Method for depositing a coating on a substrate and method for manufacturing a timepiece component - Patents.com
By separating deposition and annealing steps and using dedicated enclosures, the method efficiently transforms intermetallic coatings into desired crystalline phases for luxury items, addressing the complexity and time issues of existing methods, and achieving aesthetically pleasing colors and decorations.
Patent Information
- Application Number
- JP2022180135
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-21
- Filing Date
- 2022-11-10
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2042-11-10
AI Technical Summary
Existing thin layer deposition methods for intermetallic compounds in watchmaking and jewelry are hampered by the need for time-consuming and complex in situ annealing, which limits their practical application due to the difficulty in achieving the desired crystalline phase and color.
A method involving sequential deposition and annealing steps, where the intermetallic thin layer is deposited on a substrate and then annealed in a dedicated enclosure separate from the deposition chamber, allowing simultaneous processing of multiple substrates and reducing time and complexity.
This approach enables efficient production of intermetallic coatings with desired colors by transforming the amorphous phase to a crystalline phase, reducing manufacturing time and costs, and enabling multicolored or contrasting decorations on luxury items like watches and jewelry.
Smart Images

Figure 0007569364000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of materials, in particular those determining the appearance of external parts of timepieces, jewellery and fashion items, or more generally of various articles.
[0002] In particular, the present invention relates to a method for depositing a coating on a substrate. [Background technology]
[0003] The deposition of thin layers in controlled atmospheres is commonly used in industry in general, and in the field of watchmaking and jewellery in particular, to produce coatings for aesthetic or technical applications.
[0004] For aesthetic applications, the deposited thin layers may be made of precious metals such as gold (Au) or silver (Ag), or precious metal alloys. Such precious metal alloys are often combinations of gold, silver, and copper (Cu), sometimes with the addition of platinum (Pt) or other similar metals. In such precious metal alloys, the atoms form metallic bonds with each other, which are responsible for the color and malleability of the alloy.
[0005] Frequently used thin layer deposition techniques include physical vapor deposition (PVD), particularly cathode sputtering and evaporation, chemical vapor deposition (CVD), galvanic metal deposition, and atomic layer deposition (ALD).
[0006] There are also intermetallic compounds, particularly of the precious metals, that can provide a wider range of colors than the standard precious metal alloys, such as Pt-Al for yellow, Pt-Al-Cu for orange and pink, Au-Al for blue, and Au-In for blue-violet.
[0007] In such intermetallic compounds, the atoms form strong covalent bonds which give them their particular color but which also make them hard and brittle in bulk form, making them less malleable and more difficult to mold, and therefore less usable in bulk form, and therefore rarely used in practice.
[0008] However, such intermetallic compounds can be used in the form of more or less thin layers by carrying out any of the vacuum thin layer deposition techniques described above. For example, these deposition techniques can be carried out to deposit thin layers of intermetallic compounds formed with metals such as Au, Al, Cu, In, Pt, e.g. AuAl2 or PtAl2.
[0009] However, thin layers of intermetallic compounds deposited by these methods are out of thermodynamic equilibrium and have a predominantly amorphous phase that is typically an aesthetically unpleasing gray color rather than the desirable color that the intermetallic compound of the same composition has in bulk and crystalline form.
[0010] Indeed, the thermodynamic state of the intermetallic compound, and in particular its crystallinity and / or the presence of various phases, greatly influences the color of a given composition.
[0011] Therefore, during the deposition process, a step of annealing the layer in situ, typically at 400° C., is carried out to crystallize at least a portion of the deposited intermetallic compound layer to obtain a layer color specific to the crystalline phase of said intermetallic compound for a given composition.
