Zirconia sintered body

By unevenly distributing vanadium group elements in the surface layer of the zirconia sintered body, the material achieves enhanced fracture toughness and reduced thermal expansion, addressing the trade-off between these properties.

JP7568234B2Active Publication Date: 2024-10-16K C M +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022124979
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-04
Publication Date
2024-10-16
Estimated Expiration
2042-08-04

AI Technical Summary

Technical Problem

The challenge lies in achieving a zirconia sintered body with high fracture toughness while suppressing its thermal expansion coefficient, as incorporating vanadium group elements typically increases thermal expansion, leading to potential cracking when used with materials like porcelain.

Method used

The zirconia sintered body is designed with vanadium group elements unevenly distributed in the surface layer, maintaining a higher concentration at the surface and lower concentration inside, enhancing stress-induced phase transformation and fracture toughness while minimizing thermal expansion.

Benefits of technology

This configuration results in a zirconia sintered body with improved fracture toughness and suppressed thermal expansion, suitable for applications where thermal stress is a concern, such as dental materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568234000001
    Figure 0007568234000001
  • Figure 0007568234000002
    Figure 0007568234000002
  • Figure 0007568234000003
    Figure 0007568234000003
Patent Text Reader

Abstract

To provide a zirconia sintered body that has excellent fracture toughness on at least a portion of a surface thereof and has a suppressed coefficient of thermal expansion.SOLUTION: The zirconia sintered body disclosed herein contains zirconia and a vanadium group element, and the vanadium group element is unevenly distributed in at least a portion of a surface layer. In one embodiment of the zirconia sintered body disclosed herein, a concentration of the vanadium group element at a surface of the surface layer where the vanadium group element is unevenly distributed is 1.5 times or more higher than a concentration of the vanadium group element in a portion of the surface in a depth direction with a lowest concentration of vanadium group element, or the vanadium group element is not contained in the portion with the lowest concentration of vanadium group element.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a zirconia sintered body. [Background technology]

[0002] Zirconia sintered bodies with a small amount of yttria (Y2O3) dissolved therein (hereinafter also referred to as "partially stabilized zirconia sintered bodies") are widely used as biomaterials such as dental materials (e.g., dentures, dental prostheses, denture mill blanks, and orthodontic brackets) due to their high strength, toughness, and aesthetics. For example, Patent Document 1 discloses a zirconia sintered body containing yttrium oxide and / or ytterbium oxide in a ratio of 3.5 mol% to 5.0 mol% and niobium oxide and / or tantalum oxide in a ratio of 0.3 mol% to 1.5 mol%. This zirconia sintered body has excellent fracture toughness, excellent translucency, and excellent hydrothermal degradation resistance.

[0003] Patent Documents 2 and 3 disclose techniques for distributing desired compounds with high uniformity in a zirconia workpiece, and Patent Document 4 discloses a technique for a zirconia workpiece with an adjusted porosity. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2021-229840 [Patent Document 2] International Publication No. 2018-155459 [Patent Document 3] JP 2021-165222 A [Patent Document 4] JP 2020-33338 A [Non-patent literature]

[0005] [Non-Patent Document 1] Journal of the American Ceramic Society, 1990, vol.73, No.1, p.115-120 Summary of the Invention [Problem to be solved by the invention]

[0006] Incidentally, the present inventors have been investigating the inclusion of vanadium group elements in zirconia sintered bodies to improve fracture toughness. However, when vanadium group elements are included in zirconia sintered bodies, the thermal expansion coefficient increases. In other words, the fracture toughness value and the thermal expansion coefficient are in a trade-off relationship, and it is difficult to achieve both. If the thermal expansion coefficient of the zirconia sintered body increases, for example, when a porcelain material is baked onto the surface of the zirconia sintered body (for example, when it is used as a dental material and colored), a difference in the thermal expansion coefficient occurs between the zirconia sintered body and the porcelain material, which may cause problems such as cracking.

[0007] Therefore, the present invention has been made in consideration of the above-mentioned circumstances, and its main object is to provide a zirconia sintered body having excellent fracture toughness and a reduced thermal expansion coefficient on at least a part of its surface. [Means for solving the problem]

[0008] The zirconia sintered body disclosed herein contains zirconia and a vanadium group element, and the vanadium group element is unevenly distributed at least in a part of the surface layer. This makes it easier for stress-induced phase transformation to occur in the surface layer of the zirconia sintered body, thereby improving the fracture toughness at the surface of the surface layer. In addition, when the zirconia sintered body contains a vanadium group element, the thermal expansion coefficient generally increases, but since the concentration of the vanadium group element is relatively low in the part other than the surface layer of the zirconia sintered body (for example, the inside of the zirconia sintered body), the increase in the thermal expansion coefficient can be suppressed. As a result, the fracture toughness is improved and the thermal expansion coefficient is suppressed in at least a part of the surface.

[0009] In a preferred embodiment of the zirconia sintered body disclosed herein, the concentration of the vanadium group element at the surface of the surface layer where the vanadium group element is unevenly distributed is 1.5 times or more higher than the concentration of the vanadium group element at the portion where the concentration of the vanadium group element is lowest in the depth direction of the surface, or the vanadium group element is not contained in the portion where the concentration of the vanadium group element is lowest, thereby achieving a higher level of improvement in fracture toughness and suppression of the thermal expansion coefficient.

