelectric conversion element.

[0012] For example, Patent Document 1 reports compound (P) represented by the following formula as a hole transport material used in a hole transport layer. Compound (P) has a phenyl group as a substituent, which is different from the substituent of the methylene group of the acridan skeleton of the corresponding compound of the present invention, and is therefore considered to have low electrical stability and thermal stability. On the other hand, it is impossible to obtain a compound containing the spiroacridan skeleton of the present invention by the synthesis method described in Patent Document 1, and there is no clue to predict the excellent effect of the compound.

[0013] [ka]

[0014] Patent Document 2 also reports compound (Q) represented by the following formula as a hole transport material used in the hole transport layer. Compound (Q) has a methyl group as a substituent, which is different from the substituent of the methylene group of the acridan skeleton of the corresponding compound of the present invention, and is therefore considered to have low electrical stability and thermal stability. On the other hand, it is impossible to obtain a compound containing the spiroacridan skeleton of the present invention by the synthesis method described in Patent Document 2, and there is no clue to predict the excellent effects of the compound.

[0015] [ka]

[0016] Furthermore, Patent Document 3 reports a compound (R) represented by the following formula as a hole transport material used in a hole transport layer: It is impossible to obtain a compound containing a spiroacridan skeleton of the present invention by the synthesis method described in Patent Document 3, and there is no clue to predict the excellent effects of the compound.

[0017] [ka]

[0018] Furthermore, Patent Document 4 reports compound (S) represented by the following formula as a material having a spiroacridan skeleton of the present invention. Compound (S) is used in an emitting layer as a delayed fluorescent material, and therefore has a different application from the compound containing a spiroacridan skeleton of the present invention.

[0019] [ka] [Prior art documents] [Patent documents]

[0020] [Patent Document 1] Patent No. 6279647 [Patent Document 2] Patent No. 6193215 [Patent Document 3] European Patent No. 1840120 [Patent Document 4] International Publication No. 2018 / 207750 [Non-patent literature]

[0021] [Non-Patent Document 1] Adv. Mater., 24, 3212 (2012) [Non-Patent Document 2] Adv. Mater., 22, 2468 (2010) Summary of the Invention [Problem to be solved by the invention]

[0022] An object of the present invention is to provide a compound that can be used as a hole transport material having excellent hole injection or transport performance, electron blocking performance, light stability, electrical stability and thermal stability. Another object of the present invention is to provide a hole transport material containing the above-mentioned compound, and to provide an organic electronic device including an organic EL element or an organic photoelectric conversion element having a hole transport layer containing the above-mentioned compound, in particular, an organic electronic device including an organic EL element having a long life and high luminous efficiency. [Means for solving the problem]

[0023] As a result of extensive investigations, the inventors have succeeded in synthesizing novel compounds represented by the following general formulas (1-1) to (1-3), and have further found that the compounds are extremely useful as hole transport materials for organic EL elements or organic photoelectric conversion elements included in organic electronic devices, and in particular, can achieve high efficiency, long life, and low voltage operation of organic EL elements, thereby completing the present invention.

[0024] The inventors presume that the reason why the use of the compounds represented by the following general formulas (1-1) to (1-3) as a hole transport layer material can improve the efficiency and extend the life of an organic EL element or an organic photoelectric conversion element included in an organic electronic device is as follows. That is, the compounds represented by the following general formulas (1-1) to (1-3) have a bulky and rigid structure due to the inclusion of a spiroacridan skeleton defined by the general formula, and stacking between molecules is suppressed. As a result, it is presumed that the compounds exhibit high excitation energy, which suppresses energy transfer from the light-emitting layer and increases the efficiency of the device. In addition, it is presumed that the increased rigidity of the compounds increases the electrical stability, light stability, and thermal stability, which contributes to the longer life of the organic EL element or organic photoelectric conversion element included in the organic electronic device.

[0025] The gist of the present invention is as follows. [1] General formula (1-1)

[0026] [ka]

[0027] During the ceremony, n is 0 or 1; L represents a single bond, a phenylene group, a naphthylene group, or a divalent aromatic heterocyclic group formed from any one of a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, and a triazine ring, and the phenylene group, the naphthylene group, or the divalent aromatic heterocyclic group may further have a substituent; Ar 1 ~Ar5 each independently represents an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, or a fused polycyclic aromatic group which may have a substituent, The compound represented by the formula (I) is a compound represented by the formula (I) except for the compound (T) below. [ka]

[0028] [2] General formula (1-2) or (1-3)

[0029] [ka]

[0030] During the ceremony, n is 0 or 1; L represents a single bond, a phenylene group, a naphthylene group, or a divalent aromatic heterocyclic group formed from any one of a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, and a triazine ring, and the phenylene group, the naphthylene group, or the divalent aromatic heterocyclic group may further have a substituent; Ar 1 ~Ar 5 each independently represents an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or an optionally substituted fused polycyclic aromatic group; R is hydrogen, deuterium, a halogen group, a linear, branched or cyclic alkyl group which may have a substituent, a linear, branched or cyclic alkoxy group which may have a substituent, or an aromatic hydrocarbon group which may have a substituent; A compound represented by the formula:

[0031] [3] The compound according to [1] or [2], wherein L is a single bond, a phenylene group, or a naphthylene group. [4] Ar 4 , Ar 5are each independently a phenylene group, a biphenylene group, or a naphthylene group. [5] The compound according to any one of [2] to [4], wherein R is hydrogen or a phenyl group. [6] A hole transport material comprising the compound according to any one of [1] to [5].

[0032] [7] An organic electronic device including an organic electroluminescence element or an organic photoelectric conversion element having a hole transport layer between a cathode and an anode, The organic electronic device, wherein the hole transport layer contains the compound according to any one of [1] to [5] above.

[0033] [8] The organic electronic device according to [7] above, comprising an organic electroluminescence element having a light-emitting layer between a hole transport layer and a cathode. [9] The light-emitting layer includes a host material and a guest material made of a light-emitting material, The organic electronic device according to [8] above, wherein the host material is an electron transporting material or a positive charge transporting material having hole transporting and electron transporting properties. Effect of the Invention

[0034] The compound of the present invention can be used as a hole transporting material that can provide a hole transporting layer that is excellent in light stability, electrical stability, and thermal stability. In particular, the organic EL element of the present invention, an organic electronic device including an organic EL element having a hole transport layer containing the compound of the present invention, has a long life, high luminous efficiency, and can be driven at a low voltage. [Brief description of the drawings]

[0035] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating an example of an organic EL element included in the organic electronic device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] The present invention will now be described in further detail. The present invention relates to a compound represented by the general formula (1-1)

[0037] [ka]

[0038] During the ceremony, n is 0 or 1; L represents a single bond, a phenylene group, a naphthylene group, or a divalent aromatic heterocyclic group formed from any one of a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, and a triazine ring, and the phenylene group, the naphthylene group, or the divalent aromatic heterocyclic group may further have a substituent; Ar 1 ~Ar 5 each independently represents an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, or a fused polycyclic aromatic group which may have a substituent, The present invention relates to a compound represented by the formula: However, the compounds represented by general formula (1-1) exclude the following compound (T). [ka]

[0039] The present invention also relates to a compound represented by the general formula (1-2) or (1-3):

[0040] [ka]

[0041] During the ceremony, n is 0 or 1; L represents a single bond, a phenylene group, a naphthylene group, or a divalent aromatic heterocyclic group formed from any one of a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, and a triazine ring, and the phenylene group, the naphthylene group, or the divalent aromatic heterocyclic group may further have a substituent; Ar 1 ~Ar 5 each independently represents an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or an optionally substituted fused polycyclic aromatic group; R is hydrogen, deuterium, a halogen group, a linear, branched or cyclic alkyl group which may have a substituent, a linear, branched or cyclic alkoxy group which may have a substituent, or an aromatic hydrocarbon group which may have a substituent; The present invention relates to a compound represented by the formula:

[0042] In the general formulas (1-1) to (1-3), L is more preferably a single bond, a phenylene group, or a naphthylene group. In the general formulas (1-1) to (1-3), n is 0 or 1, and is preferably 1 when taking into consideration the electrical stability, thermal stability, film-formability, and ease of synthesis and purification of the compounds represented by the general formulas (1-1) to (1-3) as a whole.

