Intermediate transfer belt and image forming apparatus
The intermediate transfer belt with a polyimide base layer and a surface layer of controlled shrinkage and hardness addresses curling and sensor reading issues, enhancing image quality and durability.
Patent Information
- Application Number
- JP2020170035
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-10-07
AI Technical Summary
Intermediate transfer belts in electrophotographic image forming apparatuses experience curling and optical sensor reading errors due to stress concentration at bent portions, especially when used in small devices with large bending angles, making it difficult to implement tension adjusting mechanisms.
The intermediate transfer belt is composed of a base layer made of polyimide with a surface layer having a specific shrinkage amount of 4 mm to 6 mm and nanoindenter hardness of 110 MPa to 230 MPa, achieved through a combination of materials and UV curing process.
This configuration suppresses image defects related to poor patch sensor reading without worsening curling tendencies, ensuring reliable operation and durability.
Smart Images

Figure 0007566562000002 
Figure 0007566562000003 
Figure 0007566562000001
Abstract
Description
[Technical field]
[0001] The present invention relates to electrophotographic members and devices used in electrophotographic image forming apparatuses such as copying machines and printers, and more particularly to an intermediate transfer belt and an image forming apparatus. [Background technology]
[0002] In electrophotographic image forming devices, the tandem method is widely used, in which YMCK toner images are superimposed on an intermediate transfer belt, and then transferred onto paper all at once to obtain a full-color image. In general, intermediate transfer belts are required to have surface properties such as smoothness and glossiness from the viewpoints of cleaning properties, optical sensor reading, etc., in addition to electrical properties and mechanical strength.
[0003] Patent Document 1 proposes a means for controlling the surface properties by using a lapping film to rotary polish the outer peripheral surface of the intermediate transfer belt. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-181767 A [Patent Document 2] JP 2006-53492 A Summary of the Invention [Problem to be solved by the invention]
[0005] In intermediate transfer belts polished as in Patent Document 1, problems such as poor image quality due to curling tendencies and reading errors by optical sensors can occur. Normally, intermediate transfer belts are stretched under a constant tension by multiple supports arranged on the inside, rotated by a drive roller, etc., and transport the toner image.
[0006] However, when a long period of downtime occurs, stress is concentrated for a long time at the portion where the intermediate transfer belt is bent by the support or the like, and curling may remain. In particular, in an intermediate transfer belt processed by applying a large tension (stress in the circumferential direction) during polishing as in Patent Document 1, stress remains even after polishing, and the intermediate transfer belt is likely to curl.
[0007] The curling tendency becomes more severe as the angle at which the intermediate transfer belt is bent by the support becomes larger. In other words, the curling tendency is more likely to occur when the intermediate transfer belt is used in a small device, which generally has a tendency to have a larger bending angle. In the case of such a small device, it is difficult to provide a mechanism for moving the tension applying means as in Patent Document 2 due to cost, arrangement, and other factors, and this has been an issue.
[0008] An object of the present invention is to provide an intermediate transfer belt and an image forming apparatus that can suppress image defects related to reading errors of a patch sensor without worsening the curl of the intermediate transfer belt. [Means for solving the problem]
[0009] The intermediate transfer belt according to the present invention is an intermediate transfer belt having a base layer and a surface layer, the base layer being mainly composed of at least polyimide, and the surface layer having a shrinkage amount of 4 mm or more and 6 mm or less and a nanoindenter hardness of 110 MPa or more and 230 MPa or less. Effect of the Invention
[0010] According to the present invention, by making the surface layer of the intermediate transfer belt have a certain range of shrinkage, it is possible to suppress image defects related to poor reading by the patch sensor without worsening the winding tendency of the intermediate transfer belt. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic diagram of a cross section of an intermediate transfer belt of the present invention. [Diagram 2]1 is a schematic diagram showing a cross section of an image forming apparatus using an intermediate transfer belt of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings.
[0013] (Image forming device) An example of an image forming apparatus using the intermediate transfer belt of the present invention will be described with reference to Fig. 2. However, the present invention is not limited to the following description.
