Fluorine-containing ether compound, lubricant for magnetic recording medium, and magnetic recording medium

A fluorine-containing ether compound with a specific terminal group improves adhesion and wear resistance, addressing the challenges of reduced thickness in magnetic recording media by suppressing pickup and enhancing durability.

JP7567801B2Active Publication Date: 2024-10-16RESONAC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021550517
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-01
Filing Date
2020-09-08
Publication Date
2024-10-16
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

Magnetic recording media face challenges in reducing lubricant layer thickness to lower flying height, leading to reduced wear resistance and increased pickup of the fluorine-containing ether compound on the magnetic head due to insufficient adhesion and coverage.

Method used

A fluorine-containing ether compound with a specific terminal group (-OCH2CH(OH)CH2O(CH2)mOH) is used, which enhances adhesion through intermolecular interactions with the protective layer, providing improved wear resistance and suppressing pickup even at reduced thickness.

Benefits of technology

The compound forms a lubricant layer with excellent wear resistance and suppressed pickup, ensuring high reliability and durability of the magnetic recording medium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567801000040
    Figure 0007567801000040
  • Figure 0007567801000001
    Figure 0007567801000001
  • Figure 0007567801000002
    Figure 0007567801000002
Patent Text Reader

Abstract

This fluorine-containing ether compound is characterized by being represented by formula (1). (1): C6H6-n-[O-R1-O-CH2-R2-CH2-R3]n (in formula (1), n is an integer of 2 or 3, R1 is -CH2CH2-, -CH2CH2CH2-, or -CH2CH(OH)CH2-, R2 is a perfluoropolyether chain, and R3 is -OCH2CH(OH)CH2O(CH2)mOH (wherein m is an integer of 2-4)).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fluorine-containing ether compound suitable for use as a lubricant for magnetic recording media, a lubricant for magnetic recording media containing the same, and a magnetic recording medium. This application claims priority based on Japanese Patent Application No. 2019-181309, filed on October 1, 2019, the contents of which are incorporated herein by reference. [Background technology]

[0002] In order to improve the recording density of magnetic recording and reproducing devices, development of magnetic recording media suitable for high recording density is underway. Conventionally, magnetic recording media include those in which a recording layer is formed on a substrate and a protective layer such as carbon is formed on the recording layer. The protective layer protects the information recorded on the recording layer and also improves the sliding properties of the magnetic head. However, the durability of the magnetic recording medium cannot be sufficiently obtained by simply providing a protective layer on the recording layer. For this reason, a lubricant is generally applied to the surface of the protective layer to form a lubricating layer.

[0003] As a lubricant used in forming a lubricating layer of a magnetic recording medium, for example, one that contains a compound having a polar group such as a hydroxyl group at the end of a fluorine-based polymer having a repeating structure containing CF2 has been proposed. For example, Patent Document 1 discloses a fluoropolyether compound having an aromatic group and a hydroxyl group. Furthermore, Patent Document 2 discloses a fluoropolyether compound in which a benzene ring is di- or tri-substituted with a fluoropolyether chain having a hydroxyl group at the molecular end. Furthermore, Patent Document 3 discloses a compound having a plurality of hydroxyl groups at both terminal portions, in which substituents are arranged such that the shortest distance between the hydroxyl groups is 3 atoms or more. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5816919 [Patent Document 2] Patent No. 6198848 [Patent Document 3] Patent No. 4632144 Summary of the Invention [Problem to be solved by the invention]

[0005] In magnetic recording and reproducing devices, there is a demand for an even smaller flying height of the magnetic head, which in turn requires a thinner lubricating layer in the magnetic recording medium. However, generally, when the thickness of the lubricating layer is reduced, the covering property of the lubricating layer is reduced, and the wear resistance of the magnetic recording medium tends to be reduced.In addition, when the thickness of the lubricating layer is reduced, the adhesion between the lubricating layer covering the surface of the protective layer and the protective layer is insufficient, and the fluorine-containing ether compound in the lubricating layer is easily attached to the magnetic head, which is called pick-up.

[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a fluorine-containing ether compound which can form a lubricating layer that has excellent wear resistance and suppresses pick-up even when made thin, and which can be suitably used as a material for a lubricant for a magnetic recording medium. Another object of the present invention is to provide a lubricant for magnetic recording media, which contains the fluorine-containing ether compound of the present invention. Another object of the present invention is to provide a magnetic recording medium having excellent reliability and durability, which has a lubricating layer containing the fluorinated ether compound of the present invention. [Means for solving the problem]

[0007] The present inventors have conducted extensive research in order to solve the above problems. As a result, -OCH2CH(OH)CH2O(CH2) mThe present inventors have found that a fluorine-containing ether compound can be obtained by forming a perfluoropolyether chain in which an end group consisting of OH (wherein m is an integer of 2 to 4) is bonded via a methylene group (-CH2-), and in which two or three hydrogen atoms of the benzene ring are substituted by substituents bonded to a specific linking group, and have arrived at the present invention. That is, a first aspect of the present invention is the following fluorine-containing ether compound.

[0008] [1] A fluorinated ether compound represented by the following formula (1): C6H 6-n -[OR 1 -O-CH2-R 2 -CH2-R 3 ] n (1) (In formula (1), n ​​is an integer of 2 or 3, and R 1 is -CH2CH2-, -CH2CH2CH2-, or -CH2CH(OH)CH2-, and R 2 is a perfluoropolyether chain, and R 3 -OCH2CH(OH)CH2O(CH2) m OH (wherein m is an integer of 2 to 4).

[0009] The fluorine-containing ether compound according to the first aspect of the present invention can preferably include the following characteristics, as described below. Two or more of the following characteristics may be preferably combined. [2] R in the above formula (1) 2 is represented by any one of the following formulas (2) to (4):

[0010] [ka] (In formula (2), p represents 1 to 30, and q represents 0 to 30.) (In formula (3), r represents 1 to 30.) (In formula (4), s represents 1 to 20.)

[0011] [3] The fluorine-containing ether compound according to [2], which is any of the compounds represented by the following formulas (A) to (N):

[0012] [ka] (In formula (A), R 2 is expressed by the above formula (2). (In formula (B), R 2 is expressed by the above formula (3). (In formula (C), R 2 is expressed by the above formula (4). (In formula (D), R 2 is expressed by the above formula (2). (In formula (E), R 2 is expressed by the above formula (2). (In formula (F), R 2 is represented by the above formula (2). (In formula (G), R 2 is expressed by the above formula (3). (In formula (H), R 2 is expressed by the above formula (4).

[0013] [ka] (In formula (I), R 2 is expressed by the above formula (2). (In formula (J), R 2 is expressed by the above formula (2). (In formula (K), R 2 is expressed by the above formula (3). (In formula (L), R 2 is expressed by the above formula (4). (In formula (M), R 2 is represented by the above formula (2). (In formula (N), R 2 is represented by the above formula (2).

[0014] [4] The fluorinated ether compound according to any one of [1] to [3], which has a number average molecular weight in the range of 500 to 10,000.

[0015] [5] A lubricant for magnetic recording media, comprising the fluorine-containing ether compound according to any one of [1] to [4]. [6] A magnetic recording medium comprising at least a magnetic layer, a protective layer, and a lubricating layer provided in that order on a substrate, the lubricating layer comprising a fluorine-containing ether compound according to any one of [1] to [4]. [7] The magnetic recording medium according to [6], wherein the average thickness of the lubricating layer is 0.5 nm to 3 nm. Effect of the Invention

[0016] The fluorine-containing ether compound of the present invention is suitable as a material for a lubricant for a magnetic recording medium. Since the lubricant for magnetic recording media of the present invention contains the fluorine-containing ether compound of the present invention, it is possible to form a lubricating layer that has excellent wear resistance and suppresses pick-up even when the thickness is reduced. The magnetic recording medium of the present invention has excellent wear resistance and is provided with a lubricating layer that suppresses pick-up, and therefore has excellent reliability and durability. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a magnetic recording medium of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Preferred examples of the fluorine-containing ether compound, the lubricant for magnetic recording media (hereinafter sometimes abbreviated as "lubricant"), and the magnetic recording media of the present invention will be described in detail below. The present invention is not limited to the following embodiments. Within the scope of the present invention, the number, position, type, amount, ratio, combination, numerical value, size, etc. can be omitted, changed, and / or added as necessary.

[0019] [Fluorine-containing ether compounds] The fluorine-containing ether compound of the present embodiment is represented by the following formula (1). C6H 6-n -[OR 1 -O-CH2-R 2 -CH2-R 3 ] n (1) (In formula (1), n ​​is an integer of 2 or 3, and R 1 is -CH2CH2-, -CH2CH2CH2-, or -CH2CH(OH)CH2-, and R 2 is a perfluoropolyether chain, and R 3 -OCH2CH(OH)CH2O(CH2) m OH (wherein m is an integer of 2 to 4).