[0043] Ar in general formulas (1-1) to (1-3) 1 ~Ar 3Examples of the aromatic hydrocarbon group, aromatic heterocyclic group, and condensed polycyclic aromatic group in the above formula (I) or the aromatic hydrocarbon group in R include a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, anthracenyl group, a phenanthrenyl group, a fluorenyl group, an indenyl group, a pyrenyl group, a perylenyl group, a fluoranthenyl group, a triphenylenyl group, a pyridyl group, a pyrimidyl group, a triazinyl group, a furyl group, a pyrrolyl group, a thienyl group, a quinolyl group, an isoquinolyl group, a benzofuranyl group, a benzothienyl group, an indolyl group, a carbazolyl group, a benzoxazolyl group, a benzothiazolyl group, a quinoxalinyl group, a benzimidazolyl group, a pyrazolyl group, a dibenzofuranyl group, a dibenzothienyl group, a naphthyldinyl group, a phenanthrolinyl group, an acridinyl group, and a carbolinyl group. Ar 1 ~Ar 3 As the aromatic hydrocarbon group, aromatic heterocyclic group and condensed polycyclic aromatic group in the above, the total number of carbon atoms and hetero atoms forming the ring is preferably 6 to 25, more preferably 6 to 20, and even more preferably 6 to 18.

[0044] Ar in general formulas (1-1) to (1-3) 1 ~Ar 3Examples of the substituents which the aromatic hydrocarbon group, aromatic heterocyclic group and condensed polycyclic aromatic group in the formula (I) may have, the substituents which the aromatic hydrocarbon group in R may have, or the substituents which L may have include, for example, a deuterium atom; a cyano group; a nitro group; a halogen group; a straight-chain or branched alkyl group such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, or a tert-butyl group; an alkyloxy group such as a methyloxy group, an ethyloxy group, or a propyloxy group; an alkenyl group such as a vinyl group or an allyl group; an aryloxy group such as a phenyloxy group or a phenyltrioxy group; an arylalkyloxy group such as a benzyloxy group; a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, an anthracenyl group, a phenanthrenyl group, aromatic hydrocarbon groups or condensed polycyclic aromatic groups such as a fluorenyl group, an indenyl group, a pyrenyl group, a perylenyl group, a fluoranthenyl group, or a triphenylenyl group; aromatic heterocyclic groups or condensed polycyclic aromatic groups such as a pyridyl group, a pyrimidyl group, a triazinyl group, a furyl group, a pyrrolyl group, a thienyl group, a quinolyl group, an isoquinolyl group, a benzofuranyl group, a benzothienyl group, an indolyl group, a carbazolyl group, a benzoxazolyl group, a benzothiazolyl group, a quinoxalinyl group, a benzimidazolyl group, a pyrazolyl group, a dibenzofuranyl group, a dibenzothienyl group, a naphthyldinyl group, a phenanthrolinyl group, an acridinyl group, or a carbolinyl group; arylvinyl groups such as a styryl group or a naphthylvinyl group; and acyl groups such as an acetyl group. Two or more of the above-mentioned substituents may be present, and when two or more of the substituents are present, they may be different from each other.

[0045] Ar in general formulas (1-1) to (1-3) 1 ~Ar 3In terms of the substituents which the aromatic hydrocarbon group, aromatic heterocyclic group and condensed polycyclic aromatic group in the above formula may have, taking into consideration electrical stability, thermal stability, film-forming properties, ease of synthesis and purification, etc., among the above examples, preferred are linear alkyl groups having 1 to 10 carbon atoms, or phenyl groups, biphenyl groups, terphenyl groups or naphthyl groups which may be substituted with one or more linear alkyl groups having 1 to 5 carbon atoms, more preferred are methyl groups, ethyl groups, propyl groups or butyl groups, or phenyl groups or biphenyl groups which may be substituted with one or more linear alkyl groups having 1 to 3 carbon atoms, and most preferred are methyl groups or phenyl groups.

[0046] Ar in general formulas (1-1) to (1-3) 3 is preferably a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a carbazolyl group, a dibenzofuranyl group, or a dibenzothienyl group which may be bonded to L at any position and which may have a substituent, and is particularly preferably a naphthyl group, a carbazolyl group, or a dibenzofuranyl group which may be bonded to L at any position and which may have a substituent.

[0047] Ar in general formulas (1-1) to (1-3) 4 , Ar 5 Examples of the aromatic hydrocarbon group, aromatic heterocyclic group and condensed polycyclic aromatic group in the above formula (I) include a phenylene group, a biphenylene group, a terphenylene group, a naphthylene group, a fluorenylene group, a triphenylenyl group, a benzofuranylene group, a benzothienylene group, a carbazolylene group, a dibenzofuranyl group and a dibenzothienyl group. Ar 4 , Ar 5 As the aromatic hydrocarbon group, aromatic heterocyclic group and condensed polycyclic aromatic group in the above, those having a total of 6 to 18 carbon and hetero atoms forming the ring are preferred, and those having 6 to 12 are more preferred.

[0048] Ar in general formula (1-1) 4 and Ar 5 The curved line connecting Ar and Ar represents a single bond which may be bonded at any position. 4or Ar 5 is an aromatic hydrocarbon group, an aromatic heterocyclic group, or a condensed polycyclic aromatic group containing two or more rings, the two or more ring aromatic hydrocarbon group, the aromatic heterocyclic group, or the condensed polycyclic aromatic group is bound to Ar 4 or Ar 5 and the other may be bonded to any one of the two or more rings. In addition, in the general formulas (1-2) and (1-3), Ar 4 and Ar 5 forms a condensed ring via a bond represented by a solid line together with a five- or six-membered spiro ring that shares the solid line.

[0049] Ar in general formulas (1-1) to (1-3) 4 , Ar 5 Examples of the substituents which the aromatic hydrocarbon group, aromatic heterocyclic group and condensed polycyclic aromatic group in the formula (I) may have include a deuterium atom; a cyano group; a nitro group; a halogen group; a straight-chain or branched alkyl group such as a methyl group, an ethyl group, a propyl group, or an isopropyl group; an alkyloxy group such as a methyloxy group or an ethyloxy group; an alkenyl group such as a vinyl group or an allyl group; an aryloxy group such as a phenyloxy group or a phenyltrioxy group which may have a substituent; an arylalkyloxy group such as a benzyloxy group which may have a substituent; Examples of the aromatic hydrocarbon group include an aromatic hydrocarbon group or a condensed polycyclic aromatic group, each of which may have a substituent, such as a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a fluorenyl group, or a triphenylenyl group; an aromatic heterocyclic group or a condensed polycyclic aromatic group, each of which may have a substituent, such as a benzofuranyl group, a benzothienyl group, an indolyl group, a carbazolyl group, a dibenzofuranyl group, a dibenzothienyl group, a naphthyldinyl group, or a phenanthrolinyl group; an aryl vinyl group, each of which may have a substituent, such as a styryl group, a naphthylvinyl group; and an acyl group, such as an acetyl group. Two or more of the above-mentioned substituents may be present, and when two or more of the substituents are present, they may be different from each other.