[0014] The electrophotographic image forming apparatus 100 in Fig. 2 is a color electrophotographic image forming apparatus (color laser printer). In this electrophotographic image forming apparatus, image forming units Py, Pm, Pc, and Pk of the colors yellow (Y), magenta (M), cyan (C), and black (K) are arranged in the moving direction along a flat portion of an intermediate transfer belt 7 serving as an intermediate transfer body. Here, 1Y, 1M, 1C, and 1K respectively denote electrophotographic photosensitive bodies, 2Y, 2M, 2C, and 2K respectively denote charging rollers, 3Y, 3M, 3C, and 3K respectively denote laser exposure devices, 4Y, 4M, 4C, and 4K respectively denote developing devices, and 5Y, 5M, 5C, and 5K respectively denote primary transfer rollers. Since the basic configuration of each image forming unit is the same, only the yellow image forming unit Py will be described in detail as to the image forming units.
[0015] The yellow image forming unit Py has a drum-shaped electrophotographic photosensitive member (hereinafter also referred to as a "photosensitive drum" or a "first image bearing member") 1Y as an image bearing member. The photosensitive drum 1Y is formed by laminating a charge generating layer, a charge transport layer, and a surface protective layer in this order on an aluminum cylinder as a base.
[0016] Further, the yellow image forming unit Py includes a charging roller 2Y as a charging means. By applying a charging bias to the charging roller 2Y, the surface of the photosensitive drum 1Y is uniformly charged.
[0017] A laser exposure device 3Y is disposed above the photosensitive drum 1Y as an image exposure means. The laser exposure device 3Y scans and exposes the uniformly charged surface of the photosensitive drum 1Y in accordance with image information, forming an electrostatic latent image of a yellow color component on the surface of the photosensitive drum 1Y.
[0018] The electrostatic latent image formed on the photosensitive drum 1Y is developed by the developing device 4Y as a developing means with toner as a developer. That is, the developing device 4Y includes a developing roller 4Ya as a developer carrier, a regulating blade 4Yb as a developer amount regulating member, and contains yellow toner as a developer. The developing roller 4Ya to which the yellow toner is supplied is lightly pressed against the photosensitive drum 1Y in the developing section, and rotates in the forward direction with a speed difference from the photosensitive drum 1Y. The yellow toner conveyed to the developing section by the developing roller 4Ya adheres to the electrostatic latent image formed on the photosensitive drum 1Y by applying a developing bias to the developing roller 4Ya. As a result, a visible image (yellow toner image) is formed on the photosensitive drum 1Y.
[0019] The intermediate transfer belt 7 is stretched around a drive roller 71, a tension roller 72, and a driven roller 73, and is moved (rotationally driven) in the direction of the arrow in the figure while in contact with the photosensitive drum 1Y.
[0020] The yellow toner image formed on the photosensitive drum (first image carrier) that has reached the primary transfer portion Ty is primarily transferred onto the intermediate transfer belt 7 by a primary transfer body (primary transfer roller 5Y) that is arranged opposite the photosensitive drum 1Y via the intermediate transfer belt 7.
[0021] Similarly, the above image forming operation is performed in each of the magenta (M), cyan (C) and black (K) units Pm, Pc and Pk as the intermediate transfer belt 7 moves, and toner images of four colors, yellow, magenta, cyan and black, are stacked on the intermediate transfer belt 7. The four color toner layers are transported as the intermediate transfer belt 7 moves, and are transferred collectively at the secondary transfer portion T' by a secondary transfer roller 8 as a secondary transfer means onto a transfer material S (hereinafter also referred to as a "second image carrier") transported at a predetermined timing. In such secondary transfer, a transfer voltage of several kV is usually applied to ensure a sufficient transfer rate.
[0022] The transfer material S is supplied to a conveying path from a cassette 12 in which the transfer material S is stored by a pickup roller 13. The transfer material S supplied to the conveying path is conveyed to a secondary transfer portion T' in synchronization with the four-color toner image transferred to the intermediate transfer belt 7 by a conveying roller pair 14 and a registration roller pair 15.