[0020] Here, we will explain why, when a lubricating layer containing the fluorine-containing ether compound of this embodiment is used to form a lubricating layer on a protective layer of a magnetic recording medium, even if the layer is thin, excellent wear resistance is obtained and pick-up is suppressed.

[0021] The fluorine-containing ether compound of the present embodiment has a structure in which two or three of the hydrogen atoms on the benzene ring are substituted with a substituent (-[OR 1 -O-CH2-R 2 -CH2-R 3 ]) is substituted. The benzene ring contained in the fluorine-containing ether compound represented by formula (1) contributes to improving the adhesion between the fluorine-containing ether compound of this embodiment and the protective layer due to intermolecular interaction of the benzene ring and / or interaction between the benzene ring and the protective layer. For this reason, by using a lubricant containing the fluorine-containing ether compound represented by formula (1), a lubricating layer having excellent wear resistance can be obtained.

[0022] The two or three substituents contained in the fluorine-containing ether compound represented by formula (1) are each R 2When a lubricant containing a fluorine-containing ether compound is applied onto a protective layer to form a lubricating layer, the PFPE chain coats the surface of the protective layer and imparts lubricity to the lubricating layer, thereby reducing the friction between the magnetic head and the protective layer.

[0023] As shown in equation (1), R 2 The end of the PFPE chain opposite the benzene ring is connected to R via a methylene group (-CH-). 3 The terminal group represented by R 3 The terminal group represented by -OCH2CH(OH)CH2O(CH2) m OH (wherein m is an integer of 2 to 4). 3 The two hydroxyl groups (-OH) contained in the terminal group represented by the following formula (1) suppress pick-up by bonding the fluorine-containing ether compound and the protective layer in the lubricating layer containing the fluorine-containing ether compound of this embodiment.

[0024] R 3 In the terminal group represented by the formula:, two hydroxyl groups (-OH) are bonded to different carbon atoms, and the carbon atoms to which the hydroxyl groups are bonded are bonded via a linking group containing an oxygen atom (a linking group containing an -O- (ether bond)). A linking group containing an ether bond is represented by the formula: 3 For this reason, in the fluorine-containing ether compound of the present embodiment, the two hydroxyl groups contained in the terminal group are bonded to different carbon atoms, and the carbon atoms to which the hydroxyl groups are bonded are bonded to each other, so that the lubricating layer containing this fluorine-containing ether compound is more likely to be adsorbed to the protective film, and the adhesion between the lubricating layer and the protective layer is excellent.

[0025] In the fluorine-containing ether compound shown in formula (1), the benzene ring and R 2 A linking group (-OR 1The linking group containing an ether bond imparts flexibility to the fluorine-containing ether compound represented by formula (1). For this reason, the fluorine-containing ether compound of the present embodiment has, for example, a benzene ring and R 2 In comparison with a fluorine-containing ether compound in which a PFPE chain is directly bonded, as represented by the formula (1), a lubricating layer containing this compound is more likely to be adsorbed to a protective film, and the adhesion between the lubricating layer and the protective layer is excellent. From the above, it is presumed that the lubricant containing the fluorine-containing ether compound of this embodiment can cover the surface of a protective layer with a high coverage even when it is thin, and can form a lubricating layer that has excellent wear resistance and suppresses pick-up.

[0026] In the fluorine-containing ether compound of the present embodiment represented by formula (1), the substituent (-[OR 1 -O-CH2-R 2 -CH2-R 3 ]) (the number of n in formula (1)) is two or three. The two or three substituents bonded to the benzene ring may be different from each other, or may be the same. It is preferable that the two or three substituents are all the same, since this facilitates the synthesis of the fluorine-containing ether compound. When two or three substituents contained in the fluorine-containing ether compound represented by formula (1) are not the same, R 1 , R 2 , R 3 may all be different, and R 1 , R 2 , R 3 Only one or two of them may be different.

[0027] In the fluorine-containing ether compound of the present embodiment represented by formula (1), R 1 is either -CH2CH2-, -CH2CH2CH2-, or -CH2CH(OH)CH2-. R 1 When is -CHCH(OH)CH-, R 1The hydroxyl group (-OH) contained in the lubricating layer containing the fluorinated ether compound of this embodiment is preferable because it brings the fluorinated ether compound into close contact with the protective layer, thereby suppressing pick-up.

[0028] In particular, when the number n in formula (1) is 2, R 1 is preferably -CH2CH(OH)CH2-. When the number of n in formula (1) is 2, R 3 The number of hydroxyl groups in the fluorine-containing ether compound derived from the terminal group represented by the formula (1) is four. Therefore, compared with the case where the number of n in the formula (1) is three, R 3 The number of hydroxyl groups derived from the terminal group represented by the formula (1) is reduced by two. The hydroxyl groups in the fluorine-containing ether compound contribute to improving the adhesion between the lubricating layer containing the fluorine-containing ether compound and the protective layer. For example, when the number of n in the formula (1) is two, two substituents (-[OR 1 -O-CH2-R 2 -CH2-R 3 ]) 1 In this case, the number of hydroxyl groups in the fluorine-containing ether compound is R 1 Two derived from R 3 The total number of n is six, including the four from the terminal group represented by n = 2. As a result, the number of n is two, so compared to when the number of n is three, R 3 Even if the number of hydroxyl groups derived from the terminal group represented by the formula (I) is small, the adhesion between the lubricating layer containing the fluorine-containing ether compound and the protective layer becomes good, which is preferable.

[0029] In the fluorine-containing ether compound of the present embodiment represented by formula (1), R 2 is a perfluoropolyether chain (PFPE chain). R 2 may be different from each other or may include the same ones, and it is preferable that they are all the same. R 2 is not particularly limited and can be appropriately selected depending on the performance required of the lubricant containing the fluorine-containing ether compound.

[0030] R 2 is preferably any one of the following formulas (2) to (4). 2 When the formula is any one of formulas (2) to (4), the synthesis of the fluorine-containing ether compound is easy, which is preferable. Also, R 2 When R is any one of formulas (2) to (4), the ratio of the number of oxygen atoms (the number of ether bonds (-O-)) to the number of carbon atoms in the perfluoropolyether chain is appropriate. This results in a fluorine-containing ether compound with appropriate hardness. Therefore, the fluorine-containing ether compound applied onto the protective layer is less likely to aggregate on the protective layer, and a thinner lubricating layer can be formed with a sufficient coverage. In addition, R 2 When is any one of the formulas (2) to (4), the fluorine-containing ether compound provides a lubricating layer having good wear resistance.

[0031] [ka] (In formula (2), p represents 1 to 30, and q represents 0 to 30.) (In formula (3), r represents 1 to 30.) (In formula (4), s represents 1 to 20.)

[0032] In formula (2), the arrangement order of the repeating units (CF2-CF2-O) and (CF2-O) is not particularly limited. In formula (2), the number p of (CF2-CF2-O) and the number q of (CF2-O) may be the same or different. Formula (2) may include any of a random copolymer, a block copolymer, and an alternating copolymer composed of the monomer units (CF2-CF2-O) and (CF2-O).

[0033] R in formula (1) 2 When R is represented by formula (2), p, which indicates the average degree of polymerization, is 1 to 30, preferably 1 to 15, and more preferably 1 to 7. p may be 1 to 6 or 2 to 5. 2When the formula (2) is represented, q indicating the average degree of polymerization is 0 to 30, preferably 0 to 15, and more preferably 0 to 7. q may be 1 to 6 or 2 to 5. When q is 0, p is preferably 1 to 10.

[0034] In formula (3), when r, which indicates the average degree of polymerization, is 1 to 30, the number average molecular weight of the fluorinated ether compound of this embodiment tends to be in the preferred range. r is preferably 1 to 10, and more preferably 1 to 5.

[0035] In formula (4), when s, which indicates the average degree of polymerization, is 1 to 20, the number average molecular weight of the fluorinated ether compound of this embodiment tends to be in the preferred range. s is preferably 1 to 10, and more preferably 1 to 5.

[0036] In formula (1), R 3 -OCH2CH(OH)CH2O(CH2) m OH (wherein m is an integer of 2 to 4). m is an integer of 2 to 4, and is preferably 2.

