Zirconia molding suitable for dental use
A zirconia molded body with controlled porosity and stabilizer composition addresses the issue of translucency loss in dental CAD/CAM systems, ensuring high-quality dental prostheses with simplified production.
Patent Information
- Application Number
- JP2021552477
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-17
- Filing Date
- 2020-10-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-10-16
AI Technical Summary
Existing dental CAD/CAM systems face issues with zirconia sintered bodies becoming white due to the use of contaminated cooling solvents during wet processing, which affects translucency and requires complex and time-consuming production processes.
A zirconia molded body with specific open porosity, stabilizer, and binder composition that suppresses phase transition, allowing easy processing and maintaining translucency even when using contaminated cooling solvents.
The solution enables production of zirconia sintered bodies with maintained translucency and strength, reducing defects like cracks, suitable for dental prostheses, and simplifies the manufacturing process.
Smart Images

Figure 0007566764000001 
Figure 0007566764000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a zirconia molded body. [Background technology]
[0002] Conventionally, in dental applications, a technique has been used in which ceramic materials such as highly translucent and aesthetic silicate glass and high-strength zirconia are processed using dental CAD / CAM systems into shapes that fit the affected areas of the patient's teeth, sintered, and then fitted into the patient's oral cavity as the final dental prosthesis. When zirconia is used, dental zirconia is used.
[0003] In the early days, dental zirconia was strong but extremely opaque, but in recent years, in response to patient demand, its translucency has increased to a level close to that of natural teeth. In addition, while traditionally, dental prostheses were often made only from zirconia at dental laboratories, in recent years dental clinics have increasingly been using calcined zirconia bodies, which can be fired in a short time, to easily make them.
[0004] As described in Non-Patent Documents 1 and 2, generally, the processing machine of the dental CAD / CAM system uses at least one of the wet and dry processing methods, or has both wet and dry processing. In the case of processing a glass material such as silicate glass, which is a high-density material, wet processing in which a processing liquid is circulated is selected to prevent the processing tool from seizing, and for dental zirconia, which is a calcined body, at least one of the wet and dry processing methods is selected. In such a case, the cooling solvent may be shared between the glass material and the zirconia material during wet processing, but in that case, it is known that the zirconia sintered body becomes white (see Patent Document 1). Therefore, it is usually necessary to replace the cooling solvent when wet processing a zirconia material after wet processing a glass material.
[0005] On the other hand, Patent Document 1 discloses a dental zirconia calcined body that prevents the whitening of the zirconia sintered body. It is described that the whitening of the zirconia sintered body is caused by glass components dissolved in the cooling solvent, and it is disclosed that by impregnating the calcined body with a specific impregnating material, the permeation of the contaminated cooling solvent is prevented, and the whitening of the zirconia sintered body is suppressed even if wet processing is performed using a cooling solvent shared with the glass material. However, in order to prepare the zirconia calcined body disclosed in Patent Document 1, it is first necessary to press-form zirconia raw material granules to prepare a zirconia molded body, and then to obtain a strength that can withstand processing, it is usually necessary to hold and calcinate at a temperature in the range of 800 to 1200 ° C. Furthermore, since it is necessary to treat the calcined body with a specific impregnating material after preparing it, there is a disadvantage that it takes a lot of time to prepare it. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2019-108289 A [Non-patent literature]
[0007] [Non-Patent Document 1] Asahi Roentgen Industrial Co., Ltd. Product information, [online], [Searched on August 19, 2019], Internet<URL http: / / www.asahi-xray.co.jp / products / ceramill-motion2> [Non-Patent Document 2] Dentsply Sirona Co., Ltd. CEREC Milling Units, [online], [searched October 7, 2019], Internet<URL https: / / www.dentsplysirona.com / ja-jp / explore / cerec / produce-with-cerec.html> Summary of the Invention [Problem to be solved by the invention]
[0008] For these reasons, when a cooling solvent is used in combination with wet processing of glass materials and zirconia materials using a dental CAD / CAM system, it is desired to more easily produce dental mill blanks that do not whiten when processed using the cooling solvent.
