Electrophotographic photoreceptor, process cartridge, and image forming apparatus

The electrophotographic photoreceptor addresses axial image density variations by using a vinyl copolymer with specific structural units to stabilize the charge transport layer adherence, ensuring consistent sensitivity and image quality.

JP7567649B2Active Publication Date: 2024-10-16FUJIFILM BUSINESS INNOVATION CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021082267
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-14
Publication Date
2024-10-16
Estimated Expiration
2041-05-14

AI Technical Summary

Technical Problem

The existing electrophotographic photoreceptors experience differences in image density along the axial direction due to variations in the adherence time of the charge transport layer coating solution, leading to inconsistencies in electrical properties and sensitivity.

Method used

The photoreceptor is designed with a charge generation layer composed of a charge generation material and a vinyl copolymer containing a chlorine-containing structural unit, an acyloxy group-containing structural unit, and an aromatic polycarboxylic acid structure, with specific ratios of these components to enhance solvent resistance and dispersibility, thereby stabilizing the vinyl copolymer and maintaining consistent image density.

Benefits of technology

This configuration suppresses image density differences in the axial direction while maintaining high sensitivity by ensuring the vinyl copolymer's stability and dispersibility, resulting in uniform image quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567649000019
    Figure 0007567649000019
  • Figure 0007567649000020
    Figure 0007567649000020
  • Figure 0007567649000021
    Figure 0007567649000021
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor that prevents a difference in image density in an axial direction of the electrophotographic photoreceptor.SOLUTION: An electrophotographic photoreceptor has: a conductive substrate; a charge generating layer that is provided on the conductive substrate and contains a charge generating material and a vinyl-based copolymer, wherein the vinyl-based copolymer includes a constitutional unit having chlorine, a constitutional unit having an acyloxy group, and a constitutional unit having an aromatic polycarboxylic acid structure, the ratio of the constitutional unit having chlorine to all the constitutional units is 80 mass% or more, and the ratio of the constitutional unit having an aromatic polycarboxylic acid structure to all the constitutional units is 0.5 mass% or more; and a charge transport layer that is provided on the charge generating layer and contains a charge transport material and a binder resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor, a process cartridge, and an image forming apparatus. [Background technology]

[0002] Patent Document 1 discloses an electrophotographic photoreceptor having a laminated photosensitive layer composed of at least a charge generation layer and a charge transport layer on a conductive support, characterized in that the charge generation layer contains a moisture absorbent composed of a polybasic acid compound having two or more carboxyl groups in the molecule. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-19507 Summary of the Invention [Problem to be solved by the invention]

[0004] In an electrophotographic photoreceptor having a charge generation layer and a charge transport layer provided in this order on a conductive substrate, for example, a charge generation layer is formed on the conductive substrate, and then a coating liquid for forming a charge transport layer containing a solvent is applied onto the charge generation layer and dried to form a charge transport layer. When the charge generation layer contains a charge generation material and a vinyl copolymer, when the coating liquid for forming a charge transport layer is applied onto the charge generation layer, a part of the vinyl copolymer in the charge generation layer may be dissolved by the solvent in the coating liquid for forming a charge transport layer.

[0005] In the process of applying the coating liquid for forming the charge transport layer onto the charge generation layer, a dip coating method is generally used. In the dip coating method, a conductive substrate having a charge generation layer formed on its outer peripheral surface is immersed in the coating liquid for forming the charge transport layer with one axial end of the conductive substrate facing downward, and then pulled up. As a result, the coating liquid for forming the charge transport layer is attached onto the charge generation layer. Therefore, the time when the coating liquid for forming the charge transport layer adheres to the charge generating layer differs between the lower end and the upper end in the axial direction of the conductive substrate, which may result in a difference in electrical properties between one end and the other end in the axial direction of the electrophotographic photoreceptor, and a difference in sensitivity among the electrical properties may appear as a difference in image density.

[0006] The present invention aims to provide an electrophotographic photoreceptor in which, when a charge generation layer comprises a charge generation material and a vinyl-based copolymer, the vinyl-based copolymer comprises a chlorine-containing structural unit, an acyloxy group-containing structural unit, and a structural unit derived from maleic acid, the image density difference in the axial direction of the electrophotographic photoreceptor is suppressed compared to when the proportion of the chlorine-containing structural units to all structural units is less than 80 mass%, when the proportion of the structural units having an aromatic polycarboxylic acid structure to all structural units is less than 0.5 mass%, or when the solubility of the vinyl-based copolymer in 100 parts by mass of tetrahydrofuran exceeds 10 parts by mass. [Means for solving the problem]

[0007] Specific means for solving the above problems include the following aspects.

[0008] <1> A conductive substrate; a charge generating layer provided on the conductive substrate, the charge generating layer comprising a charge generating material and a vinyl copolymer, the vinyl copolymer comprising a chlorine-containing structural unit, an acyloxy group-containing structural unit, and an aromatic polycarboxylic acid structure-containing structural unit, the proportion of the chlorine-containing structural unit to all structural units being 80 mass% or more, and the proportion of the aromatic polycarboxylic acid structure-containing structural unit to all structural units being 0.5 mass% or more; a charge transport layer provided on the charge generating layer and containing a charge transport material and a binder resin; An electrophotographic photoreceptor comprising: <2> The proportion of the chlorine-containing structural units is 88 mass% or less based on all structural units constituting the vinyl copolymer. <1> The electrophotographic photoreceptor according to claim 1. <3> The proportion of the chlorine-containing structural units is 80% by mass or more and 87% by mass or less with respect to all structural units constituting the vinyl copolymer. <2> The electrophotographic photoreceptor according to claim 1.

[0009] <4> A conductive substrate; a charge generating layer provided on the conductive substrate, the charge generating layer containing a charge generating material and a vinyl copolymer, the vinyl copolymer containing a chlorine-containing structural unit, an acyloxy group-containing structural unit, and an aromatic polycarboxylic acid structure-containing structural unit, the solubility of the vinyl copolymer being 10 parts by mass or less in 100 parts by mass of tetrahydrofuran at 30° C.; a charge transport layer provided on the charge generating layer and containing a charge transport material and a binder resin; An electrophotographic photoreceptor comprising:

[0010] <5> When the ratio of the constituent units having the aromatic polycarboxylic acid structure to all constituent units constituting the vinyl copolymer is A% by mass and the content of the charge generating material in the vinyl copolymer is C% by mass, the value of A / C is 3.00×10 -3 Above 1.40 x 10 -2 Below is the <1> ~ <4> 13. The electrophotographic photoreceptor according to claim 12, <6> The structural unit having chlorine is represented by the following general formula (1), and the structural unit having an acyloxy group is represented by the following general formula (2): <1> ~ <5> 13. The electrophotographic photoreceptor according to claim 12,

[0011] [ka]

[0012] In the general formula (1), R 11 ~R 13each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; 21 ~R 23 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; R 24 represents an alkyl group having 1 to 5 carbon atoms. <7> R in the general formula (1) 11 ~R 13 are all hydrogen atoms, and R 21 ~R 23 are all hydrogen atoms, R 24 is a methyl group; <6> The electrophotographic photoreceptor according to claim 1. <8> the structural unit having an aromatic polycarboxylic acid structure is a structural unit having a phthalic acid structure; <1> ~ <7> 13. The electrophotographic photoreceptor according to claim 12, <9> <1> ~ <8> The electrophotographic photoreceptor according to any one of the above items is provided, A process cartridge that is detachably attached to an image forming apparatus. <10> <1> ~ <8> and an electrophotographic photoreceptor according to any one of the above items. a charging means for charging the surface of the electrophotographic photoreceptor; an electrostatic latent image forming means for forming an electrostatic latent image on the charged surface of the electrophotographic photoreceptor; a developing unit for developing an electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing a toner to form a toner image; a transfer means for transferring the toner image onto a surface of a recording medium; An image forming apparatus comprising: Effect of the Invention

[0013] <1> According to the invention, when the charge generation layer comprises a charge generation material and a vinyl copolymer, and the vinyl copolymer comprises a chlorine-containing structural unit, an acyloxy group-containing structural unit, and a structural unit derived from maleic acid, an electrophotographic photoreceptor is provided in which the image density difference in the axial direction of the electrophotographic photoreceptor is suppressed compared to when the proportion of the chlorine-containing structural units to all structural units is less than 80 mass%, or when the proportion of the structural units having an aromatic polycarboxylic acid structure to all structural units is less than 0.5 mass%. <2> According to the invention relating to the above, an electrophotographic photoreceptor having higher sensitivity is provided, as compared with a case in which the proportion of structural units having chlorine exceeds 88 mass %. <3> According to the present invention, an electrophotographic photoreceptor is provided which achieves both suppression of image density differences in the axial direction of the electrophotographic photoreceptor and high sensitivity, as compared with a case in which the proportion of chlorine-containing structural units is less than 80% by mass or more than 87% by mass.

[0014] <4> According to the invention, there is provided an electrophotographic photoreceptor in which the charge generation layer comprises a charge generation material and a vinyl copolymer, and in which the image density difference in the axial direction of the electrophotographic photoreceptor is suppressed compared to a case in which the solubility of the vinyl copolymer in 100 parts by mass of tetrahydrofuran is more than 10 parts by mass.

[0015] <5> According to the invention, the A / C value is 3.00×10 -3 As a result, an electrophotographic photoreceptor is provided in which the image density difference in the axial direction of the electrophotographic photoreceptor is suppressed, as compared with the case where the axial direction of the electrophotographic photoreceptor is smaller than the above. <6> , <7> or <8> According to the invention, there is provided an electrophotographic photoreceptor in which the image density difference in the axial direction of the electrophotographic photoreceptor is suppressed, as compared with a case in which the vinyl-based copolymer is composed of a chlorine-containing structural unit, an acyloxy group-containing structural unit, and a structural unit derived from maleic acid.

[0016] <9> or <10> According to the invention, there is provided a process cartridge or an image forming apparatus equipped with an electrophotographic photosensitive member in which the image density difference in the axial direction of the electrophotographic photosensitive member is suppressed compared to when the vinyl-based copolymer is composed of a chlorine-containing structural unit, an acyloxy group-containing structural unit, and a structural unit derived from maleic acid. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a schematic partial cross-sectional view showing an example of a layer structure of the electrophotographic photoreceptor according to the present embodiment. [Diagram 2] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 3] FIG. 11 is a schematic configuration diagram illustrating another example of an image forming apparatus according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described as an example. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.

[0019] Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.

[0020] [Electrophotographic photoreceptor] First embodiment The electrophotographic photoreceptor (hereinafter also referred to as "photoreceptor") according to the first embodiment has a conductive substrate, a charge generation layer provided on the conductive substrate and containing a charge generation material and a vinyl-based copolymer, and a charge transport layer provided on the charge generation layer and containing a charge transport material and a binder resin. The vinyl copolymer contains a structural unit having chlorine (hereinafter also referred to as a "chlorine-containing component"), a structural unit having an acyloxy group (hereinafter also referred to as an "acyloxy component"), and a structural unit having an aromatic polycarboxylic acid structure (hereinafter also referred to as an "aromatic polycarboxylic acid component"). In the vinyl copolymer, the proportion of the chlorine-containing component to all structural units is 80% by mass or more, and the proportion of the aromatic polycarboxylic acid component to all structural units is 0.5% by mass or more.

[0021] Here, the "chlorine-containing component (i.e., a structural unit having chlorine)" is a structural unit that has a chlorine atom and does not have an acyloxy group or two or more carboxy groups, and may have other substituents (e.g., alkyl groups, etc.). The "acyloxy component (i.e., a structural unit having an acyloxy group)" may be a structural unit that has an acyloxy group and does not have two or more carboxy groups, and may have other substituents (e.g., alkyl groups, etc.). The "aromatic polycarboxylic acid component (i.e., a structural unit having an aromatic polycarboxylic acid structure)" may be a structural unit that has an aromatic polycarboxylic acid structure, and may have a substituent other than a carboxy group (e.g., alkyl groups, etc.).