[0037] Specifically, the fluorine-containing ether compound represented by formula (1) is preferably any of the compounds represented by the following formulae (A) to (N). 2 is any one of the above formulas (2) to (4), and the above-mentioned preferable conditions for formulas (2) to (4) are 2 It is also preferable in the above. R in formulas (A) to (N) 2 The p, q, r, and s in R are values ​​that indicate the average degree of polymerization, and are not necessarily integers. 2 In the formula (2), p in the formula (2) represents 1 to 30, and q represents 0 to 30. 2 When R is the formula (3), r in the formula (3) represents 1 to 30. 2is formula (4), s in formula (4) represents 1 to 20. In all of the compounds represented by formulas (A) to (N), the two or three substituents bonded to the benzene ring are all the same.

[0038] The compound represented by formula (A) is a compound represented by formula (A) in which n is 2 and R 1 is -CH2CH(OH)CH2-, and R 2 is formula (2), and R 3 The m of is 2. The compound represented by formula (B) is a compound represented by formula (B) in which n is 2 and R 1 is -CH2CH(OH)CH2, and R 2 is formula (3), and R 3 The m of is 2. The compound represented by formula (C) is a compound represented by formula (C) in which n is 2 and R 1 is -CH2CH(OH)CH2-, and R 2 is Equation (4), and R 3 The m of is 2. The compound represented by formula (D) is a compound represented by formula (D) in which n is 2 and R 1 is -CH2CH(OH)CH2-, and R 2 is formula (2), and R 3 The m of is 3. The compound represented by formula (E) is a compound represented by formula (E) in which n is 2 and R 1 is -CH2CH(OH)CH2-, and R 2 is formula (2), and R 3 The m of is 4. The compound represented by formula (F) is a compound represented by formula (F) in which n is 2 and R 1 is -CH2CH2- and R 2 is formula (2), and R 3 The m of is 2. The compound represented by formula (G) is a compound represented by formula (G) in which n is 2 and R 1 is -CH2CH2- and R 2 is formula (3), and R 3 The m of is 2. The compound represented by formula (H) is a compound represented by formula (H) in which n is 2 and R 1 is -CH2CH2- and R 2 is Equation (4), and R 3 The m of is 2.

[0039] The compound of formula (I) is a compound in which n is 3 and R 1 is -CH2CH(OH)CH2-, and R 2 is formula (2), and R 3 The m of is 2. The compound represented by formula (J) is a compound represented by formula (J) in which n is 3 and R 1 is -CH2CH2CH2- and R 2 is formula (2), and R 3 The m of is 2. The compound represented by formula (K) is a compound represented by formula (K) in which n is 3 and R 1 is -CH2CH2CH2- and R 2 is formula (3), and R 3 The m of is 2. The compound represented by formula (L) is a compound represented by formula (L) in which n is 3 and R 1 is -CH2CH2CH2- and R 2 is Equation (4), and R 3 The m of is 2. The compound represented by formula (M) is a compound represented by formula (M) in which n is 3 and R 1 is -CH2CH2CH2- and R 2 is formula (2), and R 3 The m of is 3. The compound represented by formula (N) is a compound represented by formula (N) in which n is 3 and R 1 is -CH2CH2CH2- and R 2 is formula (2), and R 3 The m of is 4.

[0040] [ka] (In formula (A), R 2 is represented by the above formula (2). (In formula (B), R 2 is expressed by the above formula (3). (In formula (C), R 2 is expressed by the above formula (4). (In formula (D), R 2 is represented by the above formula (2). (In formula (E), R 2is represented by the above formula (2). (In formula (F), R 2 is represented by the above formula (2). (In formula (G), R 2 is expressed by the above formula (3). (In formula (H), R 2 is expressed by the above formula (4).

[0041] [ka] (In formula (I), R 2 is represented by the above formula (2). (In formula (J), R 2 is represented by the above formula (2). (In formula (K), R 2 is expressed by the above formula (3). (In formula (L), R 2 is expressed by the above formula (4). (In formula (M), R 2 is represented by the above formula (2). (In formula (N), R 2 is represented by the above formula (2).

[0042] When the compound represented by formula (1) is any of the compounds represented by the above formulas (A) to (N), the raw materials are easily available, and a lubricating layer can be formed that has better wear resistance and is more suppressed in pick-up even if it is thin. This is preferable.

[0043] The number average molecular weight (Mn) of the fluorine-containing ether compound of this embodiment is preferably within the range of 500 to 10,000. When the number average molecular weight is 500 or more, the lubricant containing the fluorine-containing ether compound of this embodiment is less likely to evaporate, and the lubricant can be prevented from evaporating and transferring to the magnetic head. The number average molecular weight of the fluorine-containing ether compound is more preferably 1,000 or more. In addition, when the number average molecular weight is 10,000 or less, the viscosity of the fluorine-containing ether compound is appropriate, and a thin lubricating layer can be easily formed by applying a lubricant containing this. The number average molecular weight of the fluorine-containing ether compound is preferably 3,000 or less, since the viscosity becomes easy to handle when applied to a lubricant.

[0044] The number average molecular weight (Mn) of fluorine-containing ether compounds was measured using AVANCEIII400 manufactured by Bruker Biospin. 1 H-NMR and 19 This is a value measured by F-NMR. In the NMR (nuclear magnetic resonance) measurement, the sample was diluted in a single or mixed solvent such as hexafluorobenzene, d-acetone, or d-tetrahydrofuran and used for the measurement. 19 The standard for F-NMR chemical shifts is the hexafluorobenzene peak at -164.7 ppm. 1 The reference for H-NMR chemical shifts was set to the acetone peak at 2.2 ppm.

[0045] "Manufacturing method" The method for producing the fluorinated ether compound of the present embodiment is not particularly limited, and the compound can be produced by a conventionally known production method. The fluorinated ether compound of the present embodiment can be produced, for example, by the production method shown below.

[0046] First, R in Equation (1) 2A compound having a perfluoropolyether chain corresponding to the above formula is prepared, and this compound is subjected to an addition reaction with benzene substituted with two or three halogenated alkoxy groups having two or three carbon atoms, or benzene substituted with two or three glycidyloxy groups, to produce a compound represented by formula (1-1). C6H 6-n -[OR 1 -O-CH2-R 2 -CH2-OH] n (1-1) (In formula (1-1), n ​​is an integer of 2 or 3, and R 1 is -CH2CH2-, -CH2CH2CH2-, or -CH2CH(OH)CH2-, and R 2 is a perfluoropolyether chain.)

[0047] Examples of the benzene substituted with three halogenated alkoxy groups used in producing the compound represented by formula (1-1) include 1,3,5-tri(bromopropoxy)benzene, 1,2,3-tri(bromopropoxy)benzene, 1,2,4-tri(bromopropoxy)benzene, 1,3,5-tri(bromoethoxy)benzene, 1,2,3-tri(bromoethoxy)benzene, and 1,2,4-tri(bromoethoxy)benzene. Examples of benzene substituted with two halogenated alkoxy groups include o-di(bromopropoxy)benzene, m-di(bromopropoxy)benzene, p-di(bromopropoxy)benzene, o-di(bromoethoxy)benzene, m-di(bromoethoxy)benzene, and p-di(bromoethoxy)benzene.

[0048] A di- or tri-substituted benzene with halogenated alkoxy groups can be obtained, for example, by the addition reaction of a dihydroxybenzene or trihydroxybenzene with 1,3-dibromopropane or 1,2-dibromoethane.

[0049] Examples of the benzene substituted with three glycidyloxy groups used in producing the compound represented by formula (1-1) include 1,3,5-tri(glycidyloxy)benzene, 1,2,3-tri(glycidyloxy)benzene, and 1,2,4-tri(glycidyloxy)benzene. Examples of benzene substituted with two glycidyloxy groups include 1,3-bis(glycidyloxy)benzene, 1,2-bis(glycidyloxy)benzene, and 1,4-bis(glycidyloxy)benzene.

[0050] A benzene substituted with two or three glycidyloxy groups can be obtained, for example, by the addition reaction of a dihydroxybenzene or trihydroxybenzene with epichlorohydrin or epibromohydrin.

[0051] Next, the compound represented by formula (1-1) is reacted with epichlorohydrin or epibromohydrin to form the compound represented by formula (1-1) with two or three substituents (-[OR 1 -O-CH2-R 2 A perfluoropolyether is produced in which the terminal hydrogen of the aryl group (-CH2-OH) is replaced by a glycidyl group. The perfluoropolyether produced is a compound in which two or three substituents having epoxy groups at the terminals are bonded to a benzene ring. Next, a compound selected from ethylene glycol, 1,3-propanediol, and 1,4-butanediol is reacted with the perfluoropolyether produced by the above method. The compound thus obtained can be separated, for example, by a method using column chromatography. By the above method, the fluorine-containing ether compound represented by formula (1) can be obtained.