[0010] In a preferred embodiment of the zirconia sintered body disclosed herein, the difference between the c / a axial length ratio of the tetragonal crystals at the surface of the surface layer where the vanadium group element is unevenly distributed, as obtained from an X-ray diffraction pattern, and the c / a axial length ratio of the tetragonal crystals at the portion in the depth direction of the surface layer where the concentration of the vanadium group element is the lowest, is 0.001 or more. This realizes a higher level of improvement in fracture toughness and suppression of the thermal expansion coefficient.

[0011] In one embodiment of the zirconia sintered body disclosed herein, the vanadium group element may include niobium (Nb).

[0012] In one embodiment of the zirconia sintered body disclosed herein, the zirconia sintered body may further contain yttrium oxide and / or ytterbium oxide as a stabilizer. In one embodiment of the zirconia sintered body disclosed herein, the concentration of the stabilizer may be 3 mol% or more and 6 mol% or less when the total of the zirconia and the stabilizer is 100 mol%.

[0013] In one embodiment of the zirconia sintered body disclosed herein, the fracture toughness value of at least a part of the surface of the surface layer in which the vanadium group element is unevenly distributed is 4.5 MPa√m or more, and the average linear expansion coefficient at 25°C to 500°C is 10 × 10 -6 / K or less. [Brief description of the drawings]

[0014] [Figure 1] 1 is a Nb mapping image (magnification: 100) of a cut surface of the zirconia sintered body of Example 1. [Diagram 2] 1 is a Nb mapping image (magnification: 100) of a cut surface of the zirconia sintered body of Reference Example 1. [Diagram 3] 1 is a graph showing the Nb2O5 concentration distribution of a zirconia sintered body based on elemental mapping. [Figure 4] 1 is a graph showing the Nb2O5 concentration distribution of a zirconia sintered body based on total element quantitative analysis. [Diagram 5] 1 is a graph showing the c / a axis length ratio of tetragonal crystals in a cut surface of the zirconia sintered body of Example 1. [Figure 6] 1 is a graph showing fracture toughness values ​​in each example. [Figure 7] 1 is a graph showing the average linear expansion coefficient in each example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the technology disclosed herein will be described. Matters other than those specifically mentioned in this specification and necessary for implementation can be understood based on the technical content taught by this specification and the general technical common sense of a person skilled in the art in the relevant field. The contents of the technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense of a person skilled in the art in the relevant field. In this specification, when a numerical range is described as "A to B (where A and B are arbitrary numerical values)", it means "A or more and B or less", and also includes the meanings of "more than A and less than B", "more than A and B or less", and "more than A and less than B".

[0016] The zirconia sintered body disclosed herein contains at least zirconia (ZrO2) and a vanadium group element. The zirconia sintered body may further contain a stabilizer. The zirconia sintered body contains zirconia as a main component. Here, "containing zirconia as a main component" means that zirconia accounts for the largest proportion of the compounds constituting the zirconia sintered body. When the entire zirconia sintered body is taken as 100 mass%, the proportion of zirconia is, for example, 70 mass% or more, preferably 80 mass% or more, and more preferably 90 mass% or more. A high proportion of zirconia can improve the strength, toughness, etc. of the zirconia sintered body.

[0017] Examples of vanadium group elements include vanadium (V), niobium (Nb), and tantalum (Ta). The zirconia sintered body contains at least one of V, Nb, and Ta. The vanadium group elements are contained in the zirconia sintered body as oxides, for example. Examples of oxides containing vanadium group elements include X2O5 (X represents a vanadium group element). According to Non-Patent Document 1, vanadium group elements dissolve in zirconia and increase the c / a axial length ratio (tetragonality) of the tetragonal crystal of the zirconia sintered body (i.e., distort the crystal). This makes it easier for stress-induced phase transformation (phase transformation from tetragonal to monoclinic) to occur, and the fracture toughness value of the zirconia sintered body can be improved.

[0018] In the zirconia sintered body disclosed herein, the vanadium group element is unevenly distributed at least in a part of the surface layer of the zirconia sintered body. When the surface area of ​​the zirconia sintered body is taken as 100%, the vanadium group element may be unevenly distributed (present) in the surface layer in a range of, for example, 2% or more of the surface area, or the vanadium group element may be unevenly distributed in the surface layer in a range of 5% or more, 10% or more, 20% or more, 30% or more, 50% or more, 70% or more, 90% or more, or 100% (i.e., the entire surface of the zirconia sintered body). This makes it easier for stress-induced phase transformation to occur in the surface layer (including the surface) of the zirconia sintered body where the vanadium group element is unevenly distributed, and the fracture toughness value of the surface of the zirconia sintered body can be improved. In addition, with this configuration, the concentration of the vanadium group element is relatively low in the portion other than the surface layer of the zirconia sintered body (for example, the inner side of the surface layer of the zirconia sintered body), so that it is possible to suppress the increase in the thermal expansion coefficient that may occur with the increase in the concentration of the vanadium group element. As a result, it is presumed that the surface layer of the zirconia sintered body in which the vanadium group element is unevenly distributed exhibits excellent fracture toughness, and the increase in the thermal expansion coefficient can be suppressed inside the zirconia sintered body, thereby improving the fracture toughness and suppressing the thermal expansion coefficient. Note that this mechanism is presumed and does not limit the present technology in any way.

