Glycidyl group-containing compound, curable resin composition, cured product, and laminate
A glycidyl group-containing compound with reversible bonds through Diels-Alder reaction addresses the limitations of epoxy resin-based products by enabling repairability, remoldability, and easy disassembly, reducing waste and extending the lifespan of materials.
Patent Information
- Application Number
- JP2024524566
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-06
- Filing Date
- 2023-08-24
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2043-08-24
AI Technical Summary
Existing epoxy resin-based cured products face challenges in long-term reliability, recyclability, and waste management due to low molecular mobility, limited mechanical strength, and issues with self-healing and remoldability, leading to environmental burden and inefficiencies in reuse and repair.
A glycidyl group-containing compound with a specific structure, formed through a Diels-Alder reaction between a conjugated diene and a parent diene, is incorporated into a curable resin composition, enabling reversible bonds that allow for repairability, remoldability, and easy disassembly without mass loss or volatile compound generation.
The solution provides cured products with enhanced repairability, remoldability, and ease of disassembly, reducing waste and extending the lifespan of materials by allowing for reshaping and recycling without mass loss or contamination during remolding.
Smart Images

Figure 0007568172000001 
Figure 0007568172000002 
Figure 0007568172000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a glycidyl group-containing compound having a specific structure, a curable resin composition containing the compound, a cured product, and a laminate containing a layer made of the cured product. [Background technology]
[0002] Cured products obtained from epoxy resins have excellent heat resistance, mechanical strength, electrical properties, adhesive properties, etc., and are essential materials in various fields such as electrical and electronics, paints, and adhesives.
[0003] On the other hand, cured products using thermosetting resins such as epoxy resins have low long-term reliability. For example, when a cured product of an epoxy resin deteriorates due to oxidation, cracks may occur.
[0004] In addition, the cured product obtained by curing thermosetting resins such as epoxy resins cannot be dissolved in solvents (is insoluble) and does not dissolve even at high temperatures (is infusible), making it difficult to recycle or reuse. In addition, the cured product becomes waste after use, so there is a need to reduce waste and alleviate the burden on the environment.
[0005] Therefore, there is a demand for solutions to issues such as extending the lifespan and reducing waste for cured products made from epoxy resins, etc., and it is believed that an effective solution to these issues would be to give the cured products easy dismantling, repairability, and remoldability.
[0006] Against this background, a method has been disclosed in which a thermally decomposable compound is incorporated into a reactive adhesive component in advance, and then, after use, a certain amount of heat is applied to reduce the adhesive strength, making the product dismantlable (see, for example, Patent Document 1).
[0007] In addition, a method has been disclosed in which, even if cracks or peeling occur in a sealing material using an epoxy resin or the like, the sealing material can be made self-repairable by using microcapsule particles containing a first thermosetting resin and a precursor of a second thermosetting resin (see, for example, Patent Document 2).
[0008] Furthermore, as a method for imparting self-repairing properties to a cured epoxy resin, the incorporation of a bonding site by a Diels-Alder reaction has also been proposed (see, for example, Non-Patent Document 1).
[0009] In addition to the above, active research is being conducted on the use of reversible bonds such as dynamic covalent bonds and supramolecular bonds in hardened materials in order to impart repairability and reshapeability. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2013-256557 A [Patent Document 2] JP 2017-041496 A [Non-patent literature]
[0011] [Non-Patent Document 1] Amendola, E., Iacono, SD, Pastore, A., Curcio, M., Giordano, M. and Iadonisi, A. "Epoxy Thermosets with Self-Healing Ability", Journal of Materials Science and Chemical Engineering,2015,3,p162-167 Summary of the Invention [Problem to be solved by the invention]
[0012] In the technology provided in Patent Document 1, the adhesive is discarded after dismantling, and although the substrate to which the adhesive is applied can be recycled, there is a problem that the overall recyclability is insufficient. In addition, the technology in Patent Document 2 has a certain degree of self-repairing ability, but it is not a solution from the viewpoint of reuse, and the problem of waste when it becomes unnecessary remains. In the technology provided in Non-Patent Document 1, the low molecular weight compound generated by the Retro-Diels-Alder reaction may volatilize from the cured product, causing a mass reduction, or may contaminate the mold during remolding.
[0013] In addition, the raw materials involved in the reversible bond need to have their molecular mobility guaranteed, so there is a problem that the raw materials used are limited to gel-like substances with poor mechanical strength, and both of these are currently in need of improvement. Therefore, the object of the present invention is to provide a compound that is a curable resin but can easily achieve repairability, remoldability, and easy dismantling in the cured product, and a curable resin composition and its cured product made using the compound. [Means for solving the problem]
[0014] Means for Solving the Problems The present inventors have conducted extensive research and found that the above-mentioned problems can be solved by using a glycidyl group-containing compound having a specific structure as a curable resin composition, thereby completing the invention.
[0015] That is, the present invention includes the following aspects. [1] A glycidyl group-containing compound, characterized in that a conjugated diene structure (A) having one or more glycidyl groups and a parent diene structure (B) having one or more glycidyl groups are linked by a Diels-Alder reaction. [2] The glycidyl group-containing compound according to [1], wherein the dissociation temperature of the linking moiety by the Diels-Alder reaction is 100°C or higher. [3] The glycidyl group-containing compound according to [1] or [2], wherein the conjugated diene structure (A) is a furan-derived structure or an anthracene-derived structure. [4] The glycidyl group-containing compound according to any one of [1] to [3], wherein the parent diene structure (B) is a structure derived from maleimide. [5] A glycidyl group-containing compound represented by the following general formula:
[0016] [ka] [In the formula, R 1 is a glycidyl group or a substituent having one or more glycidyl groups, and R 2 ~R 11 each independently represents a hydrogen atom, a halogen atom, a hydroxy group, a nitro group, a carboxy group, a cyano group, an alkoxy group, an aralkyloxy group, an aryloxy group, an amino group, an amido group, an alkyloxycarbonyl group, an aryloxycarbonyl group, an alkyl group, a cycloalkyl group, an aralkyl group, an aryl group, or a glycidyl group; The alkoxy group, aralkyloxy group, aryloxy group, amino group, amido group, alkyloxycarbonyl group, aryloxycarbonyl group, alkyl group, cycloalkyl group, aralkyl group, aryl group and glycidyl group may have a substituent on a carbon atom or a nitrogen atom. In the formulas (1) and (1'), R 2 ~R 5 At least one of R in formula (2) and (2') 2 ~R 11 At least one of the groups is a glycidyl group or a group having one or more glycidyl groups. [6] The glycidyl group-containing compound according to any one of [1] to [5], having an epoxy equivalent in the range of 100 to 500 g / eq. [7] A curable resin composition comprising, as essential components, the glycidyl group-containing compound according to any one of [1] to [6] above and a compound (I) reactive with the glycidyl group-containing compound. [8] The curable resin composition according to [7], wherein the compound (I) reactive with the glycidyl group-containing compound is a hydroxyl group-containing compound. [9] The curable resin composition according to [7] or [8], further comprising an epoxy resin having an epoxy equivalent of 100 to 10,000 g / eq other than the glycidyl group-containing compound according to any one of [1] to [5].
[10] The curable resin composition according to [9], wherein the epoxy resin is represented by the following formula (3) and has an epoxy equivalent of 500 to 10,0000 g / eq.
[0017] [ka] [In formula (3), each Ar independently represents a structure having an unsubstituted or substituted aromatic ring, X is a structural unit represented by the following formula (3-1), and Y is a structural unit represented by the following formula (3-2),
[0018] [ka] [In the formulas (3-1) and (3-2), Ar is the same as defined above, R 21 , R 22 each independently represents a hydrogen atom, a methyl group, or an ethyl group, R' is a divalent hydrocarbon group having 2 to 12 carbon atoms; R 23 , R 24 , R 27 , R 28 each independently represents a hydroxyl group, a glycidyl ether group, or a 2-methylglycidyl ether group, R 25 , R 26 , R 29 , R 30 each independently represents a hydrogen atom or a methyl group, n1 is an integer from 4 to 16, n2 is the average number of repeating units and is between 2 and 30. R 31 , R 32 each independently represents a glycidyl ether group or a 2-methylglycidyl ether group; R 33 , R 34each independently represents a hydroxyl group, a glycidyl ether group, or a 2-methylglycidyl ether group, R 35 , R 36 is a hydrogen atom or a methyl group, m1, m2, p1, p2, and q are the average values of the repetitions, m1 and m2 each independently represent 0 to 25, and m1+m2≧1; p1 and p2 each independently represent 0 to 5; q is 0.5 to 5. However, the bond between the structural unit X represented by the formula (3-1) and the structural unit Y represented by the formula (3-2) may be random or block, and the total numbers of the structural units X and Y present in one molecule are m1 and m2, respectively.
[11] The curable resin composition according to any one of [7] to
[10] , wherein a concentration of Diels-Alder reaction units relative to the total mass of the curable components in the curable resin composition is 0.10 mmol / g or more.
[12] The curable resin composition according to any one of [7] to
[11] , which is a self-repairing composition, a remolding material composition, or an easily dismantlable composition.
[13] A cured product obtained by curing the curable resin composition according to any one of [7] to
[12] .
[14] A laminate having a substrate and a layer containing the cured product according to
[13] .
[15] A heat-resistant member containing the cured product according to
[13] . Effect of the Invention
[0019] According to the present invention, it is possible to impart repairability, remoldability, and easy dismantling properties to a cured product made of a curable resin composition, and there is no mass loss during remolding, which can contribute to extending the life of the cured product itself and reducing waste. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Next, the embodiments for carrying out the present invention will be described in detail. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.
[0021] The glycidyl group-containing compound according to one embodiment of the present invention is characterized in that a conjugated diene structure (A) having one or more glycidyl groups and a parent diene structure (B) having one or more glycidyl groups are linked by a Diels-Alder reaction. The glycidyl group in the present invention does not only refer to a glycidyl group having no substituent, but also includes a glycidyl group having a substituent on a carbon atom. The Diels-Alder reaction includes not only the narrowly defined Diels-Alder reaction, which is a reaction of a conjugated diene structure or parent diene structure that does not contain a heteroatom such as an oxygen atom, a nitrogen atom, or a sulfur atom, but also a Hetero-Diels-Alder reaction, which is a reaction of a conjugated diene structure or parent diene structure that contains a heteroatom such as an oxygen atom, a nitrogen atom, or a sulfur atom.
[0022] The reversible bond by the Diels-Alder reaction is a reaction in which a conjugated diene and a parent diene undergo an addition reaction to form a six-membered ring. Since the Diels-Alder reaction is an equilibrium reaction, a Retro-Diels-Alder reaction occurs at a certain temperature, resulting in dissociation (decrosslinking). This reversibility is maintained even after the cured product (three-dimensional crosslinked product) is formed, so that when mechanical energy such as scratches or external force is applied to the cured product, the CC bond of the Diels-Alder reaction unit is preferentially broken because the CC bond of the Diels-Alder reaction unit has a lower bond energy than a normal covalent bond. However, in a temperature range lower than the dissociation temperature, the equilibrium of the CC bond of the Diels-Alder reaction unit shifts in the bond direction, so that an adduct (Diels-Alder reaction unit) is formed again, which is considered to enable repair of scratches and remolding.
[0023] Therefore, the glycidyl group-containing compound as one embodiment of the present invention is incorporated into a crosslinked structure by a curing reaction based on the glycidyl group, but when the cured product is subjected to an impact, cracks are generated, or the product is crushed, the reversible bond is cut, thereby exhibiting easy dismantling properties. However, as described above, the reversible bond can be reversibly reformed even at low temperatures including room temperature, and can exhibit functions such as repairability and remolding. For example, even if a cured product made using the glycidyl group-containing compound of the present invention is crushed, the cured product can be easily repaired based on the reversible bond by placing it at a low temperature including room temperature or in a heated or heated state, and it is also possible to remold the cured product after crushing it. At this time, the opposite end of the cut part is connected to the crosslinked structure of the cured product by a chemical bond, so that low molecular weight compounds are not generated. For this reason, the generation of volatile components is suppressed even when the product is heated or heated during remolding, there is no mass loss, and contamination of the mold used for remolding can be effectively prevented.