[0050] Ar in general formulas (1-1) to (1-3) 4 , Ar5 In terms of the substituents which the aromatic hydrocarbon group, aromatic heterocyclic group and condensed polycyclic aromatic group in the above formula may have, taking into consideration electrical stability, thermal stability, film-forming properties, ease of synthesis and purification, etc., among the above examples, preferred are linear alkyl groups having 1 to 10 carbon atoms, or phenyl groups, biphenyl groups, terphenyl groups or naphthyl groups which may be substituted with one or more linear alkyl groups having 1 to 5 carbon atoms, more preferred are methyl groups, ethyl groups, propyl groups or butyl groups, or phenyl groups or biphenyl groups which may be substituted with one or more linear alkyl groups having 1 to 3 carbon atoms, and most preferred are methyl groups or phenyl groups.

[0051] Examples of the linear alkyl group for R in general formula (1-3) include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, and an octadecyl group. Examples of the branched alkyl group for R in general formula (1-3) include a 1-methylethyl group, a 1-methylpropyl group, a 1-ethylpropyl group, a 1-n-propylpropyl group, a 1-methylbutyl group, a 1-ethylbutyl group, a 1-propylbutyl group, a 1-n-butylbutyl group, a 1-methylpentyl group, a 1-ethylpentyl group, a 1-n-propylpentyl group, a 1-n-pentylpentyl group, a 1-methylhexyl group, a 1-ethylhexyl group, a 1-n-propylhexyl group, a 1-n-butylhexyl group, a 1-n-pentylhexyl group, a 1-n-hexylhexyl group, a 1-methylheptyl group, a 1-ethylheptyl group, a 1-n-propylheptyl group, a 1-n-butylheptyl group, and a 1-n-pentylheptyl group.

[0052] Examples of the cyclic alkyl group for R in general formula (1-3) include cycloalkyl groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group, and polycyclic alkyl groups such as a bicycloalkyl group and a tricycloalkyl group. Examples of the linear, branched, or cyclic alkoxy group for R in the general formula (1-3) include the above-mentioned linear, branched, or cyclic alkoxy groups in which an oxygen atom is located at the 1-position of the alkyl group. The linear, branched or cyclic alkyl or alkoxy group preferably has 1 to 25 carbon atoms, more preferably has 1 to 15 carbon atoms, and further preferably has 1 to 8 carbon atoms, from the viewpoints of glass transition temperature, steric hindrance, etc.

[0053] Examples of the substituent that the linear, branched, or cyclic alkyl group or the linear, branched, or cyclic alkoxy group in R in the general formula (1-3) may have include an alkoxy group and a halogen group. Two or more of the above-mentioned substituents may be present, and when two or more of the substituents are present, they may be different from each other.

[0054] Taking into consideration the electrical stability, thermal stability, film-forming properties, and ease of synthesis and purification of the compound represented by general formula (1-3), R is most preferably, independently, hydrogen or a phenyl group.

[0055] The methylene portion of the acridan skeleton of the general formulae (1-1) to (1-3) is substituted with two specific (hetero)aryl groups, and the (hetero)aryl groups form a ring via a single bond, and the benzene ring of the acridan skeleton is Ar 2 By substituting with, the compound has a bulky and rigid molecular structure, and stacking between molecules is suppressed. As a result, the compound exhibits high excitation energy, and energy transfer from the light-emitting layer to the hole transport layer containing the compound is suppressed, which is presumably why electronic devices including organic electroluminescence elements are more efficient. In addition, the methylene portion of the acridan skeleton of the general formulae (1-1) to (1-3) is substituted with two specific (hetero)aryl groups, and the (hetero)aryl groups form a ring via a single bond, and the benzene ring of the acridan skeleton is Ar 2 By the substitution with, the rigidity of the compound is increased, and therefore the electrical stability, photostability and thermal stability are increased, and it is presumed that this also contributes to the extension of the life of an organic electronic device including an organic EL element or an organic photoelectric conversion element containing the compound in a hole transport layer. Furthermore, the methylene portion of the acridan skeleton of the general formulae (1-1) to (1-3) is substituted with two specific (hetero)aryl groups, the (hetero)aryl groups form a ring via a single bond, and the benzene ring of the acridan skeleton is Ar 2 By substituting with, attack of nucleophilic compounds or electrophilic compounds on the N atom is sterically suppressed, and therefore, it is presumed that the electrical stability, photostability and thermal stability are increased, and that this also contributes to the extension of the life of an organic electronic device including an organic EL element or an organic photoelectric conversion element containing the compound in a hole transport layer. The high excitation energy exhibited by the compounds represented by the general formulas (1-1) to (1-3) is particularly advantageous for use in electronic devices that include blue-emitting organic EL elements.

[0056] Specific examples of the compounds represented by the general formulas (1-1) to (1-3) are shown below, but the invention is not limited to these.

[0057] [ka]

[0058] [ka]

[0059] [ka]

[0060] [ka]

[0061] [ka]

[0062] [ka]

[0063] [ka]

[0064] Among the compounds shown as the specific examples above, particularly preferred examples of the compound from the viewpoints of charge injection characteristics, charge transport characteristics, electrical stability, and thermal stability include compounds (A) to (I) represented by the following chemical formulas.

[0065] [ka]

[0066] [ka]

[0067] [ka]

[0068] [ka]

[0069] [ka]

[0070] [ka]

[0071] [ka]

[0072] [ka]

[0073] [ka]

[0074] The compounds represented by the general formulas (1-1) to (1-3) have the above-mentioned properties and can be used as materials for organic EL elements or organic photoelectric conversion elements included in organic electronic devices, and can be particularly suitably used in the hole transport layer of an organic EL element, preferably the hole transport layer of a blue-emitting organic EL element. The compounds can particularly improve the efficiency and extend the life of the organic EL elements included in the organic electronic devices. The present invention also relates to a hole transport material containing the compound represented by any one of the general formulas (1-1) to (1-3).

[0075] The purity of the compounds represented by the general formulas (1-1) to (1-3) can be measured by high performance liquid chromatography (HPLC). High performance liquid chromatography is a method for measuring the purity of a sample by applying pressure to a mobile phase containing a sample, passing a solvent through the mobile phase at a high flow rate, separating the sample (mixture) in a column, and detecting the separated sample with a detector.

[0076] The molecular weights of the compounds represented by the general formulae (1-1) to (1-3) can be measured by mass spectrometry (MS). Mass spectrometry is performed by applying a high voltage in a vacuum to a sample introduced from a sample introduction section to ionize the sample, separating the ions according to their mass-to-charge ratio, and detecting them in a detection section. The sample introduction section can be directly connected to gas chromatography (GC / MS), high performance liquid chromatography (LC / MS), or capillary electrophoresis (CE / MS), and can measure the molecular weight as well as the purity. Note that the direct injection method (DI / MS), which directly ionizes the sample, may also be used. Ion sources employ a variety of ionization methods, including electron ionization (EI), fast atom bombardment (FAB), electrospray ionization (ESI), and inductively coupled plasma (ICP).

[0077] Nuclear magnetic resonance spectroscopy (NMR) can be used to identify the compounds represented by the general formulas (1-1) to (1-3). In NMR measurements, chemical shifts and coupling information can be obtained from the atomic bonding state, and therefore a spectrum specific to the compound can be obtained, allowing the compound to be identified. Measurements are performed by dissolving a small amount of sample in various heavy solvents. The thermal stability of the compounds represented by the general formulas (1-1) to (1-3) can be evaluated by differential scanning calorimetry (DSC). DSC measurement is performed by detecting the difference in heat quantity between a sample and a standard sample when a thermal change such as a phase transition or melting occurs in the sample. DSC measurement can reveal the melting point and glass transition temperature of the compound.