[0009] An object of the present invention is to provide a zirconia molded body and a dental mill blank that can easily produce a zirconia sintered body and that suppresses a decrease in the translucency of the zirconia sintered body when fired, even when the zirconia sintered body is wet-processed using a dental CAD / CAM system using a contaminated cooling solvent. [Means for solving the problem]
[0010] As a result of extensive research into solving the above problems, the present inventors discovered that the above-mentioned dental mill blanks can be easily produced by making a zirconia molded body having a specific open porosity, and thus completed the present invention.
[0011] That is, the present invention includes the following inventions. [1] Zirconia, A stabilizer capable of suppressing the phase transition of zirconia; A binder; A zirconia molding having an open porosity of 25% or less. [2] The zirconia molded body according to [1], wherein the open porosity is 5% or more. [3] The zirconia molded body according to [1] or [2], wherein the content of the binder is 3 to 10 mass % based on the total mass of the zirconia, the stabilizer, and the binder. [4] The zirconia molded body according to [3], wherein the binder content is 5 to 8 mass %. [5] The zirconia molded body according to any one of [1] to [4], which has a water absorption rate of 7% or less. [6] The zirconia molded body according to any one of [1] to [5], wherein the zirconia has a predominant crystal system of a monoclinic system. [7] The zirconia molded body according to any one of [1] to [6], wherein at least a part of the stabilizer is not solid-dissolved in the zirconia. [8] The zirconia molded body according to any one of [1] to [7], wherein the stabilizer is yttria. [9] The zirconia molded body according to [8], wherein the content of the yttria is 3 mol % or more and 7.5 mol % or less based on the total moles of zirconia and yttria.
[10] The zirconia molded body according to any one of [1] to [9], wherein the binder is at least one selected from the group consisting of polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, polyvinyl butyrate, wax, and acrylic binders.
[11] The zirconia molded body according to any one of [1] to
[10] , which has a biaxial flexural strength of 7 to 30 MPa.
[12] A dental mill blank comprising the zirconia molded body according to any one of [1] to
[11] . Effect of the Invention
[0012] According to the present invention, even if wet-processed in a dental CAD / CAM system using a contaminated cooling solvent, a decrease in the translucency of the zirconia sintered body is suppressed when sintered, and a dental mill blank that can easily produce a zirconia sintered body can be provided. Furthermore, according to the zirconia sintered body of the present invention, a zirconia sintered body exhibiting equivalent translucency can be obtained, and the occurrence of defects such as cracks can be suppressed, compared with a case in which a zirconia sintered body is produced by dry-processing a zirconia calcined body and then sintering it, and a dental zirconia sintered body having excellent aesthetics including translucency and useful as a dental prosthesis can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The zirconia molded body of the present invention contains zirconia, a stabilizer capable of suppressing the phase transition of zirconia, and a binder, and has an open porosity of 25% or less.
[0014] The open porosity of the zirconia molded body of the present invention is 25% or less, preferably 20% or less, more preferably 15% or less, and even more preferably 12% or less. If the open porosity exceeds 25%, the number of pores in the zirconia molded body becomes too large, and when wet processing is performed, the cooling solvent contaminated with the glass material penetrates into the zirconia molded body, and the zirconia molded body turns white after firing and cannot be used as a dental prosthesis. In addition, the open porosity is preferably 5% or more, more preferably 6% or more, even more preferably 7% or more, and particularly preferably 8% or more. If the open porosity is less than 5%, the binder is less likely to burn out in the degreasing (burning off the binder) step, and may remain. In the present invention, "open pores" means pores (pores) that communicate with the outer surface as defined in JIS Z 8890:2017. In the present invention, "open porosity" means the percentage of the volume of the open pore portion to the total volume (external volume) of the zirconia molded body. The method for measuring the open porosity in the present invention will be described in detail in the Examples below.
[0015] The zirconia molded body of the present invention contains zirconia (zirconium oxide; ZrO2). In the present invention, the "zirconia molded body" refers to a body that is formed by press molding, injection molding, stereolithography, or the like using zirconia in various forms such as powder, granules, paste, and slurry as a main raw material, and that has not yet reached either a calcined state or a sintered state. In other words, the zirconia molded body is distinguished from the zirconia calcined body and the zirconia sintered body in that it is unsintered after being formed into a molded body by molding.