[0019] In the zirconia sintered body disclosed herein, the vanadium group element concentration in the surface layer where the vanadium group element is unevenly distributed is higher than the vanadium group element concentration in the part of the surface where the vanadium group element concentration is the lowest in the depth direction, and may be, for example, 1.5 times or more, 2 times or more, 5 times or more, 10 times or more, 20 times or more, or 30 times or more higher. In the part where the vanadium group element concentration is the lowest, the vanadium group element concentration may be 0 mol% (i.e., no vanadium group element is contained). This realizes a zirconia sintered body having better fracture toughness and a reduced thermal expansion coefficient. In this specification, the "depth direction" refers to the direction from the contact point between the plane in contact with the surface of the zirconia sintered body and the surface toward the inside of the zirconia sintered body so as to be perpendicular to the plane.

[0020] The vanadium group element concentration in the surface layer of the zirconia sintered body where the vanadium group element is unevenly distributed is, for example, 0.1 mol% or more, preferably 0.3 mol% or more, more preferably 0.5 mol% or more, even more preferably 0.7 mol% or more, and particularly preferably 0.9 mol% or more, calculated as X2O5 (X indicates a vanadium group element). The high concentration of the vanadium group element tends to increase the tetragonality of the zirconia sintered body (i.e., the c / a axis length ratio of the tetragonal crystal increases). This makes it easier for a phase transformation accompanied by a volume change to occur when stress is applied to the surface of the zirconia sintered body, and the fracture toughness value can be further increased. In addition, although not particularly limited, the vanadium group element concentration in the surface of the zirconia sintered body can be, for example, 10 mol% or less, 5 mol% or less, 3 mol% or less, or 2 mol% or less, calculated as X2O5 (X indicates a vanadium group element). The concentration of vanadium group elements in the zirconia sintered body can be measured by scanning electron microscope-wavelength dispersive X-ray spectroscopy (SEM-WDX).

[0021] The concentration of the vanadium group element in the portion where the concentration of the vanadium group element is lowest in the depth direction from the surface of the zirconia sintered body (typically, near the center inside the zirconia sintered body) is, for example, less than 0.1 mol%, and may be 0.05 mol% or less, 0.03 mol% or less, 0.01 mol% or less, or 0 mol% (i.e., no vanadium group element is included) in terms of X2O5 (X represents a vanadium group element). By having a low concentration of the vanadium group element or no vanadium group element included on the inside side of the zirconia sintered body, an increase in the thermal expansion coefficient can be suppressed.

[0022] In the zirconia sintered body, when the region from the surface of the surface layer where the vanadium group elements are unevenly distributed to the part where the concentration of the vanadium group elements in the depth direction of the surface is the lowest is divided into two regions, a surface region and an inner region, the concentration of the vanadium group elements in the surface region is higher than the concentration of the vanadium group elements in the inner region. For example, the concentration of the vanadium group elements in the surface region of the zirconia sintered body may be 1.5 times or more higher than the concentration of the vanadium group elements in the inner region of the zirconia sintered body, or may be 2 times or more, 5 times or more, 10 times or more, 20 times or more, or 30 times or more higher. In addition, the inner region may not contain vanadium group elements. This realizes a zirconia sintered body having better fracture toughness and a reduced thermal expansion coefficient.

[0023] The "surface region" refers to a region closer to the surface than the midpoint of the distance from the surface of the zirconia sintered body where the vanadium group elements are unevenly distributed to the portion in the depth direction of the surface where the concentration of the vanadium group elements is the lowest. The "inner region" refers to a region farther from the surface than the midpoint of the distance from the surface of the zirconia sintered body to the portion in the depth direction of the surface where the concentration of the vanadium group elements is the lowest.

[0024] The c / a axial length ratio of the tetragonal crystals at the surface of the surface layer where the vanadium group elements are unevenly distributed in the zirconia sintered body (hereinafter also referred to as "tetragonality A") may be higher than the c / a axial length ratio of the tetragonal crystals at the part where the concentration of the vanadium group elements in the depth direction of the surface is the lowest (hereinafter also referred to as "tetragonality B"). The difference between the tetragonality A and the tetragonality B (where A>B) may be, for example, 0.001 or more, 0.00125 or more, 0.0015 or more, or 0.00175 or more. The higher the tetragonality value, the more likely the phase transformation to monoclinic occurs when stress is applied, and the fracture toughness value can be improved. On the other hand, the thermal expansion coefficient can be increased by the high tetragonality value. Therefore, by making the difference between the tetragonality A and the tetragonality B large as described above, it is possible to realize the improvement of the fracture toughness in the surface layer part of the zirconia sintered body and the suppression of the increase in the thermal expansion coefficient. The "tetragonal c / a axis length ratio" can be measured by using the integrated powder X-ray analysis software PDXL2 (manufactured by Rigaku Software Corporation) to measure the profile of the X-ray diffraction pattern in the cross section of the zirconia sintered body. In one example of a specific analysis method, the software first automatically determines the peak position from the explanatory profile. Next, the c / a axis length ratio is calculated from the lattice constant (d value) of the (004) plane corresponding to the c axis with a diffraction angle (2θ) of approximately 73°, and the d value of the (400) plane corresponding to the a axis with a 2θ of approximately 74.5°. In this way, the c / a axis length ratio of the tetragonal crystal can be obtained.