[0078] By measuring the ultraviolet-visible absorption spectrum (UV / VIS), fluorescence spectrum (PL), and phosphorescence spectrum of the compounds represented by the general formulas (1-1) to (1-3), it is possible to know not only the UV absorption wavelength, fluorescence wavelength, and phosphorescence wavelength specific to the compound, but also information such as the band gap, fluorescence quantum yield, and triplet energy of the compound. The HOMO and LUMO levels of the compounds represented by the general formulas (1-1) to (1-3) can be measured by cyclic voltammetry (CV). In addition, ionization potential (IP) is also used as an index similar to the HOMO level. In addition, a method is also used in which the optical band gap is determined from the UV absorption wavelength, and the LUMO level (or Ea) is calculated from the HOMO level (or IP).

[0079] One embodiment of the organic electronic device of the present invention includes an organic EL element including a light-emitting layer and a hole transport layer disposed on the anode side of the light-emitting layer between a cathode and an anode, the hole transport layer including a compound represented by any one of general formulas (1-1) to (1-3), and preferably includes a blue-emitting organic EL element. Fig. 1 is a schematic cross-sectional view for explaining an example of an organic EL element included in the organic electronic device of the present invention. The organic EL element 1 shown in Fig. 1 has a laminated structure in which a first electrode 9 (anode), a hole injection layer 8, a hole transport layer 7, a light emitting layer 6, an electron transport layer 5, an electron injection layer 4, and a second electrode 3 (cathode) are formed in this order on a substrate 2. The organic EL element included in the organic electronic device of the present invention may have a hole transport layer in which one or more layers are laminated. Similarly, other layers (e.g., a light-emitting layer and an electron transport layer) of the organic EL element of the present invention may also be in the form of one or more layers laminated.

[0080] The organic EL element 1 shown in FIG. 1 is formed on a substrate 2, and all of the laminated structures constituting the organic EL element are made of organic compounds. The organic EL element 1 shown in Fig. 1 may be a hybrid organic-inorganic electroluminescent element (HOILED element) in which a layer made of an inorganic compound is included in the laminated structure constituting the organic EL element 1 formed on the substrate 2. In this case, for example, the organic EL element 1 shown in Fig. 1 may be provided with an electron injection layer 4 made of an inorganic oxide and a hole injection layer 8 made of an inorganic oxide as layers made of inorganic compounds. Since inorganic compounds are more stable than organic compounds, the HOILED element is more resistant to oxygen and water than an organic EL element that does not include a layer made of an inorganic compound, and is therefore preferable.

[0081] 1 will be described taking as an example a case where an electron injection layer 4 and a hole injection layer 8 are provided, but, for example, the electron injection layer 4 and / or the hole injection layer 8 may be omitted. In addition, in the organic EL element 1 shown in FIG 1, an electron injection layer made of an inorganic compound may be provided instead of the electron injection layer 4 made of an organic compound, and a hole injection layer made of an inorganic compound may be provided instead of the hole injection layer 8 made of an organic compound.

[0082] The organic EL element 1 shown in FIG. 1 may be of a top emission type in which light is extracted to the side opposite to the substrate 2 side, or of a bottom emission type in which light is extracted to the substrate 2 side. The organic EL element 1 shown in FIG. 1 has a forward structure in which a first electrode 9 functioning as an anode is disposed between the substrate 2 and the light-emitting layer 6.

[0083] Materials for the substrate 2 include resin materials such as polyethylene terephthalate, polyethylene naphthalate, polypropylene, cycloolefin polymer, polyamide, polyethersulfone, polymethyl methacrylate, polycarbonate, and polyarylate, and glass materials such as quartz glass and soda glass, and one or more of these can be used.

[0084] When the organic EL element 1 is of a bottom emission type, the material of the substrate 2 is transparent. When the organic EL element 1 is of a top emission type, not only transparent but also opaque materials can be used for the substrate 2. Examples of opaque substrates include substrates made of ceramic materials such as alumina, substrates having an oxide film (insulating film) formed on the surface of a metal substrate such as stainless steel, and substrates made of resin materials.

[0085] The first electrode 9 in the organic EL element 1 shown in Fig. 1 functions as an anode. Examples of materials for the first electrode 9 include oxides such as ITO (indium tin oxide), IZO (indium zinc oxide), FTO (fluorine tin oxide), In3O3, SnO2, Sb-containing SnO2, and Al-containing ZnO. Among these, it is preferable to use ITO, IZO, or FTO as the material for the first electrode 9.

[0086] The material used for the hole injection layer 8 is selected from the viewpoints of the relationship between the work function of the anode and the IP of the hole transport layer, charge transport properties, etc. Examples of suitable materials include poly(3,4-ethylenedioxythiophene):poly(styrenesulfonate) (abbreviation: PEDOT:PSS), phthalocyanine compounds such as copper phthalocyanine (abbreviation: CuPc), molybdenum oxide (MoO x Acceptor heterocyclic compounds such as vanadium oxide (VO), 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HAT-CN) can be used. As long as the compound has the appropriate IP and charge transport properties, various organic and inorganic compounds, regardless of whether they are low molecular weight or high molecular weight, can be selected. In addition, two or more of these materials can be used in combination.

[0087] The hole transport layer 7 contains a compound represented by any one of the general formulae (1-1) to (1-3). The compound has a 2-substituted fluorene skeleton defined by the general formula, and thus has appropriate HOMO and LUMO levels, and is excellent in light stability, electrical stability, and thermal stability. Therefore, the charge recombination efficiency in the light-emitting layer can be increased, and an organic EL element with higher light-emitting efficiency and longer life can be realized.

[0088] The compounds represented by the general formulas (1-1) to (1-3) can be used alone as hole transport materials, but can also be used in combination with one or more existing hole transport materials. Examples of existing hole transport materials include aromatic amine compounds such as N,N-dibiphenyl-N'-terphenyl-N'-phenylbenzidine (abbreviation: HT1), N,N'-diphenyl-N,N'-di(α-naphthyl)benzidine (abbreviation: NPD), N,N'-diphenyl-N,N'-di(m-tolyl)benzidine (abbreviation: TPD), and 1,1-bis[4-[N,N-di(p-tolyl)amino]phenyl]cyclohexane (abbreviation: TAPC), and carbazole derivatives such as 4,4',4''-tri-9-carbazolyltriphenylamine (abbreviation: TCTA) and 1,3-bis(carbazol-9-yl)benzene (abbreviation: mCP).

[0089] A fluorescent material or a phosphorescent material can be used for the light-emitting layer 6. The light-emitting material can also be used by incorporating a light-emitting material (guest material) into a host material that performs charge transport and charge recombination. The host material can be a material having both hole transporting and electron transporting properties. In addition, since the hole transporting material of the present invention is also excellent in electron blocking performance, a material having electron transporting properties can also be used as the host material.

[0090] As the host material, for example, a metal complex such as an aluminum complex or a beryllium complex, an anthracene derivative, an oxadiazole derivative, a benzimidazole derivative, or a phenanthrene derivative can be used.

[0091] The luminescent material is not particularly limited, but examples of the fluorescent material include quinacridone, coumarin, rubrene, perylene and its derivatives, benzopyran derivatives, rhodamine derivatives, aminostyryl derivatives, pyrene derivatives, aromatic amine derivatives, and tetracene derivatives. Examples of the phosphorescent material include metal complexes of iridium and platinum. Examples of the green luminescent material include Ir(ppy)3, blue luminescent material include FIrpic, and red luminescent material include (Btp)2Ir(acac).