[0016] The zirconia molded body of the present invention contains a stabilizer capable of suppressing the phase transition of zirconia. The stabilizer is preferably one capable of forming partially stabilized zirconia. Examples of the stabilizer include calcium oxide (CaO), magnesium oxide (MgO), yttrium oxide (Y2O3) (hereinafter referred to as "yttria"), cerium oxide (CeO2), scandium oxide (Sc2O3), niobium oxide (Nb2O5), lanthanum oxide (La2O3), erbium oxide (Er2O3), praseodymium oxide (Pr6O11 Examples of the stabilizer include oxides such as samarium oxide (Sm2O3), europium oxide (Eu2O3) and thulium oxide (Tm2O3). The stabilizer may be used alone or in combination of two or more. The content of the stabilizer in the zirconia molded body of the present invention can be measured, for example, by inductively coupled plasma (ICP) emission spectrometry, fluorescent X-ray analysis, etc. In the zirconia molded body of the present invention, the content of the stabilizer is preferably 0.1 to 18 mol%, more preferably 1 to 15 mol%, and even more preferably 2 to 8 mol%, based on the total moles of zirconia and the stabilizer.
[0017] From the viewpoint of the strength and translucency of the obtained zirconia sintered body, the zirconia molded body preferably contains yttria as a stabilizer. The content of yttria is preferably 3 mol% or more, more preferably 3.5 mol% or more, even more preferably 3.8 mol% or more, and particularly preferably 4.0 mol% or more, based on the total moles of zirconia and yttria. When the content of yttria is 3 mol% or more, the translucency of the zirconia sintered body can be increased. In addition, the content of yttria is preferably 7.5 mol% or less, more preferably 7.0 mol% or less, even more preferably 6.5 mol% or less, and particularly preferably 6.0 mol% or less, based on the total moles of zirconia and yttria. When the content of yttria is 7.5 mol% or less, the strength decrease of the obtained zirconia sintered body can be suppressed.
[0018] The zirconia molded body of the present invention contains a binder. In the zirconia molded body of the present invention, the content of the binder relative to the total mass of zirconia, the stabilizer, and the binder is preferably 3 to 10 mass%, more preferably 4 to 9 mass%, even more preferably 5 to 8 mass%, and particularly preferably 6 to 8 mass%, since a predetermined open porosity and strength can be obtained. If the binder content is less than 3 mass%, the pores in the zirconia molded body become too many, and when performing wet processing, the cooling solvent contaminated with the glass material may penetrate into the zirconia molded body, which may whiten after firing and become unusable as a dental prosthesis. In addition, if the binder content exceeds 10 mass%, the granules become too hard, causing a problem of significantly deteriorating moldability, and the binder may become difficult to burn out in the degreasing process and remain.
[0019] As the binder, a known binder generally used in the manufacture of zirconia powder or zirconia molded body can be used. Specifically, polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, polyvinyl butyrate, wax (paraffin wax, etc.), acrylic binders, etc. can be mentioned, among which acrylic binders having a carboxyl group or a derivative thereof (for example, a salt, particularly an ammonium salt, etc.) in the molecule are preferred. Examples of the acrylic binder include polyacrylic acid, polymethacrylic acid, acrylic acid copolymers, methacrylic acid copolymers, and derivatives thereof. The binder may be used alone or in combination of two or more kinds. The type of binder can be appropriately selected according to the open porosity to be set.
[0020] The zirconia molded body of the present invention preferably has a water absorption rate of 7% or less, more preferably 5% or less, even more preferably 4% or less, and particularly preferably 3% or less. If the water absorption rate exceeds 7%, a large amount of cooling solvent contaminated with glass material may penetrate into the zirconia molded body during wet processing, causing the zirconia molded body to turn white after firing and become unusable as a dental prosthesis. The method for measuring the water absorption rate in the present invention will be described in detail in the Examples below. The water absorption rate can be adjusted by appropriately selecting the content and type of binder, the pressing pressure during molding, and the like.