[0052] The fluorine-containing ether compound of the present embodiment is a compound represented by the above formula (1). Therefore, when a lubricating layer is formed on a protective layer using a lubricant containing this compound, R 2The surface of the protective layer is covered with the PFPE chain represented by the formula (1), and the frictional force between the magnetic head and the protective layer is reduced. In addition, the lubricating layer formed using the lubricant containing the fluorine-containing ether compound of this embodiment has excellent adhesion to the protective layer due to the intermolecular interaction of the benzene ring and / or the interaction between the benzene ring and the protective layer.

[0053] In addition, the lubricating layer containing the fluorine-containing ether compound of this embodiment is preferably a lubricating layer containing the fluorine-containing ether compound R 3 The two hydroxyl groups contained in the terminal groups represented by R 3 The two hydroxyl groups contained in the terminal group represented by are bonded to different carbon atoms, and the carbon atoms to which the hydroxyl groups are bonded are bonded to each other via a linking group containing an oxygen atom, so the lubricating layer containing the fluorine-containing ether compound of this embodiment has good flexibility.Therefore, the lubricating layer containing the fluorine-containing ether compound of this embodiment is easily adsorbed to the protective film and has excellent adhesion to the protective layer. From the above, according to the fluorine-containing ether compound of this embodiment, the lubricating layer and the protective layer are firmly bonded to each other, and a lubricating layer having excellent abrasion resistance and suppressing pick-up can be obtained.

[0054] [Lubricants for magnetic recording media] The lubricant for a magnetic recording medium of this embodiment contains a fluorine-containing ether compound represented by formula (1). The lubricant of the present embodiment can be used by mixing, as necessary, known materials used as lubricant materials, so long as the properties resulting from the inclusion of the fluorinated ether compound represented by formula (1) are not impaired.

[0055] Specific examples of known materials include FOMBLIN (registered trademark) ZDIAC, FOMBLIN ZDEAL, FOMBLIN AM-2001 (all manufactured by Solvay Solexis), Moresco A20H (manufactured by Moresco), etc. The known material to be mixed with the lubricant of the present embodiment preferably has a number average molecular weight of 1,000 to 10,000.

[0056] When the lubricant of this embodiment contains a material other than the fluorinated ether compound represented by formula (1), the content of the fluorinated ether compound represented by formula (1) in the lubricant of this embodiment is preferably 50% by mass or more, more preferably 70% by mass or more. It may be 80% by mass or more, or 90% by mass or more. The upper limit can be selected arbitrarily, and may be, for example, 99% by mass or less, 95% by mass or less, or 90% by mass or less.

[0057] The lubricant of the present embodiment contains the fluorine-containing ether compound represented by formula (1), so that even if the thickness is thin, the surface of the protective layer can be covered with a high coverage rate, and a lubricant layer having excellent adhesion to the protective layer can be formed. Therefore, according to the lubricant of the present embodiment, even if the thickness is thin, a lubricant layer having excellent wear resistance and suppressed pick-up can be obtained.

[0058] [Magnetic recording media] The magnetic recording medium of this embodiment has at least a magnetic layer, a protective layer, and a lubricating layer provided in this order on a substrate. In the magnetic recording medium of this embodiment, one or more underlayers may be provided between the substrate and the magnetic layer, if necessary. Also, an adhesive layer and / or a soft magnetic layer may be provided between the underlayer and the substrate.

[0059] FIG. 1 is a schematic cross-sectional view showing one embodiment of a magnetic recording medium of the present invention. The magnetic recording medium 10 of this embodiment has a structure in which an adhesive layer 12, a soft magnetic layer 13, a first underlayer 14, a second underlayer 15, a magnetic layer 16, a protective layer 17, and a lubricating layer 18 are sequentially provided on a substrate 11.

[0060] "substrate" The substrate 11 may be, for example, a non-magnetic substrate in which a film made of NiP or a NiP alloy is formed on a base made of a metal or alloy material such as Al or an Al alloy. Furthermore, the substrate 11 may be a non-magnetic substrate made of a non-metallic material such as glass, ceramics, silicon, silicon carbide, carbon, or resin, or a non-magnetic substrate having a NiP or NiP alloy film formed on a base made of these non-metallic materials.

[0061] "Adhesion layer" The adhesive layer 12 prevents the progress of corrosion of the substrate 11, which occurs when the substrate 11 and the soft magnetic layer 13 provided on the adhesive layer 12 are disposed in contact with each other. The material of the adhesive layer 12 can be appropriately selected from, for example, Cr, a Cr alloy, Ti, a Ti alloy, CrTi, NiAl, an AlRu alloy, etc. The adhesive layer 12 can be formed by, for example, a sputtering method.

[0062] "Soft magnetic layer" The soft magnetic layer 13 preferably has a structure in which a first soft magnetic film, an intermediate layer made of a Ru film, and a second soft magnetic film are laminated in this order. That is, the soft magnetic layer 13 preferably has a structure in which the intermediate layer made of a Ru film is sandwiched between two soft magnetic films, and the soft magnetic films above and below the intermediate layer are anti-ferro-coupling (AFC).

[0063] Examples of materials for the first and second soft magnetic films include a CoZrTa alloy and a CoFe alloy. It is preferable to add any one of Zr, Ta, and Nb to the CoFe alloy used in the first and second soft magnetic films, which promotes the amorphization of the first and second soft magnetic films, improves the orientation of the first underlayer (seed layer), and reduces the flying height of the magnetic head. The soft magnetic layer 13 can be formed by, for example, a sputtering method.

[0064] "First base layer" The first underlayer 14 is a layer for controlling the orientation and crystal size of the second underlayer 15 and the magnetic layer 16 provided thereon. The first underlayer 14 may be, for example, a Cr layer, a Ta layer, a Ru layer, or a CrMo, CoW, CrW, CrV, or CrTi alloy layer. The first underlayer 14 can be formed by, for example, a sputtering method.

[0065] "Second base layer" The second underlayer 15 is a layer that controls good orientation of the magnetic layer 16. The second underlayer 15 is preferably a layer made of Ru or a Ru alloy. The second underlayer 15 may be a layer consisting of one layer, or may be composed of multiple layers. When the second underlayer 15 is composed of multiple layers, all the layers may be composed of the same material, or at least one layer may be composed of a different material. The second underlayer 15 can be formed by, for example, a sputtering method.

[0066] "Magnetic layer" The magnetic layer 16 is a magnetic film with an easy axis of magnetization oriented perpendicular or parallel to the substrate surface. The magnetic layer 16 is, for example, a layer containing Co and Pt, and may be a layer containing an oxide, Cr, B, Cu, Ta, Zr, or the like to further improve the SNR characteristics. Examples of oxides contained in the magnetic layer 16 include SiO2, SiO, Cr2O3, CoO, Ta2O3, and TiO2.

[0067] The magnetic layer 16 may be composed of a single layer, or may be composed of multiple magnetic layers made of materials with different compositions. For example, when the magnetic layer 16 is composed of three layers, a first magnetic layer, a second magnetic layer, and a third magnetic layer, stacked in order from the bottom, the first magnetic layer preferably has a granular structure made of a material containing Co, Cr, and Pt and further containing an oxide. As the oxide contained in the first magnetic layer, for example, oxides such as Cr, Si, Ta, Al, Ti, Mg, and Co are preferably used. Among them, TiO2, Cr2O3, SiO2, and the like can be particularly preferably used. In addition, the first magnetic layer is preferably made of a composite oxide to which two or more kinds of oxides are added. Among them, Cr2O3-SiO2, Cr2O3-TiO2, SiO2-TiO2, and the like can be particularly preferably used.

[0068] The first magnetic layer may preferably contain, in addition to Co, Cr, Pt, and oxides, one or more elements selected from B, Ta, Mo, Cu, Nd, W, Nb, Sm, Tb, Ru, and Re. The second magnetic layer may be made of the same material as the first magnetic layer, and preferably has a granular structure.

[0069] The third magnetic layer preferably has a non-granular structure made of a material that contains Co, Cr, and Pt and does not contain oxides. In addition to Co, Cr, and Pt, the third magnetic layer preferably contains one or more elements selected from B, Ta, Mo, Cu, Nd, W, Nb, Sm, Tb, Ru, Re, and Mn.

[0070] When the magnetic layer 16 is formed of multiple magnetic layers, it is preferable to provide a nonmagnetic layer between adjacent magnetic layers. When the magnetic layer 16 is formed of three layers, a first magnetic layer, a second magnetic layer, and a third magnetic layer, it is preferable to provide a nonmagnetic layer between the first magnetic layer and the second magnetic layer and between the second magnetic layer and the third magnetic layer.