[0022] The photoconductor according to the first embodiment has the above-mentioned configuration, and thus the image density difference in the axial direction of the photoconductor is suppressed. The reason for this is presumed to be as follows. As described above, when forming a charge transport layer on a charge generation layer provided on a conductive substrate, the charge transport layer forming coating liquid is generally applied on the charge generation layer by a dip coating method, and then dried to form the charge transport layer. At this time, a part of the vinyl copolymer contained in the charge generation layer may be dissolved by the solvent in the charge transport layer forming coating liquid. In the dip coating method, the time when the charge transport layer forming coating liquid is attached to the charge generation layer differs between the lower end and the upper end in the axial direction of the conductive substrate. Therefore, there may be a difference in sensitivity between one end and the other end in the axial direction of the photoreceptor, and the difference in sensitivity may appear as a difference in image density.

[0023] In contrast, in the first embodiment, the proportion of the chlorine-containing component to all structural units in the vinyl copolymer is 80% by mass or more, and the proportion of the aromatic polycarboxylic acid component to all structural units is 0.5% by mass or more. It is believed that the proportion of the chlorine-containing component is 80% by mass or more and the proportion of the aromatic polycarboxylic acid component is 0.5% by mass or more, so that the vinyl copolymer is less likely to dissolve in the solvent in the coating liquid for forming the charge transport layer. Specifically, when the vinyl copolymer contains an aromatic polycarboxylic acid component, the compound stability of the vinyl copolymer is higher than that of the vinyl copolymer containing a constituent unit derived from an aliphatic polycarboxylic acid such as maleic acid instead of the aromatic polycarboxylic acid component, and the vinyl copolymer is less likely to dissolve in a solvent. Similarly, when the vinyl copolymer contains an aromatic polycarboxylic acid component of 0.5% by mass or more, the vinyl copolymer is less likely to dissolve in a solvent than that of the vinyl copolymer containing an aromatic polycarboxylic acid component of less than 0.5% by mass. Furthermore, when the vinyl copolymer contains a chlorine-containing component of 80% by mass or more, the hardness of the vinyl copolymer is higher than that of the vinyl copolymer containing a chlorine-containing component of less than 80% by mass, and the vinyl copolymer is less likely to dissolve in a solvent.

[0024] Furthermore, since the vinyl copolymer is not easily dissolved in a solvent, even if the time it takes for the coating liquid for forming the charge transport layer to adhere to the charge generation layer during the dip coating method differs between the lower end and the upper end in the axial direction of the conductive substrate, differences in sensitivity are unlikely to occur, and it is presumed that the resulting differences in image density in the axial direction of the photoreceptor are suppressed. For the above reasons, it is presumed that the photoconductor according to the first embodiment suppresses the image density difference in the axial direction of the photoconductor.

[0025] In addition, since the binder resin of the charge generation layer is easily dissolved in a solvent, a photoreceptor with high sensitivity may be easily obtained. Specifically, since the binder resin in the charge generation layer is dissolved by the solvent in the coating liquid for forming the charge transport layer, the charge generation material is easily present at the interface between the charge generation layer and the charge transport layer. And, the more the charge generation material is present at the interface between the charge generation layer and the charge transport layer, the higher the sensitivity of the photoreceptor is. In contrast, in the first embodiment, even if the vinyl copolymer is not easily dissolved in the solvent, high sensitivity is obtained. The reason is not clear, but is speculated as follows. Specifically, first, it is considered that the acyloxy component contained in the vinyl copolymer enhances the dispersibility of the charge generating material in the vinyl copolymer. In addition, in the first embodiment, it is considered that the dispersibility of the charge generating material in the vinyl copolymer is further enhanced by using the acyloxy component in combination with the aromatic polycarboxylic acid component. Then, it is speculated that the charge generating material is dispersed near the interface with the charge transport layer by increasing the dispersibility of the charge generating material in the vinyl copolymer, even if the vinyl copolymer is not easily dissolved in the solvent, thereby obtaining high sensitivity. In other words, the photoconductor according to the first embodiment obtains high sensitivity while suppressing the image density difference in the axial direction of the photoconductor.

[0026] Second Embodiment The photoreceptor according to the second embodiment has a conductive substrate, a charge generation layer provided on the conductive substrate and containing a charge generation material and a vinyl copolymer, and a charge transport layer provided on the charge generation layer and containing a charge transport material and a binder resin. The vinyl copolymer contains a chlorine-containing component, an acyloxy component, and an aromatic polycarboxylic acid component, and has a solubility of 100 parts by mass of tetrahydrofuran at 30°C (hereinafter also referred to as "THF solubility") of 10 parts by mass or less.

[0027] The photoconductor according to the second embodiment has the above-mentioned configuration, and thus the image density difference in the axial direction of the electrophotographic photoconductor is suppressed. The reason for this is presumed to be as follows. As described above, when forming a charge transport layer on a charge generation layer provided on a conductive substrate, the charge transport layer forming coating liquid is generally applied on the charge generation layer by a dip coating method, and then dried to form the charge transport layer. At this time, a part of the vinyl copolymer contained in the charge generation layer may be dissolved by the solvent in the charge transport layer forming coating liquid. In the dip coating method, the time when the charge transport layer forming coating liquid is attached to the charge generation layer differs between the lower end and the upper end in the axial direction of the conductive substrate. Therefore, there may be a difference in sensitivity between one end and the other end in the axial direction of the electrophotographic photoreceptor, and the difference in sensitivity may appear as a difference in image density.

[0028] In contrast, in the second embodiment, the vinyl copolymer contains an aromatic polycarboxylic acid component and has a THF solubility of 10 parts by mass or less, which is considered to make the vinyl copolymer less soluble in a solvent. Furthermore, since the vinyl copolymer is not easily dissolved in a solvent, even if the time it takes for the coating liquid for forming the charge transport layer to adhere to the charge generation layer in a dip coating method differs between the lower end and the upper end in the axial direction of the conductive substrate, differences in sensitivity are unlikely to occur, and it is presumed that the resulting differences in image density in the axial direction of the electrophotographic photosensitive member are suppressed. For the above reasons, it is presumed that the photoconductor according to the second embodiment suppresses the image density difference in the axial direction of the electrophotographic photoconductor.

[0029] In the second embodiment, even if the vinyl copolymer is not easily dissolved in the solvent, high sensitivity is obtained. Specifically, it is considered that the acyloxy component contained in the vinyl copolymer enhances the dispersibility of the charge generating material in the vinyl copolymer, and the dispersibility of the charge generating material in the vinyl copolymer is further enhanced by using the acyloxy component in combination with the aromatic polycarboxylic acid component. It is also speculated that the charge generating material is dispersed near the interface with the charge transport layer by increasing the dispersibility of the charge generating material in the vinyl copolymer, even if the vinyl copolymer is not easily dissolved in the solvent, thereby obtaining high sensitivity. In other words, the photoconductor according to the second embodiment obtains high sensitivity while suppressing the image density difference in the axial direction of the photoconductor.

[0030] Hereinafter, a photoreceptor that corresponds to both the photoreceptor according to the first embodiment and the photoreceptor according to the second embodiment will be referred to as a "photoreceptor according to this embodiment." However, an example of the photoreceptor of the present invention may be a photoreceptor that corresponds to at least one of the photoreceptor according to the first embodiment and the photoreceptor according to the second embodiment.

[0031] Hereinafter, the electrophotographic photoreceptor according to the present embodiment will be described with reference to the drawings. Fig. 1 is a schematic partial cross-sectional view showing an example of the layer structure of an electrophotographic photoreceptor 7A according to the present embodiment. The electrophotographic photoreceptor 7A shown in Fig. 1 has a structure in which an undercoat layer 1, a charge generation layer 2, and a charge transport layer 3 are laminated in this order on a conductive substrate 4. The charge generation layer 2 and the charge transport layer 3 constitute a photosensitive layer 5.

[0032] The undercoat layer 1 is a layer that is provided as needed. That is, in the electrophotographic photoreceptor 7A, the charge generating layer 2 may be provided directly on the conductive substrate 4 (that is, without the undercoat layer 1). Furthermore, the electrophotographic photoreceptor 7A may be provided with other layers as necessary. Examples of the other layers include a protective layer further provided on the charge transport layer 3.

[0033] Hereinafter, each layer of the electrophotographic photoreceptor according to the present embodiment will be described in detail, with the reference numerals omitted.

[0034] (Conductive substrate) Examples of conductive substrates include metal plates, metal drums, and metal belts containing metals (aluminum, copper, zinc, chromium, nickel, molybdenum, vanadium, indium, gold, platinum, etc.) or alloys (stainless steel, etc.). Examples of conductive substrates include paper, resin films, belts, etc. coated, vapor-deposited, or laminated with conductive compounds (e.g., conductive polymers, indium oxide, etc.), metals (e.g., aluminum, palladium, gold, etc.) or alloys. Here, "conductive" refers to a material having a volume resistivity of 10 13 This means that the resistance is less than Ωcm.

[0035] When the electrophotographic photoreceptor is used in a laser printer, the surface of the conductive substrate is preferably roughened to a center line average roughness Ra of 0.04 μm to 0.5 μm in order to suppress interference fringes that occur when irradiating with laser light. When non-interfering light is used as the light source, roughening to prevent interference fringes is not particularly necessary, but it is suitable for extending the life of the conductive substrate since it suppresses the occurrence of defects due to unevenness on the surface.

[0036] Examples of methods for roughening the surface include wet honing, which involves spraying an abrasive suspended in water onto the support, centerless grinding, in which a conductive substrate is pressed against a rotating grindstone and continuously ground, and anodizing.

[0037] As a method for roughening the surface, there can be mentioned a method in which, without roughening the surface of the conductive substrate, a conductive or semiconductive powder is dispersed in a resin to form a layer on the surface of the conductive substrate, and the surface is roughened by the particles dispersed in the layer.

[0038] In the roughening treatment by anodization, an oxide film is formed on the surface of a conductive substrate made of metal (e.g., aluminum) by anodizing the substrate in an electrolyte solution using the substrate as the anode. Examples of electrolyte solutions include sulfuric acid solution and oxalic acid solution. However, the porous anodic oxide film formed by anodization is chemically active in its original state, easily contaminated, and has a large resistance variation depending on the environment. Therefore, it is preferable to perform a sealing treatment on the porous anodic oxide film, in which the micropores of the oxide film are filled by volume expansion caused by hydration reaction in pressurized steam or boiling water (metal salts such as nickel may be added) to change the film into a more stable hydrated oxide.

[0039] The thickness of the anodic oxide film is preferably, for example, from 0.3 μm to 15 μm. If the thickness is within this range, the film tends to exhibit a barrier property against injection and tends to suppress an increase in residual potential due to repeated use.

[0040] The conductive substrate may be subjected to a treatment with an acidic treatment solution or a boehmite treatment. Treatment with an acid treatment liquid is carried out, for example, as follows. First, an acid treatment liquid containing phosphoric acid, chromic acid, and hydrofluoric acid is prepared. The compounding ratios of phosphoric acid, chromic acid, and hydrofluoric acid in the acid treatment liquid are, for example, in the range of 10% by mass to 11% by mass for phosphoric acid, 3% by mass to 5% by mass for chromic acid, and 0.5% by mass to 2% by mass for hydrofluoric acid, and the total concentration of these acids is preferably in the range of 13.5% by mass to 18% by mass. The treatment temperature is preferably, for example, 42° C. to 48° C. The film thickness of the coating is preferably 0.3 μm to 15 μm.