[0024] The glycidyl group-containing compound according to one embodiment of the present invention is formed by linking a conjugated diene structure (A) having one or more glycidyl groups to a parent diene structure (B) having one or more glycidyl groups. From the viewpoint of availability of raw materials, the glycidyl group is preferably linked to a compound having a conjugated diene structure or parent diene structure described below as a glycidyl ether group or a diglycidyl amino group directly or via another group such as an aromatic ring. In addition, the compound may have a plurality of glycidyl groups of different forms, such as a glycidyl ether group and a diglycidyl amino group, in one molecule.
[0025] The conjugated diene structure (A) is not particularly limited, and examples thereof include aliphatic hydrocarbon skeletons such as 1,3-butadiene skeleton; aromatic hydrocarbon skeletons such as anthracene; cyclic dienes such as cyclopentadiene and dicyclopentadiene; and heterocyclic skeletons such as imidazole ring, furan ring, triazine ring, thiophene ring, and pyrrole ring. In the present invention, it is essential that the compound having these skeletons or rings has a glycidyl group, but other various substituents may be present within a range that does not inhibit the Diels-Alder reaction. The number of glycidyl groups in one molecule is not limited to one, and may be multiple. However, from the viewpoints of easy availability and synthesis of the compound, and balance between reactivity when used as a curable resin composition and easy dismantling and remolding of the cured product, it is preferable that the number is 1 to 3, and more preferably 1 to 2.
[0026] The diene parent structure (B) is not particularly limited, and examples thereof include compounds having a maleimide group, an acryloyl group, a vinyl ketone group, an acetylene group, an allyl group, a diazo group, a nitro group, a benzoquinone skeleton, and the like. In the present invention, it is essential that the compound having these functional groups has a glycidyl group, but other various substituents may be present within a range that does not inhibit the Diels-Alder reaction. The number of glycidyl groups in one molecule is not limited to one, and may be multiple, but from the viewpoints of the ease of obtaining and synthesizing the compound, and the balance between the reactivity when used as a curable resin composition and the ease of dismantling and remolding of the cured product, it is preferable that the number is 1 to 3, and more preferably 1 to 2. Compounds containing these functional groups may also contain various substituents or structures within a range that does not inhibit the Diels-Alder reaction.
[0027] The glycidyl group-containing compound as one embodiment of the present invention is not particularly limited as long as it is a combination of the above-mentioned conjugated diene structure (A) and dienophilic structure (B). From the viewpoints of reactivity when made into a curable resin composition and mechanical strength when made into a cured product, it is preferable that the epoxy equivalent of the compound is in the range of 100 to 500 g / eq.
[0028] From the viewpoints of availability of raw materials and ease of compound synthesis, and mechanical strength of the cured product, the conjugated diene structure (A) is preferably a furan-derived structure or an anthracene-derived structure, and the parent diene structure (B) is preferably a maleimide-derived structure.
[0029] In particular, when the cured product is used for heat-resistant applications, a combination that results in a dissociation temperature of 100° C. or higher is preferable, and a combination that results in a dissociation temperature of 120° C. or higher is particularly preferable. When used at higher temperatures, it is preferable that the conjugated diene structure (A) is an anthracene-derived structure and the parent diene structure (B) is a maleimide-derived structure, which can provide a dissociation temperature of 130° C. or higher.
[0030] In order to obtain a compound in which the conjugated diene structure (A) is a furan-derived structure or an anthracene-derived structure and the parent diene structure (B) is a maleimide-derived structure, a method using a furan compound or an anthracene compound having a substituent with a glycidyl group on the ring and a maleimide compound having a substituent with a glycidyl group is preferred in terms of ease of production.
[0031] The glycidyl group-containing compound according to one embodiment of the present invention can be represented by the following structural formula.
[0032] [ka]
[0033] In the formula, R 1 is a glycidyl group or a substituent having one or more glycidyl groups, and R 2 ~R 11 each independently represents a hydrogen atom, a halogen atom, a hydroxy group, a nitro group, a carboxy group, a cyano group, an alkoxy group, an aralkyloxy group, an aryloxy group, an amino group, an amido group, an alkyloxycarbonyl group, an aryloxycarbonyl group, an alkyl group, a cycloalkyl group, an aralkyl group, an aryl group, or a glycidyl group; The alkoxy group, aralkyloxy group, aryloxy group, amino group, amido group, alkyloxycarbonyl group, aryloxycarbonyl group, alkyl group, cycloalkyl group, aralkyl group, aryl group and glycidyl group may have a substituent on a carbon atom or a nitrogen atom. In the formulas (1) and (1'), R 2 ~R 5 At least one of R in formula (2) and (2') 2 ~R 11 At least one of the groups is a glycidyl group or a group having one or more glycidyl groups.
[0034] The method for producing the glycidyl group-containing compound, which is one embodiment of the present invention, is not particularly limited. It may be produced stepwise using known reactions depending on the target structure, and it may be obtained by appropriately combining commercially available raw materials. Representative synthesis methods are described below.
[0035] It is widely known that the Diels-Alder reaction, in which a conjugated diene and a parent diene undergo an addition reaction to form a six-membered ring, is an equilibrium reaction, and that at a temperature higher than the temperature at which the addition reaction proceeds, the addition reaction portion dissociates and the original conjugated diene and parent diene are returned to each other, i.e., a retro-Diels-Alder reaction, proceeds. The Diels-Alder reaction may be carried out by a known method. For example, a conjugated diene compound and a parent diene compound are mixed in equimolar amounts, or in some cases, one of the components is mixed in excess, and the mixture is melted by heating or dissolved in a solvent, and stirred at room temperature to 110°C for 1 to 24 hours. The product can be obtained by filtration or solvent distillation without purification, or by a commonly used isolation and purification method such as recrystallization, reprecipitation, and chromatography.
[0036] In order to obtain a compound in which the conjugated diene structure (A) is a furan-derived structure, it is preferable to use a furan compound having a hydroxyl group or an amino group, which is a precursor of a glycidyl group, and specifically, any of the compounds listed in the following formulas can be used. The hydroxyl group in the compound can be converted into a glycidyl ether group by a known method, for example, as described in the examples, and the amino group can be converted into a diglycidylamino group in the same manner. In the compound having a benzene ring or a naphthalene ring, the hydroxyl group or the amino group may be bonded to any position on the ring.
[0037] [ka]
[0038] Among the above formulas, the compounds shown below are particularly preferred from the viewpoint of the balance between reactivity, physical properties of the cured product, and ease of dismantling, repairability, and remoldability.
[0039] [ka]
[0040] In order to obtain a compound in which the conjugated diene structure (A) is an anthracene-derived structure, it is preferable to use an anthracene compound having a hydroxyl group or an amino group, which is a precursor of a glycidyl group, and specifically, any of the compounds listed in the following formulas can be used. Among these, 9-(4-hydroxybenzyl)-10-(4-hydroxyphenyl)anthracene and hydroxyanthracene are preferred because of their good curability, and 9-(4-hydroxybenzyl)-10-(4-hydroxyphenyl)anthracene and monohydroxyanthracene are particularly preferred in terms of the balance between reactivity and cured product properties, as well as repairability and remolding ability. The hydroxyl group in the compound can be converted into a glycidyl ether group by a known method, for example, as described in the examples, and the amino group can be converted into a diglycidylamino group.
[0041] [ka]
[0042] In order to obtain a compound in which the parent diene structure (B) is a maleimide-derived structure, it is preferable to use a maleimide compound having a hydroxyl group or an amino group, which is a precursor of a glycidyl group, as a raw material. The maleimide compound having a hydroxyl group or an amino group can be any of the compounds listed in the following formulas. Among these, when hydroxyphenylmaleimide is glycidyl etherified, it is preferable in terms of curability, and monohydroxyphenylmaleimide is a particularly preferable raw material in terms of the balance between reactivity, cured product properties, and repairability and remolding properties. Among monohydroxyphenylmaleimides, parahydroxyphenylmaleimide is particularly preferable from the viewpoint of the heat resistance of the cured product. The hydroxyl group in the compound can be converted into a glycidyl ether group by a known method such as that described in the examples, and the amino group can be converted into a diglycidylamino group.
[0043] [ka]
[0044] The structures of the furan compound, anthracene compound, and maleimide compound each include those having, independently of one another, a hydrogen atom, a halogen atom, an alkoxy group, an aralkyloxy group, an aryloxy group, a nitro group, an amide group, an alkyloxycarbonyl group, an aryloxycarbonyl group, a cyano group, an alkyl group, a cycloalkyl group, an aralkyl group, or an aryl group as a substituent. In the structures of the compounds listed in the above formulas, the alkoxy group, the aralkyloxy group, the aryloxy group, the carboxy group, the alkyloxycarbonyl group, the aryloxycarbonyl group, the alkyl group, the cycloalkyl group, the aralkyl group, and the aryl group also include those having various substituents bonded to the carbon atom or nitrogen atom thereof.
[0045] The glycidyl group-containing compound of the present invention can be used in combination with a compound (I) reactive with the glycidyl group-containing compound to form a curable resin composition. The curable resin composition can be suitably used for various electric and electronic material applications such as adhesives, paints, photoresists, printed wiring boards, and semiconductor encapsulation materials.
[0046] Examples of the compound (I) reactive with the glycidyl group-containing compound include various known curing agents for epoxy resins, such as amine compounds, acid anhydrides, amide compounds, phenolic hydroxyl group-containing compounds, carboxylic acid compounds, thiol compounds, etc. The curing agent can be appropriately selected depending on the physical properties of the desired cured product, but it is preferable to use a hydroxyl group-containing compound, particularly from the viewpoint of mechanical strength and adhesion to the substrate.
[0047] Examples of the amine compound include trimethylenediamine, ethylenediamine, N,N,N',N'-tetramethylethylenediamine, pentamethyldiethylenetriamine, triethylenediamine, dipropylenediamine, N,N,N',N'-tetramethylpropylenediamine, tetramethylenediamine, pentanediamine, hexamethylenediamine, trimethylhexamethylenediamine, N,N,N',N'-tetramethylhexamethylenediamine, N,N-dimethylcyclohexylamine, diethylenetriamine, triethylenetetramine, tetramethylhexamethylenediamine ... aliphatic amine compounds such as triethylenepentamine, dimethylaminopropylamine, diethylaminopropylamine, dibutylaminopropylamine, 1,4-diazabicyclo(2,2,2)octane (triethylenediamine), polyoxyethylenediamine, polyoxypropylenediamine, bis(2-dimethylaminoethyl)ether, dimethylaminoethoxyethoxyethanol, triethanolamine, dimethylaminohexanol, benzylmethylamine, dimethylbenzylamine, m-xylenediamine, and α-methylbenzylmethylamine;
[0048] Alicyclic and heterocyclic amine compounds such as piperidine, piperazine, menthanediamine, isophoronediamine, methylmorpholine, ethylmorpholine, N,N',N"-tris(dimethylaminopropyl)hexahydro-s-triazine, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxyspiro(5,5)undecane adduct, N-aminoethylpiperazine, trimethylaminoethylpiperazine, bis(4-aminocyclohexyl)methane, N,N'-dimethylpiperazine, 1,8-diazabicyclo-[5.4.0]-undecene (DBU);
[0049] Aromatic amine compounds such as o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, pyridine, and picoline;
[0050] Examples of modified amine compounds include epoxy compound-added polyamines, Michael addition polyamines, Mannich addition polyamines, thiourea addition polyamines, ketone-blocked polyamines, dicyandiamide, guanidine, organic acid hydrazides, diaminomaleonitrile, aminimide, boron trifluoride-piperidine complex, and boron trifluoride-monoethylamine complex.
[0051] Examples of the acid anhydride include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, maleic polypropylene glycol anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride.
[0052] Examples of the phenolic hydroxyl group-containing compound include bisphenols such as bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, and 1,1-bis(4-hydroxyphenyl)-1-phenylethane, and bis(4-hydroxyphenyl)sulfone, phenol novolac resins, cresol novolac resins, aromatic hydrocarbon formaldehyde resin-modified phenolic resins, dicyclopentadiene phenol addition type resins, phenol aralkyl resins (Zylok resins), naphthol aralkyl resins, trimethylolmethane resins, Examples of polyhydric phenol compounds include tetraphenylolethane resin, naphthol novolak resin, naphthol-phenol co-condensed novolak resin, naphthol-cresol co-condensed novolak resin, biphenyl-modified phenol resin (a polyhydric phenol compound in which a phenol nucleus is linked via a bismethylene group), biphenyl-modified naphthol resin (a polyhydric naphthol compound in which a phenol nucleus is linked via a bismethylene group), aminotriazine-modified phenol resin (a polyhydric phenol compound in which a phenol nucleus is linked via melamine, benzoguanamine, or the like), and alkoxy group-containing aromatic ring-modified novolak resin (a polyhydric phenol compound in which a phenol nucleus and an alkoxy group-containing aromatic ring are linked via formaldehyde).