[0071] The non-magnetic layer provided between adjacent magnetic layers in the magnetic layer 16 can suitably be made of, for example, Ru, a Ru alloy, a CoCr alloy, or a CoCrX1 alloy (X1 represents one or more elements selected from Pt, Ta, Zr, Re, Ru, Cu, Nb, Ni, Mn, Ge, Si, O, N, W, Mo, Ti, V, and B).

[0072] For the non-magnetic layer provided between adjacent magnetic layers of the magnetic layer 16, it is preferable to use an alloy material containing an oxide, a metal nitride, or a metal carbide. Specifically, for example, SiO2, Al2O3, Ta2O5, Cr2O3, MgO, Y2O3, TiO2, etc. can be preferably used as the oxide. For example, AlN, Si3N4, TaN, CrN, etc. can be preferably used as the metal nitride. For example, TaC, BC, SiC, etc. can be preferably used as the metal carbide. The nonmagnetic layer can be formed by, for example, a sputtering method.

[0073] In order to achieve higher recording density, the magnetic layer 16 is preferably a magnetic layer for perpendicular magnetic recording in which the axis of easy magnetization is oriented perpendicular to the substrate surface, but may also be a magnetic layer for in-plane magnetic recording. The magnetic layer 16 may be formed by any known method such as vapor deposition, ion beam sputtering, magnetron sputtering, etc. The magnetic layer 16 is usually formed by sputtering.

[0074] "Protective layer" The protective layer 17 protects the magnetic layer 16. The protective layer 17 may be made of a single layer or multiple layers. Examples of materials for the protective layer 17 include carbon, carbon containing nitrogen, and silicon carbide. A carbon-based protective layer, particularly an amorphous carbon protective layer, can be preferably used as the protective layer 17. When the protective layer 17 is a carbon-based protective layer, the interaction with the hydroxyl group contained in the fluorine-containing ether compound in the lubricating layer 18 is further enhanced, which is preferable.

[0075] The adhesion between the carbon-based protective layer and the lubricating layer 18 can be controlled by making the carbon-based protective layer from hydrogenated carbon and / or nitrogenated carbon and adjusting the hydrogen content and / or nitrogen content in the carbon-based protective layer. The hydrogen content in the carbon-based protective layer is preferably 3 to 20 atomic % when measured by hydrogen forward scattering (HFS). The nitrogen content in the carbon-based protective layer is preferably 4 to 15 atomic % when measured by X-ray photoelectron spectroscopy (XPS).

[0076] The hydrogen and / or nitrogen contained in the carbon-based protective layer does not need to be uniformly contained throughout the carbon-based protective layer. The carbon-based protective layer is preferably a compositionally graded layer in which, for example, nitrogen is contained on the lubricating layer 18 side of the protective layer 17, and hydrogen is contained on the magnetic layer 16 side of the protective layer 17. In this case, the adhesion between the magnetic layer 16 and the lubricating layer 18 and the carbon-based protective layer is further improved.

[0077] The thickness of the protective layer 17 can be selected arbitrarily, but is preferably 1 nm to 7 nm. If the thickness of the protective layer 17 is 1 nm or more, sufficient performance as the protective layer 17 can be obtained. If the thickness of the protective layer 17 is 7 nm or less, it is preferable from the viewpoint of making the protective layer 17 thinner.

[0078] The protective layer 17 can be formed by a sputtering method using a target material containing carbon, a CVD (chemical vapor deposition) method using a hydrocarbon raw material such as ethylene or toluene, an IBD (ion beam deposition) method, or the like. When a carbon-based protective layer is formed as the protective layer 17, it can be deposited by, for example, a DC magnetron sputtering method. In particular, when a carbon-based protective layer is formed as the protective layer 17, it is preferable to deposit an amorphous carbon protective layer by a plasma CVD method. The amorphous carbon protective layer deposited by the plasma CVD method has a uniform surface with small roughness.

[0079] "Lubricating layer" The lubricating layer 18 prevents contamination of the magnetic recording medium 10. In addition, the lubricating layer 18 reduces the frictional force of the magnetic head of the magnetic recording and reproducing device that slides on the magnetic recording medium 10, thereby improving the durability of the magnetic recording medium 10. 1, the lubricating layer 18 is formed on and in contact with the protective layer 17. The lubricating layer 18 contains the above-mentioned fluorine-containing ether compound.

[0080] When the protective layer 17 disposed below the lubricating layer 18 is a carbon-based protective layer, the lubricating layer 18 is bonded with a high bonding strength to the protective layer 17. As a result, even if the thickness of the lubricating layer 18 is thin, it is easy to obtain a magnetic recording medium 10 in which the surface of the protective layer 17 is covered with a high coverage rate, and contamination of the surface of the magnetic recording medium 10 can be effectively prevented.

[0081] The average thickness of the lubricating layer 18 can be selected arbitrarily, but is preferably 0.5 nm (5 Å) to 3 nm (30 Å), and more preferably 0.5 nm (5 Å) to 1 nm (10 Å). When the average thickness of the lubricating layer 18 is 0.5 nm or more, the lubricating layer 18 is formed with a uniform thickness without being island-shaped or mesh-shaped. Therefore, the surface of the protective layer 17 can be covered with the lubricating layer 18 at a high coverage rate. In addition, by setting the average thickness of the lubricating layer 18 to 3 nm or less, the lubricating layer 18 can be made sufficiently thin, and the flying height of the magnetic head can be sufficiently reduced.

[0082] If the surface of the protective layer 17 is not covered with the lubricating layer 18 at a sufficiently high coverage rate, environmental substances adsorbed to the surface of the magnetic recording medium 10 will pass through the gaps in the lubricating layer 18 and penetrate underneath the lubricating layer 18. The environmental substances that penetrate underneath the lubricating layer 18 will be adsorbed and bonded to the protective layer 17 to generate contaminants. Then, during magnetic recording and reproduction, these contaminants (aggregated components) will adhere (transfer) to the magnetic head as smear, damaging the magnetic head or degrading the magnetic recording and reproduction characteristics of the magnetic recording and reproduction device.

[0083] Examples of environmental substances that generate pollutants include siloxane compounds (cyclic siloxanes, linear siloxanes), ionic impurities, hydrocarbons with relatively high molecular weights such as octacosane, and plasticizers such as dioctyl phthalate. Examples of metal ions contained in ionic impurities include sodium ions and potassium ions. Examples of inorganic ions contained in ionic impurities include chloride ions, bromide ions, nitrate ions, sulfate ions, and ammonium ions. Examples of organic ions contained in ionic impurities include oxalate ions and formate ions.

[0084] "Method of forming lubricating layer" The method for forming the lubricating layer 18 can be selected arbitrarily, but one example is a method in which a magnetic recording medium in the middle of manufacture is prepared in which each layer up to the protective layer 17 is formed on the substrate 11, and a solution for forming a lubricating layer is applied onto the protective layer 17 and dried.

[0085] The lubricant layer forming solution can be obtained, for example, by dispersing and dissolving the lubricant for magnetic recording media of the above-mentioned embodiment in a solvent as necessary, and adjusting the viscosity and concentration to be suitable for the coating method. Examples of the solvent used in the lubricant layer forming solution include fluorine-based solvents such as Vertrel (registered trademark) XF (product name, manufactured by Mitsui DuPont Fluorochemicals).

[0086] The method for applying the solution for forming the lubricating layer is not particularly limited, but examples thereof include spin coating, spraying, paper coating, and dipping. When using the dipping method, for example, the following method can be used. First, the substrate 11 on which each layer up to the protective layer 17 has been formed is immersed in the lubricant layer forming solution placed in the immersion tank of a dip coater. Next, the substrate 11 is lifted from the immersion tank at a predetermined speed. In this way, the lubricant layer forming solution is applied to the surface of the substrate 11 above the protective layer 17. By using the dipping method, the lubricant layer forming solution can be applied uniformly onto the surface of the protective layer 17, and the lubricant layer 18 can be formed on the protective layer 17 with a uniform thickness.

[0087] In this embodiment, it is preferable to perform a heat treatment on the substrate 11 on which the lubricating layer 18 is formed. By performing the heat treatment, the adhesion between the lubricating layer 18 and the protective layer 17 is improved, and the adhesive force between the lubricating layer 18 and the protective layer 17 is improved. The heat treatment temperature can be selected arbitrarily, but is preferably 100 to 180° C. If the heat treatment temperature is 100° C. or higher, the effect of improving the adhesion between the lubricating layer 18 and the protective layer 17 can be sufficiently obtained. Furthermore, by setting the heat treatment temperature to 180° C. or lower, thermal decomposition of the lubricating layer 18 can be prevented. The heat treatment time is preferably 10 to 120 minutes.

[0088] In this embodiment, in order to further improve the adhesion of the lubricating layer 18 to the protective layer 17, the lubricating layer 18 of the substrate 11 may be irradiated with ultraviolet (UV) rays before or after the heat treatment.