[0041] The boehmite treatment is carried out, for example, by immersing the material in pure water at 90°C to 100°C for 5 to 60 minutes, or by contacting the material with heated steam at 90°C to 120°C for 5 to 60 minutes. The thickness of the coating is preferably 0.1 μm to 5 μm. This may be further anodized using an electrolyte solution having low coating solubility, such as adipic acid, boric acid, borates, phosphates, phthalates, maleates, benzoates, tartrates, or citrates.

[0042] (subbing layer) The undercoat layer is, for example, a layer containing inorganic particles and a binder resin.

[0043] As inorganic particles, for example, powder resistivity (volume resistivity) of 10 2 Ωcm or more 10 11 Examples of such particles include inorganic particles with a particle size of Ωcm or less. Among these, examples of inorganic particles having the above-mentioned resistance value include metal oxide particles such as tin oxide particles, titanium oxide particles, zinc oxide particles, and zirconium oxide particles, and zinc oxide particles are particularly preferred.

[0044] The specific surface area of ​​inorganic particles by the BET method is, for example, 10 m 2 / g or higher is preferable. The volume average particle size of the inorganic particles is, for example, from 50 nm to 2000 nm (preferably from 60 nm to 1000 nm).

[0045] The content of the inorganic particles is, for example, preferably from 10% by mass to 80% by mass, more preferably from 40% by mass to 80% by mass, based on the binder resin.

[0046] The inorganic particles may be surface-treated. Two or more types of inorganic particles having different surface treatments or different particle sizes may be used in combination.

[0047] Examples of the surface treatment agent include a silane coupling agent, a titanate coupling agent, an aluminum coupling agent, a surfactant, etc. In particular, a silane coupling agent is preferred, and a silane coupling agent having an amino group is more preferred.

[0048] Examples of silane coupling agents having an amino group include, but are not limited to, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane.

[0049] Silane coupling agents may be used in combination of two or more kinds. For example, a silane coupling agent having an amino group may be used in combination with another silane coupling agent. Examples of other silane coupling agents include, but are not limited to, vinyltrimethoxysilane, 3-methacryloxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, and 3-chloropropyltrimethoxysilane.

[0050] The surface treatment method using the surface treatment agent may be any known method, and may be either a dry method or a wet method.

[0051] The amount of the surface treatment agent to be used is preferably, for example, 0.5% by mass or more and 10% by mass or less based on the inorganic particles.

[0052] Here, it is preferable that the undercoat layer contains an electron accepting compound (acceptor compound) together with the inorganic particles, from the viewpoints of improving the long-term stability of electrical properties and carrier blocking properties.

[0053] Examples of the electron-accepting compound include electron-transporting substances such as quinone compounds such as chloranil and bromoanil; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone and 2,4,5,7-tetranitro-9-fluorenone; oxadiazole compounds such as 2-(4-biphenyl)-5-(4-t-butylphenyl)-1,3,4-oxadiazole, 2,5-bis(4-naphthyl)-1,3,4-oxadiazole and 2,5-bis(4-diethylaminophenyl)-1,3,4-oxadiazole; xanthone compounds; thiophene compounds; and diphenoquinone compounds such as 3,3',5,5'-tetra-t-butyldiphenoquinone. In particular, the electron-accepting compound is preferably a compound having an anthraquinone structure. Examples of the compound having an anthraquinone structure include hydroxyanthraquinone compounds, aminoanthraquinone compounds, and aminohydroxyanthraquinone compounds, and more specifically, anthraquinone, alizarin, quinizarin, anthrarufin, and purpurin.

[0054] The electron accepting compound may be contained in the undercoat layer in a dispersed state together with the inorganic particles, or may be contained in a state of being attached to the surfaces of the inorganic particles.

[0055] The method for attaching the electron accepting compound to the surface of the inorganic particles may be, for example, a dry method or a wet method.

[0056] The dry method is, for example, a method in which an electron-accepting compound is attached to the surface of inorganic particles by dropping an electron-accepting compound directly or dissolved in an organic solvent or spraying it together with dry air or nitrogen gas while stirring inorganic particles with a mixer or the like that exerts a large shearing force. The dropping or spraying of the electron-accepting compound is preferably performed at a temperature below the boiling point of the solvent. After dropping or spraying the electron-accepting compound, baking may be performed at 100° C. or higher. The temperature and time of baking are not particularly limited as long as electrophotographic properties can be obtained.

[0057] The wet method is a method in which, for example, an electron-accepting compound is added while dispersing inorganic particles in a solvent by stirring, ultrasonic waves, a sand mill, an attritor, a ball mill, etc., and the inorganic particles are stirred or dispersed, and then the solvent is removed to attach the electron-accepting compound to the surface of the inorganic particles. The solvent is removed, for example, by filtration or distillation. After the solvent is removed, baking may be performed at 100°C or higher. The baking temperature and time are not particularly limited as long as electrophotographic properties are obtained. In the wet method, moisture contained in the inorganic particles may be removed before adding the electron-accepting compound, and examples of such methods include a method of removing the moisture while stirring and heating in a solvent, and a method of removing the moisture by azeotropy with the solvent.

[0058] The attachment of the electron accepting compound may be carried out before or after the inorganic particles are subjected to a surface treatment with a surface treatment agent, or the attachment of the electron accepting compound and the surface treatment with the surface treatment agent may be carried out simultaneously.

[0059] The content of the electron accepting compound is, for example, from 0.01% by mass to 20% by mass, and preferably from 0.01% by mass to 10% by mass, based on the inorganic particles.

[0060] Examples of the binder resin used in the undercoat layer include known materials such as acetal resins (e.g., polyvinyl butyral, etc.), polyvinyl alcohol resins, polyvinyl acetal resins, casein resins, polyamide resins, cellulose resins, gelatin, polyurethane resins, polyester resins, unsaturated polyester resins, methacrylic resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate-maleic anhydride resins, silicone resins, silicone-alkyd resins, urea resins, phenol resins, phenol-formaldehyde resins, melamine resins, urethane resins, alkyd resins, and epoxy resins; zirconium chelate compounds; titanium chelate compounds; aluminum chelate compounds; titanium alkoxide compounds; organic titanium compounds; and silane coupling agents. Examples of the binder resin used in the undercoat layer include charge transporting resins having charge transporting groups, conductive resins (such as polyaniline, etc.), and the like.

[0061] Among these, the binder resin used in the undercoat layer is preferably a resin that is insoluble in the coating solvent of the upper layer, and in particular, a resin obtained by reacting at least one resin selected from the group consisting of thermosetting resins such as urea resins, phenol resins, phenol-formaldehyde resins, melamine resins, urethane resins, unsaturated polyester resins, alkyd resins, and epoxy resins, with a curing agent is preferred. When two or more of these binder resins are used in combination, the mixing ratio is set as necessary.

[0062] The undercoat layer may contain various additives for improving electrical properties, environmental stability, and image quality. Examples of the additives include known materials such as polycyclic condensation and azo-based electron transport pigments, zirconium chelate compounds, titanium chelate compounds, aluminum chelate compounds, titanium alkoxide compounds, organic titanium compounds, silane coupling agents, etc. As described above, silane coupling agents are used for surface treatment of inorganic particles, and may also be added to the undercoat layer as an additive.

[0063] Examples of silane coupling agents as additives include vinyltrimethoxysilane, 3-methacryloxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, and the like.

[0064] Examples of the zirconium chelate compound include zirconium butoxide, zirconium ethyl acetoacetate, zirconium triethanolamine, acetylacetonate zirconium butoxide, ethyl acetoacetate zirconium butoxide, zirconium acetate, zirconium oxalate, zirconium lactate, zirconium phosphonate, zirconium octanoate, zirconium naphthenate, zirconium laurate, zirconium stearate, zirconium isostearate, methacrylate zirconium butoxide, stearate zirconium butoxide, and isostearate zirconium butoxide.

[0065] Examples of titanium chelate compounds include tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate, titanium acetylacetonate, polytitanium acetylacetonate, titanium octylene glycolate, titanium lactate ammonium salt, titanium lactate, titanium lactate ethyl ester, titanium triethanolamine, and polyhydroxytitanium stearate.

[0066] Examples of aluminum chelate compounds include aluminum isopropylate, monobutoxyaluminum diisopropylate, aluminum butyrate, diethylacetoacetate aluminum diisopropylate, and aluminum tris(ethylacetoacetate).

[0067] These additives may be used alone or as a mixture or polycondensation product of a plurality of compounds.

[0068] The undercoat layer preferably has a Vickers hardness of 35 or more. The surface roughness (ten-point average roughness) of the undercoat layer is preferably adjusted to between 1 / (4n) (n is the refractive index of the upper layer) and 1 / 2 of the wavelength λ of the exposure laser used in order to suppress moire images. Resin particles or the like may be added to the undercoat layer to adjust the surface roughness. Examples of the resin particles include silicone resin particles and crosslinked polymethyl methacrylate resin particles. The surface of the undercoat layer may be polished to adjust the surface roughness. Examples of the polishing method include buffing, sandblasting, wet honing, grinding, and the like.

[0069] The formation of the undercoat layer is not particularly limited, and a well-known formation method can be used. For example, the undercoat layer can be formed by forming a coating film of a coating solution for forming the undercoat layer in which the above-mentioned components are added to a solvent, drying the coating film, and heating it as necessary.

[0070] Examples of the solvent for preparing the coating liquid for forming the undercoat layer include known organic solvents, such as alcohol-based solvents, aromatic hydrocarbon solvents, halogenated hydrocarbon solvents, ketone-based solvents, ketone alcohol-based solvents, ether-based solvents, and ester-based solvents. Specific examples of these solvents include ordinary organic solvents such as methanol, ethanol, n-propanol, iso-propanol, n-butanol, benzyl alcohol, methyl cellosolve, ethyl cellosolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, ethyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, methylene chloride, chloroform, chlorobenzene, and toluene.

[0071] Examples of the method for dispersing the inorganic particles when preparing the coating liquid for forming the undercoat layer include known methods such as those using a roll mill, a ball mill, a vibrating ball mill, an attritor, a sand mill, a colloid mill, and a paint shaker.

[0072] Examples of the method for applying the coating liquid for forming the undercoat layer onto the conductive substrate include ordinary methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.

[0073] The thickness of the undercoat layer is set, for example, preferably at least 15 μm, and more preferably within the range of from 20 μm to 50 μm.

[0074] (Middle class) Although not shown, an intermediate layer may be further provided between the undercoat layer and the photosensitive layer. The intermediate layer is, for example, a layer containing a resin. Examples of the resin used in the intermediate layer include polymer compounds such as acetal resins (e.g., polyvinyl butyral, etc.), polyvinyl alcohol resins, polyvinyl acetal resins, casein resins, polyamide resins, cellulose resins, gelatin, polyurethane resins, polyester resins, methacrylic resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate-maleic anhydride resins, silicone resins, silicone-alkyd resins, phenol-formaldehyde resins, and melamine resins. The intermediate layer may be a layer containing an organometallic compound. Examples of the organometallic compound used in the intermediate layer include organometallic compounds containing metal atoms such as zirconium, titanium, aluminum, manganese, and silicon. The compounds used in the intermediate layer may be used alone or as a mixture or polycondensation product of a plurality of compounds.

[0075] Among these, the intermediate layer is preferably a layer containing an organometallic compound containing zirconium atoms or silicon atoms.

[0076] The formation of the intermediate layer is not particularly limited, and a well-known formation method can be used. For example, the intermediate layer can be formed by forming a coating film of a coating solution for forming an intermediate layer in which the above components are added to a solvent, drying the coating film, and heating it as necessary. The intermediate layer can be formed by any of the usual coating methods, such as dip coating, push-up coating, wire bar coating, spray coating, blade coating, knife coating and curtain coating.