[0053] Examples of the amide-based compound include dicyandiamide and polyamidoamine, etc. Examples of the polyamidoamine include those obtained by reacting an aliphatic dicarboxylic acid such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, etc., or a carboxylic acid compound such as a fatty acid or a dimer acid, with an aliphatic polyamine or a polyamine having a polyoxyalkylene chain, etc.
[0054] Examples of the carboxylic acid compound include carboxylic acid polymers such as carboxylic acid-terminated polyesters, polyacrylic acid, and maleic acid-modified polypropylene glycol.
[0055] The thiol compound preferably contains two or more thiol groups in two molecules. For example, 3,3'-dithiodipropionic acid, trimethylolpropane tris(thioglycolate), pentaerythritol tetrakis(thioglycolate), ethylene glycol dithioglycolate, 1,4-bis(3-mercaptobutyryloxy)butane, tris[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), dipentaerythritol hexakis(3-mercaptopropionate), 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril, 4-butanedithiol, 1,6-hexaneedithiol, 1,10-decanedithiol, and the like.
[0056] When using these curing agents, only one type of curing agent may be used, or two or more types may be mixed. In applications such as underfill materials and general coating applications, it is preferable to use the amine compounds, carboxylic acid compounds, and / or acid anhydride compounds. In applications such as adhesives and flexible wiring boards, amine compounds, particularly dicyandiamide, are preferred from the viewpoints of workability, curability, and long-term stability. In applications such as semiconductor encapsulation materials, solid-type phenol compounds are preferred from the viewpoint of heat resistance of the cured product. In applications such as batteries, aliphatic amines and thiol compounds are preferred from the viewpoint of low-temperature curing.
[0057] Furthermore, in the curable resin composition of the present invention, epoxy resins other than the glycidyl group-containing compound of the present invention can be used in combination within the range that does not impair the effects of the present invention.
[0058] Examples of the other epoxy resins include liquid epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AD type epoxy resins, polyhydroxybenzene type epoxy resins, polyhydroxynaphthalene type epoxy resins, biphenyl type epoxy resins, and tetramethylbiphenyl type epoxy resins; brominated epoxy resins such as brominated phenol novolac type epoxy resins; solid bisphenol A type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, triphenylmethane type epoxy resins, and tetraphenylethane type epoxy resins. Examples of such epoxy resins include dicyclopentadiene-phenol addition reaction type epoxy resins, phenol aralkyl type epoxy resins, phenylene ether type epoxy resins, naphthylene ether type epoxy resins, naphthol novolac type epoxy resins, naphthol aralkyl type epoxy resins, naphthol-phenol co-condensed novolac type epoxy resins, naphthol-cresol co-condensed novolac type epoxy resins, aromatic hydrocarbon formaldehyde resin modified phenol resin type epoxy resins, biphenyl modified novolac type epoxy resins, and the like. These may be used alone or in combination of two or more kinds, and it is preferable to select and use various types depending on the intended use, the physical properties of the cured product, and the like.
[0059] Among these, it is preferable to use an epoxy resin having an epoxy equivalent of 100 to 10,000 g / eq in combination from the viewpoint of achieving an excellent balance between the curability and the crosslink density of the resulting cured product, and it is particularly preferable to use an epoxy resin represented by the following formula (3) and having an epoxy equivalent of 500 to 10,000 g / eq.
[0060] [ka] [In formula (3), each Ar independently represents a structure having an unsubstituted or substituted aromatic ring, X is a structural unit represented by the following formula (3-1), and Y is a structural unit represented by the following formula (3-2),
[0061] [ka]
[0062] In the formulas (3-1) and (3-2), Ar is the same as defined above. R 21 , R 22 each independently represents a hydrogen atom, a methyl group, or an ethyl group, R' is a divalent hydrocarbon group having 2 to 12 carbon atoms; R 23 , R 24 , R 27 , R 28 each independently represents a hydroxyl group, a glycidyl ether group, or a 2-methylglycidyl ether group, R 25 , R 26 , R 29 , R 30 each independently represents a hydrogen atom or a methyl group, n1 is an integer from 4 to 16, n2 is the average number of repeating units and is between 2 and 30. R 31 , R 32 each independently represents a glycidyl ether group or a 2-methylglycidyl ether group; R 33 , R 34 each independently represents a hydroxyl group, a glycidyl ether group, or a 2-methylglycidyl ether group, R 35 , R 36 is a hydrogen atom or a methyl group, m1, m2, p1, p2, and q are the average values of the repetitions, m1 and m2 each independently represent 0 to 25, and m1+m2≧1; p1 and p2 each independently represent 0 to 5; q is 0.5 to 5. However, the bond between the structural unit X represented by the formula (3-1) and the structural unit Y represented by the formula (3-2) may be random or block, and the total numbers of the structural units X and Y present in one molecule are m1 and m2, respectively.
[0063] As the epoxy resin, for example, an epoxy resin represented by the following formula may be used: By using such an epoxy resin, the effects of repairability and remoldability of the epoxy resin cured product are improved, and a good balance between flexibility and toughness is achieved.
[0064] [ka] (In formula (5), p1, p2, q, m1, and n1 are average values of repetitions, and each independently, p1 is 0 to 5, p2 is 0 to 5, q is 0.5 to 5, m1 is 0 to 25, and n1 is 2 to 30.)
[0065] The epoxy resin represented by the general formula (3) may be used alone in combination to form a curable resin composition. However, from the viewpoint of imparting further flexibility to the cured product and making it easier to dismantle, it is also preferable to use an epoxy resin having an epoxy equivalent of 100 to 300 g / eq in combination.
[0066] The epoxy resin that can be used in combination is not limited in structure as long as its epoxy equivalent is in the range of 100 to 300 g / eq. Examples of the epoxy resin include liquid epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AD type epoxy resin, polyhydroxybenzene type epoxy resin, polyhydroxynaphthalene type epoxy resin, biphenyl type epoxy resin, and tetramethylbiphenyl type epoxy resin; brominated epoxy resins such as brominated phenol novolac type epoxy resin; solid bisphenol A type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, triphenylmethane type epoxy resin, tetraphenylethane type epoxy resin, dicyclohexyl ether type epoxy resin, and the like. Examples of such epoxy resins include isopropyl alcohol-based epoxy resins, isopropyl alcohol-based epoxy resins, and the like. Examples of such epoxy resins include isopropyl alcohol-based epoxy resins, isopropyl alcohol-based epoxy resins, and the like. Examples of such epoxy resins include isopropyl alcohol-based epoxy resins, isopropyl alcohol-based epoxy resins, and the like. Examples of such epoxy resins include isopropyl alcohol-based epoxy resins, isopropyl alcohol-based epoxy resins, and the like.
[0067] Among these, it is preferable to use liquid epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AD type epoxy resins, polyhydroxybenzene type epoxy resins, polyhydroxynaphthalene type epoxy resins, biphenyl type epoxy resins, and tetramethylbiphenyl type epoxy resins, and it is particularly preferable to use epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, and bisphenol AD ... the like, each having an epoxy equivalent of 100 to 300 g / eq.
[0068] The ratio of the epoxy resin represented by the general formula (3) to the epoxy resin having an epoxy equivalent of 100 to 300 g / eq is not particularly limited, but from the viewpoint of facilitating phase separation in the cured product, the mass ratio of the former to the latter is 97:3 to 3:97, preferably 10:90 to 90:10, and particularly preferably 80:20 to 20:80. Phase separation in the cured product results in a sea-island structure, which achieves both adhesiveness and stress relaxation ability of the cured product, exhibits high adhesive strength in a particularly wide temperature range, and has the effect of reducing the molding shrinkage rate before and after heat curing of the resin composition.
[0069] The concentration of the reversible bond in the curable resin composition of the present invention is preferably 0.10 mmol / g or more relative to the total mass of the curable components in the curable resin composition. According to such a configuration, both the repairability and remoldability of the cured product obtained from the curable resin composition are further improved. The concentration of the reversible bond is more preferably 0.10 to 3.00 mmol / g, and even more preferably 0.15 to 2.00 mmol / g. The concentration of the reversible bond can be appropriately selected based on the glass transition temperature defined by the tan δ peak top of the target cured product in a dynamic viscoelasticity measuring device (DMA). For example, when the glass transition temperature is used as a guideline, if the glass transition temperature of the cured product is near room temperature, sufficient repairability and remoldability functions are likely to be expressed even at the low concentration side of the preferred range. On the other hand, if the glass transition temperature of the target cured product exceeds 100 ° C. as a guideline, the functions are likely to be expressed at the high concentration side of the preferred range. However, in the temperature range exceeding the glass transition temperature measured by DMA, molecular mobility is generally high, and even if the concentration of the glycidyl group-containing compound is low, sufficient repairability and reshapeability functions are easily expressed, so for example, the effect of expressing the repairability and reshapeability functions can be adjusted by appropriately adjusting the aging temperature for repair and the heating temperature for reshaping. Thus, the relationship between the glass transition temperature of the cured product and the concentration of reversible bonds is not limited to these.
[0070] The ratio of the total number of glycidyl groups to the total number of active groups capable of reacting with the glycidyl groups in the curable resin composition of the present invention is not particularly limited, but in terms of good mechanical properties and the like of the resulting cured product, it is preferable that the amount of active groups capable of reacting with the glycidyl groups be 0.4 to 1.5 equivalents per equivalent of the total number of glycidyl groups in the resin composition.
[0071] The curable resin composition may contain a curing accelerator. Various types of curing accelerators can be used, including urea compounds, phosphorus compounds, tertiary amines, imidazole, imidazoline, organic acid metal salts, Lewis acids, and amine complex salts. When used as an adhesive, urea compounds, particularly 3-(3,4-dichlorophenyl)-1,1-dimethylurea (DCMU), are preferred because of their excellent workability and low-temperature curing properties. When used as a semiconductor encapsulating material, triphenylphosphine is preferred as a phosphorus compound, and 1,8-diazabicyclo-[5.4.0]-undecene is preferred as a tertiary amine because of their excellent curing properties, heat resistance, electrical properties, and moisture resistance reliability.
[0072] Examples of the phosphorus compound include alkyl phosphines such as ethylphosphine and butylphosphine, primary phosphines such as phenylphosphine, dialkyl phosphines such as dimethylphosphine and dipropylphosphine, secondary phosphines such as diphenylphosphine and methylethylphosphine, and tertiary phosphines such as trimethylphosphine, triethylphosphine and triphenylphosphine.
[0073] Examples of the imidazole include imidazole, 1-methylimidazole, 2-methylimidazole, 3-methylimidazole, 4-methylimidazole, 5-methylimidazole, 1-ethylimidazole, 2-ethylimidazole, 3-ethylimidazole, 4-ethylimidazole, 5-ethylimidazole, 1-n-propylimidazole, 2-n-propylimidazole, 1-isopropylimidazole, 2-isopropylimidazole, and isopropylimidazole, 1-n-butylimidazole, 2-n-butylimidazole, 1-isobutylimidazole, 2-isobutylimidazole, 2-undecyl-1H-imidazole, 2-heptadecyl-1H-imidazole, 1,2-dimethylimidazole, 1,3-dimethylimidazole, 2,4-dimethylimidazole, 2-ethyl-4-methylimidazole, 1-phenylimidazole, 2-phenyl-1H-imidazole Midazole, 4-methyl-2-phenyl-1H-imidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenylimidazole isocyanuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 1-cyanoethyl-2-phenyl-4,5-di(2-cyanoethoxy)methylimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 1-benzyl-2-phenylimidazole hydrochloride, etc.
[0074] Examples of the imidazoline compound include 2-methylimidazoline and 2-phenylimidazoline.
[0075] Examples of the urea compound include p-chlorophenyl-N,N-dimethylurea, 3-phenyl-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-N,N-dimethylurea, and N-(3-chloro-4-methylphenyl)-N',N'-dimethylurea.
[0076] The curable resin composition of the present invention may be used in combination with other thermosetting resins or thermoplastic resins within the range that does not impair the effects of the present invention.