[0089] The magnetic recording medium 10 of this embodiment is a medium in which at least a magnetic layer 16, a protective layer 17, and a lubricating layer 18 are sequentially provided on a substrate 11. In the magnetic recording medium 10 of this embodiment, a lubricating layer 18 containing the above-mentioned fluorine-containing ether compound is formed on the protective layer 17. Even though the lubricating layer 18 is thin, it covers the surface of the protective layer 17 with a high coverage rate. Therefore, in the magnetic recording medium 10 of this embodiment, environmental substances that generate contaminants such as ionic impurities are prevented from penetrating through the gaps in the lubricating layer 18. Therefore, the magnetic recording medium 10 of this embodiment has a small amount of contaminants present on its surface. In addition, the lubricating layer 18 in the magnetic recording medium 10 of this embodiment is less likely to generate foreign matter (smear), and can suppress pickup. In addition, the lubricating layer 18 in the magnetic recording medium 10 of this embodiment has excellent wear resistance. Therefore, the magnetic recording medium 10 of this embodiment has excellent reliability and durability. EXAMPLES

[0090] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0091] Example 1 The compound represented by the following formula (5) was produced by the method shown below.

[0092] [ka] (In formula (5), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0093] The compound represented by the following formula (6) was synthesized by reacting 1,3-dihydroxybenzene with epichlorohydrin in an acetone solvent in the presence of potassium carbonate.

[0094] [ka]

[0095] Then, under a nitrogen gas atmosphere, HOCH2CF2O(CF2CF2O) was added to a 100 mL eggplant flask. p (CF2O) q 30.0 g of a compound (number average molecular weight 650, molecular weight distribution 1.1) represented by CF2CH2OH (q in the formula is 3.0, q is 3.0), 1.35 g of a compound represented by formula (6) (molecular weight 222, 6.1 mmol), and 20 mL of t-butanol (t-BuOH) were charged and stirred at room temperature until homogenous. 0.50 g of potassium tert-butoxide (t-BuOK) (molecular weight 112, 4.5 mmol) was further added to this homogenous liquid, and the mixture was reacted at 70°C for 16 hours with stirring.

[0096] The reaction product obtained was cooled to 25°C, transferred to a separatory funnel containing 40 mL of water, and extracted twice with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated with anhydrous sodium sulfate. After filtering off the drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 7.6 g (number average molecular weight 1669, 4.6 mmol) of the compound represented by the following formula (7).

[0097] [ka] (In formula (7), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0098] Next, 7.5 g of the compound represented by formula (7), 1.25 g of epibromohydrin (molecular weight 137, 9.1 mmol), and 25 mL of t-BuOH were added and stirred at room temperature until the mixture became homogeneous. 1.00 g of t-BuOK (molecular weight 112, 8.9 mmol) was added to the homogeneous solution and reacted at 70°C for 6 hours with stirring. The reaction product obtained was cooled to 25°C, transferred to a separatory funnel containing 30 mL of water, and extracted twice with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated with anhydrous sodium sulfate. After filtering off the drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 6.3 g (number average molecular weight 1781, 3.5 mmol) of the compound represented by the following formula (8).

[0099] [ka] (In formula (8), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0100] Next, 6.0 g of the compound represented by formula (8), 1.67 g of ethylene glycol (molecular weight 62, 26.9 mmol), and 30 mL of t-BuOH were added and stirred at room temperature until the mixture became homogeneous. 0.40 g of t-BuOK (molecular weight 112, 3.6 mmol) was added to the homogeneous solution and reacted at 70°C for 6 hours with stirring. The reaction product obtained was cooled to 25°C, transferred to a separatory funnel containing 30 mL of water, and extracted twice with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated with anhydrous sodium sulfate. After filtering off the drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 4.3 g of the compound represented by the above formula (5).

[0101] The obtained compound (5) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(36H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-55.5~-51.5(12F), -78.5(4F), -80.5(4F), -91.0~-88.5(24F)

[0102] Example 2 HOCH2CF2O(CF2CF2O) used in Example 1 p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2O(CF2CF2O) p (CF2O) q 4.4 g of a compound represented by the following formula (9) was obtained in the same manner as in Example 1, except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CH2OH (wherein p is 4.5 and q is 0) was used.

[0103] [ka] (In formula (9), R 2 is expressed by the following formula (2): (In formula (2), p is 4.5 and q is 0.)

[0104] The obtained compound (9) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(36H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-78.5(4F), -81.3(4F), -90.0~-88.5(36F)

[0105] Example 3 HOCH2CF2O(CF2CF2O) used in Example 1 p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2CF2O (CF2CF2CF2O) r 4.4 g of a compound represented by the following formula (10) was obtained in the same manner as in Example 1, except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CF2CH2OH (where r is 2.5) was used.

[0106] [ka] (In formula (10), R 2 is expressed by the following formula (3). (In formula (3), r is 2.5.)

[0107] The obtained compound (10) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(36H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-84.0~-83.0(20F), -86.4(8F), -124.3(8F), -130.0~-129.0(10F)

[0108] Example 4 HOCH2CF2O(CF2CF2O) used in Example 1 p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2CF2CF2O (CF2CF2CF2CF2O) s 3.9 g of a compound represented by the following formula (11) was obtained in the same manner as in Example 1, except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CF2CF2CH2OH (where s is 1.5) was used.

[0109] [ka] (In formula (11), R 2 is expressed by the following formula (4). (In formula (4), s is 1.5.)

[0110] The obtained compound (11) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(36H), 6.6~6.8(4H) 19F-NMR (acetone-D6): δ[ppm]=-84.0~-83.0(20F), -122.5(8F), -126.0(12F), -129.0~-128.0(8F)

[0111] Example 5 The procedure of Example 1 was repeated except that 1,3-propanediol was used instead of ethylene glycol, to obtain 4.5 g of a compound represented by the following formula (12).

[0112] [ka] (In formula (12), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0113] The obtained compound (12) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]1.00~1.40(4H), 3.3~4.2(36H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-55.5~-51.5(12F), -78.5(4F), -80.5(4F), -91.0~-88.5(24F)

[0114] Example 6 The procedure of Example 1 was repeated except that 1,4-butanediol was used instead of ethylene glycol, to obtain 4.2 g of a compound represented by the following formula (13).

[0115] [ka] (In formula (13), R 2is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0116] The obtained compound (13) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]1.00~1.40(8H), 3.3~4.2(36H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-55.5~-51.5(12F), -78.5(4F), -80.5(4F), -91.0~-88.5(24F)

[0117] Example 7 A compound represented by the following formula (14) was synthesized by a substitution reaction method using 1,3-dihydroxybenzene and 1,2-dibromoethane under basic conditions.

[0118] [ka]

[0119] Then, 3.8 g of a compound represented by the following formula (15) was obtained in the same manner as in Example 1, except that the compound represented by the above formula (14) was used instead of the compound represented by the above formula (6) used in Example 1.

[0120] [ka] (In formula (15), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0121] The obtained compound (15) 1 H-NMR and 19F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(34H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-55.5~-51.5(12F), -78.5(4F), -80.5(4F), -91.0~-88.5(24F)

[0122] Example 8 HOCH2CF2O(CF2CF2O) used in Example 1 p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2O(CF2CF2O) p (CF2O) q The same procedure as in Example 1 was repeated to obtain 3.9 g of the compound represented by the following formula (16), except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CH2OH (where p is 4.5 and q is 0) was used, and the compound represented by the above formula (14) was used instead of the compound represented by the above formula (6).

[0123] [ka] (In formula (16), R 2 is expressed by the following formula (2): (In formula (2), p is 4.5 and q is 0.)

[0124] The obtained compound (16) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(34H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-78.5(4F), -81.3(4F), -90.0~-88.5(36F)

[0125] Example 9 HOCH2CF2O(CF2CF2O) used in Example 1 p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2CF2O (CF2CF2CF2O) r 3.9 g of the compound represented by the following formula (17) was obtained in the same manner as in Example 1, except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CF2CH2OH (wherein r is 2.5) was used, and the compound represented by the above formula (14) was used instead of the compound represented by the above formula (6).

[0126] [ka] (In formula (17), R 2 is expressed by the following formula (3). (In formula (3), r is 2.5.)

[0127] The obtained compound (17) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(34H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-84.0~-83.0(20F), -86.4(8F), -124.3(8F), -130.0~-129.0(10F)

[0128] Example 10 HOCH2CF2O(CF2CF2O) used in Example 1p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2CF2CF2O (CF2CF2CF2CF2O) s The same procedure as in Example 1 was repeated, except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CF2CF2CH2OH (where s is 1.5) was used, and the compound represented by the above formula (14) was used instead of the compound represented by the above formula (6), to obtain 4.1 g of the compound represented by the following formula (18).