[0023] The toner image transferred to the transfer material S is fixed by a fixing device 9 to become, for example, a full-color image. The fixing device 9 has a fixing roller 91 equipped with a heating means and a pressure roller 92, and fixes the unfixed toner image on the transfer material S by applying heat and pressure. Thereafter, the transfer material S is discharged outside the machine by a pair of conveying rollers 16, a pair of discharge rollers 17, etc.
[0024] A cleaning unit for the intermediate transfer belt 7 is disposed downstream of the secondary transfer portion T' in the driving direction of the intermediate transfer belt 7, and removes residual toner that has not been transferred to the transfer material S at the secondary transfer portion T' and remains on the intermediate transfer belt 7.
[0025] As described above, the electrical transfer process of the toner image is repeated from the photoconductor to the intermediate transfer belt and from the intermediate transfer belt to the transfer material. Furthermore, by repeating recording on a large number of transfer materials, the electrical transfer process is further repeated.
[0026] (Intermediate transfer belt) As shown in FIG. 1, the intermediate transfer belt 7 of the present invention is made up of two layers: a base layer 10 and a surface layer 11 provided on the outer periphery of the base layer 10 .
[0027] (base layer) <Resin materials> The resin material constituting the base layer 10 is mainly composed of polyimide (PI), and other resins such as polyphenylene sulfide (PPS), polyetherimide (PEI), polyetheretherketone (PEEK), polyamideimide (PAI), and polyamide (PA) can be used as secondary components.
[0028] <Conductive filler> At least one type of carbon black or metal particles is blended as a conductive filler into the resin material for the purpose of imparting electrical conductivity to the belt member, etc. Among these, carbon black is preferred from the viewpoint of mechanical properties.
[0029] Carbon black is known by various names depending on its manufacturing method and raw materials, such as ketjen black, furnace black, acetylene black, thermal black, and gas black.
[0030] As the carbon black, various known ones can be used. Specific examples include the following. Ketjen black, furnace black, acetylene black, thermal black, and gas black can be mentioned. Among these, acetylene black and furnace black are preferred because they contain less impurities, have less frequency of foreign matter defects when molded into a film shape together with the thermoplastic resin, and are easy to obtain the desired conductivity. Specific examples of acetylene black include the "Denka Black" series (manufactured by Denki Kagaku Kogyo Co., Ltd.), the "Mitsubishi Conductive Filler" series (manufactured by Mitsubishi Chemical Corporation), the "Vulcan" series (manufactured by Cabot Corporation), the "Brintex" series (manufactured by Degussa), and "SRF" (manufactured by Asahi Carbon Co., Ltd.). Specific examples of furnace black include the "Toka Black" series (manufactured by Tokai Carbon Co., Ltd.) and the "Asahi Carbon Black" series (manufactured by Asahi Carbon Co., Ltd.).
[0031] (Method of manufacturing base layer) The base layer 10 of the intermediate transfer belt 7 can be prepared by the following method.
[0032] For example, carbon black, which is a conductive filler, is dispersed as a varnish together with a precursor of polyimide (thermosetting resin) or a soluble thermosetting resin and a solvent, and this varnish is coated onto a mold of a centrifugal molding device. Next, the coated film is baked to form a semiconductive film. The thickness of the semiconductive film that serves as the base layer is preferably 50 μm or more and 80 μm or less.
[0033] Furthermore, polishing is performed in order to control the surface properties such as smoothness and glossiness. The lapping film used in the present invention may be a known commercially available product. For example, the abrasive grain type may be aluminum oxide (WA), silicon carbide (GC), diamond (D), etc., and the film size may be selected from #600, #800, #1000, #2000, etc. In addition, as a tensioning means for the intermediate transfer belt during rotary polishing, there are a tensioning roller movement method in which tension is applied by moving a tensioning roller from the inner side of the intermediate transfer belt to the outer side, and a core method in which tension is applied by holding the intermediate transfer belt in a cylindrical core having an outer periphery length that is several percent larger than the inner periphery length of the intermediate transfer belt, and any of the tensioning means may be used.
[0034] (Surface layer) The material constituting the surface layer 11 mainly includes an ultraviolet curing resin, a photopolymerization initiator, a conductive substance, etc. In order to improve releasability, a fluorine-based resin, etc. may be added.