[0021] In the zirconia molded body of the present invention, the main crystal system of the zirconia is preferably a monoclinic system. In the present invention, the term "main crystal system is a monoclinic system" refers to the ratio f of the monoclinic system in the zirconia to the total amount of all crystal systems (monoclinic system, tetragonal system, and cubic system) in the zirconia. m The proportion of monoclinic crystals f is 50% or more. m is preferably 55% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 75% or more, particularly preferably 80% or more, even more particularly preferably 85% or more, and most preferably 90% or more. In the zirconia molded body of the present invention, the peaks of the tetragonal and cubic crystal systems may not be substantially detected. That is, the monoclinic crystal ratio f m The monoclinic ratio f can be 100%. m can be calculated from the following formula (1) based on the peaks of the X-ray diffraction (XRD) pattern using CuKα radiation. The main crystal system in the zirconia molded body may contribute to the increase in the shrinkage temperature and the shortening of the firing time.
[0022]
number
[0023] In formula (1), I m (111) and I m(11-1) indicates the peak intensity of the (111) and (11-1) planes of the monoclinic crystal system of zirconia, respectively. t (111) indicates the peak intensity of the (111) plane of the zirconia tetragonal crystal system. I c (111) indicates the peak intensity of the (111) plane of the cubic crystal system of zirconia.
[0024] In the zirconia molded body of the present invention, the stabilizer is preferably present such that at least a part of the zirconia crystal is monoclinic. That is, at least a part of the stabilizer is preferably not solid-dissolved in zirconia. The fact that a part of the stabilizer is not solid-dissolved in zirconia can be confirmed, for example, by an XRD pattern. When a peak derived from the stabilizer is confirmed in the XRD pattern of the zirconia molded body, it means that the stabilizer that is not solid-dissolved in zirconia is present in the zirconia molded body. When the entire amount of the stabilizer is solid-dissolved, basically, no peak derived from the stabilizer is confirmed in the XRD pattern. However, depending on conditions such as the crystal state of the stabilizer, even if there is no stabilizer peak in the XRD pattern, the stabilizer may not be solid-dissolved in zirconia. When the main crystal system of zirconia is tetragonal and / or cubic and there is no stabilizer peak in the XRD pattern, it is considered that most of the stabilizer, basically all of it, is solid-dissolved in zirconia. In the zirconia molded body of the present invention, the stabilizer does not have to be entirely dissolved in zirconia. In the present invention, the stabilizer being dissolved in solid solution means, for example, that an element (atom) contained in the stabilizer is dissolved in solid solution in zirconia.
[0025] The zirconia molded body of the present invention may contain additives as necessary. Examples of additives include colorants (including pigments, composite pigments, and fluorescent pigments), alumina (Al2O3), titanium oxide (TiO2), silica (SiO2), etc. The additives may be used alone or in combination of two or more.
[0026] The pigment may be, for example, an oxide of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, Tb and Er (specifically, NiO, Cr2O3, etc.), and is preferably an oxide of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd and Tb, and more preferably an oxide of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Sm, Eu, Gd and Tb. The zirconia molded body of the present invention may not contain erbium oxide (Er2O3). Examples of the composite pigment include composite oxides such as (Zr,V)O2, Fe(Fe,Cr)2O4, (Ni,Co,Fe)(Fe,Cr)2O4·ZrSiO4, and (Co,Zn)Al2O4. Examples of the fluorescent pigment include Y2SiO5:Ce, Y2SiO5:Tb, (Y,Gd,Eu)BO3, Y2O3:Eu, YAG:Ce, ZnGa2O4:Zn, BaMgAl 10 O 17 :Eu, etc.
[0027] From the viewpoint of machinability and free machinability, the zirconia molded body of the present invention preferably has a biaxial bending strength that satisfies a specific range. Specifically, the biaxial bending strength is preferably 7 to 30 MPa, more preferably 8 to 25 MPa, and even more preferably 9 to 19 MPa. Examples of a method for measuring the biaxial bending strength include the method described in the Examples below.
[0028] The method for producing the zirconia molded body of the present invention is not particularly limited as long as it exhibits the effects of the present invention. For example, zirconia, a stabilizer, and a binder are wet-mixed in water to form a slurry. Next, the slurry is dried and granulated. Thereafter, the granulated product is press-molded to obtain a zirconia molded body. The binder may be added to the slurry obtained by adding a primary powder consisting of a mixture of zirconia powder and a stabilizer to water to form a slurry, and then pulverizing the slurry. In this case, after adding the binder to the slurry, the slurry is dried, and the obtained granulated product (secondary powder) is press-molded to obtain a zirconia molded body. As a method for press-molding the granulated product, a known method is used without any restrictions, and may include, for example, a uniaxial press molding step and / or a cold isostatic pressing (CIP) step. As the uniaxial press molding step, a method in which zirconia is filled into a press mold (die) of a desired size and pressed by uniaxial pressing using an upper punch and a lower punch is suitable. The pressing pressure is set to an appropriate optimum value depending on the size, open porosity, water absorption, biaxial bending strength, and zirconia particle size of the target molded body, and is usually 10 MPa to 1000 MPa. By increasing the pressing pressure during molding in the above-mentioned production method, the pores of the obtained zirconia molded body are filled more, and the open porosity can be set low.