[0077] The thickness of the intermediate layer is preferably set in the range of, for example, 0.1 μm to 3 μm. The intermediate layer may also be used as an undercoat layer.

[0078] (Charge generation layer) The charge generating layer is a layer containing a charge generating material and a vinyl copolymer containing a chlorine-containing component, an acyloxy component, and an aromatic polycarboxylic acid component as a binder resin, and may contain other components as necessary. Hereinafter, the vinyl copolymer containing a chlorine-containing component, an acyloxy component, and an aromatic polycarboxylic acid component is also referred to as a "specific copolymer."

[0079] -Charge generating materials- Examples of the charge generating material include azo pigments such as bisazo and trisazo; condensed aromatic pigments such as dibromoanthanthrone; perylene pigments; pyrrolopyrrole pigments; phthalocyanine pigments; zinc oxide; and trigonal selenium.

[0080] Among these, the charge generating material is preferably a "phthalocyanine pigment" having a high charge generating ability. Examples of the phthalocyanine pigment include metal phthalocyanine pigments and metal-free phthalocyanine pigments. Specifically, examples of the phthalocyanine pigment include hydroxygallium phthalocyanine pigments disclosed in JP-A-5-263007 and JP-A-5-279591, etc.; chlorogallium phthalocyanine pigments disclosed in JP-A-5-98181, etc.; dichlorotin phthalocyanine pigments disclosed in JP-A-5-140472 and JP-A-5-140473, etc.; and titanyl phthalocyanine pigments disclosed in JP-A-4-189873, etc.

[0081] Among these, the phthalocyanine pigment is preferably at least one selected from hydroxygallium phthalocyanine pigments and chlorogallium phthalocyanine pigments from the viewpoint of charge generating ability, and more preferably hydroxygallium phthalocyanine pigments.

[0082] In addition, when a phthalocyanine pigment having a particularly high charge generation ability (at least one of chlorogallium phthalocyanine and hydroxygallium phthalocyanine, which have a particularly high charge generation ability) is used as a charge generating material, if a charge trap is present in the charge generating layer, the amount of accumulated charge increases and positive ghosts are likely to occur due to the high charge generation ability. However, in this embodiment, as described above, the amount of generated charge traps is reduced by using a specific copolymer as the binder resin. Therefore, it is presumed that positive ghosts are suppressed even when a phthalocyanine pigment is used as a charge generating material, and especially when at least one of chlorogallium phthalocyanine and hydroxygallium phthalocyanine is used.

[0083] Among the hydroxygallium phthalocyanine pigments, V-type hydroxygallium phthalocyanine pigments are preferred. In particular, as the hydroxygallium phthalocyanine pigment, for example, a hydroxygallium phthalocyanine pigment having a maximum peak wavelength in the range of 810 nm or more and 839 nm or less in a spectral absorption spectrum in the wavelength region of 600 nm or more and 900 nm or less is preferred from the viewpoint of obtaining superior dispersibility.

[0084] In addition, the hydroxygallium phthalocyanine pigment having a maximum peak wavelength in the range of 810 nm to 839 nm preferably has an average particle size in a specific range and a BET specific surface area in a specific range. Specifically, the average particle size is preferably 0.20 μm or less, and more preferably 0.01 μm to 0.15 μm. On the other hand, the BET specific surface area is preferably 45 m 2 / g or more, and 2 / g or more is more preferable, and 55m 2 / g or more 120m 2 / g or less is particularly preferable. The average particle size is the volume average particle size (d50 average particle size) measured by a laser diffraction scattering type particle size distribution measuring device (LA-700, manufactured by Horiba, Ltd.). Also, it is a value measured by a nitrogen substitution method using a BET type specific surface area measuring device (Shimadzu Corporation: Flow Soap II 2300).

[0085] The maximum particle size (maximum primary particle size) of the hydroxygallium phthalocyanine pigment is preferably 1.2 μm or less, more preferably 1.0 μm or less, and even more preferably 0.3 μm or less.

[0086] The hydroxygallium phthalocyanine pigment has an average particle size of 0.2 μm or less, a maximum particle size of 1.2 μm or less, and a specific surface area of ​​45 m 2 It is preferable that the molecular weight is 1 / g or more.

[0087] The hydroxygallium phthalocyanine pigment is preferably a V-type pigment having diffraction peaks at Bragg angles (2θ±0.2°) of at least 7.3°, 16.0°, 24.9°, and 28.0° in an X-ray diffraction spectrum using CuKα characteristic X-rays.

[0088] The charge generating material may be used alone or in combination of two or more kinds. The content of the charge generating material in the entire charge generating layer is, for example, 30 volume % or more and 80 volume % or less. From the viewpoint of suppressing positive ghosts, the content is preferably 40 volume % or more and 70 volume % or less, and more preferably 50 volume % or more and 60 volume % or less.

[0089] -Specific copolymer- The specific copolymer is a vinyl-based copolymer containing a chlorine-containing component, an acyloxy component, and an aromatic polycarboxylic acid component. In the first embodiment, the ratio of the chlorine-containing component to all structural units in the specific copolymer is 80% by mass or more, and the ratio of the aromatic polycarboxylic acid component to all structural units is 0.5% by mass or more. The ratio of each structural unit to the total structural units can be determined by analyzing the specific copolymer by NMR.

[0090] The specific copolymer contains at least a chlorine-containing component, an acyloxy component, and an aromatic polycarboxylic acid component, and may contain other structural units (for example, structural units derived from diols). However, the ratio of other structural units is preferably 5 mol% or less, more preferably 3 mol% or less, and even more preferably 1 mol% or less, based on the total structural units, and is particularly preferably free of other structural units. That is, the specific copolymer is particularly preferably a copolymer consisting of a chlorine-containing component, an acyloxy component, and an aromatic polycarboxylic acid component.

[0091] --Chlorine-containing components-- As described above, the chlorine-containing component is a structural unit which has a chlorine atom and does not have an acyloxy group or two or more carboxy groups. The specific copolymer may contain only one type of chlorine-containing component, or may contain two or more types of chlorine-containing components. The number of chlorine atoms contained in the chlorine-containing component is, for example, from 1 to 5, preferably from 1 to 3, more preferably from 1 to 2, and even more preferably 1. In addition, the chlorine-containing component preferably has chlorine atoms directly bonded to a straight chain. Examples of other substituents that the chlorine-containing component may have include alkyl groups, alkoxy groups, and halogen atoms other than chlorine. The chlorine-containing component is preferably a structural unit derived from vinyl chloride or a vinyl chloride derivative. The chlorine-containing component is preferably a constitutional unit represented by the following general formula (1).

[0092] [ka]

[0093] In general formula (1), R 11 ~R 13 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.

[0094] R in general formula (1) 11 ~R 13 are each independently preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, more preferably a hydrogen atom or a methyl group, and even more preferably a hydrogen atom. R in general formula (1) 11 ~R 13 may be different from each other or may be the same group. The chlorine-containing component is, among others, represented by the general formula (1) and R 11 ~R 13 are preferably structural units in which all of

[0095] --Acyloxy component-- As described above, the acyloxy component is a structural unit having an acyloxy group. The specific copolymer may contain only one type of acyloxy component, or may contain two or more types. The number of acyloxy groups in the acyloxy component is, for example, from 1 to 2, and more preferably 1. In addition, the acyloxy component preferably has an acyloxy group directly bonded to a straight chain. Other substituents that the acyloxy component may have include, for example, an alkyl group, an alkoxy group, and a halogen atom. The acyloxy component is preferably a building block derived from vinyl acetate or a vinyl acetate derivative. The acyloxy component is preferably a constitutional unit represented by the following general formula (2).

[0096] [ka]

[0097] In general formula (2), R 21 ~R 23 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; R 24 represents an alkyl group having 1 to 5 carbon atoms.

[0098] R in general formula (2) 21 ~R 23 are each independently preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, more preferably a hydrogen atom or a methyl group, and even more preferably a hydrogen atom. R in general formula (2) 21 ~R 23 may be different from each other or may be the same group. 21 ~R 23 are preferably all hydrogen atoms. R in general formula (2) 24 is preferably an alkyl group having 1 to 5 carbon atoms, more preferably a methyl group or an ethyl group, and even more preferably a methyl group. The acyloxy component is, among others, represented by general formula (2), and R 21 ~R 23 are all hydrogen atoms, and R24 is preferably a methyl group.

[0099] --Aromatic polycarboxylic acid component-- As described above, the aromatic polycarboxylic acid component is a structural unit having an aromatic polycarboxylic acid structure. The specific copolymer may contain only one type of aromatic polycarboxylic acid component, or may contain two or more types. Examples of the aromatic ring contained in the aromatic polycarboxylic acid component include a benzene ring and a naphthalene ring, and among these, a benzene ring is preferred. The aromatic ring may be directly bonded to the main chain of the specific copolymer or may be bonded via a linking group such as an alkylene group, and is preferably directly bonded.

[0100] The number of carboxy groups in the aromatic polycarboxylic acid component is, for example, 2 to 4, preferably 2 to 3, and more preferably 2. In addition, in the aromatic polycarboxylic acid component, two or more carboxy groups may be directly bonded to the aromatic ring, or may be bonded via a linking group such as an alkylene group. In the aromatic polycarboxylic acid component, it is preferable that all of the two or more carboxy groups are directly bonded to the aromatic ring. Examples of other substituents that the aromatic polycarboxylic acid component may have include an alkyl group, an alkoxy group, and a halogen atom.

[0101] Examples of the aromatic polycarboxylic acid structure contained in the aromatic polycarboxylic acid component include a phthalic acid structure, an isophthalic acid structure, a terephthalic acid structure, and a naphthalenedicarboxylic acid structure. Among these, a phthalic acid structure is preferred, and a phthalic acid structure having no other substituents is more preferred. The aromatic polycarboxylic acid component is preferably one in which an aromatic polycarboxylic acid structure is directly bonded to the main chain of the specific copolymer, and more preferably one in which a phthalic acid structure is directly bonded to the main chain of the specific copolymer. The aromatic polycarboxylic acid component is preferably a structural unit derived from phthalic acid, vinylphthalic acid, or a derivative thereof. The aromatic polycarboxylic acid component may be a structural unit located at the end of the main chain of the specific copolymer, such as a structural unit represented by the following formula (3-1), or may be a structural unit located at a position other than the end, such as a structural unit represented by the following formula (3-2). The aromatic polycarboxylic acid component is preferably a structural unit located at the end of the main chain of the specific copolymer.

[0102] [ka]

[0103] --Combination of each ingredient-- The specific copolymer is preferably a copolymer containing a constituent unit represented by general formula (1) as a chlorine-containing component and a constituent unit represented by general formula (2) as an acyloxy component, and more preferably a copolymer containing a constituent unit represented by general formula (1), a constituent unit represented by general formula (2), and a constituent unit having a phthalic acid structure. The specific copolymer is represented by general formula (1) as a chlorine-containing component, and R 11 ~R 13 Each of the structural units is a hydrogen atom, and the acyloxy component is represented by the general formula (2). 21 ~R 23 are all hydrogen atoms, and R in general formula (2) 24 It is more preferable that the copolymer is a copolymer containing a structural unit in which R in the general formula (1) is a methyl group. 11 ~R 13 A structural unit represented by general formula (2), in which R 21 ~R 23 are all hydrogen atoms, and R in general formula (2) 24 It is particularly preferable that the copolymer contains a structural unit in which the substituent is a methyl group and a structural unit having a phthalic acid structure having no other substituent.