[0129] [ka] (In formula (18), R 2 is expressed by the following formula (4). (In formula (4), s is 1.5.)

[0130] The obtained compound (18) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(34H), 6.6~6.8(4H) 19 F-NMR (acetone-D6): δ[ppm]=-84.0~-83.0(20F), -122.5(8F), -126.0(12F), -129.0~-128.0(8F)

[0131] Example 11 A compound represented by the following formula (19) was synthesized in the same manner as for the compound represented by formula (6) in Example 1, except that 1,3,5-trihydroxybenzene and epichlorohydrin were used.

[0132] [ka]

[0133] Then, 3.4 g of a compound represented by the following formula (20) was obtained in the same manner as in Example 1, except that the compound represented by the above formula (19) was used instead of the compound represented by the above formula (6) used in Example 1.

[0134] [ka] (In formula (20), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0135] The obtained compound (20) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(54H), 6.6~6.8(3H) 19 F-NMR (acetone-D6): δ[ppm]=-55.5~-51.5(18F), -78.5(6F), -80.5(6F), -91.0~-88.5(36F)

[0136] Example 12 A compound represented by the following formula (21) was synthesized in the same manner as for the compound represented by formula (14) in Example 7, except that 1,3,5-trihydroxybenzene and 1,3-dibromopropane were used.

[0137] [ka]

[0138] Then, 4.7 g of a compound represented by the following formula (22) was obtained in the same manner as in Example 1, except that the compound represented by the above formula (21) was used instead of the compound represented by the above formula (6) used in Example 1.

[0139] [ka] (In formula (22), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0140] The obtained compound (22) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(57H), 6.6~6.8(3H) 19 F-NMR (acetone-D6): δ[ppm]=-55.5~-51.5(18F), -78.5(6F), -80.5(6F), -91.0~-88.5(36F)

[0141] Example 13 HOCH2CF2O(CF2CF2O) used in Example 1 p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2O(CF2CF2O) p (CF2O) q The same procedure as in Example 1 was repeated, except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CH2OH (wherein p is 4.5 and q is 0) was used, and the compound represented by the above formula (21) was used instead of the compound represented by the above formula (6), to obtain 4.8 g of the compound represented by the following formula (23).

[0142] [ka] (In formula (23), R 2is expressed by the following formula (2): (In formula (2), p is 4.5 and q is 0.)

[0143] The obtained compound (23) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(57H), 6.6~6.8(3H) 19 F-NMR (acetone-D6): δ[ppm]=-78.5(6F), -81.3(6F), -90.0~-88.5(54F)

[0144] Example 14 HOCH2CF2O(CF2CF2O) used in Example 1 p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2CF2O (CF2CF2CF2O) r The same procedure as in Example 1 was repeated, except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CF2CH2OH (wherein r is 2.5) was used, and the compound represented by the above formula (21) was used instead of the compound represented by the above formula (6), to obtain 4.7 g of the compound represented by the following formula (24).

[0145] [ka] (In formula (24), R 2 is expressed by the following formula (3). (In formula (3), r is 2.5.)

[0146] The obtained compound (24) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(57H), 6.6~6.8(3H) 19 F-NMR (acetone-D6): δ[ppm]=-84.0~-83.0(30F), -86.4(12F), -124.3(12F), -130.0~-129.0(15F)

[0147] Example 15 HOCH2CF2O(CF2CF2O) used in Example 1 p (CF2O) q Instead of the fluoropolyether represented by CF2CH2OH (where p is 3.0 and q is 3.0), HOCH2CF2CF2CF2O (CF2CF2CF2CF2O) s The same procedure as in Example 1 was repeated, except that a fluoropolyether (number average molecular weight 650, molecular weight distribution 1.2) represented by CF2CF2CF2CH2OH (where s is 1.5) was used, and the compound represented by the above formula (21) was used instead of the compound represented by the above formula (6), to obtain 4.2 g of the compound represented by the following formula (25).

[0148] [ka] (In formula (25), R 2 is expressed by the following formula (4). (In formula (4), s is 1.5.)

[0149] The obtained compound (25) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]3.3~4.2(57H), 6.6~6.8(3H) 19F-NMR (acetone-D6): δ[ppm]=-84.0~-83.0(30F), -122.5(12F), -126.0(18F), -129.0~-128.0(12F)

[0150] Example 16 The same procedure as in Example 1 was carried out except that the compound represented by the above formula (21) was used instead of the compound represented by the above formula (6) used in Example 1, and 1,3-propanediol was used instead of ethylene glycol, to obtain 4.6 g of the compound represented by the following formula (26).

[0151] [ka] (In formula (26), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0152] The obtained compound (26) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]1.00~1.40(6H), 3.3~4.2(57H), 6.6~6.8(3H) 19 F-NMR (acetone-D6): δ[ppm]=-55.5~-51.5(18F), -78.5(6F), -80.5(6F), -91.0~-88.5(36F)

[0153] (Example 17) The same procedure as in Example 1 was repeated except that the compound represented by the above formula (21) was used instead of the compound represented by the above formula (6) used in Example 1, and 1,4-butanediol was used instead of ethylene glycol, to obtain 4.6 g of a compound represented by the following formula (27).

[0154] [ka] (In formula (27), R 2 is expressed by the following formula (2): (In formula (2), p is 3.0 and q is 3.0.)

[0155] The obtained compound (27) 1 H-NMR and 19 F-NMR measurement was performed, and the structure was identified based on the following results. (Identification data) 1 H-NMR (acetone-D6): δ[ppm]1.00~1.40(12H), 3.3~4.2(57H), 6.6~6.8(3H) 19 F-NMR (acetone-D6): δ[ppm]=-55.5~-51.5(18F), -78.5(6F), -80.5(6F), -91.0~-88.5(36F)

[0156] Comparative Example 1 The compound represented by the following formula (28) was synthesized by the method described in Patent Document 1.

[0157] [ka] (In formula (28), R 2 is expressed by the following formula (4). (In formula (4), s is 1.5.)

[0158] Comparative Example 2 The compound represented by the following formula (29) was synthesized by the method described in Patent Document 1.

[0159] [ka] (In formula (29), R 2 is expressed by the following formula (4). (In formula (4), s is 1.5.)

[0160] Comparative Example 3 The compound represented by the following formula (30) was synthesized by the method described in Patent Document 2.

[0161] [ka] (In formula (30), R 2 is expressed by the following formula (4). (In formula (4), s is 1.5.)

[0162] Comparative Example 4 The compound represented by the following formula (31) was synthesized by the method described in Patent Document 3.

[0163] [ka] (In formula (31), p is 9.0 and q is 9.0.)

[0164] The number of n (the number of benzene substituents) in the formula (1) of the compounds of Examples 1 to 17 thus obtained, R 3 m number, R 1 ~R 2 The structure is shown in Table 1.

[0165] [Table 1]

[0166] The number average molecular weights of the compounds of Examples 1 to 17 and Comparative Examples 1 to 4 thus obtained were determined by the method described above. 1 H-NMR and 19 The results were obtained by F-NMR measurement, and are shown in Table 2.

[0167] [Table 2] In Table 2, ◎ means excellent results, ○ means good results, △ means fair results, and × means poor results.

[0168] Next, a solution for forming a lubricant layer was prepared by the method described below using the compounds obtained in Examples 1 to 17 and Comparative Examples 1 to 4. Then, the obtained solution for forming a lubricant layer was used to form a lubricant layer for a magnetic recording medium by the method described below, thereby obtaining the magnetic recording media of Examples 1 to 17 and Comparative Examples 1 to 4.

[0169] "Lubricant layer forming solution" The compounds obtained in Examples 1 to 17 and Comparative Examples 1 to 4 were each dissolved in a fluorine-based solvent, Vertrel (registered trademark) XF (product name, manufactured by Mitsui DuPont Fluorochemicals Co., Ltd.), and further diluted with Vertrel XF so that the film thickness when applied onto the protective layer would be 9 Å to 10 Å, to prepare a solution for forming a lubricating layer.

[0170] "Magnetic recording media" A magnetic recording medium was prepared by sequentially providing an adhesive layer, a soft magnetic layer, a first underlayer, a second underlayer, a magnetic layer, and a protective layer on a substrate having a diameter of 65 mm. The protective layer was made of carbon. On the protective layer of the magnetic recording medium on which each layer up to the protective layer had been formed, the lubricant layer forming solutions of Examples 1 to 17 and Comparative Examples 1 to 4 were applied by dipping under the conditions of an immersion speed of 10 mm / sec, an immersion time of 30 sec, and a pull-up speed of 1.2 mm / sec. The magnetic recording medium coated with the lubricant layer-forming solution was then placed in a thermostatic chamber at 120°C and heated for 10 minutes to remove the solvent in the lubricant layer-forming solution, thereby forming a lubricant layer on the protective layer and obtaining the magnetic recording medium.