[0012] Although thin layers of intermetallic compounds offer an interesting option in terms of color choice compared to thin layers of standard precious metal alloys, they are still rarely used in practice due to the lengthy and complicated deposition methods required to perform the thin layers, due to the need for in situ annealing. Summary of the Invention [Problem to be solved by the invention]
[0013] The present invention is intended to solve the above problems. [Means for solving the problem]
[0014] In view of this situation, the present invention relates to a method for depositing a coating on a substrate, comprising the steps of: depositing on said substrate a thin layer formed by an intermetallic compound to obtain an external part of a timepiece, a piece of jewellery or a fashion item; and annealing said external part in a dedicated enclosure different from the one in which the deposition of the thin intermetallic compound layer was performed.
[0015] In contrast to prior art techniques in which in situ annealing is used for the deposition of thin layers, the present invention has the advantage that many substrates can be processed simultaneously, such as in a large furnace, thus reducing the time required to carry out the method for each part. This approach also allows thin layer deposition methods that do not allow in situ annealing to be used, at least without unacceptable method and / or equipment complexity.
[0016] In particular embodiments, the invention may further comprise one or more of the following features, taken alone or according to any technically possible combination:
[0017] In a particular embodiment, the depositing step is carried out by carrying out a PVD deposition process by cathode or ion sputtering, thermal evaporation, arc or electron beam evaporation, or pulsed laser beam ablation.
[0018] In a particular embodiment, the thin layer is deposited from at least one target composed of a composite of at least two types of metals or from at least two targets composed of different pure metals. When using pure metal targets, the thin layer is deposited by co-sputtering, i.e., by simultaneously cathodic sputtering at least two different pure metal targets, in which case the intermetallic compound is formed on the substrate by the merging of at least two atomic streams. Alternatively, the thin layer is deposited by co-evaporation, i.e., by simultaneously evaporating targets of different pure metals (for example in the form of powders or granules in a crucible or the like), in which case the intermetallic compound is formed on the substrate by the merging of atomic streams coming from at least two targets. The powers applied to the at least two targets are independently selected so that the sputtering rates of the at least two different metals result in the desired layer composition. However, the deposition rate of a metal varies with the wear of the corresponding target, and as a result, the composition of the layer varies as the target is utilized. Such deposition rate variations can be compensated for by correcting the power delivered to each target according to their wear, either manually based on a calibration table or automatically thanks to a feedback loop based on in situ measurements (e.g. spectral measurements of the optical emission of the plasma in the case of cathode sputtering).
[0019] When using an alloy target, the composition of the target is selected to obtain the desired layer composition directly on the substrate, which has the advantage that it does not depend on wear of the alloy target.
[0020] In a particular embodiment, the depositing step is carried out such that the thin intermetallic compound layer has a thickness of 20 to 1000 nm, preferably 200 to 500 nm, more preferably 300 nm.
[0021] In a particular embodiment, the annealing step is carried out by performing a global annealing operation in which the entire thin intermetallic layer is heat treated to crystallize it and impart the desired color.
[0022] In a particular embodiment, during said overall annealing operation, said outer part is brought to a temperature between 200° C. and 500° C., preferably substantially 300° C., for a duration between 30 minutes and 120 minutes, preferably 60 minutes.
[0023] In a particular embodiment, the global annealing step is carried out in a traditional furnace in air or in a protective atmosphere of an inert gas, e.g., argon (Ar), or in vacuum to avoid chemical interaction of the thin intermetallic compound layer with the atmosphere.
[0024] In a particular embodiment, the annealing step is performed by performing a local annealing operation on predetermined areas of the thin intermetallic layer, thus obtaining a color contrast between the non-annealed areas, which are mainly amorphous and gray, and the annealed areas, which are crystallized and colored.
[0025] In a particular embodiment, said annealing step is performed by performing a local annealing operation after said global annealing operation.
[0026] In a particular embodiment, the local annealing operation is performed with a laser beam having a diameter of 10 μ m~100 μ m, or even 50 μ m~100 μ This is done using a laser with a wavelength of 1000 nm.
[0027] In a particular embodiment, said local annealing operation is performed using a laser configured to emit pulses with a duration between 4 ns and 350 ns at a variable frequency between 10 kHz and 1 MHz.