[0025] The value of tetragonality A is not particularly limited, but may be 1.0165 or more, 1.0170 or more, 1.0175 or more, or 1.018 or more. The higher the tetragonality, the easier it is for phase transformation to monoclinic to occur when stress is applied, and the fracture toughness value can be improved. In addition, the value of tetragonality A is not particularly limited, but may be, for example, 1.02 or less, 1.019 or less, or 1.0185 or less.

[0026] The value of tetragonality B is not particularly limited, but may be, for example, 1.012 or more, 1.013 or more, or 1.014 or more. Also, the value of tetragonality B is not particularly limited, but may be, for example, less than 1.017, or 1.0168 or less. By keeping the tetragonality B within the above range, the increase in the thermal expansion coefficient can be suppressed.

[0027] Examples of stabilizers that can be included in the zirconia sintered body include oxides containing rare earth elements such as yttrium oxide (Y2O3), ytterbium oxide (Yb2O3), cerium oxide (Ce2O3), and erbium oxide (Er2O3), oxides containing alkaline earth metal elements such as calcium oxide (CaO) and magnesium oxide (MgO), and oxides containing other transition metal elements. Among these, yttrium oxide and ytterbium oxide are preferably used. By including yttrium oxide and / or ytterbium oxide, the proportion of tetragonal crystals in the zirconia sintered body can be increased, and the fracture toughness value and strength can be improved. The stabilizer may be included alone or in combination with two or more kinds. In addition, all of the stabilizers may be solid-dissolved in zirconia, or an undissolved stabilizer that is not solid-dissolved in zirconia may be included.

[0028] The concentration of the stabilizer is not particularly limited, but may be, for example, 1.5 mol% or more, 2 mol% or more, 2.5 mol% or more, or 3 mol% or more, when the total of zirconia and the stabilizer is 100 mol%. The concentration of the stabilizer may be, for example, 6 mol% or less, 5 mol% or less, 4.5 mol% or less, 4.2 mol% or less, or 3.5 mol% or less. In addition, when yttrium oxide and / or ytterbium oxide are contained as the stabilizer, the above-mentioned concentration range of the stabilizer is particularly preferably adopted.

[0029] The zirconia sintered body may further contain aluminum oxide (Al2O3). Aluminum oxide can lower the firing temperature for producing the zirconia sintered body. In addition, in the zirconia sintered body containing alumina, abnormal grain growth is suppressed, so that the strength and translucency of the zirconia sintered body can be improved. In addition, the low-temperature deterioration resistance can be improved, so that the strength and translucency of the zirconia sintered body can be maintained for a long period of time. On the other hand, since alumina remains as an impurity inside the sintered body and acts as a light scattering factor, it is better that the alumina content is not too high. Therefore, when the entire zirconia sintered body is taken as 100 mass%, the alumina content may be, for example, 0.30 mass% or less, and may be 0.15 mass% or less, 0.1 mass% or less, or 0.05 mass% or less.

[0030] The zirconia sintered body may contain a conventionally known coloring agent within a range in which the effect of the technology disclosed herein is not significantly impaired. Examples of the coloring agent include transition metal elements and lanthanoid rare earth elements. Examples of such elements include iron, nickel, cobalt, manganese, praseodymium, neodymium, europium, gadolinium, erbium, etc. The coloring agent may be, for example, 5% by mass or less, 1% by mass or less, or 0.5% by mass or less, based on the entire zirconia sintered body.

[0031] In addition, the zirconia sintered body may contain elements that may be inevitably mixed in. For example, hafnium, silicon, titanium, etc. The total content of these elements is preferably 2.5 mass% or less, more preferably 2 mass% or less, for example 1.8 mass% or less, calculated as oxide, based on the entire zirconia sintered body.

[0032] The shape of the zirconia sintered body is not particularly limited, and may be, for example, a columnar shape such as a disk shape, a cylindrical shape, or a rectangular column shape; a polyhedral shape such as a rectangular parallelepiped shape, a cube shape, or a polygonal shape; a spherical shape, a rugby ball shape, or an irregular shape, etc. The zirconia sintered body may be in a shape as a dental material, for example, a denture such as a front tooth denture or a back tooth denture, a denture mill blank, an orthodontic bracket, a dental prosthesis, a bridge, a crown, etc.

[0033] The shortest distance from the surface of the surface layer of the zirconia sintered body where the vanadium group elements are unevenly distributed to the part in the depth direction of the surface where the concentration of the vanadium group elements is the lowest is not particularly limited, but is preferably 1.5 mm or more, and may be 2 mm or more, 2.5 mm or more, or 3 mm or more. This makes it possible to improve the fracture toughness of the surface layer of the zirconia sintered body and suppress an increase in the thermal expansion coefficient.