[0092] Examples of materials that can be used for the electron transport layer 5 include metal complexes of quinolinol derivatives such as Alq3 and BAlq, anthracene derivatives, pyridine derivatives, pyrimidine derivatives, benzimidazole derivatives, quinoxaline derivatives, phenanthroline derivatives, triazine derivatives, carbazole derivatives, and triazole derivatives. When an electron transport layer containing a material with an appropriate LUMO level is provided between the light-emitting layer and the cathode or the electron injection layer, the electron injection barrier from the cathode or the electron injection layer to the electron transport layer can be alleviated, and further, the electron injection barrier from the electron transport layer to the light-emitting layer can be alleviated. In addition, when the material has an appropriate HOMO level, it can prevent holes from flowing out to the counter electrode without recombining in the light-emitting layer, confine holes in the light-emitting layer, and increase the recombination efficiency in the light-emitting layer.

[0093] The material used for the electron injection layer 4 is selected from the viewpoints of the work function of the cathode and the LUMO level of the electron transport layer. When no electron transport layer is provided, the material is selected in consideration of the LUMO level of the light emitting material or the host material described below. The electron injection material may be an organic compound or an inorganic compound. When the electron injection layer is made of an inorganic compound, for example, in addition to an alkali metal or an alkaline earth metal, lithium fluoride, sodium fluoride, potassium fluoride, cesium fluoride, or cesium carbonate can be used.

[0094] The cathode of an organic EL element plays a role in injecting electrons into the electron injection layer or electron transport layer. For the cathode, various metal materials with relatively small work functions, various alloys, and other materials that act as cathodes are used. Examples include aluminum, silver, magnesium, calcium, gold, indium tin oxide (ITO), indium zinc oxide (IZO), magnesium indium alloy (MgIn), and silver alloy. When a bottom emission type is adopted, the cathode can be an opaque electrode made of metal, or a reflective electrode. When the top emission method is adopted, a transparent electrode such as ITO or IZO can be used for the cathode. Here, ITO has a large work function, which makes it difficult to inject electrons. In addition, sputtering or ion beam deposition is used to form an ITO film, but this may damage the electron transport layer during film formation. Therefore, in order to improve electron injection and reduce damage to the electron transport layer during film formation, a magnesium layer or copper phthalocyanine layer can be provided between the electron transport layer and ITO.

[0095] The organic photoelectric conversion element included in the organic electronic device of the present invention can also be produced in a similar manner to the organic EL element described above. EXAMPLES

[0096] The present invention will be described in more detail below with reference to examples, which are intended to illustrate specific embodiments of the present invention and are not intended to limit the present invention.

[0097] [Synthesis of compounds] Example 1 Compound (A) was synthesized according to the synthetic route shown below.

[0098] [ka]

[0099] Compound (a-1) was synthesized by the method shown below. 2-Bromotriphenylamine (5.31 g, 16.4 mmol) and tetrahydrofuran (328 mL) were placed in a 500 mL four-neck flask equipped with a stirrer and purged with argon, and the flask was cooled to -78°C while stirring. n-Butyllithium (1.6 M hexane solution, 12.5 mL, 19.7 mmol) was added dropwise thereto. After stirring for 1 hour, fluorenone (4.43 g, 24.6 mmol) was added and stirred for another 1 hour. Distilled water (50 mL) was added in small portions to stop the reaction. The contents were transferred to a separatory funnel, ethyl acetate was added to separate the organic and aqueous phases, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was purified by silica gel column chromatography (developing solvent: hexane / dichloromethane=3 / 1) to obtain the target compound (a-1) (yield: 6.21 g, 89%).

[0100] Compound (a-2) was synthesized by the method shown below. Compound (a-1) (6.21 g, 14.6 mmol), dichloromethane (292 mL), and trifluoromethanesulfonic acid (0.50 mL, 5.65 mmol) were placed in a 500 mL single-neck flask equipped with a stirrer and purged with argon, and the contents were stirred at room temperature for 30 minutes. Then, saturated aqueous sodium bicarbonate solution (30 mL) was added little by little to stop the reaction. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated. The aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was purified by washing with methanol to obtain the desired compound (a-2) (yield 5.41 g, 91%).

[0101] Compound (a-3) was synthesized by the method shown below. Compound (a-2) (2.00 g, 4.91 mmol) and dichloromethane (98 mL) were placed in a 300 mL Schlenk flask equipped with a stirrer and purged with argon, and bromine (0.78 mL, 15.2 mmol) was added dropwise thereto. The mixture was stirred at room temperature for 3 hours. The reaction vessel was then cooled to 0°C, and saturated aqueous sodium thiosulfate solution (30 mL) was added thereto little by little to stop the reaction. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was purified by washing with methanol to obtain the desired compound (a-3) (yield 2.96 g, 94%).

[0102] Compound (A) was synthesized by the method shown below. In a 300 mL Schlenk flask equipped with a stirrer and purged with argon, compound (a-3) (2.96 g, 4.60 mmol), 1-naphthaleneboronic acid (2.45 g, 14.2 mmol), potassium carbonate (2.54 g, 18.4 mmol), toluene (83 mL), water (9.2 mL), and tetrakistriphenylphosphinepalladium(0) (212 mg, 0.184 mmol) were placed and sealed, followed by stirring at 100°C for 2 hours. The reaction vessel was then allowed to cool to approximately room temperature. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: hexane / ethyl acetate = 30 / 1) and then washed with hexane to obtain the desired compound (A) (yield: 928 mg, 26%). MS: m / z = 785

[0103] Example 2 Compound (B) was synthesized according to the synthetic route shown below.

[0104] [ka]

[0105] Compound (B) was synthesized by the method shown below. In a 300 mL Schlenk flask equipped with a stirrer and purged with argon, compound (a-3) (3.21 g, 4.99 mmol), 2-naphthaleneboronic acid (2.66 g, 15.5 mmol), potassium carbonate (2.76 g, 19.9 mmol), toluene (90 mL), water (10 mL), and tetrakistriphenylphosphinepalladium(0) (231 mg, 0.199 mmol) were placed and sealed, followed by stirring at 100°C for 3 hours. The reaction vessel was then allowed to cool to approximately room temperature. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: hexane / dichloromethane = 1 / 1) and then washed with ethyl acetate to obtain the desired compound (B) (yield: 1.42 g, 36%). MS: m / z = 785

[0106] Example 3 Compound (C) was synthesized according to the synthetic route shown below.

[0107] [ka]

[0108] Compound (C) was synthesized by the method shown below. In a 300 mL Schlenk flask equipped with a stirrer and purged with argon, compound (a-3) (2.92 g, 4.53 mmol), dibenzofuran-4-boronic acid (3.07 g, 14.5 mmol), potassium carbonate (2.50 g, 18.1 mmol), toluene (65 mL), water (26 mL), and tetrakistriphenylphosphine palladium (0) (209 mg, 0.181 mmol) were placed and sealed, and then stirred at 100°C for 2 hours. The reaction vessel was then allowed to cool to around room temperature. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: hexane / ethyl acetate = 3 / 1) and then washed with hexane to obtain the desired compound (C) (yield: 900 mg, 22%). MS: m / z = 905

[0109] Example 4 Compound (D) was synthesized according to the synthetic route shown below.

[0110] [ka]

[0111] Compound (d-1) was synthesized by the method shown below. 10H-spiro[acridine-9,9'-fluorene] (2.43 g, 7.34 mmol), N,N-dimethylformamide (147 mL), and 1,3-dibromo-5,5-dimethylhydantoin (2.31 g, 8.08 mmol) were placed in a 300 mL four-neck flask equipped with a stirrer and purged with argon, and the mixture was stirred at room temperature for 2 hours. The reaction vessel was then cooled to 0°C, and saturated aqueous sodium thiosulfate solution (30 mL) was added thereto little by little to stop the reaction. The contents were transferred to a separatory funnel, toluene was added to separate the organic and aqueous phases, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was purified by silica gel column chromatography (developing solvent: hexane / ethyl acetate=3 / 1) to obtain the target compound (d-1) (yield: 2.60 g, 72%).