[0104] --Proportion of each ingredient-- From the viewpoint of suppressing image density differences in the axial direction of the photoreceptor, the proportion of the chlorine-containing component is preferably 80% by mass or more, more preferably 82% by mass or more, and even more preferably 85% by mass or more, based on the total constituent components of the specific copolymer. In addition, from the viewpoint of obtaining high sensitivity, the proportion of chlorine-containing components is preferably 88 mass % or less, more preferably 87 mass % or less, and even more preferably 86 mass % or less, based on the total constituent components of the specific copolymer. When the proportion of the chlorine-containing component is 87% by mass or less, the hardness of the vinyl copolymer is not so high as compared with the case where the proportion of the chlorine-containing component is too high, and the dispersibility of the charge-generating material is not so low as to be caused by the hardness being too high. Also, when the proportion of the chlorine-containing component is 87% by mass or less, the proportion of the acyloxy component is relatively high as compared with the case where the proportion of the chlorine-containing component is too high, and the dispersibility of the charge-generating material is easily obtained. As a result, it is presumed that the charge-generating material is easily present near the interface with the charge-transporting layer, and high sensitivity is obtained. From the viewpoint of achieving both suppression of image density differences in the axial direction of the photoreceptor and high sensitivity, the proportion of chlorine-containing components is preferably 80% by mass or more and 88% by mass or less, more preferably 82% by mass or more and 87% by mass or less, and even more preferably 85% by mass or more and 86% by mass or less.

[0105] From the viewpoint of suppressing image density differences in the axial direction of the photoreceptor, the proportion of the aromatic polycarboxylic acid component is preferably 0.5 mass% or more, more preferably 0.5 mass% or more, and more preferably 0.8 mass% or more, based on the total constituent components of the specific copolymer. Furthermore, from the viewpoint of obtaining high sensitivity, the proportion of the aromatic polycarboxylic acid component is preferably 2.5% by mass or less, and more preferably 1.5% by mass or less, based on the total constituent components of the specific copolymer. When the proportion of the aromatic polycarboxylic acid component is 2.0% by mass or less, the proportion of the acyloxy component is relatively high, and the charge generating material is easily dispersible, compared with the case where the proportion of the aromatic polycarboxylic acid component is too high. As a result, the charge generating material is easily present near the interface with the charge transport layer, and it is presumed that high sensitivity is obtained. The proportion of the aromatic polycarboxylic acid component is preferably 0.5% by mass or more and 2.0% by mass or less, from the viewpoint of achieving both suppression of image density difference in the axial direction of the photoreceptor and high sensitivity.

[0106] When the ratio of the aromatic polycarboxylic acid component to all the components of the specific copolymer is A% by mass and the content of the charge generating material in the specific copolymer is C% by mass, the value of A / C is set to 3.00×10 -3 It is preferable that the value is 5.00×10 or more. -3 More preferably, it is equal to or greater than this. In order to obtain high sensitivity, the A / C value is set to 1.40×10 -2 It is preferable that the value is less than 1.00×10 -2 It is more preferable that: The value of A / C is set to 3.00×10 from the viewpoint of suppressing the image density difference in the axial direction of the photoconductor and achieving high sensitivity. -3 Above 1.40 x 10 -2 Preferably, it is 5.00×10 or less. -3 Above 1.00 x 10 -2 It is preferable that: The weight average molecular weight is a value measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh Corporation GPC HLC-8120GPC as a measuring device, a Tosoh Corporation TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve prepared with monodisperse polystyrene standard samples.

[0107] The solubility of the specific copolymer in 100 parts by mass of tetrahydrofuran at 30°C (hereinafter also referred to as "THF solubility") is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 7.5 parts by mass or less, from the viewpoint of suppressing image density differences in the axial direction of the photoreceptor. The THF solubility is determined by putting a polymer to be measured into tetrahydrofuran at 30° C., leaving it to stand for 5 minutes, and then measuring the mass of the remaining polymer.

[0108] The method for producing the specific copolymer is not particularly limited, and examples thereof include a method in which monomers corresponding to each structural unit are polymerized by suspension polymerization or the like.

[0109] -Other additives- The charge generating layer may contain other well-known additives.

[0110] - Formation of charge generation layer - The formation of the charge generation layer is not particularly limited, and a well-known formation method can be used. For example, the charge generation layer can be formed by forming a coating film of a coating liquid for forming the charge generation layer in which the above components are added to a solvent, drying the coating film, and heating it if necessary.

[0111] Examples of the solvent for preparing the coating liquid for forming the charge generating layer include methanol, ethanol, n-propanol, n-butanol, benzyl alcohol, methyl cellosolve, ethyl cellosolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, methylene chloride, chloroform, chlorobenzene, toluene, etc. These solvents may be used alone or in combination of two or more.

[0112] Examples of methods for dispersing particles (e.g., charge generating material) in the coating liquid for forming a charge generating layer include media dispersers such as ball mills, vibration ball mills, attritors, sand mills, and horizontal sand mills, and medialess dispersers such as stirrers, ultrasonic dispersers, roll mills, and high-pressure homogenizers. Examples of high-pressure homogenizers include a collision method in which the dispersion liquid is dispersed by liquid-liquid collision or liquid-wall collision under high pressure, and a penetration method in which the dispersion liquid is dispersed by penetrating a fine flow path under high pressure. During this dispersion, it is effective to adjust the average particle size of the charge generating material in the coating liquid for forming the charge generating layer to 0.5 μm or less, preferably 0.3 μm or less, and more preferably 0.15 μm or less.

[0113] Examples of a method for applying the coating liquid for forming the charge generating layer onto the undercoat layer (or onto the intermediate layer) include conventional methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.

[0114] The thickness of the charge generating layer is set within the range, for example, preferably from 0.05 to 5.0 μm, more preferably from 0.1 to 2.0 μm, further preferably from 0.1 to 1.0 μm, and particularly preferably from 0.1 to 0.5 μm.

[0115] (charge transport layer) The charge transport layer is a layer containing a charge transport material and a binder resin, and may be a layer containing a polymer charge transport material.

[0116] Examples of the charge transport material include electron transporting compounds such as quinone compounds such as p-benzoquinone, chloranil, bromanil, and anthraquinone; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone; xanthone compounds; benzophenone compounds; cyanovinyl compounds; and ethylene compounds. Examples of the charge transport material include hole transporting compounds such as triarylamine compounds, benzidine compounds, arylalkane compounds, aryl-substituted ethylene compounds, stilbene compounds, anthracene compounds, and hydrazone compounds. These charge transport materials may be used alone or in combination, but are not limited to these.

[0117] As the charge transport material, from the viewpoint of charge mobility, a triarylamine-based charge transport material represented by the following general formula (a-1) (hereinafter also referred to as "triarylamine-based charge transport material (a-1)"), a charge transport material represented by the following general formula (CT1) (hereinafter also referred to as "butadiene-based charge transport material (CT1)") which is an example of the triarylamine-based charge transport material, and a charge transport material represented by the following general formula (CT2) (hereinafter also referred to as "benzidine-based charge transport material (CT2)") are preferable. As the charge transport material, a butadiene-based charge transport material (CT1) and a benzidine-based charge transport material (CT2) may be used in combination.

[0118] The triarylamine-based charge transport material (a-1) will now be described. The triarylamine-based charge transport material (a-1) is a charge transport material represented by the following general formula (a-1).

[0119] [ka]

[0120] In general formula (a-1), Ar T1 , Ar T2 , and Ar T3 each independently represents a substituted or unsubstituted aryl group, -CH-C(R T4)=C(R T5 )(R T6 ), or -CH-CH=CH-CH=C(R T7 )(R T8 ) is shown. T4 , R T5 , R T6 , R T7 , and R T8 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group. Examples of the substituent for each of the above groups include a halogen atom, an alkyl group having from 1 to 5 carbon atoms, and an alkoxy group having from 1 to 5 carbon atoms. Examples of the substituent for each of the above groups also include a substituted amino group substituted with an alkyl group having from 1 to 3 carbon atoms.

[0121] The butadiene-based charge transport material (CT1) will be explained. The butadiene-based charge transport material (CT1) is a charge transport material represented by the following general formula (CT1).

[0122] [ka]

[0123] In the general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 each independently represents a hydrogen atom, a halogen atom, an alkyl group having from 1 to 20 carbon atoms, an alkoxy group having from 1 to 20 carbon atoms, or an aryl group having from 6 to 30 carbon atoms, and two adjacent substituents may be bonded to each other to form a hydrocarbon ring structure. n and m each independently represent 0, 1 or 2.

[0124] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16Examples of the halogen atom represented by include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. Among these, as the halogen atom, a fluorine atom and a chlorine atom are preferable, and a chlorine atom is more preferable.

[0125] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 The alkyl group represented by the formula (I) includes a linear or branched alkyl group having 1 to 20 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of the straight-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, an n-hexadecyl group, an n-heptadecyl group, an n-octadecyl group, an n-nonadecyl group, and an n-icosyl group. Specific examples of branched alkyl groups include isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl, sec-hexyl, tert-hexyl, isoheptyl, sec-heptyl, tert-heptyl, isooctyl, sec-octyl, tert-octyl, isononyl, sec-nonyl, tert-nonyl, isodecyl, sec-decyl, tert-decyl, isoundecyl, sec-undecyl, tert-undecyl, neoundecyl, isododecyl, sec-dodecyl, tert-dodecyl, neododecyl, isotridecyl, sec-tridecyl, tert-tridecyl, neotridecyl, isotetradecyl, group, sec-tetradecyl group, tert-tetradecyl group, neotetradecyl group, 1-isobutyl-4-ethyloctyl group, isopentadecyl group, sec-pentadecyl group, tert-pentadecyl group, neopentadecyl group, isohexadecyl group, sec-hexadecyl group, tert-hexadecyl group, neohexadecyl group, 1-methylpentadecyl group, isoheptadecyl group, sec Examples of the isooctadecyl group include a 1-heptadecyl group, a tert-heptadecyl group, a neoheptadecyl group, an isooctadecyl group, a sec-octadecyl group, a tert-octadecyl group, a neooctadecyl group, an isononadecyl group, a sec-nonadecyl group, a tert-nonadecyl group, a neononadecyl group, a 1-methyloctyl group, an isoicosyl group, a sec-icosyl group, a tert-icosyl group, and a neoicosyl group. Among these, the alkyl group is preferably a lower alkyl group such as a methyl group, an ethyl group, or an isopropyl group.

[0126] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 The alkoxy group represented by the formula (I) includes a linear or branched alkoxy group having 1 to 20 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of linear alkoxy groups include a methoxy group, an ethoxy group, an n-propoxy group, an n-butoxy group, an n-pentyloxy group, an n-hexyloxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, an n-decyloxy group, an n-undecyloxy group, an n-dodecyloxy group, an n-tridecyloxy group, an n-tetradecyloxy group, an n-pentadecyloxy group, an n-hexadecyloxy group, an n-heptadecyloxy group, an n-octadecyloxy group, an n-nonadecyloxy group, and an n-icosyloxy group. Specific examples of branched alkoxy groups include an isopropoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an isopentyloxy group, a neopentyloxy group, a tert-pentyloxy group, an isohexyloxy group, a sec-hexyloxy group, a tert-hexyloxy group, an isoheptyloxy group, a sec-heptyloxy group, a tert-heptyloxy group, an isooctyloxy group, a sec-octyloxy group, a tert-octyloxy group, an isononyloxy group, a se c-nonyloxy group, tert-nonyloxy group, isodecyloxy group, sec-decyloxy group, tert-decyloxy group, isoundecyloxy group, sec-undecyloxy group, tert-undecyloxy group, neoundecyloxy group, isododecyloxy group, sec-dodecyloxy group, tert-dodecyloxy group, neododecyloxy group, isotridecyloxy group, sec-tridecyloxy group, tert-tridecyloxy group, neotridecyloxy group, isotetradecyloxy group, hexadecyloxy group, sec-hexadecyloxy group, tert-hexadecyloxy group, neohexadecyloxy group, 1-methylpentadecyloxy group, isohept ...tert-hexadecyloxy group, neohexadecyloxy group, 1-methylpentadecyloxy group, isoheptadecyloxy group, sec-hexadecyloxy group, tert-hexadecyloxy group, neohex Examples of such an aryloxy group include a heptadecyloxy group, a tert-heptadecyloxy group, a neoheptadecyloxy group, an isooctadecyloxy group, a sec-octadecyloxy group, a tert-octadecyloxy group, a neooctadecyloxy group, an isononadecyloxy group, a sec-nonadecyloxy group, a tert-nonadecyloxy group, a neononadecyloxy group, a 1-methyloctyloxy group, an isoicosyloxy group, a sec-icosyloxy group, a tert-icosyloxy group, and a neoicosyloxy group. Among these, the alkoxy group is preferably a methoxy group.