[0035] Examples of ultraviolet-curable resins obtained by curing ultraviolet-curable materials include urethane resins, acrylic resins, epoxy resins, polyester resins, methacrylic resins, maleimide resins, oxetane resins, polyether resins, and polyvinyl ether resins. Among these, acrylic resins having high hardness are particularly preferable in consideration of rubbing against other members such as photoconductors and cleaning blades. Such ultraviolet-curable resins can be obtained by curing ultraviolet-curable monomers, oligomers, prepolymers, and the like.
[0036] Examples of the photopolymerization initiator include radical-generating photopolymerization initiators such as benzophenone, thioxanthone, benzyl dimethyl ketal, α-hydroxyketone, α-hydroxyalkylphenone, α-aminoketone, α-aminoalkylphenone, monoacylphosphine oxide, bisacylphosphine oxide, hydroxybenzophenone, aminobenzophenone, titanocene, oxime ester, and oxyphenylacetic acid ester.
[0037] Examples of the conductive material include inorganic conductive particles of carbon such as carbon black, carbon fiber, and carbon nanotubes, and metal oxides such as zinc antimonate, zinc oxide, tin oxide, and titanium oxide.
[0038] The surface layer is formed by first dissolving and dispersing the above-mentioned components in an appropriate organic solvent to obtain a surface layer coating liquid. Next, the outer periphery of the base layer is coated with the coating liquid by a method such as ring coating, dip coating, or spray coating, and then drying is performed to remove the organic solvent. The drying is preferably performed in an environment of about 50 to 80°C so as not to induce a radical reaction. Then, the coating liquid is cured with ultraviolet light using an ultraviolet irradiator to obtain the intermediate transfer belt 7 of the present invention.
[0039] The thickness of the surface layer is preferably 4 μm or more and 10 μm or less. If the thickness of the surface layer is less than 4 μm, the shrinkage stress of the surface layer will be weak, and there is a risk that the curling tendency will not be alleviated, and if the thickness is more than 10 μm, the adhesion between the base layer and the surface layer will deteriorate, and peeling will occur.
[0040] In addition, the surface layer 11 shrinks when it hardens, and as a result, stress acts on the outer peripheral surface side of the curling tendency acting on the inner peripheral surface side of the base layer 10, and the curling tendency can be alleviated. A physical property that correlates with the stress during this shrinkage is the amount of shrinkage (the amount of warping of the surface layer is measured, and the measurement method will be described later). The surface layer 11 needs to have this amount of shrinkage of 4 mm or more and 6 mm or less, and the nanoindenter hardness of the surface layer surface of 110 MPa or more and 230 MPa or less. If the amount of shrinkage is less than 4 mm, the force that alleviates the curling tendency stress acting on the base layer 10 becomes small, so that the curling tendency of the intermediate transfer body 7 becomes large, and there is a risk of a sensor reading error. If the amount of shrinkage is more than 6 mm, there is a risk of peeling due to the stress acting on the outer peripheral surface side of the surface layer 11.
[0041] Methods for adjusting the amount of shrinkage include the resin composition, the amount of ultraviolet light exposure, and the coat thickness.
[0042] Regarding the nano indenter hardness of the surface layer, if it is less than 110 MPa, the pressure from the cleaning blade will cause the belt side to be depressed, and when the pressure exceeds the depression on the belt side, a larger pressure will be applied, which may induce blade curling. Also, if it is more than 230 MPa, the film will become too hard and the folding resistance may decrease.
[0043] Also, from a material perspective, similar to the amount of shrinkage of surface layer 11, the shrinkage stress acting upon hardening of surface layer 11 is a stress generated as a result of shrinkage at the molecular level during each polymerization reaction, and is thought to be correlated with the total number of polymerization reactions in surface layer 11.
[0044] The sum of the number of reactions is the [average acrylic equivalent / curing rate]. The surface layer 11 needs to have this [average acrylic equivalent / curing rate] of 192 or more and 201 or less.
[0045] If this [average acrylic equivalent / curing rate] is less than 192, there is a risk of peeling due to the stress acting on the outer surface side of the surface layer 11. If it is greater than 201, the force acting on the base layer 10 to relieve the curling stress will be small, causing the intermediate transfer belt 7 to curl more significantly, which may result in a sensor reading error.