[0112] Compound (d-2) was synthesized by the method shown below. In a 50 mL Schlenk tube equipped with a stirrer and purged with argon, compound (d-1) (1.17 g, 2.93 mmol), dibenzofuran-4-boronic acid (1.06 g, 5.02 mmol), potassium phosphate (870 mg, 7.17 mmol), toluene (16 mL), water (4 mL), and dichlorobis[di-tert-butyl(4-dimethylaminophenyl)phosphine]palladium(II) (16.9 mg, 0.0239 mmol) were placed and sealed, and then stirred at 100°C for 3 hours. The reaction vessel was then allowed to cool to around room temperature. The contents were transferred to a separatory funnel, dichloromethane was added to separate the organic and aqueous phases, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was washed with hexane to obtain the desired compound (d-2) (yield: 1.47 g, 92%).

[0113] Compound (D) was synthesized by the method shown below. In a 50 mL Schlenk tube equipped with a stirrer and purged with argon, compound (d-2) (1.46 g, 2.19 mmol), 2-(4-bromophenyl)naphthalene (682 mg, 2.41 mmol), bis(tri-tert-butylphosphine)palladium(0) (11.2 mg, 0.0219 mmol), toluene (22 mL), and sodium tert-butoxide (316 mg, 3.29 mmol) were placed and sealed, and then stirred at 100°C for 2 hours. The reaction vessel was then allowed to cool to approximately room temperature, and water (30 mL) was added thereto. The contents were transferred to a separatory funnel, dichloromethane was added to separate the organic and aqueous phases, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: hexane / dichloromethane = 2 / 1) and then washed with toluene to obtain the desired compound (D) (yield: 1.52 g, 80%). MS: m / z = 865

[0114] Example 5 Compound (E) was synthesized according to the synthetic route shown below.

[0115] [ka]

[0116] Compound (e-1) was synthesized by the method shown below. In a 100 mL Schlenk flask equipped with a stirrer and purged with argon, compound (d-1) (3.35 g, 6.84 mmol), 2-naphthaleneboronic acid (2.59 g, 15.0 mmol), potassium carbonate (2.84 g, 20.5 mmol), toluene (31 mL), water (3.4 mL), and dichlorobis[di-tert-butyl(4-dimethylaminophenyl)phosphine]palladium(II) (14.5 mg, 0.0205 mmol) were placed, sealed, and stirred at 100°C for 3 hours. The reaction vessel was then allowed to cool to approximately room temperature, hexane (30 mL) was added, and the precipitate was collected by filtration. The precipitate obtained was washed with hexane to obtain the target compound (e-1) (yield 3.42 g, 86%).

[0117] Compound (E) was synthesized by the method shown below. In a 100 mL Schlenk flask equipped with a stirrer and purged with argon, compound (e-1) (1.80 g, 3.08 mmol), 2-bromo-9,9'-spirobi[9H-fluorene] (1.34 g, 3.39 mmol), bis(tri-tert-butylphosphine)palladium(0) (15.8 mg, 0.0308 mmol), toluene (32 mL), and sodium tert-butoxide (445 mg, 3.73 mmol) were placed and sealed, and then stirred at 100°C for 4 hours. The reaction vessel was then allowed to cool to approximately room temperature, and water (30 mL) was added thereto. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed, and the organic phase was further washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: cyclohexane / toluene = 1 / 1) and then washed with ethyl acetate to obtain the desired compound (E) (yield: 1.29 g, 42%). MS: m / z = 897

[0118] Example 6 Compound (F) was synthesized according to the synthetic route shown below.

[0119] [ka]

[0120] Compound (F) was synthesized by the method shown below. In a 200 mL Schlenk flask equipped with a stirrer and purged with argon, compound (d-2) (1.65 g, 2.48 mmol), 9-(4-bromophenyl)carbazole (1.04 g, 3.23 mmol), bis(tri-tert-butylphosphine)palladium(0) (50.8 mg, 0.0993 mmol), toluene (60 mL), and sodium tert-butoxide (358 mg, 3.73 mmol) were placed and sealed, and then stirred at 100°C for 23 hours. The reaction vessel was then allowed to cool to approximately room temperature, and water (30 mL) was added thereto. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: hexane / dichloromethane = 3 / 1) and then washed with hexane to obtain the desired compound (F) (yield: 862 mg, 38%). MS: m / z = 904

[0121] Example 7 Compound (G) was synthesized according to the synthetic route shown below.

[0122] [ka]

[0123] Compound (g-1) was synthesized by the method shown below. In a 200 mL Schlenk flask equipped with a stirrer and purged with argon, 2-bromoaniline (5.00 g, 29.1 mmol), 1-chloro-4-iodobenzene (17.3 g, 72.7 mmol), bis(tri-tert-butylphosphine)palladium(0) (594 mg, 1.16 mmol), toluene (291 mL), and sodium tert-butoxide (6.98 g, 72.7 mmol) were placed and sealed, and then stirred at 100°C for 15 hours. The reaction vessel was then allowed to cool to approximately room temperature, and water (30 mL) was added thereto. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (developing solvent: hexane / dichloromethane=25 / 1) to obtain the target compound (g-1) (yield: 6.49 g, 57%).

[0124] Compound (g-2) was synthesized by the following method. Compound (g-1) (9.11 g, 23.2 mmol) and tetrahydrofuran (232 mL) were placed in a 500 mL four-neck flask equipped with a stirrer and purged with argon, and the mixture was stirred and cooled to -78°C. n-Butyllithium (1.6 M hexane solution, 17.7 mL, 27.8 mmol) was added dropwise thereto. After stirring for 1 hour, fluorenone (6.27 g, 34.8 mmol) was added and stirred for another 1 hour. Then, distilled water (50 mL) was added little by little thereto to stop the reaction. The contents were transferred to a separatory funnel, ethyl acetate was added thereto to separate the organic phase and the aqueous phase, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. Then, the sodium sulfate was removed by filtration, and the organic phase was concentrated. The resulting mixture was purified by silica gel column chromatography (developing solvent: hexane / dichloromethane=3 / 1) to obtain the target compound (g-2) (yield: 4.54 g, 40%).

[0125] Compound (g-3) was synthesized by the following method. Compound (g-2) (4.64 g, 9.39 mmol), dichloromethane (188 mL), and trifluoromethanesulfonic acid (0.25 mL, 2.82 mmol) were placed in a 500 mL single-neck flask equipped with a stirrer and purged with argon, and stirred at room temperature for 1 hour. Then, saturated aqueous sodium bicarbonate solution (30 mL) was added little by little to stop the reaction. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated. The aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was washed with hexane to obtain the desired compound (g-3) (yield 2.68 g, 60%).

[0126] Compound (G) was synthesized by the method shown below. In a 300 mL Schlenk flask equipped with a stirrer and purged with argon, compound (g-3) (2.68 g, 5.61 mmol), dibenzofuran-4-boronic acid (4.17 g, 19.7 mmol), potassium phosphate (4.77 g, 22.5 mmol), dioxane (112 mL), and bis(di-tert-butyl(4-dimethylaminophenyl)phosphine)dichloropalladium(II) (159 mg, 0.225 mmol) were placed and sealed, and then stirred at 110° C. for 30 hours. The reaction vessel was then allowed to cool to around room temperature. The contents were transferred to a separatory funnel, water was added to separate the organic and aqueous phases, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: hexane / dichloromethane = 1 / 1) and then washed with hexane to obtain the desired compound (G) (yield: 1.45 g, 35%). MS: m / z = 739

[0127] Example 8 Compound (H) was synthesized according to the synthetic route shown below.