[0127] In general formula (CT1), R C11 , R C12, R C13 , R C14 , R C15 , and R C16 The aryl group represented by the formula (I) includes an aryl group having 6 or more and 30 or less carbon atoms (preferably 6 or more and 20 or less, more preferably 6 or more and 16 or less). Specific examples of the aryl group include a phenyl group, a naphthyl group, a phenanthryl group, and a biphenylyl group. Among these, the aryl group is preferably a phenyl group or a naphthyl group.

[0128] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 Each of the above-mentioned substituents represented by also includes a group having a further substituent. The substituent includes the above-mentioned atoms and groups (e.g., halogen atoms, alkyl groups, alkoxy groups, aryl groups, etc.).

[0129] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 Two adjacent substituents (e.g., R C11 and R C12 Fellow, R C13 and R C14 Fellow, R C15 and R C16 In the hydrocarbon ring structure in which the substituents (atomic groups) are linked to each other, examples of the group linking the substituents to each other include a single bond, a 2,2'-methylene group, a 2,2'-ethylene group, and a 2,2'-vinylene group. Among these, a single bond and a 2,2'-methylene group are preferred. Specific examples of the hydrocarbon ring structure include a cycloalkane structure, a cycloalkene structure, and a cycloalkanepolyene structure.

[0130] In the general formula (CT1), n ​​and m are preferably 1.

[0131] In the general formula (CT1), from the viewpoint of forming a photosensitive layer (charge transport layer) having high charge transport ability, R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, and preferably, m and n each represent 1 or 2; R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 It is more preferable that m and n each represent 1. That is, the butadiene-based charge transport material (CT1) is more preferably a charge transport material represented by the following structural formula (CT1A) (exemplary compound (CT1-3)).

[0132] [ka]

[0133] Specific examples of the butadiene-based charge transport material (CT1) are shown below, but the present invention is not limited thereto.

[0134] [ka]

[0135] The abbreviations in the above exemplary compounds have the following meanings: The numbers before the substituents indicate the substitution positions on the benzene ring. CH3: Methyl group OCH3: Methoxy group

[0136] The butadiene-based charge transport material (CT1) may be used alone or in combination of two or more kinds.

[0137] The benzidine-based charge transport material (CT2) will be described. The benzidine-based charge transport material (CT2) is a charge transport material represented by the following general formula (CT2).

[0138] [ka]

[0139] In the general formula (CT2), R C21 , R C22 , and R C23 each independently represents a hydrogen atom, a halogen atom, an alkyl group having from 1 to 10 carbon atoms, an alkoxy group having from 1 to 10 carbon atoms, or an aryl group having from 6 to 10 carbon atoms.

[0140] In general formula (CT2), R C21 , R C22 , and R C23 Examples of the halogen atom represented by include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. Among these, as the halogen atom, a fluorine atom and a chlorine atom are preferable, and a chlorine atom is more preferable.

[0141] In general formula (CT2), R C21 , R C22 , and R C23 The alkyl group represented by the formula (I) includes a linear or branched alkyl group having 1 to 10 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of the straight-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group. Specific examples of branched alkyl groups include an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, an isohexyl group, a sec-hexyl group, a tert-hexyl group, an isoheptyl group, a sec-heptyl group, a tert-heptyl group, an isooctyl group, a sec-octyl group, a tert-octyl group, an isononyl group, a sec-nonyl group, a tert-nonyl group, an isodecyl group, a sec-decyl group, and a tert-decyl group. Among these, the alkyl group is preferably a lower alkyl group such as a methyl group, an ethyl group, or an isopropyl group.

[0142] In general formula (CT2), R C21 , R C22 , and R C23 The alkoxy group represented by the formula (I) includes a linear or branched alkoxy group having 1 to 10 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of linear alkoxy groups include a methoxy group, an ethoxy group, an n-propoxy group, an n-butoxy group, an n-pentyloxy group, an n-hexyloxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, and an n-decyloxy group. Specific examples of branched alkoxy groups include an isopropoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an isopentyloxy group, a neopentyloxy group, a tert-pentyloxy group, an isohexyloxy group, a sec-hexyloxy group, a tert-hexyloxy group, an isoheptyloxy group, a sec-heptyloxy group, a tert-heptyloxy group, an isooctyloxy group, a sec-octyloxy group, a tert-octyloxy group, an isononyloxy group, a sec-nonyloxy group, a tert-nonyloxy group, an isodecyloxy group, a sec-decyloxy group, and a tert-decyloxy group. Among these, the alkoxy group is preferably a methoxy group.

[0143] In general formula (CT2), R C21 , RC22 , and R C23 The aryl group represented by the formula (I) includes an aryl group having 6 to 10 carbon atoms (preferably 6 to 9, more preferably 6 to 8). Specific examples of the aryl group include a phenyl group and a naphthyl group. Among these, the aryl group is preferably a phenyl group.

[0144] In general formula (CT2), R C21 , R C22 , and R C23 Each of the above-mentioned substituents represented by also includes a group having a further substituent. The substituent includes the above-mentioned atoms and groups (e.g., halogen atoms, alkyl groups, alkoxy groups, aryl groups, etc.).

[0145] In general formula (CT2), from the viewpoint of forming a photosensitive layer (charge transport layer) having high charge transport ability, R C21 , R C22 , and R C23 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; R C21 , and R C23 represents a hydrogen atom, and R C22 More preferably, represents an alkyl group having 1 to 10 carbon atoms (particularly, a methyl group). Specifically, the benzidine-based charge transport material (CT2) is particularly preferably a charge transport material represented by the following structural formula (CT2A) (exemplary compound (CT2-2)).

[0146] [ka]

[0147] Specific examples of the benzidine-based charge transport material (CT2) are shown below, but the present invention is not limited thereto.

[0148] [ka]

[0149] The abbreviations in the above exemplary compounds have the following meanings: The numbers before the substituents indicate the substitution positions on the benzene ring. CH3: Methyl group C2H5: Ethyl group OCH3: Methoxy group OC2H5: Ethoxy group

[0150] The benzidine-based charge transport material (CT2) may be used alone or in combination of two or more kinds.

[0151] As the polymer charge transport material, known materials having charge transport properties such as poly-N-vinylcarbazole and polysilane are used. In particular, polyester-based polymer charge transport materials disclosed in JP-A-8-176293 and JP-A-8-208820 are particularly preferred. The polymer charge transport material may be used alone or in combination with a binder resin.

[0152] Examples of the binder resin used in the charge transport layer include polycarbonate resin, polyester resin, polyarylate resin, methacrylic resin, acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl acetate resin, styrene-butadiene copolymer, vinylidene chloride-acrylonitrile copolymer, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-maleic anhydride copolymer, silicone resin, silicone alkyd resin, phenol-formaldehyde resin, styrene-alkyd resin, poly-N-vinylcarbazole, polysilane, etc. Among these, polycarbonate resin or polyarylate resin is suitable as the binder resin. These binder resins are used alone or in combination of two or more. The compounding ratio of the charge transport material to the binder resin is preferably from 10:1 to 1:5 by mass.

[0153] The charge transport layer may contain other well-known additives.

[0154] The formation of the charge transport layer is not particularly limited, and a known formation method can be used. For example, the charge transport layer can be formed by forming a coating film of a coating liquid for forming the charge transport layer in which the above components are added to a solvent, drying the coating film, and heating it as necessary.

[0155] Examples of solvents for preparing the coating liquid for forming the charge transport layer include ordinary organic solvents such as aromatic hydrocarbons such as benzene, toluene, xylene, and chlorobenzene, ketones such as acetone and 2-butanone, halogenated aliphatic hydrocarbons such as methylene chloride, chloroform, and ethylene chloride, and cyclic or linear ethers such as tetrahydrofuran and ethyl ether. These solvents may be used alone or in combination of two or more.

[0156] Examples of a coating method for coating the coating liquid for forming the charge transport layer on the charge generating layer include ordinary methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating and curtain coating.

[0157] The thickness of the charge transport layer is set, for example, preferably in the range of 5 μm to 50 μm, more preferably 10 μm to 45 μm, and further preferably 20 μm to 42 μm.

[0158] (protective layer) A protective layer is provided on the photosensitive layer as necessary for the purpose of, for example, preventing chemical changes in the photosensitive layer when the photosensitive layer is charged and further improving the mechanical strength of the photosensitive layer. Therefore, it is preferable to apply a layer composed of a cured film (crosslinked film) as the protective layer. Examples of such a layer include the following layers 1) and 2).

[0159] 1) A layer composed of a cured film of a composition containing a reactive group-containing charge transport material having a reactive group and a charge transport skeleton in the same molecule (i.e., a layer containing a polymer or crosslinked product of the reactive group-containing charge transport material). 2) A layer composed of a cured film of a composition containing a non-reactive charge transport material and a reactive group-containing non-charge transport material that does not have a charge transport skeleton and has a reactive group (i.e., a layer containing a non-reactive charge transport material and a polymer or crosslinked body of the reactive group-containing non-charge transport material).

[0160] The reactive group of the reactive group-containing charge transport material may be a chain polymerizable group, an epoxy group, -OH, -OR (wherein R represents an alkyl group), -NH2, -SH, -COOH, or -SiR. Q1 3-Qn (OR Q2 ) Qn [However, R Q1 represents a hydrogen atom, an alkyl group, or a substituted or unsubstituted aryl group; R Q2 represents a hydrogen atom, an alkyl group, or a trialkylsilyl group; Qn represents an integer of 1 to 3.

[0161] The chain polymerizable group is not particularly limited as long as it is a functional group capable of radical polymerization, and is, for example, a functional group having a group containing at least a carbon double bond.Specific examples include groups containing at least one selected from vinyl groups, vinyl ether groups, vinyl thioether groups, vinylphenyl groups, acryloyl groups, methacryloyl groups, and derivatives thereof.Among them, the chain polymerizable group is preferably a group containing at least one selected from vinyl groups, vinylphenyl groups, acryloyl groups, methacryloyl groups, and derivatives thereof, because of its excellent reactivity.

[0162] The charge transporting skeleton of the reactive group-containing charge transporting material is not particularly limited as long as it is a known structure in electrophotographic photoreceptors, and examples thereof include a skeleton derived from a nitrogen-containing hole transporting compound such as a triarylamine compound, a benzidine compound, a hydrazone compound, etc., and a structure conjugated with a nitrogen atom. Among these, a triarylamine skeleton is preferred.

[0163] The reactive group-containing charge transport material having a reactive group and a charge transporting skeleton, the non-reactive charge transport material, and the reactive group-containing non-charge transport material may be selected from well-known materials.

[0164] The protective layer may contain other well-known additives.

[0165] The formation of the protective layer is not particularly limited, and a well-known formation method can be used. For example, the protective layer can be formed by forming a coating film of a coating liquid for forming the protective layer in which the above components are added to a solvent, drying the coating film, and, if necessary, subjecting it to a curing treatment such as heating.