[0077] Examples of other thermosetting resins include cyanate ester resins, resins having a benzoxazine structure, active ester resins, vinylbenzyl compounds, acrylic compounds, copolymers of styrene and maleic anhydride, etc. When the other thermosetting resins described above are used in combination, the amount of use is not particularly limited as long as it does not inhibit the effects of the present invention, but is preferably in the range of 1 to 50 parts by mass in 100 parts by mass of the curable resin composition.
[0078] Examples of the cyanate ester resin include bisphenol A type cyanate ester resin, bisphenol F type cyanate ester resin, bisphenol E type cyanate ester resin, bisphenol S type cyanate ester resin, bisphenol sulfide type cyanate ester resin, phenylene ether type cyanate ester resin, naphthylene ether type cyanate ester resin, biphenyl type cyanate ester resin, tetramethylbiphenyl type cyanate ester resin, polyhydroxynaphthalene type cyanate ester resin, phenol novolac type cyanate ester resin, cresol novolac type cyanate ester resin, triphenyl Examples of the cyanate ester resin include tetraphenylethane type cyanate ester resin, dicyclopentadiene-phenol addition reaction type cyanate ester resin, phenol aralkyl type cyanate ester resin, naphthol novolac type cyanate ester resin, naphthol aralkyl type cyanate ester resin, naphthol-phenol co-condensed novolac type cyanate ester resin, naphthol-cresol co-condensed novolac type cyanate ester resin, aromatic hydrocarbon formaldehyde resin modified phenol resin type cyanate ester resin, biphenyl modified novolac type cyanate ester resin, anthracene type cyanate ester resin, etc. These may be used alone or in combination of two or more.
[0079] Among these cyanate ester resins, it is preferable to use bisphenol A type cyanate ester resin, bisphenol F type cyanate ester resin, bisphenol E type cyanate ester resin, polyhydroxynaphthalene type cyanate ester resin, naphthylene ether type cyanate ester resin, and novolac type cyanate ester resin, in that a cured product having excellent heat resistance can be obtained, and it is preferable to use dicyclopentadiene-phenol addition reaction type cyanate ester resin in that a cured product having excellent dielectric properties can be obtained.
[0080] The resin having a benzoxazine structure is not particularly limited, and examples thereof include a reaction product of bisphenol F, formalin, and aniline (Fa-type benzoxazine resin), a reaction product of diaminodiphenylmethane, formalin, and phenol (Pd-type benzoxazine resin), a reaction product of bisphenol A, formalin, and aniline, a reaction product of dihydroxydiphenyl ether, formalin, and aniline, a reaction product of diaminodiphenyl ether, formalin, and phenol, a reaction product of dicyclopentadiene-phenol addition type resin, formalin, and aniline, a reaction product of phenolphthalein, formalin, and aniline, a reaction product of diphenyl sulfide, formalin, and aniline, etc. Each of these may be used alone, or two or more of them may be used in combination.
[0081] The active ester resin is not particularly limited, but generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester resin is preferably obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester resin obtained from a carboxylic acid compound or its halide and a hydroxy compound is preferred, and an active ester resin obtained from a carboxylic acid compound or its halide and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, and the like, or halides thereof. Examples of the phenol compound or naphthol compound include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, dihydroxydiphenyl ether, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, and dicyclopentadiene-phenol adduct resins.
[0082] Specific examples of the active ester resin include active ester resins containing a dicyclopentadiene-phenol addition structure, active ester resins containing a naphthalene structure, active ester resins which are acetylated phenol novolac, and active ester resins which are benzoylated phenol novolac. Of these, the active ester resins containing a dicyclopentadiene-phenol addition structure and the active ester resins containing a naphthalene structure are more preferred in terms of their excellent ability to improve peel strength.
[0083] Furthermore, various novolak resins, addition polymerization resins of alicyclic diene compounds such as dicyclopentadiene and phenol compounds, modified novolak resins of phenolic hydroxyl group-containing compounds and alkoxy group-containing aromatic compounds, phenol aralkyl resins (Zylok resins), naphthol aralkyl resins, trimethylolmethane resins, tetraphenylolethane resins, biphenyl-modified phenol resins, biphenyl-modified naphthol resins, aminotriazine-modified phenol resins, and various vinyl polymers may be used in combination.
[0084] More specifically, the various novolak resins include polymers obtained by reacting a phenolic hydroxyl group-containing compound, such as phenol, phenylphenol, resorcinol, biphenyl, bisphenol such as bisphenol A or bisphenol F, naphthol, or dihydroxynaphthalene, with an aldehyde compound under acid catalyst conditions.
[0085] Examples of the various vinyl polymers include homopolymers of vinyl compounds such as polyhydroxystyrene, polystyrene, polyvinylnaphthalene, polyvinylanthracene, polyvinylcarbazole, polyindene, polyacenaphthylene, polynorbornene, polycyclodecene, polytetracyclododecene, polynortricyclene, and poly(meth)acrylate, or copolymers thereof.
[0086] Thermoplastic resin refers to a resin that can be melt molded by heating. Specific examples thereof include polyethylene resin, polypropylene resin, polystyrene resin, rubber-modified polystyrene resin, acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-styrene (AS) resin, polymethyl methacrylate resin, acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyethylene terephthalate resin, ethylene vinyl alcohol resin, cellulose acetate resin, ionomer resin, polyacrylonitrile resin, polyamide resin, polyacetal resin, polybutylene terephthalate resin, polylactic acid resin, polyphenylene ether resin, modified polyphenylene ether resin, polycarbonate resin, polysulfone resin, polyphenylene sulfide resin, polyetherimide resin, polyethersulfone resin, polyarylate resin, thermoplastic polyimide resin, polyamideimide resin, polyetheretherketone resin, polyketone resin, liquid crystal polyester resin, fluororesin, syndiotactic polystyrene resin, and cyclic polyolefin resin. These thermoplastic resins can be used alone or in combination of two or more.
[0087] When these other resins are used, the blending ratio of the glycidyl group-containing compound of the present invention to the other resins can be set arbitrarily depending on the application. From the viewpoint of not impairing the repairability and remoldability exhibited by the present invention, however, the blending ratio of the other resins is preferably 0.5 to 100 parts by mass per 100 parts by mass of the glycidyl group-containing compound of the present invention.
[0088] When the curable resin composition of the present invention is used in an application requiring high flame retardancy, a non-halogen flame retardant substantially containing no halogen atoms may be blended therein.
[0089] Examples of the non-halogen flame retardant include phosphorus-based flame retardants, nitrogen-based flame retardants, silicone-based flame retardants, inorganic flame retardants, and organic metal salt-based flame retardants. There are no limitations on the use of these flame retardants. They may be used alone or in combination with a plurality of flame retardants of the same type. Also, flame retardants of different types may be used in combination.
[0090] The phosphorus-based flame retardant may be either inorganic or organic. Examples of inorganic compounds include red phosphorus, ammonium phosphates such as monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate, and inorganic nitrogen-containing phosphorus compounds such as phosphoric acid amide.
[0091] The red phosphorus is preferably surface-treated for the purpose of preventing hydrolysis and the like. Examples of the surface treatment method include (i) a method of coating with an inorganic compound such as magnesium hydroxide, aluminum hydroxide, zinc hydroxide, titanium hydroxide, bismuth oxide, bismuth hydroxide, bismuth nitrate, or a mixture thereof, (ii) a method of coating with a mixture of an inorganic compound such as magnesium hydroxide, aluminum hydroxide, zinc hydroxide, titanium hydroxide, and a thermosetting resin such as a phenolic resin, and (iii) a method of doubly coating with a thermosetting resin such as a phenolic resin on a coating of an inorganic compound such as magnesium hydroxide, aluminum hydroxide, zinc hydroxide, titanium hydroxide, etc.
[0092] Examples of the organophosphorus compound include general-purpose organophosphorus compounds such as phosphate ester compounds, phosphonic acid compounds, phosphinic acid compounds, phosphine oxide compounds, phosphorane compounds, and organic nitrogen-containing phosphorus compounds, as well as cyclic organophosphorus compounds such as 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, and 10-(2,7-dihydroxynaphthyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, and derivatives thereof reacted with compounds such as epoxy resins and phenol resins.
[0093] The amount of these phosphorus-based flame retardants to be added is appropriately selected depending on the type of phosphorus-based flame retardant, other components of the resin composition, and the desired level of flame retardancy. For example, in 100 parts by mass of a resin composition containing all of the non-halogenated flame retardants and other fillers and additives, when red phosphorus is used as the non-halogenated flame retardant, it is preferably added in a range of 0.1 to 2.0 parts by mass, and when an organic phosphorus compound is used, it is similarly preferably added in a range of 0.1 to 10.0 parts by mass, and more preferably added in a range of 0.5 to 6.0 parts by mass.
[0094] When the phosphorus-based flame retardant is used, hydrotalcite, magnesium hydroxide, boron compounds, zirconium oxide, black dyes, calcium carbonate, zeolite, zinc molybdate, activated carbon, etc. may be used in combination with the phosphorus-based flame retardant.
[0095] Examples of the nitrogen-based flame retardant include triazine compounds, cyanuric acid compounds, isocyanuric acid compounds, and phenothiazines, with triazine compounds, cyanuric acid compounds, and isocyanuric acid compounds being preferred.
[0096] Examples of the triazine compounds include melamine, acetoguanamine, benzoguanamine, melon, melam, succinoguanamine, ethylenedimelamine, melamine polyphosphate, triguanamine, and the like, as well as (1) aminotriazine sulfate compounds such as guanylmelamine sulfate, melem sulfate, and melam sulfate, (2) co-condensates of phenols such as phenol, cresol, xylenol, butylphenol, and nonylphenol with melamines such as melamine, benzoguanamine, acetoguanamine, and formguanamine and formaldehyde, (3) mixtures of the co-condensates of (2) with phenolic resins such as phenol-formaldehyde condensates, and (4) compounds obtained by further modifying (2) and (3) with tung oil, isomerized linseed oil, or the like.
[0097] Examples of the cyanuric acid compound include cyanuric acid and melamine cyanurate.
[0098] The amount of the nitrogen-based flame retardant to be blended is appropriately selected depending on the type of nitrogen-based flame retardant, other components of the resin composition, and the desired level of flame retardancy. For example, it is preferable to blend in an amount of 0.05 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the resin composition containing all of the non-halogen flame retardant and other fillers and additives.
[0099] When the nitrogen-based flame retardant is used, a metal hydroxide, a molybdenum compound, etc. may be used in combination.
[0100] The silicone flame retardant can be used without any particular limitation as long as it is an organic compound containing silicon atoms, and examples thereof include silicone oil, silicone rubber, silicone resin, etc. The amount of the silicone flame retardant is appropriately selected according to the type of silicone flame retardant, other components of the resin composition, and the desired level of flame retardancy, but it is preferable to mix it in the range of 0.05 to 20 parts by mass in 100 parts by mass of the resin composition containing all of the non-halogen flame retardant and other fillers and additives. When using the silicone flame retardant, a molybdenum compound, alumina, etc. may be used in combination.
[0101] Examples of the inorganic flame retardant include metal hydroxides, metal oxides, metal carbonate compounds, metal powders, boron compounds, and low-melting glass.
[0102] Examples of the metal hydroxide include aluminum hydroxide, magnesium hydroxide, dolomite, hydrotalcite, calcium hydroxide, barium hydroxide, and zirconium hydroxide.
[0103] Examples of the metal oxide include zinc molybdate, molybdenum trioxide, zinc stannate, tin oxide, aluminum oxide, iron oxide, titanium oxide, manganese oxide, zirconium oxide, zinc oxide, molybdenum oxide, cobalt oxide, bismuth oxide, chromium oxide, nickel oxide, copper oxide, and tungsten oxide.
[0104] Examples of the metal carbonate compound include zinc carbonate, magnesium carbonate, calcium carbonate, barium carbonate, basic magnesium carbonate, aluminum carbonate, iron carbonate, cobalt carbonate, and titanium carbonate.
[0105] Examples of the metal powder include aluminum, iron, titanium, manganese, zinc, molybdenum, cobalt, bismuth, chromium, nickel, copper, tungsten, and tin.
[0106] Examples of the boron compound include zinc borate, zinc metaborate, barium metaborate, boric acid, and borax.