[0029] Another embodiment of the present invention includes a zirconia sintered body obtained by firing the zirconia molded body. By using the zirconia molded body of the present invention, a zirconia sintered body (e.g., a dental prosthesis) having excellent translucency can be easily manufactured in a single firing step without going through a complicated process of calcining the zirconia molded body at a temperature range of about 800 to 1200 ° C to obtain a calcined body, cooling the calcined body, processing (e.g., cutting, etc.) into a desired shape (e.g., a dental crown shape, etc.) as necessary, and firing the calcined body again. The firing (sintering) step of the zirconia molded body preferably includes a degreasing step (burning and removing the binder) by heating the zirconia molded body at a temperature range of 800 ° C or less before reaching the maximum firing temperature.
[0030] A general dental porcelain firing furnace can be used for the firing (sintering) process of the zirconia molded body and the dental mill blank. A commercially available product may be used as the dental porcelain firing furnace. Examples of commercially available products include Noritake Katana (registered trademark) F-1N and Noritake Katana (registered trademark) F-2 (both of which are manufactured by SK Medical Electronics Co., Ltd.). The retention time for holding the zirconia molded body in the dental porcelain firing furnace is preferably 1 to 140 minutes. The temperature of the sintering process is not particularly limited, but it is preferable to perform the sintering process at a maximum firing temperature of 1400 to 1600°C. When the main firing is a short-time firing, the retention time for holding the zirconia molded body in the firing furnace is preferably less than 30 minutes at the maximum firing temperature, more preferably 20 minutes or less, and even more preferably 15 minutes or less. According to the present invention, even when wet processing is performed using a dental CAD / CAM system using a contaminated cooling solvent, not only in the case of normal firing but also in the case of short-time firing, the decrease in the translucency of the zirconia sintered body can be suppressed.
[0031] Another embodiment of the present invention is a dental mill blank made of the zirconia molded body. The zirconia molded body of the present invention can be used as a dental material, and can be particularly suitably used as a dental mill blank. In one embodiment, the dental mill blank of the present invention can be obtained by processing the zirconia molded body in an unfired state. The dental mill blank is processed (e.g., cut or cut) into a desired size and shape (e.g., disk-like, rectangular, etc.) as necessary, and then surface-polished and shipped as a product. The size of the dental mill blank of the present invention is preferably molded or processed after molding to an appropriate size that can be set in a commercially available dental CAD / CAM system. Examples of preferred sizes include, for example, a 40mm x 20mm x 15mm prism suitable for making a one-tooth missing bridge, a 17mm x 10mm x 10mm prism suitable for making an inlay or onlay, a 14mm x 18mm x 20mm prism suitable for making a full crown, and a disk shape with a diameter of 100mm and a thickness of 10 to 28mm suitable for making a long span bridge or denture base, but are not limited to these sizes. The dental mill blank of the present invention has improved strength due to the large amount of binder in the zirconia molded body, and can be cut without problems using a general dental CAD / CAM system before firing.
[0032] Examples of dental prostheses manufactured by firing the dental mill blank of the present invention include crown restorations such as inlays, onlays, veneers, crowns, and bridges, as well as abutments, dental posts, dentures, denture bases, and implant components (fixtures and abutments). The cutting process is preferably performed using a commercially available dental CAD / CAM system. Examples of such CAD / CAM systems include the CEREC system manufactured by Dentsply Sirona Inc. and the Katana (registered trademark) system manufactured by Kuraray Noritake Dental Co., Ltd.
[0033] Furthermore, the zirconia molded article of the present invention can be used for applications other than dental applications, such as electronic materials applications such as sealing materials and laminate molding materials, general-purpose composite material members, construction materials, electrical appliances, household goods, and toys.