[0028] In a particular embodiment, the localized annealing operation is carried out in an enclosure in ambient or protective atmosphere of an inert gas, e.g., argon (Ar), or in vacuum to avoid chemical interactions between the thin intermetallic compound layer and the atmosphere.
[0029] In a particular embodiment, the deposition step is preceded by a surface structuring step in which the surface of the substrate is structured, for example in only one portion.
[0030] In certain embodiments, portions of the structured surface of the substrate correspond to predetermined areas that have been subjected to a localized annealing operation, and the appearance contrast of the surface adds to the color contrast to provide advantageous aesthetic effects.
[0031] In a particular embodiment, the structuring is carried out over the entire surface of the substrate that is to be covered with the thin intermetallic layer.
[0032] In a particular embodiment, the method comprises, after the deposition step and the global and / or local annealing step, a step of depositing a layer for protecting the thin intermetallic compound layer from environmental hazards, the thin intermetallic compound layer being covered with a protective stack of thin dielectric layers deposited by one or more vacuum deposition techniques such as PVD, CVD or ALD.
[0033] In a particular embodiment, the thickness and composition of the dielectric thin layers forming the protective stack are selected to compensate for the optical interference effects of the dielectric thin layers with the aim of preserving the original color of the intermetallic compound thin layer.
[0034] In certain embodiments, the thickness and composition of the dielectric thin layers forming the protective stack are selected such that the optical interference effect of the dielectric thin layers can aesthetically alter the color of the intermetallic thin layers, for example by increasing the color saturation or by changing the hue in selected orientations.
[0035] In a particular embodiment, the protective layer is a semi-transparent polymer layer that is deposited by spraying or by any other method known to those skilled in the art.
[0036] In a particular embodiment, the protective layer is a composite layer, a combination of a polymer layer and a dielectric layer, deposited by techniques known to those skilled in the art.
[0037] According to another aspect, the invention further relates to a timepiece component comprising a substrate on which there is a coating deposited by carrying out said method, said timepiece component having a predetermined final color.
[0038] Other characteristics and advantages of the invention will appear clearly on reading the following detailed description, given by way of example. [Brief description of the drawings]
[0039]
Figure 1
[0040] The present invention relates to a method for depositing a coating on a substrate 100, which method comprises a deposition step for depositing a thin intermetallic layer 110 on the substrate 100 to obtain an outer part 10 of a timepiece, a piece of jewellery or a fashion item. In particular, such an outer part 10 may form a component for a timepiece.
[0041] The substrate 100 may be made of any suitable material, such as metallic materials, ceramics, etc.
[0042] The method includes a deposition step in which a thin intermetallic layer 110 is deposited on a substrate 100, followed by an annealing step in which said external component 10 is annealed in a dedicated enclosure so that the external component 10 has a predetermined final color.
[0043] The step of depositing the thin intermetallic layer 110 is carried out by carrying out a PVD deposition method, in particular by carrying out any of the following methods: ion or cathode sputtering, thermal evaporation, arc or electron beam evaporation, or pulsed laser beam ablation.
[0044] The thin intermetallic layer 110 is deposited from at least two targets, each composed of a specific metal, and / or from at least one target composed of a composite of at least two metals.
[0045] Preferably, in order to simplify the execution of the step of depositing the thin intermetallic layer 110, the thin intermetallic layer 110 is produced from a target composed of a composite of at least two metals, and the results obtained in the tests have demonstrated that the composition of the thin intermetallic layer 110 becomes more reproducible if the step of depositing the thin intermetallic layer 110 is executed by supplying it from a single target composed of a composite of metals.
[0046] By way of example, but without being limited thereto, the metal used may be selected from Pt, Al, Cu, In, Au or a composite of these metals.
[0047] In particular, the metals are selected such that the thin intermetallic layer 110 contains intermetallic bonds of, for example, Au-Al, Au-In, Pt-Al, or Pt-Al-Cu.