[0107] Examples of the low-melting glass include glassy compounds such as Seapley (Boxey Brown), hydrated glass SiO2-MgO-H2O, PbO-B2O3, ZnO-P2O5-MgO, P2O5-B2O3-PbO-MgO, P-Sn-OF, PbO-V2O5-TeO2, Al2O3-H2O, and lead borosilicate.
[0108] The amount of the inorganic flame retardant to be blended is appropriately selected depending on the type of inorganic flame retardant, other components of the resin composition, and the desired level of flame retardancy. For example, it is preferable to blend in an amount of 0.05 to 20 parts by mass, and more preferably 0.5 to 15 parts by mass, per 100 parts by mass of the resin composition containing all of the non-halogen flame retardant and other fillers and additives.
[0109] Examples of the organometallic salt flame retardant include ferrocene, acetylacetonate metal complexes, organometallic carbonyl compounds, organocobalt salt compounds, organosulfonic acid metal salts, and compounds in which a metal atom is ionic- or coordinate-bonded to an aromatic compound or a heterocyclic compound.
[0110] The amount of the organometallic salt flame retardant to be blended is appropriately selected depending on the type of organometallic salt flame retardant, the other components of the resin composition, and the desired level of flame retardancy. For example, it is preferable to blend in an amount of 0.005 to 10 parts by mass per 100 parts by mass of the resin composition containing all of the non-halogen flame retardant and other fillers, additives, etc.
[0111] The curable resin composition of the present invention may contain a filler. Examples of the filler include inorganic fillers and organic fillers. Examples of the inorganic filler include inorganic fine particles.
[0112] Examples of inorganic fine particles include those with excellent heat resistance, such as alumina, magnesia, titania, zirconia, and silica (quartz, fumed silica, precipitated silica, silicic anhydride, fused silica, crystalline silica, and ultrafine amorphous silica); those with excellent thermal conductivity, such as boron nitride, aluminum nitride, alumina oxide, titanium oxide, magnesium oxide, zinc oxide, silicon oxide, and diamond; those with excellent electrical conductivity, such as metal fillers and / or metal-coated fillers using simple metals or alloys (e.g., iron, copper, magnesium, aluminum, gold, silver, platinum, zinc, manganese, and stainless steel); and those with excellent barrier properties, such as minerals such as mica, clay, kaolin, talc, zeolite, wollastonite, and smectite, potassium titanate, magnesium sulfate, sepiolite, zonolite, and the like. , aluminum borate, calcium carbonate, titanium oxide, barium sulfate, zinc oxide, magnesium hydroxide; those with a high refractive index include barium titanate, zirconia oxide, titanium oxide, etc.; those exhibiting photocatalytic properties include photocatalytic metals such as titanium, cerium, zinc, copper, aluminum, tin, indium, phosphorus, carbon, sulfur, ruthenium, nickel, iron, cobalt, silver, molybdenum, strontium, chromium, barium, lead, etc., composites of the above metals, and oxides thereof; those with excellent wear resistance include metals such as silica, alumina, zirconia, magnesium oxide, etc., composites and oxides thereof; those with excellent electrical conductivity include metals such as silver and copper, tin oxide, indium oxide, etc.; those with excellent insulation properties include silica, etc.; those with excellent ultraviolet shielding properties include titanium oxide, zinc oxide, etc. These inorganic fine particles can be selected appropriately depending on the application, and can be used alone or in combination of multiple types. In addition, the above inorganic fine particles have various properties other than those listed as examples, so they can be selected appropriately according to the application.
[0113] For example, when silica is used as inorganic fine particles, known silica fine particles such as powdered silica and colloidal silica can be used without any particular limitation. Commercially available powdered silica fine particles include, for example, Aerosil 50 and 200 manufactured by Nippon Aerosil Co., Ltd., Sildex H31, H32, H51, H52, H121, and H122 manufactured by Asahi Glass Co., Ltd., E220A and E220 manufactured by Nippon Silica Industry Co., Ltd., SYLYSIA470 manufactured by Fuji Silysia Co., Ltd., and SG Flake manufactured by Nippon Sheet Glass Co., Ltd.
[0114] Examples of commercially available colloidal silica include methanol silica sol, IPA-ST, MEK-ST, NBA-ST, XBA-ST, DMAC-ST, ST-UP, ST-OUP, ST-20, ST-40, ST-C, ST-N, ST-O, ST-50, and ST-OL, all of which are manufactured by Nissan Chemical Industries, Ltd.
[0115] Surface-modified silica fine particles may be used, for example, the silica fine particles are surface-treated with a reactive silane coupling agent having a hydrophobic group, or modified with a compound having a (meth)acryloyl group. Commercially available powdered silica modified with a compound having a (meth)acryloyl group includes Aerosil RM50, R711, etc. manufactured by Nippon Aerosil Co., Ltd., and commercially available colloidal silica modified with a compound having a (meth)acryloyl group includes MIBK-SD, etc. manufactured by Nissan Chemical Industries, Ltd.
[0116] The shape of the silica fine particles is not particularly limited, and spherical, hollow, porous, rod-like, plate-like, fibrous, or amorphous shapes can be used. The primary particle size is preferably in the range of 5 to 200 nm.
[0117] As the titanium oxide fine particles, not only extender pigments but also ultraviolet light responsive photocatalysts can be used, for example, anatase type titanium oxide, rutile type titanium oxide, brookite type titanium oxide, etc. can be used. Furthermore, particles designed to respond to visible light by doping different elements into the crystal structure of titanium oxide can also be used. As the element to be doped into titanium oxide, anion elements such as nitrogen, sulfur, carbon, fluorine, phosphorus, etc., and cationic elements such as chromium, iron, cobalt, manganese, etc. are preferably used. In addition, as the form, powder, sol dispersed in an organic solvent or water, or slurry can be used. As commercially available powdered titanium oxide fine particles, for example, Aerosil P-25 manufactured by Nippon Aerosil Co., Ltd., ATM-100 manufactured by Teika Co., Ltd., etc. can be used. In addition, as commercially available slurry-like titanium oxide fine particles, for example, TKD-701 manufactured by Teika Co., Ltd., etc. can be used.
[0118] The curable resin composition of the present invention may further contain a fibrous substrate. The fibrous substrate is not particularly limited, but is preferably one used in fiber-reinforced resins, such as inorganic fibers and organic fibers.
[0119] Examples of inorganic fibers include inorganic fibers such as carbon fibers, glass fibers, boron fibers, alumina fibers, and silicon carbide fibers, as well as carbon fibers, activated carbon fibers, graphite fibers, tungsten carbide fibers, silicon carbide fibers (silicon carbide fibers), ceramic fibers, natural fibers, mineral fibers such as basalt, boron nitride fibers, boron carbide fibers, and metal fibers. Examples of the metal fibers include aluminum fibers, copper fibers, brass fibers, stainless steel fibers, and steel fibers.
[0120] Examples of organic fibers include synthetic fibers made of resin materials such as polybenzazole, aramid, PBO (polyparaphenylene benzoxazole), polyphenylene sulfide, polyester, acrylic, polyamide, polyolefin, polyvinyl alcohol, and polyarylate; natural fibers such as cellulose, pulp, cotton, wool, and silk; and regenerated fibers such as protein, polypeptide, and alginic acid.
[0121] Among these, carbon fiber and glass fiber are preferred because they have a wide range of industrial applications. Of these, only one type may be used, or a plurality of types may be used simultaneously.
[0122] The fibrous substrate may be an assembly of fibers, the fibers may be continuous or discontinuous, and may be in the form of a woven or nonwoven fabric. It may also be a fiber bundle in which the fibers are aligned in one direction, or in the form of a sheet in which fiber bundles are arranged. It may also be a three-dimensional shape in which a thickness is added to an assembly of fibers.
[0123] The curable resin composition of the present invention may contain a dispersion medium for the purpose of adjusting the solid content and viscosity of the resin composition. The dispersion medium may be any liquid medium that does not impair the effects of the present invention, and examples of the dispersion medium include various organic solvents and liquid organic polymers.
[0124] Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone (MEK), and methyl isobutyl ketone (MIBK); cyclic ethers such as tetrahydrofuran (THF), and dioxolane; esters such as methyl acetate, ethyl acetate, and butyl acetate; aromatics such as toluene and xylene; and alcohols such as carbitol, cellosolve, methanol, isopropanol, butanol, and propylene glycol monomethyl ether. These can be used alone or in combination, but of these, methyl ethyl ketone is preferred from the standpoint of volatility during coating and solvent recovery.
[0125] The liquid organic polymer is a liquid organic polymer that does not directly contribute to the curing reaction, and examples thereof include acrylic polymers (Floren WK-20: Kyoeisha), amine salts of special modified phosphate esters (HIPLAAD ED-251: Kusumoto Chemicals), and modified acrylic block copolymers (DISPERBYK2000; BYK-Chemie).
[0126] The resin composition of the present invention may contain other compounds, such as catalysts, polymerization initiators, inorganic pigments, organic pigments, extender pigments, clay minerals, waxes, surfactants, stabilizers, flow control agents, coupling agents, dyes, leveling agents, rheology control agents, ultraviolet absorbers, antioxidants, flame retardants, plasticizers, and reactive diluents.
[0127] The resin composition of the present invention can be cured to obtain a cured product. When curing, the resin composition may be cured at room temperature or by heating. When performing heat curing, the resin composition may be cured by one heating step or may be cured by multiple heating steps.
[0128] The curable resin composition of the present invention can also be cured by active energy rays. In that case, a photocationic polymerization initiator may be used as the polymerization initiator. The active energy rays may be visible light, ultraviolet light, X-rays, electron beams, etc.
[0129] Examples of the photocationic polymerization initiator include aryl-sulfonium salts and aryl-iodonium salts, and specifically, arylsulfonium hexafluorophosphate, arylsulfonium hexafluoroantimonate, arylsulfonium tetrakis(pentafluoro)borate, tri(alkylphenyl)sulfonium hexafluorophosphate, etc. The photocationic polymerization initiator may be used alone or in combination of two or more kinds.
[0130] The curable resin composition of the present invention can be prepared by uniformly mixing the above-mentioned components, and the method is not particularly limited. For example, the composition can be prepared by uniformly mixing the components using a pot mill, a ball mill, a bead mill, a roll mill, a homogenizer, a super mill, a homodisper, a universal mixer, a Banbury mixer, a kneader, or the like.
[0131] The curable resin composition of the present invention is prepared by dissolving the above-mentioned glycidyl group-containing compound of the present invention and the compound (I) reactive with the above-mentioned glycidyl group-containing compound, and further the above-mentioned curing agent that can be used in combination, filler, fibrous substrate, dispersion medium, and resin other than the above-mentioned various compounds in a dispersion medium such as the above-mentioned organic solvent, if necessary. After dissolving, the solvent is distilled off and the curable resin composition can be obtained by drying under reduced pressure using a vacuum oven or the like. The curable resin composition of the present invention may be in a state in which the above-mentioned constituent materials are uniformly mixed. At this time, it is preferable to mix uniformly using a mixer or the like. The blending ratio of each constituent material can be appropriately adjusted according to the desired characteristics of the cured product, such as mechanical strength, heat resistance, repairability, and remoldability. In addition, in the preparation of the curable resin composition, the specific order of mixing the constituent materials is not particularly limited.
[0132] The cured product of the present invention is obtained by curing a compound (I) reactive with the glycidyl group-containing compound with the glycidyl group-containing compound of the present invention. The curing method can be appropriately selected and adopted from known methods depending on the properties of the compound (I) reactive with the glycidyl group-containing compound used.
[0133] As described above, the cured product of the present invention is cured by the glycidyl group-containing compound of the present invention, and thus can maintain good mechanical strength by exhibiting a suitable crosslinking density. In addition, when mechanical energy such as scratches or external force is applied to the cured product of the present invention, the reversible bond is broken, but the equilibrium shifts in the bond direction, so that an adduct is formed again, which is considered to enable repair of the scratches and remolding.
[0134] The structure of the obtained cured product can be confirmed by infrared absorption (IR) spectroscopy using Fourier transform infrared spectroscopy (FT-IR) or the like, elemental analysis, X-ray scattering, or the like.
[0135] As described above, the cured product, which is one embodiment of the present invention, can be obtained by using the glycidyl group-containing compound of the present invention as one component of a curable resin composition. However, it is also possible to use a conjugated diene having one or more glycidyl groups, which is an intermediate of the glycidyl group-containing compound, and a parent diene, and form the glycidyl group-containing compound during the curing process (while synthesizing in situ) to produce a cured product.