[0046] Here, the acrylic equivalent is the monomer molecular weight / number of functional groups, which is an inherent value of the monomer, and the average acrylic equivalent is the value calculated by the molar average of the blending ratio of each monomer and dividing it by the volume ratio of the acrylic component in the surface layer 11. The curing rate is the polymerization reaction rate of the functional groups during UV curing, and can be measured by a Fourier transform infrared spectrophotometer (FT-IR), and the measurement method will be described later. EXAMPLES
[0047] The intermediate transfer belt was prepared in the following manner. The base layer was a cylindrical film made of polyimide resin containing an electronic conductive material with a thickness of 60 μm, volume resistivity ρv = 5E+9 (Ω·cm), and surface resistivity ρs = 1E+10 (Ω / □).The outer surface of the film was polished using a polishing film (KOVAX Corporation's Lapica WA#800) to a gloss meter of 60 on a Horiba Corporation IG-320, to obtain the base layer 10 shown in Figure 1.
[0048] [Coating liquid 1] The coating solution for forming the surface layer is as follows. Dipentaerythritol hexaacrylate 31.0 parts by mass Pentaerythritol triacrylate 4.0 parts by mass Pentaerythritol tetraacrylate 11.0 parts by mass Methyl ethyl ketone 60 parts by weight PTFE particles 0.2 μm (Lubron manufactured by Daikin) 35.0 parts by mass Dispersant (Aron GF-420, manufactured by Toagosei Co., Ltd.) 20.0 parts by weight Antimony-doped tin oxide particles (Ishihara Sangyo Kaisha, Ltd. SN-100P) 7.0 parts by mass Photoinitiator (Omnirad 184 made by IGM Resins) 5.0 parts by mass For the surface layer, the above-mentioned coating liquid 1 was mixed and dispersed using a stirring homogenizer, and then dispersed using a dispersing device Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.) to obtain a mixed dispersion liquid.
[0049] The mixed dispersion liquid was applied to the polished base layer made of polyimide resin by ring coating, and placed in a drying oven at 60° C. for 2 minutes. Then, it was cured with ultraviolet light of 1500 mJ / cm to obtain an intermediate transfer belt 1 with a surface layer thickness of 5 μm.
[0050] The amount of shrinkage of the surface layer of this intermediate transfer belt 1 was 5.2 mm, the nano indenter hardness of the surface layer was 150 MPa, and the hardening rate was 92%. The method of measuring the amount of shrinkage of the surface layer, the nano indenter hardness of the surface layer, and the hardening rate will be described later.
[0051] The intermediate transfer belt 1 thus produced was mounted on an evaluation device, and an image was formed on the belt. The output image was evaluated, and a cross-cut test was performed to check for peeling, and an MIT test was performed to check the bending resistance of the intermediate transfer belt. The detailed image evaluation method, cross-cut test method, and MIT test method will be described later.
[0052] The evaluation results are shown in Table 1.
[0053] [Table 1] EXAMPLES
[0054] An intermediate transfer belt 2 was obtained in the same manner as in Example 1, except that the following coating liquid 2 was used. The measurement results and evaluation results are shown in Table 1 above.
[0055] [Coating liquid 2] The coating solution for forming the surface layer is as follows. Dipentaerythritol hexaacrylate 26.0 parts by mass Pentaerythritol tetraacrylate 20.0 parts by mass Methyl ethyl ketone 60 parts by weight PTFE particles 0.2 μm (Lubron manufactured by Daikin) 35.0 parts by mass Dispersant (Aron GF-420, manufactured by Toagosei Co., Ltd.) 20.0 parts by weight Antimony-doped tin oxide particles (Ishihara Sangyo Kaisha, Ltd. SN-100P) 7.0 parts by mass Photoinitiator (Omnirad 184 made by IGM Resins) 5.0 parts by mass EXAMPLES
[0056] An intermediate transfer belt 3 was obtained in the same manner as in Example 1, except that the following coating liquid 3 was used. The measurement results and evaluation results are shown in Table 1 above.