[0034] The fracture toughness value of at least a part of the surface of the surface layer where the vanadium group elements of the zirconia sintered body are unevenly distributed is, for example, 4.5 MPa√m or more, and may be 6 MPa√m or more, 9 MPa√m or more, 10 MPa√m or more, 11 MPa√m or more, or 12 MPa√m or more. In this specification, the "fracture toughness value" refers to a value measured in accordance with the IF method specified in JIS R 1607:2015.

[0035] In this specification, the thermal expansion coefficient of the zirconia sintered body is evaluated using as an index the average linear expansion coefficient at 25°C to 500°C measured in accordance with JIS R 1618. The average linear expansion coefficient of the zirconia sintered body at 25°C to 500°C is, for example, 10 × 10 -6 / K or less, 9.9×10 -6 / K or less, or 9.8×10 -6 / K or less.

[0036] The zirconia sintered body disclosed herein may roughly include a molding step, a calcination step, a vanadium group element providing step, a drying step, and a firing step. Note that the manufacturing process including these steps is an example of manufacturing the zirconia sintered body disclosed herein, and does not limit the manufacturing method of the zirconia sintered body disclosed herein. In addition, these steps may be omitted as necessary, and other steps may be included in an appropriate order.

[0037] In the molding step, first, a raw material powder of the zirconia sintered body disclosed herein is prepared. At least zirconia powder is prepared as the raw material powder. The zirconia powder may be appropriately changed depending on the composition of the zirconia sintered body to be manufactured, and may be, for example, a partially stabilized zirconia powder containing a stabilizer in a ratio that can be contained in the above-mentioned zirconia sintered body. In addition, aluminum oxide powder may be mixed with the zirconia powder so that it is in a ratio that can be contained in the above-mentioned zirconia sintered body. The raw material powder may be used as it is in powder form, or may be prepared into granules by spray drying or the like before use.

[0038] Next, the prepared raw material powder is molded to obtain a molded body. The molding method is not particularly limited, and for example, pressure molding, injection molding, extrusion molding, casting molding, etc. can be adopted. As the pressure molding, for example, cold isostatic pressing (CIP), hot isostatic pressing (HIP), etc. are preferably adopted. According to CIP or HIP, a high density molded body can be produced, and therefore the fracture toughness value can be further improved.

[0039] In the calcination step, the molded body is heated to calcinate it to obtain a calcined body. By such heating, it is possible to remove components such as moisture and impurities that may be contained in the molded body. In addition, by calcination, it is possible to reduce voids that may exist in the treated body, and therefore it is possible to suitably prevent cracks that may occur during sintering due to high temperature and high speed heating. Calcination can be performed at a heating temperature of, for example, 800°C to 1200°C, preferably 900°C to 1100°C. The heating time may vary depending on the shape, size, composition, etc. of the treated body, and may be appropriately adjusted, but may be, for example, 0.5 hours to 5 hours. Heating of the treated body can be performed by a known method, and for example, a heating device such as a muffle furnace, an electric furnace, or a microwave furnace can be used.

[0040] In the vanadium group element providing step, vanadium group elements are provided to the vanadium group element-containing material presintered body. The vanadium group element-containing material may be, for example, a solution, a sol, etc., and is particularly preferably a sol. Examples of the solution include a chloride solution of a vanadium group element, a metal alkoxide solution, etc. When the vanadium group element-containing material is a sol, it is preferable that particles containing the vanadium group element are dispersed in a dispersion medium. Examples of the particles include oxides containing vanadium group elements. Specific examples of such oxides include V2O5, Nb2O5, Ta2O5, etc. The dispersion medium is not particularly limited, but may be, for example, water, an organic solvent, etc. In the sol, the ratio of particles containing vanadium group elements to the entire sol (sol concentration) is not particularly limited, but may be, for example, 1% by mass to 10% by mass, preferably about 5% by mass to 10% by mass. If the sol concentration (proportion of particles) is too low, the vanadium group element will not be sufficiently arranged on the surface of the pre-sintered body, and when a zirconia sintered body is produced, the improvement in fracture toughness may be insufficient.

[0041] Methods for applying the vanadium group element material to the presintered body include, for example, impregnating a part or the whole of the presintered body with the vanadium group element-containing material, and coating the surface of the presintered body with the vanadium group element-containing material.

[0042] When the pre-sintered body is impregnated with the vanadium group element-containing material, the impregnation time can be appropriately changed depending on the shape and size of the pre-sintered body, and can be, for example, about 0.1 to 48 hours, preferably about 4 to 24 hours.

[0043] The drying step is a step of drying the provisionally sintered body after the vanadium group element providing step, and removing liquid components (e.g., dispersion medium) and the like contained in the vanadium group element-containing material. The drying method is not particularly limited, and may be appropriately selected from natural drying, air drying, hot air drying, drying by heating using a heating furnace or the like, vacuum drying, suction drying, freeze drying, and the like. In one example of drying by heating, drying may be performed under conditions of 80°C to 150°C for about 0.5 hours to 20 hours. The drying step is not an essential step, and may be omitted as appropriate.