[0136] The curable resin composition of the present invention and a cured product produced from the curable resin composition are easily dismantled, repaired, and remoldable, and are useful for the following applications.
[0137] The curable resin cured product of the present invention can be laminated with a substrate to form a laminate. The substrate of the laminate may be an inorganic material such as metal or glass, or an organic material such as plastic or wood, and may be used as appropriate depending on the application. The substrate may be in the shape of a laminate, a flat plate, a sheet, or a three-dimensional structure, or may be three-dimensional. The substrate may have any shape according to the purpose, such as a shape having a curvature on the entire surface or in a part. There is no restriction on the hardness, thickness, etc. of the substrate. The first substrate, a layer made of the cured product of the curable resin composition of the present invention, and a second substrate may be laminated in this order to form a multilayer laminate. The curable resin composition of the present embodiment has excellent adhesiveness, and can be suitably used as an adhesive for bonding a first substrate and a second substrate. The curable resin cured product of the present invention may be used as a substrate, and the cured product of the present invention may be further laminated.
[0138] In addition, the cured product of the curable resin of the present invention can relieve stress, and therefore can be suitably used for bonding different materials. For example, even in a laminate in which the substrate is a metal and / or metal oxide and the second substrate is a different material such as a plastic layer, the adhesive strength is maintained due to the stress relaxation ability of the cured product of the present invention.
[0139] In the laminate obtained by laminating the cured product of the present invention and the substrate, the layer containing the cured product may be formed by direct coating or molding on the substrate, or an already molded product may be laminated. When directly coating, the coating method is not particularly limited, and examples thereof include spraying, spin coating, dip coating, roll coating, blade coating, doctor roll, doctor blade, curtain coating, slit coating, screen printing, and inkjet. When directly molding, examples include in-mold molding, insert molding, vacuum molding, extrusion lamination molding, and press molding. When laminating a molded composition, an uncured or semi-cured composition layer may be laminated and then cured, or a layer containing a cured product obtained by completely curing the composition may be laminated on the substrate. In addition, the cured product of the present invention may be laminated by coating a precursor that can be a substrate and curing it, or the precursor that can be a substrate or the composition of the present invention may be adhered in an uncured or semi-cured state and then cured. The precursor that can be a substrate is not particularly limited, and examples thereof include various curable resin compositions.
[0140] The cured product obtained by using the curable resin composition of the present invention has particularly high adhesion to metals and / or metal oxides, and can be particularly well used as a primer for metals. Metals include copper, aluminum, gold, silver, iron, platinum, chromium, nickel, tin, titanium, zinc, various alloys, and composite materials thereof, and metal oxides include single oxides and / or composite oxides of these metals. In particular, the cured product has excellent adhesion to iron, copper, and aluminum, and can be particularly well used as an adhesive for iron, copper, and aluminum.
[0141] The curable resin composition of the present invention can be suitably used as an adhesive for structural members in the fields of automobiles, trains, civil engineering and construction, electronics, aircraft, and the space industry. Even when used to bond different materials such as between metal and nonmetal, the adhesive can maintain high adhesion without being affected by changes in temperature environment, and peeling is unlikely to occur. In addition to structural member applications, the adhesive can also be used as an adhesive for general office use, medical use, carbon fiber, storage battery cells, modules, and cases, and can be used as an adhesive for bonding optical components, an adhesive for bonding optical disks, an adhesive for mounting printed wiring boards, a die bonding adhesive, an adhesive for semiconductors such as underfill, an underfill for reinforcing BGA, an anisotropic conductive film, an anisotropic conductive paste, and other mounting adhesives.
[0142] When the curable resin composition of the present invention has a fibrous substrate, and the fibrous substrate is a reinforcing fiber, the curable resin composition containing the fibrous substrate can be used as a fiber-reinforced resin. The method of adding the fibrous substrate to the composition is not particularly limited as long as it does not impair the effects of the present invention, and includes methods of compounding the fibrous substrate and the composition by kneading, coating, impregnation, injection, pressure bonding, etc., and can be appropriately selected depending on the form of the fiber and the use of the fiber-reinforced resin.
[0143] There is no particular limitation on the method of molding the fiber-reinforced resin. If a plate-shaped product is to be manufactured, an extrusion molding method is generally used, but it can also be manufactured by a flat press. In addition, extrusion molding, blow molding, compression molding, vacuum molding, injection molding, etc. can be used. If a film-shaped product is to be manufactured, in addition to the melt extrusion method, a solution casting method can be used. When a melt molding method is used, examples of the method include inflation film molding, cast molding, extrusion lamination molding, calendar molding, sheet molding, fiber molding, blow molding, injection molding, rotational molding, and coating molding. In addition, in the case of a resin that is cured by active energy rays, a cured product can be manufactured using various curing methods using active energy rays. In particular, when a thermosetting resin is used as the main component of the matrix resin, examples of the molding method include a molding method in which the molding material is made into a prepreg and pressurized and heated by a press or autoclave, and other examples of the molding method include RTM (Resin Transfer Molding) molding, VaRTM (Vacuum assist Resin Transfer Molding) molding, lamination molding, and hand layup molding.
[0144] The curable resin composition of the present invention, when used in a cured product, has restorability, remoldability, and ease of dismantling, and can therefore be used as a molding material for large cases, motor housings, casting materials for the inside of cases, gears, pulleys, etc. These may be cured products of the resin alone, or may be cured products reinforced with fibers such as glass chips.
[0145] The fiber reinforced resin can form a state called an uncured or semi-cured prepreg. After distributing the product in the prepreg state, final curing may be performed to form a cured product. When forming a laminate, it is preferable to form a prepreg, then laminate other layers and then perform final curing, since this allows the formation of a laminate in which each layer is in close contact with each other. The mass ratio of the composition and the fibrous substrate used at this time is not particularly limited, but it is usually preferable to prepare the resin content in the prepreg to be 20 to 60 mass%.
[0146] The cured product of the present invention has repairability, easy dismantling and remolding properties, and can be used as a heat-resistant material and an electronic material, especially when a combination with a high dissociation temperature is used. In particular, it can be suitably used for semiconductor encapsulation materials, circuit boards, build-up films, build-up boards, adhesives and resist materials. It can also be suitably used as a matrix resin for fiber-reinforced resins, and is particularly suitable as a highly heat-resistant prepreg. The heat-resistant and electronic components thus obtained can be suitably used for various applications, such as industrial machine parts, general machine parts, automobile, railway and vehicle parts, space and aviation related parts, electronic and electrical parts, building materials, containers and packaging materials, daily necessities, sports and leisure goods, and housing members for wind power generation, but are not limited thereto.
[0147] In particular, the adhesive can be suitably used as an adhesive for structural members in the fields of automobiles, trains, civil engineering and construction, electronics, aircraft, and the space industry, taking advantage of its excellent characteristics such as easy dismantling in the cured product. The adhesive of the present invention can maintain high adhesiveness even when used to bond different materials such as between metal and nonmetal. In addition to structural member applications, the adhesive of the present invention can also be used as an adhesive for general office use, medical use, carbon fiber, storage battery cells, modules, and cases, and examples thereof include adhesives for bonding optical components, adhesives for bonding optical disks, adhesives for mounting printed wiring boards, die bonding adhesives, adhesives for semiconductors such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films and anisotropic conductive pastes.
[0148] Below, we will explain some representative products by giving examples.
[0149] 1. Semiconductor encapsulation materials As a method for obtaining a semiconductor encapsulation material from the resin composition of the present invention, the resin composition, the curing accelerator, and compounding agents such as inorganic fillers are melt-mixed sufficiently until homogeneous using an extruder, kneader, roll, etc. as necessary. In this case, fused silica is usually used as the inorganic filler, but when used as a high thermal conductivity semiconductor encapsulation material for power transistors and power ICs, it is preferable to use highly filled crystalline silica, alumina, silicon nitride, etc., which have a higher thermal conductivity than fused silica, or fused silica, crystalline silica, alumina, silicon nitride, etc. The filling rate is preferably in the range of 30 to 95 mass% per 100 parts by mass of the curable resin composition, and among them, in order to improve flame retardancy, moisture resistance, and solder crack resistance and to reduce the linear expansion coefficient, it is more preferable that the inorganic filler is 70 parts by mass or more, and even more preferable that the inorganic filler is 80 parts by mass or more.
[0150] 2. Semiconductor Devices The semiconductor package molding for obtaining a semiconductor device from the curable resin composition of the present invention can be carried out by molding the semiconductor encapsulating material using a casting machine, a transfer molding machine, an injection molding machine or the like, and then heating the molded product at 50 to 250°C for 2 to 10 hours.
[0151] 3. Printed Circuit Boards A method for obtaining a printed circuit board from the composition of the present invention includes laminating the above prepreg by a conventional method, appropriately overlaying copper foil, and heat-pressing the laminate at 170 to 300°C under a pressure of 1 to 10 MPa for 10 minutes to 3 hours.
[0152] 4. Flexible board The method for producing a flexible substrate from the crosslinkable resin composition of the present invention includes a method comprising the following three steps: The first step is to apply the crosslinkable resin composition containing a resin component, an organic solvent, etc., to an electrical insulating film using a coater such as a reverse roll coater or a comma coater, the second step is to heat the electrical insulating film to which the crosslinkable resin composition has been applied at 60 to 170°C for 1 to 15 minutes using a heater to volatilize the solvent from the electrical insulating film and to bring the crosslinkable resin composition to a B-stage, and the third step is to thermocompress (preferably a compression pressure of 2 to 200 N / cm and a compression temperature of 40 to 200°C) a metal foil to an adhesive on the electrical insulating film to which the crosslinkable resin composition has been brought to a B-stage using a heating roll or the like. If sufficient adhesive performance is obtained by going through the above three steps, the process may be terminated here, but if complete adhesive performance is required, it is preferable to further post-cure under conditions of 100 to 200° C. for 1 to 24 hours. The thickness of the resin composition layer after final curing is preferably in the range of 5 to 100 μm.
[0153] 5. Build-up board The method for obtaining a build-up board from the composition of the present invention includes, for example, the following steps. First, the above composition, which is appropriately blended with rubber, filler, etc., is applied to a circuit board on which a circuit is formed by using a spray coating method, a curtain coating method, etc., and then cured (step 1). Then, if necessary, a predetermined through-hole portion or the like is drilled, treated with a roughening agent, and the surface is washed with hot water to form unevenness, and a metal such as copper is plated (step 2). These operations are repeated as desired, and a resin insulating layer and a conductor layer of a predetermined circuit pattern are alternately built up to form the build-up (step 3). Note that the through-hole portion is drilled after the formation of the outermost resin insulating layer. In addition, the build-up board of the present invention can also be produced by forming a roughened surface by heating and pressing the resin-coated copper foil, which is obtained by semi-curing the resin composition on the copper foil, on a wiring board on which a circuit is formed, at 170 to 300 ° C., thereby omitting the steps of forming a roughened surface and plating.
[0154] 6. Build-up film A build-up film can be obtained from the composition of the present invention by applying the composition to the surface of a support film (Y) as a substrate, and then drying the organic solvent by heating or blowing hot air or the like to form a layer of the composition (X).
[0155] As the organic solvent used here, for example, ketones such as acetone, methyl ethyl ketone, cyclohexanone, etc., acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, carbitol acetate, etc., carbitols such as cellosolve, butyl carbitol, etc., aromatic hydrocarbons such as toluene, xylene, etc., dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc. are preferably used, and it is also preferable to use them in a proportion such that the nonvolatile content is 30 to 60 mass%.
[0156] The thickness of the layer (X) formed is usually equal to or greater than the thickness of the conductor layer. Since the thickness of the conductor layer of the circuit board is usually in the range of 5 to 70 μm, the thickness of the resin composition layer is preferably 10 to 100 μm. The layer (X) of the composition in the present invention may be protected with a protective film described below. By protecting the layer with a protective film, it is possible to prevent the adhesion of dirt and the like to the surface of the resin composition layer and prevent scratches.
[0157] The above-mentioned support film and protective film may be made of polyolefins such as polyethylene, polypropylene, and polyvinyl chloride, polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate, polycarbonate, polyimide, and even release paper and metal foils such as copper foil and aluminum foil. The support film and protective film may be subjected to a matte treatment, a corona treatment, or a release treatment. The thickness of the support film is not particularly limited, but is usually 10 to 150 μm, and is preferably in the range of 25 to 50 μm. The thickness of the protective film is preferably 1 to 40 μm.