[0034] The present invention includes embodiments in which the above configurations are combined in various ways within the scope of the technical concept of the present invention, as long as the effects of the present invention are achieved. EXAMPLES
[0035] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples, and many modifications within the scope of the technical concept of the present invention are possible by those having ordinary skill in the art.
[0036] [Preparation of zirconia raw powder] A method for producing the raw powder used to produce the zirconia molded body of each Example and Comparative Example will be described. First, a mixture was produced using approximately 100% monoclinic zirconia powder and yttria powder such that the content of yttria was 6 mol% relative to the total moles of zirconia and yttria. Next, this mixture was added to water to produce a slurry, which was wet-pulverized and mixed in a ball mill until the average particle size was 0.13 μm or less. The pulverized slurry was dried with a spray dryer, and the obtained powder was fired at 950° C. for 2 hours to produce a powder (primary powder). The average particle size can be determined by a laser diffraction scattering method. Specifically, the laser diffraction scattering method can be measured on a volume basis using a laser diffraction particle size distribution analyzer (SALD-2300: manufactured by Shimadzu Corporation) using a 0.2% sodium hexametaphosphate aqueous solution as a dispersion medium.
[0037] The obtained primary powder was added to water to prepare a slurry, which was then wet-pulverized and mixed in a ball mill until the average particle size was 0.13 μm or less. A binder (acrylic binder, Japan Coating Resin Co., Ltd. "SA-200") was added to the pulverized slurry in the amount shown in Table 1, and the mixture was dried in a spray dryer to prepare granules (secondary powder). The prepared granules were used as raw powder to manufacture the zirconia molded body described below.
[0038] [Preparation of zirconia compact] The raw material powder was placed in a cylindrical mold having a diameter of about 15 mm so that the thickness of the zirconia sintered body after sintering would be 1.3 to 1.5 mm. Next, the zirconia powder was press-molded under a load of 100 kN to obtain a zirconia molded body.
[0039] [Measurement of open porosity and water absorption rate of zirconia compact] The open porosity and water absorption rate of the zirconia molded bodies of each Example and Comparative Example were calculated based on the following formula using the dry mass (M1), the mass in water (M2), and the wet mass (M3) measured by the Archimedes method. Open porosity (%)=100×(M3-M1) / (M3-M2) Water absorption rate (%)=100×(M3-M1) / M1 Measurements using the Archimedes method were performed using a density measurement kit (ML-DNY-43) attached to an electronic balance (ML204 / 02) manufactured by Mettler Toledo. The underwater mass (M2) is the mass of a dried zirconia molded body measured while it was suspended in water after immersing it in water for 1 hour. The water-containing mass (M3) is the mass of a dried zirconia molded body measured after immersing it in water for 1 hour, removing the zirconia molded body from the water after measuring the underwater mass (M2), removing water droplets from the surface of the zirconia molded body, and filling the open pores of the sample with water. The open porosity and water absorption obtained are shown in Table 1.
[0040] [Translucency evaluation of zirconia sintered body] For the zirconia molded bodies of each Example and Comparative Example, a sintering furnace "Noritake Katana (registered trademark) F-1" manufactured by SK Medical Electronics Co., Ltd. was used to perform main sintering including a degreasing process at 1550 ° C. for 15 minutes to obtain a zirconia sintered body sample. Both sides of the obtained sample were polished with #600 to obtain a zirconia sintered body having a thickness of 1.2 mm, and the translucency was evaluated by the following method (n = 3). As a measuring device, a dental color measuring device "Crystal Eye" (7band LED light source) manufactured by Olympus Corporation was used, and first, the background (underlay) of the sample was made white (the opposite side of the measuring device with respect to the sample was made white) and the L * value of the L * a * b * color system (JIS Z 8781-4: 2013 Colorimetry-Part 4: CIE 1976 L * a * b * color space) was measured, and this was taken as the first L * value. Next, for the same sample that was used to measure the first L* value, the background (backing) of the sample is made black (the side opposite the measuring device is made black relative to the sample) and the L* value in the L*a*b* color system is measured, and this is used as the second L* value. In the present invention, the difference between the first L* value and the second L* value (the value obtained by subtracting the second L* value from the first L* value) is regarded as the translucency, and is expressed as ΔL*. A high ΔL* indicates high translucency, and a low ΔL* indicates low translucency. For the black and white background (underlay) in the chromaticity measurement, the hiding power test paper used in the measurement of paints described in JIS K 5600-4-1:1999 can be used. The measurement results (average value) of the translucency of the zirconia sintered body by short-time firing using this measurement method are shown in Table 1 as "Translucency (ΔL*) when fired by normal method".