[0048] The deposition step is carried out such that the thickness of the thin intermetallic layer 110 is measured to be between 20 and 1000 nm, preferably between 200 and 500 nm, more preferably 300 nm. The thin intermetallic layer 110 thus preferably represents a good compromise between being thick enough to be opaque and configured to withstand the mechanical stresses to which the thin intermetallic layer 110 may be subjected, and being thin enough so that the amount of precious metal used is not too high and the time for depositing the thin intermetallic layer 110 is not too long.
[0049] The deposition process is carried out such that the thin intermetallic layer 110 has a predominantly amorphous phase after its deposition.
[0050] The parameters of the PVD deposition process, in particular the powers simultaneously applied to the various sources, are selected so that the resulting thin intermetallic layer 110 has a composition that has the desired final color after the annealing step.
[0051] By way of example, the thin intermetallic layer 110 can be made of a Pt-Al-Cu composite with a composition of 61.7% Pt, 18.3% Al, and 20.0% Cu by weight, the deposition step being carried out by cathodic co-sputtering from three pure Pt, Al, and Cu targets. At the end of the deposition step, the thin intermetallic layer 110 is poorly crystallized and has a color characterized by parameters (L*, a*, b*)=(77.5, 1.9, 2.6). It is therefore only slightly pinkish-gray, which is not very aesthetically advantageous. After an annealing step at 500° C. for 2 hours in a vacuum tube furnace, this layer is crystallized to have a color characterized by parameters (L*, a*, b*)=(78.2, 10.8, 20.8), and thus has a final pinkish-orange color that is very strong and aesthetically advantageous.
[0052] Said annealing step is preferably carried out in a dedicated enclosure different from the one in which the deposition of the thin intermetallic layer 110 took place, ie different from the deposition chamber in which the PVD deposition took place.
[0053] The annealing step has the effect of changing the phase of the thin intermetallic layer 110 by converting it from a primarily amorphous phase to a crystalline phase.
[0054] This technique of the invention has the advantage that it can be performed using standard equipment found on the market, without the need to create expensive specific equipment for in situ annealing of the layer, and the annealing step can be performed simultaneously on many outer parts 10 in the same enclosure, which tends to reduce manufacturing costs by shortening the time it would take to perform the method for each outer part 10.
[0055] Said annealing step can be carried out by carrying out a global annealing operation such as heat treating the entire thin intermetallic layer 110 and therefore the entire outer component 10 .
[0056] When performing a global annealing operation, the dedicated enclosure comprises a furnace.
[0057] Preferably, the overall annealing operation is carried out in a furnace with a controlled atmosphere, such as an argon or nitrogen atmosphere. Alternatively, the overall annealing operation can be carried out in a vacuum, with an operating pressure of, for example, 10 -4 ~1N / m 2 (10 -6 ~10 -2 mbar), preferably 10 -2 N / m 2 (10 -4 mbar).
[0058] The temperature of the outer part 10 during the overall annealing operation is, for example, between 200° C. and 500° C., preferably substantially 300° C. The duration of the overall annealing operation is, for example, between 30 minutes and 120 minutes, preferably 60 minutes.
[0059] Alternatively, the annealing step can be performed by performing a local annealing operation on a predetermined area 111 of the thin intermetallic layer 110 .
[0060] Said local annealing operation can be performed on the thin intermetallic layer 110 directly after its deposition, i.e., when it has mainly an amorphous phase, or it can be performed after a global annealing operation in which annealing is performed on the entire outer component 10.
[0061] This localized annealing step has the effect of locally changing the color of the thin intermetallic layer 110 in order to create decoration in the form of dial indices, numerals, logos, etc.