[0158] The support film (Y) is peeled off after laminating it on a circuit board or after forming an insulating layer by heat curing. If the support film (Y) is peeled off after the curable resin composition layer constituting the build-up film is heat cured, adhesion of dust and the like during the curing process can be prevented. When peeling off after curing, the support film is usually subjected to a release treatment in advance.
[0159] A multilayer printed circuit board can be manufactured using the build-up film obtained as described above. For example, when the layer (X) is protected by a protective film, the protective film is peeled off, and then the layer (X) is laminated, for example, by a vacuum lamination method on one or both sides of the circuit board so as to be in direct contact with the circuit board. The lamination method may be a batch method or a continuous method using a roll. If necessary, the build-up film and the circuit board may be heated (preheated) before lamination. The lamination conditions are preferably a pressure bonding temperature (lamination temperature) of 70 to 140°C and a pressure bonding pressure of 1 to 11 kgf / cm. 2 (9.8×10 4 ~107.9×10 4 N / m 2 ), and lamination is preferably performed under reduced air pressure of 20 mmHg (26.7 hPa) or less.
[0160] 7.Conductive paste A method for obtaining a conductive paste from the composition of the present invention includes, for example, dispersing conductive particles in the composition. The conductive paste can be a paste resin composition for circuit connection or an anisotropic conductive adhesive depending on the type of conductive particles used. EXAMPLES
[0161] The present invention will now be described in detail with reference to examples and comparative examples, in which "parts" and "%" are by weight unless otherwise specified, and the present invention is not limited thereto.
[0162] 1 H and 13 C-NMR, FD-MS spectrum, and GPC were measured under the following conditions.
[0163] 1 H-NMR: “JNM-ECA600” manufactured by JEOL RESONANCE Magnetic field strength: 600MHz Number of times: 32 Solvent: CDCl3, DMSO-d6 Sample concentration: 30% by mass
[0164] 13 C-NMR: “JNM-ECA600” manufactured by JEOL RESONANCE Magnetic field strength: 150MHz Number of times: 320 Solvent: DMSO-d6 Sample concentration: 30% by mass
[0165] FD-MS: JEOL Ltd. "JMS-T100GC AccuTOF" Measurement range: m / z=50.00~2000.00 Rate of change: 25.6mA / min Final current value: 40mA Cathode voltage: -10kV
[0166] GPC: Tosoh Corporation "HLC-8320GPC" Column: Tosoh Corporation "TSK-GEL G2000HXL" + "TSK-GEL G3000HXL" + "TSK-GEL G4000HXL" Detector: RI (Differential Refractometer) Measurement conditions: 40℃ Mobile phase: Tetrahydrofuran Flow rate: 1ml / min Standard: Tosoh Corporation "PStQuick A", "PStQuick B", "PStQuick E", "PStQuick F"
[0167] The epoxy equivalent of the synthesized epoxy resin was measured according to JIS K7236, and the epoxy equivalent (g / eq) was calculated.
[0168] The number of repeating units can be calculated, for example, from the results of GPC molecular weight measurement, or various appropriate instrumental analyses such as FD-MS and NMR.
[0169] Synthesis Example 1 151g (1.0 mol) of 4-hydroxyacetanilide, 300g of acetone, and 166g (1.2 mol) of potassium carbonate were charged in a flask equipped with a thermometer and a stirrer, and the temperature was raised to the reflux temperature. Then, 144g (1.2 mol) of allyl bromide was dropped and reacted for another 7 hours. The mixture was cooled to room temperature, the potassium carbonate was removed by filtration, and the acetone and excess allyl bromide in the filtrate were distilled off under reduced pressure using an evaporator. The obtained solid was dissolved in 222g of ethanol, 417g (4.0 mol) of 35% aqueous hydrochloric acid was dropped, and the mixture was reacted at 60 to 65°C for 12 hours. After cooling to room temperature, the mixture was neutralized with 880g (4.4 mol) of 20% aqueous sodium hydroxide solution, and separated three times with 373g of ethyl acetate. The organic layer was dehydrated with sodium sulfate, and then ethyl acetate was distilled off under reduced pressure using an evaporator to obtain 113 g (0.76 mol, yield 76%) of 4-allyloxyaniline.
[0170] [ka]
[0171] 82g (0.84 mol) of maleic anhydride was added to a flask equipped with a thermometer and a stirrer, and dissolved in 1590g of toluene and 9.0g of DMF. While keeping the temperature below 10°C in an ice bath, 113g (0.76 mol) of 4-allyloxyaniline dissolved in 150g of DMF was added dropwise, and the mixture was reacted at 25°C for 2 hours. Subsequently, 10g of 95% sulfuric acid was added, and the mixture was reacted at 110°C for 5 hours, after which the toluene was distilled off under reduced pressure. 1200g of ethyl acetate was added and separated three times, and then separated twice with a 2% aqueous sodium bicarbonate solution. The organic layer was dehydrated with sodium sulfate, and the ethyl acetate was distilled off under reduced pressure using an evaporator to obtain 150g (0.66 mol, yield 87%) of N-allyloxyphenylmaleimide.
[0172] [ka]
[0173] In a flask equipped with a thermometer and a stirrer, 150g (0.66 mol) of N-allyloxyphenylmaleimide and 3390g of dichloromethane were charged and dissolved. While keeping the temperature below 10℃ in an ice bath, 1200g of m-chlorobenzoic acid was added dropwise, and then the mixture was reacted at room temperature for 72 hours. After neutralization with 402g of saturated aqueous sodium hydrogen carbonate solution, 403g of saturated aqueous sodium sulfite solution was added dropwise. After removing the water layer, the mixture was separated three times with 2% aqueous sodium hydrogen carbonate solution and four times with water. After dehydrating the organic layer with sodium sulfate, dichloromethane was distilled off under reduced pressure using an evaporator to obtain 60g (0.24 mol, yield 37%) of a brown solid. The epoxy equivalent was 253g / eq. 1 H-NMR analysis confirmed that 4-glycidyloxyphenylmaleimide (M-1) was obtained. 1 H-NMR (DMSO-d6, 600MHz):2.72-2.87(m,2H),3.84-3.90(m,1H),4.36(dd,1H),4.39(dd,1H),7.16(s,2H),7.03-7.30(m,4H).
[0174] [ka]
[0175] Synthesis Example 2 In a flask equipped with a thermometer, a dropping funnel, a cooling tube and a stirrer, 38.8g (0.20 mol) of 9-anthrone was added to 180ml of dimethylacetamide to form a slurry while immersing it in an ice-water bath under a nitrogen atmosphere, and 110g (0.22 mol) of 8.09% aqueous sodium hydroxide solution was added thereto. Then, 27.7g (0.20 mol) of epibromohydrin dissolved in 40ml of dimethylacetamide was added dropwise. After stirring for 1 hour, the ice-water bath was removed, 70g of water was added, and the precipitated solid was filtered and dried under reduced pressure to obtain 23.6g of solid (yield 47%). 1 H-NMR analysis confirmed that 9-(2-glycidyloxy)anthracene (A-1) was obtained. The epoxy equivalent was 265 g / eq. 1 H-NMR (CDCl3, 600MHz): δ=2.79-2.96(m,2H),3.54-3.62(m,1H),4.17(dd,1H),4. 50(dd,1H),7.40-7.56(m,4H),7.94-8.05(m,2H),8.24(s,1H),8.30-8.42(m,2H).
[0176] [ka]
[0177] Synthesis Example 3 In a flask equipped with a thermometer, a dropping funnel, a condenser, and a stirrer, 18.8 g of 9-(4-hydroxybenzyl)-10-(4-hydroxyphenyl)anthracene (manufactured by Asahi Organic Chemicals Co., Ltd.: product name BIP-ANT: hydroxyl equivalent 188 g / eq) was charged and dissolved while purging with nitrogen gas. After heating to 65°C, the pressure was reduced to the pressure at which azeotropy occurred, and 7.35 g (0.09 mol) of 49% aqueous sodium hydroxide solution was added dropwise over 5 hours. Stirring was then continued for 0.5 hours under the same conditions. During this time, the distillate distilled by azeotropy was separated using a Dean-Stark trap, the aqueous layer was removed, and the oil layer was returned to the reaction system while the reaction was continued. Thereafter, unreacted epichlorohydrin was distilled off by reduced pressure distillation. The crude product thus obtained was dissolved in 150g of methyl isobutyl ketone and 150g of n-butanol. Furthermore, 10g of 10% aqueous sodium hydroxide solution was added to this solution and reacted at 80°C for 2 hours, after which washing with 50g of water was repeated three times until the pH of the washing liquid became neutral. Next, the system was dehydrated by azeotropy, and after passing through precision filtration, the solvent was distilled off under reduced pressure to obtain 22.0g of glycidyl group-containing anthracene compound (A-2). The epoxy equivalent was 257g / eq. In addition, the glycidyl group-containing anthracene compound (A-2) was measured by mass spectrometry, and a peak of M+=488 was obtained, which corresponds to the theoretical structure shown in the following structural formula. Therefore, it was confirmed that the glycidyl group-containing anthracene compound (A-2) contains the following structural formula.
[0178] [ka]
[0179] Synthesis Example 4 The same procedure as in Synthesis Example 3 was carried out except that 18.8 g of 9-(4-hydroxybenzyl)-10-(4-hydroxyphenyl)anthracene (manufactured by Asahi Organic Chemicals Co., Ltd.: product name BIP-ANT: hydroxyl group equivalent 188 g / eq) in Synthesis Example 3 was changed to 9.65 g of 2-aminoanthracene, and 12.2 g of a glycidyl group-containing anthracene compound (A-3) was obtained. The epoxy equivalent was 183 g / eq. In addition, the glycidyl group-containing anthracene compound (A-3) was measured by mass spectrometry, and a peak of M+=305 was obtained, which corresponds to the theoretical structure shown in the following structural formula. Therefore, it was confirmed that the glycidyl group-containing anthracene compound (A-3) contains the following structural formula.
[0180] [ka]
[0181] Example 1 In a flask equipped with a thermometer, a stirrer, and a condenser, 30.4 g (0.12 mol) of (M-1) obtained in Synthesis Example 1, 26.5 g (0.1 mol) of (A-1) obtained in Synthesis Example 2, 180 g of toluene, and 180 g of methyl isobutyl ketone were charged and reacted at 80°C for 12 hours. After that, the mixture was cooled to room temperature, and the precipitate was collected by suction filtration and dried under reduced pressure to obtain a glycidyl group-containing compound (D-1) which is a Diels-Alder reaction adduct. The epoxy equivalent was 337 g / eq, and the yield was 38.9 g, resulting in a 75% yield.
[0182] [ka]
[0183] Example 2 In a flask equipped with a thermometer, a stirrer, and a condenser, 30.4 g (0.12 mol) of (M-1) obtained in Synthesis Example 1, 51.4 g (0.1 mol) of (A-2) obtained in Synthesis Example 3, 200 g of toluene, and 200 g of methyl isobutyl ketone were charged and reacted at 80°C for 12 hours. After that, the mixture was cooled to room temperature, and the precipitate was collected by suction filtration and dried under reduced pressure to obtain a glycidyl group-containing compound (D-2) which is a Diels-Alder reaction adduct. The epoxy equivalent was 307 g / eq, and the yield was 61.4 g, resulting in a yield of 80%.
[0184] [ka]
[0185] Example 3 In a flask equipped with a thermometer, a stirrer, and a condenser, 30.4 g (0.12 mol) of (M-1) obtained in Synthesis Example 1, 15.4 g (0.1 mol) of furfuryl glycidyl ether (Merck reagent), 180 g of toluene, and 180 g of methyl isobutyl ketone were charged and reacted at 80°C for 12 hours. After that, the mixture was cooled to room temperature, and the precipitate was collected by suction filtration and dried under reduced pressure to obtain a mixture of glycidyl group-containing compounds (D-3) and (D'-3), which are Diels-Alder reaction adducts. The epoxy equivalent was 224 g / eq, the yield was 36.7 g, and the yield was 90%.