[0041] [Evaluation of the translucency of zirconia sintered bodies after immersion in a contaminated cooling solvent and then firing] In order to confirm the influence of the contaminated cooling solvent on the translucency of the zirconia sintered body, the translucency of the zirconia sintered body was evaluated by the following method. First, a glass material (e.max: Ivoclar Vivadent) was wet-cut 25 times using a dry and wet dual-purpose processing machine (Cerec MCXL: manufactured by Dentsply Sirona Co., Ltd.) to prepare a contaminated cooling solvent (processing fluid (hydrophilic solvent whose main component is water), product name: DENTATEC, manufactured by Dentsply Sirona Co., Ltd.). Next, in order to reproduce the state in which the contaminated processing fluid comes into contact during wet cutting, the prepared processing fluid was placed in a container, and the samples of the zirconia molded bodies of each Example and Comparative Example were immersed for 15 minutes, which is equivalent to the processing time of an actual dental prosthesis, to allow the processing fluid to penetrate the samples (n=3). Next, a sintering furnace "Noritake Katana (registered trademark) F-1" manufactured by SK Medical Electronics Co., Ltd. was used to hold the samples at 1550 ° C. for 15 minutes as the main firing, to obtain a sample of the zirconia sintered body. The light transmittance ΔL* of the obtained samples was measured in the same manner as described above. The average values are shown in Table 1 as the measurement results.
[0042] [Strength evaluation of zirconia compacts] Separately from the preparation of the above zirconia molded bodies, strength measurement samples were prepared for the zirconia molded bodies of each of the Examples and Comparative Examples so that the size of the zirconia molded body was about 15 mm in diameter and 1.2 mm in thickness, and the biaxial bending strength was measured (n=5) using a universal testing machine (manufactured by Instron) with a crosshead speed set to 0.5 mm / min in accordance with ISO6872:2015. The average values are shown in Table 1 as the measurement results.
[0043] [Table 1]
[0044] The zirconia molded bodies of Examples 1 to 5 have an open porosity of 25% or less, and even when immersed in a contaminated cooling solvent, the penetration of the contaminated cooling solvent into the pores is suppressed, so that the translucency after sintering is maintained. On the other hand, the zirconia molded body of Comparative Example 1 has a high open porosity of 28%, so that the contaminated cooling solvent penetrates into the pores, and the translucency of the sintered body is greatly reduced, and the strength is also lower than that of the Examples. In addition, the zirconia molded body of Comparative Example 2 has an open porosity of more than 25% and contains too much binder, so that the moldability is deteriorated, the granules are not sufficiently crushed during pressing, and the translucency is deteriorated when sintered by a normal method, and when immersed in a contaminated cooling solvent, the translucency is further reduced and the strength is further lower.
[0045] With respect to numerical ranges set forth herein, unless otherwise stated, any numerical value or range falling within the range should be construed as being specifically set forth herein. [Industrial Applicability]
[0046] The zirconia molded body of the present invention can be suitably used for dental products for producing dental prostheses and the like.
Claims
[Claim 1] wet processing the zirconia compact; The zirconia molded body, The composition contains zirconia, a stabilizer capable of suppressing a phase transition of the zirconia, and a binder, The binder content is 4 to 10% by mass, A method for producing a zirconia sintered body having an open porosity of 25% or less.
Citation Information
Patent Citations
Colored and light-transmitting sintered zirconia compact and use of the same
JP2013049616A
Zirconia calcined body for dentistry
JP2019108289A
Zirconia sintered body, and mixture, pre-sintered compact and pre-sintered calcined body for sintering zirconia sintered body
WO2011021698A1
Zirconia sintered body, zirconia composition and zirconia calcined body, production method of these, and dental prosthesis
WO2014181828A1
Zirconia composition, calcined object and sintered compact, and method for producing same