[0044] In the firing step, the provisionally sintered body is fired to obtain a zirconia sintered body. The firing method can be performed by a known method, and for example, firing can be performed using a heating device such as a muffle furnace, an electric furnace, or a microwave furnace. The firing temperature is not particularly limited, and may be, for example, 1300°C to 1600°C, or 1400°C to 1500°C. The retention time after reaching the firing temperature may be, for example, 1 hour to 5 hours, or 1.5 hours to 3 hours.

[0045] The zirconia sintered body disclosed herein can be used in various applications in which zirconia sintered bodies have conventionally been used, and can be suitably used, for example, as structural members, dental materials, etc. Examples of dental materials include dentures such as front teeth dentures and back teeth dentures, denture mill blanks, orthodontic brackets, dental prostheses, bridges, crowns, etc.

[0046] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A zirconia sintered body comprising zirconia and a vanadium group element, the vanadium group element being unevenly distributed in at least a portion of a surface layer. Item 2: A zirconia sintered body according to Item 1, wherein the concentration of the vanadium group element at the surface of a surface layer in which the vanadium group element is unevenly distributed is 1.5 times or more higher than the concentration of the vanadium group element at a portion in the depth direction of the surface in which the concentration of the vanadium group element is lowest; or the vanadium group element is not contained in the portion in which the concentration of the vanadium group element is lowest. Item 3: A zirconia sintered body according to Item 1 or 2, wherein the difference between the c / a axial length ratio of tetragonal crystals at the surface of the surface layer in which the vanadium group element is unevenly distributed, obtained from an X-ray diffraction pattern, and the c / a axial length ratio of tetragonal crystals at a portion in the depth direction of the surface layer in which the concentration of the vanadium group element is lowest, is 0.001 or more. Item 4: The zirconia sintered body according to any one of Items 1 to 3, containing niobium (Nb) as the vanadium group element. Item 5: The zirconia sintered body according to any one of Items 1 to 4, further comprising yttrium oxide and / or ytterbium oxide as a stabilizer. Item 6: The zirconia sintered body according to Item 5, wherein the concentration of the stabilizer is 3 mol% or more and 6 mol% or less when the total amount of the zirconia and the stabilizer is 100 mol%. Item 7: The fracture toughness value of at least a part of the surface of the surface layer in which the vanadium group element is unevenly distributed is 4.5 MPa√m or more, and the average linear expansion coefficient at 25 ° C to 500 ° C is 10 × 10 -6 7. The zirconia sintered body according to any one of items 1 to 6, wherein the zirconia sintered body has a viscosity of 1000:1 or less.

[0047] Hereinafter, examples of the technology disclosed herein will be described, but such examples are not intended to limit the technology disclosed herein.

[0048] <Test 1> In Test 1, the Nb distribution and c / a axial length ratio (tetragonality) in the zirconia sintered body were analyzed.

[0049] Example 1 Zirconia powder (manufactured by Kyoritsu Material Co., Ltd.) containing 3 mol% yttrium oxide (Y2O3) was prepared. 15 g of this powder was filled into a mold with a bottom surface of 50 mm in length and 15 mm in width, and then premolded at a pressure of 20 MPa to produce a premolded body. After removing the premolded body from the mold, CIP molding was performed on the premolded body at a pressure of 196 MPa to produce a molded body. The molded body was a rectangular parallelepiped with a length of 50 mm, a width of 14 mm, and a height of 6.8 mm. This molded body was calcined at 1000°C for 30 minutes to obtain a calcined body. The calcined body was impregnated with Nb2O5 sol (manufactured by Taki Chemical Co., Ltd., product number: Nb-G6000, sol concentration: 6 mass%) for 24 hours, and then dried at 120°C for 16 hours. After drying, it was fired at 1450°C for 2 hours to obtain the zirconia sintered body of Example 1. The sintered body was a rectangular parallelepiped with a length of 40 mm, a width of 11.5 mm and a height of 5.6 mm.

[0050] (Reference example 1) Zirconia powder (manufactured by Kyoritsu Material Co., Ltd.) containing 3 mol% yttrium oxide (Y2O3) was mixed with Nb2O5 powder so that the Nb2O5 powder was 1 mol% of the total powder to prepare a raw material powder. 15 g of the raw material powder was filled into a metal mold with a bottom surface of 50 mm in length and 15 mm in width, and then a pressure of 20 MPa was applied to perform preforming to produce a preform. After removing the preform from the metal mold, CIP molding was performed on the preform at a pressure of 196 MPa to produce a molded body. The molded body was a rectangular parallelepiped with a length of 50 mm, a width of 14 mm, and a height of 6.8 mm. The molded body was calcined at 1000°C for 30 minutes to obtain a calcined body. The calcined body was fired at 1450°C for 2 hours to obtain the zirconia sintered body of Reference Example 1. The sintered body was a rectangular parallelepiped with a length of 40 mm, a width of 11.5 mm, and a height of 5.6 mm.

[0051] (Analysis of Nb concentration distribution) The zirconia sintered body was cut perpendicularly to the long side direction (40 mm side direction) to prepare a test piece having a cut surface (11.5 mm x 5.6 mm) at the midpoint of the long side. After mirror finishing of the cut surface, the cut surface was analyzed by scanning electron microscope-wavelength dispersive X-ray spectroscopy (SEM-WDX). For SEM-WDX, JXA-iHP200F Hyper Probe manufactured by JEOL Ltd. was used as an electron probe microanalyzer (EPMA). Two methods were used to measure the Nb concentration distribution: a method using the results of Nb characteristic X-ray intensity of element mapping image and a method using the results of total element quantitative analysis.