[0186] [ka]
[0187] Example 4 In a flask equipped with a thermometer, a stirrer, and a condenser, 30.4 g (0.12 mol) of (M-1) obtained in Synthesis Example 1, 36.6 g (0.1 mol) of (A-4) obtained in Synthesis Example 4, 200 g of toluene, and 200 g of methyl isobutyl ketone were charged and reacted at 80°C for 12 hours. After that, the mixture was cooled to room temperature, and the precipitate was collected by suction filtration and dried under reduced pressure to obtain a mixture of glycidyl group-containing compounds (D-4) and (D'-4), which are Diels-Alder reaction adducts. The epoxy equivalent was 210 g / eq, the yield was 57.0 g, and the yield was 85%.
[0188] [ka]
[0189] Comparative Example 1 In a flask equipped with a thermometer, stirrer, and cooling tube, 43.0g (0.12 mol) of BMI-1000 (4,4'-diphenylmethane bismaleimide manufactured by Daiwa Chemical Industry Co., Ltd.), 30.8g (0.2 mol) of furfuryl glycidyl ether (a reagent manufactured by Merck), 200g of toluene, and 200g of methyl isobutyl ketone were charged and reacted at 80°C for 12 hours. After that, the mixture was cooled to room temperature, and the precipitate was collected by suction filtration and dried under reduced pressure to obtain the Diels-Alder reaction adduct (D-5). The epoxy equivalent was 400g / eq, the yield was 40.0g, and the yield was 60%.
[0190] [ka]
[0191] Synthesis Example 5 A flask equipped with a thermometer and a stirrer was charged with 445g (0.5 mol) of polytetramethylene glycol diglycidyl ether (Nagase ChemteX "Denacol EX-991L": epoxy equivalent 445g / eq) and 171g (0.75 mol) of bisphenol A (hydroxyl equivalent 114g / eq), and the temperature was raised to 140°C over 30 minutes, after which 3.1g of 4% aqueous sodium hydroxide solution was added. The temperature was then raised to 150°C over 30 minutes, and the mixture was further reacted at 150°C for 16 hours. A neutralizing amount of sodium phosphate was then added to obtain 616g of a hydroxy compound represented by the following formula (Ph-1). The hydroxy compound was confirmed to contain a PTMG (polytetramethylene ether glycol) type (BPA: bisphenol A) hydroxy compound, since a peak of M+=1380 corresponding to the theoretical structure of m1=1 and n1=11 in the following formula was obtained in the mass spectrum. The hydroxyl equivalent of this hydroxy compound (Ph-1) calculated by GPC was 1080 g / eq, the average value of n1 was 10.6, and the average value of m1 was 0.76.
[0192] [ka]
[0193] Synthesis Example 6 In a flask equipped with a thermometer, a dropping funnel, a condenser and a stirrer, 200 g of the hydroxy compound (Ph-1) obtained in Synthesis Example 5, 437 g (4.72 mol) of epichlorohydrin and 118 g of n-butanol were added and dissolved while purging with nitrogen gas. After heating to 65°C, the pressure was reduced to an azeotropic pressure, and 6.66 g (0.08 mol) of a 49% aqueous sodium hydroxide solution was added dropwise over 5 hours. Next, stirring was continued for 0.5 hours under the same conditions. During this time, the distillate distilled by azeotropy was separated using a Dean-Stark trap, the water layer was removed, and the oil layer was returned to the reaction system while the reaction was continued. After that, the unreacted epichlorohydrin was distilled off by vacuum distillation. 150 g of methyl isobutyl ketone and 150 g of n-butanol were added to the obtained crude epoxy resin and dissolved. Further, 10 g of a 10% aqueous solution of sodium hydroxide was added to this solution, and the mixture was reacted at 80° C. for 2 hours, after which the mixture was washed three times with 50 g of water until the pH of the washing liquid became neutral. Next, the system was dehydrated by azeotropy, and after microfiltration, the solvent was distilled off under reduced pressure to obtain 190 g of epoxy resin (Ep-1). The epoxy equivalent of the obtained epoxy resin (Ep-1) was 1192 g / eq. The epoxy resin (Ep-1) was confirmed to contain a PTMG type (BPA) epoxy resin, since a peak of M+=1492 was obtained in the mass spectrum, which corresponds to the theoretical structure of m1=1, n1=11, q=1, p1=0, and p2=0 in the following formula.
[0194] [ka]
[0195] Preparation of composition and cured product 1 Each compound was melt-kneaded for 10 minutes at 100° C. using a two-roll mill according to the formulation in the table (the numbers in the table are by weight) to obtain a curable resin composition. This curable resin composition was press-molded at 180° C. for 60 minutes and then further cured at 180° C. for 5 hours to obtain a cured product having a thickness of 0.7 mm.
[0196] <Remolding test-1> The prepared cured product was freeze-pulverized. 0.07 g of the pulverized cured product was placed in a 10 mm square, 0.5 mm thick mold and vacuum pressed at 150°C for 3 hours. The appearance of the obtained cured product and the contamination of the pressed mirror surface were visually observed. The evaluation criteria were as follows:
[0197] Appearance of cured product A: The seams disappeared and the hardened material became one piece. B: Some of the seams are visible to the naked eye, but the hardened material has become one piece. C: It had a solidified shape and broke apart when light pressure was applied.
[0198] Contamination of the pressed mirror surface A: No contamination B: There is a small amount of contamination, but it can be removed. C: Contamination is present and cannot be removed without the use of a solvent
[0199] <Repair Test> The cured product was cut with a razor, the resulting fractured surfaces were brought into contact with each other, and then aged in a dryer at 150°C for 24 hours. After removing from the dryer, the cut surfaces of the cured products were visually inspected for adhesion. The criteria for evaluation were as follows: A: The bond does not come apart even when the cured product is bent 90 degrees. B: The material is bonded, and when the hardened material is bent, the bond comes apart. C: No bonding.
[0200] <Dismantling test> Each compound was used according to the formulation in the table (numbers in the table are based on mass), and melt-kneaded for 10 minutes at 100°C using two rolls to obtain a curable resin composition. This curable resin composition was evenly spread on one of two cold-rolled steel plates (TP Giken Co., Ltd. "SPCC-SD", 1.0mm x 25mm x 100mm) without any gaps, glass beads (Potters Ballotini Co., Ltd. "J-80") were added as spacers, and the other SPCC-SD was attached (adhesive area: 25mm x 12.5mm). This was heat-cured at 180°C for 60 minutes to obtain a test piece. This test piece was hung in a dryer at 120°C, and a load of 500g was applied to one side of the substrate. It was left to stand for 30 minutes in this state, and the adhesion state of the substrate was evaluated. The evaluation criteria are as follows. A: The adhesive part shifted, and the adhesive base material on the side to which the load was applied fell. B: The adhesive part became misaligned. C: No change occurred in the substrate.
[0201] Preparation of composition and cured product 2 Each compound was mixed according to the formula shown in the table (the numbers in the table are by mass), 2-ethyl-4-methyl-imidazole was added in an amount of 0.5 mass% based on the total mass of the epoxy resin and the curing agent, and the non-volatile content was adjusted to 58 mass% with methyl ethyl ketone to obtain a curable resin composition. Next, a glass cloth (2116 type, width 210 mm × length 280 mm × thickness 100 μm, manufactured by Nitto Boseki Co., Ltd.) was impregnated with the mixture, and then dried at 160°C for 2 minutes to volatilize the solvent, obtaining a prepreg. Six sheets of this prepreg were stacked and press molded at 200°C for 90 minutes to obtain a laminated cured product.
[0202] <Remolding test-2> The flat laminated cured product thus produced was placed in a mold with a depression in the center measuring 100 mm in width, 100 mm in length, and 10 mm in depth, and vacuum pressed at 180°C for 3 hours. The appearance of the resulting cured product was visually observed. The evaluation criteria were as follows:
[0203] Appearance of cured product A: A hardened product was obtained without cracks and molded exactly as in the mold. B: Some cracks were visible to the naked eye, but a cured product was obtained that was molded exactly as in the mold. C: Cracks occurred because the material could not keep up with the deformation.
[0204] [Table 1]
[0205] [Table 2]
[0206] EPICLON850-S: BPA-type liquid epoxy resin, epoxy equivalent 188g / eq DICY: Dicyandiamide DCMU: 3-(3,4-dichlorophenyl)-1,1-dimethylurea
[0207] [Table 3]
[0208] [Table 4]
[0209] TD2131: Phenol novolac resin, hydroxyl equivalent 104g / eq 2E4MZ: 2-ethyl-4-methyl-imidazole
Claims
1. A glycidyl group-containing compound represented by the following general formula: 【Chemistry 1】 [In the formula, R 1 is a glycidyl group or a substituent having one or more glycidyl groups, R 2 ~R 11 each independently represents a hydrogen atom, a halogen atom, a hydroxy group, a nitro group, a carboxy group, a cyano group, an alkoxy group, an aralkyloxy group, an aryloxy group, an amino group, an amido group, an alkyloxycarbonyl group, an aryloxycarbonyl group, an alkyl group, a cycloalkyl group, an aralkyl group, an aryl group, or a glycidyl group; The alkoxy group, aralkyloxy group, aryloxy group, amino group, amido group, alkyloxycarbonyl group, aryloxycarbonyl group, alkyl group, cycloalkyl group, aralkyl group, aryl group and glycidyl group may have a substituent on a carbon atom or a nitrogen atom. In the formulas (2) and (2′), R 2 ~R 11 At least one of the groups is a glycidyl group or a group having one or more glycidyl groups.
2. 2. The glycidyl group-containing compound according to claim 1, having an epoxy equivalent in the range of 100 to 500 g / eq.
3. 3. A curable resin composition comprising, as essential components, the glycidyl group-containing compound according to claim 1 and a compound (I) reactive with the glycidyl group-containing compound.
4. 4. The curable resin composition according to claim 3, wherein the compound (I) reactive with the glycidyl group-containing compound is a hydroxyl group-containing compound.
5. The curable resin composition according to claim 3, further comprising an epoxy resin having an epoxy equivalent of 100 to 10,000 g / eq other than the glycidyl group-containing compound according to any one of claims 1 and 2.
6. The curable resin composition according to claim 5, wherein the epoxy resin is represented by the following formula (3) and has an epoxy equivalent of 500 to 10,000 g / eq. 【Chemistry 2】 In formula (3), each Ar is independently a structure having an unsubstituted or substituted aromatic ring, X is a structural unit represented by the following formula (3-1), and Y is a structural unit represented by the following formula (3-2): 【Chemistry 3】 [In formulas (3-1) and (3-2), Ar is the same as defined above, R 21 , R 22 each independently represents a hydrogen atom, a methyl group, or an ethyl group, R' is a divalent hydrocarbon group having 2 to 12 carbon atoms; R 23 , R 24 , R 27 , R 28 each independently represents a hydroxyl group, a glycidyl ether group, or a 2-methylglycidyl ether group, R 25 , R 26 , R 29 , R 30 each independently represents a hydrogen atom or a methyl group, n 1 is an integer from 4 to 16, n 2 is the average value of the repeating units and is from 2 to 30. R 31 , R 32 each independently represents a glycidyl ether group or a 2-methylglycidyl ether group, R 33 , R 34 each independently represents a hydroxyl group, a glycidyl ether group, or a 2-methylglycidyl ether group, R 35 , R 36 is a hydrogen atom or a methyl group, m1, m2, p1, p2, and q are the average values of the repetitions, m1 and m2 each independently represent 0 to 25, and m1+m2≧1; p1 and p2 each independently represent 0 to 5; q is 0.5 to 5. However, the bond between the structural unit X represented by the formula (3-1) and the structural unit Y represented by the formula (3-2) may be random or block, and the total numbers of the structural units X and Y present in one molecule are m1 and m2, respectively.
7. The curable resin composition according to claim 3, wherein a concentration of the Diels-Alder reaction unit relative to the total mass of the curable components in the curable resin composition is 0.10 mmol / g or more.
8. The curable resin composition according to claim 3, which is a self-repairing composition, a remolding material composition or an easily dismantlable composition.
9. A cured product obtained by curing the curable resin composition according to claim 3.
10. A laminate comprising a substrate and a layer comprising the cured product according to claim 9.
11. A heat-resistant component comprising the cured product according to claim 9.
Citation Information
Patent Citations
Tung oil source imido glycidyl ester and preparation method and application thereof
CN109748907A
Epoxy resin monomer based on p-hydroxycinnamic acid as well as preparation method and application of epoxy resin monomer
CN112409298A
Adhesive composition and method of decomposing adhesion structure
JP2013256557A
Semiconductor device
JP2017041496A