[0062] The local annealing operation is carried out with a laser, the diameter of the laser beam being for example 10 μm to 100 μm, or even 50 μm to 100 μm, the movement of the laser beam being preferably controlled by a scanning system intrinsic to the laser and based on a mechanical or optical axis, or by a scanning system intrinsic to the substrate and based on a mechanical axis, which gives a highly accurate position of the point of impact of the laser beam on the thin intermetallic compound layer 110.
[0063] The laser beam creates a localized increase in temperature at the point where it strikes the thin intermetallic layer 110, which causes a localized phase change in the thin intermetallic layer 110, resulting in a localized change in color.
[0064] The laser beam can be generated by a nanosecond pulsed laser, a microsecond pulsed laser, or in some cases by a continuous laser.
[0065] Specifically, during the local annealing step, the laser can be made to emit pulses of duration 4 ns to 350 ns with a variable frequency of 10 kHz to 1 MHz that can reach an average power of the order of 40 W.
[0066] Alternatively, the local annealing step can be performed using a picosecond or femtosecond pulsed laser, taking advantage of the fast heat accumulation effect at frequencies from 100-200 kHz to 10 MHz, or by a pulse sequence of bursts spaced apart from each other by a few picoseconds to a few nanoseconds as known to those skilled in the art.
[0067] The wavelength of the laser beam is chosen to favor the absorbance of the material of the thin intermetallic layer 110 that the beam impinges upon.
[0068] For example, the wavelength of the laser light can be within the infrared spectrum, the visible spectrum, or the ultraviolet spectrum.
[0069] During the local annealing step, the color of the intermetallic layer 110 changes depending on the variation in the energy of the pulses of the laser beam, their repetition frequency and their degree of overlap.
[0070] It is therefore possible to create multi-color or high contrast decorations based on a single deposition of a thin intermetallic layer 110 of homogeneous composition.
[0071] Advantageously, the deposition step and the annealing step of the thin intermetallic layer can be preceded by a structuring step in which the surface 112 of the substrate 100 is structured in part, referred to in the remainder of the specification as "structured portion 113", so as to generate a surface structure contrast on said surface 112.
[0072] The structured portion 113 of the surface 112 of the substrate 100 may correspond to a predetermined area 111 of the intermetallic layer 110 that is to be heat treated during a localized annealing operation, with the advantageous effect that the appearance of said predetermined area 111 is more distinct from the appearance of the remaining part of the thin intermetallic layer 110.
[0073] Instead, in an alternative embodiment of the invention, the entire surface 112 of the substrate 100 is structured.
[0074] Such a surface structuring step may involve partially or totally applying to the surface 112 of the substrate 100, for example a polished, matt or satin finish, depending on the variant considered.
[0075] To facilitate the local annealing step and reduce the local contribution of heat required to cause the phase transformation of the thin intermetallic layer, the outer part 10 can be preheated to a temperature close to the phase transformation temperature, thereby reducing the additional energy contribution by the laser.
[0076] During a subsequent deposition step, the thin intermetallic layer 110 obtained after said deposition step can preferably be covered with a protective layer 120, for example formed by a stack of thin dielectric layers intended to protect the thin intermetallic layer 110 from environmental hazards, this deposition step being carried out in the same deposition equipment as that used to carry out the step of depositing the thin intermetallic layer 110. This stack of thin dielectric layers can also have the effect of modifying the visual appearance of the external component 10, for example by increasing the luminance and / or by changing the color of the intermetallic layer 110 by taking advantage of advantageous interference effects.
[0077] The step of depositing the protective layer 120 is preferably the last step of the method according to the invention.
[0078] The stack of thin dielectric layers can be formed from various oxides, nitrides and oxynitrides such as TiO2, Al2O3, SiO2, SiN, Si3N4 and can be deposited by ALD and / or PVD and / or CVD deposition methods.
[0079] Alternatively, the step of depositing the protective layer 120 may involve depositing a varnish layer, for example a polymer varnish layer of the Zapon or Parylene type.