[0052] Elemental mapping was performed using a Nb WDS detector PET, accelerating voltage: 15.0 kV, and irradiation current: 5.0 × 10 -8 A, collection time: 10 ms, pixel size: 0.025 μm (magnification: 10000), 2.5 μm (magnification: 100). Element mapping was performed along the short side direction of the cut surface so as to pass through the center of the cut surface. A mapping image of Nb in Example 1 (magnification: 100) is shown in FIG. 1. A mapping image of Nb in Reference Example 1 (magnification: 100) is shown in FIG. 2. In the mapping image of Nb, a relatively bright part (a part relatively close to white) indicates a high Nb concentration, and a relatively dark part (a part relatively close to black) indicates a low Nb concentration. The Nb2O5 concentration of the zirconia sintered body in Example 1 was calculated by subtracting the background from the average value of the characteristic X-ray intensity of Nb in Reference Example 1 to 1 mol% Nb2O5. Specifically, a number line was drawn in the direction of the short side of the cut surface (the vertical direction in Figure 1) with the center of the cut surface as the origin (0 mm), and the Nb2O5 concentrations were calculated at positions 0 mm, ±0.5 mm, ±1.5 mm, ±2.5 mm, and ±2.7 mm, with the upward direction of the mapping image being the positive direction and the downward direction being the negative direction. The results are shown in Figure 3.

[0053] For quantitative analysis of all elements, the detector was a Nb WDS detector PET, the accelerating voltage was 15.0 kV, and the probe current was 5.0 × 10 -8A, collection time: 500 ms. Total element quantitative analysis was performed from the midpoint of one of the long sides (11.5 mm side) of the cut surface toward the center of the cut surface (in the depth direction). The Nb concentration measured on the cut surface of the test piece of Reference Example 1 was converted to Nb2O5 concentration, and the average concentration was set to 1 mol%. The Nb concentration on the cut surface of the test piece of Example 1 was converted to Nb2O5 concentration and standardized using the results of Reference Example 1. The results are shown in FIG. 4. In the graph shown in FIG. 4, the horizontal axis indicates the distance (depth) from the surface in the short side direction of the cut surface, and the vertical axis indicates the Nb2O5 concentration.

[0054] (Measurement of c / a axial length ratio) An X-ray diffraction pattern profile was obtained for the cut surface of the test piece of Example 1 using an X-ray diffraction device (device name: Ultima IV, manufactured by Rigaku Corporation). The X-ray diffraction pattern profile was used to measure the c / a axis length ratio of the tetragonal crystals using integrated powder X-ray analysis software: PDXL2 (manufactured by Rigaku Software Corporation). The results are shown in FIG. 5. The horizontal axis of the graph in FIG. 5 indicates the distance from the surface in the short side direction of the cut surface, and the vertical axis indicates the c / a axis length ratio of the tetragonal crystals. The measurement conditions for X-ray diffraction (XRD) are as follows: X-ray detector: D / tex Ultra (accessory device) Scan speed: 0.4° / min Sampling width: 0.02° Divergence slit: 1.0mm Divergence vertical slit: 10mm Scattering slit: 8mm Receiving slit: open Voltage: 40kV ·Current: 40mA ·Measurement area: 72~76°

[0055] (Evaluation of Test 1) As shown in Figures 1, 3, and 4, in Example 1, Nb was hardly detected in the inner part of the zirconia sintered body, and Nb was found to be unevenly distributed in the surface layer. In addition, as shown in Figure 5, it is found that the c / a axis length ratio of the tetragonal crystal is large on the surface where Nb is unevenly distributed. On the other hand, as shown in Figures 2 to 4, it is found that Nb is almost evenly distributed in the zirconia sintered body in Reference Example 1.

[0056] <Test 2> In Test 2, the fracture toughness and the average linear expansion coefficient were evaluated.

[0057] Example 2 Zirconia powder (manufactured by Kyoritsu Material Co., Ltd.) containing 3 mol% Y2O3 was prepared. After filling about 1.5 g of this powder into a die with a diameter of 7 mm, it was premolded at a pressure of 0.78 MPa to produce a premolded body. After removing the premolded body from the die, it was subjected to CIP molding at a pressure of 196 MPa to produce a molded body. This molded body was calcined at 1000°C for 30 minutes to obtain a calcined body. This calcined body was impregnated with Nb2O5 sol (manufactured by Taki Chemical Co., Ltd., product number: Nb-G6000, sol concentration: 6 mass%) for 4.5 hours, and then dried at 120°C for 16 hours. After drying, it was fired at 1450°C for 2 hours to obtain a zirconia sintered body of Example 2. The sintered body was a cylinder with a diameter of 5.5 mm and a height of 10 mm.

[0058] Example 3 A zirconia sintered body of Example 3 was obtained in the same manner as in Example 2, except that the Y2O3 concentration was changed from 3 mol% to 4.2 mol%.