[0057] [Coating liquid 3] The coating solution for forming the surface layer is as follows. Dipentaerythritol hexaacrylate 37.0 parts by mass Pentaerythritol triacrylate 8.0 parts by mass Pentaerythritol tetraacrylate 1.0 part by mass Methyl ethyl ketone 60 parts by weight PTFE particles 0.2 μm (Lubron manufactured by Daikin) 35.0 parts by mass Dispersant (Aron GF-420, manufactured by Toagosei Co., Ltd.) 20.0 parts by weight Antimony-doped tin oxide particles (Ishihara Sangyo Kaisha, Ltd. SN-100P) 7.0 parts by mass Photoinitiator (Omnirad 184 made by IGM Resins) 5.0 parts by mass EXAMPLES
[0058] An intermediate transfer belt 4 was obtained in the same manner as in Example 1, except that the following coating liquid 4 was used and the amount of ultraviolet light irradiation was set to 3000 mJ / cm 2 .
[0059] [Coating liquid 4] The coating solution for forming the surface layer is as follows. Dipentaerythritol hexaacrylate 31.0 parts by mass Pentaerythritol triacrylate 4.0 parts by mass Pentaerythritol tetraacrylate 11.0 parts by mass Methyl ethyl ketone 60 parts by weight PTFE particles 0.2 μm (Lubron manufactured by Daikin) 37.0 parts by mass Dispersant (Aron GF-420, manufactured by Toagosei Co., Ltd.) 22.8 parts by weight Antimony-doped tin oxide particles (Ishihara Sangyo Kaisha, Ltd. SN-100P) 8.0 parts by mass Photoinitiator (Omnirad 184 made by IGM Resins) 5.0 parts by mass EXAMPLES
[0060] An intermediate transfer belt 5 was obtained in the same manner as in Example 1, except that the coating liquid 4 in Example 4 was used and the ultraviolet ray irradiation amount was set to 4000 mJ / cm2.
[0061] An intermediate transfer belt 6 was obtained in the same manner as in Example 1, except that the coating liquid 2 in Example 2 was used and the amount of ultraviolet light irradiation was set to 800 mJ / cm2.
[0062] An intermediate transfer belt 7 was obtained in the same manner as in Example 1, except that the coating liquid 2 in Example 3 was used and the ultraviolet ray irradiation amount was set to 3000 mJ / cm2.
[0063] An intermediate transfer belt 8 was obtained in the same manner as in Example 1, except that the coating liquid 1 in Example 1 was used and the amount of ultraviolet light irradiation was set to 3000 mJ / cm2.
[0064] An intermediate transfer belt 9 was obtained in the same manner as in Example 1, except that the coating liquid 4 in Example 4 was used and the amount of ultraviolet light irradiation was set to 1500 mJ / cm 2 .
[0065] Next, the methods for measuring the contraction force, nanoindenter hardness, and hardening rate of the surface layer, as well as the evaluation methods such as image evaluation, cross-cut test, and MIT test will be explained.
[0066] [Shrinkage measurement] The mixed dispersion liquid shown in the Examples was applied to a base layer made of polyimide resin cut into a sheet shape with a size of 50 mm x 100 mm (without the polishing process described in the Examples) to a thickness of 5 μm using a tabletop bar coater (K Control Coater made by RK Print Coat Instruments), and the intermediate transfer body with a size of 50 mm x 100 mm was produced by curing it with ultraviolet light after placing it in a drying oven at 60°C for 2 minutes. The height of the warp at the center position of the short side of the long side end was measured and recorded as the amount of shrinkage.
[0067] [Nano indenter hardness measurement] The nanoindenter hardness of the surface layer described above was measured using an ultra-microhardness tester nanoindenter (manufactured by MTS Systems). The intermediate transfer belt was measured in the same environment after being left for 24 hours in a temperature of 23°C and humidity of 50% RH. The measurement method was the continuous stiffness measurement method (CSM), in which the indenter was a triangular pyramid (Berkovich type) made of a diamond tip, the vibration frequency was 45 Hz, the target value of the displacement response amplitude was 1 nm, and measurements were taken to a depth of 1.5 μm, and the saturated hardness value was evaluated in the displacement amount-hardness curve. The measurement was performed five times, and the average value was used.