[0128] [ka]

[0129] Compound (h-1) was synthesized by the method shown below. 2-Bromo-9-fluorenone (2.50 g, 9.65 mmol), phenylboronic acid (1.29 g, 10.6 mmol), potassium carbonate (2.67 g, 19.3 mmol), toluene (87 mL), water (9.7 mL), and tetrakistriphenylphosphine palladium (0) (223 mg, 0.193 mmol) were placed in a 200 mL Schlenk flask equipped with a stirrer and purged with argon, and the flask was sealed and stirred at 100 ° C for 4 hours. The reaction vessel was then allowed to cool to about room temperature. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated. The aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was washed with hexane to obtain the desired compound (h-1) (yield 2.33 g, 94%).

[0130] Compound (h-2) was synthesized by the method shown below. 2-Bromotriphenylamine (2.60g, 8.02mmol) and tetrahydrofuran (160mL) were placed in a 500mL four-neck flask equipped with a stirrer and purged with argon, and the flask was cooled to -78°C. n-Butyllithium (1.6M hexane solution, 6.13mL, 9.62mmol) was added dropwise thereto. After stirring for 1 hour, compound (h-1) (2.45g, 9.62mmol) was added and stirred for another 1 hour. Distilled water (50mL) was added little by little to stop the reaction. The contents were transferred to a separatory funnel, ethyl acetate was added to separate the organic and aqueous phases, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. Then, the sodium sulfate was removed by filtration, and the organic phase was concentrated. The resulting mixture was purified by silica gel column chromatography (developing solvent: hexane / dichloromethane=3 / 1) to obtain the desired compound (h-2) (yield 3.63 g, 90%).

[0131] Compound (h-3) was synthesized by the method shown below. Compound (h-2) (3.63 g, 7.24 mmol), dichloromethane (145 mL), and trifluoromethanesulfonic acid (0.25 mL, 2.82 mmol) were placed in a 300 mL single-necked flask equipped with a stirrer and stirred at room temperature for 30 minutes. Then, saturated aqueous sodium bicarbonate solution (30 mL) was added little by little to stop the reaction. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated. The aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was washed with methanol to obtain the desired compound (h-3) (yield 3.22 g, 92%).

[0132] Compound (h-4) was synthesized by the method shown below. Compound (h-3) (3.22 g, 6.66 mmol) and dichloromethane (133 mL) were placed in a 300 mL Schlenk flask equipped with a stirrer and purged with argon, and bromine (1.20 mL, 23.3 mmol) was added dropwise thereto. The mixture was stirred at room temperature for 2 hours. The reaction vessel was then cooled to 0°C, and saturated aqueous sodium thiosulfate solution (30 mL) was added thereto little by little to stop the reaction. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was washed with methanol to obtain the desired compound (h-4) (yield 5.01 g, 100%).

[0133] Compound (H) was synthesized by the method shown below. In a 100 mL Schlenk flask equipped with a stirrer and purged with argon, compound (h-4) (3.46 g, 4.80 mmol), 2-naphthaleneboronic acid (2.64 g, 15.4 mmol), potassium carbonate (2.65 g, 19.2 mmol), toluene (22 mL), water (2.4 mL), and bis(di-tert-butyl(4-dimethylaminophenyl)phosphine)dichloropalladium(II) (34.0 mg, 0.0480 mmol) were placed and sealed, and then stirred at 100°C for 3 hours. The reaction vessel was then allowed to cool to around room temperature. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: dichloromethane) and then washed with ethyl acetate to obtain the desired compound (H) (yield: 734 mg, 18%). MS: m / z=861

[0134] Example 9 Compound (I) was synthesized according to the synthetic route shown below.

[0135] [ka]

[0136] Compound (i-1) was synthesized by the method shown below. 2-Bromodiphenylamine (2.50 g, 10.1 mmol) and tert-butyl methyl ether (50 mL) were placed in a 500 mL four-neck flask equipped with a stirrer and purged with argon, and the mixture was stirred and cooled to 0°C. n-Butyllithium (1.6 M hexane solution, 13.0 mL, 20.2 mmol) was added dropwise thereto. After stirring for 1 hour, 11H-benzo[b]fluoren-11-one (4.64 g, 20.2 mmol) was added and stirred for another 1 hour. Distilled water (20 mL) was then added little by little thereto to stop the reaction. The contents were transferred to a separatory funnel, ethyl acetate was added thereto to separate the organic and aqueous phases, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. Then, the sodium sulfate was removed by filtration, and the organic phase was concentrated. The resulting mixture was placed in a 200 mL single-neck flask equipped with a stirrer, and dichloromethane (34 mL) and trifluoromethanesulfonic acid (0.267 mL, 3.02 mmol) were added and stirred at room temperature for 30 minutes. Then, saturated aqueous sodium bicarbonate solution (30 mL) was added little by little to stop the reaction. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated. The aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was purified by silica gel column chromatography (developing solvent: hexane / dichloromethane = 3 / 1) to obtain the desired compound (i-1) (yield 3.78 g, 98%).

[0137] Compound (i-2) was synthesized by the method shown below. Compound (i-1) (3.78 g, 9.91 mmol), N,N-dimethylformamide (99 mL), and 1,3-dibromo-5,5-dimethylhydantoin (2.85 g, 9.91 mmol) were placed in a 300 mL Schlenk flask equipped with a stirrer and purged with argon, and the flask was stirred at room temperature for 1 hour. Then, 5% aqueous sodium sulfite solution (20 mL) was added little by little to stop the reaction. The contents were transferred to a separatory funnel, toluene was added to separate the organic and aqueous phases, the aqueous phase was removed, and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The resulting mixture was washed with hexane to obtain the desired compound (i-2) (yield 4.31 g, 81%).

[0138] Compound (i-3) was synthesized by the method shown below. In a 100mL Schlenk flask equipped with a stirrer and purged with argon, compound (i-2) (2.30g, 4.27mmol), 2-naphthaleneboronic acid (1.64g, 9.38mmol), potassium carbonate (1.77g, 12.8mmol), toluene (19mL), water (2.1mL), and bis(di-tert-butyl(4-dimethylaminophenyl)phosphine)dichloropalladium(II) (9.1mg, 0.0128mmol) were placed, sealed, and stirred at 100°C for 3 hours. The reaction vessel was then allowed to cool to around room temperature. Distilled water (5mL) and hexane (20mL) were added thereto, and the precipitate was collected by filtration to obtain the target compound (i-3) (yield 2.35g, 87%).

[0139] Compound (I) was synthesized by the method shown below. In a 150 mL Schlenk flask equipped with a stirrer and purged with argon, compound (i-3) (2.94 g, 4.65 mmol), 2-(4-bromophenyl)naphthalene (1.45 g, 5.11 mmol), bis(tri-tert-butylphosphine)palladium(0) (23.7 mg, 0.047 mmol), toluene (67 mL), and sodium tert-butoxide (670 mg, 6.97 mmol) were placed and sealed, and then stirred at 100°C for 2 hours. The reaction vessel was then allowed to cool to approximately room temperature, and water (30 mL) was added thereto. The contents were transferred to a separatory funnel, and the organic and aqueous phases were separated, after which the aqueous phase was removed and the organic phase was washed with water. The organic phase was dried over sodium sulfate. The sodium sulfate was then removed by filtration, and the organic phase was concentrated. The concentrated mixture was purified by silica gel column chromatography (eluent: cyclohexane / tetrahydrofuran=1 / 1) and then washed with ethyl acetate to obtain the desired compound (I) (yield: 1.67 g, 35%). MS: m / z=835

[0140] Example 10 DSC measurements were carried out on compound (A) synthesized in Example 1 above, compound (B) synthesized in Example 2 above, compound (C) synthesized in Example 3 above, compound (D) synthesized in Example 4 above, compound (E) synthesized in Example 5 above, compound (F) synthesized in Example 6 above, compound (G) synthesized in Example 7 above, compound (H) synthesized in Example 8 above, compound (I) synthesized in Example 9 above, and the following comparative compounds (X) to (Z). [ka]

[0141] The Tg and decomposition temperatures are shown in Table 1.