[0080] Overall, the method according to the invention, if all of the steps described above are carried out in sequence, starts with a step of structuring the surface of the substrate 100, then a step of depositing a thin intermetallic layer 110, followed by a global and / or local annealing step and finally a step of depositing a protective layer 120.
[0081] Thus, the present invention proposes an approach involving the use of intermetallic compounds, in particular based on precious metals, to provide a wide range of new colors for aesthetic applications in watches, jewellery and any other luxury items.
[0082] More generally, it should be noted that the implementations and embodiments discussed above have been described by way of example, and other variations are possible. [Explanation of symbols]
[0083] 10 Outer parts 100 Base material 110 Intermetallic compound thin layer 111 Predetermined area 112 sides 113 Structured part 120 protective layer
Claims
1. A method for depositing a coating on a substrate (100), comprising the steps of: a depositing step for depositing a thin layer (110) containing intermetallic bonds on said substrate (100) to obtain an outer part (10) of a timepiece, jewellery or fashion item; an annealing step in which the outer part (10) is annealed in a dedicated enclosure different from the one in which the thin layer (110) was deposited; The depositing step is carried out by carrying out a PVD deposition method by cathode or ion sputtering, thermal evaporation, arc or electron beam evaporation, or pulsed laser beam ablation; The deposition of said thin layer is carried out from at least two targets composed of different pure metals, The power applied to the target is compensated for wear of the target. A method comprising:
2. The deposition step is carried out such that the thin layer (110) has a thickness of 20 to 1000 nm, or 200 to 500 nm, or 300 nm.
2. The method of claim 1 .
3. The annealing step is carried out by carrying out a global annealing operation in which the entire thin layer (110) is heat treated.
2. The method of claim 1 .
4. During the general annealing operation, the outer part (10) is subjected to a temperature of between 200° C. and 500° C., or substantially 300° C., for a duration of between 30 minutes and 120 minutes, or 60 minutes.
4. The method according to claim 3 .
5. The annealing step is carried out by performing a local annealing operation on a predetermined area (111) of the thin layer (110).
2. The method of claim 1 .
6. The annealing step is carried out by performing a local annealing operation on a predetermined area (111) of the thin layer (110) after the global annealing operation.
4. The method according to claim 3 .
7. The local annealing operation is carried out using a laser with a laser beam diameter of 10 μm to 100 μm.
7. The method according to claim 5 or 6.
8. The local annealing operation is carried out using a laser configured to emit pulses with durations between 4 ns and 350 ns at a variable frequency between 10 kHz and 1 MHz.
7. The method according to claim 5 or 6.
9. The deposition step is preceded by a surface structuring step in which the surface (112) of the substrate (100) is structured.
2. The method of claim 1 .
10. Only the structured portion (113) of the surface (112) of the substrate (100) is structured, which portion corresponds to the predetermined area (111) of the thin layer (110) that is to be subjected to a local annealing operation.
10. The method of claim 9.
11. The structuring is performed on the entire surface (112) of the substrate (100).
10. The method of claim 9.
12. After the deposition and annealing steps, a protective layer deposition step is performed in which a protective layer (120) is deposited.
2. The method of claim 1 .
13. During the protective layer deposition step, the thin layer (110) is covered with a protective stack of dielectric thin layers and / or a semi-transparent polymer layer.
13. The method of claim 12.
14. The composition and thickness of the dielectric thin layers of the protective stack (120) are specifically selected to preserve the original color of the thin layer (110) or to be able to change the color of the thin layer (110) in a selected orientation.
14. The method of claim 13.
15. A method for manufacturing a timepiece component comprising a substrate (100), comprising the steps of: depositing a coating on said substrate (100) by carrying out the method of claim 1; The timepiece component has a predetermined final color.
2. A method for manufacturing a timepiece component, comprising:
Citation Information
Patent Citations
Amorphous alloy for ornament
JP1989123042A
Decorative member and method for manufacturing the same
JP2020116392A
Cherry blossom pink decorative member and production method therefor
WO2017170324A1