[0171] The thickness of the lubricating layer of each of the magnetic recording media thus obtained in Examples 1 to 17 and Comparative Examples 1 to 4 was measured using an FT-IR (product name: Nicolet iS50, manufactured by Thermo Fisher Scientific Co., Ltd.) The results are shown in Table 2.

[0172] Furthermore, the magnetic recording media of Examples 1 to 17 and Comparative Examples 1 to 4 were subjected to the following measurement of adhesion (bond ratio) between the lubricating layer and the protective layer, pickup suppression test, and wear resistance test. The results are shown in Table 2.

[0173] (Measurement of adhesion (bond ratio) between lubricating layer and protective layer) The magnetic recording medium with the lubricating layer formed thereon was immersed in a solvent, Vertrel XF, for 10 minutes and then pulled up for cleaning. The magnetic recording medium was immersed in the solvent at a speed of 10 mm / sec and pulled up at a speed of 1.2 mm / sec. Thereafter, the thickness of the lubricating layer was measured in the same manner as in the measurement of the thickness of the lubricating layer before cleaning.

[0174] The thickness of the lubricant layer before cleaning was designated A, and the thickness of the lubricant layer after cleaning (immersion in the solvent) was designated B, and the bonding rate (bonding rate) of the lubricant was calculated from the ratio of A to B ((B / A) x 100(%)). Using the calculated bonding rate, the adhesion between the lubricant layer and the protective layer was evaluated according to the following criteria.

[0175] "Adhesion (bond rate) evaluation" ○(Good): Bond rate is 65% or more △(Acceptable): Bond ratio is 50% or more and less than 65% × (Not acceptable): Bond rate is less than 50%

[0176] (Pickup suppression test) The magnetic recording medium and the magnetic head were mounted on a spin stand, and the magnetic head was floated at a fixed point for 10 minutes while rotating the magnetic recording medium under reduced pressure (approximately 250 torr) at room temperature. After that, the surface of the magnetic head facing the magnetic recording medium (the surface of the lubricant layer) was analyzed using an ESCA (Electron Spectroscopy for Chemical Analysis) analyzer. Then, the amount of lubricant attached to the magnetic head was evaluated according to the criteria shown in Table 3 from the intensity (signal intensity (au)) of the peak derived from fluorine measured by ESCA.

[0177] [Table 3] In Table 3, ◎ means excellent results, ○ means good results, and × means poor results.

[0178] (Wear resistance test) Using a pin-on-disk type friction and wear tester, an alumina ball with a diameter of 2 mm was slid as a contact on the lubricating layer of the magnetic recording medium at a load of 40 gf and a sliding speed of 0.25 m / sec to measure the friction coefficient of the surface of the lubricating layer. The sliding time until the friction coefficient of the surface of the lubricating layer suddenly increased was then measured. The sliding time until the friction coefficient suddenly increased was measured four times for the lubricating layer of each magnetic recording medium, and the average value (time) was used as an index of the wear resistance of the lubricant coating.

[0179] In the magnetic recording media of Examples 1 to 17 and Comparative Examples 1 to 4, the wear resistance was evaluated based on the sliding time until the coefficient of friction increased sharply, as follows. "Wear resistance (sliding time) evaluation" ◎(Excellent): 650sec or more ○(Good): 550 sec or more, less than 650 sec △ (OK): 450 sec or more, less than 550 sec × (Not acceptable): Less than 450 seconds

[0180] The time until the friction coefficient increases sharply can be used as an index of the wear resistance of the lubricating layer for the following reason. The lubricating layer of the magnetic recording medium wears away as the magnetic recording medium is used, and when the lubricating layer is worn away, the contact and the protective layer come into direct contact, causing a sharp increase in the friction coefficient. The time until the friction coefficient increases sharply is thought to be correlated with the friction test.

[0181] As shown in Table 2, in Examples 1 to 17, the evaluation results of the adhesion (bond ratio) between the lubricating layer and the protective layer, the results of the pick-up suppression test and the wear resistance test were all good. mIn Comparative Examples 1 and 2, which used a compound that is -OCH2CH(OH)CH2OH instead of OH (where m is an integer of 2 to 4), the pick-up inhibition test was evaluated as × (fail). In Comparative Example 3, which used a compound having an -OH terminal group, the bond ratio and the pick-up suppression test were evaluated as × (fail). In addition, in Comparative Example 4, which used a compound in which a perfluoropolyether chain was located in the center of the molecule, the bond ratio and the pick-up suppression test were evaluated as × (unacceptable). Comparative Examples 1 to 4 were inferior to Examples 1 to 17 in the bond ratio, the pick-up suppression test, and the abrasion resistance test.

[0182] From the above results, it was found that by forming a lubricating layer containing the compounds of Examples 1 to 17 on the protective layer of a magnetic recording medium, even if the thickness is as thin as 9 Å to 10 Å, a lubricating layer that has excellent adhesion to the protective layer, is less likely to cause pick-up, and has excellent wear resistance can be obtained. [Industrial Applicability]

[0183] The present invention provides a fluorine-containing ether compound that can form a lubricating layer that has excellent wear resistance and suppresses pick-up even when the thickness is thin, and can be suitably used as a material for a lubricant for a magnetic recording medium. By using a lubricant for a magnetic recording medium containing the fluorine-containing ether compound of the present invention, a lubricating layer that has excellent wear resistance and suppresses pick-up even when the thickness is thin can be formed. [Explanation of symbols]

[0184] 10 magnetic recording medium, 11 substrate, 12 adhesion layer, 13 soft magnetic layer, 14 first underlayer, 15 second underlayer, 16 magnetic layer, 17 protective layer, and 18 lubricating layer.

Claims

1. A fluorine-containing ether compound represented by the following formula (1): C 6 H 6-n -[O-R 1 -O-CH 2 -R 2 -CH 2 -R 3 ] n (1) (In formula (1), n ​​is an integer of 2 or 3, and R 1 Ha-CH 2 CH 2 --, --CH 2 CH 2 CH 2 --, --CH 2 CH(OH)CH 2 -, and R 2 is a perfluoropolyether chain, R 3 Ha-OCH 2 CH(OH)CH 2 O (CH 2 ) m OH (wherein m is an integer from 2 to 4).

2. R in the formula (1) 2 is represented by any one of the following formulas (2) to (4): 【Chemistry 1】 (In formula (2), p represents 1 to 30, and q represents 0 to 30.) (In formula (3), r represents 1 to 30.) (In formula (4), s represents 1 to 20.)

3. 3. The fluorine-containing ether compound according to claim 2, which is any of compounds represented by the following formulas (A) to (N): 【Chemistry 2】 (In formula (A), R 2 is represented by the above formula (2). (In formula (B), R 2 is represented by the above formula (3). (In formula (C), R 2 is represented by the above formula (4). (In formula (D), R 2 is represented by the above formula (2). (In formula (E), R 2 is represented by the above formula (2). (In formula (F), R 2 is represented by the above formula (2). (In formula (G), R 2 is represented by the above formula (3). (In formula (H), R 2 is represented by the above formula (4). 【Chemistry 3】 (In formula (I), R 2 is represented by the above formula (2). (In formula (J), R 2 is represented by the above formula (2). (In formula (K), R 2 is represented by the above formula (3). (In formula (L), R 2 is represented by the above formula (4). (In formula (M), R 2 is represented by the above formula (2). (In formula (N), R 2 is represented by the above formula (2).

4. The fluorine-containing ether compound according to any one of claims 1 to 3, having a number average molecular weight in the range of 500 to 10,000.

5. A lubricant for magnetic recording media, comprising the fluorine-containing ether compound according to any one of claims 1 to 4.

6. A magnetic recording medium comprising at least a magnetic layer, a protective layer, and a lubricating layer provided in this order on a substrate, the lubricating layer comprising the fluorine-containing ether compound according to any one of claims 1 to 4.

7. 7. The magnetic recording medium according to claim 6, wherein the average thickness of the lubricating layer is from 0.5 nm to 3 nm.

Citation Information

Patent Citations

  • Automobile air conditioner

    JP1983016919A

  • Reinforcing bar

    JP1986098848A

  • Method for manufacturing magnetic disk

    JP2012009090A

  • Lubricant composition, fluorine compound, and use thereof

    JP2012184339A

  • Magnetic recording media

    JP4632144B2