[0142] [Table 1]

[0143] As shown in Table 1, the compounds of the present invention have a Tg of 135° C. or more, a high decomposition temperature, and are materials with excellent thermal stability. 2 It is believed that the substitution with acts as one factor that provides favorable thermal stability.

[0144] [Creating organic electroluminescence devices] Example 11 A hole injection layer was formed by vacuum-depositing a compound HAT-CN of the following structural formula to a thickness of 10 nm on a glass substrate on which an ITO (indium tin oxide) film of 110 nm was formed. A first hole transport layer was formed by vacuum-depositing a compound HT1 of the following structural formula to a thickness of 80 nm on the hole injection layer. Next, a second hole transport layer was formed by vacuum-depositing the compound (A) prepared above to a thickness of 10 nm on the first hole transport layer. Next, a 25 nm-thick light-emitting layer was formed on the second hole transport layer using a compound BD1 of the following structural formula as a guest material and a compound BH1 of the following structural formula as a host material, with the guest material content in the light-emitting layer being 4% by weight. Next, a compound HB1 (25 nm) of the following structural formula and a compound ET1 (10 nm) of the following structural formula were sequentially vacuum-deposited on the light-emitting layer to form an electron transport layer. Next, lithium fluoride (LiF) (1 nm) and aluminum (80 nm) were successively deposited on the electron transport layer by vacuum deposition to form an electron injection layer and a cathode.

[0145] [ka]

[0146] Example 12 An organic EL device was formed in the same manner as in Example 11, except that the material of the second hole transport layer was changed to compound (B).

[0147] Example 13 An organic EL device was formed in the same manner as in Example 11, except that the material of the second hole transport layer was changed to compound (C).

[0148] Example 14 An organic EL device was formed in the same manner as in Example 11, except that the material of the second hole transport layer was changed to compound (D).

[0149] Example 15 An organic EL device was formed in the same manner as in Example 11, except that the material of the second hole transport layer was changed to compound (E).

[0150] Example 16 An organic EL device was formed in the same manner as in Example 11, except that the material of the second hole transport layer was changed to compound (F).

[0151] Example 17 An organic EL device was formed in the same manner as in Example 11, except that the material of the second hole transport layer was changed to compound (H).

[0152] Example 18 An organic EL device was formed in the same manner as in Example 11, except that the material of the second hole transport layer was changed to compound (I).

[0153] Comparative Example 1 An organic EL device was formed in the same manner as in Example 11, except that the material for the second hole transport layer was changed to the above comparative compound (X).

[0154] Comparative Example 2 An organic EL device was formed in the same manner as in Example 11, except that the material for the second hole transport layer was changed to the above comparative compound (Y).

[0155] Comparative Example 3 An organic EL device was formed in the same manner as in Example 11, except that the material for the second hole transport layer was changed to the above comparative compound (Z).

[0156] The organic EL devices obtained in Examples 11 to 19 and Comparative Examples 1 to 3 had a luminance of 1000 cd / m 2 The voltage, external quantum efficiency, and chromaticity coordinates were measured at 1000 Hz and 1000 Hz, respectively. The device lifetime was also measured, and the results are shown in Table 2 below. The element life is 100mA / cm 2 In the constant current measurement, the time until the luminance (initial luminance) of the element decayed to 50% was measured.

[0157] [Table 2]

[0158] The organic EL devices of Examples 11 to 18 and Comparative Examples 1 to 3 all emitted blue light. As shown in Table 2, the organic EL devices of Examples 11 to 18 having a hole transport layer containing the compound of the present invention can be driven at a low voltage and exhibit high external quantum efficiency and long device life. 2 By substituting with, the material becomes excellent in thermal stability, and the attack of nucleophilic compounds or electrophilic compounds on the N atom is sterically suppressed, resulting in a material with excellent photostability and electrical stability. It is considered that this compound makes it possible to achieve a reduction in voltage, high efficiency, and long life for organic EL devices containing the compound in the hole transport layer. On the other hand, the organic EL elements of Comparative Examples 1 to 3 having a hole transport layer containing the comparative compound did not necessarily have good driving voltages and external quantum efficiency, and furthermore, the element lifetime was extremely short, so that sufficient characteristics for use in displays, lighting, etc. could not be obtained. [Explanation of symbols]

[0159] 1. Organic EL element 2. Board 3 Second electrode (cathode) 4 Electron injection layer 5 Electron transport layer 6. Light-emitting layer 7 Hole transport layer 8 Hole injection layer 9 1st electrode (anode)

Claims

1.

1. [Case 2] [C3] [C4] [C5] [C6] [C7] A compound selected from the group consisting of:

2. General formula (1-2) or (1-3) [C8] During the ceremony, n is 0 or 1; L represents a single bond, a phenylene group, a naphthylene group, or a divalent aromatic heterocyclic group formed from any one of a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, and a triazine ring, and the phenylene group, the naphthylene group, or the divalent aromatic heterocyclic group may further have a substituent; In formula (1-2), Ar 1 to Ar 5 are each independently an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, or a condensed polycyclic aromatic group which may have a substituent. Here, at least one of Ar 4 to Ar 5 is a condensed polycyclic aromatic group which may have a substituent. In formula (1-3), Ar 1 to Ar4 are each independently an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, or a fused polycyclic aromatic group which may have a substituent; R is hydrogen, deuterium, a halogen group, a linear, branched or cyclic alkyl group which may have a substituent, a linear, branched or cyclic alkoxy group which may have a substituent, or an aromatic hydrocarbon group which may have a substituent; A compound represented by the formula:

3. The compound according to claim 2 , wherein L is a single bond, a phenylene group, or a naphthylene group.

4. In the formula (1-2), Ar 4 , Ar 5 At least one of is a naphthylene group; The compound according to claim 2, wherein, in formula (1-3), Ar 4 is a phenylene group, a biphenylene group, or a naphthylene group.

5. The compound according to any one of claims 2 to 4, wherein R is hydrogen or a phenyl group.

6. A hole transport material comprising the compound according to any one of claims 1 to 5.

7. An organic electronic device including an organic electroluminescence element or an organic photoelectric conversion element having a hole transport layer between a cathode and an anode, An organic electronic device, characterized in that the hole transport layer comprises a compound according to any one of claims 1 to 5.

8. 8. The organic electronic device of claim 7, comprising an organic electroluminescent element having a light-emitting layer between a hole-transporting layer and a cathode.

9. the light-emitting layer contains a host material and a guest material made of a light-emitting material, 9. The organic electronic device according to claim 8, wherein the host material is an electron transporting material or a dual charge transporting material having hole transporting and electron transporting properties.

Citation Information

Patent Citations

  • Organic electroluminescence luminescent compound, organic electroluminescence luminescent device and application thereof

    CN108117539A

  • N-Heterocyclic compounds and their use in electronic, optoelectronic and electroluminiscent components

    EP1840120A1

  • Low-noise variable valve timing mechanism

    JP1986093215A

  • Thin plate deforming device

    JP1987079647A

  • New organic light-emitting material and organic light-emitting device using the same (6)

    JP2008511155A