[0166] Examples of solvents for preparing a coating solution for forming a protective layer include aromatic solvents such as toluene and xylene, ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone, ester solvents such as ethyl acetate and butyl acetate, ether solvents such as tetrahydrofuran and dioxane, cellosolve solvents such as ethylene glycol monomethyl ether, and alcohol solvents such as isopropyl alcohol and butanol. These solvents may be used alone or in combination of two or more. The protective layer-forming coating liquid may be a solvent-free coating liquid.

[0167] Examples of a method for applying the protective layer-forming coating liquid onto a photosensitive layer (e.g., a charge transport layer) include conventional methods such as dip coating, push-up coating, wire bar coating, spray coating, blade coating, knife coating, and curtain coating.

[0168] The thickness of the protective layer is set, for example, preferably in the range of 1 μm or more and 20 μm or less, and more preferably in the range of 2 μm or more and 10 μm or less.

[0169] [Image forming device (and process cartridge)] The image forming apparatus according to the present embodiment includes an electrophotographic photoreceptor, a charging unit for charging the surface of the electrophotographic photoreceptor, an electrostatic latent image forming unit for forming an electrostatic latent image on the surface of the charged electrophotographic photoreceptor, a developing unit for developing the electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing toner to form a toner image, and a transfer unit for transferring the toner image to the surface of a recording medium. The electrophotographic photoreceptor according to the present embodiment is applied as the electrophotographic photoreceptor.

[0170] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as an apparatus provided with a fixing means for fixing a toner image transferred onto the surface of a recording medium; an apparatus of a direct transfer type for directly transferring a toner image formed on the surface of an electrophotographic photosensitive member onto a recording medium; an apparatus of an intermediate transfer type for primarily transferring a toner image formed on the surface of an electrophotographic photosensitive member onto the surface of an intermediate transfer member, and then secondarily transferring the toner image transferred onto the surface of the intermediate transfer member onto the surface of a recording medium; an apparatus provided with a cleaning means for cleaning the surface of an electrophotographic photosensitive member before charging after the transfer of a toner image; an apparatus provided with a discharging means for irradiating the surface of an electrophotographic photosensitive member with discharging light to discharge the surface before charging after the transfer of a toner image; and an apparatus provided with an electrophotographic photosensitive member heating member for increasing the temperature of the electrophotographic photosensitive member and reducing the relative temperature.

[0171] In the case of an intermediate transfer type device, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the electrophotographic photosensitive body onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.

[0172] The image forming apparatus according to the present embodiment may be either a dry development type image forming apparatus or a wet development type image forming apparatus (a development type using a liquid developer).

[0173] In the image forming apparatus according to the present embodiment, for example, a portion including an electrophotographic photoreceptor may be a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge including the electrophotographic photoreceptor according to the present embodiment is preferably used. In addition to the electrophotographic photoreceptor, the process cartridge may include at least one selected from the group consisting of a charging means, an electrostatic latent image forming means, a developing means, and a transfer means.

[0174] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.

[0175] FIG. 2 is a schematic diagram showing an example of the image forming apparatus according to the present embodiment. As shown in FIG. 2, the image forming apparatus 100 according to the present embodiment includes a process cartridge 300 including an electrophotographic photoreceptor 7, an exposure device 9 (an example of an electrostatic latent image forming means), a transfer device 40 (a primary transfer device), and an intermediate transfer body 50. In the image forming apparatus 100, the exposure device 9 is disposed at a position where it can expose the electrophotographic photoreceptor 7 from the opening of the process cartridge 300, the transfer device 40 is disposed at a position facing the electrophotographic photoreceptor 7 via the intermediate transfer body 50, and the intermediate transfer body 50 is disposed with a part of it in contact with the electrophotographic photoreceptor 7. Although not shown, the image forming apparatus 100 also includes a secondary transfer device that transfers the toner image transferred to the intermediate transfer body 50 to a recording medium (e.g., paper). The intermediate transfer body 50, the transfer device 40 (a primary transfer device), and the secondary transfer device (not shown) correspond to an example of a transfer means.

[0176] 2 supports an electrophotographic photoreceptor 7, a charging device 8 (an example of a charging means), a developing device 11 (an example of a developing means), and a cleaning device 13 (an example of a cleaning means) integrally within a housing. The cleaning device 13 has a cleaning blade (an example of a cleaning member) 131, which is disposed so as to come into contact with the surface of the electrophotographic photoreceptor 7. The cleaning member may not be in the form of the cleaning blade 131, but may be a conductive or insulating fibrous member, which may be used alone or in combination with the cleaning blade 131.

[0177] FIG. 2 shows an example of an image forming apparatus equipped with a fibrous member 132 (roll-shaped) that supplies lubricant 14 to the surface of electrophotographic photosensitive member 7, and a fibrous member 133 (flat brush-shaped) that assists in cleaning, which may be arranged as needed.

[0178] Hereinafter, each configuration of the image forming apparatus according to this embodiment will be described.

[0179] -Charging device- As the charging device 8, for example, a contact type charger using a conductive or semiconductive charging roller, charging brush, charging film, charging rubber blade, charging tube, etc. Also, a non-contact type roller charger, a scorotron charger or corotron charger that utilizes corona discharge, or other chargers known per se, can be used.

[0180] -Exposure equipment- The exposure device 9 may be, for example, an optical device that exposes the surface of the electrophotographic photoreceptor 7 with light such as semiconductor laser light, LED light, or liquid crystal shutter light in a predetermined image. The wavelength of the light source is within the spectral sensitivity range of the electrophotographic photoreceptor. The wavelength of the semiconductor laser is mainly near infrared light having an oscillation wavelength of about 780 nm. However, it is not limited to this wavelength, and a laser having an oscillation wavelength of 600 nm or a blue laser having an oscillation wavelength of 400 nm to 450 nm may also be used. In addition, a surface-emitting laser light source capable of outputting multiple beams is also effective for forming a color image.

[0181] -Developing device- The developing device 11 may be, for example, a general developing device that develops by contacting or non-contacting a developer. The developing device 11 is not particularly limited as long as it has the above-mentioned functions, and may be selected according to the purpose. For example, it may be a known developing device that has a function of attaching a one-component developer or a two-component developer to the electrophotographic photoreceptor 7 using a brush, roller, or the like. Among them, it is preferable to use a developing roller that holds a developer on its surface.

[0182] The developer used in the developing device 11 may be a one-component developer containing only toner, or may be a two-component developer containing toner and a carrier. The developer may be magnetic or non-magnetic. Well-known developers are used.

[0183] -Cleaning device- The cleaning device 13 is a cleaning blade type device equipped with a cleaning blade 131 . In addition to the cleaning blade system, a fur brush cleaning system or a simultaneous development and cleaning system may also be used.

[0184] -Transfer device- Examples of the transfer device 40 include known transfer chargers such as a contact type transfer charger using a belt, roller, film, rubber blade, etc., and a scorotron transfer charger or corotron transfer charger that utilizes corona discharge.

[0185] -Intermediate transfer body- A belt-like intermediate transfer belt containing semiconductive polyimide, polyamideimide, polycarbonate, polyarylate, polyester, rubber, etc. is used as the intermediate transfer body 50. The intermediate transfer body may be in the form of a drum other than a belt.

[0186] FIG. 3 is a schematic diagram showing another example of the image forming apparatus according to the present embodiment. 3 is a tandem-type multi-color image forming apparatus equipped with four process cartridges 300. In the image forming apparatus 120, the four process cartridges 300 are arranged in parallel on the intermediate transfer body 50, and one electrophotographic photosensitive body is used for each color. The image forming apparatus 120 has the same configuration as the image forming apparatus 100, except that it is a tandem type. EXAMPLES

[0187] Hereinafter, the present embodiment will be described in detail with reference to examples, but the present embodiment is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.

[0188] <Example 1> 100 parts by mass of zinc oxide (product name: MZ 300, manufactured by Teika Corporation), 10 parts by mass of a 10% by mass toluene solution of N-2-(aminoethyl)-3-aminopropyltriethoxysilane as a silane coupling agent, and 200 parts by mass of toluene were mixed and stirred, and refluxed for 2 hours. After that, the toluene was distilled off under reduced pressure at 10 mmHg, and a surface treatment was performed by baking at 135°C for 2 hours.

[0189] 33 parts by mass of surface-treated zinc oxide, 6 parts by mass of blocked isocyanate (product name: Sumidur 3175, manufactured by Sumitomo Bayer Urethane Co., Ltd.), 1 part by mass of a compound represented by the following structural formula (AK-1) as an electron accepting compound, and 25 parts by mass of methyl ethyl ketone were mixed for 30 minutes, after which 5 parts by mass of butyral resin (product name: S-LEC BM-1, manufactured by Sekisui Chemical Co., Ltd.), 3 parts by mass of silicone balls (product name: Tospearl 120, manufactured by Momentive Performance Materials, Inc.), and 0.01 parts by mass of silicone oil (product name: SH29PA, manufactured by Dow Corning Co., Ltd.) as a leveling agent were added, and the mixture was dispersed for 3 hours using a sand mill to obtain a coating liquid for forming an undercoat layer.

[0190] [ka]

[0191] The coating solution for forming the undercoat layer was then applied onto an aluminum substrate having a diameter of 30 mm, a length of 365 mm and a thickness of 1 mm by dip coating, and dried and cured at 180° C. for 30 minutes to obtain an undercoat layer having a thickness of 25 μm.

[0192] Next, a mixture of hydroxygallium phthalocyanine pigment (HOGaPc) as a charge generating material, the following specific copolymer (1) as a binder resin, and acetone was placed in a 100 mL glass bottle together with 1.0 mmφ glass beads (filling rate 50%) and dispersed for 2.5 hours using a paint shaker to obtain a coating liquid for forming a charge generating layer. Specific copolymer (1): R represented by the above general formula (1) as a chlorine-containing component 11 ~R 13 and R 21 ~R 23 are all hydrogen atoms and R 24 A vinyl copolymer comprising a structural unit in which the benzene ring of a phthalic acid structure having no other substituents is directly bonded to the main chain as an aromatic polycarboxylic acid component, and the proportion of each structural unit is as shown in Table 1. The weight average molecular weight and THF solubility of the specific copolymer (1) are also shown in Table 1.

[0193] Here, the content of the hydroxygallium phthalocyanine pigment relative to the total amount of the hydroxygallium phthalocyanine pigment and the specific copolymer (1) contained in the coating liquid for forming a charge generating layer was 60 mass %, and the solid content of the coating liquid for forming a charge generating layer was 6.0 mass %.

[0194] The hydroxygallium phthalocyanine pigment is a V-type hydroxygallium phthalocyanine pigment having diffraction peaks at Bragg angles (2θ±0.2°) of at least 7.3°, 16.0°, 24.9°, and 28.0° in an X-ray diffraction spectrum using Cukα characteristic X-rays (maximum peak wavelength in a spectral absorption spectrum in a wavelength range of 600 nm to 900 nm: 820 nm; average particle size: 0.12 μm; maximum particle size: 0.2 μm; specific surface area value: 60 m 2 / g).

[0195] The resulting coating liquid for forming a charge generating layer was dip-coated on the undercoat layer and dried at 150° C. for 5 minutes to form a charge generating layer having a thickness of 0.14 μm.

[0196] Next, 12 parts by weight of a charge transport material represented by the following structural formula (CT1A), 28 parts by weight of a charge transport material represented by the following structural formula (CT2A), and 60 parts by weight of bisphenol Z type polycarbonate resin (molecular weight 40,000) were added and dissolved in 340 parts by weight of tetrahydrofuran to obtain a coating liquid for forming a charge transport layer. The obtained coating liquid for forming the charge transport layer was dip-coated on the charge generating layer, and dried at 150° C. for 40 minutes to form a charge transport layer with a thickness of 40 μm.