[0059] (Reference example 2) Zirconia powder (manufactured by Kyoritsu Material Co., Ltd.) containing 3 mol% yttrium oxide (Y2O3) was mixed with Nb2O5 powder so that the Nb2O5 powder was 1 mol% of the total powder to prepare a raw material powder. After filling about 1.5 g of this powder into a die with a diameter of 7 mm, premolding was performed at a pressure of 0.78 MPa to prepare a premolded body. After removing the premolded body from the die, CIP molding was performed on the premolded body at a pressure of 196 MPa to prepare a molded body. This molded body was calcined at 1000°C for 30 minutes to obtain a calcined body. This calcined body was fired at 1450°C for 2 hours to obtain a zirconia sintered body of Reference Example 2. The sintered body was a cylinder with a diameter of 5.5 mm and a height of 10 mm.

[0060] (Reference example 3) The zirconia sintered body of Reference Example 3 was obtained in the same manner as in the manufacturing method of the zirconia sintered body of Reference Example 2, except that the Y2O3 concentration was changed from 3 mol% to 4.2 mol%.

[0061] Comparative Example 1 The zirconia sintered body of Comparative Example 1 was obtained in the same manner as in the manufacturing method of the zirconia sintered body of Reference Example 2, except that the Nb2O5 powder was not mixed.

[0062] Comparative Example 2 The zirconia sintered body of Comparative Example 2 was obtained in the same manner as in the manufacturing method of the zirconia sintered body of Reference Example 3, except that the Nb2O5 powder was not mixed.

[0063] (Measurement of fracture toughness value) The surface of the zirconia sintered body was mirror-polished to a depth of approximately 0.05 mm, and the fracture toughness value of this surface was measured. The measurement was performed in accordance with the IF method of JIS R 1607:2015. The indentation load of the Vickers indenter was 10 kgf (approximately 98 N), and the indentation holding time of the Vickers indenter was 30 seconds. The results are shown in Figure 6.

[0064] (Measurement of average linear expansion coefficient) The average linear expansion coefficient was measured at 25°C to 500°C using a thermomechanical analyzer (manufactured by NETZSCH, product name: TMA4000SA). The measurement was performed in accordance with JIS R 1618. The load was 20 g, the heating rate was 5 K / min, and the measurement atmosphere was air. The results are shown in FIG.

[0065] (Evaluation of Test 2) As shown in Fig. 6, the zirconia sintered bodies of Examples 2 and 3 and Reference Examples 2 and 3 containing Nb2O5 had higher fracture toughness values ​​than Comparative Examples 1 and 2 not containing Nb2O5. On the other hand, as shown in Fig. 7, the average linear expansion coefficients of Reference Examples 2 and 3 were larger than those of Comparative Examples 1 and 2, whereas the increase in the average linear expansion coefficient was suppressed in Examples 2 and 3. Therefore, it can be seen that the uneven distribution of Nb in the surface layer of the zirconia sintered body realizes fracture toughness equivalent to that of a zirconia sintered body in which Nb is distributed almost uniformly, and also realizes a thermal expansion coefficient equivalent to that of a zirconia sintered body not containing Nb.

[0066] Although specific examples of the technology disclosed herein have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.

Claims

1. Contains zirconia and a vanadium group element, The vanadium group element is unevenly distributed in at least a part of the surface layer, the vanadium group element is niobium (Nb); A zirconia sintered body having an average linear expansion coefficient of 9.9×10 −6 / K or less at 25° C. to 500° C.

2. 2. The zirconia sintered body according to claim 1, wherein the concentration of the vanadium group element at the surface of the surface layer in which the vanadium group element is unevenly distributed is 1.5 times or more higher than the concentration of the vanadium group element in a portion in the depth direction of the surface in which the concentration of the vanadium group element is the lowest, or the vanadium group element is not contained in the portion in which the concentration of the vanadium group element is the lowest.

3. 2. The zirconia sintered body according to claim 1, wherein a difference between a c / a axial length ratio of tetragonal crystals at the surface of a surface layer in which the vanadium group element is unevenly distributed, obtained from an X-ray diffraction pattern, and a c / a axial length ratio of tetragonal crystals at a portion in the depth direction of the surface in which the concentration of the vanadium group element is lowest, is 0.001 or more.

4. The zirconia sintered body according to any one of claims 1 to 3, further comprising yttrium oxide and / or ytterbium oxide as a stabilizer.

5. The zirconia sintered body according to claim 4, wherein the concentration of the stabilizer is 3 mol% or more and 6 mol% or less when the total of the zirconia and the stabilizer is 100 mol%.

6. the fracture toughness value of at least a portion of the surface of the surface layer in which the vanadium group element is unevenly distributed is 4.5 MPa√m or more; The zirconia sintered body according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Coated zro2 base ceramics and manufacture

    JP1987288182A

  • Coated zro2 base ceramics and manufacture

    JP1988050383A

  • Zirconia cutting object for dental cutting and method for producing the same

    JP2020033338A

  • Method of manufacturing zirconia cut body for dental cutting using precipitant

    JP2021165222A

  • Method For Enhancing Mechanical Properties In Sintered Ceramic Bodies Having Applications In Dental Restorations

    US20220081369A1