[0068] [Curing rate measurement] Acrylic resin cures when UV light irradiation cleaves the C=C bonds (olefins) in the monomer into single bonds and polymerizes them. In other words, the degree of cure of the acrylic resin can be estimated by examining the amount of remaining C=C bonds that have not yet been cleaved into single bonds. To examine the amount of remaining C=C groups, a band assigned to the C=CH in-plane bending vibration (1408 cm-1) was selected and normalized by the peak height of the band assigned to the CH2 bending vibration originating from the acrylic in the same film at around 1470 cm-1. The intensity (peak height) of the band of the C=CH in-plane bending vibration (1408 cm-1) in the surface layer 11 before and after UV light irradiation was obtained, and the cure rate was calculated using the following formula. Cure rate (%) = {1-(band intensity after UV irradiation / band intensity before UV irradiation) x 100}
[0069] [Image evaluation method] Each intermediate transfer belt of the examples and comparative examples was attached to the image forming apparatus shown in Fig. 2 and left for 100 hours in a high temperature and high humidity environment (30°C / 80%). After leaving it, five sheets of halftone magenta A3 size plain paper (CS068, Canon Inc.) were continuously fed, and the horizontal streaks caused by curling were evaluated according to the following criteria. (Horizontal streak evaluation) A: No horizontal lines were observed. B: Horizontal lines less than 1 mm wide were observed. C: Horizontal lines 1 mm or wider were observed.
[0070] [Cross-cut test] A cross-cut test was carried out to evaluate the degree of peeling of the film. The measurement method for the cross-cut test was performed according to JIS K5600-5-6. The test was carried out at a position 5 mm inward from the cut edge of each elastic transfer belt. The peeling was judged as follows: ○: Of the 25 squares, not a single square was found to have peeled off. ×: One or more squares out of 25 are peeled off.
[0071] [MIT Exam] The intermediate transfer belt was subjected to the MIT test specified in JIS P8115 as a bending resistance test. The MIT test was performed 50,000 times, and a test piece that did not break after 50,000 times was marked as O, and a test piece that broke after less than 50,000 times was marked as ×.
[0072] The MIT test was performed using an MIT-D (manufactured by Toyo Seiki Co., Ltd.) under the following conditions: winding curvature diameter: 20 mm, angle: 90 degrees, load: 0.5 kg / mm2.
[0073] The measurement results of the shrinkage rate, nanoindenter hardness, hardening rate, etc., as well as the evaluation results of the image evaluation and crosscut test, etc., of the intermediate transfer belts 1 to 8 according to each of the examples and comparative examples are summarized in Table 1 above.
[0074] The results in Table 1 show that by setting the shrinkage amount to 4 mm or more and 6 mm or less and the nano indenter hardness to 120 MPa or more and 230 MPa or less, an intermediate transfer belt is obtained that does not peel off and does not have horizontal streaks in the image evaluation. [Explanation of symbols]
[0075] 7 Intermediate transfer belt 10 Base layer 11 Surface layer
Claims
1. An intermediate transfer belt onto which a toner image is transferred, The intermediate transfer belt has two or more layers, including a base layer mainly composed of at least polyimide and a surface layer provided on the outer circumferential surface of the base layer, and is characterized in that the amount of shrinkage of the surface layer is 4 mm or more and 6 mm or less, and the nanoindenter hardness of the surface layer is 110 MPa or more and 230 MPa or less.
2. An intermediate transfer belt onto which a toner image is transferred, The intermediate transfer belt has two or more layers, including at least a base layer mainly composed of polyimide and a surface layer mainly composed of acrylic provided on the outer periphery of the base layer, wherein the surface layer has an [average acrylic equivalent / curing rate] of 192 or more and 201 or less, and the surface layer has a nanoindenter hardness of 110 MPa or more and 230 MPa or less.
3. 3. An image forming apparatus using the intermediate transfer belt according to claim 1.
Citation Information
Patent Citations
Method for manufacturing polyimide endless belt
JP2005181767A
Image forming device
JP2006053492A
Image formation device
JP2013024898A
Image forming apparatus
JP2016099440A
Conductive endless belt and image forming apparatus
JP2020201317A