[0197] [ka]

[0198] [ka]

[0199] Through the above steps, the electrophotographic photoreceptor of Example 1 was obtained.

[0200] <Examples 2 to 7> An electrophotographic photoreceptor was obtained in the same manner as in Example 1, except that specific copolymers (2) to (7) in which the proportions of each structural unit in specific copolymer (1) were changed as shown in Table 1 were used as the binder resin used in preparing the coating liquid for forming the charge generating layer. The weight average molecular weights and THF solubilities of the specific copolymers (2) to (7) are also shown in Table 1.

[0201] <Examples 8 to 14> Each electrophotographic photoreceptor was obtained in the same manner as in Examples 1 to 7, except that the type of charge generating material used in preparing the coating liquid for forming a charge generating layer was changed to chlorogallium phthalocyanine pigment (ClGaPc).

[0202] <Examples 15 to 21> Each electrophotographic photoreceptor was obtained in the same manner as in Examples 1 to 7, except that the type of charge generating material used in preparing the coating liquid for forming a charge generating layer was changed to titanyl phthalocyanine pigment (TiOPc).

[0203] <Comparative Example 1> An electrophotographic photoreceptor was obtained in the same manner as in Example 1, except that the following vinyl copolymer (C1) was used as the binder resin in the preparation of the coating liquid for forming a charge generating layer. Vinyl copolymer (C1): R represented by the above general formula (1) as a chlorine-containing component 11 ~R 13 and R 21 ~R 23 are all hydrogen atoms and R 24 A vinyl copolymer consisting of a structural unit in which the methyl group is a methyl group and a component derived from maleic acid as another polycarboxylic acid component, the ratio of each structural component being as shown in Table 1. The weight average molecular weight and THF solubility of the vinyl copolymer (C1) are also shown in Table 1.

[0204] <Comparative Examples 2 to 7> An electrophotographic photoreceptor was obtained in the same manner as in Comparative Example 1, except that vinyl copolymers (C2) to (C7) in which the proportions of each structural unit in the vinyl copolymer (C1) were changed as shown in Table 1 were used as the binder resin used in preparing the coating liquid for forming the charge generating layer. The weight average molecular weights and THF solubilities of the vinyl copolymers (C2) to (C7) are also shown in Table 1.

[0205] <Comparative Examples 8 to 9> An electrophotographic photoreceptor was obtained in the same manner as in Example 1, except that specific copolymers (8) to (9) in which the ratio of each structural unit in specific copolymer (1) was changed as shown in Table 1 were used as the binder resin used in preparing the coating liquid for forming the charge generating layer. The weight average molecular weights and THF solubilities of the specific copolymers (8) to (9) are also shown in Table 1.

[0206] <Comparative Example 10> An electrophotographic photoreceptor was obtained in the same manner as in Example 1, except that the following vinyl copolymer (C8) was used as the binder resin in the preparation of the coating liquid for forming a charge generating layer. Vinyl copolymer (C8): R represented by the general formula (1) as a chlorine-containing component 11 ~R 13 and R 21 ~R 23 are all hydrogen atoms and R 24 A vinyl copolymer consisting of a structural unit in which the carboxyl group is a methyl group and a component derived from hydroxybutyl acrylate as another polycarboxylic acid component, the ratio of each structural component being as shown in Table 1.

[0207] <Comparative Example 11> An electrophotographic photoreceptor was obtained in the same manner as in Comparative Example 10, except that a vinyl copolymer (C9) in which the ratio of each structural unit in the vinyl copolymer (C8) was changed as shown in Table 1 was used as the binder resin used in preparing the coating liquid for forming the charge generating layer. The weight average molecular weight and THF solubility of the vinyl copolymer (C9) are also shown in Table 1.

[0208] <Comparative Examples 12 to 18> Each electrophotographic photoreceptor was obtained in the same manner as in Comparative Examples 1 to 7, except that the type of charge generating material used in preparing the coating liquid for forming a charge generating layer was changed to chlorogallium phthalocyanine pigment (ClGaPc).

[0209] <Comparative Examples 19 to 25> Each electrophotographic photoreceptor was obtained in the same manner as in Comparative Examples 1 to 7, except that the type of charge generating material used in preparing the coating liquid for forming a charge generating layer was changed to titanyl phthalocyanine pigment (TiOPc).

[0210] [Table 1]

[0211] <Evaluation> (Evaluation of Image Density Difference) The electrophotographic photoreceptor obtained in each example was mounted on an electrophotographic image forming apparatus (ApeosPort-V C7776 manufactured by Fuji Xerox Co., Ltd.), and 1000 sheets of A3 size paper were printed with a full-face halftone image (full-face halftone image of cyan color) with an image density of 70%. All image printing was performed in an environment of 10°C and 15% RH. For the full-surface halftone image on the 1000th sheet, the image density was measured and averaged using an image densitometer (X-Rite938: manufactured by X-Rite) at five locations in each region corresponding to one end and the other end in the axial direction of the electrophotographic photosensitive member, and the image density difference (i.e., the absolute value of "average image density at one end" - "average image density at the other end") was calculated and evaluated according to the following evaluation criteria. The results are shown in Tables 2 and 3. Note that up to G2 is within the acceptable range.

[0212] -Evaluation criteria- G0:0 ≦ Image density difference ≦ 0.05 G1:0.05 < Image density difference ≦ 0.1 G2:0.1 < image density difference ≦ 0.2 G3:0.2 < Image density difference ≦ 0.25 G4:0.25 < Image density difference ≦ 0.3 G5:0.3 < Image density difference ≦ 0.35 G6:0.35 < image density difference

[0213] (Sensitivity evaluation) The sensitivity of the electrophotographic photosensitive member of each example was evaluated in terms of the half-life exposure when the electrophotographic photosensitive member was charged to +800V. Specifically, first, using an electrostatic copying paper tester (Electrostatic Analyzer EPA-8100, manufactured by Kawaguchi Electric Co., Ltd.), the electrophotographic photoconductor of each example was charged to +800 V in an environment of temperature 20°C / relative humidity 40%. Thereafter, the light of a tungsten lamp was converted to monochromatic light of 800 nm using a monochromator, and 1 μW / cm was applied to the surface of the electrophotographic photoconductor. 2 The light amount was adjusted so that the surface potential Vo (V) of the electrophotographic photosensitive member immediately after charging was reduced by half due to the light irradiation (μJ / cm 2 The half-life exposure values ​​obtained were classified according to the following criteria. The results are shown in Tables 2 and 3.

[0214] G1: Half-life exposure is 0.10μJ / cm 2 The results were as follows. G2: Half-life exposure is 0.10μJ / cm 2 Exceeds 0.13μJ / cm 2 The results were as follows. G3: Half-life exposure is 0.13μJ / cm 2 Exceeds 0.15μJ / cm 2 The results were as follows. G4: Half-life exposure is 0.15μJ / cm 2 Exceeds 0.18μJ / cm 2 The results were as follows. G5: Half-life exposure is 0.18μJ / cm 2 It exceeded that.

[0215] In each example, the ratio of the polycarboxylic acid component to the total components of the specific copolymer or vinyl-based copolymer is A mass %, and the content of the charge generating material relative to the specific copolymer or vinyl-based copolymer is C mass %. The A / C value is also shown in Tables 2 to 3.

[0216] [Table 2]

[0217] [Table 3]

[0218] From the above results, it is understood that the electrophotographic photosensitive member of this example has a suppressed image density difference in the axial direction of the electrophotographic photosensitive member, as compared with the electrophotographic photosensitive member of the comparative example. [Explanation of symbols]

[0219] 1 undercoat layer, 2 charge generation layer, 3 charge transport layer, 4 conductive substrate, 5 photosensitive layer, 7 electrophotographic photoreceptor, 7A electrophotographic photoreceptor, 8 charging device, 9 exposure device, 11 developing device, 13 cleaning device, 14 lubricant, 40 transfer device, 50 intermediate transfer body, 100 image forming apparatus, 120 image forming apparatus, 131 cleaning blade, 132 fibrous member (roll-shaped), 133 fibrous member (flat brush-shaped), 300 process cartridge

Claims

1. A conductive substrate; a charge generating layer provided on the conductive substrate, the charge generating layer comprising a charge generating material and a vinyl copolymer, the vinyl copolymer comprising a chlorine-containing structural unit, an acyloxy group-containing structural unit, and an aromatic polycarboxylic acid structure-containing structural unit, the proportion of the chlorine-containing structural unit to all structural units being 80% by mass or more, and the proportion of the aromatic polycarboxylic acid structure-containing structural unit to all structural units being 0.5% by mass or more; a charge transport layer provided on the charge generating layer and containing a charge transport material and a binder resin; An electrophotographic photoreceptor comprising:

2. 2. The electrophotographic photoreceptor according to claim 1, wherein the proportion of the chlorine-containing structural units is 88% by mass or less based on all structural units constituting the vinyl copolymer.

3. 3. The electrophotographic photoreceptor according to claim 2, wherein the proportion of the chlorine-containing structural units is 80% by mass or more and 87% by mass or less with respect to all structural units constituting the vinyl copolymer.

4. A conductive substrate; a charge generating layer provided on the conductive substrate, the charge generating layer containing a charge generating material and a vinyl copolymer, the vinyl copolymer containing a chlorine-containing structural unit, an acyloxy group-containing structural unit, and an aromatic polycarboxylic acid structure-containing structural unit, the solubility of the vinyl copolymer in 100 parts by mass of tetrahydrofuran at 30° C. being 10 parts by mass or less; a charge transport layer provided on the charge generating layer and containing a charge transport material and a binder resin; An electrophotographic photoreceptor comprising:

5. When the ratio of the structural unit having the aromatic polycarboxylic acid structure to all structural units constituting the vinyl copolymer is A% by mass, and the content of the charge generating material in the vinyl copolymer is C% by mass, the value of A / C is 3.00×10 -3 Above 1.40 x 10 -2 The electrophotographic photoreceptor according to any one of claims 1 to 4, wherein:

6. The electrophotographic photoreceptor according to any one of claims 1 to 5, wherein the structural unit having chlorine is represented by the following general formula (1), and the structural unit having an acyloxy group is represented by the following general formula (2): 【Chemistry 1】 [In the above general formula (1), R 11 ~R 13 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; 21 ~R 23 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; R 24 represents an alkyl group having 1 to 5 carbon atoms.

7. R in the general formula (1) 11 ~R 13 are all hydrogen atoms, and R 21 ~R 23 are all hydrogen atoms, R 24 The electrophotographic photoreceptor according to claim 6 , wherein is a methyl group.

8. 8. The electrophotographic photoreceptor according to claim 1, wherein the structural unit having an aromatic polycarboxylic acid structure is a structural unit having a phthalic acid structure.

9. The electrophotographic photoreceptor according to any one of claims 1 to 8 is provided, A process cartridge that is detachably attached to an image forming apparatus.

10. An electrophotographic photoreceptor according to any one of claims 1 to 8, a charging means for charging the surface of the electrophotographic photoreceptor; an electrostatic latent image forming means for forming an electrostatic latent image on the charged surface of the electrophotographic photoreceptor; a developing unit for developing an electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing a toner to form a toner image; a transfer means for transferring the toner image onto a surface of a recording medium; An image forming apparatus comprising:

Citation Information

Patent Citations

  • Electrophotographic sensitive body

    JP1993019507A

  • Electro-photoreceptor and electrophotographic device

    JP1999174695A

  • Electrophotographic photoreceptor, its production and electrophotographic device

    JP2000267317A

  • Electrophotographic photoreceptor, process cartridge, and image forming apparatus

    JP2019184700A